Negative electrode material, negative electrode for nonaqueous electrolyte batteries, and nonaqueous electrolyte secondary battery
The use of an aluminum alloy with specific elements in non-aqueous electrolyte secondary batteries improves cycle characteristics by forming a non-aluminum phase that enhances structural support, addressing the degradation issues in existing negative electrodes and maintaining high efficiency and capacity retention.
Patent Information
- Application Number
- PCT/JP2024/013778
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-17
AI Technical Summary
Non-aqueous electrolyte secondary batteries, particularly lithium-ion batteries, face challenges in maintaining high cycle characteristics due to degradation of negative electrodes during repeated charging and discharging, leading to reduced efficiency and capacity retention.
A negative electrode material composed of an aluminum alloy with specific elements like Si, Ge, Mn, B, Ti, V, Cr, Fe, Co, Ni, Sr, Y, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, La, Ce, and Nd, which form a non-aluminum phase and substitute for aluminum atoms, enhancing structural support and stability, thereby improving cycle performance.
The proposed negative electrode material significantly enhances cycle characteristics by maintaining high discharge capacity retention and initial charge/discharge efficiency, outperforming conventional aluminum alloys by suppressing damage and maintaining structural integrity during repeated cycles.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000027_0000
Abstract
Description
Negative electrode materials, negative electrodes for nonaqueous electrolyte batteries, and nonaqueous electrolyte secondary batteries
[0001] The present invention relates to a negative electrode material, a negative electrode for a non-aqueous electrolyte battery, and a non-aqueous electrolyte secondary battery. This application claims priority to Japanese Patent Application No. 2023-063675, filed April 10, 2023, the contents of which are incorporated herein by reference.
[0002] Known rechargeable secondary batteries include those that use a nonaqueous electrolyte as the electrolyte (hereinafter referred to as nonaqueous electrolyte secondary batteries) and those that use a solid electrolyte (all-solid-state secondary batteries). Of these, nonaqueous electrolyte secondary batteries have already been put to practical use not only in small power sources for mobile phones and notebook computers, but also in medium- and large-sized power sources for automobiles and power storage.
[0003] Regarding non-aqueous electrolyte secondary batteries, studies are being conducted on electrodes and active materials contained in the electrodes in order to improve their performance. For example, regarding lithium secondary batteries, which are a type of non-aqueous electrolyte secondary battery, studies are being conducted on improving battery performance by using a material with a larger theoretical capacity for the negative electrode constituting the lithium secondary battery than graphite, which is a conventional negative electrode material. As such a material, attention is being paid to, for example, metal materials that can absorb and release lithium ions, similar to graphite.
[0004] As an example of a negative electrode formed from a metal material, for example, Non-Patent Document 1 describes the use of an aluminum alloy in which iron (Fe) is added to aluminum (Al) as a negative electrode material for a lithium ion secondary battery.
[0005] "Application of aluminum to negative electrodes for Li-ion batteries and elucidation of the charge / discharge mechanism," Abstracts of the 141st Autumn Meeting of the Japan Institute of Light Metals, Japan Society of Mineral Resources and Materials Science, pp. 169-170
[0006] As the application fields of non-aqueous electrolyte secondary batteries expand, further improvements in the cycle characteristics of non-aqueous electrolyte secondary batteries are required. In the negative electrode described in Non-Patent Document 1, the charge / discharge efficiency, which was initially about 80%, decreased to less than 60% after 10 charge / discharge cycles, leaving room for improvement in the cycle characteristics.
[0007] Furthermore, negative electrode materials with improved cycle characteristics are required not only for lithium ion secondary batteries but also for other non-aqueous electrolyte secondary batteries.
[0008] The "cycle characteristics" are evaluated by the rate at which discharge capacity is maintained when charging and discharging are repeated. A nonaqueous electrolyte secondary battery that has a high rate at which discharge capacity is maintained when charging and discharging are repeated is evaluated as having "good cycle characteristics."
[0009] The present invention has been made in view of the above circumstances, and has an object to provide a negative electrode material for a nonaqueous electrolyte secondary battery that can improve the cycle characteristics of the nonaqueous electrolyte secondary battery. Another object is to provide a negative electrode for a nonaqueous electrolyte battery that uses such a negative electrode material, and a nonaqueous electrolyte secondary battery that uses the same.
[0010] In order to solve the above problems, one aspect of the present invention includes the following aspects.
[0011] [1] A negative electrode material made of an aluminum alloy, the negative electrode material comprising aluminum, an element M1 having a solid solubility limit in aluminum of 1.5 mass % or more, and an element M2 having a solid solubility limit in aluminum of less than 1.5 mass %, wherein the element M1 is one or more elements selected from the group consisting of Si, Ge, and Mn, and the element M2 is one or more elements selected from the group consisting of B, Ti, V, Cr, Fe, Co, Ni, Sr, Y, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, La, Ce, Pr, and Nd, the aluminum purity of the remainder, when the elements M1 and M2 are removed from the entire negative electrode material, is 99 mass % or more, the element M1 is present by substituting aluminum atoms in aluminum metal crystals in the negative electrode material, and the element M2 forms a non-aluminum phase having a length of 10 nm to 10 μm in a cross-sectional image obtained under the following conditions: (Conditions) The negative electrode material before charge / discharge is rolled to a thickness of 50 μm, and the resulting rolled material is cut perpendicular to the rolling direction. An element mapping image of the resulting cut surface is created by SEM-EDX, and this is used as the cross-sectional image.
[0012] [2] The negative electrode material according to [1], wherein the total content of the element M1 and the element M2 relative to the entire negative electrode material is 0.5 mass % or more and 8 mass % or less.
[0013] [3] The negative electrode material according to [1] or [2], having a Vickers hardness of 10 HV or more and 70 HV or less.
[0014] [4] The negative electrode material according to any one of [1] to [3], which is obtained by heating a negative electrode material precursor, which is a rolled material made of aluminum, the element M1, and the element M2, at 100°C or more and 350°C or less, and which has an aluminum content of 99 mass% or more in the remainder obtained by excluding the element M1 and the element M2 from the entire rolled material.
[0015] [5] A negative electrode for a non-aqueous electrolyte battery, comprising the negative electrode material according to any one of [1] to [4].
[0016] [6] A non-aqueous electrolyte secondary battery having the negative electrode for a non-aqueous electrolyte battery according to [5].
[0017] According to the present invention, it is possible to provide a negative electrode material for a nonaqueous electrolyte secondary battery that can improve the cycle characteristics of the nonaqueous electrolyte secondary battery, and also to provide a negative electrode for a nonaqueous electrolyte battery using such a negative electrode material, and a nonaqueous electrolyte secondary battery using the same.
[0018] Fig. 1 is a cross-sectional view of an aluminum negative electrode of a lithium ion secondary battery. Fig. 2 is a cross-sectional view of an aluminum negative electrode of a lithium ion secondary battery. Fig. 3 is a schematic view showing an example of a non-aqueous electrolyte secondary battery.
[0019] <<Negative Electrode Material, Negative Electrode for Non-Aqueous Electrolyte Battery>> The negative electrode material of this embodiment is a negative electrode material made of an aluminum alloy. The negative electrode for a non-aqueous electrolyte battery of this embodiment is made of the negative electrode material described below.
[0020] The negative electrode material has the following characteristics. Requirement (1): It consists of aluminum, element M1 having a solid solubility limit in aluminum of 1.5 mass% or more, and element M2 having a solid solubility limit in aluminum of less than 1.5 mass%. Requirement (2): The aluminum purity of the remainder, excluding elements M1 and M2 from the entire negative electrode material, is 99 mass% or more. Requirement (3): Element M1 exists by substituting aluminum atoms in the aluminum metal crystal in the negative electrode material. Requirement (4): Element M2 forms a non-aluminum phase having a length of 10 nm to 10 μm in a cross-sectional image of the negative electrode material obtained under the following conditions: (Conditions) The negative electrode material before charge / discharge is rolled to a thickness of 50 μm, and the obtained rolled material is cut perpendicular to the rolling direction. An element mapping image of the obtained cut surface is created by SEM-EDX to obtain a cross-sectional image.
[0021] [Requirement (1)] The negative electrode material contains aluminum, an element M1, and an element M2.
[0022] The aluminum used as the material for the negative electrode material may have a purity of 99.9% by mass or more, high-purity aluminum with a purity of 99.99% by mass or more, etc. High-purity aluminum can be produced by appropriately employing a known method for increasing the purity of aluminum, such as a segregation method, a three-layer electrolysis method, a zone melting refining method, or an ultra-high vacuum melting method.
[0023] Aluminum may contain impurities that are inevitably contained (unavoidable impurities). Examples of inevitable impurities include manufacturing residues that are inevitably mixed in during the refining process. Specific examples include iron and copper. The copper content of the high-purity aluminum is preferably 300 ppm by mass or less, more preferably 100 ppm by mass or less, and even more preferably 50 ppm by mass or less, relative to the total mass of the high-purity aluminum. Furthermore, the copper content of the high-purity aluminum may be 0 ppm by mass, relative to the total mass of the high-purity aluminum.
[0024] The elements M1 and M2 differ in their solid solubility limits (solubility limit concentration, mass %) in aluminum. Specifically, the element M1 has a solid solubility limit in aluminum of 1.5 mass % or more, while the element M2 has a solid solubility limit in aluminum of less than 1.5 mass %.
[0025] The element M1 is at least one element selected from the group consisting of Si, Ge, and Mn. As the element M1, either one or both of Si and Mn are preferred, and Si is more preferred.
[0026] The element M2 is at least one selected from the group consisting of B, Ti, V, Cr, Fe, Co, Ni, Sr, Y, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, La, Ce, Pr, and Nd. The element M2 is preferably at least one selected from the group consisting of B, Ti, V, Cr, Fe, Co, Ni, Sr, Y, Zr, Sn, and Ce, more preferably at least one selected from the group consisting of Cr, Fe, Ni, Ce, and Co, and even more preferably at least one selected from the group consisting of Cr, Fe, Ni, Ce, and Co.
[0027] As a specific combination, for example, when Si is used as the element M1, the element M2 can be one selected from the group consisting of Cr, Fe, Ni, Ce, and Co. Also, when Mn is used as the element M1, Cr can be used as the element M2.
[0028] Whether an element A corresponds to element M1 or element M2 can be determined using the literature value of the solid solubility limit of element A in aluminum.
[0029] Furthermore, after preparing an aluminum alloy by adding 1.5 mass % of element A to aluminum, if the resulting aluminum alloy satisfies the following (i) and (ii), or (i) and (iii), it can be determined that element A is dissolved in aluminum. That is, the solid solubility limit of element A in aluminum can be determined to be 1.5 mass % or more, and element A can be determined to correspond to element M1. (i) The presence of element M1 can be confirmed by the above-mentioned ICP analysis. (ii) In the diffraction pattern of the negative electrode material measured by X-ray diffraction (XRD), no peaks attributable to element M1 alone or a compound containing element M1 can be confirmed. (iii) The lattice constant of aluminum determined from the diffraction pattern of the negative electrode material measured by X-ray diffraction (XRD) is shifted.
[0030] [Requirement (2)] The aluminum purity (aluminum content) of the remainder, excluding the elements M1 and M2, from the entire negative electrode material is 99% by mass or more. That is, the aluminum purity of the remainder, excluding the intentionally added elements M1 and M2, of the negative electrode material is 99% by mass or more. This aluminum purity is preferably 99.9% by mass or more.
[0031] The composition of the negative electrode material is measured using, for example, a solid-state optical emission spectrometer (eg, ARL-4460 manufactured by Thermo) or an ICP (inductively coupled plasma) optical emission spectrometer (eg, SPS5000 manufactured by Seiko Instruments Inc.).
[0032] The aluminum purity can be determined by determining the composition of the entire negative electrode material using the above-mentioned device, determining the aluminum content (mol %) of the remainder obtained by subtracting elements corresponding to elements M1 and M2 from the obtained composition, and converting the aluminum content (mol %) into mass %.
[0033] [Requirement (3)] The element M1 forms a substitutional solid solution with aluminum in the negative electrode material, and exists by substituting aluminum atoms in the aluminum metal crystals.
[0034] Whether the element M1 substitutes for an aluminum atom in an aluminum metal crystal can be easily evaluated by confirming that the conditions (i) and (ii) or (i) and (iii) described in the above [Requirement (1)] are satisfied.
[0035] [Requirement (4)] In a cross-sectional image obtained under the above conditions, element M2 forms a non-aluminum phase having a length of 10 nm or more and 10 μm or less. The size (length) of the non-aluminum phase is preferably 100 nm or more, and more preferably 500 nm or more. The size of the non-aluminum phase is preferably 5 μm or less, and more preferably 4 μm or less.
[0036] The upper and lower limits of the size of the non-aluminum phases can be arbitrarily combined. The size of the non-aluminum phases may be 100 nm or more and 5 μm or less, 500 nm or more and 5 μm or less, or 500 nm or more and 4 μm or less.
[0037] The method for measuring the size of the non-aluminum phase will be described in detail below.
[0038] (Method for measuring the size of non-aluminum phase) First, the negative electrode material before charge / discharge is rolled to a thickness of 50 μm, and the obtained rolled material is cut perpendicular to the rolling direction. In detail, first, the rolled material is cut using a diamond cutter. Thereafter, the cross section is further processed using a focused ion beam processing machine to prepare a cross section. <Processing conditions> Argon ion milling device: IB-19520CCP (manufactured by JEOL Ltd.) Acceleration voltage: 6 kV Atmosphere: Air Temperature: -100°C
[0039] Scanning electron microscope images (SEM and SEM-EDX images) of the obtained cross section are obtained using the following scanning electron microscope (equipped with an energy dispersive X-ray analyzer) under the following conditions: <Measurement conditions> Scanning electron microscope: JSM-5500 (manufactured by JEOL Ltd.) Energy dispersive X-ray fluorescence analyzer: X-MaxN (manufactured by OXFORD INSTRUMENTS) Acceleration voltage: 10 kV (for SEM observation), 10 kV (for SEM-EDX) Magnification: 1,000 to 10,000 times
[0040] The elemental mapping image to be created is the cross-sectional image. From the elemental mapping image, it can be confirmed that the element M2 is contained in the non-aluminum phase.
[0041] Next, for the non-aluminum phase contained in the cross-sectional image, the smallest rectangle circumscribing the non-aluminum phase is assumed, and the length of the long side of the rectangle is measured.
[0042] When the number of non-aluminum phases contained in the cross-sectional image is 20 or more at a magnification of 1000 times, the length of all non-aluminum phases is measured according to the above definition, and the arithmetic mean value of the lengths obtained is determined as the "size (length) of the non-aluminum phase." When the length of the non-aluminum phase is small and difficult to measure, the magnification is increased to determine the length.
[0043] If the number of non-aluminum phases contained in the cross-sectional image is less than 20, cross-sectional images of different fields are created, and similar measurements are performed on non-aluminum phases whose total number contained in the multiple cross-sectional images is 20 or more, to determine the "size of the non-aluminum phases."
[0044] The size of the non-aluminum phase can be controlled by the cooling rate during aluminum casting, as described below. As the cooling rate during aluminum casting increases, the size of the non-aluminum phase tends to decrease.
[0045] The inventors considered that the elements M1 and M2 finely dispersed in the structure as in requirements (3) and (4) function like a filler to support the structure of the negative electrode material, and suppress damage to the negative electrode during repeated charge and discharge. It is known that when conventional aluminum or aluminum alloy negative electrodes are used in negative electrodes of non-aqueous electrolyte secondary batteries, repeated charge and discharge gradually disintegrates the surface that transfers ions, causing the negative electrode to be damaged.
[0046] In contrast, in the negative electrode made of the negative electrode material of this embodiment, it is believed that element M1, which penetrates into the aluminum metal crystals, and element M2, which is present as a larger mass than element M1 and precipitates between the metal crystals, work together to support the metal crystals. As a result, in the negative electrode made of the negative electrode material of this embodiment, damage to the negative electrode due to charge and discharge can be suppressed.
[0047] In particular, when the negative electrode material is produced by annealing (heat treating) a rolled aluminum alloy material, the following effects can be expected.
[0048] 1 and 2 are cross-sectional views of aluminum anodes of conventional lithium-ion secondary batteries, and enlarged photographs showing the anodes after charging. Fig. 1 shows the appearance of anode 50A made of an annealed anode material, and Fig. 2 shows the appearance of anode 50B made of an unannealed anode material.
[0049] 1 and 2 are manufactured from a conventional negative electrode material in which 1 mass % of Si is added as element M1 to high-purity aluminum having a purity of 99.99 mass % or more, and no element M2 is added. In the lithium-ion secondary battery, surface 50 a of negative electrodes 50A and 50B faces the positive electrode, and lithium ions are inserted and removed from surface 50 a.
[0050] The enlarged photographs in Figures 1 and 2 were taken in the following manner: A coin-type battery fabricated by the method described later in "(Method for measuring initial efficiency and discharge capacity retention rate), (1) Fabrication of lithium secondary battery" was subjected to five cycles of charge and discharge, with one cycle consisting of charging and discharging.
[0051] Next, the discharged coin-type battery was disassembled in an argon glove box with an inert atmosphere, and the removed negative electrode was washed with anhydrous dimethyl carbonate. The obtained negative electrode was dried and then cut parallel to the thickness direction with a cutter blade, and the cut surface was further processed with a focused ion beam. The obtained cross section was observed with an SEM. The conditions for the focused ion beam processing and SEM observation were the same as those described above (Method for measuring the size of the non-aluminum phase).
[0052] 1, in the negative electrode 50A, a Li—Al alloy layer 51 grows from the surface 50a in the thickness direction of the negative electrode 50A (the normal direction to the surface 50a). Reference numeral 50x denotes a portion of the negative electrode 50A where the Li—Al alloy layer 51 is not formed and where the original composition of the negative electrode 50A remains. In the Li—Al alloy layer 51, Li is inserted (forming a Li—Al alloy) in the black portion (reference numeral A).
[0053] 1, in the negative electrode 50A after the annealing treatment, Li penetrates in the thickness direction of the negative electrode 50A, and the region indicated by the symbol A forms a striped pattern in the thickness direction of the negative electrode 50A. That is, in the negative electrode 50A, the structure is subdivided in the width direction of the negative electrode 50A (the same direction as the surface 50a).
[0054] In contrast, as shown in Figure 2, in the negative electrode 50B that has not been annealed, the portion (symbol A) in which Li is inserted in the Li-Al alloy layer 51 is formed in the width direction of the negative electrode 50B (the same direction as the surface 50a).
[0055] Due to these differences, the negative electrode 50A is easy to insert and remove Li, and therefore tends to have a higher initial charge-discharge efficiency than the negative electrode 50B. On the other hand, the structure of the negative electrode 50A, which is subdivided in the width direction, tends to collapse with repeated charge and discharge, and the cycle characteristics tend to be lower than those of the negative electrode 50B.
[0056] If the above-mentioned element M2 is further added to the negative electrode (negative electrode material) after such annealing treatment to form the negative electrode material of this embodiment, a non-aluminum phase of element M2 is formed in the negative electrode (the above-mentioned requirement (4)). The non-aluminum phase is thought to function to connect the finely divided structures in the width direction of the negative electrode, and is expected to improve cycle characteristics.
[0057] On the other hand, it is believed that the annealed negative electrode material of this embodiment maintains the effect that Li penetrates in the thickness direction of the negative electrode and Li is easily inserted and removed.
[0058] As a result, the negative electrode material of this embodiment that has been annealed can easily achieve both improved cycle characteristics and high initial charge / discharge efficiency.
[0059] The negative electrode material after the annealing treatment described above can be produced, for example, by using a rolled material composed of aluminum, element M1, and element M2 as a negative electrode material precursor. The negative electrode material precursor (rolled material) has an aluminum content of 99 mass% or more in the remainder, excluding elements M1 and M2, from the entire rolled material.
[0060] The annealed negative electrode material is obtained by heating the above-mentioned rolled material at 100° C. or more and 550° C. or less. The method for producing the annealed negative electrode material includes a step of heating the above-mentioned rolled material at 100° C. or more and 350° C. or less. The temperature of the annealing treatment (annealing temperature) may be 150° C. or more and 350° C. or less, or may be 200° C. or more and 350° C. or less.
[0061] The cycle characteristics are evaluated by measuring the retention rate of discharge capacity by the following method.
[0062] (Method of Measuring Initial Efficiency and Discharge Capacity Retention Rate) (1) Manufacture of Lithium Secondary Battery First, an aluminum negative electrode having a thickness of 50 μm is cut into a disk shape having a diameter of 16 mm as a measurement object.
[0063] Next, LiCoO 2 The resultant was molded into a disk shape with a diameter of 14 mm to serve as a counter electrode (positive electrode).
[0064] Next, LiBF was added to a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of EC:DMC=50:50. 4 The above is dissolved in a proportion of 1.0 mol / L to prepare an electrolyte solution.
[0065] A polyethylene porous separator was placed between the aluminum negative electrode and the counter electrode, and the resultant was housed in a battery case (standard 2032). The above electrolyte solution was poured into the battery case, and the battery case was sealed to produce a coin-type (full cell) lithium secondary battery with a diameter of 20 mm and a thickness of 3.2 mm.
[0066] (2) Measurement of initial efficiency For the manufactured lithium secondary battery, the current setting value for both charging and discharging was set at a test temperature of 25°C, with a positive electrode area of 0.6 mA / cm 2 (0.2 CA), charge and discharge are performed with a maximum charge voltage of 4.2 V and a minimum discharge voltage of 3.0 V. The discharge capacity is measured, and the charge capacity is measured, and the obtained value is taken as the "initial charge capacity" (mAh). The discharge capacity is further measured, and the obtained value is taken as the "initial discharge capacity" (mAh), i.e., the discharge capacity at the first cycle.
[0067] The initial efficiency is calculated using the initial discharge capacity value and the initial charge capacity value according to the following formula: Initial efficiency (%) = Initial discharge capacity (mAh) ÷ Initial charge capacity (mAh) × 100
[0068] (3) Measurement of Discharge Capacity Retention Rate After the initial charge / discharge, charge and discharge are repeated under the same conditions as the initial charge / discharge, with each charge and discharge being counted as one cycle. The discharge capacity is measured at each cycle, and the discharge capacity retention rate is calculated as a ratio to the initial discharge capacity.
[0069] The discharge capacity retention rate is evaluated by determining the maximum number of cycles at which the initial discharge capacity is 80% or more. The larger the "maximum number of cycles" determined, the better the cycle characteristics are judged to be.
[0070] (Composition) In the negative electrode material, the total content of the element M1 and the element M2 relative to the entire negative electrode material is preferably 0.5 mass% or more and 8 mass% or less, more preferably 0.5 mass% or more and 5 mass% or less, and even more preferably 0.5 mass% or more and 3 mass% or less.
[0071] In addition, in the negative electrode material, the content of element M1 relative to the entire negative electrode material is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.5 mass% or more. Furthermore, the content of element M1 is preferably 5 mass% or less, more preferably 2 mass% or less, and even more preferably 1 mass% or less. The upper and lower limits of the content of element M1 can be combined arbitrarily.
[0072] Furthermore, in the negative electrode material, the content of element M2 relative to the entire negative electrode material is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, and even more preferably 0.5 mass% or more. Furthermore, the content of element M2 is preferably less than 8 mass%, more preferably 5 mass% or less, and even more preferably 3 mass% or less, because rolling processing is easy. The upper and lower limits of the content of element M2 can be combined arbitrarily.
[0073] (Vickers Hardness) The Vickers hardness of the negative electrode material is preferably 10 HV or more and 70 HV or less, more preferably 20 HV or more and 70 HV or less, and even more preferably 30 HV or more and 70 HV or less.
[0074] The Vickers hardness is measured by the following method using a micro Vickers hardness tester (HV0.05).
[0075] (Method for Measuring Vickers Hardness) The Vickers hardness is a value measured in accordance with JIS Z2244:2009 "Vickers Hardness Test - Test Method." To measure the Vickers hardness, a square pyramidal diamond indenter is pressed into the surface of a test piece of a negative electrode material, and after the test force is released, the Vickers hardness is calculated from the diagonal length of the indentation remaining on the surface.
[0076] The above standard stipulates that the hardness symbol be changed depending on the test force. In this embodiment, the micro Vickers hardness HV0.05 is measured when the test force is 0.05 kgf (=0.4903 N).
[0077] It is presumed that when the Vickers hardness is equal to or less than the upper limit, distortion of the crystalline structure can be alleviated when aluminum absorbs lithium, and the crystalline structure can be maintained. Therefore, a negative electrode for a non-aqueous electrolyte battery manufactured from the negative electrode material can easily maintain its discharge capacity even when used in, for example, a lithium secondary battery and is repeatedly charged and discharged.
[0078] [Method for Producing Negative Electrode Material] The above-mentioned production method preferably includes a casting step and a rolling step of the alloy.
[0079] (Casting Process) When casting is performed, for example, predetermined amounts of elements M1 and M2 are added to high purity aluminum, and the aluminum is melted at a temperature of about 680° C. to 800° C. to obtain a molten alloy of aluminum and metal.
[0080] The molten alloy is preferably subjected to a cleaning treatment (e.g., vacuum treatment of molten aluminum) to remove gases and non-metallic inclusions. The vacuum treatment is performed, for example, at a temperature of 700°C to 800°C for 1 hour to 10 hours at a vacuum level of 0.1 Pa to 100 Pa.
[0081] The molten alloy can be purified by blowing in flux, inert gas, or chlorine gas. The molten alloy purified by vacuum treatment or the like is usually cast into a mold to obtain an ingot.
[0082] The mold is made of iron or graphite heated to 50° C. or higher and 200° C. or lower. The negative electrode material of this embodiment can be cast by pouring a molten alloy at 680° C. or higher and 800° C. or lower into the mold. Alternatively, an ingot can be obtained by commonly used semi-continuous casting.
[0083] (Rolling process) In the rolling process of the ingot, for example, hot rolling (first rolling) and cold rolling (secondary rolling) are performed to process the ingot into a plate material (rolled material). Hot rolling is performed, for example, at a temperature of 350°C to 550°C and at a rolling rate of 2% to 30% per rolling, repeatedly until the ingot reaches a target thickness.
[0084] After hot rolling, intermediate annealing is usually performed before cold rolling. In the intermediate annealing, for example, the hot-rolled sheet material may be heated to 350°C or higher and 550°C or lower and cooled immediately after the temperature rise, or may be held for 1 hour to 5 hours and then cooled. If the cooling step is performed by rapid cooling, the non-aluminum phase tends to become smaller. On the other hand, if the cooling is performed at a slow cooling rate, the metal particles constituting the non-aluminum phase tend to grow. The cooling step may be adjusted appropriately depending on the desired size of the non-aluminum phase. The cooling treatment softens the material, resulting in a state suitable for cold rolling.
[0085] Cold rolling is performed repeatedly at a temperature below the recrystallization temperature of aluminum, with a reduction ratio per rolling of 1% to 20%, until the aluminum ingot reaches a target thickness. The cold rolling temperature may be from room temperature to 80°C.
[0086] After cold rolling, the rolled material may be subjected to the above-mentioned annealing treatment in which the rolled material is heated at 100°C or higher and 350°C or lower. The heat treatment after cold rolling is usually performed in air, but may also be performed in a nitrogen atmosphere or a vacuum atmosphere. The heat treatment can soften work-hardened sheet material and may also adjust various physical properties by controlling the crystal structure.
[0087] In this embodiment, it is preferable to perform heat treatment after cold rolling. By performing heat treatment, a non-aluminum phase can be grown. By adjusting the heat treatment temperature and time, physical properties such as strength and electrical conductivity can be adjusted to desired ranges.
[0088] The negative electrode material and the negative electrode for a non-aqueous electrolyte battery having the above-described configuration can improve the cycle characteristics of a non-aqueous electrolyte secondary battery.
[0089] 《Nonaqueous electrolyte secondary battery》
[0090] 3 is a schematic diagram showing an example of a nonaqueous electrolyte secondary battery. The lithium secondary battery (nonaqueous electrolyte secondary battery) 10 has a positive electrode 2, an aluminum negative electrode (negative electrode) 3, and a nonaqueous electrolyte (electrolyte) 6.
[0091] The cylindrical lithium secondary battery 10 is manufactured as follows: First, as shown in Fig. 3 , a pair of strip-shaped separators 1, a strip-shaped positive electrode 2 having a positive electrode lead 21 at one end, and a strip-shaped negative electrode 3 having a negative electrode lead 31 at one end are stacked in this order: separator 1, positive electrode 2, separator 1, negative electrode 3, and then wound to form an electrode group 4.
[0092] Next, the electrode group 4 and an insulator (not shown) are housed in the battery can 5, the bottom of the can is sealed, the electrode group 4 is impregnated with an electrolyte solution 6, and the electrolyte is disposed between the positive electrode 2 and the negative electrode 3. Furthermore, the top of the battery can 5 is sealed with a top insulator 7 and a sealing member 8, whereby a lithium secondary battery 10 can be manufactured.
[0093] The shape of the electrode group 4 can be, for example, a columnar shape such that the cross-sectional shape when the electrode group 4 is cut perpendicular to the winding axis is a circle, an ellipse, a rectangle, or a rectangle with rounded corners.
[0094] The shape of a lithium secondary battery having such an electrode group 4 can be any shape specified in IEC 60086, which is a standard for batteries established by the International Electrotechnical Commission (IEC), or JIS C 8500. Examples of shapes include a cylindrical shape and a rectangular shape.
[0095] Furthermore, the lithium secondary battery is not limited to the above-mentioned wound type configuration, and may be a stacked type configuration in which a stacked structure of a positive electrode, a separator, a negative electrode, and a separator is repeatedly stacked. Examples of stacked lithium secondary batteries include so-called coin type batteries, button type batteries, and paper type (or sheet type) batteries.
[0096] The separator 1, the positive electrode 2, and the negative electrode lead 31 can be made of materials known for use in lithium secondary batteries.
[0097] The aluminum negative electrode of the present embodiment described above can be used for the negative electrode 3. That is, the negative electrode 3 has a negative electrode body made of aluminum, and in the lithiation reaction measured under the measurement conditions described above, has a lithiation capacity of 1 mAh / cm 2 The resistance value is 6.5 kΩ cm 2 An aluminum anode can be employed that is:
[0098] The negative electrode 3 may be an aluminum negative electrode having a negative electrode body made of aluminum and a coating formed on the surface of the negative electrode body, the coating being made of any one material selected from the group consisting of gold, carbon, and alumina hydrate.
[0099] The electrolyte 6 is a non-aqueous electrolyte. Examples of organic solvents contained in the electrolytic solution include carbonates such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 4-trifluoromethyl-1,3-dioxolan-2-one, and 1,2-di(methoxycarbonyloxy)ethane; ethers such as 1,2-dimethoxyethane, 1,3-dimethoxypropane, pentafluoropropyl methyl ether, 2,2,3,3-tetrafluoropropyl difluoromethyl ether, tetrahydrofuran, and 2-methyltetrahydrofuran; esters such as methyl formate, methyl acetate, propyl propionate, and γ-butyrolactone; nitriles such as acetonitrile and butyronitrile; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; carbamates such as 3-methyl-2-oxazolidone; sulfolane, dimethyl sulfoxide, and 1,3-propane sultone; The above organic solvents may further contain fluoro groups (organic solvents in which one or more hydrogen atoms have been substituted with fluorine atoms).
[0100] As the organic solvent, it is preferable to use a mixture of two or more of these. Among them, a mixed solvent containing a carbonate is preferable, and a mixed solvent of a cyclic carbonate and an acyclic carbonate and a mixed solvent of a cyclic carbonate and an ether are more preferable. As a mixed solvent of a cyclic carbonate and an acyclic carbonate, a mixed solvent containing ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate is preferable. An electrolyte solution using such a mixed solvent has many advantages, such as a wide operating temperature range, resistance to deterioration even when charged and discharged at a high current rate, and resistance to deterioration even when used for a long time.
[0101] The electrolyte contained in the electrolytic solution is LiClO 4 , LiPF 6 , LiAsF 6 , LiSbF 6 , LiBF 4 , LiCF 3 SO 3 , LiN(SO2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) (COCF 3 ), Li(C 4 F 9 SO 3 ), LiC(SO 2 CF 3 ) 3 , Li 2 B 10 Cl 10 , LiBOB (wherein BOB is bis(oxalato)borate), LiFSI (wherein FSI is bis(fluorosulfonyl)imide), lithium salts of lower aliphatic carboxylic acids, LiAlCl 4 The electrolyte may be a fluorine-containing lithium salt such as LiPF 6 , LiAsF 6 , LiSbF 6 , LiBF 4 , LiCF 3 SO 3 , LiN(SO 2 CF 3 ) 2 and LiC(SO 2 CF 3 ) 3 It is preferable to use a material containing at least one selected from the group consisting of:
[0102] Furthermore, the inventors have investigated LiBF 4 In addition to the lithium ion conductivity as an electrolyte, 6 It has been found that the electrolyte solution has the effect of suppressing the formation of the above-mentioned film X compared to other electrolytes such as LiBF. 4 When the electrolyte contains LiBF 4 From BF 3 For example, when ethylene carbonate (EC) is used as the solvent for the electrolyte, BF 3It is believed that this protects the unshared electron pair of EC and suppresses decomposition of the electrolyte.
[0103] According to the lithium secondary battery 10 described above, the cycle characteristics can be improved.
[0104] While the preferred embodiments of the present invention have been described above with reference to the accompanying drawings, the present invention is not limited to these examples. The shapes and combinations of the components shown in the above examples are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention.
[0105] In addition, as another aspect, the present invention includes the following embodiment.
[0106] <1> A negative electrode material made of an aluminum alloy, the negative electrode material comprising aluminum, an element M1 having a solid solubility limit in aluminum of 1.5% by mass or more, and an element M2 having a solid solubility limit in aluminum of less than 1.5% by mass, the element M1 being at least one element selected from the group consisting of Si, Ge, and Mn, and the element M2 being at least one element selected from the group consisting of B, Ti, V, Cr, Fe, Co, Ni, Sr, Y, Zr, Nb, Mo, Sn, Hf, Ta, W, P The negative electrode material is one or more elements selected from the group consisting of b, La, Ce, Pr, and Nd, and the aluminum purity of the remainder, excluding the elements M1 and M2 from the entire negative electrode material, is 99 mass% or more, the element M1 is present by substituting aluminum atoms in aluminum metal crystals in the negative electrode material, and the element M2 forms a non-aluminum phase having a length of 500 nm to 5 μm in a cross-sectional image obtained under the following conditions: (Conditions) The negative electrode material before charge / discharge is rolled to a thickness of 50 μm, and the obtained rolled material is cut perpendicular to the rolling direction. An element mapping image of the obtained cut surface is created by SEM-EDX, and this is used as the cross-sectional image.
[0107] <2> The negative electrode material according to <1>, wherein the total content of the element M1 and the element M2 relative to the entire negative electrode material is 0.5 mass % or more and 3 mass % or less.
[0108] <3> The negative electrode material according to <1> or <2>, having a Vickers hardness of 30 HV or more and 70 HV or less.
[0109] <4> A negative electrode for a non-aqueous electrolyte battery, comprising the negative electrode material according to any one of <1> to <3>.
[0110] <5> A nonaqueous electrolyte secondary battery having the negative electrode for a nonaqueous electrolyte battery according to <4>.
[0111] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0112] In this example, the following measurements were carried out as appropriate.
[0113] (Measurement of Size of Non-Aluminum Phase) The size of the non-aluminum phase was measured by the method described above in (Method for measuring size of non-aluminum phase).
[0114] (Initial Efficiency and Discharge Capacity Retention Rate) The initial efficiency and discharge capacity retention rate were measured according to the above-mentioned (Method for measuring initial efficiency and discharge capacity retention rate).
[0115] (Vickers Hardness) The Vickers hardness was measured according to the above-mentioned (Method for measuring Vickers hardness).
[0116] <Evaluation 1: Example 1> [Fabrication of Negative Electrode] High-purity aluminum (purity: 99.99% by mass or more), high-purity chemically produced silicon (purity: 99.999% by mass or more), and iron (purity: 99.9% by mass) were heated to and maintained at 760°C to obtain a molten aluminum-silicon-iron alloy with a silicon content of 0.5% by mass and an iron content of 1% by mass (M1+M2=1.5% by mass).
[0117] Next, the molten alloy was purified by being held at a temperature of 740°C for 2 hours under a vacuum of 50 Pa. The molten alloy was cast into a cast iron mold (22 mm x 150 mm x 200 mm) dried at 150°C to obtain an ingot.
[0118] The rolling was carried out under the following conditions: Both sides of the ingot were machined by 2 mm, and then cold-rolled from a thickness of 18 mm at a processing rate of 99.6%. The thickness of the obtained rolled material was 50 μm.
[0119] The rolled material was heat treated at 350° C. for 3 hours to obtain the negative electrode material of Example 1. The size of the non-aluminum phase in the obtained negative electrode material was 2.8 μm.
[0120] The obtained negative electrode material was cut into a disk shape with a diameter of 16 mm to obtain the negative electrode of Example 1.
[0121] [Preparation of Positive Electrode] 90 parts by mass of lithium cobalt oxide (product name: Cellseed, manufactured by Nippon Chemical Industry Co., Ltd.; average particle size (D50): 10 μm) as a positive electrode active material, 5 parts by mass of polyvinylidene fluoride (manufactured by Kureha Corporation) as a binder, and 5 parts by mass of acetylene black (product name: Denka Black, manufactured by Denka Company, Ltd.) as a conductive material were mixed, and 70 parts by mass of N-methyl-2-pyrrolidone was further mixed to prepare an electrode mixture for the positive electrode.
[0122] The obtained electrode mixture was applied to a 15 μm thick aluminum foil current collector by a doctor blade method. The applied electrode mixture was dried at 60°C for 2 hours and then further vacuum dried at 150°C for 10 hours to volatilize N-methyl-2-pyrrolidone. The coating amount of the positive electrode active material after drying was 21.5 mg / cm. 2 It was.
[0123] The obtained laminate of the electrode mixture layer and the current collector was rolled and then cut into a disk shape with a diameter of 14 mm, thereby producing a positive electrode, which was a laminate of a positive electrode mixture layer containing lithium cobalt oxide as a forming material and a current collector.
[0124] [Preparation of Electrolyte Solution] LiBF was added to a mixed solvent obtained by mixing ethylene carbonate (EC) and dimethyl carbonate (DMC) at a volume ratio of EC:DMC=50:50. 4 The above was dissolved in a proportion of 1 mol / L to prepare an electrolyte solution.
[0125] [Production of Lithium Secondary Battery] A polyethylene porous separator was placed between the negative electrode and the positive electrode, and the resulting battery was housed in a battery case (standard 2032). The above electrolyte solution was poured into the battery case, and the battery case was sealed to produce a coin-shaped lithium secondary battery (lithium secondary battery including the negative electrode of Example 1) having a diameter of 20 mm and a thickness of 3.2 mm.
[0126] Example 2 An anode material and an anode of Example 2 having a silicon content of 0.5 mass% and a nickel content of 1 mass% (M1 + M2 = 1.5 mass%) were obtained in the same manner as in Example 1, except that nickel (purity 99.9%) was used instead of iron. A lithium secondary battery was fabricated using the anode of Example 2. The size of the non-aluminum phase in the obtained anode material was 2.2 μm.
[0127] Example 3 An anode material and an anode of Example 3 having a silicon content of 0.5 mass% and a cobalt content of 1 mass% (M1 + M2 = 1.5 mass%) were obtained in the same manner as in Example 1, except that cobalt (purity 99.9%) was used instead of iron. A lithium secondary battery was fabricated using the anode of Example 3. The size of the non-aluminum phase in the obtained anode material was 2.1 μm.
[0128] Example 4 An anode material and an anode of Example 4 having a silicon content of 0.5 mass% and a cerium content of 1 mass% (M1 + M2 = 1.5 mass%) were obtained in the same manner as in Example 1, except that cerium (purity 99.9%) was used instead of iron. A lithium secondary battery was fabricated using the anode of Example 4. The size of the non-aluminum phase in the obtained anode material was 3.5 μm.
[0129] Comparative Example 1 An anode material and an anode of Comparative Example 1 having a silicon content of 1 mass % (M1 + M2 = 1 mass %, with the proviso that M2 = 0 mass %) were obtained in the same manner as in Example 1, except that iron was not used and the amount of silicon was changed. A lithium secondary battery was produced using the anode of Comparative Example 1. A non-aluminum phase consisting of Si was confirmed in the obtained anode material.
[0130] <Comparative Example 2> An anode material and an anode of Comparative Example 2 having a silicon content of 0.5 mass% (M1 + M2 = 0.5 mass%, with the proviso that M2 = 0 mass%) were obtained in the same manner as in Example 1, except that iron was not used and the amount of silicon was changed. A lithium secondary battery was produced using the anode of Comparative Example 2. No non-aluminum phase consisting of Si was confirmed in the obtained anode material.
[0131] <Comparative Example 3> An anode material and an anode of Comparative Example 3 were obtained in the same manner as in Example 1, except that iron and silicon were not used and only aluminum was used. A lithium secondary battery was produced using the anode of Comparative Example 2. No non-aluminum phase was confirmed in the obtained anode material.
[0132] <Evaluation 2: Example 5> An anode material and an anode of Example 5 having a manganese content of 1.4 mass% and a chromium content of 0.6 mass% (M1 + M2 = 2 mass%) were obtained in the same manner as in Example 1, except that high-purity chemically produced manganese (purity: 99.999 mass% or more) was used instead of silicon and chromium (purity: 99.9%) was used instead of iron. A lithium secondary battery was produced using the anode of Example 5. The size of the non-aluminum phase in the obtained anode material was 3.1 μm.
[0133] Comparative Example 4 A negative electrode material and a negative electrode of Comparative Example 4 having a manganese content of 2 mass% (M1 + M2 = 2 mass%) were obtained in the same manner as in Example 5, except that chromium was not used and the amount of manganese was changed. A lithium secondary battery was produced using the negative electrode of Comparative Example 4. A non-aluminum phase consisting of Mn was confirmed in the obtained negative electrode material.
[0134] The evaluation results are shown in Tables 1 and 2. Table 1 shows the results of Evaluation 1, and Table 2 shows the results of Evaluation 2. In the tables, "%" in the columns M1 and M2 means "% by mass."
[0135]
[0136]
[0137] As a result of the evaluation, the negative electrodes of Examples 1 to 5 all exhibited higher discharge capacity retention rates and better cycle characteristics than the comparative examples. Furthermore, considering that the charge-discharge efficiency of the negative electrodes using the Al—Fe alloys described in the prior art documents described above decreased to below 60% after 10 charge-discharge cycles, the negative electrodes of Examples 1 to 5 are considered to have better cycle characteristics than the Al—Fe alloys.
[0138] The above results confirmed the usefulness of the present invention.
[0139] 3. Negative electrode, 6. Electrolyte, 6. Non-aqueous electrolyte (electrolyte), 10. Lithium secondary battery (non-aqueous electrolyte secondary battery)
Claims
1. A negative electrode material made of an aluminum alloy, the negative electrode material comprising aluminum, an element M1 having a solid solubility limit in aluminum of 1.5 mass% or more, and an element M2 having a solid solubility limit in aluminum of less than 1.5 mass%, the element M1 being at least one element selected from the group consisting of Si, Ge, and Mn, the element M2 being at least one element selected from the group consisting of B, Ti, V, Cr, Fe, Co, Ni, Sr, Y, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, La, Ce, Pr, and Nd, the aluminum purity of the remainder of the negative electrode material excluding the element M1 and the element M2 from the entire negative electrode material is 99 mass% or more, the element M1 is present by substituting an aluminum atom in the aluminum metal crystal in the negative electrode material, The element M2 forms a non-aluminum phase having a length of 10 nm to 10 μm in a cross-sectional image obtained under the following conditions: (Conditions) The negative electrode material before charging and discharging is rolled to a thickness of 50 μm, and the obtained rolled material is cut perpendicularly to the rolling direction. An element mapping image is created by SEM-EDX for the obtained cut surface, and this is used as the cross-sectional image.
2. The negative electrode material according to claim 1, wherein the total content of the elements M1 and M2 in the entire negative electrode material is 0.5 mass % or more and 8 mass % or less.
3. The negative electrode material according to claim 1 or 2, having a Vickers hardness of 10 HV or more and 70 HV or less.
4. The negative electrode material according to claim 1 or 2, which is a rolled material consisting of aluminum, element M1, and element M2, and is obtained by heating a negative electrode material precursor, in which the aluminum content is 99 mass% or more in the remainder after excluding element M1 and element M2 from the entire rolled material, at 100°C or more and 350°C or less.
5. A negative electrode for a non-aqueous electrolyte battery, comprising the negative electrode material according to claim 1 or 2.
6. A non-aqueous electrolyte secondary battery comprising the negative electrode for a non-aqueous electrolyte battery according to claim 5.
Citation Information
Patent Citations
Negative electrode active material, and secondary battery and capacitor using the same
JP2011228058A
Aluminum anode material for brine air cell, brine aluminum air cell and manufacturing method of aluminum anode material for brine air cell
JP2016204712A
Battery electrode foil for the production of lithium-ion batteries
JP2022153358A
Negative-electrode active material for non-aqueous electrolyte secondary cell, negative electrode, cell, and laminate
WO2020105330A1
Negative electrode active material for lithium secondary battery, metal negative electrode, and lithium secondary battery