Grain-oriented electrical steel sheet and method for forming insulating coating film
The grain-oriented electrical steel sheet with a crystalline metal phosphate intermediate layer and tension coating layer addresses the issues of forsterite-based coatings by ensuring excellent adhesion and magnetic properties, reducing iron loss, and maintaining the transformer's space factor, thus improving its performance and efficiency.
Patent Information
- Application Number
- PCT/JP2024/014841
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
Grain-oriented electrical steel sheets with forsterite-based coatings hinder domain wall movement, leading to increased iron loss, and existing methods for removing or replacing these coatings are costly and inefficient, while also compromising magnetic properties and adhesion.
A grain-oriented electrical steel sheet with an insulating coating comprising a crystalline metal phosphate intermediate layer and a tension coating layer, formed through a chemical conversion treatment with a specific ion ratio, ensuring excellent adhesion and magnetic properties without reducing the transformer's space factor.
The solution achieves improved adhesion and magnetic properties while maintaining the transformer's space factor, reducing iron loss and enhancing corrosion resistance and heat resistance.
Smart Images

Figure JP2024014841_17102024_PF_FP_ABST
Abstract
Description
Grain-oriented electrical steel sheet and method for forming insulating coating
[0001] The present invention relates to a grain-oriented electrical steel sheet and a method for forming an insulating coating. This application claims priority to Japanese Patent Application No. 2023-064826, filed on April 12, 2023, the contents of which are incorporated herein by reference.
[0002] Grain-oriented electrical steel sheets are primarily used in transformers. Transformers are continuously excited over a long period of time, from installation to disposal, and continue to generate energy loss. Therefore, the energy loss during magnetization with AC, i.e., core loss, is a major indicator that determines the performance of a transformer.
[0003] To reduce the iron loss of grain-oriented electrical steel sheets, many technologies have been developed to date, including (a) increasing the concentration in the {110}<001> orientation (Goss orientation), (b) increasing the content of solid solution elements such as Si to increase the electrical resistance of the steel sheet, or (c) reducing the thickness of the electrical steel sheet.
[0004] Furthermore, applying tension to steel sheets is effective in reducing iron loss. Forming a coating made of a material with a smaller thermal expansion coefficient than the steel sheet at high temperatures on the steel sheet surface is an effective means for reducing iron loss. A forsterite-based coating (inorganic coating) with excellent coating adhesion is produced by the reaction of oxides on the steel sheet surface with an annealing separator during the finish annealing process of electrical steel sheets. This coating can apply tension to steel sheets.
[0005] Furthermore, for example, the method disclosed in Patent Document 1, in which a coating liquid mainly composed of colloidal silica and phosphate is baked onto the surface of a steel sheet to form an insulating coating, is an effective method for reducing iron loss because it is highly effective in applying tension to the steel sheet. Therefore, a common method for producing grain-oriented electrical steel sheets is to leave the forsterite-based coating formed in the final annealing step and then apply an insulating coating mainly composed of phosphate on top of it.
[0006] However, in recent years, there has been an increasing demand for smaller and higher-performance transformers. To achieve this, grain-oriented electrical steel sheets are required to have excellent high-field iron loss characteristics, even at high magnetic flux densities. At the same time, it has become clear that forsterite-based coatings hinder domain wall movement, adversely affecting iron loss. In grain-oriented electrical steel sheets, magnetic domains undergo domain wall movement under an AC magnetic field. Smooth and rapid domain wall movement is effective in reducing iron loss. However, forsterite-based coatings are nonmagnetic and have an uneven structure at the steel sheet / coating interface. This uneven structure is thought to hinder domain wall movement and adversely affect iron loss. Therefore, methods for removing inorganic coatings using mechanical means such as polishing or chemical means such as pickling have been studied as a means of improving high-field iron loss. Other technologies being researched include a technology for producing grain-oriented electrical steel sheets that do not have inorganic coatings by preventing the formation of inorganic coatings during high-temperature finish annealing, and a technology for making the steel sheet surface mirror-finished (in other words, a technology for magnetically smoothing the steel sheet surface).
[0007] As a technique for preventing the formation of inorganic coatings, for example, Patent Document 2 discloses a technique in which the steel sheet is subjected to normal finish annealing, pickled to remove surface deposits, and then chemically or electrolytically polished to a mirror finish on the surface. It has been found that forming a tensioned insulating coating on the surface of an inorganic-coating-free grain-oriented electrical steel sheet obtained by such a known method can provide an even more excellent iron loss improvement effect. Furthermore, tensioned insulating coatings can impart various properties, such as corrosion resistance, heat resistance, and slipperiness, in addition to improving iron loss.
[0008] However, inorganic coatings not only provide insulation but also function as intermediate layers that ensure adhesion when forming tension coatings (tension-applying insulating coatings). In other words, inorganic coatings are formed deep within the steel sheet, providing excellent adhesion to the metal steel sheet. Therefore, when a tension-applying coating (tension coating) containing colloidal silica, phosphate, or the like as a main component is formed on the surface of an inorganic coating, excellent coating adhesion is achieved. However, because bonding between metal and oxide is generally difficult, it has been difficult to ensure sufficient adhesion between the tension coating and the steel sheet surface in the absence of an inorganic coating. Therefore, when forming a tension coating on grain-oriented electrical steel sheets that do not have an inorganic coating, the provision of a layer that serves as an intermediate layer for the inorganic coating has been considered.
[0009] For example, Patent Document 3 discloses that grain-oriented electrical steel sheets that do not have an inorganic coating are annealed in a weakly reducing atmosphere to selectively thermally oxidize silicon that is inevitably contained in the silicon steel sheets, thereby forming SiO on the steel sheet surface. 2 Patent Document 4 discloses a technique for forming a tension-applying insulating coating on the surface of a grain-oriented electrical steel sheet that does not have an inorganic coating by subjecting the sheet to an anodic electrolysis treatment in a silicate solution. 2 After the layers are formed, a tensioned insulating coating is applied.
[0010] However, the technique disclosed in Patent Document 3 requires the preparation of annealing equipment capable of controlling the atmosphere in order to perform annealing in a weakly reducing atmosphere, which results in a problem of processing costs. Also, in the technique disclosed in Patent Document 4, anodic electrolysis is performed in a silicate aqueous solution, thereby forming SiO 2 which maintains sufficient adhesion with the tension-imparting insulating coating. 2 In order to obtain such a layer on the surface of the steel sheet, it is necessary to prepare new electrolytic treatment equipment, which increases the treatment cost.
[0011] In contrast, Patent Document 5 discloses a grain-oriented electrical steel sheet having a base steel sheet and an insulating coating formed on the surface of the base steel sheet, the insulating coating being formed on the base steel sheet side, an intermediate layer containing a crystalline metal phosphate, and a tensile coating layer formed on the surface side of the insulating coating. In this grain-oriented electrical steel sheet, the intermediate layer can be formed by chemical conversion treatment.
[0012] Furthermore, Patent Document 6 relates to a method for manufacturing a grain-oriented silicon steel sheet, and describes a method for forming a tension-applying insulating film by applying 0.1 g / m2 of a secondarily recrystallized grain-oriented silicon steel sheet to one side of the steel sheet prior to forming a tension-applying insulating film. 2 10g / m or more 2 The following method for forming a coating mainly composed of zinc phosphate is disclosed.
[0013] Japanese Unexamined Patent Publication No. 48-039338 Japanese Unexamined Patent Application No. 49-96920 Unexamined Japanese Patent Application No. 6-184762 Unexamined Japanese Patent Publication No. 11-209891 International Publication No. 2022 / 215710 Unexamined Japanese Patent Application No. 2005-139481
[0014] However, as a result of the inventors' investigation of the conventional techniques described in Patent Documents 5 and 6, it was found that in grain-oriented electrical steel sheets obtained by conventional methods, improving adhesion with a coating (intermediate layer) mainly composed of metal phosphate may result in a deterioration of magnetic properties. Further investigation into this point revealed that the cause of the deterioration of magnetic properties is that when the intermediate layer is formed, i.e., during chemical conversion treatment, the surface of the base material is etched simultaneously with the precipitation of phosphate crystals, forming an uneven structure at the interface between the base material and the intermediate layer, which results in the suppression of the flow of magnetic flux in the base material.
[0015] Therefore, an object of the present invention is to provide a grain-oriented electrical steel sheet and a method for forming an insulating coating that has excellent adhesion and magnetic properties of a tensile coating and does not reduce the space factor of a transformer (core).
[0016] The inventors have discovered that when providing a layer containing a metal phosphate as an intermediate layer to improve adhesion between the base steel sheet and the tensile coating layer, the interface between the intermediate layer and the base steel can be smoothed by adjusting the ratio of metal ions, phosphate ions, and nitrate ions in the chemical conversion treatment solution within a specific range, and as a result, a grain-oriented electrical steel sheet can be obtained that has excellent adhesion and magnetic properties of the tensile coating and does not reduce the space factor of the transformer (core).
[0017] The present invention has been made in view of the above findings. The gist of one aspect of the present invention is as follows.
[0018] [1] A grain-oriented electrical steel sheet according to one aspect of the present invention comprises a base steel sheet and an insulating coating formed on a surface of the base steel sheet, wherein the insulating coating comprises: an intermediate layer formed on the base steel sheet side and containing a crystalline metal phosphate; and a tensile coating layer formed on the surface side of the insulating coating, wherein, in a cross section along the thickness direction of the intermediate layer, when the interface between the base steel sheet and the intermediate layer is observed at 5000x magnification with a scanning electron microscope, the ratio of the interface length L to the observed image width W is 100.0 to 120.0%. [2] In the grain-oriented electrical steel sheet according to [1] above, the tensile coating layer may contain a metal phosphate and silica. [3] A method of forming an insulating coating according to one aspect of the present invention is a method of forming the insulating coating provided in the grain-oriented electrical steel sheet according to [1] above, comprising: 2 O 3a finish annealing process in which an annealing separator containing 10 to 100 mass % of the above is applied to the steel sheet, dried, and then finish annealed; an annealing separator removing process in which excess annealing separator is removed from the steel sheet after the finish annealing process; a pickling process in which the steel sheet after the annealing separator removing process is pickled with 0.1 to 5 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid for 1 to 20 seconds; an immersion process in which the steel sheet after the pickling process is immersed in a treatment solution containing a metal phosphate, an oxidizing agent, and iron ions; and a drying process in which the steel sheet after the immersion process is pulled out of the treatment solution, excess treatment solution is removed, and then the steel sheet is dried. and a tensile coating layer forming step of applying a coating liquid containing a metal phosphate and colloidal silica, and having a total concentration of the metal phosphate and colloidal silica of 10 to 40 mass % in terms of solids content, to the steel sheet after the drying step, drying the coating liquid, and then maintaining the steel sheet at a temperature of 700 to 950°C for 10 to 120 seconds, wherein the treatment liquid has a metal ion concentration of 1.0 to 10.0 g / L, a phosphate ion concentration of 2.0 to 25.0 g / L, a nitrate ion concentration of 2.0 to 40.0 g / L, and an iron ion concentration of 1.0 to 20.0 g / L, a ratio of the phosphate ion concentration to the metal ion concentration of 1.5 to 5.0, and a ratio of the nitrate ion concentration to the phosphate ion concentration of 0.5 to 10.0. [4] In the method for forming an insulating coating described in [3] above, in the immersion step, the steel sheet after the pickling step may be immersed for 2 to 60 seconds in the treatment solution at a solution temperature of 20 to 85° C. [5] In the method for forming an insulating coating described in [3] above, the nitrate ion concentration may be 2.0 to 25.0 g / L.
[0019] According to one aspect of the present invention, it is possible to provide a grain-oriented electrical steel sheet and an insulating coating forming method that have excellent adhesion and magnetic properties of a tensile coating and do not reduce the space factor of a transformer (core).
[0020] 1 is a schematic diagram illustrating a method for determining an unevenness index according to an embodiment of the present invention;
[0021] A grain-oriented electrical steel sheet according to an embodiment of the present invention (the grain-oriented electrical steel sheet according to the present embodiment) and a method for manufacturing the grain-oriented electrical steel sheet according to the present embodiment, including a method for forming an insulating coating provided on the grain-oriented electrical steel sheet according to the present embodiment, will be described. First, the grain-oriented electrical steel sheet according to the present embodiment will be described.
[0022] As shown in FIG. 1 , the grain-oriented electrical steel sheet 100 according to this embodiment has a base steel sheet 1 and an insulating coating 2 formed on the surface of the base steel sheet 1 .
[0023] The grain-oriented electrical steel sheet 100 according to this embodiment does not substantially have a forsterite-based coating on the surface of the base steel sheet 1. In other words, in this embodiment, a forsterite-based coating is not intentionally formed on the surface of the base steel sheet 1, but the coating amount of the forsterite-based coating is 1 g / m 2 The presence of the insulating coating 2 is acceptable if the content is less than 0 to 1 g / m. 2 The forsterite-based coating may be formed of the above.
[0024] The insulating coating 2 has a tensile coating layer 22 formed on the surface side of the insulating coating 2 (i.e., the surface side of the grain-oriented electrical steel sheet 100), and an intermediate layer 21 formed on the base steel sheet 1 side and containing a crystalline metal phosphate.
[0025] When the interface between the base steel sheet and the intermediate layer is observed at 5000x magnification with a scanning electron microscope in a cross section along the thickness direction of the intermediate layer, the ratio of the interface length L to the observed image width W (irregularity index) of the intermediate layer 21 is 100 to 120%. Each component of the grain-oriented electrical steel sheet 100 will be described below.
[0026] <Base Steel Sheet> (Chemical Composition) The grain-oriented electrical steel sheet 100 according to this embodiment is significantly characterized by the structure of the insulating coating 2 formed on the surface of the base steel sheet 1, and the base steel sheet 1 included in the grain-oriented electrical steel sheet 100 is not limited in terms of its chemical composition. However, in order to obtain the properties generally required of a grain-oriented electrical steel sheet, it is preferable that the chemical components include the following: In this embodiment, % relating to the chemical components is % by mass unless otherwise specified.
[0027] C: 0.010% or less C (carbon) is an element effective for controlling the structure of steel sheets in the manufacturing process up to the completion of the decarburization annealing process. However, if the C content exceeds 0.010%, the magnetic properties of the finished grain-oriented electrical steel sheet deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the C content is preferably 0.010% or less. The C content is more preferably 0.005% or less. Although a lower C content is preferable, reducing the C content to less than 0.0001% saturates the effect of structural control and simply increases manufacturing costs. Therefore, the C content may be 0.0001% or more.
[0028] Si: 2.50 to 4.00% Si (silicon) is an element that increases the electrical resistance of grain-oriented electrical steel sheets and improves their iron loss characteristics. If the Si content is less than 2.50%, a sufficient eddy current loss reduction effect cannot be obtained. Therefore, the Si content is preferably 2.50% or more. The Si content is more preferably 2.70% or more, and even more preferably 3.00% or more. On the other hand, if the Si content exceeds 4.00%, the grain-oriented electrical steel sheets become embrittled and their threading properties deteriorate significantly. Furthermore, the workability of the grain-oriented electrical steel sheets decreases, and the steel sheets may break during rolling. Therefore, the Si content is preferably 4.00% or less. The Si content is more preferably 3.80% or less, and even more preferably 3.70% or less.
[0029] Mn: 0.01 to 0.50% Mn (manganese) is an element that combines with S to form MnS during the manufacturing process. This precipitate functions as an inhibitor (a suppressor of normal grain growth) and induces secondary recrystallization in the steel. Mn also enhances the hot workability of the steel. If the Mn content is less than 0.01%, the above-mentioned effects cannot be fully achieved. Therefore, the Mn content is preferably 0.01% or more. The Mn content is more preferably 0.02% or more. On the other hand, if the Mn content exceeds 0.50%, secondary recrystallization does not occur and the magnetic properties of the steel deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Mn content is preferably 0.50% or less. The Mn content is more preferably 0.20% or less, and even more preferably 0.10% or less.
[0030] N: 0.010% or less N (nitrogen) is an element that bonds with Al during the manufacturing process to form AlN, which functions as an inhibitor. However, if the N content exceeds 0.010%, excessive inhibitors remain in the grain-oriented electrical steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the N content is preferably 0.010% or less. The N content is more preferably 0.008% or less. On the other hand, the lower limit of the N content is not particularly specified, but reducing the N content to less than 0.001% only increases manufacturing costs. Therefore, the N content may be 0.001% or more.
[0031] Sol. Al: 0.020% or less Sol. Al (acid-soluble aluminum) is an element that bonds with N to form AlN, which functions as an inhibitor, during the manufacturing process of grain-oriented electrical steel sheets. However, if the sol. Al content of the base steel sheet exceeds 0.020%, excessive inhibitors remain in the base steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the sol. Al content is preferably 0.020% or less. The sol. Al content is more preferably 0.010% or less, and even more preferably less than 0.001%. There is no particular restriction on the lower limit of the sol. Al content, but reducing it to less than 0.0001% only increases manufacturing costs. Therefore, the sol. Al content may be 0.0001% or more.
[0032] S: 0.010% or less S (sulfur) is an element that combines with Mn during the manufacturing process to form MnS, which functions as an inhibitor. However, if the S content exceeds 0.010%, the magnetic properties will be reduced due to the remaining inhibitor. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the S content is preferably 0.010% or less. The S content in the grain-oriented electrical steel sheet is preferably as low as possible. For example, less than 0.001%. However, reducing the S content in the grain-oriented electrical steel sheet to less than 0.0001% will only increase the manufacturing cost. Therefore, the S content in the grain-oriented electrical steel sheet may be 0.0001% or more.
[0033] Balance: Fe and impurities The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment may contain the above-mentioned elements, with the balance being Fe and impurities. However, for the purpose of improving magnetic properties, etc., Sn, Cu, Se, and Sb may also be contained in the ranges shown below. Furthermore, even if other elements, such as W, Nb, Ti, Ni, Co, V, Cr, and Mo, are contained in a total of 1.0% or less, the effects of the grain-oriented electrical steel sheet according to this embodiment are not impaired. Here, impurities refer to elements that are mixed in from raw materials such as ore, scrap, or the manufacturing environment during industrial production of the base steel sheet, and are allowed to be contained in amounts that do not adversely affect the function of the grain-oriented electrical steel sheet according to this embodiment.
[0034] Sn: 0 to 0.50% Sn (tin) is an element that contributes to improving magnetic properties through primary crystal structure control. To obtain the effect of improving magnetic properties, the Sn content is preferably 0.01% or more. The Sn content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Sn content exceeds 0.50%, secondary recrystallization becomes unstable and magnetic properties deteriorate. Therefore, the Sn content is preferably 0.50% or less. The Sn content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0035] Cu: 0 to 0.50% Cu (copper) is an element that contributes to increasing the Goss orientation occupancy rate in the secondary recrystallized structure. To achieve the above effect, the Cu content is preferably 0.01% or more. The Cu content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Cu content exceeds 0.50%, the steel sheet becomes embrittled during hot rolling. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Cu content is preferably 0.50% or less. The Cu content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0036] Se: 0 to 0.020% Se (selenium) is an element that has the effect of improving magnetic properties. When Se is contained, the Se content is preferably 0.001% or more to effectively exhibit the effect of improving magnetic properties. The Se content is more preferably 0.003% or more, and even more preferably 0.006% or more. On the other hand, if the Se content exceeds 0.020%, the adhesion of the coating deteriorates. Therefore, the Se content is preferably 0.020% or less. The Se content is more preferably 0.015% or less, and even more preferably 0.010% or less.
[0037] Sb: 0 to 0.50% Sb (antimony) is an element that has the effect of improving magnetic properties. When Sb is contained, the Sb content is preferably 0.005% or more to effectively exhibit the effect of improving magnetic properties. The Sb content is more preferably 0.01% or more, and even more preferably 0.02% or more. On the other hand, if the Sb content exceeds 0.50%, the adhesion of the coating significantly deteriorates. Therefore, the Sb content is preferably 0.50% or less. The Sb content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0038] As described above, the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet in this embodiment is, for example, one that contains the above-mentioned elements with the balance being Fe and impurities.
[0039] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment can be measured using a known ICP atomic emission spectroscopy. However, if an insulating coating is formed on the surface, it must be removed before measurement. The removal can be achieved by immersing the sample in a highly concentrated alkaline solution (e.g., a 30% sodium hydroxide solution heated to 85°C) for 20 minutes or more. Peeling can be determined visually. For small samples, removal can also be achieved by surface grinding.
[0040] <Insulating coating> The grain-oriented electrical steel sheet 100 according to this embodiment has an insulating coating 2 formed on the surface of a base steel sheet 1. The insulating coating 2 has a structure in which an intermediate layer 21 and a tensile coating layer 22 are laminated in this order from the base steel sheet 1 side.
[0041] (Intermediate Layer) As described above, grain-oriented electrical steel sheets generally have a forsterite-based coating formed in the final annealing process and an insulating coating (tensile insulating coating) formed thereon. However, in recent years, it has become clear that this forsterite-based coating hinders the movement of domain walls and adversely affects iron loss. Therefore, grain-oriented electrical steel sheets without a forsterite-based coating have been studied to further improve magnetic properties. However, without a forsterite-based coating, it is difficult to ensure sufficient adhesion between the tensile insulating coating and the surface of the base steel sheet.
[0042] In the grain-oriented electrical steel sheet 100 according to this embodiment, an intermediate layer 21 containing a crystalline metal phosphate is formed between the base steel sheet 1 and the tensile coating layer 2, thereby improving the adhesion between the base steel sheet 1 and the tensile coating layer 22 via the intermediate layer 21. This is because, when the intermediate layer 21 contains a crystalline metal phosphate, the tensile coating formed thereon (which becomes the tensile coating layer 22 after formation) also contains a metal phosphate, resulting in high affinity and excellent adhesion between the intermediate layer and the tensile coating layer. Furthermore, when the intermediate layer 1 is formed by immersion in a treatment solution containing a metal phosphate, as described below, it can be formed on the surface of the base steel sheet 1 by utilizing a chemical reaction, and adhesion between the intermediate layer 21 and the base steel sheet 1 can also be ensured.
[0043] If the intermediate layer 21 does not contain a crystalline metal phosphate, the above-mentioned effect cannot be obtained. The proportion of the crystalline metal phosphate in the intermediate layer 21 is preferably 80 mass % or more, and may be 100 mass %. In terms of adhesion, the metal phosphate is preferably one of zinc phosphate, manganese phosphate, zinc calcium phosphate, and iron manganese phosphate. The intermediate layer 21 may contain oxides and elements such as Fe and Si diffused from the base steel sheet 1 as the remainder of the metal phosphate.
[0044] The inventors of the present invention have investigated the adhesion and magnetic properties of intermediate layers 21 that use metal phosphates, and have found that using an intermediate layer primarily made of metal phosphates to improve adhesion between the base material and the insulating coating can sometimes result in a deterioration of the magnetic properties of the grain-oriented electrical steel sheet. Further investigation into this point has revealed that the cause of the deterioration of magnetic properties is that, during the formation of the intermediate layer, i.e., during chemical conversion treatment, the surface of the base steel sheet is etched simultaneously with the precipitation of phosphate crystals, forming an uneven structure at the interface between the base steel sheet and the intermediate layer, which in turn obstructs the flow of magnetic flux through the base steel sheet.
[0045] Furthermore, as a result of the inventor's investigations, it was found that the unevenness index also affects the space factor. The unevenness index increases because the chemical conversion treatment solution used to form the intermediate layer etches the surface of the steel sheet, but at the same time, the fine unevenness on the surface side of the intermediate layer 21 also increases. As a result, the fine unevenness of the tensile coating layer 22 formed above the intermediate layer 21 also increases, resulting in a decrease in the space factor.
[0046] Therefore, in the grain-oriented electrical steel sheet according to this embodiment, deterioration of the magnetic properties is suppressed while maintaining good adhesion and space factor by reducing the degree of unevenness (irregularity level) at the interface between the base steel sheet 1 and the intermediate layer 21. Specifically, in the grain-oriented electrical steel sheet according to this embodiment, when the interface between the base steel sheet 1 and the intermediate layer 21 is observed at 5000x magnification with a scanning electron microscope (SEM) in a cross section along the thickness direction of the intermediate layer 21, L / W, which is the ratio of the interface length L to the observed image width W (irregularity index), is 100.0 to 120.0%.
[0047] FIG. 2 is a schematic diagram illustrating how to determine the unevenness index L / W, and is a cross-sectional schematic diagram along the thickness direction of the intermediate layer 21. First, as shown in FIG. 2 , the cross section is observed at 5000x magnification using an SEM to obtain an observation image including the interface between the base steel sheet 1 and the intermediate layer 21. Then, the distance between two points on the observation image, which are connected by a straight line between both ends of the interface between the base steel sheet 1 and the intermediate layer 21, is defined as the observation image width W, and the actual interface path (i.e., the curved path tracing the actual interface) between both ends of the interface is defined as the interface length L, and the unevenness index L / W (%) is calculated. This unevenness index L / W is an index of the degree of unevenness at the interface; a smaller unevenness index L / W indicates a smaller degree of unevenness and superior interface smoothing. Note that the degree of observed unevenness varies depending on the magnification of the SEM observation. Therefore, the magnification of the SEM observation is set to a range suitable for observing the interface, which is 5000x in this embodiment. Of the cross sections of the grain-oriented electrical steel sheet, the cross section from which the observation image for measuring the unevenness index L / W is obtained is selected from a flat portion on the surface of the grain-oriented electrical steel sheet that is not subjected to surface defects or fine processing, and when calculating the unevenness index L / W, the average value of the values measured from the observation images at three locations is used.
[0048] The observed image width W and the interface length L can be easily determined by using an application system such as "Luzex AP" manufactured by Nireco Corporation for a cross-sectional image obtained by an electron microscope.
[0049] In this embodiment, the unevenness index L / W is 100.0 to 120.0%. If the unevenness index L / W exceeds 120.0%, the degree of unevenness at the interface increases, which may result in deterioration of magnetic properties. Therefore, the unevenness index is 120.0% or less. It is preferably less than 120.0%, more preferably 118.0% or less, even more preferably 115.0% or less, and even more preferably 110.0% or less. The lower limit of the unevenness index L / W is 100.0%. A case where the unevenness index L / W is 100.0% means that the observed image width W and the interface length L are the same, that is, the degree of unevenness is zero and the interface is smooth.
[0050] The thickness of the intermediate layer 21 is preferably 1.0 to 9.0 μm. If the average thickness of the intermediate layer 21 is less than 1.0 μm, the effect of improving the adhesion between the base steel sheet 1 and the insulating coating 2 via the intermediate layer 21 may not be sufficiently obtained. On the other hand, if the average thickness of the intermediate layer 21 exceeds 9.0 μm, the magnetic properties may deteriorate.
[0051] The thickness of the intermediate layer 21 can be determined by the following method. It is possible to determine the thickness of the intermediate layer 21 by measurement using a scanning electron microscope (SEM) and an energy dispersive elemental analyzer. That is, a sample consisting of the base steel sheet 1 and the insulating coating layer 2 is cut, and the polished cross section is observed with a scanning electron microscope at 5000x magnification to measure the thickness of the insulating coating layer 2. At this time, the energy dispersive elemental analyzer is used to determine the thickness of the intermediate layer 21 by calculating the thickness of the insulating coating layer 2, with the portion of the insulating coating layer 2 that contains Si being the tensile coating layer 22 and the portion that does not contain Si being the intermediate layer 21. Measurements are taken at five or more locations, and the average is taken as the thickness of the intermediate layer 21.
[0052] The intermediate layer 21 is formed at a different time from the tensile coating layer 22 formed thereon, but both the intermediate layer 21 and the tensile coating layer 22 function as the insulating coating 2 .
[0053] The mass proportion of the crystalline metal phosphate and the type of the metal phosphate in the intermediate layer 21 can be determined by measuring a cross section of the intermediate layer 21 along the thickness direction using a scanning electron microscope (SEM) and an energy dispersive elemental analyzer. Whether the metal phosphate in the intermediate layer 21 is a crystalline metal phosphate can be determined by X-ray crystal structure analysis.
[0054] The base steel sheet 1 and the insulating coating 2 can be distinguished by the presence or absence of phosphorus. Of the insulating coating 2, the intermediate layer 21 and the tensile coating layer 22 can be distinguished by the presence or absence of silicon.
[0055] (Tension Coating Layer) In the grain-oriented electrical steel sheet 100 according to this embodiment, a tensile coating is formed on the surface of the intermediate layer 21, thereby providing a tensile coating layer 22 on the surface side of the insulating coating 2. There are no particular restrictions on the tensile coating layer 22 as long as it is used as an insulating coating for a grain-oriented electrical steel sheet, but from the viewpoint of adhesion to the intermediate layer 21 (adhesion to the base steel sheet 1 via the intermediate layer 21), it is preferable that the tensile coating layer 22 contain a metal phosphate. In particular, it is preferable that the tensile coating layer 22 have a composition mainly composed of aluminum phosphate and silica.
[0056] The tensile coating layer 22 preferably contains metal phosphate and silica (derived from colloidal silica in the coating liquid) so that the silica content is 20.0% by mass or more. On the other hand, if the silica content of the tensile coating layer 22 exceeds 60.0% by mass, it may cause powdering, so it is preferably 60.0% by mass or less. Furthermore, it preferably contains a total of 70.0% by mass or more of metal phosphate and silica. The remainder other than the metal phosphate and silica may contain ceramic particles such as alumina or silicon nitride. Aluminum phosphate is preferred as the metal phosphate from the viewpoint of heat resistance.
[0057] Although the thickness of the tensile coating layer 22 is not limited, the average thickness of the insulating coating 2 (intermediate layer 21 + tensile coating layer 22) is preferably 2.0 to 20.0 μm, assuming that the average thickness of the intermediate layer 21 is within the above range. If the average thickness of the insulating coating 2 is less than 2.0 μm, sufficient coating tension cannot be obtained. Furthermore, there is a large amount of phosphate elution. This can cause stickiness and reduced corrosion resistance, and may even lead to coating peeling. Furthermore, if the thickness of the insulating coating 2 exceeds 20.0 μm, the space factor can decrease, resulting in deterioration of magnetic properties, or cracks can occur, resulting in reduced adhesion and reduced corrosion resistance.
[0058] In the tensile coating layer 22, the mass percentage of the metal phosphate and the type of the metal phosphate can be determined in a cross section along the thickness direction in the same manner as for the intermediate layer 21. As described above, the tensile coating layer 22 and the intermediate layer 21 can be distinguished from each other by the difference in the silica content.
[0059] The thickness of the tensile coating layer 22 can be determined in the same manner as the intermediate layer 21. The sum of the thickness of the tensile coating layer 22 and the thickness of the intermediate layer 21 is the thickness of the insulating coating 2.
[0060] <Method for manufacturing grain-oriented electrical steel sheet> The grain-oriented electrical steel sheet according to this embodiment can be suitably manufactured by a manufacturing method that satisfies the manufacturing conditions described below. However, it goes without saying that the grain-oriented electrical steel sheet according to this embodiment is not particularly limited to a manufacturing method. In other words, a grain-oriented electrical steel sheet having the configuration described above is considered to be the grain-oriented electrical steel sheet according to this embodiment, regardless of its manufacturing conditions.
[0061] The grain-oriented electrical steel sheet according to this embodiment can be manufactured by a manufacturing method including the following steps: (I) a hot rolling step of hot-rolling a steel slab having a predetermined chemical composition to obtain a hot-rolled sheet, (II) a hot-rolled sheet annealing step of annealing the hot-rolled sheet, (III) a cold-rolling step of cold-rolling the hot-rolled sheet after the hot-rolled sheet annealing step to obtain a steel sheet (cold-rolled sheet), (IV) a decarburization annealing step of decarburizing the steel sheet after the cold-rolling step, and (V) a step of adding Al to the steel sheet. 2 O 3 (VII) an annealing separator removing step of removing excess annealing separator from the steel sheet after the final annealing step, (VIII) a pickling step of pickling the steel sheet after the annealing separator removing step with 0.1 to 5 mass% of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid for 1 to 20 seconds, (IX) an immersion step of immersing the steel sheet after the pickling step in a treatment solution containing a metal phosphate, nitric acid, and iron ions at a solution temperature of 20 to 85°C for 5 to 150 seconds, and (X) a drying step of removing the steel sheet after the immersion step from the treatment solution, removing excess treatment solution, and then drying. (XI) A tensile coating layer forming step of applying a coating liquid containing a metal phosphate and colloidal silica, and having a total concentration of the metal phosphate and colloidal silica of 10.0 to 40.0 mass % in terms of solid content, to the steel sheet after the drying step, drying the coating liquid, and then maintaining the steel sheet at a sheet temperature of 700 to 950°C for 10 to 120 seconds.
[0062] In the method for producing a grain-oriented electrical steel sheet according to this embodiment, the treatment liquid in the immersion step satisfies the following conditions: (A) metal ion concentration: 1.0 to 10.0 g / L, (B) phosphate ion concentration: 2.0 to 25.0 g / L, (C) nitrate ion concentration: 2.0 to 40.0 g / L, (D) iron ion concentration: 1.0 to 20.0 g / L, (E) ratio of phosphate ion concentration to metal ion concentration: 1.5 to 5.0, (F) ratio of nitrate ion concentration to phosphate ion concentration: 0.5 to 10.0.
[0063] The method for producing a grain-oriented electrical steel sheet according to this embodiment may further include one or both of the following: (XII) a nitriding step in which the steel sheet is nitrided between the decarburization annealing step and the finish annealing step; and (XIII) a magnetic domain refining step in which magnetic domain control of the steel sheet is performed after the tension coating layer forming step. Of these, the production of a grain-oriented electrical steel sheet according to this embodiment is characterized by the steps (V) finish annealing step to (XI) tension coating layer forming step (which may be collectively referred to as the insulation coating forming step), which are primarily related to the formation of the insulating coating. Known conditions can be used for other steps or for conditions not described. These steps are described below.
[0064] [Hot Rolling Process] In the hot rolling process, a steel billet such as a slab having a predetermined chemical composition is heated and then hot rolled to obtain a hot-rolled sheet. The heating temperature of the steel billet is preferably within the range of 1100 to 1450°C. The heating temperature is more preferably 1300 to 1400°C.
[0065] The chemical composition of the slab may be changed depending on the chemical composition of the grain-oriented electrical steel sheet that is ultimately desired to be obtained, but an example of such a chemical composition may include, in mass %, C: 0.01 to 0.20%, Si: 2.50 to 4.00%, sol. Al: 0.01 to 0.040%, Mn: 0.01 to 0.50%, N: 0.020% or less, S: 0.005 to 0.040%, Cu: 0 to 0.50%, Sn: 0 to 0.50%, Se: 0 to 0.020%, Sb: 0 to 0.50%, and the balance being Fe and impurities.
[0066] The hot rolling conditions are not particularly limited and may be appropriately set based on the desired properties. The thickness of the hot rolled sheet is preferably within a range of 2.0 mm to 3.0 mm, for example.
[0067] [Hot-rolled sheet annealing process] The hot-rolled sheet annealing process is a process of annealing the hot-rolled sheet manufactured through the hot rolling process. By performing such annealing treatment, recrystallization occurs in the steel sheet structure, making it possible to achieve good magnetic properties, which is preferable.
[0068] When hot-rolled sheet annealing is performed, the hot-rolled sheet produced through a hot rolling process may be annealed according to a known method. The means for heating the hot-rolled sheet during annealing is not particularly limited, and known heating methods can be used. The annealing conditions are also not particularly limited. For example, the hot-rolled sheet may be annealed in a temperature range of 900 to 1200°C for 10 seconds to 5 minutes.
[0069] [Cold Rolling Step] In the cold rolling step, the hot rolled sheet after the hot rolled sheet annealing step is subjected to cold rolling to obtain a steel sheet (cold rolled sheet). The cold rolling may be a single cold rolling (a series of cold rolling steps without annealing in between), or may be multiple cold rolling steps with intermediate annealing between them, in which the cold rolling is interrupted and at least one or two or more intermediate annealing steps are performed before the final pass of the cold rolling step.
[0070] When intermediate annealing is performed, it is preferable to hold the steel sheet at a temperature of 1000 to 1200°C for 5 to 180 seconds. The annealing atmosphere is not particularly limited. In consideration of production costs, it is preferable to perform intermediate annealing three times or less. Furthermore, the surface of the hot-rolled steel sheet may be pickled before the cold rolling step.
[0071] In the cold rolling process according to this embodiment, the hot-rolled sheet after the hot-rolled sheet annealing process is cold-rolled according to a known method to obtain a steel sheet. For example, the final reduction can be in the range of 80 to 95%. A final reduction of 80% or more is preferable because it is possible to obtain Goss nuclei with a high concentration of {110}<001> orientation in the rolling direction. On the other hand, a final reduction of more than 95% is not preferable because it increases the possibility of secondary recrystallization becoming unstable in the subsequent finish annealing process. The final reduction is the cumulative reduction of cold rolling, and if intermediate annealing is performed, it is the cumulative reduction of cold rolling after final intermediate annealing.
[0072] [Decarburization Annealing Step] In the decarburization annealing step, the obtained steel sheet is subjected to decarburization annealing. In the decarburization annealing, the conditions for the decarburization annealing are not limited as long as the steel sheet undergoes primary recrystallization and C, which adversely affects magnetic properties, can be removed from the steel sheet. For example, the oxidation degree (PH) in the annealing atmosphere (furnace atmosphere) can be adjusted. 2 O / PH 2 ) is set to 0.3 to 0.6, and the annealing temperature is set to 800 to 900° C., and the holding is performed for 10 to 600 seconds.
[0073] [Nitriding Process] Nitriding may be performed between the decarburization annealing process and the finish annealing process described below. In the nitriding process, for example, the steel sheet after the decarburization annealing process is maintained at approximately 700 to 850°C in a nitriding atmosphere (an atmosphere containing hydrogen, nitrogen, and ammonia or other nitriding gases) to perform nitriding. When AlN is used as an inhibitor, it is preferable to set the N content of the steel sheet after the nitriding process to 40 ppm or more by the nitriding process. On the other hand, if the N content of the steel sheet after the nitriding process exceeds 1000 ppm, excess AlN remains in the steel sheet even after the completion of secondary recrystallization in the finish annealing. Such AlN can cause iron loss degradation. For this reason, it is preferable to set the N content of the steel sheet after the nitriding process to 1000 ppm or less.
[0074] [Finish annealing step] In the finish annealing step, Al is added to the steel sheet after the decarburization annealing step or after the nitriding treatment (after the nitriding treatment step). 2 O 3After drying, finish annealing is performed.
[0075] In conventional methods for producing grain-oriented electrical steel sheets, a forsterite-based coating is formed on the surface of the steel sheet (cold-rolled sheet) by applying an annealing separator mainly composed of MgO and then performing finish annealing. In contrast, in the method for producing grain-oriented electrical steel sheets according to the present embodiment, an Al SiO 2 -based coating is applied to the steel sheet so that a forsterite-based coating is hardly formed. 2 O 3 An annealing separator containing
[0076] On the other hand, Al 2 O 3 The ratio of Al may be 100 mass %, but 2 O 3 From the viewpoint of preventing seizure of Al, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator preferably contains MgO. Although the content of MgO may be 0%, in order to obtain the above effect, the content of MgO is preferably 5 mass% or more. When MgO is contained, the content of MgO is preferably 10 mass% or more. 2 O 3 The content of MgO is preferably 50% by mass or less.
[0077] Furthermore, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator may further contain chloride. When the annealing separator contains chloride, the effect of making it more difficult for a forsterite-based coating to form is obtained. The chloride content is not particularly limited and may be 0%, but to obtain the above effect, a content of 0.5 to 10 mass% is preferable. Effective chlorides include, for example, bismuth chloride, calcium chloride, cobalt chloride, iron chloride, and nickel chloride.
[0078] The conditions for the finish annealing are not limited, but for example, conditions in which the steel is held at a temperature of 1150 to 1250° C. for 10 to 60 hours can be adopted.
[0079] [Annealing Separator Removal Step] In the annealing separator removal step, excess annealing separator is removed from the steel sheet after the finish annealing step. For example, the excess annealing separator can be removed by washing with water.
[0080] [Pickling Process] In the pickling process, the steel sheet after the annealing separator removal process is pickled for 1 to 20 seconds with one inorganic acid selected from sulfuric acid, phosphoric acid, nitric acid, and chloric acid, at a concentration of 0.1 to 10 mass % and heated to 30 to 85°C. Pickling under these conditions has the effect of sufficiently removing the forsterite-based coating and, if any MgO remains, removing it. However, in the pickling process of this embodiment, so-called pickling pits are unlikely to form.
[0081] [Immersion Step] [Drying Step] In the immersion step, the steel sheet after the pickling step is immersed in a treatment solution containing a metal phosphate and nitric acid for 5 to 150 seconds, and in the drying step, the steel sheet after the immersion step is pulled out of the treatment solution, excess treatment solution is removed, and then the steel sheet is dried. This forms an intermediate layer on the surface of the base steel sheet.
[0082] In the immersion step, the treatment solution is adjusted to satisfy the following conditions (A) to (F).
[0083] (A) Metal ion concentration: 1.0 to 10.0 g / L (B) Phosphate ion concentration: 2.0 to 25.0 g / L The treatment solution contains a metal phosphate and nitric acid as an oxidizing agent. Examples of metal phosphate include zinc phosphate, manganese phosphate, zinc calcium phosphate, and iron manganese phosphate. From the viewpoint of controllability of the roughness index, zinc phosphate is preferred. The metal ion concentration and phosphate ion concentration in the treatment solution are 1.0 to 10.0 g / L and 2.0 to 25.0 g / L, respectively. If the metal ion concentration is less than 1.0 g / L, the precipitation rate of the phosphate salt is relatively slow, resulting in etching of the steel sheet surface, which may increase the degree of roughness at the interface, increase the roughness index L / W, and potentially degrade magnetic properties. Similarly, if the phosphate ion concentration is less than 2.0 g / L, the degree of roughness at the interface may increase, increase the roughness index L / W, and potentially degrade magnetic properties. Therefore, the metal ion concentration and the phosphate ion concentration are preferably 1.0 g / L or more and 2.0 g / L or more, respectively. On the other hand, if the metal ion concentration exceeds 10.0 g / L, the pH of the treatment solution increases, and the deposition rate of the metal phosphate also decreases, resulting in an increase in the degree of interface roughness, an increase in the roughness index L / W, and a risk of deterioration in magnetic properties. Similarly, if the phosphate ion concentration exceeds 25.0 g / L, the degree of interface roughness also increases, the roughness index L / W, and a risk of deterioration in magnetic properties. Therefore, the metal ion concentration and the phosphate ion concentration are preferably 10.0 g / L or less and 25.0 g / L or less, respectively.
[0084] (C) Nitrate ion concentration: 2.0 to 40.0 g / L. As described above, nitric acid is added as an oxidizing agent to the treatment solution according to this embodiment. Using nitric acid as an oxidizing agent prevents hydrogen gas generation and efficiently forms a dense intermediate layer. However, if the amount of nitric acid added to the treatment solution is excessively large, the steel sheet surface may be excessively oxidized, reducing the rate of phosphate precipitation. This may result in increased interface roughness, an increased L / W index, and potentially degraded magnetic properties. Therefore, the nitrate ion concentration is preferably 40.0 g / L or less, and more preferably 25.0 g / L or less. On the other hand, if the amount of nitric acid added to the treatment solution is too small, hydrogen gas generation cannot be suppressed, resulting in the formation of regions with too little phosphate precipitation, which may result in increased interface roughness, an increased L / W index, and potentially degraded magnetic properties. Therefore, the nitrate ion concentration is preferably 2.0 g / L or more.
[0085] (D) Iron ion concentration: 1.0 to 20.0 g / L. It is believed that the appropriate presence of iron ions in the treatment solution inhibits the etching action of the metal phosphate treatment solution and slows the rate at which the steel sheet surface dissolves. To achieve this effect, a concentration of 1.0 g / L or more is desirable. On the other hand, if an excessive amount of iron ions is present in the treatment solution, iron will precipitate in the resulting intermediate layer, resulting in reduced adhesion, and therefore a concentration of 20.0 g / L or less is preferred.
[0086] (E) Ratio of Phosphate Ion Concentration to Metal Ion Concentration: 1.5 to 5.0 While it is effective to set the phosphate concentration and metal ion concentration within the above ranges from the viewpoint of optimizing the unevenness index, it is also preferable to adjust the ratio of the phosphate ion concentration to the metal ion concentration. Specifically, the ratio of the phosphate ion concentration to the metal ion concentration (phosphate ion concentration / metal ion concentration) is set to 1.5 to 5.0. If the ratio of the phosphate ion concentration to the metal ion concentration is too high, etching may proceed, causing excessive unevenness on the steel sheet and resulting in a poor space factor. Therefore, the ratio of the phosphate ion concentration to the metal ion concentration is preferably set to 5.0 or less. On the other hand, if the ratio of the phosphate ion concentration to the metal ion concentration is too low, the pH may increase, preventing precipitation of metal phosphate or requiring a very long time for precipitation. Therefore, the ratio of the phosphate ion concentration to the metal ion concentration is preferably set to 1.5 or more.
[0087] (F) Ratio of Nitrate Ion Concentration to Phosphate Ion Concentration: 0.5 to 10.0 Furthermore, from the viewpoint of the deposition rate, the ratio of the nitrate ion concentration to the phosphate ion concentration is also adjusted. Specifically, the ratio of the nitrate ion concentration to the phosphate ion concentration (nitrate ion concentration / phosphate ion concentration) is set to 0.5 to 10.0. If the ratio of the nitrate ion concentration to the phosphate ion concentration is too high, excessive etching of the steel sheet may occur. Therefore, the ratio of the nitrate ion concentration to the phosphate ion concentration is preferably set to 10.0 or less. On the other hand, if the ratio of the nitrate ion concentration to the phosphate ion concentration is too low, the deposition of the metal phosphate salt may be suppressed, and the formation of the intermediate layer may take a long time. Therefore, the ratio of the nitric acid concentration to the phosphate ion concentration is preferably set to 0.5 or more.
[0088] The temperature of the treatment solution is preferably 20 to 85°C, and the immersion time is preferably 5 to 150 seconds. If the solution temperature is below 20°C or the treatment time is less than 5 seconds, the intermediate layer may not be formed sufficiently, resulting in poor adhesion. On the other hand, if the solution temperature is above 85°C or the treatment time is more than 150 seconds, the intermediate layer may have regions where the crystalline metal phosphate is excessively precipitated, resulting in poor space factor.
[0089] In the drying step, if the drying temperature is high, voids may occur and adhesion may be deteriorated, so the drying temperature is preferably 300° C. or lower, more preferably 200° C. or lower. The drying temperature is preferably 100° C. or higher.
[0090] [Tension coating layer forming process] In the tensile coating layer forming process, a coating liquid containing a metal phosphate salt and colloidal silica and having a concentration of 10 to 40 mass % is applied to the steel sheet after the drying process, dried, and then heated and held at a sheet temperature of 700 to 950°C for 10 to 50 seconds, thereby forming a tensile coating layer on the surface of the intermediate layer.
[0091] If the sheet temperature during holding is less than 700°C, the tension will be low and the magnetic properties will be inferior. Therefore, it is preferable that the sheet temperature be 700°C or higher. On the other hand, if the sheet temperature is higher than 950°C, the rigidity of the steel sheet will decrease and it will be more likely to deform. In this case, strain may be introduced into the steel sheet due to transportation, etc., resulting in inferior magnetic properties. Therefore, it is preferable that the sheet temperature be 950°C or lower.
[0092] Furthermore, if the retention time is less than 10 seconds, the elution property will be poor. Therefore, the retention time is set to 10 seconds or more. On the other hand, if the retention time is more than 50 seconds, the adhesion of the tensile coating layer may be poor. Therefore, the retention time is preferably 50 seconds or less.
[0093] The coating liquid (insulating coating solution) is adjusted to contain a total of 10 to 40 mass % of metal phosphate and colloidal silica, calculated as solids. If the total concentration of metal phosphate and colloidal silica is less than 10 mass %, the applied treatment liquid may easily flow, resulting in uneven application. If the total concentration of metal phosphate and colloidal silica exceeds 40 mass %, the viscosity may be too high, resulting in uneven patterns and coating.
[0094] As the metal phosphate, for example, one or a mixture of two or more selected from aluminum phosphate, zinc phosphate, magnesium phosphate, nickel phosphate, copper phosphate, lithium phosphate, cobalt phosphate, etc. can be used. Among these, aluminum phosphate is preferred.
[0095] The coating liquid may contain additional elements such as vanadium, tungsten, molybdenum, zirconium, etc. When these elements are contained, they can be added to the coating liquid as, for example, an oxygen acid.
[0096] Colloidal silica can be of type S or type C. Type S colloidal silica refers to colloidal silica in which the silica solution is alkaline, while type C colloidal silica refers to silica particles whose surfaces are aluminum-treated, resulting in an alkaline to neutral silica solution. Type S colloidal silica is widely used and relatively inexpensive, but care must be taken as there is a risk of aggregation and precipitation when mixed with an acidic metal phosphate solution. Type C colloidal silica is stable even when mixed with a metal phosphate solution and there is no risk of precipitation, but it is relatively expensive due to the large number of processing steps required. It is preferable to use the appropriate type depending on the stability of the coating solution to be prepared.
[0097] [Magnetic Domain Refinement Process] The manufacturing method of the grain-oriented electrical steel sheet according to this embodiment may further include a magnetic domain refinement process in which the steel sheet after the tension coating layer formation process is subjected to magnetic domain refinement. Performing the magnetic domain refinement process can further reduce the iron loss of the grain-oriented electrical steel sheet. Examples of magnetic domain refinement processes include narrowing the width of 180° magnetic domains (refining 180° magnetic domains) by forming linear or point-like grooves extending in a direction intersecting the rolling direction at predetermined intervals along the rolling direction, and narrowing the width of 180° magnetic domains (refining 180° magnetic domains) by forming linear or point-like stress-strain portions or grooves extending in a direction intersecting the rolling direction at predetermined intervals along the rolling direction. Laser beam irradiation, electron beam irradiation, and other methods can be used to form stress-strain portions. Grooves can be formed by mechanical groove formation using gears or the like, chemical groove formation using electrolytic etching, or thermal groove formation using laser irradiation. If the insulating coating is damaged by the formation of stress-strained portions or grooves, and the insulating properties and other characteristics are deteriorated, the insulating coating may be formed again to repair the damage.
[0098] A slab containing, by mass%, C: 0.08%, Si: 3.31%, sol.Al: 0.028%, N: 0.008%, Mn: 0.07%, S: less than 0.0005%, with the balance being Fe and impurities was cast. The slab was heated to 1350 ° C and then hot rolled to obtain a hot-rolled sheet having a thickness of 2.2 mm. This hot-rolled sheet was annealed at 1100 ° C for 10 seconds (hot-rolled sheet annealing). The hot-rolled sheet was then cold-rolled to obtain a cold-rolled sheet having a thickness of 0.22 mm. This cold-rolled sheet was then decarburized at 830 ° C for 90 seconds.
[0099] After decarburization annealing, MgO and Al 2 O 3 95% bismuth chloride, BiCl 3 The steel sheet was then coated with an annealing separator containing 5% by mass of ammonium nitrate, dried, and then subjected to finish annealing at 1200°C for 20 hours. After the finish annealing, the steel sheet was rinsed with water to remove excess annealing separator, and no forsterite-based coating was formed on the steel sheet surface. The steel sheet was then lightly pickled with 3% by mass sulfuric acid at 80°C for 10 seconds.
[0100] After light pickling, an intermediate layer was formed using the treatment solution shown in Table 1. Steel wool was used as the iron ion source, and the treatment solution was adjusted to the concentration shown in Table 1. The immersion conditions were as shown in Table 1. The obtained intermediate layer had the properties shown in Table 1.
[0101] Thereafter, an insulating coating treatment solution containing metal phosphate and colloidal silica as its main components, as shown in Table 2, was applied, and the steel sheet was dried at 850°C for 20 seconds to form a tensile coating layer on the surface. Note that the "metal element molar ratio" in Table 2 indicates the abundance ratio of the metal elements when two or more metal elements are present in the metal phosphate. The thickness of the insulating coating (intermediate layer and tensile coating layer) was as shown in Table 2. The tensile coating layer consisted essentially of metal phosphate and silica.
[0102] The resulting steel sheet (grain-oriented electrical steel sheet) was subjected to magnetic domain refinement by irradiating it with a laser beam at a UA (irradiation energy density) of 2.0 J and an irradiation interval of 5.0 mm. The iron loss W17 / 50 (iron loss at 50 Hz and 1.7 T) of the steel sheet after the magnetic domain refinement treatment was measured using a single sheet magnetic property measurement method (Single Sheet Tester: SST) in accordance with JIS C2556 (2015). If the iron loss W17 / 50 was 0.68 W / kg or less, it was determined that good magnetic properties were ensured. The space factor was also measured as follows.
[0103] [Space Factor] The space factor was measured according to a method in accordance with JIS C 2550-5 (2020). Thirty test pieces, each 30 mm wide and 320 mm long, were used. After measuring the total mass of the sample, the distance between the upper and lower backing plates sandwiching the laminate was measured under a pressure of 1 MPa, and then calculated. If the space factor was 96.0% or higher, it was determined that a high space factor was ensured.
[0104] The coating adhesion, coating tension, corrosion resistance, and elution resistance of the steel sheets after the magnetic domain refining treatment were evaluated by the following methods. The interface roughness index was also determined by the following method. The results are shown in Tables 2 and 3.
[0105] [Interface roughness index] First, a scanning electron microscope was used to observe the region including the interface between the base steel sheet and the intermediate layer at 5000x magnification to obtain an observation image. Then, the distance between two points on the observation image, drawn by a straight line connecting both ends of the interface between the base steel sheet and the intermediate layer, was defined as the observation image width W, and this observation image width W was calculated. Furthermore, the actual interface path (i.e., the curved path tracing the actual interface) was set as the interface length L, and the interface length L was calculated, and the roughness index L / W was obtained. The observation image width W and interface length L were calculated using the application system "Luzex AP" manufactured by Nireco Corporation for the cross-sectional image obtained by the electron microscope.
[0106] [Coating Adhesion] Coating adhesion was evaluated by taking a sample 30 mm wide and 300 mm long from the steel sheet, annealing the sample for two hours at 800°C for stress relief in a nitrogen stream, and then winding it around a 10 mm diameter cylinder and unwinding it to conduct a bending adhesion test. The coating adhesion was evaluated based on the degree of peeling (area ratio) of the coating. The evaluation criteria were as follows, with ⊚ or ◯ being considered to indicate excellent coating adhesion: ⊚: Peeling area ratio 0 to 0.5%; ◯: Peeling area ratio more than 0.5% and 5.0% or less; △: Peeling area ratio more than 5.0%.
[0107] [Coating Tension] The coating tension was calculated by back-calculating from the state of curvature when one side of the insulating coating was peeled off. When the obtained coating tension was 4.0 MPa or more, it was determined that the coating tension was sufficient.
[0108] [Corrosion Resistance] Corrosion resistance was evaluated by subjecting a sample to a salt spray test (JIS Z2371:2015) in which a 5% NaCl aqueous solution was allowed to fall naturally onto the sample for 7 hours in an atmosphere at 35°C. The rust area was then evaluated on a 10-point scale. The evaluation criteria were as follows: A score of 5 or higher was considered to be excellent in corrosion resistance. 10: No rust occurred 9: Very little rust occurred (area rate 0.10% or less) 8: Area rate where rust occurred = more than 0.10% but not more than 0.25% 7: Area rate where rust occurred = more than 0.25% but not more than 0.50% 6: Area rate where rust occurred = more than 0.50% but not more than 1.0% 5: Area rate where rust occurred = more than 1.0% but not more than 2.5% 4: Area rate where rust occurred = more than 2.5% but not more than 5.0% 3: Area rate where rust occurred = more than 5.0% but not more than 10% 2: Area rate where rust occurred = more than 10% but not more than 25% 1: Area rate where rust occurred = more than 25% but not more than 50%
[0109] [Elution Resistance] Elution resistance was evaluated based on whether or not the elution of phosphoric acid from the sample could be suppressed. The amount of elution was measured by boiling the sample in boiling pure water for 10 minutes, measuring the amount of phosphoric acid eluted in the pure water, and dividing the amount of phosphoric acid by the area of the insulating coating of the boiled grain-oriented electrical steel sheet. The amount of phosphoric acid eluted in the pure water was measured by cooling the pure water (solution) into which the phosphoric acid had eluted, and measuring the phosphoric acid concentration of the sample obtained by diluting the cooled solution with pure water using ICP-AES. When the elution amount was 40 mg / m 2 If the resistance is less than this, the resin is deemed to have excellent resistance to elution.
[0110]
[0111]
[0112]
[0113] As can be seen from Tables 1 to 3, the examples of the present invention are extremely excellent in various properties, including coating adhesion, and have improved core loss and space factor. On the other hand, the comparative examples are inferior in one or more of coating adhesion, magnetic properties, corrosion resistance, elution resistance, and transformer (core) space factor.
[0114] 100 Grain-oriented electrical steel sheet 1 Base steel sheet 2 Insulation coating 21 Intermediate layer 22 Tensile coating layer
[0115] According to the above aspect of the present invention, a grain-oriented electrical steel sheet can be obtained that has excellent adhesion of a tensile coating and magnetic properties, and that does not reduce the space factor of a transformer (core). Therefore, the grain-oriented electrical steel sheet obtained can be suitably used as an iron core material for transformers, and has high industrial applicability.
Claims
1. A grain-oriented electrical steel sheet comprising: a base steel sheet; and an insulating coating formed on the surface of the base steel sheet, wherein the insulating coating comprises: an intermediate layer formed on the side of the base steel sheet and containing a crystalline metal phosphate; and a tensile coating layer formed on the surface side of the insulating coating, wherein, when the interface between the base steel sheet and the intermediate layer in a cross section taken along the thickness direction of the intermediate layer is observed at 5000x magnification using a scanning electron microscope, the ratio of interface length L to observed image width W is 100.0 to 120.0%.
2. The grain-oriented electrical steel sheet according to claim 1, wherein the tensile coating layer contains a metal phosphate and silica.
3. A method for forming the insulating coating of the grain-oriented electrical steel sheet according to claim 1, comprising the steps of: 2 O 3 a finish annealing step of applying an annealing separator containing 10 to 100 mass % of the above-mentioned, drying the steel sheet, and then finish annealing the steel sheet; an annealing separator removing step of removing excess annealing separator from the steel sheet after the finish annealing step; a pickling step of pickling the steel sheet after the annealing separator removing step with 0.1 to 5 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid for 1 to 20 seconds; an immersion step of immersing the steel sheet after the pickling step in a treatment solution containing a metal phosphate, an oxidizing agent, and iron ions; and a drying step of pulling out the steel sheet after the immersion step from the treatment solution, removing excess treatment solution, and then drying the steel sheet. and a tensile coating layer forming step of applying a coating liquid containing a metal phosphate and colloidal silica, and having a total concentration of the metal phosphate and colloidal silica of 10 to 40 mass % in terms of solid content, to the steel sheet after the drying step, drying the coating liquid, and then maintaining the sheet at a temperature of 700 to 950°C for 10 to 120 seconds, wherein the treatment liquid has a metal ion concentration of 1.0 to 10.0 g / L, a phosphate ion concentration of 2.0 to 25.0 g / L, a nitrate ion concentration of 2.0 to 40.0 g / L, and an iron ion concentration of 1.0 to 20.0 g / L, a ratio of the phosphate ion concentration to the metal ion concentration of 1.5 to 5.0, and a ratio of the nitrate ion concentration to the phosphate ion concentration of 0.5 to 10.
0.
4. The method for forming an insulating coating according to claim 3, characterized in that in the immersion step, the steel sheet after the pickling step is immersed in the treatment liquid having a liquid temperature of 20 to 85°C for 2 to 60 seconds.
5. The method for forming an insulating coating according to claim 3, wherein the nitrate ion concentration is 2.0 to 25.0 g / L.
Citation Information
Patent Citations
JP1973039338A
JP1974096920A
Formation of insulated film on grain-oriented silicon steel sheet
JP1994184762A
Formation of insulated film on silicon steel sheet
JP1999209891A
Method for manufacturing grain-oriented silicon steel sheet having excellent adhesiveness of tension impartable insulation film
JP2005139481A