Polyethylene terephthalate film for vapor deposition, and transparent gas barrier film

The modification of PET films via corona treatment to achieve a dynamic contact angle of 26.0° or more enables the formation of a dense inorganic layer, enhancing the gas barrier performance of transparent gas barrier films, addressing the insufficient barrier properties of existing PET films.

WO2024214768A1PCT designated stage expired Publication Date: 2024-10-17TOYOBO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014651
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-11
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Current PET films for transparent gas barrier applications do not achieve sufficient gas barrier performance even with an inorganic layer deposition due to insufficient surface modification, leading to inadequate barrier properties.

Method used

A polyethylene terephthalate film with a modified surface achieved through corona treatment, resulting in a dynamic contact angle of 26.0° or more after diiodomethane droplet placement, which allows for the deposition of a dense inorganic layer, specifically aluminum oxide and silicon oxide, enhancing the gas barrier properties without the need for an additional overcoat.

Benefits of technology

The modified PET film effectively improves the barrier performance of the transparent gas barrier film, maintaining excellent transparency and extending the storage period of contents by reducing water vapor transmission rates and preventing corona strike-through phenomena.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014651_17102024_PF_FP_ABST
    Figure JP2024014651_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a polyethylene terephthalate film (PET film) for manufacturing a transparent gas barrier film that is inexpensive, that has excellent transparency, that can maintain barrier properties, and that enables preservation of contents for a long period of time; and a transparent gas barrier film in which the PET film is used as the base material and which has improved barrier performance. In order to improve barrier properties of transparent gas barrier films, the present inventors have strenuously studied the optimum surface state of a PET film serving as the material, and have arrived at the present invention through the discovery of a PET film that has a surface state for having a fine inorganic matter layer. Specifically, the present invention pertains to a polyethylene terephthalate film, for vapor deposition, used in vapor deposition of an inorganic matter layer. The polyethylene terephthalate film is characterized by having a property-modified surface on the side on which vapor deposition of the inorganic matter layer is to be performed, and is characterized in that the dynamic contact angle of the property-modified surface as measured 1 second after having diiodomethane dripped thereon is 26.0° or more.
Need to check novelty before this filing date? Find Prior Art

Description

Polyethylene terephthalate film for vapor deposition and transparent gas barrier film

[0001] The present invention relates to a polyethylene terephthalate film (PET film) that is excellent in transparency, gas barrier properties, printability, and flexibility and is used as a packaging material for foods, medicines, electronic components, etc., which require airtightness, or as a base material for a transparent gas barrier film that has excellent properties as a gas blocking material, and to a transparent gas barrier film using the same.

[0002] Transparent gas barrier films are made by laminating an inorganic material onto a plastic film. Metal oxides are often used as the inorganic material from the viewpoint of transparency. In particular, films made by laminating silicon oxide, aluminum oxide, or mixtures of these metal oxides by vapor deposition or CVD are mainly commercially available (see, for example, Patent Document 1).

[0003] The surface of the PET film on which the inorganic material barrier layer is laminated is subjected to anchor coating to improve the adhesive strength between the barrier layer and the PET film or the barrier properties, or the surface of the PET film is modified with plasma or the like.

[0004] There is a laminate in which a polyamide resin film is subjected to corona treatment or the like to reduce the contact angle of water to 70° or less, and the contact angle of diiodomethane to 35° or less, preferably 10 to 20°, and an inorganic layer is laminated on the film, and a sealant film is laminated on the film, thereby improving the barrier stability against retort treatment (see, for example, Patent Document 2).

[0005] Furthermore, with regard to PET films for battery exteriors other than transparent gas barrier films, a polyester film for battery exteriors is known in which the static contact angle of diiodomethane is increased to 22° or more by subjecting the film surface to corona treatment or the like (see, for example, Patent Document 3).

[0006] Japanese Patent No. 2638797 Japanese Patent Application Publication No. 10-52879 Japanese Patent Application Publication No. 2012-238491

[0007] However, according to the investigations of the present inventors, it has been found that the polyester film for battery exteriors described in Patent Document 3 does not have a sufficient degree of corona treatment, and even if an inorganic layer is vapor-deposited, sufficient barrier performance cannot be obtained.

[0008] Therefore, an object of the present invention is to provide a PET film, which is a vapor-deposited raw sheet of a transparent gas barrier film, having an improved surface condition that improves barrier performance, without using an anchor coat in which another resin is laminated on the substrate or an overcoat in which a resin is laminated on the inorganic layer that serves as a barrier layer, in order to improve the gas barrier performance of the transparent gas barrier film having an inorganic substance formed on the PET film.An object of the present invention is also to provide a transparent gas barrier film using the PET film as a substrate and having improved barrier performance.

[0009] The present inventors have conducted extensive research into the optimal surface condition of the PET film used as the raw material in order to improve the barrier properties of a transparent gas barrier film having an inorganic layer laminated thereon, and have discovered a PET film with a surface condition that densifies the inorganic layer, leading to the present invention.

[0010] That is, the present invention includes the following: [1] A polyethylene terephthalate film for vapor deposition used in applications in which an inorganic layer is vapor-deposited, the polyethylene terephthalate film having a modified surface on the side on which the inorganic layer is vapor-deposited, the modified surface having a dynamic contact angle of 26.0° or more measured 1 second after the addition of a drop of diiodomethane. [2] The polyethylene terephthalate film for vapor deposition according to [1], wherein the modified surface is formed by corona treatment. [3] A transparent gas barrier film comprising a polyethylene terephthalate film having a modified surface having a dynamic contact angle of 26.0° or more measured 1 second after the addition of a drop of diiodomethane, and an inorganic layer vapor-deposited on the modified surface. [4] The transparent gas barrier film according to [3], wherein the modified surface is formed by corona treatment. [5] The transparent gas barrier film according to [3] or [4], wherein the inorganic layer contains aluminum oxide and silicon oxide.

[0011] The present invention provides a PET film for producing a transparent gas barrier film that is inexpensive, has excellent transparency, and can maintain its barrier properties, allowing contents to be stored for a long period of time. It also provides a transparent gas barrier film that uses the PET film as a substrate and has improved barrier properties.

[0012] 1 is a cross-sectional view for explaining a dynamic contact angle; FIG. 2 is a cross-sectional view for explaining a corona treatment; FIG. 3 is a schematic diagram of an electron beam heating type vapor deposition apparatus;

[0013] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0014] The polyethylene terephthalate film for vapor deposition of the present invention is a polyethylene terephthalate film for vapor deposition used for vapor-depositing an inorganic layer, characterized in that it has a modified surface on the side on which the inorganic layer is to be vapor-deposited, and that the dynamic contact angle of the modified surface measured 1 second after the dropping of diiodomethane is 26.0° or more.

[0015] The inorganic layer in the present invention may be made of a metal such as Al, Si, Ti, Zn, Zr, Mg, Sn, Cu, or Fe, or an oxide, nitride, fluoride, or sulfide of these metals. Specific examples include SiOx (x=1.0 to 2.0), alumina, magnesia, zinc sulfide, titania, zirconia, cerium oxide, or a mixture thereof.

[0016] In particular, aluminum oxide, silicon oxide and mixtures thereof are suitable for use as transparent gas barrier films, and the modified surface of the present invention is particularly effective for the binary vapor deposition of aluminum oxide and silicon oxide.

[0017] The PET film referred to in the present invention refers to a film obtained by melt-extruding a PET resin whose main raw material is polyethylene terephthalate obtained by polymerizing ethylene glycol and terephthalic acid, to which other polymers may be mixed to adjust the film properties, or to which known additives such as ultraviolet absorbers, antistatic agents, plasticizers, lubricants, and colorants may be added, and then, as necessary, stretching in the machine direction (MD) and / or the transverse direction (TD), cooling, and heat setting.

[0018] The thickness of the PET film is not particularly limited, but the thickness of the PET film of the present invention is preferably in the range of 5 to 1000 μm, and more preferably in the range of 7 to 25 μm for roll-to-roll vacuum deposition.

[0019] As shown in Figure 1, the dynamic contact angle referred to in the present invention is the internal angle (θ) formed between the tangent 3 to the surface of a droplet 2 and the surface of the PET film 1 one second after the droplet 2 is placed on the PET film 1. The contact angle measured one second after the droplet is a dynamic contact angle, and is a value measured under extremely short conditions among dynamic contact angles. On the other hand, the static contact angle described in paragraph 0052 of JP 2012-238491 is a contact angle generally measured after 30 to 60 seconds, and is a measurement value different from the dynamic contact angle.

[0020] The diiodomethane referred to in the present invention is a special grade diiodomethane having a purity of 99% or more. The dynamic contact angle referred to in the present invention is a value measured in an environment at room temperature of 23°C and humidity of 50%.

[0021] The dynamic contact angle of diiodomethane is 26.0° or more, preferably 26.5° or more, and more preferably 27.0° or more. A contact angle of 26.0° or more tends to improve the water vapor transmission rate (WVTR). Even when forming an inorganic layer by vapor deposition, deterioration of the WVTR is minimized even in poor conditions of the vapor deposition apparatus and relatively high pressure. Furthermore, the dynamic contact angle of diiodomethane is preferably 29.0° or less. When the contact angle is 29.0° or less, corona strike-through (the phenomenon in which the back side of the treated surface is treated) is less likely to occur, and blocking is less likely to occur when the film is wound into a roll.

[0022] In the present invention, as a preferred condition of the PET film, a corona treatment is preferred as a method for making the dynamic contact angle of diiodomethane 26.0° or more.

[0023] A high dynamic contact angle is preferable, but since the PET film may be treated on surfaces other than the intended surface or may be damaged by heat during the treatment process, the dynamic contact angle is set to a value within the allowable range of other physical properties.

[0024] Corona treatment is a method of treating the surface of PET with plasma by generating a discharge in the atmosphere. For example, the corona treatment method shown in Figure 2 can be used to corona treat a long PET film. A high AC voltage of 10 to 60 kHz is applied to an electrode 4 in the atmosphere to cause a discharge. The PET film 6 to be treated runs over a dielectric-coated roll 5 covered with silicone rubber or the like, and is treated with the plasma generated between the dielectric-coated roll 5 and the electrode 4.

[0025] The treatment degree, which is related to the dynamic contact angle of diiodomethane, can be adjusted by adjusting the distance between the electrode 4 and the dielectric-coated roll 5, the power applied to the electrode 4 and the dielectric-coated roll 5, and the running speed of the PET film 6.

[0026] Generally, the gap between the electrode 4 and the dielectric-coated roll 5 is set to 5 mm or less. If the gap is too large, discharge becomes difficult. If the gap is narrowed, the treatment degree increases and the dynamic contact angle of diiodomethane increases. A narrow gap is preferable, but if it is too narrow, the electrode will deform and the film will flutter, causing contact between the film and the electrode and scratches.

[0027] Increasing the power applied to the electrode 4 and the dielectric-coated roll 5 increases the degree of treatment and the dynamic contact angle of diiodomethane. Simply increasing the power can cause abnormal discharge or the electrodes to overheat and deform, so the number and shape of the electrodes must be selected appropriately.

[0028] Furthermore, when the treatment is performed with the same power, if the traveling speed of the PET film 6 is slowed down, the treatment degree increases and the dynamic contact angle of diiodomethane increases.

[0029] Although it is possible to supply gas such as nitrogen or helium between the discharge electrodes to generate a discharge, it is preferable to use normal atmospheric air containing 78% nitrogen and 21% oxygen. To ensure stable processing, a fixed amount of atmospheric air with a stable temperature and humidity is blown through a filter.

[0030] Corona discharge converts some of the oxygen in the air into ozone, which changes the surface of the PET film. Free release of ozone can have an adverse effect on the human body and also on the degree of surface treatment, so it is preferable to surround the corona treatment area and exhaust the air uniformly.

[0031] The corona treatment can be carried out on a PET film that has already been formed using a rewinder equipped with a corona treatment device or a slitter that changes the width of the film, but it is preferable to carry out the corona treatment on the PET film during film formation.

[0032] That is, it is preferable to melt the PET resin, extrude it through a T-die, stretch it in the MD (film running direction), stretch it in the TD (film width direction), and then treat it through a corona treatment machine.

[0033] By carrying out the treatment in the same step, not only can the treatment be carried out easily, but also the corona treatment can be carried out in a fresher state on the surface of the PET film, which is preferable.

[0034] Furthermore, the transparent gas barrier film of the present invention is a transparent gas barrier film characterized by laminating an inorganic layer on the above-mentioned PET film. That is, the transparent gas barrier film of the present invention is a transparent gas barrier film comprising a polyethylene terephthalate film having a modified surface in which the dynamic contact angle measured 1 second after the dropping of diiodomethane is 26.0° or more, and an inorganic layer vapor-deposited on the modified surface.

[0035] As a method for laminating an inorganic layer on the PET film of the present invention, a dry process using a vacuum is suitable. Among them, a vapor deposition method is suitable. The vapor deposition method allows for laminating an inorganic layer over a large area at high speed.

[0036] The deposition method can be any of the following: a resistance heating method in which the deposition material is evaporated using a resistance heating boat; an induction heating method in which the deposition material is placed in a carbon crucible and heated by applying a high-frequency electromagnetic field; and an electron beam heating method in which the deposition material is heated using an electron gun.

[0037] 3 is a schematic diagram of an electron beam heating type vapor deposition apparatus. A process for laminating an inorganic layer will be described, but the present invention is not limited to this.

[0038] A PET film having a modified surface with a dynamic contact angle of 26.0° or more with diiodomethane according to the present invention (hereinafter referred to as the present PET film) is prepared on the unwinding roll 7 of the vapor deposition device.

[0039] The present PET film 8 is unwound from the unwinding roll 7 and its surface is treated by a plasma treatment device 9. The plasma treatment device 9 has electrodes and is designed to allow gas to be introduced between the electrodes and the present PET film 8. A direct current or alternating current voltage is applied to the electrodes to cause a discharge and generate plasma. The surface is treated by this plasma. The purpose of the plasma treatment is to remove moisture and other substances that adhere to the present PET film 8 when it is stored in the atmosphere. For this purpose, a rare gas such as argon is preferably introduced.

[0040] After passing through the plasma treatment device 9, the present PET film 8 is transferred to a coating roll 10 cooled to −20° C. An electron beam 12 emitted from an electron gun 11 heats a deposition material 13 placed in a crucible, evaporating the material, and an inorganic layer is laminated on the modified surface of the present PET film 8.

[0041] A transparent gas barrier film (hereinafter referred to as the transparent gas barrier film of the present invention) having an inorganic layer laminated on the modified surface of the PET film 8 of the present invention has electrons charged on the surface of the transparent gas barrier film of the present invention removed by a static eliminator 14 before leaving the coating roll 10. The transparent gas barrier film of the present invention is detached from the coating roll 10 and taken up onto a take-up roll 17, but before that the film thickness or film thickness and composition of the laminated inorganic layer are measured using an optical film thickness meter 15, a fluorescent X-ray film thickness meter 16, or both. In order to achieve the target film thickness or film thickness and composition, the measured values ​​are fed back to the electron gun 11, and the intensity and scanning of the electron beam 12 are adjusted to the target values.

[0042] The inorganic layer of the transparent gas barrier film of the present invention preferably has a thickness of 5 nm to 30 nm. If it is too thin, the film will not be uniform and the barrier properties will not be maintained. If it is too thick, the inorganic layer will crack when the transparent gas barrier film of the present invention is deformed, resulting in a decrease in the barrier properties.

[0043] As described above, aluminum oxide, silicon oxide, and mixtures thereof are suitable for the inorganic layer of the transparent gas barrier film of the present invention. A mixture of aluminum oxide and silicon oxide is particularly suitable. In particular, in the mixture of aluminum oxide and silicon oxide, the aluminum oxide content is preferably 20 to 60 mass %. When the aluminum oxide content is 20 mass % or more, the barrier properties are improved. When the content is 60 mass % or less, the inorganic layer does not become too hard, and it is possible to prevent the inorganic layer from cracking and the barrier properties from decreasing when the transparent gas barrier film is deformed.

[0044] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The physical properties and characteristics in the examples were measured or evaluated by the following methods.

[0045] (1) Dynamic Contact Angle The dynamic contact angle was measured in a room adjusted to a room temperature of 23°C and a humidity of 50%. The measuring device used was a DROP SHAPE ANALYER-DSA100 manufactured by KRUESS. Purified water from Trusco Nakayama Corporation was used. Special grade diiodomethane from Nacalai Tesque Inc. was used.

[0046] For the measurement, a droplet of 0.8 μL of diiodomethane was made using a 0.5 mm diameter PTFE needle and dropped onto the surface of the PET film. After 1 second, an image of the droplet was taken and the dynamic contact angle was calculated using the θ / 2 method (width-height method). Measurements were made at 10 points, and the average value was used as the dynamic contact angle of the sample.

[0047] (2) Water Vapor Transmission Rate (WVTR) Water vapor transmission rate (WVTR) was measured in accordance with JIS K7129 Method B using a water vapor transmission rate measuring device (MOCON Corporation, USA, PRMATRAN-W3 / 34G) under measurement conditions of a temperature of 40°C and a humidity of 90% RH. (Example 1) PET resin was melted, extruded through a T-die, stretched in the MD, and then stretched in the TD, after which the PET film surface was treated with a corona treatment device. The dynamic contact angle of diiodomethane was confirmed, and the distance between the PET film and the electrode was adjusted, and the power applied to the electrode was adjusted to achieve a value of 26.0°. After the corona treatment, the PET film was wound up on a take-up roll as a roll film. The film thickness of the PET film was 12 μm.

[0048] The wound PET film was slit to a width suitable for processing in an electron beam deposition apparatus, and the PET film was placed in an electron beam deposition apparatus as shown in Figure 3. Alumina and silica with a purity of 99% or higher were placed in a crucible. After evacuating the deposition apparatus, the placed PET film was withdrawn from the unwinding roll and passed through an argon gas plasma. An alumina and silica mixed film was laminated as an inorganic layer on a coating roll cooled to -20°C. After laminating the alumina-silica film, the film was neutralized and peeled from the coating roll. The film thickness and composition were measured using a fluorescent X-ray film thickness meter. The electron gun was controlled to achieve a film thickness of 13 nm and an aluminum oxide content of 45% by mass. After winding the transparent gas barrier film onto the winding roll and opening it to the atmosphere, a sample was taken of the film, and the WVTR was measured. The results are shown in Table 1. Furthermore, the remaining PET film remaining on the unwinding roll was sampled to confirm the dynamic contact angle, and the dynamic contact angle of diiodomethane was measured. The results are shown in Table 1.

[0049] (Examples 2 to 10) PET films were produced in the same manner as in Example 1. The power conditions of the corona treatment device and the film speed were changed to obtain PET films with the dynamic contact angles shown in Table 1. An alumina-silica inorganic layer was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 1.

[0050] (Example 11) A PET film was produced in the same manner as in Example 1. The power conditions of the corona treater and the film speed were changed to obtain PET films with the dynamic contact angles shown in Table 1. Furthermore, a transparent gas barrier film was produced under the same conditions as in Example 1, except that instead of laminating an inorganic layer of alumina-silica, only alumina with a purity of 99% or higher was laminated, and the WVTR was measured. The results are shown in Table 1.

[0051] (Comparative Examples 1 to 5) PET films were produced in the same manner as in Example 1. The power conditions of the corona treatment device and the film speed were changed to obtain PET films with the dynamic contact angles shown in Table 1. An alumina-silica inorganic layer was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 1.

[0052] Comparative Example 6 A PET film was produced in the same manner as in Example 1. However, the corona treatment device was stopped from operating. An inorganic layer of alumina-silica was laminated in the same manner as in Example 1, and the WVTR was measured. The results are shown in Table 1.

[0053] Comparative Example 7 A transparent gas barrier film was produced under the same conditions as in Example 1 of the present application using a PET film that had been subjected to a corona treatment under the same conditions as in Example 1 of JP 2012-238491 A, and the WVTR was measured. That is, a PET film was produced in the same manner as in Example 1 of the present application, and then the upper surface of the film was subjected to a corona discharge treatment with an E value of 30 and wound up to obtain a polyester film. The results are shown in Table 1. The E value is the corona discharge treatment intensity, and is a function of the applied voltage (Vp), applied current (Ip), treatment speed (S), and treatment width (Wt), where E = (Vp × Ip) / (S × Wt).

[0054] Comparative Example 8 A transparent gas barrier film was produced under the same conditions as in Example 1 of the present application using a PET film that had been subjected to a corona treatment under the same conditions as in Example 3 of JP 2012-238491 A, and the WVTR was measured. That is, a PET film was produced in the same manner as in Example 1 of the present application, and then the upper surface of the film was subjected to a corona discharge treatment with an E value of 60 and taken up to obtain a polyester film. The results are shown in Table 1.

[0055]

[0056] As the results in Table 1 show, in Examples 1 to 11, the dynamic contact angle of diiodomethane was 26.0° or more, and therefore the WVTR of the transparent gas barrier films using those PET films was small. This is thought to be because a dense inorganic layer could be formed, and as can be seen from a comparison between Examples 6 and 11, this effect was particularly remarkable when an alumina-silica inorganic layer was formed. In contrast, in Comparative Examples 1 to 8, the dynamic contact angle of diiodomethane was smaller than 26.0°, and therefore the WVTR of the transparent gas barrier films using those PET films was large.

[0057] The present invention can provide a PET film that is a substrate for producing a transparent gas barrier film that has excellent properties as a gas barrier material, and can also provide a transparent gas barrier film that uses the substrate and has excellent properties as a gas barrier material.

[0058] 1: Substrate (PET film) 2: Droplet (diiodomethane, etc.) 3: Tangent line 4: Electrode 5: Dielectric-coated roll 6: PET film 7: Unwinding roll 8: PET film of the present invention 9: Plasma treatment device 10: Coating roll 11: Electron gun 12: Electron beam 13: Vapor deposition material 14: Static neutralizer 15: Optical film thickness gauge 16: Fluorescent X-ray film thickness gauge 17: Winding roll

Claims

1. A polyethylene terephthalate film for deposition used in applications involving the deposition of an inorganic layer, the polyethylene terephthalate film having a modified surface on the side on which the inorganic layer is to be deposited, the dynamic contact angle of the modified surface being 26.0° or greater, measured 1 second after the dropping of diiodomethane onto the modified surface.

2. The polyethylene terephthalate film for deposition according to claim 1, wherein the modified surface is formed by corona treatment.

3. A transparent gas barrier film comprising: a polyethylene terephthalate film having a modified surface in which the dynamic contact angle measured 1 second after diiodomethane is dropped is 26.0° or more; and an inorganic layer vapor-deposited on the modified surface.

4. The transparent gas barrier film according to claim 3, wherein the modified surface is formed by corona treatment.

5. The transparent gas barrier film according to claim 3 or 4, wherein the inorganic layer contains aluminum oxide and silicon oxide.

Citation Information

Patent Citations

  • Vapor deposited film

    JP1987077453A

  • Polyester-based film for vapor deposition

    JP1991126860A

  • Gas barrier laminated film and its manufacturing method

    JP2007210208A

  • Vapor-deposited polyester film

    JP2017065264A