Pure-phase polyanionic sulfate sodium ion battery positive electrode material and preparation method therefor

By preparing NaxMyAzSO4, a pure-phase polyanionic sulfate sodium-ion battery cathode material, the problems of unstable structure and insufficient performance of existing sodium-ion battery cathode materials have been solved, and high discharge potential and excellent rate performance have been achieved, making it suitable for commercial applications.

WO2024212632A1PCT designated stage expired Publication Date: 2024-10-17SHENZHEN JANAENERGY TECH CO LTD

Patent Information

Application Number
PCT/CN2024/071510
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-01-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing sodium-ion battery cathode materials have problems such as structural instability, presence of impurities, poor conductivity, strong water absorption, poor storage and poor rate performance, which limit their application in sodium-ion batteries.

Method used

The chemical formula of pure phase polyanionic sodium sulfate sodium ion battery cathode material is NaxMyAzSO4, M is Mn, Fe, Co, Ni, Cu and/or Zn, A is Li, K and/or Na, and is prepared by inert atmosphere sintering , forming a material of the triclinic P21/c space group, improving structural stability and electrochemical performance.

Benefits of technology

The material has good structural stability, excellent rate performance, good cycle performance, simple preparation method and low cost. It has high discharge potential and sodium storage capacity, and is suitable for the commercial application of sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024071510_17102024_PF_FP_ABST
    Figure CN2024071510_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a pure-phase polyanionic sulfate sodium ion battery positive electrode material and a preparation method therefor. The chemical general formula of the pure-phase polyanionic sulfate sodium ion battery positive electrode material is NaxMyAzSO4, wherein M is one or two or more of Mn, Fe, Co, Ni, Cu, and / or Zn, A is one or two or more of Li, K, and / or Na, and the value ranges of variables are: 0.75≤x≤0.85, 0.52≤y≤0.58, 0<z≤0.1, and x+2y+z=2. The pure-phase polyanionic sulfate sodium ion battery positive electrode material has the characteristics of good structural stability, excellent rate performance, good cycle performance, simple preparation method, and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Pure phase polyanion sulfate sodium ion battery positive electrode material and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a pure phase polyanion sulfate sodium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] The establishment of the dual carbon goals has spurred the rapid development of the new energy industry. In recent years, the adoption of new energy electric vehicles has steadily increased, and this rapid growth has been accompanied by innovations in secondary battery technology. Due to their mature technology and high energy conversion efficiency, secondary batteries are currently an ideal choice for both power and energy storage. While there are a wide variety of secondary batteries, including lead-acid, nickel-metal hydride, nickel-cadmium, alkaline zinc-manganese, and lithium-ion / sodium-ion batteries, lithium-ion / sodium-ion batteries are undoubtedly the mainstream choice for the future of new energy. However, based on process maturity, environmental adaptability, and energy conversion efficiency, lithium-ion / sodium-ion batteries are undoubtedly the mainstream choice for the future of new energy.

[0003] However, lithium-ion batteries rely heavily on lithium resources, which are limited in reserves, and cannot meet the low-cost requirements of energy storage in the long term. In contrast, sodium resources are abundant and relatively low-cost. Sodium-ion batteries operate on the same principles as lithium-ion batteries, making them a potential and feasible alternative to lithium-ion batteries.

[0004] Currently, sodium-ion cathode materials include layered oxides, Prussian blue and its analogs, and polyanionic materials, each with its own advantages and disadvantages. For example, layered oxides often undergo multiple phase transitions during the redox and deintercalation of sodium, leading to structural collapse and thus affecting the material's cyclic stability. For example, during the synthesis of Prussian blue-based materials, a large amount of lattice water is incorporated into the structure, which decomposes at high potentials to produce large amounts of gas, causing battery swelling and failure. Compared to the first two types of materials, polyanionic materials, with their stable 3D framework structure and excellent electrochemical performance, have better application prospects in sodium battery cathodes.

[0005] Currently, the main polyanion materials include V-based phosphates such as Na₃V₂(PO₄)₃ and NaVPO₄F, and Fe-based phosphates such as Na₂FeP₂Oₐ, Na₄Fe₃(PO₄)₂P₂Oₐ, and NaFePO₄. Although V-based phosphates have high redox potentials (3.4-3.6 V) and suitable discharge capacities, their toxicity makes them difficult to scale up for application. In contrast, Fe-based phosphates, due to their non-toxic, pollution-free, and inexpensive properties, form the basis for their large-scale application. However, their low redox potential (~3 V) leads to low energy density in battery systems. Consequently, iron-based sulfate cathode materials, with their extremely low cost and high operating potential, are considered the most ideal cathode materials for sodium-ion batteries. However, these iron-based sulfate cathode materials suffer from disadvantages such as poor conductivity, strong water absorption, poor storage, poor stability, and poor rate performance.

[0006] Chinese invention application CN114400309A addresses the shortcomings of existing carbon-based materials and iron-based sulfate cathode materials by combining them to improve the performance of iron-based sulfate cathode materials. The invention discloses a sodium-ion cathode material, its preparation method, and its application. The sodium-ion cathode material comprises a core and a coating layer coated on the surface of the core. The core comprises a polyanionic sodium-ion cathode material having the general chemical formula NaxMy(SO4)3, where M comprises any one or a combination of at least two of Ni, Co, Mn, Fe, Cu, or Zn, with 2≤x≤3, 1.5≤y≤2, and x+2y=6. The coating layer comprises a carbon material coated with a conductive polymer. This improves the electronic conductivity of the material, increases the lattice parameter of the coated material, contributes to the stability of the material structure, and effectively enhances the capacity, rate capability, and cycling performance of the sodium-ion cathode material. However, in terms of its lattice system, the polyanionic sodium ion cathode material disclosed herein belongs to the monoclinic system and the Pnma space group. Although it shows good crystallinity, it also contains a lot of impurities. For example, from its XRD in Figure 1, it can be seen that there are multiple diffraction peaks in the range of 20-24° for 2θ (theoretical main diffraction peaks are 2). After searching, some of its diffraction peaks (21° and 23°, etc.) come from Na6Fe(SO4)4 impurities. The presence of this impurity means an imbalance in the ratio of Na, Fe and SO4. At the same time, the presence of this impurity will reduce the proportion of active material content, which is not conducive to the gram capacity. Due to the uncontrollability of the impurities, it brings uncertainty to the discharge potential, rate performance, cycle performance, etc., which is not conducive to actual large-scale production and application.

[0007] Summary of the Invention

[0008] The present invention aims to provide a pure phase polyanion sulfate sodium ion battery cathode material and a preparation method thereof, which has the characteristics of good structural stability, excellent rate performance, good cycle performance, simple preparation method and low cost.

[0009] The present invention can be achieved through the following technical solutions:

[0010] The present invention discloses a pure phase polyanion type sodium sulfate ion battery positive electrode material, the chemical general formula of the pure phase polyanion type sodium sulfate ion battery positive electrode material is Na x M y A z SO4; wherein M is one or more of Mn, Fe, Co, Ni, Cu and / or Zn; A is one or more of Li, K and / or Na; the value range of each variable is: 0.75≤x≤0.85, 0.52≤y≤0.58; 0 <z≤0.1、x+2y+z=2。

[0011] Furthermore, the pure phase polyanionic sulfate sodium ion battery positive electrode material is a triclinic P21 / c space group.

[0012] Furthermore, in terms of site division, Na, S and O are located at the 4e site, and M and A are located at the 8f site; Na / S-O4 is a tetrahedron, and M / A-O6 is an octahedron, and the tetrahedron and octahedron are connected at the same point / face.

[0013] Furthermore, in the triclinic P21 / c space group, the lattice parameters vary within the range:

[0014] Another aspect of the present invention is to protect the preparation method of the above-mentioned pure phase polyanionic sulfate sodium ion battery positive electrode material, comprising the following steps: uniformly mixing a sodium source, a metal source, an alkali metal source, an anion source and a carbon source according to a stoichiometric ratio, and sintering in an inert atmosphere to obtain the corresponding pure phase polyanionic sulfate sodium ion battery positive electrode material.

[0015] Furthermore, the sodium source is an inorganic sodium source and / or an organic sodium source, the inorganic sodium source is one or more of sodium hydroxide, sodium chloride, sodium sulfate, sodium nitrate and / or sodium carbonate, and the organic sodium source is one or more of sodium formate, sodium acetate, sodium ethoxide and / or sodium benzoate.

[0016] Furthermore, the metal source is a manganese source, an iron source, a cobalt source, a nickel source, a copper source, and / or a zinc source; the manganese source is one or more of manganese sulfate, manganese carbonate, manganese chloride, and / or manganese acetate; the iron source is one or more of ferrous sulfate, ferric chloride, ferrous oxide, and / or iron acetate; the cobalt source is one or more of cobalt sulfate, cobalt nitrate, cobalt chloride, and / or cobalt acetate; the nickel source is one or more of nickel sulfate, nickel nitrate, nickel chloride, and / or nickel acetate; the copper source is one or more of copper sulfate, copper chloride, and / or copper acetate; the zinc source is one or more of zinc sulfate, zinc chloride, and / or zinc acetate.

[0017] Furthermore, the alkali metal source is a sodium source, a lithium source, and / or a potassium source.

[0018] Furthermore, the sodium source as the alkali metal source is an inorganic sodium source and / or an organic sodium source. The inorganic sodium source is one or more of sodium hydroxide, sodium chloride, sodium sulfate, sodium nitrate, and / or sodium carbonate. The organic sodium source is one or more of sodium formate, sodium acetate, sodium ethoxide, and / or sodium benzoate.

[0019] Furthermore, the lithium source is one or more of lithium sulfate, lithium carbonate, and / or lithium hydroxide.

[0020] Furthermore, the potassium source is one or more of potassium sulfate, potassium hydroxide, potassium chloride, potassium nitrate, and / or potassium carbonate.

[0021] Furthermore, the anion source is one or more of sulfuric acid, sodium sulfate, ammonium ferrous sulfate, ferrous sulfate, and / or ammonium sulfate.

[0022] Furthermore, the carbon source is a carbon material such as SurpP, KB, carbon nanotubes, graphene, and one or more of glucose, citric acid, and / or sucrose.

[0023] Furthermore, the uniform mixing method is a liquid-phase mixing method or a solid-phase mixing method; the inert atmosphere is argon, nitrogen, or a mixed gas of argon and hydrogen, nitrogen and hydrogen; the sintering temperature is 200 - 400 °C.

[0024] The pure-phase polyanionic sulfate sodium-ion battery cathode material and its preparation method of the present invention have the following beneficial effects:

[0025] The polyanionic sulfate sodium-ion battery cathode material Na x M y A z SO4 shows a single pure phase within the range of 0.75 ≤ x ≤ 0.85, 0.52 ≤ y ≤ 0.58; 0 < z ≤ 0.1, x + 2y + z = 2, and has optimal electrochemical performance.

[0026] This material is a triclinic crystal with a P21 / c space group. The M and A in its structure occupy the same 8f position, which can effectively weaken the Coulomb force between adjacent MMs, thereby improving the structural stability of the material and achieving a faster sodium deintercalation rate.

[0027] The material has a high discharge potential (3.7VvNa / Na + ) and sodium storage capacity (110mAh / g); excellent long-cycle stability (100% retention rate for 1000 cycles at 10C rate) and outstanding rate performance (60mAh / g at 30C rate).

[0028] The preparation process of this material is simple and is compatible with traditional solid-phase method, liquid-phase method and solid-liquid mixing method. In addition, the raw materials are abundant and the material cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 shows Na 0.82 Fe 0.55 Na 0.08 SO4 material XRD;

[0030] Figure 2 shows Na 0.82 Fe 0.55 Na 0.08 SO4 material SEM;

[0031] Figure 3 shows Na 0.82 Fe 0.55 Na 0.08 Charge and discharge curve of SO4 electrode in the first week;

[0032] Figure 4 shows Na 0.82 Fe 0.55 Na 0.08 SO4 electrode rate performance curve;

[0033] Figure 5 shows Na 0.82 Fe 0.55 Na 0.08 SO4 electrode cycle curve;

[0034] Figure 6 shows Na 0.85 Fe 0.53 Li 0.09 SO4 material XRD;

[0035] Figure 7 shows Na 0.78 Fe 0.57 K 0.08 SO4 material XRD;

[0036] Figure 8 shows Na 0.92 Fe 0.50 K 0.08 SO4 material XRD;

[0037] Figure 9 shows Na 0.74 Fe 0.59 Li 0.08 SO4 material XRD;

[0038] Figure 10 shows Na 0.92 Fe 0.50 K 0.08 SO4 / Na 0.74 Fe 0.59 Li 0.08 Charge and discharge curve of SO4 electrode in the first week;

[0039] Figure 11 shows Na 0.92 Fe 0.50 K 0.08 SO4 / Na 0.74 Fe 0.59 Li 0.08 SO4 electrode cycle curve. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below with reference to the embodiments and drawings.

[0041] The present invention discloses a pure phase polyanion type sodium sulfate ion battery positive electrode material, the chemical general formula of the pure phase polyanion type sodium sulfate ion battery positive electrode material is Na x M y A z SO4; wherein M is one or more of Mn, Fe, Co, Ni, Cu and / or Zn; A is one or more of Li, K and / or Na; the value range of each variable is: 0.85≤x≤0.95, 0.52≤y≤0.58; 0 <z≤0.1、x+2y+z=2。

[0042] Furthermore, the pure phase polyanionic sulfate sodium ion battery positive electrode material is a triclinic P21 / c space group.

[0043] Furthermore, in terms of site division, Na, S and O are located at the 4e site, and M and A are located at the 8f site; Na / S-O4 is a tetrahedron, and M / A-O6 is an octahedron, and the tetrahedron and octahedron are connected at the same point / face.

[0044] Furthermore, in the triclinic P21 / c space group, the lattice parameters vary within the range:

[0045] Another aspect of the present invention is to protect the preparation method of the above-mentioned pure phase polyanionic sulfate sodium ion battery positive electrode material, comprising the following steps: uniformly mixing a sodium source, a metal source, an alkali metal source, an anion source and a carbon source according to a stoichiometric ratio, and sintering in an inert atmosphere to obtain the corresponding pure phase polyanionic sulfate sodium ion battery positive electrode material.

[0046] Furthermore, the sodium source is an inorganic sodium source and / or an organic sodium source, the inorganic sodium source is one or more of sodium hydroxide, sodium chloride, sodium sulfate, sodium nitrate and / or sodium carbonate, and the organic sodium source is one or more of sodium formate, sodium acetate, sodium ethanol and / or sodium benzoate.

[0047] Furthermore, the metal source is a manganese source, an iron source, a cobalt source, a nickel source, a copper source and / or a zinc source; the manganese source is one or more of manganese sulfate, manganese carbonate, manganese chloride and / or manganese acetate; the iron source is one or more of ferrous sulfate, ferric chloride, ferrous oxide and / or ferric acetate; the cobalt source is one or more of cobalt sulfate, cobalt nitrate, cobalt chloride and / or cobalt acetate; the nickel source is one or more of nickel sulfate, nickel nitrate, nickel chloride and / or nickel acetate; the copper source is one or more of copper sulfate, copper chloride and / or copper acetate; and the zinc source is one or more of zinc sulfate, zinc chloride and / or zinc acetate.

[0048] Furthermore, the alkali metal source is a sodium source, a lithium source and / or a potassium source.

[0049] Furthermore, the sodium source serving as the alkali metal source is an inorganic sodium source and / or an organic sodium source, the inorganic sodium source is one or more of sodium hydroxide, sodium chloride, sodium sulfate, sodium nitrate and / or sodium carbonate, and the organic sodium source is one or more of sodium formate, sodium acetate, sodium ethanol and / or sodium benzoate.

[0050] Furthermore, the lithium source is one or more of lithium sulfate, lithium carbonate and / or lithium hydroxide.

[0051] Furthermore, the potassium source is one or more of potassium sulfate, potassium hydroxide, potassium chloride, potassium nitrate and / or potassium carbonate.

[0052] Furthermore, the anion source is one or more of sulfuric acid, sodium sulfate, ferrous ammonium sulfate, ferrous sulfate and / or ammonium sulfate.

[0053] Furthermore, the carbon source is one or more of carbon materials such as SurpP, KB, carbon nanotubes, graphene, glucose, citric acid and / or sucrose.

[0054] Furthermore, the uniform mixing method is a liquid phase mixing method or a solid phase mixing method; the inert atmosphere is argon, nitrogen, or a mixed gas of argon, hydrogen, nitrogen and hydrogen; and the sintering temperature is 200-400°C.

[0055] Specifically, the liquid-phase mixing method involves dissolving a sodium source, a metal source, an alkali metal source, an anion source, and a carbon source in an organic or inorganic solvent and drying the resulting mixture to obtain a uniformly mixed precursor. Drying methods include one or more of high-temperature drying methods such as forced air drying and spray drying, low-temperature drying methods such as freeze drying, and low-pressure drying methods such as vacuum drying. The inorganic solvent is water, and the organic solvent is one or more of methanol, ethanol, acetonitrile, and the like.

[0056] Specifically, the solid phase mixing method involves uniformly mixing the sodium source, metal source, alkali metal source, anion source, and carbon source through mechanical force, wherein the mechanical force is provided by sand milling, ball milling, and other techniques.

[0057] Example 1

[0058] This embodiment involves Na 0.82 Fe 0.55 Na 0.08 The synthesis of SO4 and its electrochemical properties are as follows:

[0059] Sodium hydroxide, ferrous acetate, sodium acetate and ammonium sulfate were added to the ball mill in a molar ratio of 0.82:0.55:0.05:1. The carbon source was KB. 20 mL of acetone was poured into the ball mill (N2 protection). The ball-to-material ratio was 20:1. The rotation speed was 400 r / min. The total ball milling time was 7 hours, with an interval downtime of 10 minutes. Finally, the ball-milled precursor gel was placed in an Ar / H2 (90:10) atmosphere at a heating rate of 1°C / min and kept at 100°C for 3 hours. Then, it was kept at 200°C for 3 hours at a heating rate of 1°C / min. Then, it was continued to be heated to 350°C at a heating rate of 1°C / min and kept at this temperature for 5 hours. After the temperature dropped to room temperature, Na 0.82 Fe 0.55 Na 0.08 Figure 1 shows Na 0.82 Fe 0.55 Na 0.08 The XRD diffraction peaks of SO4 powder are completely consistent with the theoretical calculated diffraction peaks, indicating that it is a single pure phase with high crystallinity. In the pure phase structure, ions migrate smoothly along specific crystal planes, with high rates and good rate performance. In addition, the active material accounts for a very high proportion in the pure phase structure, and its capacity utilization is close to the actual theoretical specific capacity. Figure 2 shows the Na 0.82 Fe 0.55 Na 0.08 The morphology of SO4 material presents nano-scale agglomerated particles. The smaller particle size can effectively reduce the distance of the sodium ion deintercalation process, thereby increasing the rate of sodium deintercalation in the material.

[0060] Will Na0.82 Fe 0.55 Na 0.08 SO4, AB, and PVDF were mixed into a slurry at a mass ratio of 7:2:1. The black slurry was then coated onto aluminum foil using a 150 μm four-sided film preparation device. The film was then dried in a vacuum drying oven at 100°C for 2 hours. The electrode film was punched into discs with a radius of 0.6 mm using a sheet puncher. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0061] The button cell was subjected to constant current charge and discharge tests at a current density of 0.1C (1C = 100 mAh / g). 0.82 Fe 0.55 Na 0.08 The charge and discharge curve of SO4 electrode in the first week shows that the reversible specific capacity is 110mAh / g in the voltage range of 2.0-4.3V and the average discharge potential is 3.7V. 0.82 Fe 0.55 Na 0.08 As shown in the figure, the capacity of SO4 electrode is 60mAh / g at 30C rate. 0.82 Fe 0.55 Na 0.08 The long-term cycle stability of the SO4 electrode shows that the capacity of the electrode has almost no attenuation after 1000 cycles at 10C, demonstrating good structural stability.

[0062] Example 2

[0063] This embodiment involves Na 0.85 Fe 0.53 Li 0.09 The synthesis of SO4 and its electrochemical properties are as follows:

[0064] Lithium sulfate, ferrous acetate and sodium sulfate were added to the ball mill in a molar ratio of 0.045:0.53:0.425. The carbon source was KB. 20 mL of acetone was poured into the ball mill (N2 protection). The ball-to-material ratio was 20:1. The rotation speed was 400 r / min. The total ball milling time was 7 hours, with an interval downtime of 10 minutes. Finally, the ball-milled precursor gel was placed in an Ar / H2 (90:10) atmosphere at a heating rate of 1°C / min and kept at 100°C for 3 hours. Then, it was kept at 200°C for 3 hours at a heating rate of 1°C / min. Then, it was continued to be heated to 350°C at a heating rate of 1°C / min and kept at this temperature for 5 hours. After the temperature dropped to room temperature, the Na 0.85 Fe 0.53Li 0.09 Figure 6 shows Na 0.85 Fe 0.53 Li 0.09 The XRD diffraction characteristic peaks of SO4 powder are completely consistent with the theoretically calculated diffraction peak positions, indicating that it is a single pure phase with high crystallinity.

[0065] Will Na 0.85 Fe 0.53 Li 0.09 SO4, AB, and PVDF were mixed into a slurry at a mass ratio of 7:2:1. The black slurry was then coated onto aluminum foil using a 150 μm four-sided film preparation device. The film was then dried in a vacuum drying oven at 100°C for 2 hours. The electrode film was punched into discs with a radius of 0.6 mm using a sheet puncher. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0066] The button cell was subjected to constant current charge and discharge tests at a current density of 0.1 C (1 C = 100 mAh / g). Within a voltage range of 2.0-4.3 V, the reversible specific capacity was 109 mAh / g.

[0067] Example 3

[0068] This embodiment involves Na 0.78 Fe 0.57 K 0.08 The synthesis of SO4 and its electrochemical properties are as follows:

[0069] Potassium sulfate, ferrous sulfate and sodium sulfate were added to the ball mill in a molar ratio of 0.04:0.285:0.39. The carbon source was KB. 20 mL of acetone was poured into the ball mill (N2 protection). The ball-to-material ratio was 20:1. The rotation speed was 400 r / min. The total ball milling time was 7 hours, with an interval downtime of 10 minutes. Finally, the ball-milled precursor gel was placed in an Ar / H2 (90:10) atmosphere at a heating rate of 1°C / min and kept at 100°C for 3 hours. Then, it was kept at 200°C for 3 hours at a heating rate of 1°C / min. Then, it was continued to be heated to 350°C at a heating rate of 1°C / min and kept at this temperature for 5 hours. After the temperature dropped to room temperature, the Na 0.78 Fe 0.57 K 0.08 Figure 7 shows the Na 0.78 Fe 0.57 K 0.08 The XRD diffraction characteristic peaks of SO4 powder are completely consistent with the theoretically calculated diffraction peak positions, indicating that it is a single pure phase with high crystallinity.

[0070] Will Na 0.78 Fe 0.57 K 0.08 SO4, AB, and PVDF were mixed into a slurry at a mass ratio of 7:2:1. The black slurry was then coated onto aluminum foil using a 150 μm four-sided film preparation device. The film was then dried in a vacuum drying oven at 100°C for 2 hours. The electrode film was punched into discs with a radius of 0.6 mm using a sheet puncher. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0071] The button cell was subjected to constant current charge and discharge tests with a current density of 0.1C (1C=100mAh / g). Within a voltage range of 2.0-4.3V, the reversible specific capacity was 112mAh / g.

[0072] Example 4

[0073] This embodiment involves Na 0.86 Fe 0.52 K 0.1 The synthesis of SO4 and its electrochemical properties are as follows:

[0074] Sulfuric acid, sodium carbonate, ferrous oxalate and potassium chloride were added to the flask in a molar ratio of 1.0:0.425:0.52:0.1, and 50 mL of deionized water was added to the flask. Glucose was used as a carbon source and ascorbic acid was used as an antioxidant. After dissolution, a light green solution was obtained. The above solution was spray dried, the inlet temperature was set to 250 ° C, the peristaltic pump speed was 15 r / min, and the outlet temperature was controlled at 110 ° C to obtain a pure white precursor powder. Finally, in an Ar atmosphere, the temperature was kept at 200 ° C for 3 hours at a heating rate of 1 ° C / min, and then the temperature was increased to 350 ° C at a heating rate of 2 ° C / min and kept at this temperature for 6 hours. After the temperature dropped to room temperature, the black Na 0.86 Fe 0.52 K 0.1 SO4 material.

[0075] Will Na 0.86 Fe 0.52 K 0.1SO4, surpP, and PVDF were mixed in a mass ratio of 8:1:1 and coated onto aluminum foil using a 200μm four-sided coating machine. The electrode film was then dried in a vacuum oven at 100°C for 3 hours. A sheet puncher was used to punch the electrode film into discs with a radius of 0.6mm. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1mol / L NaClO4EC+DEC (1:1 vol%)+5%FEC as the electrolyte, and a glass fiber separator.

[0076] The button cell was subjected to constant current charge and discharge tests with a current density of 0.1C (1C=100mAh / g). Within a voltage range of 2.0-4.3V, the reversible specific capacity was 105mAh / g.

[0077] Example 5

[0078] This embodiment involves Na 0.83 Fe 0.58 Li 0.01 The synthesis of SO4 and its electrochemical properties are as follows:

[0079] Ferrous sulfate, lithium carbonate, ammonium sulfate, and sodium hydroxide were added to a beaker at a molar ratio of 0.58:0.01:0.42:0.83. Dissolved in 50 mL of deionized water, a light green solution was obtained. The solution was then spray-dried with the inlet air temperature set at 250°C, the peristaltic pump speed at 15 rpm, and the outlet air temperature controlled at 110°C to obtain a pure white precursor powder. The precursor powder was then dried in a vacuum drying oven at 200°C for 10 hours. The precursor powder was then mixed with KB and subjected to high-energy ball milling at a ball-to-material ratio of 20:1 and a frequency of 50 Hz for approximately 3 hours. The resulting black powder was then heated at 200°C in an N2 atmosphere at a heating rate of 1°C / min for 3 hours. The temperature was then increased to 350°C at a rate of 2°C / min and maintained at this temperature for 6 hours. After the temperature dropped to room temperature, the black NaOH was removed. 0.83 Fe 0.58 Li 0.01 SO4 material.

[0080] Will Na 0.83 Fe 0.58 Li 0.01SO4, KB, and PVDF were mixed in a mass ratio of 8:1:1 and coated onto aluminum foil using a 100 μm four-sided coating machine. The resulting electrode film was then dried in a vacuum oven at 100°C for 3 hours. A sheet puncher was used to punch the electrode film into discs with a radius of 0.6 mm. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0081] The button cell was subjected to constant current charge and discharge tests with a current density of 0.1C (1C=100mAh / g). Within a voltage range of 2.0-4.3V, the reversible specific capacity was 107mAh / g.

[0082] Example 6

[0083] This embodiment involves Na 0.86 Mn 0.54 Na 0.06 The synthesis of SO4 and its electrochemical properties are as follows:

[0084] Manganese acetate, sodium acetate, ammonium sulfate and sodium chloride were added to a beaker in a molar ratio of 0.54:0.86:1.0:0.06, and 50 mL of deionized water was taken to dissolve. After the dissolution was completed, a light green solution was obtained. The solution was then spray dried, the inlet temperature was set to 250 ° C, the peristaltic pump speed was 15r / min, and the outlet temperature was controlled at 110 ° C to obtain a pure white precursor powder. After that, the precursor powder was dried in a vacuum drying oven at 200 ° C for 10 hours. The precursor powder was then mixed with KB for high-energy ball milling with a ball-to-material ratio of 20:1, a frequency of 50 Hz, and a duration of about 3 hours. The evenly mixed black powder material was then placed in a N2 atmosphere at a heating rate of 1 ° C / min, kept at 200 ° C for 3 hours, and then heated to 350 ° C at a heating rate of 2 ° C / min and kept at this temperature for 6 hours. After the temperature dropped to room temperature, the black Na 0.86 Mn 0.54 Na 0.06 SO4 material.

[0085] Will Na 0.86 Mn 0.54 Na 0.06SO4, KB, and PVDF were mixed in a mass ratio of 8:1:1 and coated onto aluminum foil using a 100μm four-sided coating machine. The resulting electrode film was then dried in a vacuum oven at 100°C for 3 hours. A sheet puncher was used to punch the electrode film into discs with a radius of 0.6mm. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0086] The button cell was subjected to constant current charge and discharge tests with a current density of 0.1C (1C=100mAh / g). Within a voltage range of 2.0-4.8V, the reversible specific capacity was 100mAh / g.

[0087] Example 7

[0088] This embodiment involves Na 0.88 Co 0.55 Li 0.02 The synthesis of SO4 and its electrochemical properties are as follows:

[0089] Sodium hydroxide, cobalt sulfate, lithium acetate and ammonium sulfate were added to the ball mill in a molar ratio of 0.88:0.55:0.02:0.45. The carbon source was KB. 20 mL of acetone was poured into the ball mill (N2 protection). The ball-to-material ratio was 20:1. The rotation speed was 400 r / min. The total ball milling time was 7 hours, with an interval downtime of 10 minutes. Finally, the ball-milled precursor gel was placed in an Ar / H2 (90:10) atmosphere at a heating rate of 1°C / min and kept at 100°C for 3 hours. Then, it was kept at 200°C for 3 hours at a heating rate of 1°C / min. Then, it was continued to be heated to 350°C at a heating rate of 1°C / min and kept at this temperature for 5 hours. After the temperature dropped to room temperature, the Na 0.88 Co 0.55 Li 0.02 SO4 material

[0090] Will Na 0.88 Co 0.55 Li 0.02 SO4, KB, and PVDF were mixed in a mass ratio of 8:1:1 and coated onto aluminum foil using a 100 μm four-sided coating machine. The resulting electrode film was then dried in a vacuum oven at 100°C for 3 hours. A sheet puncher was used to punch the electrode film into discs with a radius of 0.6 mm. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0091] The above coin-type battery was subjected to constant current charge and discharge tests at a current density of 0.1 C (1 C = 100 mAh / g). Within the voltage range of 2.0 - 4.8 V, the reversible specific capacity was 90 mAh / g.

[0092] In the present invention, the structural general formula of the pure-phase polyanionic sulfate sodium-ion battery cathode material is Na x M y A z SO4, where the value range of x is 0.85 ≤ x ≤ 0.95, the value range of y is 0.52 ≤ y ≤ 0.58, A is an alkali metal group element such as Li, K, Na, etc., the value range of z is 0 < z ≤ 0.1, and x + 2y + z = 2. Its preparation method is to uniformly mix a sodium source, a metal source, an alkali metal source, an anion source (SO4 2- ) and a carbon source in a certain proportion, and sinter them in an inert atmosphere to obtain the corresponding material. This material has a relatively high redox potential (3.7 V vs Na / Na + ) and sodium storage capacity; due to the stable 3D open framework structure and large sodium-ion diffusion channels, this material exhibits excellent long-cycle stability and outstanding rate performance. Compared with other sodium-ion battery cathode materials, the elements Na, Fe, alkali metal elements, and SO4 contained in this material are rich in natural resources and have low mining costs, and Na x M y A z SO4 material has a simple preparation process and excellent performance, and is expected to become a commercial sodium-ion battery cathode material.

[0093] Comparative Example 1

[0094] This example relates to the synthesis and electrochemical performance of Na 0.92 Fe 0.50 K 0.08 SO4, specifically as follows:

[0095] Sodium sulfate, ferrous sulfate, and potassium sulfate were added to a ball milling jar according to a molar ratio of 0.46:0.50:0.04. The carbon source was KB. 20 mL of acetone was poured into the above ball milling jar (under N2 protection), the ball-to-material ratio was 20:1, the rotation speed was 400 r / min, and the total ball milling duration was 7 h, with an intermittent shutdown time of 10 min. Finally, the ball-milled precursor gel was placed in an Ar / H2 (90:10) atmosphere, heated at a heating rate of 1 °C / min, held at 100 °C for 3 h, then heated at a heating rate of 1 °C / min and held at 200 °C for 3 h, and then continuously heated at a heating rate of 1 °C / min to 350 °C and held at this temperature for 5 h. After the temperature dropped to room temperature, the Na 0.92 Fe 0.50 K 0.08 SO4 material was taken out. Figure 8 shows Na0.92 Fe 0.50 K 0.08 The XRD pattern of SO4 powder shows a significant increase in the 20-25° 2θ range, compared to the theoretical diffraction curve. This peak is consistent with the diffraction peaks of the Na6Fe(SO4)4 impurity phase, indicating an imbalance in the ratio of elements such as Na, Fe, and SO4. The presence of impurities reduces the proportion of active material, leading to a decrease in the material's specific capacity. Furthermore, the presence of impurities hinders ion diffusion at the material interface, increasing electrode polarization and reducing rate performance.

[0096] Will Na 0.92 Fe 0.50 K 0.08 SO4, AB, and PVDF were mixed into a homogenous slurry at a mass ratio of 7:2:1. The black slurry was coated onto aluminum foil using a 150 μm four-sided film preparation device and then dried in a vacuum oven at 100°C for 2 hours. The electrode film was punched into discs with a radius of 0.6 mm using a sheet puncher. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0097] The button cell was subjected to constant current charge and discharge tests at a current density of 0.1C (1C = 100 mAh / g). 0.92 Fe 0.50 K 0.08 The charge-discharge curve of the SO4 electrode in the first week shows that the reversible specific capacity is 92 mAh / g in the voltage range of 2.0-4.3 V, and the average discharge potential is 3.5 V. The capacity and potential are lower than those in Example 1, indicating that the presence of impurities has an adverse effect on the electrochemical performance of the material. 0.92 Fe 0.50 K 0.08 The SO4 electrode has a cycle stability of 500 cycles at 10C, and the capacity retention rate is only 85%, indicating that the presence of impurities reduces the stability of the material interface, resulting in severe cycle attenuation.

[0098] Comparative Example 2

[0099] This embodiment involves Na 0.74 Fe 0.59 Li 0.08 The synthesis of SO4 and its electrochemical properties are as follows:

[0100] Sodium sulfate, ferrous sulfate and lithium sulfate were added to the ball mill in a molar ratio of 0.37:0.59:0.04. The carbon source was KB. 20 mL of acetone was poured into the ball mill (N2 protection). The ball-to-material ratio was 20:1. The rotation speed was 400 r / min. The total ball milling time was 7 hours, with an interval downtime of 10 minutes. Finally, the ball-milled precursor gel was placed in an Ar / H2 (90:10) atmosphere at a heating rate of 1°C / min and kept at 100°C for 3 hours. Then, it was kept at 200°C for 3 hours at a heating rate of 1°C / min. Then, it was continued to be heated to 350°C at a heating rate of 1°C / min and kept at this temperature for 5 hours. After the temperature dropped to room temperature, the Na 0.74 Fe 0.59 Li 0.08 Figure 9 shows the Na 0.74 Fe 0.59 Li 0.08 The XRD pattern of SO4 powder shows a significant presence of impurity peaks in the 20-25° 2θ range compared to the theoretical diffraction curve. These peaks are consistent with the diffraction peaks of Na6Fe(SO4)4 and FeSO4 impurity phases, indicating an imbalance in the ratio of elements such as Na, Fe, and SO4. The presence of impurities reduces the proportion of active material, leading to a decrease in the material's specific capacity. Furthermore, the presence of impurities hinders ion diffusion at the material interface, increasing electrode polarization and reducing rate performance.

[0101] Will Na 0.74 Fe 0.59 Li 0.08 SO4, AB, and PVDF were mixed into a slurry at a mass ratio of 7:2:1. The black slurry was then coated onto aluminum foil using a 150 μm four-sided film preparation device. The film was then dried in a vacuum drying oven at 100°C for 2 hours. The electrode film was punched into discs with a radius of 0.6 mm using a sheet puncher. CR2016 button cells were assembled in a glove box using sodium metal as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%)+5% FEC as the electrolyte, and a PP / PE / PP three-layer separator.

[0102] The button cell was subjected to constant current charge and discharge tests at a current density of 0.1C (1C = 100 mAh / g). 0.74 Fe 0.59 Li 0.08 The charge-discharge curve of the SO4 electrode in the first week shows that in the voltage range of 2.0-4.3V, the reversible specific capacity is 80mAh / g and the average discharge potential is 3.45V. The capacity and potential are lower than those in Example 1, indicating that the presence of impurities has an adverse effect on the electrochemical performance of the material. 0.74 Fe 0.59 Li0.08 The SO4 electrode has a cycle stability of 500 cycles at 10C, and the capacity retention rate is only 78%, indicating that the presence of impurities reduces the stability of the material interface, resulting in severe cycle attenuation.

[0103] It should be explained and emphasized that, although only the case where M is Fe and A is Na is listed in the above embodiments, based on basically similar properties, M being Mn, Co, Ni, Cu and / or Zn and A being Li and / or K all have predictable performance and effects and also fall within the scope of the present invention.

[0104] The above embodiments are merely specific embodiments of the present invention, and their descriptions are relatively specific and detailed. However, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art would be able to make various modifications and improvements without departing from the scope of the present invention, and such obvious alternatives are all within the scope of protection of the present invention.

Claims

1. A pure phase polyanion sulfate sodium ion battery positive electrode material, characterized in that: The chemical formula of the pure phase polyanion sulfate sodium ion battery cathode material is Na x M y A z SO4; wherein M is one or more of Mn, Fe, Co, Ni, Cu and / or Zn; A is one or more of Li, K and / or Na; the value range of each variable is: 0.75≤x≤0.85, 0.52≤y≤0.58; 0 <z≤0.1、x+2y+z=2。 2. The pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 1, characterized in that: The pure phase polyanion sulfate sodium ion battery positive electrode material has a triclinic P21 / c space group.

3. The pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 2, characterized in that: In terms of site division, Na, S and O are located at the 4e site, and M and A are located at the 8f site; Na / S-O4 is a tetrahedron, and M / A-O6 is an octahedron, and the tetrahedron and octahedron are connected at the same point / face.

4. The pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 3, characterized in that: In the triclinic P21 / c space group, the lattice parameters vary within the range of:

5. A method for preparing a pure phase polyanionic sulfate sodium ion battery positive electrode material according to any one of claims 1 to 4, characterized in that The following steps are involved: The sodium source, metal source, alkali metal source, anion source and carbon source are uniformly mixed according to a stoichiometric ratio, and sintered in an inert atmosphere to obtain the corresponding pure phase polyanion sulfate sodium ion battery positive electrode material.

6. The method for preparing the pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 5, characterized in that: The sodium source is an inorganic sodium source and / or an organic sodium source, the inorganic sodium source is one or more of sodium hydroxide, sodium chloride, sodium sulfate, sodium nitrate and / or sodium carbonate, and the organic sodium source is one or more of sodium formate, sodium acetate, sodium ethoxide and / or sodium benzoate.

7. The method for preparing the pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 5, characterized in that: The metal source is a manganese source, an iron source, a cobalt source, a nickel source, a copper source and / or a zinc source; The manganese source is one or more of manganese sulfate, manganese carbonate, manganese chloride and / or manganese acetate; The iron source is one or more of ferrous sulfate, ferric chloride, ferrous oxide and / or ferric acetate; The cobalt source is one or more of cobalt sulfate, cobalt nitrate, cobalt chloride and / or cobalt acetate; The nickel source is one or more of nickel sulfate, nickel nitrate, nickel chloride and / or nickel acetate; The copper source is one or more of copper sulfate, copper chloride and / or copper acetate; The zinc source is one or more of zinc sulfate, zinc chloride and / or zinc acetate.

8. The method for preparing the pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 5, characterized in that: The alkali metal source is a sodium source, a lithium source and / or a potassium source; The sodium source is an inorganic sodium source and / or an organic sodium source, the inorganic sodium source is one or more of sodium hydroxide, sodium chloride, sodium sulfate, sodium nitrate and / or sodium carbonate, and the organic sodium source is one or more of sodium formate, sodium acetate, sodium ethoxide and / or sodium benzoate; The lithium source is one or more of lithium sulfate, lithium carbonate and / or lithium hydroxide; The potassium source is one or more of potassium sulfate, potassium hydroxide, potassium chloride, potassium nitrate and / or potassium carbonate.

9. The method for preparing the pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 5, characterized in that: The anion source is one or more of sulfuric acid, sodium sulfate, ferrous ammonium sulfate, ferrous sulfate and / or ammonium sulfate; The carbon source is one or more of SurpP, KB, carbon nanotubes, graphene, glucose, citric acid and / or sucrose.

10. The method for preparing the pure phase polyanionic sulfate sodium ion battery positive electrode material according to claim 5, characterized in that: The uniform mixing method is a liquid phase mixing method or a solid phase mixing method; the inert atmosphere is argon, nitrogen or a mixed gas of argon, hydrogen, nitrogen and hydrogen; and the sintering temperature is 200-400°C.

Citation Information

Patent Citations

  • Sodium ion positive electrode material and preparation method and application thereof

    CN114400309A

  • Preparation methods of monoclinic-phase FeSO4.H2O and triclinic-phase NaFe1-xMxSO4F (M=Co, Ni)

    CN103078111A

  • Sodium ferrous sulfate / graphene composite positive electrode material for sodium ion battery, and preparation method thereof

    CN106848236A

  • Battery positive electrode material as well as preparation method and application thereof

    CN111326715A

  • Preparation method of sodium ion battery positive electrode material

    CN115385380A

Cited By

  • Sodium ion positive electrode material, preparation method thereof and sodium ion battery

    CN118867211A

  • High-conductivity sodium ion battery positive electrode material / organic conductive polymer composite material and preparation method thereof

    CN119560511A