Grain-oriented electrical steel sheet and method for forming insulating coating film

The integration of a crystalline metal phosphate intermediate layer with amorphous silica and metal oxides in grain-oriented electrical steel sheets addresses the adhesion and magnetic property issues associated with forsterite-free coatings, resulting in improved adhesion and magnetic performance without reducing the transformer's space factor.

WO2024214822A1PCT designated stage expired Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014848
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-12
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Grain-oriented electrical steel sheets without forsterite coatings face challenges in achieving sufficient adhesion for tension coatings, leading to impaired magnetic properties and increased iron loss due to the uneven structure and non-magnetic nature of forsterite coatings, which hinder domain wall movement.

Method used

A grain-oriented electrical steel sheet with a surface layer containing a crystalline metal phosphate intermediate layer, combined with amorphous silica, inorganic fillers, and metal oxides, which enhances adhesion and suppresses crystallization of metal phosphate crystals, ensuring improved magnetic properties and reduced iron loss without compromising the space factor.

Benefits of technology

The solution provides excellent tension coating adhesion and magnetic properties while maintaining the space factor of the transformer core, thereby enhancing the performance and efficiency of grain-oriented electrical steel sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014848_17102024_PF_FP_ABST
    Figure JP2024014848_17102024_PF_FP_ABST
Patent Text Reader

Abstract

This grain-oriented electrical steel sheet has a base steel sheet and an insulating coating film that is formed on the surface of the base steel sheet. The insulating coating film has: an intermediate layer that is formed on the base steel sheet side and contains a crystalline metal phosphate salt and at least one of amorphous silica, an inorganic filler, and a metal oxide; and a tension coating layer that is formed on the surface side of the insulating coating film. The average particle diameter of the at least one of the amorphous silica, the inorganic filler, and the metal oxide is 10-500 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Grain-oriented electrical steel sheet and method for forming insulating coating

[0001] The present invention relates to a grain-oriented electrical steel sheet and a method for forming an insulating coating. This application claims priority to Japanese Patent Application No. 2023-064836, filed on April 12, 2023, the contents of which are incorporated herein by reference.

[0002] Grain-oriented electrical steel sheets are primarily used in transformers. Transformers are continuously excited over a long period of time, from installation to disposal, and continue to generate energy loss. Therefore, the energy loss during magnetization with AC, i.e., core loss, is a major indicator that determines the performance of a transformer.

[0003] To reduce the iron loss of grain-oriented electrical steel sheets, many technologies have been developed to date, including (a) increasing the concentration in the {110}<001> orientation (Goss orientation), (b) increasing the content of solid solution elements such as Si to increase the electrical resistance of the steel sheet, or (c) reducing the thickness of the electrical steel sheet.

[0004] Furthermore, applying tension to steel sheets is effective in reducing iron loss. Forming a coating made of a material with a smaller thermal expansion coefficient than the steel sheet at high temperatures on the steel sheet surface is an effective means for reducing iron loss. A forsterite-based coating (inorganic coating) with excellent coating adhesion is produced by the reaction of oxides on the steel sheet surface with an annealing separator during the finish annealing process of electrical steel sheets. This coating can apply tension to steel sheets.

[0005] Furthermore, for example, the method disclosed in Patent Document 1, in which a coating liquid mainly composed of colloidal silica and phosphate is baked onto the surface of a steel sheet to form an insulating coating, is an effective method for reducing iron loss because it is highly effective in applying tension to the steel sheet. Therefore, a common method for producing grain-oriented electrical steel sheets is to leave the forsterite-based coating formed in the final annealing step and then apply an insulating coating mainly composed of phosphate on top of it.

[0006] However, in recent years, there has been an increasing demand for smaller and higher-performance transformers. To achieve this, grain-oriented electrical steel sheets are required to have excellent high-field iron loss characteristics, i.e., good iron loss even at high magnetic flux densities. At the same time, it has become clear that forsterite-based coatings hinder domain wall movement, adversely affecting iron loss. In grain-oriented electrical steel sheets, magnetic domains change due to domain wall movement under an AC magnetic field. Smooth and rapid domain wall movement is effective in reducing iron loss. However, forsterite-based coatings are themselves nonmagnetic and have an uneven structure at the interface between the steel sheet and the coating. This uneven structure is thought to hinder domain wall movement and adversely affect iron loss. Therefore, as means for improving high magnetic field iron loss, research has been conducted on a variety of techniques, including methods for removing the forsterite-based coating (inorganic coating) by mechanical means such as polishing or by chemical means such as pickling, techniques for producing grain-oriented electrical steel sheets that do not have a forsterite-based coating by preventing the formation of a forsterite-based coating during high-temperature finish annealing, and techniques for making the steel sheet surface mirror-finished (in other words, techniques for magnetically smoothing the steel sheet surface).

[0007] As a technique for preventing the formation of a forsterite-based coating, for example, Patent Document 2 discloses a technique in which, after normal finish annealing, the steel sheet is pickled to remove surface deposits, and then chemically or electrolytically polished to a mirror finish. It has been found that forming a tensioned insulating coating on the surface of a grain-oriented electrical steel sheet that does not have a forsterite-based coating and that has been obtained by such a known method can provide an even more excellent iron loss improvement effect. Furthermore, the tensioned insulating coating can impart various properties, such as corrosion resistance, heat resistance, and slip resistance, in addition to improving iron loss.

[0008] However, in addition to exhibiting insulating properties, forsterite-based coatings also function as intermediate layers that ensure adhesion when forming tension coatings (tension-applying insulating coatings). That is, because forsterite-based coatings are formed in a state where they penetrate deeply into the steel sheet, they have excellent adhesion to the metal steel sheet. Therefore, when a tension-applying coating (tension coating) containing colloidal silica, phosphate, or the like as a main component is formed on the surface of a forsterite-based coating, the coating exhibits excellent adhesion. On the other hand, because bonding between metal and oxide is generally difficult, it has been difficult to ensure sufficient adhesion between the tension coating and the steel sheet surface in the absence of a forsterite-based coating. Therefore, when forming a tension coating on a grain-oriented electrical steel sheet that does not have a forsterite-based coating, the provision of a layer that serves as an intermediate layer for the forsterite-based coating has been considered.

[0009] For example, Patent Document 3 discloses that grain-oriented electrical steel sheets that do not have a forsterite-based coating (inorganic coating) are annealed in a weakly reducing atmosphere to selectively thermally oxidize silicon that is inevitably contained in the silicon steel sheets, thereby forming SiO on the steel sheet surface. 2 Patent Document 4 discloses a technique in which a grain-oriented electrical steel sheet having no forsterite-based coating (inorganic coating) is subjected to an anodic electrolysis treatment in a silicate solution to form a SiO layer on the surface of the steel sheet. 2 After the layers are formed, a tensioned insulating coating is applied.

[0010] However, the technique disclosed in Patent Document 3 requires the preparation of annealing equipment capable of controlling the atmosphere in order to perform annealing in a weakly reducing atmosphere, which results in a problem of processing costs. Also, in the technique disclosed in Patent Document 4, anodic electrolysis is performed in a silicate aqueous solution, thereby forming SiO 2 which maintains sufficient adhesion with the tension-imparting insulating coating. 2 In order to obtain such a layer on the surface of the steel sheet, it is necessary to prepare new electrolytic treatment equipment, which increases the treatment cost.

[0011] In contrast, Patent Document 5 discloses a grain-oriented electrical steel sheet having a base steel sheet and an insulating coating formed on the surface of the base steel sheet, the insulating coating being formed on the base steel sheet side, an intermediate layer containing a crystalline metal phosphate, and a tensile coating layer formed on the surface side of the insulating coating. In this grain-oriented electrical steel sheet, the intermediate layer can be formed by chemical conversion treatment.

[0012] Japanese Unexamined Patent Publication No. 48-039338 Japanese Unexamined Patent Application No. 49-96920 Unexamined Japanese Patent Application No. 6-184762 Unexamined Japanese Patent Application No. 11-209891 International Publication No. 2022 / 215709

[0013] The technology of Patent Document 5 improves coating adhesion, coating tension, and magnetic properties by providing an intermediate layer made of a crystalline metal phosphate between the base steel sheet and the tension coating. Furthermore, since the intermediate layer can be formed by chemical conversion treatment, no special equipment is required. Therefore, this technology is useful. However, as a result of studies by the present inventors, it was found that improving adhesion in the grain-oriented electrical steel sheet of Patent Document 5 may result in a deterioration of the magnetic properties of the transformer. Further investigation into this point revealed that the cause of the deterioration in magnetic properties is the coarsening of the crystals of the metal phosphate precipitated by the chemical conversion treatment, which reduces the space factor when an actual transformer is manufactured.

[0014] Therefore, the present invention aims to provide a grain-oriented electrical steel sheet in which a layer containing metal phosphate is formed on the surface of a steel sheet having a forsterite-based coating by chemical conversion treatment, which has excellent adhesion and magnetic properties of a tension coating and does not reduce the space factor of a transformer (core), provided that the basic properties required of the coating, such as corrosion resistance and resistance to leaching of phosphoric acid, are not reduced.

[0015] The inventors have discovered that when a layer containing metal phosphate is provided as an intermediate layer to improve adhesion between the base steel sheet and the tensile coating layer, the coarsening of metal phosphate crystals can be suppressed by adding a substance that suppresses phosphate crystallization to the chemical conversion treatment solution.

[0016] The present invention was made in light of the above findings. The gist of the present invention is as follows. [1] A grain-oriented electrical steel sheet according to one aspect of the present invention comprises a base steel sheet and an insulating coating formed on the surface of the base steel sheet, wherein the insulating coating is formed on the base steel sheet side and comprises an intermediate layer containing a crystalline metal phosphate and one or more of amorphous silica, an inorganic filler, and a metal oxide; and a tensile coating layer formed on the surface side of the insulating coating, wherein the amorphous silica, the inorganic filler, and the metal oxide have an average particle size of 10 to 500 nm. [2] In the grain-oriented electrical steel sheet according to [1], the inorganic filler may comprise one or more of alumina, BN, AlN, and kaolin. [3] In the grain-oriented electrical steel sheet according to [1] or [2], the metal oxide may be one or more of titanium oxide, zinc oxide, and calcium oxide. [4] In the grain-oriented electrical steel sheet according to any one of [1] to [3], the crystalline metal phosphate may have an average crystal grain size of 1.0 to 12.0 μm. [5] A method for forming an insulating coating according to another aspect of the present invention is a method for forming the insulating coating provided on the grain-oriented electrical steel sheet according to [1], comprising the steps of: 2 O 3a finish annealing step of applying an annealing separator containing 10 to 100 mass % of the above-mentioned compound to the steel sheet, drying the steel sheet, and then finish annealing the steel sheet; an annealing separator removing step of removing excess annealing separator from the steel sheet after the finish annealing step; a light pickling step of pickling the steel sheet after the annealing separator removing step with a pickling solution containing 0.10 to 10.0 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid at a solution temperature of 30 to 85°C for 1 to 20 seconds; and the steel sheet after the immersion step is removed from the treatment solution, and excess treatment solution is removed, followed by drying; and a tensile coating layer forming step is performed in which a coating solution containing a metal phosphate and colloidal silica, the metal phosphate and the colloidal silica having a total concentration of 10 to 40 mass %, is applied to the steel sheet after the drying step, dried, and then heated and maintained at a sheet temperature of 700 to 950°C for 10 to 50 seconds.

[0017] According to the above aspect of the present invention, it is possible to provide a grain-oriented electrical steel sheet that has excellent adhesion of a tension coating and magnetic properties, and does not reduce the space factor of a transformer (core).

[0018] 1 is an example of a cross-sectional view of a grain-oriented electrical steel sheet according to an embodiment of the present invention.

[0019] A grain-oriented electrical steel sheet according to an embodiment of the present invention (the grain-oriented electrical steel sheet according to the present embodiment) and a method for manufacturing the grain-oriented electrical steel sheet according to the present embodiment, including a method for forming an insulating coating provided on the grain-oriented electrical steel sheet according to the present embodiment, will be described. First, the grain-oriented electrical steel sheet according to the present embodiment will be described.

[0020] As shown in Fig. 1, the grain-oriented electrical steel sheet 100 according to this embodiment has a base steel sheet 1 and an insulating coating 2 formed on the surface of the base steel sheet 1. In the grain-oriented electrical steel sheet 100 according to this embodiment, a forsterite-based coating is not intentionally formed on the surface of the base steel sheet 1, and in many cases a forsterite-based coating is not present.2 Its presence is permitted if it is below the specified value (in which case it is present between the base steel sheet 1 and the insulating coating 2). The insulating coating 2 has a tensile coating layer 22 formed on the surface side of the insulating coating 2 (i.e., the surface side of the grain-oriented electrical steel sheet 100), and an intermediate layer 21 formed on the side of the base steel sheet 1 and containing a crystalline metal phosphate. The intermediate layer 21 contains the crystalline metal phosphate and one or more of amorphous silica, an inorganic filler, and a metal oxide, each having an average particle size of 10 to 500 nm. Each of these will be described below.

[0021] <Base Steel Sheet> (Chemical Composition) The grain-oriented electrical steel sheet 100 according to this embodiment is significantly characterized by the structure of the insulating coating 2 formed on the surface of the base steel sheet 1, and the base steel sheet 1 included in the grain-oriented electrical steel sheet 100 is not limited in terms of its chemical composition. However, in order to obtain the properties generally required of a grain-oriented electrical steel sheet, it is preferable that the chemical components contain the following: In this embodiment, % relating to the chemical components is % by mass unless otherwise specified.

[0022] C: 0.010% or less C (carbon) is an element effective for controlling the structure of the steel sheet in the manufacturing process up to the completion of the decarburization annealing process. However, if the C content exceeds 0.010%, the magnetic properties of the finished grain-oriented electrical steel sheet deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the C content is preferably 0.010% or less. The C content is more preferably 0.005% or less. Although a lower C content is preferable, reducing the C content to less than 0.0001% saturates the effect of structural control and simply increases manufacturing costs. Therefore, the C content may be 0.0001% or more.

[0023] Si: 2.50 to 4.00% Si (silicon) is an element that increases the electrical resistance of grain-oriented electrical steel sheets and improves their iron loss characteristics. If the Si content is less than 2.50%, a sufficient eddy current loss reduction effect cannot be obtained. Therefore, the Si content is preferably 2.50% or more. The Si content is more preferably 2.70% or more, and even more preferably 3.00% or more. On the other hand, if the Si content exceeds 4.00%, the grain-oriented electrical steel sheets become embrittled and their threading properties deteriorate significantly. Furthermore, the workability of the grain-oriented electrical steel sheets decreases, and the steel sheets may break during rolling. Therefore, the Si content is preferably 4.00% or less. The Si content is more preferably 3.80% or less, and even more preferably 3.70% or less.

[0024] Mn: 0.01 to 0.50% Mn (manganese) is an element that combines with S to form MnS during the manufacturing process. This precipitate functions as an inhibitor (a suppressor of normal grain growth) and induces secondary recrystallization in the steel. Mn also enhances the hot workability of the steel. If the Mn content is less than 0.01%, the above-mentioned effects cannot be fully achieved. Therefore, the Mn content is preferably 0.01% or more. The Mn content is more preferably 0.02% or more. On the other hand, if the Mn content exceeds 0.50%, secondary recrystallization does not occur and the magnetic properties of the steel deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Mn content is preferably 0.50% or less. The Mn content is more preferably 0.20% or less, and even more preferably 0.10% or less.

[0025] N: 0.010% or less N (nitrogen) is an element that bonds with Al during the manufacturing process to form AlN, which functions as an inhibitor. However, if the N content exceeds 0.010%, excessive inhibitors remain in the base steel sheet of the grain-oriented electrical steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the N content is preferably 0.010% or less. The N content is more preferably 0.008% or less. On the other hand, the lower limit of the N content is not particularly specified, but reducing the N content to less than 0.001% only increases manufacturing costs. Therefore, the N content may be 0.001% or more.

[0026] Sol. Al: 0.020% or less Sol. Al (acid-soluble aluminum) is an element that bonds with N to form AlN, which functions as an inhibitor, during the manufacturing process of grain-oriented electrical steel sheets. However, if the sol. Al content of the base steel sheet exceeds 0.020%, excessive inhibitors remain in the base steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the sol. Al content is preferably 0.020% or less. The sol. Al content is more preferably 0.010% or less, and even more preferably less than 0.001%. There is no particular restriction on the lower limit of the sol. Al content, but reducing it to less than 0.0001% only increases manufacturing costs. Therefore, the sol. Al content may be 0.0001% or more.

[0027] S: 0.010% or less S (sulfur) is an element that combines with Mn during the manufacturing process to form MnS, which functions as an inhibitor. However, if the S content exceeds 0.010%, the magnetic properties will be reduced due to the remaining inhibitor. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the S content is preferably 0.010% or less. The S content in the grain-oriented electrical steel sheet is preferably as low as possible. For example, less than 0.001%. However, reducing the S content in the base steel sheet of the grain-oriented electrical steel sheet to less than 0.0001% will only increase the manufacturing cost. Therefore, the S content in the base steel sheet of the grain-oriented electrical steel sheet may be 0.0001% or more.

[0028] Balance: Fe and impurities The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment may contain the above-mentioned elements, with the balance being Fe and impurities. However, for the purpose of improving magnetic properties, etc., Sn, Cu, Se, and Sb may also be contained in the ranges shown below. Furthermore, even if other elements, such as W, Nb, Ti, Ni, Co, V, Cr, and Mo, are contained in a total of 1.0% or less, the effects of the grain-oriented electrical steel sheet according to this embodiment are not impaired. Here, impurities refer to elements that are mixed in from raw materials such as ore, scrap, or the manufacturing environment during industrial production of the base steel sheet, and are allowed to be contained in amounts that do not adversely affect the function of the grain-oriented electrical steel sheet according to this embodiment.

[0029] Sn: 0 to 0.50% Sn (tin) is an element that contributes to improving magnetic properties through controlling the primary recrystallization structure. To obtain the effect of improving magnetic properties, the Sn content is preferably 0.01% or more. The Sn content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Sn content exceeds 0.50%, secondary recrystallization becomes unstable and magnetic properties deteriorate. Therefore, the Sn content is preferably 0.50% or less. The Sn content is more preferably 0.30% or less, and even more preferably 0.10% or less.

[0030] Cu: 0 to 0.50% Cu (copper) is an element that contributes to increasing the Goss orientation occupancy rate in the secondary recrystallized structure. To achieve the above effect, the Cu content is preferably 0.01% or more. The Cu content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Cu content exceeds 0.50%, the steel sheet becomes embrittled during hot rolling. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Cu content is preferably 0.50% or less. The Cu content is more preferably 0.30% or less, and even more preferably 0.10% or less.

[0031] Se: 0 to 0.020% Se (selenium) is an element that has the effect of improving magnetic properties. When Se is contained, the Se content is preferably 0.001% or more to effectively exhibit the effect of improving magnetic properties. The Se content is more preferably 0.003% or more, and even more preferably 0.006% or more. On the other hand, if the Se content exceeds 0.020%, the adhesion of the coating deteriorates. Therefore, the Se content is preferably 0.020% or less. The Se content is more preferably 0.015% or less, and even more preferably 0.010% or less.

[0032] Sb: 0 to 0.50% Sb (antimony) is an element that has the effect of improving magnetic properties. When Sb is contained, the Sb content is preferably 0.005% or more to effectively exhibit the effect of improving magnetic properties. The Sb content is more preferably 0.01% or more, and even more preferably 0.02% or more. On the other hand, if the Sb content exceeds 0.50%, the adhesion of the coating significantly deteriorates. Therefore, the Sb content is preferably 0.50% or less. The Sb content is more preferably 0.30% or less, and even more preferably 0.10% or less.

[0033] As described above, the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet in this embodiment is, for example, one that contains the above-mentioned elements with the balance being Fe and impurities.

[0034] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment can be measured using a known ICP atomic emission spectroscopy. However, when an insulating coating is formed on the surface, it is removed before measurement. The removal can be achieved by immersing the sample in a highly concentrated alkaline solution (e.g., a 30% sodium hydroxide solution heated to 85°C) for 20 minutes or more. Peeling can be determined visually. For small samples, removal can also be achieved by surface grinding.

[0035] <Insulating Coating> The grain-oriented electrical steel sheet 100 according to this embodiment has an insulating coating 2 formed on the surface of a base steel sheet 1. The insulating coating 2 is made up of, in order from the base steel sheet 1 side, an intermediate layer 21 and a tensile coating layer 22.

[0036] (Intermediate Layer) As described above, grain-oriented electrical steel sheets generally have a forsterite-based coating formed in the final annealing process and an insulating coating (tensile insulating coating) formed thereon. However, in recent years, it has become clear that this forsterite-based coating hinders the movement of domain walls and adversely affects iron loss. Therefore, grain-oriented electrical steel sheets without a forsterite-based coating have been studied to further improve magnetic properties. However, if a forsterite-based coating is not present, it is difficult to ensure sufficient adhesion between the tensile coating and the surface of the base steel sheet.

[0037] In the grain-oriented electrical steel sheet 100 according to this embodiment, an intermediate layer 21 containing a crystalline metal phosphate is formed between the base steel sheet 1 and the tensile coating, thereby improving adhesion between the base steel sheet 1 and the tensile coating layer 22 via the intermediate layer 21. When the intermediate layer 21 contains a crystalline metal phosphate, the tensile coating formed thereon (which becomes the tensile coating layer 22 after formation) also contains a metal phosphate, resulting in high affinity and excellent adhesion between the intermediate layer and the tensile coating layer. Furthermore, when the intermediate layer is formed by immersion in a treatment solution containing a metal phosphate, as described below, it can be formed on the surface of the base steel sheet 1 using a chemical reaction, thereby ensuring adhesion between the intermediate layer 21 and the base steel sheet 1. If the intermediate layer 21 does not contain a crystalline metal phosphate, the above-described effect cannot be obtained. The proportion of the crystalline metal phosphate in the intermediate layer is preferably 80% by mass or more, preferably 90% by mass or more, and may be 99% by mass or more. In terms of adhesion, the metal phosphate is preferably one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate. The intermediate layer may contain oxides and elements such as Fe and Si diffused from the base steel sheet as the remainder of the metal phosphate.

[0038] However, if the crystals of the crystalline metal phosphate in the intermediate layer become coarse, the space factor decreases during the manufacture of an actual transformer, resulting in a decrease in magnetic flux density per unit volume and increased transformer iron loss. Therefore, in the grain-oriented electrical steel sheet according to this embodiment, in order to suppress the crystallization of the crystalline metal phosphate and thereby suppress the coarsening of the crystals, the treatment solution used to form the intermediate layer contains one or more additives selected from colloidal silica, inorganic filler, and metal oxide, each having an average particle size of 10 to 500 nm. As a result, the intermediate layer contains the crystalline metal phosphate and one or more of amorphous silica, inorganic filler, and metal oxide, with the amorphous silica, inorganic filler, and metal oxide having an average particle size of 10 to 500 nm. In such an intermediate layer, the average crystal grain size of the crystalline metal phosphate is, for example, 1.0 to 12.0 μm. At least one of colloidal silica, inorganic filler, and metal oxide having an average particle size of 10 to 500 nm is preferably dispersed uniformly in the intermediate layer without localization, for example, in the form of aggregates of several μm or less even if secondary aggregation occurs.

[0039] Among the amorphous silica, inorganic fillers, and metal oxides added as additives and remaining in the intermediate layer, amorphous silica is preferred in terms of ease of availability. Amorphous silica differs in both form and effect from crystalline silica produced by thermal oxidation annealing, etc. Furthermore, the inorganic filler preferably contains one or more of alumina, BN, AlN, and kaolin in an amount of 90% by mass or more (with a purity of 90% by mass or more). BN preferably has a hexagonal crystal structure in consideration of ease of dispersion. Furthermore, the metal oxide is preferably one or more of titanium oxide, zinc oxide, and calcium oxide in terms of the stability of the treatment solution. While carbonates can be used as additives, they do not remain in the intermediate layer under normal baking conditions, and special baking conditions are required to obtain an intermediate layer containing carbonates, making them undesirable. Furthermore, the content of one or more of amorphous silica, inorganic fillers, and metal oxides is preferably 0.01 to 1.00% by mass. If the content is less than 0.01% by mass, the effect of inhibiting the crystal coarsening of the metal phosphate will be inferior, and if it exceeds 1.00% by mass, there is a concern that the adhesion as an intermediate layer will be inferior.

[0040] The intermediate layer 21 is formed at a different time from the tensile coating formed thereon, but the intermediate layer 21 and the tensile coating layer 22 together function as the insulating coating 2 .

[0041] The thickness of the intermediate layer is preferably 1.0 to 9.0 μm. If the average thickness of the intermediate layer 21 is less than 1.0 μm, the effect of improving the adhesion between the base steel sheet and the insulating coating via the intermediate layer may not be sufficiently obtained. On the other hand, if the average thickness of the intermediate layer exceeds 9.0 μm, the magnetic properties may deteriorate.

[0042] The mass fraction and type of crystalline metal phosphate in the intermediate layer can be determined by measuring a cross section of the intermediate layer in the thickness direction using a scanning electron microscope and an energy dispersive elemental analyzer. Whether the metal phosphate in the intermediate layer 21 is crystalline can be determined by X-ray crystal structure analysis. The base steel sheet and the insulating coating can be distinguished by the P (phosphorus) concentration (if the P content is 1.0 mass% or more, it is determined to be an insulating coating, and if it is less than 1.0 mass%, it is determined to be a steel sheet). Within the insulating coating 2, the intermediate layer 21 and the tensile coating layer 22 can be distinguished by the difference in Si concentration (if the Si content is 10 mass% or more, it is determined to be a tensile coating layer, and if it is less than 10 mass%, it is determined to be an intermediate layer).

[0043] The average crystal grain size of the crystalline metal phosphate can be determined by the following method. A steel sheet is cut into pieces of several millimeters square to facilitate observation, and subjected to ion milling (CP processing) to remove microscopic shape defects such as sagging and cracks. Then, a cross section parallel to the rolling direction and thickness direction of the steel sheet, as well as a cross section perpendicular to the rolling direction and parallel to the thickness direction of the steel sheet, are observed using a scanning electron microscope. The crystalline morphology of the metal phosphate observed in the cross section is observed, and the average values ​​of the major and minor axes of at least five crystals are measured in each cross section, and these measurements are used as the grain size. The electron microscope magnification during observation is 1000x.

[0044] The contents and average particle diameters of amorphous silica, inorganic filler, and metal oxide can be determined by the following method. Regarding the contents, a steel sheet is cut into pieces several millimeters square for easy observation, and then subjected to ion milling (CP processing) to remove microscopic shape defects such as sagging and cracks. Then, cross sections parallel to the rolling direction and thickness direction of the steel sheet, as well as cross sections perpendicular to the rolling direction and parallel to the thickness direction of the steel sheet, are observed with a scanning electron microscope at 5,000x magnification. At least five cross sections are measured for each section, and the intermediate layer is analyzed using an energy dispersive elemental analyzer. Regarding the average particle diameter, the presence of amorphous silica, inorganic filler, and metal oxide is confirmed by elemental analysis at 10 or more locations in the intermediate layer of a cross-sectional sample similarly subjected to ion milling processing using a transmission electron microscope. The particle diameter is then calculated as the average of the major and minor axes of the particles observed at 20,000x magnification.

[0045] The thickness of the intermediate layer can be determined by the following method. The cross section of the sample is observed with a scanning electron microscope, and the thickness is measured at five or more points, allowing the average total thickness of the intermediate layer and the insulating coating to be determined. The intermediate layer and the insulating coating can be distinguished by the difference in silicon (Si) concentration derived from silica. Therefore, the thickness of the intermediate layer can be calculated by subtracting the thickness of the insulating coating from the total average thickness at each measurement point.

[0046] (Tension Coating Layer) In the grain-oriented electrical steel sheet 100 according to this embodiment, a tension coating is formed on the surface of the intermediate layer 21, resulting in a tension coating layer 22 on the surface side of the insulating coating 2. The tensile coating layer 22 is not particularly limited as long as it is used as an insulating coating for a grain-oriented electrical steel sheet. However, from the viewpoint of adhesion to the intermediate layer 21 (adhesion to the base steel sheet 1 via the intermediate layer 21), it is preferable that the tensile coating layer 22 has a composition primarily composed of metal phosphate and silica. It is more preferable that the tensile coating layer 22 essentially consists of metal phosphate and silica. The tensile coating layer 22 preferably contains metal phosphate and silica (derived from colloidal silica in the coating liquid) so that the silica content is 20.0% by mass or more. On the other hand, a silica content of more than 60.0% by mass can cause powdering, so the silica content of the tensile coating layer 22 is preferably 60.0% by mass or less. Furthermore, the tensile coating layer 22 preferably contains a total of 70% by mass or more of metal phosphate and silica. The total of the metal phosphate and silica may be 100% by mass. The remainder, other than the metal phosphate and silica, may include ceramic particles such as alumina or silicon nitride. Aluminum phosphate is preferred as the metal phosphate in terms of heat resistance. While the thickness of the tensile coating layer 22 is not limited, the average thickness of the insulating coating 2 (intermediate layer 21 + tensile coating layer 22) is preferably 1.0 to 20.0 μm, assuming that the average thickness of the intermediate layer 21 is within the above range. If the average thickness of the insulating coating 2 is less than 1.0 μm, sufficient coating tension cannot be obtained. Furthermore, excessive phosphate leaching occurs. This can cause stickiness and reduced corrosion resistance, potentially leading to coating peeling. Furthermore, if the thickness of the insulating coating 2 exceeds 20.0 μm, the space factor decreases, resulting in poor magnetic properties, and cracks can cause poor adhesion and reduced corrosion resistance.

[0047] In the tensile coating layer 22, the mass percentage of the metal phosphate and the type of the metal phosphate can be determined in the cross section in the thickness direction in the same manner as for the intermediate layer. As described above, the tensile coating layer and the intermediate layer can be distinguished by the Si content.

[0048] The thickness of the tensile coating layer can be determined in the same manner as for the intermediate layer. The sum of the thickness of the tensile coating layer and the thickness of the intermediate layer is the thickness of the insulating coating.

[0049] <Manufacturing Method> The grain-oriented electrical steel sheet according to this embodiment can be suitably manufactured by a manufacturing method that satisfies the manufacturing conditions described below. However, it goes without saying that the grain-oriented electrical steel sheet according to this embodiment is not particularly limited to a manufacturing method. In other words, a grain-oriented electrical steel sheet having the configuration described above is considered to be the grain-oriented electrical steel sheet according to this embodiment, regardless of its manufacturing conditions.

[0050] The grain-oriented electrical steel sheet according to this embodiment can be manufactured by a manufacturing method including the following steps: (I) a hot rolling step of hot-rolling a steel billet such as a slab having a predetermined chemical composition to obtain a hot-rolled sheet, (II) a hot-rolled sheet annealing step of annealing the hot-rolled sheet, (III) a cold-rolling step of cold-rolling the hot-rolled sheet after the hot-rolled sheet annealing step to obtain a steel sheet (cold-rolled sheet), (IV) a decarburization annealing step of decarburizing the steel sheet after the cold-rolling step, and (V) a step of adding Al to the steel sheet. 2 O 3(VI) an annealing separator removing step of removing excess annealing separator from the steel sheet after the final annealing step; and (VII) a light pickling step of pickling the steel sheet after the annealing separator removing step with a pickling solution containing 0.10 to 10.0 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid at a solution temperature of 30 to 85°C for 1 to 20 seconds. (VIII) an immersion step of immersing the steel sheet after the light pickling step in a treatment solution containing 0.3 to 10.0 mass % of a metal phosphate and 0.01 to 10.0 g / L of one or more of colloidal silica having an average particle size of 10 to 500 nm, an inorganic filler, and a metal oxide at a liquid temperature of 30 to 85°C for 5 to 150 seconds; (IX) a drying step of removing the steel sheet after the immersion step from the treatment solution, removing excess treatment solution, and then drying; and (X) a tensile coating layer formation step of applying a coating solution containing a metal phosphate and colloidal silica, wherein the total concentration of the metal phosphate and the colloidal silica is 10 to 40 mass %, to the steel sheet after the drying step, drying, and then heating and maintaining the steel sheet at a temperature of 700 to 950°C for 10 to 50 seconds. The method for producing a grain-oriented electrical steel sheet according to this embodiment may further include one or both of the following: (XI) a nitriding step in which the steel sheet is nitrided between the decarburization annealing step and the finish annealing step; and (XII) a magnetic domain refining step in which magnetic domain control of the steel sheet is performed after the tension coating layer forming step. Of these, the production of a grain-oriented electrical steel sheet according to this embodiment is characterized by the steps (V) finish annealing step to (X) tension coating layer forming step (which may be collectively referred to as the method for forming an insulation coating), which are primarily related to the formation of an insulation coating. Known conditions can be used for other steps or for conditions not described. These steps are described below.

[0051] [Hot Rolling Process] In the hot rolling process, a billet such as a slab having a predetermined chemical composition is heated and then hot rolled to obtain a hot-rolled sheet. The heating temperature of the billet is preferably within the range of 1100 to 1450°C. The heating temperature is more preferably 1300 to 1400°C. The chemical composition of the billet may be changed depending on the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet that is ultimately to be obtained, and may be, for example, in mass %, C: 0.01 to 0.20%, Si: 2.50 to 4.00%, sol. An example of a chemical composition is Al: 0.01 to 0.040%, Mn: 0.01 to 0.50%, N: 0.020% or less, S: 0.005 to 0.040%, Cu: 0 to 0.50%, Sn: 0 to 0.50%, Se: 0 to 0.020%, Sb: 0 to 0.50%, and the balance being Fe and impurities. The hot rolling conditions are not particularly limited and may be set appropriately based on the desired properties. The thickness of the hot-rolled sheet is preferably within the range of 2.0 to 3.0 mm, for example.

[0052] [Hot-rolled sheet annealing process] The hot-rolled sheet annealing process is a process of annealing a hot-rolled sheet manufactured through a hot rolling process. This annealing process is preferable because it causes recrystallization in the steel sheet structure and enables the realization of good magnetic properties. When hot-rolled sheet annealing is performed, the hot-rolled sheet manufactured through the hot rolling process may be annealed according to a known method. The means for heating the hot-rolled sheet during annealing is not particularly limited, and known heating methods can be adopted. The annealing conditions are also not particularly limited. For example, the hot-rolled sheet can be annealed in a temperature range of 900 to 1200°C for 10 seconds to 5 minutes.

[0053] [Cold Rolling Process] In the cold rolling process, the hot-rolled sheet after the hot-rolled sheet annealing process is subjected to cold rolling to obtain a steel sheet (cold-rolled sheet). The cold rolling may be a single cold rolling (a series of cold rolling processes without annealing in between), or multiple cold rolling processes with intermediate annealings may be performed by interrupting the cold rolling and performing at least one or two or more intermediate annealings before the final pass of the cold rolling process. When intermediate annealing is performed, it is preferable to hold the temperature at 1000 to 1200°C for 5 to 180 seconds. The annealing atmosphere is not particularly limited. Considering production costs, the number of intermediate annealings is preferably three or less. Furthermore, the surface of the hot-rolled sheet may be pickled before the cold rolling process.

[0054] In the cold rolling process according to this embodiment, the hot-rolled sheet after the hot-rolled sheet annealing process is cold-rolled according to a known method to obtain a steel sheet. For example, the final reduction can be in the range of 80 to 95%. A final reduction of 80% or more is preferable because it is possible to obtain Goss nuclei with a high concentration of {110}<001> orientation in the rolling direction. On the other hand, a final reduction of more than 95% is not preferable because it increases the possibility of secondary recrystallization becoming unstable in the subsequent finish annealing process. The final reduction is the cumulative reduction of cold rolling, and if intermediate annealing is performed, it is the cumulative reduction of cold rolling after final intermediate annealing.

[0055] [Decarburization Annealing Step] In the decarburization annealing step, the obtained steel sheet is subjected to decarburization annealing. In the decarburization annealing, the conditions for the decarburization annealing are not limited as long as the steel sheet undergoes primary recrystallization and C, which adversely affects magnetic properties, can be removed from the steel sheet. For example, the oxidation degree (PH) in the annealing atmosphere (furnace atmosphere) can be adjusted. 2 O / PH 2 ) is set to 0.3 to 0.6, the annealing temperature is 800 to 900°C, and the holding time is 10 to 600 seconds.

[0056] [Nitriding Process] Nitriding may be performed between the decarburization annealing process and the finish annealing process described below. In the nitriding process, for example, the steel sheet after the decarburization annealing process is maintained at approximately 700 to 850°C in a nitriding atmosphere (an atmosphere containing hydrogen, nitrogen, and ammonia or other nitriding gases) to perform nitriding. When AlN is used as an inhibitor, it is preferable to set the N content of the steel sheet after the nitriding process to 40 ppm or more by the nitriding process. On the other hand, if the N content of the steel sheet after the nitriding process exceeds 1000 ppm, excess AlN remains in the steel sheet even after the completion of secondary recrystallization in the finish annealing. Such AlN can cause iron loss degradation. For this reason, it is preferable to set the N content of the steel sheet after the nitriding process to 1000 ppm or less.

[0057] [Finish annealing step] In the finish annealing step, Al is added to the steel sheet after the decarburization annealing step or after the nitriding treatment (after the nitriding treatment step). 2 O 3 In a conventional method for producing grain-oriented electrical steel sheets, an annealing separator containing 10 to 100 mass % of Al is applied, dried, and then finish annealed. In contrast, in the method for producing grain-oriented electrical steel sheets according to the present embodiment, a forsterite-based coating is formed on the surface of the steel sheet (cold-rolled sheet) by applying an annealing separator mainly containing MgO and then finish annealing. 2 O 3 On the other hand, an annealing separator containing Al is used. 2 O 3 The ratio of Al may be 100 mass %, but 2 O 3 From the viewpoint of preventing seizure of Al, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator preferably contains MgO. Although the content of MgO may be 0%, in order to obtain the above effect, the content of MgO is preferably 5 mass% or more. When MgO is contained, the content of MgO is preferably 10 mass% or more. 2 O 3 The content of Al relative to the annealing separator is 90 mass % or less to ensure this. The content of MgO is preferably 50 mass % or less. 2 O 3The total of MgO and MgO may be more than 50% by mass in terms of solid content. Furthermore, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator may further contain chloride. The inclusion of chloride in the annealing separator provides the effect of making it more difficult for a forsterite-based coating to form. The chloride content is not particularly limited and may be 0%, but to obtain the above effect, 0.5 to 10% by mass is preferred. Examples of effective chlorides include bismuth chloride, calcium chloride, cobalt chloride, iron chloride, and nickel chloride. The finish annealing conditions are not limited, but for example, a temperature of 1150 to 1250°C for 10 to 60 hours can be employed.

[0058] [Annealing Separator Removal Step] In the annealing separator removal step, excess annealing separator is removed from the steel sheet after the finish annealing step. For example, the excess annealing separator can be removed by washing with water.

[0059] [Light Pickling Process] In the light pickling process, the steel sheet after the annealing separator removal process is pickled at a solution temperature of 30 to 85°C with 0.1 to 10.0 mass% of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid for 1 to 20 seconds. The inorganic acid is preferably one selected from sulfuric acid, nitric acid, and phosphoric acid. This has the effect of densifying the crystalline metal phosphate. If the light pickling conditions are inappropriate, the adhesion of the tension coating layer may be poor or the elution resistance may be poor.

[0060] [Immersion Process] [Drying Process] In the immersion process, the steel sheet after the light pickling process is immersed in a treatment solution for 5 to 150 seconds. In the drying process, the steel sheet after the immersion process is removed from the treatment solution, excess treatment solution is removed, and the steel sheet is then dried. This results in the formation of an intermediate layer on the surface of the base steel sheet. In the immersion process, the treatment solution is adjusted to a temperature of 30 to 85°C and to contain 0.3 to 10 mass% of a metal phosphate salt and 0.01 to 10.0 g / L of one or more of colloidal silica, inorganic filler, and metal oxide, each having an average particle size of 10 to 500 nm. The inclusion of colloidal silica (which becomes amorphous silica in the intermediate layer), inorganic filler, and one or more of metal oxide (sometimes referred to as additives) suppresses crystallization of the metal phosphate salt that forms the intermediate layer, resulting in a smaller average crystal particle size of the crystalline metal phosphate salt in the intermediate layer. However, if the content of the additive in the treatment solution is less than 0.01 g / L, sufficient effects cannot be obtained. On the other hand, if it exceeds 10.0 g / L, the treatment solution becomes unstable. Furthermore, if the average particle size of the additive is less than 10 nm, aggregation occurs, making the treatment solution unstable. Alternatively, if the average particle size is more than 500 nm, the particles precipitate, resulting in poor dispersibility in the treatment solution.

[0061] If the temperature of the treatment solution is below 30°C or the treatment time is less than 5 seconds, the adhesion will be poor. On the other hand, if the temperature of the solution is above 85°C or the treatment time is more than 150 seconds, the average crystal grain size of the crystalline metal phosphate will become too large. On the other hand, if the metal phosphate content of the treatment solution is more than 10% by mass, the average crystal grain size of the metal phosphate will become coarse, which may cause a decrease in adhesion. The metal phosphate contained in the treatment solution may be one or more of zinc phosphate, manganese phosphate, and zinc calcium phosphate. On the other hand, if the metal phosphate content of the treatment solution is less than 0.3% by mass, the formation of the intermediate layer will be slow, resulting in high industrial costs. To achieve a uniform thickness for the intermediate layer, the metal phosphate content is preferably 1.0% by mass or more. Furthermore, since a high drying temperature may cause voids to form, resulting in poor adhesion, the drying temperature is preferably 300°C or less, more preferably 200°C or less. The drying temperature is preferably 100°C or more.

[0062] [Tension Coating Layer Formation Process] In the tension coating layer formation process, a coating liquid containing a metal phosphate and colloidal silica, with a total concentration of the metal phosphate and colloidal silica of 10 to 40% by mass, is applied to the steel sheet after the drying process, dried, and then heated and held at a sheet temperature of 700 to 950°C for 10 to 50 seconds to form a tension coating layer on the surface of the intermediate layer. If the sheet temperature during holding is less than 700°C, the tension will be low and the magnetic properties will be poor. Therefore, it is preferable that the sheet temperature be 700°C or higher. On the other hand, if the sheet temperature is higher than 950°C, the rigidity of the steel sheet will decrease and it will be prone to deformation. In this case, the steel sheet may be distorted during transportation, etc., resulting in poor magnetic properties. Therefore, it is preferable that the sheet temperature be 950°C or lower. Furthermore, if the holding time is less than 10 seconds, the elution resistance will be poor. Therefore, the holding time is set to 10 seconds or more. On the other hand, if the holding time is longer than 50 seconds, the adhesion of the tensile coating layer will be poor. Therefore, the retention time is preferably 50 seconds or less. The coating liquid (insulation coating solution) should contain 10 to 40 mass% of metal phosphate and colloidal silica. If the total concentration of metal phosphate and colloidal silica is less than 10 mass%, the applied treatment liquid will tend to flow, causing uneven application. If it exceeds 40 mass%, the viscosity will be too high, causing uneven patterns and application. As the metal phosphate, for example, one or a mixture of two or more selected from aluminum phosphate, zinc phosphate, magnesium phosphate, nickel phosphate, copper phosphate, lithium phosphate, cobalt phosphate, etc. can be used. Aluminum phosphate is preferred in terms of the stability of the treatment liquid.

[0063] The coating solution may contain additional elements such as vanadium, tungsten, molybdenum, and zirconium. When these elements are contained, they can be added to the coating solution, for example, as an oxyacid. S-type and C-type colloidal silica can be used. S-type colloidal silica refers to an alkaline silica solution, while C-type colloidal silica refers to an alkaline to neutral silica solution in which the silica particle surface is aluminum-treated. S-type colloidal silica is widely used and relatively inexpensive, but caution is required as it may aggregate and precipitate when mixed with an acidic metal phosphate solution. C-type colloidal silica is stable even when mixed with a metal phosphate solution and does not precipitate, but is relatively expensive due to the large number of processing steps required. It is preferable to use the appropriate type depending on the stability of the coating solution to be prepared.

[0064] [Magnetic Domain Refinement Process] The manufacturing method of the grain-oriented electrical steel sheet according to this embodiment may further include a magnetic domain refinement process in which the steel sheet after the tension coating layer formation process is subjected to magnetic domain refinement. Performing the magnetic domain refinement process can further reduce the iron loss of the grain-oriented electrical steel sheet. Examples of magnetic domain refinement processes include narrowing the width of 180° magnetic domains (refining 180° magnetic domains) by forming linear or point-like grooves extending in a direction intersecting the rolling direction at predetermined intervals along the rolling direction, and narrowing the width of 180° magnetic domains (refining 180° magnetic domains) by forming linear or point-like stress-strained portions or grooves extending in a direction intersecting the rolling direction at predetermined intervals along the rolling direction. Laser beam irradiation, electron beam irradiation, and the like can be used to form stress-strained portions. Grooves can be formed by mechanical groove formation using gears or the like, chemical groove formation using electrolytic etching, or thermal groove formation using laser irradiation. If the insulating coating is damaged by the formation of stress-strained portions or grooves, and the insulating properties and other characteristics are deteriorated, the insulating coating may be formed again to repair the damage.

[0065] A slab containing, by mass%, C: 0.08%, Si: 3.31%, sol. Al: 0.028%, N: 0.008%, Mn: 0.07%, S: less than 0.0005%, with the balance being Fe and impurities was cast. The slab was heated to 1350°C and then hot-rolled to obtain a hot-rolled sheet having a thickness of 2.2 mm. This hot-rolled sheet was annealed at 1100°C for 10 seconds. (Hot-rolled sheet annealing) The hot-rolled sheet was then cold-rolled to obtain a cold-rolled sheet having a thickness of 0.22 mm. This cold-rolled sheet was subjected to decarburization annealing at 830°C for 90 seconds. After decarburization annealing, 45 mass% MgO and Al were added. 2 O 3 50% by mass of bismuth chloride BiCl 3 An annealing separator containing 5% by mass of the above was applied to the steel sheet, which was then dried and then finish annealed at 1200°C for 20 hours. After finish annealing, the steel sheet was rinsed with water to remove excess annealing separator, and it was found that no forsterite-based coating was formed on the steel sheet surface. This steel sheet was lightly pickled under the conditions shown in Table 2-1. After light pickling, an intermediate layer was formed using a treatment solution containing a mixture of phosphate and additives shown in Table 1. The drying temperature was 200°C. The obtained intermediate layer was as shown in Table 2-2. The proportion of crystalline metal phosphate in the intermediate layer was 80% by mass or more.

[0066] Thereafter, an insulating coating treatment solution containing metal phosphate and colloidal silica as its main components, as shown in Table 2-3, was applied to the steel sheet surface, which was then dried at 850°C for 20 seconds to form a tensile coating layer. The thickness of the insulating coating (intermediate layer and tensile coating layer) was as shown in Table 2-3. The tensile coating layer consisted essentially of metal phosphate and silica.

[0067]

[0068]

[0069]

[0070]

[0071] The resulting steel sheet (grain-oriented electrical steel sheet) was subjected to magnetic domain refinement by irradiating it with a laser beam at a UA (irradiation energy density) of 2.0 J and a 5.0 mm interval. The iron loss W17 / 50 (iron loss at 50 Hz and 1.7 T) of the steel sheet after the magnetic domain refinement treatment was measured using a single sheet tester (SST) in accordance with JIS C2556 (2015). The space factor was also measured as follows.

[0072] [Space Factor] The space factor was measured according to a method in accordance with JIS C 2550-5 (2020). Thirty test pieces, each 30 mm wide and 320 mm long, were used. After measuring the total mass of the sample, the distance between the upper and lower backing plates sandwiching the laminate was measured under a pressure of 1 MPa, and then calculated. If the space factor was 96.0% or higher, it was determined that a high space factor was ensured.

[0073] The steel sheets after the magnetic domain refining treatment were evaluated for coating adhesion, coating tension, corrosion resistance, and elution resistance by the following methods. The results are shown in Table 3.

[0074] [Coating Adhesion] Coating adhesion was evaluated by taking a sample 30 mm wide and 300 mm long from the steel sheet, subjecting this sample to stress relief annealing at 800°C for 2 hours in a nitrogen stream, and then winding it around a 10 mmφ cylinder and unwinding it to a bending adhesion test. The coating adhesion was evaluated based on the degree of peeling (area ratio) of the coating. The evaluation criteria were as follows, and A or B was determined to be excellent in coating adhesion. A: Peeling area ratio 0 to 0.5% B: Peeling area ratio more than 0.5% and 5.0% or less C: Peeling area ratio more than 5.0% and 20% or less D: Peeling area ratio more than 20% and 50% or less E: Peeling area ratio more than 50%

[0075] [Coating Tension] The coating tension was calculated by back-calculating from the state of curvature when one side of the insulating coating was peeled off. When the obtained coating tension was 4.0 MPa or more, it was determined that the coating tension was sufficient.

[0076] [Corrosion Resistance] Corrosion resistance was evaluated in accordance with the JIS salt spray test (JIS Z2371:2015), in which a 5% NaCl aqueous solution was allowed to fall naturally onto the sample for 7 hours in an atmosphere at 35°C. The rust area was then evaluated on a 10-point scale. The evaluation criteria were as follows: A score of 5 or more (5 to 10) was considered to be excellent in corrosion resistance. 10: No rust occurred 9: Very little rust occurred (area ratio = 0.10% or less) 8: Area ratio where rust occurred = more than 0.10% but not more than 0.25% 7: Area ratio where rust occurred = more than 0.25% but not more than 0.50% 6: Area ratio where rust occurred = more than 0.50% but not more than 1.0% 5: Area ratio where rust occurred = more than 1.0% but not more than 2.5% 4: Area ratio where rust occurred = more than 2.5% but not more than 5.0% 3: Area ratio where rust occurred = more than 5.0% but not more than 10% 2: Area ratio where rust occurred = more than 10% but not more than 25% 1: Area ratio where rust occurred = more than 25% but not more than 50%

[0077] [Elution Resistance] Elution resistance was evaluated based on whether or not the elution of phosphoric acid from the sample could be suppressed. The amount of elution was measured by boiling the sample in boiling pure water for 10 minutes, measuring the amount of phosphoric acid eluted in the pure water, and dividing the amount of phosphoric acid by the area of ​​the insulating coating of the boiled grain-oriented electrical steel sheet. The amount of phosphoric acid eluted in the pure water was measured by cooling the pure water (solution) into which the phosphoric acid had eluted, and measuring the phosphoric acid concentration of the sample obtained by diluting the cooled solution with pure water using ICP-AES. When the elution amount was 40 mg / m 2 If the resistance is less than this, the resin is deemed to have excellent resistance to elution.

[0078]

[0079] As can be seen from Tables 1 to 3, the examples of the present invention were extremely excellent in the main coating properties, including adhesion, and had improved core loss and space factor. On the other hand, the comparative examples did not have a desirable insulating coating configuration, and were inferior in one or more of the adhesion of the tensile coating, magnetic properties, corrosion resistance, resistance to phosphoric acid elution, and space factor of the transformer (core).

[0080] According to the present invention, it is possible to provide a grain-oriented electrical steel sheet that has excellent adhesion of a tension coating and magnetic properties, and that does not reduce the space factor of a transformer (core), and therefore has high industrial applicability.

[0081] 100 Grain-oriented electrical steel sheet 1 Base steel sheet 2 Insulation coating 21 Intermediate layer 22 Tensile coating layer

Claims

1. A grain-oriented electrical steel sheet comprising: a base steel sheet; and an insulating coating formed on the surface of the base steel sheet, wherein the insulating coating comprises: an intermediate layer formed on the base steel sheet side and containing a crystalline metal phosphate and one or more of amorphous silica, an inorganic filler, and a metal oxide; and a tensile coating layer formed on the surface side of the insulating coating, wherein the average particle size of the one or more of the amorphous silica, the inorganic filler, and the metal oxide is 10 to 500 nm.

2. The grain-oriented electrical steel sheet according to claim 1, wherein the inorganic filler contains one or more of alumina, BN, AlN, and kaolin.

3. The grain-oriented electrical steel sheet according to claim 1 or 2, wherein the metal oxide is one or more of titanium oxide, zinc oxide, and calcium oxide.

4. The grain-oriented electrical steel sheet according to claim 1 or 2, wherein the average crystal grain size of the crystalline metal phosphate is 1.0 to 12.0 μm.

5. A method for forming the insulating coating of the grain-oriented electrical steel sheet according to claim 1, comprising the steps of: 2 O 3 a final annealing step of applying an annealing separator containing 10 to 100 mass% of the above-mentioned, drying the steel sheet, and then performing final annealing; an annealing separator removing step of removing excess annealing separator from the steel sheet after the final annealing step; a light pickling step of pickling the steel sheet after the annealing separator removing step with a pickling solution containing 0.10 to 10.0 mass% of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid at a liquid temperature of 30 to 85°C for 1 to 20 seconds; and an immersion step of immersing the steel sheet after the light pickling step in a treatment solution containing 0.3 to 10.0 mass% of a metal phosphate and 0.01 to 10.0 g / l of one or more of colloidal silica, inorganic filler, and metal oxide having an average particle size of 10 to 500 nm at a liquid temperature of 30 to 85°C for 5 to 150 seconds. a drying step of removing the steel sheet after the immersion step from the treatment liquid, removing excess treatment liquid, and then drying the steel sheet; and a tensile coating layer formation step of applying a coating liquid containing a metal phosphate and colloidal silica, the metal phosphate and the colloidal silica having a total concentration of 10 to 40 mass %, to the steel sheet after the drying step, drying the steel sheet, and then heating the steel sheet to maintain a sheet temperature of 700 to 950° C. for 10 to 50 seconds.

Citation Information

Patent Citations

  • JP1973039338A

  • JP1974096920A

  • Video recording and reproducing system

    JP1989209891A

  • Formation of insulated film on grain-oriented silicon steel sheet

    JP1994184762A

  • Communication device, communication system, and communication method

    JP2023064836A