MgO POWDER, MgO SLURRY, PRODUCTION METHODS OF THOSE, AND METHOD FOR PRODUCING GRAIN-ORIENTED ELECTRICAL STEEL SHEET

The controlled particle size and shape distribution in MgO powder and slurry address the issue of coil shape changes during annealing in grain-oriented electrical steel sheet production, enhancing yield and magnetic properties by preventing local volume reduction and steel plate slipping.

WO2024214722A1PCT designated stage expired Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014481
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

In the production of grain-oriented electrical steel sheets, existing annealing separators with coarse MgO aggregates can cause local volume reduction during final annealing, leading to coil shape changes and decreased yield due to steel plate sliding, which is not effectively addressed by existing technologies.

Method used

The development of MgO powder and slurry with controlled particle size and shape ratios, where the mass of granular particles with a long axis to short axis ratio less than 1.50 constitutes 10 to 85% of the total powder, and the average particle size ratio of plate-like to granular particles is over 1.00, preventing local volume reduction and maintaining coil shape stability during annealing.

Benefits of technology

The use of the MgO powder and slurry with specific particle size distributions effectively minimizes coil deformation during final annealing, ensuring a stable coil shape and improved yield by preventing steel plate slipping and maintaining desired magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014481_17102024_PF_FP_ABST
    Figure JP2024014481_17102024_PF_FP_ABST
Patent Text Reader

Abstract

This MgO powder has an MgO content of 90% or more, the mass of granular particles is 10-85% of the mass of the whole MgO powder, and if Lfave is the average particle diameter of plate-like particles and Lgave is the average particle diameter of the granular particles, Lgave / Lfave is more than 1.00.
Need to check novelty before this filing date? Find Prior Art

Description

MgO powder, MgO slurry, and methods for producing them, and method for producing grain-oriented electrical steel sheet

[0001] The present invention relates to an MgO powder, an MgO slurry, methods for producing them, and a method for producing a grain-oriented electrical steel sheet using them. This application claims priority based on Japanese Patent Application No. 2023-063669, filed on April 10, 2023, the contents of which are incorporated herein by reference.

[0002] Grain-oriented electrical steel sheets are soft magnetic materials that are primarily used as iron core materials in transformers. Therefore, grain-oriented electrical steel sheets are required to have magnetic properties, including high magnetization and low iron loss. Iron loss is the power loss consumed as thermal energy when an iron core is excited by an AC magnetic field, and from the perspective of energy conservation, iron loss should be as low as possible.

[0003] In the manufacture of grain-oriented electrical steel sheets, a manufacturing method is generally applied in which a slab adjusted to a predetermined chemical composition is subjected to the following processes: hot rolling, hot-rolled sheet annealing, cold rolling, decarburization annealing, and finish annealing. Among these processes, in the finish annealing process, the steel sheet wound into a coil is annealed at a high temperature for a long time to concentrate the crystal orientation into the Goss orientation, which is good for magnetic properties (to increase the degree of orientation concentration). During this process, an annealing separator is applied to prevent the coil from seizing.

[0004] The annealing separator applied to the coil is often one containing magnesium oxide (MgO) as its main component. The reason for this is that by using an annealing separator containing MgO as its main component, silicon dioxide (SiO 2 ) reacts with MgO, forming forsterite (Mg 2 SiO 4 This is because a MgO-based coating (primary coating) can be formed on the steel sheet surface. This primary coating applies tension to the steel sheet surface and also provides insulation to the steel sheet. The use of an annealing separator containing MgO as its main component not only prevents seizure during final annealing, but also improves the magnetic properties of the grain-oriented electrical steel sheet.

[0005] As described above, in the production of grain-oriented electrical steel sheets, the properties of the grain-oriented electrical steel sheets can change depending on the annealing separator. Therefore, in recent years, research has been conducted on trace elements contained in magnesium oxide contained in annealing separators. Furthermore, research has been conducted not only on the content of trace elements but also on the structure of compounds containing trace element elements in magnesium oxide for annealing separators.

[0006] For example, Patent Document 1 discloses a powder for an annealing separator containing 0.04 mass % or more and 0.30 mass % or less of boron and containing magnesium oxide as a main component, characterized in that the proportion of tricoordinate boron in the boron is 70% or more and 95% or less.

[0007] Patent Document 2 discloses a method for producing a powder for an annealing separator, which comprises calcining a raw material containing either or both of magnesium hydroxide and magnesium carbonate and boron, and then adjusting the ratio of tricoordinated boron by controlling the humidity of the calcined product, in which the ratio of tricoordinated boron in the boron contained in the powder for an annealing separator is 70% or more and 95% or less.

[0008] In both Patent Documents 1 and 2, it is stated that 1) the purification of impurities is affected by the behavior of the film reaction at high temperatures (1100°C or higher), 2) the behavior of the film reaction at high temperatures is affected by boron in a three-coordinated state, and 3) boron in a four-coordinated state not only does not contribute to the purification of impurities but also penetrates into the steel sheet during high-temperature annealing and becomes Fe. 2 The ratio of tricoordinated boron is specified based on the knowledge that tricoordinated boron forms B and causes deterioration due to repeated bending.

[0009] Japanese Patent Publication No. 2017-128772 Japanese Patent Publication No. 2020-15982

[0010] If coarse MgO aggregates are present in the annealing separator, local volume reduction may occur in the primary coating during finish annealing. If local volume reduction occurs in the primary coating, the steel sheets may slide against each other, causing a change in shape in the width direction of the coil. If the shape of the coil in the width direction changes, the coil will buckle during annealing, causing a drop in yield in the width direction, which is undesirable.

[0011] The above-mentioned Patent Documents 1 and 2 do not take into consideration changes in the shape of the coil in the width direction.

[0012] The present invention has been made in view of the above-mentioned problems, and aims to provide an MgO powder, an MgO slurry, and methods for producing the same, for producing grain-oriented electrical steel sheets that exhibit minimal change in shape in the width direction, as well as a method for producing the grain-oriented electrical steel sheets.

[0013] The gist of the present invention is as follows: (1) An MgO powder according to one aspect of the present invention is an MgO powder containing MgO particles, wherein the Mg content of the MgO powder is 90% or more, and the mass of the MgO particles having an La / Lb ratio of less than 1.50, where La is the long axis length of the MgO particles and Lb is the short axis length of the MgO particles, is 10 to 85% of the mass of the entire MgO powder, and the average particle size of the MgO particles having an La / Lb ratio of 1.50 or more is Lf ave and the average particle size of the MgO particles having La / Lb of less than 1.50 is Lg ave When this is done, Lg ave / Lf aveis greater than 1.00. (2) An MgO slurry according to another aspect of the present invention comprises the MgO powder according to (1) above and water. (3) A method for producing an MgO powder according to another aspect of the present invention is a method for producing an MgO powder according to (1) above, using a raw material powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, wherein, when the major axis length of the raw material particles is taken as la and the minor axis length of the raw material particles is taken as lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 accounts for 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave and the average particle size of the raw material particles having an 1a / 1b ratio of less than 1.50 is 1g ave When the raw material particles having the la / lb ratio of 1.50 or more and the raw material particles having the la / lb ratio of less than 1.50 are mixed together by 1g ave / lf ave (4) Another aspect of the present invention provides a method for producing an MgO slurry, which is described in (2) above, using a raw material powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, and water, wherein, when the major axis length of the raw material particles is taken as la and the minor axis length of the raw material particles is taken as lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 accounts for 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave and the average particle size of the raw material particles having an 1a / 1b ratio of less than 1.50 is 1g ave When the raw material particles having the la / lb ratio of 1.50 or more and the raw material particles having the la / lb ratio of less than 1.50 are mixed together by 1g ave / lf ave(5) Another aspect of the present invention provides a method for producing an MgO slurry, which comprises: calcining the raw material powder at a temperature in the range of 700 to 1100°C for 5 to 120 minutes, pulverizing the calcined raw material powder, and mixing the calcined raw material powder with water. (6) Another aspect of the present invention provides a method for producing an MgO slurry, which comprises using water and a raw material powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, and wherein, when the major axis length of the raw material particles is la and the minor axis length of the raw material particles is lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 accounts for 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave and the average particle size of the raw material particles having an 1a / 1b ratio of less than 1.50 is 1g ave When the raw material particles having an Ia / Ib ratio of 1.50 or more are fired in a temperature range of 700 to 1100°C for 5 to 120 minutes, and the raw material particles having an Ia / Ib ratio of less than 1.50 are fired in a temperature range of 700°C or more for 5 to 120 minutes, and each is crushed as necessary, and then ave / lf ave The sintered raw material particles are mixed in water so that the MgO content exceeds 1.00. (6) A method for producing a grain-oriented electrical steel sheet according to another aspect of the present invention uses the MgO powder described in (1) above. (7) A method for producing a grain-oriented electrical steel sheet according to another aspect of the present invention uses the MgO slurry described in (2) above.

[0014] According to the above aspect of the present invention, it is possible to provide an MgO powder, an MgO slurry, and methods for producing the same, for producing a grain-oriented electrical steel sheet that exhibits little change in shape in the width direction, as well as a method for producing the grain-oriented electrical steel sheet.

[0015] 1 is a diagram illustrating the coil shape before and after final annealing, and FIG. 2 is a diagram illustrating a method for measuring the coil deformation amount at a deformed portion of the coil after final annealing.

[0016] The MgO powder, MgO slurry, and methods for producing them, as well as the method for producing a grain-oriented electrical steel sheet according to this embodiment will be described in more detail below. However, the present invention is not limited to the configurations disclosed in this embodiment, and various modifications are possible within the scope of the present invention.

[0017] <MgO Powder> The MgO powder according to this embodiment is an MgO powder containing MgO particles, wherein the Mg powder has an Mg content of 90% or more, and among the MgO particles, when the major axis length of the MgO particles is La and the minor axis length of the MgO particles is Lb, the mass of the MgO particles having an La / Lb ratio of less than 1.50 is 10 to 85% of the mass of the entire MgO powder, and the average particle size of the MgO particles having an La / Lb ratio of 1.50 or more is Lf ave and the average particle size of the MgO particles having La / Lb of less than 1.50 is Lg ave When this is done, Lg ave / Lf ave is greater than 1.00. This will be explained in more detail below.

[0018] The MgO powder according to this embodiment contains MgO particles. The MgO powder according to this embodiment contains, for example, 50.0% or more of MgO particles. The content of MgO particles in the MgO powder is preferably 80.0% by mass or more, more preferably 90.0% by mass or more, and even more preferably 99.0% by mass.

[0019] The MgO powder may contain impurities such as Al, B, Fe, Si, etc. When the content of each impurity element is 0.5 mass% or less, or when the total content is 1.0 mass% or less, the influence on the magnetic properties or coating properties of the grain-oriented electrical steel sheet is small.

[0020] Amount of Mg in MgO powder: 90% or more The amount of Mg in MgO powder can be expressed by the left side of the following equation. The amount of Mg in MgO powder being 90% or more means that the Mg mass concentration [Mg] when the MgO powder is chemically analyzed satisfies the following equation. The chemical analysis is performed by quantitative analysis of elements using ICP-MS. [Mg] x 40 / 24 ≥ 90%

[0021] If the Mg content in the MgO powder is less than 90%, it is not possible to obtain a grain-oriented electrical steel sheet with minimal change in shape in the width direction. Therefore, the Mg content in the MgO powder is set to 90% or more, and preferably 95% or more.

[0022] Mass of MgO particles with La / Lb less than 1.50: 10 to 85%. By controlling the proportion of granular particles within a predetermined range and the ratio of the average particle size of the flat, plate-like particles to the average particle size of the granular particles within a desired range, fine MgO particles that are prone to sintering can be highly dispersed, preventing local volume loss. Furthermore, the plate-like particles act as a framework, preventing the steel sheets from sliding against each other. As a result, deformation of the coil width during finish annealing can be prevented.

[0023] In this embodiment, when the major axis length of an MgO particle contained in an MgO powder is La and the minor axis length of the MgO particle is Lb, MgO particles with an La / Lb ratio of less than 1.50 are considered to be granular particles. Conversely, MgO particles with an La / Lb ratio of 1.50 or more are considered to be plate-like particles. Note that in MgO powder, MgO particles may aggregate together to form secondary particles, but the major axis length and minor axis length referred to here refer to the major axis length and minor axis length of the primary particle of the MgO particle.

[0024] The mass of granular particles (MgO particles with La / Lb less than 1.50) of the entire MgO powder is 10 to 85%. The mass of the granular particles is preferably 20% or more, more preferably 30% or more. The mass of the granular particles is preferably 50% or less.

[0025] Ratio of average particle size (Lg ave / Lf ave ): 1.00 or more The average particle size of plate-like particles (MgO particles having La / Lb of 1.50 or more) is Lf ave and the average particle size of granular particles (MgO particles with La / Lb less than 1.50) is Lg ave When this is done, Lg ave / Lf aveBy increasing the ratio of the average particle size of the granular particles to the average particle size of the plate-like particles, the plate-like particles can suitably function as a framework. ave / Lf ave is preferably 1.10 or more. In addition, from the viewpoint of further reducing the change in shape in the width direction, the average particle diameter Lf of the plate-like particles is ave and the average particle size of the granular particles Lg ave are each preferably less than 2.000 μm, more preferably 1.500 μm or less or 1.000 μm or less, and even more preferably 0.500 μm or less.

[0026] The measurement method is explained below. A scanning electron microscope (SEM) is used to take an enlarged photograph of MgO particles in the MgO powder. The shape of one primary particle among the MgO particles is traced, and the major axis length (La) and minor axis length (Lb) of the primary particle are calculated by image analysis. This operation is performed on 50 or more randomly selected particles. This identifies MgO particles with an La / Lb ratio of 1.50 or more (plate-like particles) and MgO particles with an La / Lb ratio of less than 1.50 (granular particles).

[0027] The circle-equivalent diameters of the identified plate-like particles and granular particles are calculated, and the average value thereof is calculated to determine the average particle diameter of the plate-like particles (Lf ave ) and the average particle size of the granular particles (Lg ave ) is obtained.

[0028] Method for measuring the mass of granular particles Average particle size of plate-like particles (Lf ave ) and the average particle size of the granular particles (Lg ave From the same enlarged photograph as when measuring the La / Lb ratio, the La / Lb of 50 or more randomly selected particles is calculated, and the number frequency ff (%) of MgO particles (plate-like particles) having an La / Lb ratio of 1.50 or more and the number frequency fg (%) of MgO particles (granular particles) having an La / Lb ratio of less than 1.50 are calculated. The mass % (Wg (%)) of the granular particles is calculated using the obtained values ​​and formula (1).

[0029] Wg = ff x Lf ave 3 / (50×(Lf ave3 + Lg ave 3 )) ... (1)

[0030] <MgO Slurry> The MgO slurry according to this embodiment contains the MgO powder containing the above-described MgO particles, and water. The MgO powder and MgO particles have been described above, so a detailed description will be omitted. The mass of the MgO powder in the MgO slurry may be 5 to 30%.

[0031] When the above-mentioned measurements are carried out on the MgO powder in the MgO slurry, the MgO slurry is held in a thermostatic chamber at 80° C. for a predetermined time to evaporate the water, and the above-mentioned measurements are carried out on the MgO powder obtained.

[0032] <Method of manufacturing MgO powder> Next, a method of manufacturing the above-mentioned MgO powder will be described. The method of manufacturing the MgO powder according to this embodiment is a method of manufacturing MgO powder using a raw material powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, wherein, when the major axis length of the raw material particles is la and the minor axis length of the raw material particles is lb, the mass of the raw material particles having an la / lb ratio of less than 1.5 accounts for 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave and the average particle size of the raw material particles having an 1a / 1b ratio of less than 1.50 is 1g ave When the raw material particles having the la / lb ratio of 1.50 or more and the raw material particles having the la / lb ratio of less than 1.50 are mixed together by 1g ave / lf ave The raw material powder is obtained by mixing the raw material powder so that the average molecular weight of the raw material is greater than 1.00, and the raw material powder is fired at a temperature in the range of 700 to 1100° C. for 5 to 120 minutes, and then pulverized as necessary.

[0033] The raw material powder contains one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate. In addition to these raw material particles, the raw material powder may also contain magnesium chloride, calcium carbonate, and calcium chloride.

[0034] Mass of raw material particles with an l a / l b ratio of less than 1.50: 10 to 85%. When the major axis length of the raw material particles in the raw material powder is l a and the minor axis length of the raw material particles is l b , the mass of raw material particles with an l a / l b ratio of less than 1.50 is 10 to 85% of the total mass of the raw material powder. This allows the mass of granular particles in the MgO powder to be controlled within a preferred range. The mass of raw material particles with an l a / l b ratio of less than 1.50 is preferably 20% or more, more preferably 30% or more. Furthermore, the mass of raw material particles with an l a / l b ratio of less than 1.50 is preferably 40% or less.

[0035] Ratio of average particle size (lg ave / lf ave ) 1.00 or more, the average particle size of raw material particles having an 1a / 1b ratio of 1.50 or more is 1f ave The average particle size of raw material particles having an Ia / Ib ratio of less than 1.50 is Ig ave When this is done, lg ave / lf ave is set to be greater than 1.00. This makes it possible to control the average particle size of the plate-like particles and the average particle size of the granular particles in the MgO powder within a preferred range. ave / lf ave is preferably 1.10 or more. In addition, from the viewpoint of further reducing the change in shape in the width direction, the average particle diameter lf of the plate-like particles is ave It is preferable that the average particle diameter lf of the plate-like particles is 10,000 μm or less. ave and the average particle size of the granular particles, lg ave are each preferably less than 2.000 μm, more preferably 1.500 μm or less or 1.000 μm or less, and even more preferably 0.500 μm or less.

[0036] The mass and average particle size ratio of raw material particles having an 1a / 1b ratio of less than 1.50 (1g ave / lf ave In order to control the particle size distribution within the above range, it is sufficient to adjust the mixing ratio of two or more types of raw material particles having different average particle size, major axis length, minor axis length, etc. The major axis length, minor axis length, and average particle size of the raw material powder can be measured by the same method as for the MgO powder described above.

[0037] Next, the raw material powder is fired at a temperature in the range of 700 to 1100°C. This allows MgO powder to be obtained. After firing, the MgO powder may be pulverized using a method such as a ball mill, if necessary. Note that these pulverization methods do not destroy the primary particles of the raw material powder. The firing temperature is preferably 720°C or higher, more preferably 750°C or higher. The firing temperature is preferably 1080°C or lower, more preferably 1040°C or lower. The firing time is 5 to 120 minutes to favorably control the Mg content in the MgO powder. From the viewpoint of eliminating firing unevenness, the firing time is preferably 8 minutes or longer, more preferably 10 minutes or longer. On the other hand, from the viewpoint of economy, the firing time is preferably 80 minutes or shorter, more preferably 60 minutes or shorter. However, when firing only raw material particles having an 1a / 1b ratio of less than 1.50, firing at a temperature above 1100°C is acceptable.

[0038] The firing atmosphere is preferably an air atmosphere or a nitrogen atmosphere, and any other atmosphere is economically disadvantageous and therefore not preferred.

[0039] <Method for Producing MgO Slurry> The method for producing an MgO slurry according to this embodiment includes a method for mixing raw material powder with water, and a method for mixing two or more types of raw material particles in water. The only difference between these two methods is whether the mixing of the two or more types of raw material particles is performed before or during the mixing with water.

[0040] In the method of mixing raw material powder and water, MgO slurry is obtained by mixing the raw material powder and water. More specifically, this is a method of producing MgO slurry using raw material powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, and water, wherein, when the major axis length of the raw material particles is la and the minor axis length of the raw material particles is lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 accounts for 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf aveand the average particle size of the raw material particles having an 1a / 1b ratio of less than 1.50 is 1g ave When the raw material particles having the la / lb ratio of 1.50 or more and the raw material particles having the la / lb ratio of less than 1.50 are mixed together by 1g ave / lf ave The raw material powder is obtained by mixing the raw material powder so that the molecular weight ratio exceeds 1.00, and the raw material powder is fired at a temperature range of 700 to 1100°C for 5 to 120 minutes, and then pulverized as necessary. After that, the fired raw material powder and the water are mixed.

[0041] In the method of mixing two or more kinds of raw material particles in water, two or more kinds of raw material particles are mixed in water so that the raw material powder after mixing has the above-mentioned ratio of mass and average particle size, thereby obtaining MgO slurry. More specifically, this is a method of producing MgO slurry using a raw material powder containing one or more kinds of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, and water, wherein, when the major axis length of the raw material particles is la and the minor axis length of the raw material particles is lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 accounts for 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave and the average particle size of the raw material particles having an 1a / 1b ratio of less than 1.50 is 1g ave When the raw material particles having an Ia / Ib ratio of 1.50 or more are fired in a temperature range of 700 to 1100°C for 5 to 120 minutes, and the raw material particles having an Ia / Ib ratio of less than 1.50 are fired in a temperature range of 700°C or more for 5 to 120 minutes, and each is crushed as necessary, and then ave / lf ave The raw material particles after firing are mixed in water so that the sintering ratio exceeds 1.00.

[0042] <Method for Manufacturing Grain-Oriented Electrical Steel Sheet> In the method for manufacturing a grain-orientated electrical steel sheet according to this embodiment, the above-described MgO powder is used as an annealing separator. The method for manufacturing a grain-orientated electrical steel sheet according to this embodiment includes, for example, a hot rolling step in which a slab is hot-rolled to obtain a hot-rolled sheet, a hot-rolled sheet annealing step in which the hot-rolled sheet is annealed, a cold-rolling step in which the hot-rolled sheet after the hot-rolled sheet annealing step is cold-rolled to obtain a cold-rolled sheet, a decarburization annealing step in which the cold-rolled sheet is decarburized and annealed, and a finish annealing step in which an annealing separator containing the MgO powder is applied to the cold-rolled sheet after the decarburization annealing step, the cold-rolled sheet is dried, and then finish annealed. This manufacturing method using the MgO powder or MgO slurry according to this embodiment makes it possible to manufacture a grain-orientated electrical steel sheet with small differences in magnetic properties in the width direction.

[0043] In this embodiment, the annealing separator to be applied before finish annealing is an annealing separator prepared by mixing the MgO powder according to the embodiment described above with water to form an MgO slurry. In the above manufacturing method, known manufacturing conditions for grain-oriented electrical steel sheets can be applied to the chemical composition of the slab and the conditions of each step, except for the annealing separator used.

[0044] Next, the effects of one embodiment of the present invention will be explained in more detail using examples, but the conditions in the examples are merely examples adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.

[0045] (Example 1) The average particle size, the major axis length of the primary particles la, the minor axis length of the primary particles lb, the average aspect ratio (la / lb), and the particle size ratio (lg) are shown in Table 1. ave / lf ave ) were fired at a temperature range of 700 to 1100°C for 5 to 120 minutes and pulverized to obtain MgO particles 1 and MgO particles 2. These MgO particles 1 and MgO particles 2 were mixed with water to obtain an annealing separator (aqueous slurry). Note that the average particle diameters of MgO particles 1 and MgO particles 2 are not shown in the table.

[0046] The annealing separator thus obtained was used to evaporate the water content by the above-mentioned method to obtain MgO powder. MgO particles (plate-like particles) having an La / Lb ratio of 1.50 or more and MgO particles (granular particles) having an La / Lb ratio of less than 1.50 were identified, and their contents, average aspect ratios, average particle diameters, particle diameter ratios (Lg ave / Lf ave In the test numbers that satisfy the preferable conditions, the amount of Mg is 90% or more, the mass of MgO particles having La / Lb of less than 1.50 is 10 to 85% of the mass of the entire MgO powder, and Lg ave / Lf ave was over 1.00.

[0047] Next, the above-mentioned annealing separator was applied to the cold-rolled steel sheet after primary recrystallization annealing. For all test numbers, the cold-rolled steel sheet with the annealing separator applied to its surface was subjected to a baking treatment at 300°C for 30 seconds to dry the annealing separator. After the baking treatment, a final annealing treatment was performed. For all test numbers, the final annealing treatment was performed by holding the steel sheet at 1200°C for 20 hours.

[0048] Through the above manufacturing process, the base steel plate and forsterite (Mg 2 SiO 4 Grain-oriented electrical steel sheets having a glass coating containing a complex oxide such as Cr, Ni, or Ni-based oxide were manufactured. The height of the obtained grain-oriented electrical steel sheet coil was then measured from the lower end of the coil, where the deformation amount of the coil was greatest, to the upper end of a region where deformation of 1% or more occurred in the outer or inner circumferential direction, based on the diameter at the center of the width direction, to obtain the coil deformation amount (mm) of the grain-oriented electrical steel sheet. Specifically, the coil deformation amount (mm) of the grain-oriented electrical steel sheet was obtained by measuring the coil deformation amount at the position shown in FIG. 2 for cross section A ( FIG. 2 ) of the coil, which was deformed from the coil before finish annealing shown in FIG. 1( a) to the shape shown in FIG. 1( b) by finish annealing.

[0049] When the coil deformation amount of the obtained grain-oriented electrical steel sheet was less than 70 mm, the grain-oriented electrical steel sheet was judged to have small shape change in the width direction and to have passed the test.When the coil deformation amount of the obtained grain-oriented electrical steel sheet was 70 mm or more, the grain-oriented electrical steel sheet was judged to have large shape change in the width direction and to have passed the test.

[0050] In test numbers 1 and 2, the average aspect ratio of all MgO raw material particles was 1.50 or more, and therefore there was a shortage of MgO particles with an La / Lb ratio of less than 1.50. As a result, loosening of the coil occurred, and the coil deformation of the grain-oriented electrical steel sheet reached 70 mm or more. In test number 12, the particle size ratio (lg ave / lf ave ) was 1.00 or less, the coil loosened, and the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more.

[0051] In test number 6, the amount of MgO raw material particles with a small aspect ratio was small, resulting in a shortage of MgO particles with an La / Lb ratio of less than 1.50, and the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more. In test number 7, the amount of MgO raw material particles with a small aspect ratio was large, resulting in an excess of MgO particles with an La / Lb ratio of less than 1.50, and the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more.

[0052] In test numbers 3 to 5, 8 to 11, and 13 to 19, the average aspect ratios of the two types of MgO raw material particles were within the preferred range, and their particle size ratios and contents were also appropriate. Therefore, the mass and Lg of MgO particles with La / Lb of less than 1.50 were ave / Lf ave was within the preferred range, the coil deformation of the grain-oriented electrical steel sheet was less than 70 mm.

[0053] In particular, in test numbers 8 to 11, the particle size ratio of the MgO raw material particles (lg ave / lf ave ) was higher, so Lg ave / Lf ave The value was 1.10 or more, the steel sheet was less likely to slip, and the coil deformation amount was 20 mm or less.

[0054]

[0055] Example 2 MgO particles 1 were obtained by firing MgO raw material particles 1 shown in Table 2 under the conditions described in Table 2. MgO particles 2 were obtained by firing MgO raw material particles 2 shown in Table 3 under the conditions described in Table 3. MgO particles 1 and MgO particles 2 were mixed in the amounts described in Tables 2 and 3, respectively, to obtain MgO powder described in Table 4. The obtained MgO powder was mixed with water to obtain an annealing separator (aqueous slurry).

[0056] The annealing separator thus obtained was used to evaporate the water content by the above-mentioned method to obtain MgO powder. MgO particles (plate-like particles) having an La / Lb ratio of 1.50 or more and MgO particles (granular particles) having an La / Lb ratio of less than 1.50 were identified, and their contents, average aspect ratios, average particle diameters, particle diameter ratios (Lg ave / Lf ave ) was obtained.

[0057] Next, the above-mentioned annealing separator was applied to the cold-rolled steel sheet after primary recrystallization annealing. For all test numbers, the cold-rolled steel sheet with the annealing separator applied to its surface was subjected to a baking treatment at 300°C for 30 seconds to dry the annealing separator. After the baking treatment, a final annealing treatment was performed. For all test numbers, the final annealing treatment was performed by holding the steel sheet at 1200°C for 20 hours.

[0058] Through the above manufacturing process, the base steel plate and forsterite (Mg 2 SiO 4 Grain-oriented electrical steel sheets having a glass coating containing a composite oxide such as Cr, Ni, Ni, and Cu, were manufactured. The coil deformation of the obtained grain-oriented electrical steel sheets was measured in the same manner as in Example 1. Table 4 shows the test results.

[0059] In test numbers 20, 22, 24, and 25, the firing conditions for the MgO raw material particles were not within the preferred conditions, so the raw material remained and the Mg content of the MgO powder after firing was 90% or less. As a result, the magnetic unevenness in the width direction of the grain-oriented electrical steel sheet was 0.015 T or more.

[0060] In test number 23, the firing conditions for MgO raw material particles 2 having a large average aspect ratio (1a / 1b) were outside the preferred conditions, resulting in coarsening of the particles and resulting in an excessively large average particle size of the plate-like particles.

[0061] In Test Nos. 26 and 27, the average aspect ratio of all raw material particles was 1.50 or more, and therefore there was a shortage of MgO particles with an La / Lb ratio of less than 1.50. As a result, the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more.

[0062] In test numbers 28 and 29, the content of MgO, which has a small aspect ratio, was outside the preferred range, and therefore the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more.

[0063] In test numbers 30 and 31, the particle size ratio of the two types of MgO particles was within the preferred range and the contents thereof were appropriate, so the coil deformation of the grain-oriented electrical steel sheets was less than 70 mm.

[0064] In particular, in test number 31, the particle size ratio (Lg ave / Lf ave ) was 1.10 or more, the steel sheet was less likely to slip, and the coil deformation amount was 20 mm or less.

[0065]

[0066]

[0067]

[0068] Example 3 A raw material powder was obtained by mixing MgO raw material particles 1 and MgO raw material particles 2 shown in Tables 5 and 6 in the blending amounts shown in Tables 5 and 6. The obtained raw material powder was fired under the conditions shown in Table 7. As a result, the MgO powder shown in Table 7 was obtained. The obtained MgO powder was mixed with water to obtain an annealing separator (aqueous slurry).

[0069] The annealing separator thus obtained was used to evaporate the water content by the above-mentioned method to obtain MgO powder. MgO particles (plate-like particles) having an La / Lb ratio of 1.50 or more and MgO particles (granular particles) having an La / Lb ratio of less than 1.50 were identified, and their contents, average aspect ratios, average particle diameters, particle diameter ratios (Lg ave / Lf ave ) was obtained.

[0070] Next, the above-mentioned annealing separator was applied to the cold-rolled steel sheet after primary recrystallization annealing. For all test numbers, the cold-rolled steel sheet with the annealing separator applied to its surface was subjected to a baking treatment at 300°C for 30 seconds to dry the annealing separator. After the baking treatment, a final annealing treatment was performed. For all test numbers, the final annealing treatment was performed by holding the steel sheet at 1200°C for 20 hours.

[0071] Through the above manufacturing process, the base steel plate and forsterite (Mg 2 SiO 4 Grain-oriented electrical steel sheets having a glass coating containing a composite oxide such as Cr, Ni, Ni, and Cu, were manufactured. The coil deformation of the obtained grain-oriented electrical steel sheets was measured in the same manner as in Example 1. Table 7 shows the test results.

[0072] In test numbers 36 and 38, the firing conditions for the MgO raw material powder were not within the preferred conditions, so the raw material remained.

[0073] In test number 37, the firing conditions for the MgO raw material powder were not within the preferred conditions, resulting in a decrease in plate-like particles and an excessive increase in the content of granular particles. As a result, the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more.

[0074] In test numbers 39 and 40, the average aspect ratio of all the MgO raw material particles was 1.50 or more, and therefore there was a shortage of MgO particles with an La / Lb ratio of less than 1.50. As a result, the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more.

[0075] In test numbers 41 and 42, the content of the MgO raw material particles with a small aspect ratio was outside the preferred range, and therefore the coil deformation of the grain-oriented electrical steel sheet was 70 mm or more.

[0076] In test numbers 43 and 44, the particle size ratio of the two types of MgO particles was within the preferred range and the contents thereof were appropriate, so the coil deformation of the grain-oriented electrical steel sheets was less than 70 mm.

[0077] In particular, in test number 44, the particle size ratio (Lg ave / Lf ave ) was 1.10 or more, the steel sheet was less likely to slip, and the coil deformation amount was 20 mm or less.

[0078]

[0079]

[0080]

[0081] According to the above aspects of the present invention, it is possible to provide an MgO powder, an MgO slurry, and methods for producing the same, for producing a grain-oriented electrical steel sheet that exhibits little change in shape in the width direction, as well as a method for producing the grain-oriented electrical steel sheet.

Claims

1. An MgO powder containing MgO particles, wherein the MgO powder contains 90% or more Mg, and among the MgO particles, when the major axis length of the MgO particles is La and the minor axis length of the MgO particles is Lb, the mass of the MgO particles having La / Lb less than 1.50 is 10 to 85% of the total mass of the MgO powder, and the average particle size of the MgO particles having La / Lb of 1.50 or more is Lf ave The average particle size of the MgO particles having La / Lb of less than 1.50 is defined as Lg ave Then, Lg ave / Lf ave The MgO powder is characterized in that the MgO powder has a molecular weight of more than 1.

00.

2. A MgO slurry comprising the MgO powder according to claim 1 and water.

3. The method for producing MgO powder according to claim 1, using a raw material powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, wherein, among the raw material particles, when the major axis length of the raw material particle is la and the minor axis length of the raw material particle is lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 is 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave The average particle size of the raw material particles having an la / lb ratio of less than 1.50 is defined as lg ave When the raw material particles having the la / lb ratio of 1.50 or more and the raw material particles having the la / lb ratio of less than 1.50 are mixed, the raw material particles are mixed with the raw material particles having the la / lb ratio of 1.50 or more. ave / lf ave obtaining the raw material powder by mixing the raw material powder so that the average molecular weight of the raw material exceeds 1.00; sintering the raw material powder at a temperature range of 700 to 1100° C. for 5 to 120 minutes, and pulverizing the raw material powder as required.

4. The method for producing MgO slurry according to claim 2, which uses water and a raw powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, wherein, among the raw material particles, when the major axis length of the raw material particles is la and the minor axis length of the raw material particles is lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 is 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave The average particle size of the raw material particles having an la / lb ratio of less than 1.50 is defined as lg ave When the raw material particles having the la / lb ratio of 1.50 or more and the raw material particles having the la / lb ratio of less than 1.50 are mixed, the raw material particles are mixed by the following formula: ave / lf ave to obtain a raw material powder, sintering the raw material powder at a temperature range of 700 to 1100°C for 5 to 120 minutes, pulverizing the raw material powder as necessary, and then mixing the sintered raw material powder with the water.

5. A method for producing MgO slurry according to claim 2, using a raw material powder containing one or more types of raw material particles selected from the group consisting of magnesium hydroxide, basic magnesium carbonate, and magnesium carbonate, and water, wherein, among the raw material particles, when the major axis length of the raw material particle is la and the minor axis length of the raw material particle is lb, the mass of the raw material particles having an la / lb ratio of less than 1.50 is 10 to 85% of the mass of the entire raw material powder, and the average particle size of the raw material particles having an la / lb ratio of 1.50 or more is lf ave The average particle size of the raw material particles having an la / lb ratio of less than 1.50 is defined as lg ave When the raw material particles having an la / lb ratio of 1.50 or more are fired in a temperature range of 700 to 1100° C. for 5 to 120 minutes, and the raw material particles having an la / lb ratio of less than 1.50 are fired in a temperature range of 700° C. or more for 5 to 120 minutes, and each is crushed as necessary, and then ave / lf ave The method for producing an MgO slurry is characterized in that the raw material particles after sintering are mixed in water so that the MgO content exceeds 1.

00.

6. A method for producing grain-oriented electrical steel sheet, comprising using the MgO powder according to claim 1.

7. A method for producing a grain-oriented electrical steel sheet, comprising using the MgO slurry according to claim 2.

Citation Information

Patent Citations

  • Powder for annealing separation agent, production of the powder, and directive magnetic steel sheet

    JP2017128772A

  • Manufacturing method of powder for annealing separation agent

    JP2020015982A

  • Encoder, motor unit, and actuator

    JP2023063669A

  • Magnesium oxide for oriented silicon steel annealing separant, and preparation method

    CN111186850A

  • MANUFACTURING METHOD OF MgO FOR ANNEALING SEPARATING AGENT

    JP2005171387A