Nickel-coated graphite powder, additive, electroplating solution and electroplating process therefor

By using particle electroplating nano-nickel additives in the process of nickel-coated graphite powder, combined with electroless plating and electroplating, the problems of high temperature, high pressure and low coating rate in the nickel-coated graphite powder process are solved, and high coating rate, low resistance and resistance are achieved. Aged nickel-coated graphite powder, suitable as conductive filler.

WO2024212678A1PCT designated stage expired Publication Date: 2024-10-17YAAN BESTRY PERFORMANCE MATERIALS CORP +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/074747
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-01-30
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The existing nickel-coated graphite powder process has problems such as high temperature and high pressure reaction, low coating rate, high surface porosity and easy oxidation, resulting in high resistance.

Method used

Using particle electroplating nano-nickel additives, through a process that combines chemical plating and electroplating, nickel-coated graphite powder with high coverage rate and low resistance is formed. The additives include complexing agents, current dispersants and low-potential deposition accelerators to control nickel ions. The adsorption and generation of hydrogen inclusions form a uniform and dense nickel plating layer.

Benefits of technology

The nickel-coated graphite powder has the properties of high coating rate, low resistance, aging resistance and easy water washing. It is suitable as a conductive filler and improves the conductivity and dispersion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024074747_17102024_PF_FP_ABST
    Figure CN2024074747_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses nickel-coated graphite powder, an additive, an electroplating solution and an electroplating process therefor. The additive is a particulate matter electroplating nano-nickel additive, and comprises a complexing agent, a current dispersing agent, a low-potential deposition accelerator, and a lubricant, the mass ratio of the complexing agent to the current dispersing agent to the low-potential deposition accelerator is 40-100:10:1, and electroplating is carried out within the proportion, so that a large number of micro crystal nucleuses can be formed, but the growth of the micro crystal nucleuses is inhibited, and thus a fine-crystallized nano-nickel electroplated layer is obtained. The electroplating solution comprises the additive, the process parameters are stable during plating, and the plated nickel-coated graphite has the advantages of being easy to wash, low in surface resistance, resistant to aging and the like. According to the electroplating process, a layer of nickel is firstly plated on the surface of graphite by using chemical plating so as to completely cover the surfaces of particles, and then a layer of electroplating nickel is electroplated on chemical nickel to obtain the nickel-coated graphite powder; the nickel-coated graphite powder is better in surface conductivity, good in bonding force, good in dispersity, and uniform in plating, and has excellent performance when serving as a conductive filler.
Need to check novelty before this filing date? Find Prior Art

Description

Nickel-coated graphite powder, additive, electroplating solution and electroplating process thereof

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application with application number 202310396446.X filed with the Chinese Patent Office on April 14, 2023, entitled “A nickel-coated graphite powder, additive, electroplating solution and electroplating process thereof”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the field of electroplating technology, and in particular to nickel-coated graphite powder, additives, electroplating solution and electroplating process thereof. Background Art

[0004] Nickel-coated graphite powder is a composite powder material formed by chemically coating a core graphite powder with a layer of metallic nickel. This composite material combines the superior lubricity of graphite with the excellent electrical and thermal conductivity of metal. It is widely used in electromagnetic shielding, radar absorption, thermal spraying, and other fields.

[0005] Existing nickel-coated graphite powder is mostly produced by hydrogen compression reduction. The process is roughly as follows: degreasing - water washing - pretreatment - water washing - hydrogen compression reduction - water washing - drying. This process has the following main problems:

[0006] 1. The reaction needs to be carried out under high temperature and high pressure;

[0007] 2. The coverage rate is not high enough and the surface porosity is high;

[0008] 3. The coating density is not enough and it is easy to oxidize, resulting in high surface resistance.

[0009] Application Contents

[0010] Based on this, the present application provides a nickel-coated graphite powder, an additive, an electroplating solution and an electroplating process thereof. The additive is a nano-nickel additive for electroplating of particles, and has a complexing agent, a current dispersant, a low-potential deposition accelerator and a lubricant. The mass ratio of the complexing agent, the current dispersant and the low-potential deposition accelerator is 40 to 100:10:1. Electroplating within this ratio can form a large number of micro-crystal nuclei, but their growth is inhibited, thereby obtaining a finely crystalline nano-crystalline nickel electroplating layer. The electroplating solution contains the additive, and the process parameters are stable during the plating process. The nickel-coated graphite after plating has the advantages of easy water washing, low surface resistance and aging resistance. The electroplating process first utilizes chemical plating to plate a layer of nickel on the graphite surface, with a high particle surface coverage rate, and then electroplates a layer of finely crystalline electroplated nickel on the chemical nickel to obtain nickel-coated graphite powder. The surface conductivity of the nickel-coated graphite powder is better, and the bonding force is good, the dispersibility is good, the plating layer is uniform, and the nickel-coated graphite powder has excellent performance as a conductive filler.

[0011] The technical solution adopted in this application is:

[0012] A nickel-coated graphite powder with a D50 of 80 to 120 μm and a specific surface area of ​​0.1 to 0.2 m 2 / g, powder resistance is less than 0.012Ω·mm, and oxidation weight loss is less than 1.5%.

[0013] The nickel-coated graphite powder provided in the present application has a small specific surface area, a small powder resistance, and a very small oxidation weight loss, indicating that the surface of the graphite powder is completely covered with a nickel layer, and the nickel layer is very evenly coated, which can make the bonding force between the graphite powder and the nickel coating layer good, the nickel coating layer more uniform, and the nickel-coated graphite powder has good electrical conductivity and dispersibility, and has excellent performance as a conductive filler.

[0014] In the nickel-coated graphite powder disclosed in the present application, the coverage rate of the nickel layer is not less than 98%.

[0015] In the nickel-coated graphite powder disclosed in the present application, the coverage rate of the nickel layer is not less than 98%, and the thickness of the nickel layer is 1 μm to 6 μm.

[0016] In the nickel-coated graphite powder disclosed in the present application, the coverage rate of the nickel layer is not less than 98%, and the nickel-coated graphite powder meets the following requirements: when oxidized in air at 500° C. for 77 minutes, the oxidation weight gain is 1% to 1.5%.

[0017] An additive comprising:

[0018] Complexing agent, which is citric acid or salicylic acid;

[0019] The current dispersant is one or more of sodium salt of bisbenzenesulfonimide and sodium saccharin;

[0020] Low potential deposition accelerator, which is one or more of thiourea, ATPN, and UPS;

[0021] Wetting agent, which is one or more of 2-ethylhexyl sulfate sodium salt, dioctyl sodium sulfosuccinate, and sodium lauryl sulfate;

[0022] The mass ratio of the complexing agent, the current dispersant and the low-potential deposition accelerator is 40-100:10:1.

[0023] The additive provided in this application can be used as an additive for electroplating solution. When electroplating chemical nickel-coated graphite powder, since the nickel-coated graphite powder has a large specific surface area, low potential characteristics, and a very small cathode current, a current dispersant and a low-potential deposition accelerator are added to the additive, and a complexing agent is added to make nickel ions easily adsorbed on the surface of the chemical nickel-coated graphite powder so as to form a large number of micro-crystal nuclei on its surface. In addition, the wetting agent can prevent the hydrogen generated by electroplating from being mixed in the coating and precipitate the hydrogen, thereby making the coating more dense. Furthermore, the mass ratio of the complexing agent, the current dispersant, and the low-potential deposition accelerator is 40 to 100:10:1, which can make the dispersion of the chemical nickel-coated graphite powder more uniform, form a large number of micro-crystal nuclei during electroplating, but their growth is suppressed, thereby obtaining a nano-nickel electroplating layer with fine crystals and a uniform and dense electroplated nickel layer.

[0024] In the additive disclosed in the present application, the mass ratio of the complexing agent to the wetting agent is 5 to 50:1.

[0025] In the additive disclosed in the present application, the mass ratio of the complexing agent, the current dispersant, and the low-potential deposition accelerator is 60-100:10:1.

[0026] Based on the same inventive concept, the present application also provides an electroplating solution, including a main solution and the aforementioned additives.

[0027] The electroplating solution provided in the present application contains the above-mentioned additives, so that the performance of the nickel-coated graphite powder can be improved within a relatively wide range of the electroplating process during the electroplating process. The performance of the nickel-coated graphite powder under different electroplating process parameters is relatively consistent, the parameter requirements of the electroplating process are not high, and the stability of the nickel-coated graphite powder finally obtained is also better, which is conducive to industrial production.

[0028] In the electroplating solution disclosed in the present application, the concentration of the complexing agent in the electroplating solution is 1 g / L to 50 g / L.

[0029] In the electroplating solution disclosed in the present application, the concentration of the current spreader in the electroplating solution is 0.05 g / L to 5 g / L.

[0030] In the electroplating solution disclosed in the present application, the concentration of the low-potential deposition accelerator in the electroplating solution is 10 ppm to 2000 ppm.

[0031] In the electroplating solution disclosed in the present application, the concentration of the wetting agent in the electroplating solution is 0.1 to 1 g / L.

[0032] In the electroplating solution disclosed in the present application, the main solution includes 50-250 g / L of main salt, 20-60 g / L of buffer, and 2-20 g / L of anode activator.

[0033] In the electroplating solution disclosed in the present application, the main salt is one or more of nickel sulfamate and nickel sulfate.

[0034] In the electroplating solution disclosed in the present application, the buffer is one or more of boric acid, aminoacetic acid, and sodium acetate, which can play a pH buffering role and make the environment of the electroplating solution more stable.

[0035] In the electroplating solution disclosed herein, the anode activator is one or more of potassium chloride, nickel chloride, and sodium chloride. This activator promotes the dissolution of the anode nickel block, replenishing nickel ions in the electrolyte solution so that nickel ions can be electroplated onto the chemically nickel-plated graphite powder to form a uniform and dense nickel coating.

[0036] Based on the same inventive concept, the present application also provides an electroplating process using the aforementioned electroplating solution, comprising the following steps:

[0037] Step S1: chemical plating, mixing graphite particles with a chemical nickel plating solution, stirring and reacting for 30 to 90 minutes to obtain chemical nickel-plated graphite;

[0038] Step S2. Wash the chemical nickel-plated graphite with water until the conductivity is less than 20 μS / cm;

[0039] Step S3: electroplating, mixing the chemically nickel-plated graphite with an electroplating solution, using direct current for electroplating for 20 to 80 hours to obtain electroplated graphite;

[0040] Step S4: washing the electroplated graphite powder with water for the second time until the conductivity is less than 20 μS / cm, and drying the electroplated graphite powder to obtain the nickel-coated graphite powder.

[0041] In the electroplating process provided by the present application, chemical nickel plating can be first achieved by immersion, so that a thin nickel layer can be formed on the surface of the graphite powder and in the nanopores inside. The nickel layer has a high coverage rate, which improves the conductivity of the particles. Then, on this basis, the nickel layer is electroplated to avoid leaking plating. By combining with the components of the electroplating solution, the electroplated nickel layer can be made more uniform and dense, and the nickel can basically completely fill the nanopores of the graphite powder and form a nano-scale electroplated nickel layer. The final nickel-coated graphite powder can have a smaller specific surface area, a smaller powder resistance, and better performance.

[0042] In the electroplating process disclosed in the present application, in step S1, the chemical nickel plating solution includes: 150-300 g / L nickel sulfate, 150-300 g / L sodium hypophosphite, 50-150 mL / L ammonia water, and 10-60 g / L ammonium chloride.

[0043] In the electroplating process disclosed in the present application, in step S1, the reaction temperature is 50-90° C., and the pH is 9-11.

[0044] In the electroplating process disclosed in the present application, the particle loading amount for chemical plating is 10 to 40 g / L, and the particle loading amount for electroplating is 50 to 100 m2 / L.

[0045] In the electroplating process disclosed in the present application, in step S3, the electroplating temperature is 30-60° C., the pH is 2.5-5.5, and the current is 0.1-5 A / m².

[0046] The beneficial effects of the invention are:

[0047] (1) The additive of the present application is a nano-nickel additive for electroplating of particulate matter, which contains a complexing agent, a current dispersant, a low-potential deposition accelerator and a lubricant. Each component plays a different role and is consumed in different amounts during the electroplating process. The present application found that when the mass ratio of the complexing agent, the current dispersant and the low-potential deposition accelerator is 40 to 100:10:1, the graphite powder has good dispersibility and no agglomeration phenomenon. A large number of micro-crystal nuclei can be formed during electroplating, but their growth is inhibited, thereby obtaining a nano-nickel electroplating layer with fine crystals.

[0048] (2) The electroplating solution of the present application has a particulate electroplating nano-nickel additive and is a nano-electroplating solution. The process parameters are stable during the plating process, and the nickel-coated graphite after plating has the advantages of being easy to wash with water, having low surface resistance after drying, and being resistant to aging.

[0049] (3) The electroplating process steps of the present application are chemical plating-water washing-electroplating-water washing-drying. First, a layer of nickel is plated on the surface of the graphite particles by chemical plating to completely cover the surface of the particles, further improving the conductivity, facilitating subsequent electroplating, and preventing leakage plating. Then, a layer of electroplated nickel with fine crystallization is electroplated on the chemical nickel to make the plating uniform, with good bonding force, low porosity, good dispersibility, good aging resistance, low surface resistance, better conductivity, and excellent performance as a conductive filler. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0051] FIG1 is a microscopic image (×500) of nickel-coated graphite powder provided in Example 1 of the present application;

[0052] FIG2 is a microscopic image (×3000) of nickel-coated graphite powder provided in Example 1 of the present application;

[0053] Figure 3 is a microscopic image (ⅹ285) of the nickel-coated graphite powder provided in Comparative Example 1. DETAILED DESCRIPTION

[0054] In the following, only certain exemplary embodiments are briefly described. As those skilled in the art would realize, the described embodiments may be modified in various different ways without departing from the spirit or scope of the present application.

[0055] References to "embodiments" in this application mean that a particular feature, structure, or characteristic described in connection with the embodiment may be included in at least one embodiment of the application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0056] The embodiments of the present application are described in detail below.

[0057] The present application provides an additive, comprising:

[0058] Complexing agent, which is citric acid or salicylic acid;

[0059] The current dispersant is one or more of sodium salt of bisbenzenesulfonimide and sodium saccharin;

[0060] Low potential deposition accelerator, which is one or more of thiourea, ATPN (S-carboxyethylisothiourea nitrate), and UPS (sodium 3-S-isothiourea propanesulfonate);

[0061] Wetting agent, which is one or more of 2-ethylhexyl sulfate sodium salt, dioctyl sodium sulfosuccinate, and sodium lauryl sulfate;

[0062] The mass ratio of the complexing agent, the current dispersant and the low-potential deposition accelerator is 40-100:10:1.

[0063] The additive provided in the present application can be used as an additive for electroplating solution. When electroplating chemical nickel-coated graphite powder, since the nickel-coated graphite powder has a large specific surface area, low potential characteristics, and a very small cathode current, a current dispersant and a low-potential deposition promoter are added to the additive, and a complexing agent is added to make nickel ions easily adsorbed on the surface of the chemical nickel-coated graphite powder so as to form a large number of micro-crystal nuclei on its surface. In addition, the wetting agent can prevent the hydrogen generated by electroplating from being mixed in the coating, and precipitate the hydrogen, thereby making the coating denser.

[0064] The additive of the present application is a nano-nickel additive for particulate electroplating, which contains a complexing agent, a current dispersant, a low-potential deposition accelerator and a lubricant. Each component plays a different role and is consumed in different amounts during the electroplating process. The present application found that when the mass ratio of the complexing agent, the current dispersant and the low-potential deposition accelerator is 40 to 100:10:1, the graphite micropowder has good dispersibility and no agglomeration phenomenon. A large number of micro-crystal nuclei can be formed during electroplating, but their growth is inhibited, thereby obtaining a nano-nickel electroplating layer with fine crystals.

[0065] During the electroplating process, metal ions are transferred to the cathode to form adsorbed atoms, ultimately forming microcrystalline nuclei. The key steps in the electrodeposition process are the growth of microcrystalline nuclei and the growth of crystals, both of which directly affect the grain state of the resulting coating. The use of this additive gives the nano-nickel additive for particulate electroplating a high cathode overpotential, a high total number of adsorbed atoms, and a low atomic adsorption surface mobility, which are necessary conditions for the formation of a large number of microcrystalline nuclei and the inhibition of their growth. Because the growth of the crystal nuclei is suppressed, a nanocrystalline nickel electroplating layer is obtained.

[0066] As an example, the mass ratio of the complexing agent, the current dispersant, and the low potential deposition accelerator is 40:10:1, 50:10:1, 60:10:1, 70:10:1, 80:10:1, 90:10:1, or 100:10:1. Alternatively, the mass ratio of the complexing agent, the current dispersant, and the low potential deposition accelerator is 60 to 100:10:1.

[0067] In the additive disclosed in the present application, the mass ratio of the complexing agent to the wetting agent is 5 to 50:1. As an example, the mass ratio of the complexing agent to the wetting agent is 5:1, 10:1, 20:1, 30:1, 40:1 or 50:1. The present application also provides an electroplating solution comprising a main solution and the aforementioned particulate electroplating nano-nickel additive.

[0068] The electroplating solution provided in the present application contains the above-mentioned additives, so that the performance of the nickel-coated graphite powder can be improved within a relatively wide range of the electroplating process during the electroplating process. The performance of the nickel-coated graphite powder under different electroplating process parameters is relatively consistent, the parameter requirements of the electroplating process are not high, and the stability of the nickel-coated graphite powder finally obtained is also better, which is conducive to industrial production.

[0069] The electroplating solution of the present application has a particulate electroplating nano-nickel additive and is a nano-electroplating solution. The process parameters are stable during the plating process. The nickel-coated graphite after plating has the advantages of being easy to wash with water, having low surface resistance after drying, and being resistant to aging.

[0070] The main solution includes 50-250g / L of main salt, 20-60g / L of buffer, and 2-20g / L of anode activator. The concentrations of the main salt, buffer, and anode activator in the main solution are calculated based on the aqueous solvent in the electroplating solution. For example, 1L of the aqueous solvent contains 50-250g of main salt, 20-60g of buffer, and 2-20g of anode activator. The inclusion of the anode activator facilitates the dissolution of the anode.

[0071] The main salt is one or more of nickel sulfamate and nickel sulfate; the buffer is one or more of boric acid, aminoacetic acid and sodium acetate; and the anode activator is one or more of potassium chloride, nickel chloride and sodium chloride.

[0072] In the electroplating solution disclosed in the present application, the concentration of the complexing agent in the electroplating solution is 1 g / L to 50 g / L;

[0073] In the electroplating solution disclosed in the present application, the concentration of the current dispersant in the electroplating solution is 0.05 g / L to 5 g / L;

[0074] In the electroplating solution disclosed in the present application, the concentration of the low potential deposition accelerator in the electroplating solution is 10 ppm to 2000 ppm;

[0075] In the electroplating solution disclosed in the present application, the concentration of the wetting agent in the electroplating solution is 0.1 to 1 g / L. Based on the above electroplating solution, the present application also provides an electroplating process, comprising the following steps:

[0076] Step S1: chemical plating, mixing graphite particles with a chemical nickel plating solution, stirring and reacting for 30 to 90 minutes to obtain chemical nickel-plated graphite;

[0077] Step S2. Wash the chemical nickel-plated graphite with water until the conductivity is less than 20 μS / cm;

[0078] Step S3: electroplating, mixing the chemically nickel-plated graphite with an electroplating solution, using direct current for electroplating for 20 to 80 hours to obtain electroplated graphite;

[0079] Step S4: washing the electroplated graphite powder with water for the second time until the conductivity is less than 20 μS / cm, and drying the electroplated graphite powder to obtain nickel-coated graphite powder.

[0080] The electroplating process steps of the present application are chemical plating-water washing-electroplating-water washing-drying. First, a layer of nickel is plated on the surface of the graphite particles by chemical plating to completely cover the surface of the particles, further improving the conductivity, facilitating subsequent electroplating, and preventing leaking plating; then a layer of electroplated nickel with fine crystallization is electroplated on the chemical nickel to make the plating uniform, with good bonding strength, low porosity, good dispersibility, good aging resistance, low surface resistance, better conductivity, and excellent performance as a conductive filler.

[0081] Specifically, in step S1, the chemical nickel plating solution includes: 150-300 g / L of nickel sulfate, 150-300 g / L of sodium hypophosphite, 50-150 mL / L of ammonia water, and 10-60 g / L of ammonium chloride.

[0082] Specifically, in step S1, the reaction temperature is 50-90° C., and the pH is 9-11.

[0083] Specifically, the particle loading capacity for chemical plating is 10-40 g / L, and the particle loading capacity for electroplating is 50-100 m2 / L. The particle loading capacity for electroplating refers to the following: first calculate the specific surface area of ​​the powder, then multiply the specific surface area by the loading capacity of 50-100 m2 to calculate the mass of the particles, and then load them.

[0084] Specifically, in step S3, the electroplating temperature is 30-60° C., the pH is 2.5-5.5, and the current is 0.1-5 A / m².

[0085] Through the above electroplating process, in combination with the electroplating solution containing the above additives, nickel-coated graphite powder can be obtained. The nickel-coated graphite powder satisfies the following requirements: D50 is 80-120 μm, and the specific surface area is 0.1-0.2 m 2 / g, powder resistance is less than 0.012Ω·mm, and oxidation weight loss is less than 1.5%.

[0086] Because immersion chemical plating is performed before electroplating, a thin nickel layer can be evenly formed on the surface and in the internal pores of the graphite powder, so that in the subsequent electroplating process, the nickel can basically completely fill the micropores of the graphite powder, thereby making the nickel-coated graphite powder have a low porosity and a small specific surface area. In addition, by continuing to electroplating after chemical plating and coordinating with additives in the electroplating solution, the nickel plating layer can be thickened (because of the nickel coating, the D50 of the nickel-coated graphite powder is greater than the D50 of the raw graphite powder), so that the resistance of the powder is small and the conductive performance of the nickel-coated graphite powder is better. In addition, the nickel layer is dense and uniform, has good aging resistance, lower resistivity, and good bonding between the electroplated layer and the chemically plated layer, so that the nickel-coated graphite powder has excellent performance.

[0087] In the nickel-coated graphite powder disclosed in this application, the nickel layer has a coverage rate of not less than 98%. Since the chemical plating is an immersion method, the coating can basically completely cover the graphite. Electroplating on this basis can not only thicken the coating, but also make the coating uniform and dense.

[0088] In the nickel-coated graphite powder disclosed in this application, the nickel layer has a coverage rate of not less than 98%, and a nickel layer thickness of 1 μm to 6 μm. By combining chemical plating and electroplating, the nickel coating can be made within this range, with a thicker thickness and better conductivity.

[0089] The nickel-coated graphite powder disclosed in this application has a nickel coating coverage of no less than 98%. The nickel-coated graphite powder meets the following requirements: oxidation weight gain of 1% to 1.5% when oxidized in air at 500°C for 77 minutes. Because the nickel coating is uniform and dense, only the surface nickel reacts with oxygen to form nickel oxide during the oxidation process. This minimizes the nickel oxidation weight gain, typically between 1% and 1.5%.

[0090] Example 1

[0091] Prepare chemical nickel plating solution according to the formula: 200 g / L nickel sulfate, 200 g / L sodium hypophosphite, 100 ml / L ammonia water, and 30 g / L ammonium chloride.

[0092] Graphite particles (D50 = 100 μm) were reacted with a chemical nickel plating solution at 60°C, pH 10, and a loading of 25 g / L with stirring for 60 minutes to plate a layer of nickel on the surface of the graphite particles to obtain chemical nickel-plated graphite. The graphite was then washed with water to reduce the electrical conductivity to less than 20 μS / cm.

[0093] The plating solution was prepared according to the following formula: 150 g / L nickel sulfamate, 10 g / L nickel chloride, 30 g / L boric acid; nano-nickel additives for particulate electroplating: 0.5 g / L sodium 2-ethylhexyl sulfate, 0.2 g / L citric acid, 0.02 g / L sodium saccharin, 2 ppm ATPN (the mass ratio of the complexing agent, current dispersant, and low-potential deposition accelerator is 100:10:1).

[0094] The chemical nickel-plated graphite and the electroplating solution are placed at a temperature of 45°C, pH 3, a current of 2A / m2, a loading amount of 70m2 / L, and direct current for electroplating for 40 hours. A layer of finely crystalline electroplated nickel is then electroplated on the chemical nickel. The powder is then washed with water until the conductivity is less than 20μS / cm and dried to obtain nickel-coated graphite powder.

[0095] Please refer to Figures 1 and 2. The surface of nickel-coated graphite powder is finely crystallized and the coating is uniform. The D50 of nickel-coated graphite powder is measured to be 112μm, and the specific surface area is 0.1273m 2 / g, the powder resistance is less than 0.012Ω·mm (specifically 0.0085Ω·mm); after the nickel-coated graphite powder is oxidized in air at 500°C for 77 minutes, the oxidation weight gain is 1.45%.

[0096] Example 2

[0097] Prepare chemical nickel plating solution according to the formula: 150g / L nickel sulfate, 150g / L sodium hypophosphite, 50ml / L ammonia water, and 10g / L ammonium chloride.

[0098] Graphite particles (D50 = 100 μm) were reacted with a chemical nickel plating solution at 50°C, pH 9, and a loading of 10 g / L, with stirring for 30 minutes to plate a layer of nickel on the surface of the graphite particles to obtain chemical nickel-plated graphite. The graphite was then washed with water to reduce the electrical conductivity to less than 20 μS / cm.

[0099] The plating solution was prepared according to the following formula: 50 g / L nickel sulfamate, 2 g / L nickel chloride, 20 g / L boric acid; nano-nickel additives for particulate electroplating: 0.1 g / L dioctyl sodium sulfosuccinate, 0.2 g / L salicylic acid, 0.02 g / L sodium salt of bisbenzenesulfonyl imide, 2 ppm UPS (the mass ratio of complexing agent, current dispersant, and low-potential deposition accelerator is 100:10:1).

[0100] The chemical nickel-plated graphite and the electroplating solution are placed at a temperature of 30°C, pH 2.5, a current of 5A / m2, a loading amount of 50m2 / L, and direct current for electroplating for 20 hours. A layer of finely crystalline electroplated nickel is then electroplated on the chemical nickel, and then washed with water until the conductivity is less than 20μS / cm, and dried to obtain nickel-coated graphite powder.

[0101] The D50 of nickel-coated graphite powder was determined to be 110 μm, and the specific surface area was 0.1417 m 2 / g, the powder resistance is less than 0.012Ω·mm (specifically 0.0083Ω·mm); after the nickel-coated graphite powder is oxidized in air at 500°C for 77 minutes, the oxidation weight gain is 1.43%.

[0102] Example 3

[0103] Prepare chemical nickel plating solution according to the formula: 300 g / L nickel sulfate, 300 g / L sodium hypophosphite, 150 ml / L ammonia water, and 60 g / L ammonium chloride.

[0104] Graphite particles (D50 = 100 μm) were reacted with a chemical nickel plating solution at 90°C, pH 11, and a loading of 40 g / L with stirring for 90 minutes to plate a layer of nickel on the surface of the graphite particles to obtain chemical nickel-plated graphite. The graphite was then washed with water to reduce the electrical conductivity to less than 20 μS / cm.

[0105] The plating solution was prepared according to the following formula: 250 g / L nickel sulfamate, 20 g / L nickel chloride, 60 g / L boric acid; nano-nickel additives for particulate electroplating: 1 g / L sodium 2-ethylhexyl sulfate, 0.2 g / L citric acid, 0.02 g / L sodium saccharin, 2 ppm ATPN (the mass ratio of the complexing agent, current dispersant, and low-potential deposition accelerator is 100:10:1).

[0106] The chemical nickel-plated graphite and the electroplating solution are placed at a temperature of 60°C, pH 5.5, a current of 0.1A / m2, a loading amount of 100 m2 / L, and direct current for electroplating for 80 hours. A layer of finely crystalline electroplated nickel is then electroplated on the chemical nickel, and then washed with water until the conductivity is less than 20μS / cm, and dried to obtain nickel-coated graphite powder.

[0107] The D50 of nickel-coated graphite powder was determined to be 108 μm, and the specific surface area was 0.1346 m 2 / g, the powder resistance is less than 0.012Ω·mm (specifically 0.0081Ω·mm); after the nickel-coated graphite powder is oxidized in air at 500°C for 77 minutes, the oxidation weight gain is 1.41%.

[0108] Example 4

[0109] The mass ratio of the complexing agent, the current dispersant, and the low-potential deposition accelerator in the additive for electroplating nano-nickel on particles was changed to 80:10:1, and the rest was the same as in Example 1.

[0110] The D50 of nickel-coated graphite powder was determined to be 106 μm, and the specific surface area was 0.18 m 2 / g, the powder resistance is less than 0.012Ω·mm (specifically 0.0095Ω·mm); after the nickel-coated graphite powder is oxidized in air at 500°C for 77 minutes, the oxidation weight gain is 1.6%.

[0111] Example 5

[0112] The mass ratio of the complexing agent, the current dispersant, and the low-potential deposition accelerator in the additive for electroplating nano-nickel on particles was changed to 60:10:1, and the rest was the same as in Example 1.

[0113] The D50 of nickel-coated graphite powder was determined to be 112 μm, with a specific surface area of ​​0.17 m 2 / g, the powder resistance is less than 0.012Ω·mm (specifically 0.009Ω·mm); after the nickel-coated graphite powder is oxidized in air at 500°C for 77 minutes, the oxidation weight gain is 1.5%.

[0114] Example 6

[0115] The mass ratio of the complexing agent, the current dispersant, and the low-potential deposition accelerator in the additive for electroplating nano-nickel on particles was changed to 40:10:1, and the rest was the same as in Example 1.

[0116] The D50 of nickel-coated graphite powder was determined to be 108 μm, and the specific surface area was 0.2 m 2 / g, the powder resistance is less than 0.012Ω·mm (specifically 0.0094Ω·mm); after the nickel-coated graphite powder is oxidized in air at 500°C for 77 minutes, the oxidation weight gain is 1.6%.

[0117] Example 7

[0118] The mass ratio of the complexing agent, current dispersant, and low-potential deposition accelerator in the nano-nickel electroplating additive for particles was changed to 20:10:1, and the rest was the same as in Example 1.

[0119] The D50 of nickel-coated graphite powder was determined to be 109 μm, and the specific surface area was 0.19 m 2 / g, the powder resistance is less than 0.012Ω·mm (specifically 0.0092Ω·mm); after the nickel-coated graphite powder is oxidized in air at 500°C for 77 minutes, the oxidation weight loss is 1.7%.

[0120] Comparative Example 1

[0121] Oerlikon's Efill-2701 nickel-coated graphite powder has a D50 of 112 μm and a specific surface area of ​​0.444 m 2 / g, the powder resistance is 0.0289Ω·mm; after the nickel-coated graphite powder is oxidized in air at 500℃ for 77min, the oxidation weight gain is 2.83%.

[0122] Experimental Example 1

[0123] The parameters of the nickel-coated graphite powder provided in Examples 1 to 7 of the present application and Comparative Example 1 are shown in Table 1.

[0124] Table 1 Parameters of nickel-coated graphite powder

[0125] Figure 3 is a microscopic image (ⅹ285) of the nickel-coated graphite powder provided in Comparative Example 1. By comparing Figure 1 and Figure 3, it can be seen that the nickel-coated graphite powder provided in Comparative Example 1 has many small black spots (Figure 3), indicating that the nickel coating in the nickel-coated graphite powder obtained by the method provided in Comparative Example 1 is uneven, and the carbon at the small black spots is not coated with nickel.

[0126] In combination with the contents in Table 1, it can be seen that the specific surface area of ​​the nickel-coated graphite powder in Comparative Example 1 is greater than the specific surface area of ​​the nickel-coated graphite powder provided in Example 1. In combination with Figures 1 and 3, it can be seen that the nickel-coated graphite powder obtained by the method provided in the comparative example has a poor coating effect, resulting in it still having a large porosity, thereby making its specific surface area higher; while the nickel-coated graphite powder obtained by the method provided in Example 1 has a good coating effect, the pores of the graphite are filled, and the coating layer is uniform and dense, which can reduce the porosity and have a lower specific surface area.

[0127] In combination with the contents in Table 1, it can be seen that the powder resistance of the nickel-coated graphite powder in Comparative Example 1 is greater than the powder resistance of the nickel-coated graphite powder provided in Example 1, which can indicate that the nickel-coated layer of the nickel-coated graphite powder provided in this application is uniform, has good density, and has better conductive properties.

[0128] The oxidation weight gain of the nickel-coated graphite powder in Comparative Example 1 is greater than the oxidation weight gain of the nickel-coated graphite powder provided in Example 1. Combined with Figures 1 and 3, it can be seen that the nickel-coated graphite powder obtained by the method provided in the comparative example has a poor coating effect, which causes the nickel to be easily oxidized, thereby causing it to gain more oxidation weight; while the nickel-coated graphite powder obtained by the method provided in Example 1 has a good coating effect, a uniform and dense nickel layer, the internal nickel is not easily oxidized, only the surface layer is oxidized, and the oxidation weight gain is low.

[0129] Experimental Example 2

[0130] The dispersibility and agglomeration of the nickel-coated graphite powder provided in Examples 1 to 7 of the present application and Comparative Example 1 are shown in Table 2.

[0131] Table 2 Effect of nickel-coated graphite powder

[0132] It can be seen from Table 2 that the nickel-coated graphite powder provided in the present application has a better dispersion effect, while the nickel-coated graphite powder provided in the comparative example has a poor dispersion effect.

[0133] When the ratio of complexing agent, current dispersant and low potential deposition accelerator is 40-100:10:1, the dispersion is good and there is no agglomeration.

[0134] The nickel-coated graphite powder provided in Example 1 and Comparative Example 1 was mixed with a two-component silica gel at a mass ratio of 1:1 to prepare conductive silica gels with varying filling levels. The resistivity, aging performance (surface resistance of the conductive silica gel was measured after four weeks of treatment at 85% humidity and 85°C), and shielding performance of the resulting conductive silica gels with varying filling levels of the nickel-coated graphite powder provided in Example 1 and Comparative Example 1 are compared in Table 3.

[0135] Table 3 Effect of nickel-coated graphite powder

[0136] As can be seen from Table 3, compared with Comparative Example 1, the nickel-coated graphite powder provided in the present application has better conductivity, the conductive silica gel obtained also has better conductivity, and has better aging performance and shielding performance, and better comprehensive performance.

[0137] The above are merely preferred embodiments of the present application and are not intended to limit the present application. Persons skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of protection of the present application.

Claims

1. A nickel-coated graphite powder, characterized in that: The nickel-coated graphite powder has a D50 of 80 to 120 μm and a specific surface area of ​​0.1 to 0.2 m 2 / g, powder resistance is less than 0.012Ω·mm, and oxidation weight loss is less than 1.5%.

2. The nickel-coated graphite powder according to claim 1, characterized in that The nickel-coated graphite powder meets one or more of the following conditions: a) The coverage of the nickel layer is not less than 98%; b) the coverage rate of the nickel layer is not less than 98%, and the thickness of the nickel layer is 1 μm to 6 μm; c) The coverage rate of the nickel layer is not less than 98%, and the nickel-coated graphite powder meets the following conditions: when oxidized in air at 500° C. for 77 minutes, the oxidation weight gain is 1% to 1.5%.

3. An additive, characterized in that: include: Complexing agent, which is citric acid or salicylic acid; The current dispersant is one or more of sodium salt of bisbenzenesulfonimide and sodium saccharin; Low potential deposition accelerator, which is one or more of thiourea, ATPN, and UPS; Wetting agent, which is one or more of 2-ethylhexyl sulfate sodium salt, dioctyl sodium sulfosuccinate, and sodium dodecyl sulfate; Wherein, the mass ratio of the complexing agent, the current dispersing agent and the low potential deposition accelerator is 40-100:10:

1.

4. The additive according to claim 3, characterized in that The additive meets one or more of the following conditions: d) the mass ratio of the complexing agent to the wetting agent is 5 to 50:1; e) The mass ratio of the complexing agent, the current dispersing agent and the low potential deposition accelerator is 60 to 100:10:

1.

5. An electroplating solution, characterized in that: It comprises a main solution and the additive according to claim 3 or 4.

6. The electroplating solution according to claim 5, characterized in that The electroplating solution satisfies one or more of the following conditions: f) the concentration of the complexing agent in the electroplating solution is 1 g / L to 50 g / L; g) the concentration of the current dispersant in the electroplating solution is 0.05 g / L to 5 g / L; h) the concentration of the low potential deposition accelerator in the electroplating solution is 10 ppm to 2000 ppm; i) The concentration of the wetting agent in the electroplating solution is 0.1-1 g / L.

7. The electroplating solution according to claim 6, characterized in that The main solution comprises 50-250 g / L of main salt, 20-60 g / L of buffer, and 2-20 g / L of anode activator.

8. The electroplating solution according to claim 7, characterized in that The main solution meets one or more of the following conditions: j) the main salt is one or more of nickel sulfamate and nickel sulfate; k) the buffer is one or more of boric acid, aminoacetic acid, and sodium acetate; 1) The anode activator is one or more of potassium chloride, nickel chloride and sodium chloride.

9. An electroplating process using the electroplating solution according to any one of claims 5 to 8, characterized in that: The following steps are involved: Step S1. Chemical plating, mixing graphite particles with chemical nickel plating solution, stirring and reacting for 30 to 90 minutes to obtain chemical nickel-plated graphite; Step S2. Wash the chemical nickel-plated graphite with water until the conductivity is less than 20 μS / cm; Step S3. electroplating, mixing the chemical nickel-plated graphite with the electroplating solution according to any one of claims 5 to 8, using direct current for electroplating for 20 to 80 hours to obtain electroplated graphite; Step S4. Wash the electroplated graphite powder with water for the second time until the conductivity is less than 20 μS / cm, and dry it to obtain the nickel-coated graphite powder as claimed in claim 1 or 2.

10. The electroplating process according to claim 9, characterized in that: The electroplating process meets one or more of the following conditions: m) In step S1, the chemical nickel plating solution includes: 150-300 g / L nickel sulfate, 150-300 g / L sodium hypophosphite, 50-150 mL / L ammonia water, and 10-60 g / L ammonium chloride; n) In step S1, the reaction temperature is 50-90° C. and the pH is 9-11; o) The particle loading amount of the chemical plating is 10-40 g / L, and the particle loading amount of the electroplating is 50-100 m2 / L; p) In step S3, the electroplating temperature is 30-60° C., the pH is 2.5-5.5, and the current is 0.1-5 A / m2.

Citation Information

Patent Citations

  • Nickel plating solution

    CN111118554A

  • Nickel plating liquid additive, nickel plating liquid and electroplating process

    CN111778530A

  • Nickel-coated graphite powder and application thereof in electromagnetic shielding material

    CN115488332A

  • Preparation method of nickel-coated graphite powder

    CN115519133A

  • Nickel-coated graphite powder, additive, electroplating solution and electroplating process thereof