Secondary battery and preparation method therefor and electric device
By using silane-type additives in lithium-ion batteries to react with the carbon material coating to form a CEI film, and forming an SEI film on the surface of the negative electrode, the problem of side reactions between the electrolyte and the electrode material is solved, and the cycle performance and performance of the battery are improved. High temperature performance extends battery life.
Patent Information
- Application Number
- PCT/CN2024/086582
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-24
AI Technical Summary
Existing lithium-ion batteries have serious side reactions between electrolyte and electrode materials under high temperature conditions, leading to active lithium consumption, carbon material coating layer clogging and battery performance degradation, and cannot effectively reduce side reactions between electrolyte and electrode materials. , affecting cycle stability and energy density.
Silane-type additives are introduced into the battery, and their dosage is determined based on the specific surface area of the positive active material and the carbon material content, so that it reacts with the active sites of the carbon material coating layer to form a CEI film and passivate the carbon material coating layer. Suppress side reactions and form an SEI film on the surface of the negative electrode to isolate the electrolyte from contact with the electrode material.
It effectively reduces battery impedance, improves cycle performance and high temperature performance, extends battery life, and improves electrochemical performance and safety performance.
Smart Images

Figure CN2024086582_24102024_PF_FP_ABST
Abstract
Description
Secondary battery and preparation method thereof, and electrical equipment
[0001] This application claims priority to the Chinese patent application filed with the State Intellectual Property Office on April 17, 2023, with application number 202310458768.2 and application name “Secondary battery and its preparation method, and electrical equipment”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of battery technology, and in particular to a secondary battery, a preparation method thereof, and electrical equipment. Background Art
[0003] Lithium-ion batteries, with their high energy density, high discharge voltage, and long cycle life, are widely used in electronic devices, electric vehicles (EVs), hybrid electric vehicles (HEVs), energy storage, and other fields. With the development of the power and energy storage markets, people's requirements for lithium-ion battery life and operating environment are constantly increasing. Developing lithium-ion batteries with long life and a wide temperature range has become a top priority.
[0004] Especially under extreme conditions such as high temperature and low temperature, problems such as the circulation and safety of lithium-ion batteries become particularly prominent. As an important component of lithium-ion batteries, the electrolyte is closely related to various performances of the battery. At present, in order to improve the conductivity of the positive electrode material, a carbon material layer is often coated on the surface of the positive electrode material. However, the carbon material on its surface is prone to defects or loose coating during the preparation process, causing the electrolyte to decompose at the interface between the positive electrode and the electrolyte under the action of the oxidation potential, and consume active lithium, resulting in an increase in electrolyte side reactions. Especially under high temperature conditions, the side reactions of the electrolyte will be aggravated, which will accelerate the decomposition at the interface between the positive electrode and the electrolyte, consume active lithium, and even cause the lithium-conducting channels of the carbon material coated on the surface of the positive electrode active material to be blocked or the structure to collapse, resulting in the dissolution of metal ions in the positive electrode active material, causing the battery's electrochemical properties such as cycle stability, energy density, and rate performance to decay rapidly.
[0005] Summary of the Invention
[0006] The purpose of the present application is to provide a secondary battery and a preparation method thereof, as well as an electrical device, in order to solve the problem that the side reaction between the electrolyte and the electrode material in the existing secondary battery limits the battery performance.
[0007] To achieve the above application objectives, the technical solutions adopted in this application are as follows:
[0008] In a first aspect, the present application provides a secondary battery, which includes a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode contains a positive electrode active material, the positive electrode active material includes an active material core and a carbon material coating layer, the electrolyte includes an electrolyte salt, an organic solvent and an additive, and the additive includes a silane-type additive; wherein the amount of the silane-type additive is determined according to the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material.
[0009] The secondary battery provided herein includes an electrolyte additive containing a silane-type additive. During the initial charge and discharge process of the battery, the silane-type additive preferentially reacts with active sites such as oxygen-containing functional groups in the carbon material on the surface of the positive electrode active material, preferentially being oxidized to form silane and heteroatom-containing compounds, forming a CEI film on the positive electrode surface. This deactivates the reactivity of the surface of the carbon material coating, inhibits disordering of the carbon material coating, and prevents the active sites in the carbon material coating in the positive electrode active material from contacting with other components in the electrolyte to catalyze side reactions. This reduces the irreversible consumption of active metal ions and the risk of blockage or structural collapse of the metal ion-conducting channels in the carbon material coating in the positive electrode active material, thereby increasing the order of the carbon material coating and ensuring metal ion transport. This achieves the goals of reducing battery impedance, improving battery cycle performance, and improving high-temperature performance. Furthermore, the dosage of the silane-type additive in this application is determined based on the specific surface area of the positive electrode active material and the carbon material content in the positive electrode active material. The appropriate dosage of the required additive is determined based on the physical and chemical properties of the electrode material, which can guide the design of the electrode material and electrolyte combination. Avoid problems such as inappropriate use of additives in the electrolyte, which leads to the inability to effectively reduce side reactions between the electrolyte and electrode materials and reduce internal resistance, thereby better ensuring the electrochemical performance of the secondary battery.
[0010] As some possible implementations of the secondary battery of the present application, in the secondary battery, the mass percentage of the silane type additive in the electrolyte is marked as f, in %, and the specific surface area of the positive electrode active material is marked as a, in m 2 / g, and the mass percentage of the carbon material in the positive electrode active material is marked as e, in units of %, so that Z = f / (a*e) satisfies 0.001≤Z≤15. In this case, the electrode material and electrolyte in the battery have a better matching effect, which can effectively reduce the side reaction between the electrolyte and the electrode material, reduce impedance and improve the battery cycle performance, thereby improving the high-temperature performance of the battery.
[0011] As some possible implementations of the secondary battery of the present application, the silane additive includes at least one of tris(trimethylsilane) phosphate, tris(trimethylsilane) borate, tris(trimethylsilane) phosphite, tris(triethylsilane) phosphate, tris(triethylsilane) borate, tris(triethylsilane) phosphite, tris(trifluoromethylsilane) phosphate, tris(trifluoromethylsilane) borate, tris(trifluoromethylsilane) phosphite, tris(trifluoroethylsilane) phosphate, tris(trifluoroethylsilane) borate, and tris(trifluoroethylsilane) phosphite. In this case, these silane additives have a more suitable oxidation potential than other additives. During the first charge and discharge process of the battery, the silane additive preferentially reacts with active sites such as oxygen-containing functional groups in the carbon material on the surface of the positive electrode active material, passivates the reactivity of the carbon material coating layer, inhibits the disorder of the carbon material coating layer, and is preferentially oxidized to generate silanes and compounds containing heteroatoms such as phosphorus and boron, forming a CEI film on the positive electrode surface.
[0012] As some possible implementations of the secondary battery of the present application, the mass percentage of the silane-type additive in the electrolyte is 0.01% to 1.0%. In the case of this added content, the reactive sites and defects on the surface of the carbon material coating layer can be fully passivated, a CEI film can be formed on the positive electrode surface, the disorder of the carbon material coating layer can be better reduced, the ion transfer efficiency can be improved, the side reactions between the electrolyte and the positive electrode material can be reduced, the irreversible consumption of active metal ions can be reduced, the structure of the metal ion channel of the carbon material coating layer can be maintained, the battery impedance can be reduced, the battery cycle performance and safety performance can be improved, and the high-temperature performance can be improved.
[0013] As some possible implementations of the secondary battery of this application, the mass percentage of carbon material in the positive electrode active material is 0.5% to 5%. In this case, the content of the carbon material coating layer in the positive electrode active material can ensure sufficient and complete coating of the active material core, improve the conductivity of the active material core, and help reduce internal resistance and polarization, thereby improving the battery's cycle life, fast charging performance, and energy efficiency.
[0014] As some possible implementations of the secondary battery of the present application, the specific surface area of the positive electrode active material is 0.1 m 2 / g~20m 2 This specific surface area not only ensures a large active surface area for ion deintercalation during the charge and discharge process, but also helps control the side reactions between the positive electrode active material and the electrolyte.
[0015] As some possible implementations of the secondary battery of the present application, the active material core includes at least one of metal oxides and polyanion salts. In this case, the active materials contained in the core of the positive electrode active material have high capacity, safety and other characteristics.
[0016] As some possible implementations of the secondary battery of the present application, the metal oxides include at least one of lithium cobaltate, lithium nickelate, lithium nickel cobalt manganeseate, lithium nickel cobalt aluminumate, lithium manganeseate, lithium nickel manganeseate, and lithium vanadate; these active materials have high capacity, safety and other characteristics.
[0017] As some possible implementations of the secondary battery of the present application, the polyanion salt includes at least one of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium nickel phosphate, lithium iron silicate, lithium ferrous fluorosulfate, lithium iron borate, and lithium iron titanate. In this case, the core of the polyanion salt positive electrode active material has a stable polyhedral framework structure, which has better structural and thermodynamic stability, and can achieve higher cyclability and safety.
[0018] As some possible implementations of the secondary battery of the present application, when the active material core includes metal oxides, the specific surface area of the positive electrode active material is 0.1 m 2 / g~1.0m 2 / g, and satisfying 0.01≤Z≤15. Under this condition, the side reactions between the electrolyte and the electrode material can be effectively reduced, the impedance can be reduced, the battery cycle performance can be improved, and the high-temperature performance of the battery can be improved.
[0019] As some possible implementations of the secondary battery of the present application, when the active material core includes metal oxides, the specific surface area of the positive electrode active material is 0.2 m 2 / g~0.8m 2 / g, and satisfying 0.02≤Z≤10. In this case, the side reaction between the electrolyte and the electrode material can be more effectively reduced, the impedance can be reduced, the battery cycle performance can be improved, and the high-temperature performance of the battery can be improved.
[0020] As some possible implementations of the secondary battery of the present application, when the active material core includes polyanion salts, the specific surface area of the positive electrode active material is 7m 2 / g~20m 2 / g; and 0.001≤Z≤0.2. Under these conditions, the side reactions between the electrolyte and the electrode materials can be effectively reduced, the impedance can be reduced, the battery cycle performance can be improved, and the high-temperature performance of the battery can be improved.
[0021] As some possible implementations of the secondary battery of the present application, when the active material core includes polyanion salts, the specific surface area of the positive electrode active material is 9m 2 / g~15m 2 / g; and 0.002≤Z≤0.1. In this case, the side reactions between the electrolyte and the electrode material can be more effectively reduced, the impedance can be reduced, the battery cycle performance can be improved, and the high-temperature performance of the battery can be improved.
[0022] As some possible implementations of the secondary battery of the present application, the peak intensity ratio of the D peak to the G peak of the positive electrode active material Raman test is R=I D / I G , R ranges from 0.6 to 1.3. In this case, it is ensured that there are suitable ion migration and transmission channels in the carbon material coating layer on the surface of the positive electrode active material.
[0023] As some possible implementations of the secondary battery of the present application, the peak intensity ratio R of the D peak to the G peak in the Raman test of the positive electrode active material ranges from 0.8 to 1.2. In this case, the surface carbon material coating layer in the positive electrode active material of the secondary battery can better balance improving the conductivity of the core of the positive electrode active material and achieving more suitable ion migration and transmission efficiency.
[0024] As some possible implementations of the secondary battery of the present application, the additive also includes vinylene carbonate. In this case, the vinylene carbonate can undergo an electrochemical reaction on the negative electrode surface during the initial charge and discharge process of the secondary battery to form a solid electrolyte interface film, or SEI film, which effectively inhibits the embedding of solvent molecules and the battery's bloating, thereby improving the battery capacity and lifespan.
[0025] As some possible implementations of the secondary battery of the present application, the weight percentage of vinylene carbonate in the electrolyte is 0.1% to 5%. In this case, the weight percentage of vinylene carbonate in the electrolyte of 0.1% to 5% fully ensures its film-forming effect on the surface of the negative electrode, forming a SEI film, isolating the electrolyte from the negative electrode material, and inhibiting the deposition and reduction of metal ions at the negative electrode to form dendrites that damage the negative electrode structure and the stability of the SEI film.
[0026] As some possible implementations of the secondary battery of the present invention, electrolyte salts include LiClO4, LiBF4, LiPF6, LiAsF6, LiCF3SO3, LiTDI, Li[(CF3SO2)2N], Li[(FSO2)2N], Li[(C m F 2m+1 SO2)(C n F 2n+1 SO2)N], wherein m and n are natural numbers. In this case, these electrolytic salts can ensure high ionic conductivity of the electrolyte, do not cause harmful side reactions with electrode materials, electrolytes, diaphragms, etc., and have good chemical stability.
[0027] As some possible implementations of the secondary battery of the present application, the molar concentration of the electrolyte salt is 0.01 mol / L to 5.0 mol / L. In this case, the electrolyte salt with a molar concentration of 0.01 mol / L to 5.0 mol / L in the electrolyte can ensure high ionic conductivity of the electrolyte.
[0028] In some possible implementations of the secondary battery of the present application, the organic solvent includes at least one of a carbonate solvent, an ether solvent, and a carboxylate solvent. In this case, the at least one organic solvent among the carbonate solvent, the ether solvent, and the carboxylate solvent has good solubility for the electrolyte salt, and also has a low melting point, a high boiling point, a low vapor pressure, a wide operating temperature range, a high dielectric constant, a low viscosity, and high conductivity.
[0029] As some possible implementation methods of the secondary battery of the present application, the electrolyte also contains at least one auxiliary additive of biphenyl, fluorobenzene, trifluoromethyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, vinyl ethylene carbonate, 1,3-propane sultone, 1,4-butane sultone, 1,3-propylene sulfate lactone, vinyl sulfate, vinyl sulfite, methanedisulfonic acid methylene ester, succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,3,6-hexanetrinitrile, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), and lithium difluorophosphate. In this case, the electrolyte may also contain auxiliary additives. By adding auxiliary additives, the stability of the CEI and SEI films can be further improved, the safety performance of the battery can be improved, the acid and water content in the electrolyte can be controlled, and the conductivity and other properties of the electrolyte can be improved.
[0030] As some possible implementations of the secondary battery of the present application, the secondary battery includes a lithium-ion battery.
[0031] As some possible implementations of the secondary battery of the present application, the negative electrode includes at least one negative electrode active material selected from carbon-based negative electrode materials, silicon-based negative electrode materials, and lithium titanate. These negative electrode active materials store and release energy in the secondary battery, facilitating ion insertion and extraction.
[0032] As some possible implementations of the secondary battery of the present application, the secondary battery includes at least one of a battery cell, a battery module, and a battery pack.
[0033] A second aspect of the present application provides a method for preparing a secondary battery, comprising the following steps:
[0034] Obtaining a positive electrode, a negative electrode, and a separator, wherein the positive electrode contains a positive electrode active material, and the positive electrode active material includes an active material core and a carbon material coating layer;
[0035] preparing an electrolyte solution comprising an electrolyte salt, an organic solvent and an additive; wherein the additive comprises a silane-type additive; and determining the amount of the silane-type additive based on the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material;
[0036] Assemble the positive electrode, negative electrode, separator and electrolyte into a secondary battery.
[0037] The preparation method of the secondary battery provided by the present application, after preparing an electrolyte comprising an electrolyte salt, an organic solvent and an additive, assembling the electrolyte with a positive electrode, a negative electrode and a separator to obtain a secondary battery. Wherein, the electrolyte contains a silane-type additive whose amount is determined according to the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material. On the one hand, the silane-type additive can preferentially react with active sites such as oxygen-containing functional groups in the carbon material on the surface of the positive electrode active material, preferentially form a CEI film on the positive electrode surface, passivate the reactivity of the surface of the carbon material coating layer, reduce the irreversible consumption of active metal ions, inhibit the disorder of the carbon material coating layer, ensure the metal ion transmission channel, and thus improve the battery cycle performance. On the other hand, the reasonable amount of the required additive is determined by the physicochemical properties of the electrode material, avoiding the problems such as the inability to effectively reduce the side reactions between the electrolyte and the electrode material and reduce the internal resistance due to improper use of additives in the electrolyte, thereby better ensuring the electrochemical performance of the secondary battery.
[0038] As some possible implementations of the preparation method of the secondary battery of the present application, in the secondary battery, the mass percentage of the silane type additive in the electrolyte is marked as f, and the unit is %, and the specific surface area of the positive electrode active material is marked as a, and the unit is m 2 / g, and the mass percentage of the carbon material in the positive electrode active material is marked as e, in units of %, so that Z = f / (a*e) satisfies 0.001≤Z≤15. In this case, the electrode material and electrolyte in the battery have a better matching effect, which can effectively reduce the side reaction between the electrolyte and the electrode material, reduce impedance and improve the battery cycle performance, thereby improving the high-temperature performance of the battery.
[0039] As some possible implementations of the preparation method of the secondary battery of the present application, the silane-type additive includes at least one of tris(trimethylsilane) phosphate, tris(trimethylsilane) borate, tris(trimethylsilane) phosphite, tris(triethylsilane) phosphate, tris(triethylsilane) borate, tris(triethylsilane) phosphite, tris(trifluoromethylsilane) phosphate, tris(trifluoromethylsilane) borate, tris(trifluoromethylsilane) phosphite, tris(trifluoroethylsilane) phosphate, tris(trifluoroethylsilane) borate, and tris(trifluoroethylsilane) phosphite.
[0040] As some possible implementations of the method for preparing the secondary battery of the present application, the mass percentage of the silane-type additive in the electrolyte is 0.01% to 1.0%.
[0041] As some possible implementations of the method for preparing the secondary battery of the present application, the mass percentage of the carbon material in the positive electrode active material is 0.5% to 5%.
[0042] As some possible implementations of the method for preparing the secondary battery of the present application, the specific surface area of the positive electrode active material is 0.1 m 2 / g~20m 2 / g.
[0043] A third aspect of the present application provides an electrical device, which includes the secondary battery described above, or the secondary battery prepared by the method described above.
[0044] The electrical equipment provided in the present application includes the secondary battery with high safety performance and excellent electrochemical performance, thereby improving the safety and stability of the electrical equipment.
[0045] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] FIG1 is a schematic structural diagram of a secondary battery provided in an embodiment of the present application;
[0047] FIG2 is a schematic flow chart of a method for preparing a secondary battery provided in an embodiment of the present application;
[0048] FIG3 is a schematic diagram of a mobile terminal electric device provided in an embodiment of the present application;
[0049] FIG4 is a comparison chart of the cycle performance tests of the lithium-ion batteries provided in Example 1 and Comparative Example 1 of the present application.
[0050] The reference numerals are as follows: 10 - positive electrode, 101 - positive electrode current collector, 102 - positive electrode active material, 20 - negative electrode, 201 - negative electrode current collector, 202 - negative electrode active material, 30 - separator, 40 - electrolyte, 300 - mobile terminal. DETAILED DESCRIPTION
[0051] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.
[0052] In this application, the term "and / or" describes the relationship between associated objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0053] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0054] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0055] The terms used in the embodiments of the present application are for the purpose of describing specific embodiments only and are not intended to limit the present application. The singular forms "a," "an," and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise.
[0056] The term "primary cell" in English means a device that uses the different potentials of two electrodes to generate a potential difference, thereby causing electrons to flow and generate current, which can convert chemical energy into electrical energy.
[0057] The term "battery cell" refers to a single electrochemical cell containing a positive and negative electrode. It is the smallest unit of a power battery and the energy storage unit. A battery cell consists of four main components: a positive electrode, a negative electrode, an electrolyte, and a separator.
[0058] The term "battery module" refers to when multiple battery cells are encapsulated together in the same shell frame and connected to the outside through a unified boundary, this forms a module.
[0059] The term "battery pack" refers to a group of battery cells or battery modules that are jointly controlled or managed by the battery management system (BMS) and the thermal management system. This unified whole is called a battery pack.
[0060] The term "secondary battery" is called rechargeable battery in English, also known as rechargeable battery or storage battery. It refers to a battery that can be recharged to activate the active material after the battery is discharged and continue to be used.
[0061] The term "positive electrode" is called Cathode in English. It means that in the primary battery, the electrode where the current flows out has a higher potential and is the positive electrode, which obtains electrons to perform a reducing effect; in the electrolytic cell, the positive electrode is the electrode connected to the positive pole of the power supply, which loses electrons to perform an oxidizing effect.
[0062] The term "negative electrode" is called Anode in English. It means that in the primary battery, the electrode where the current flows has a lower potential and is the negative electrode. It loses electrons and performs oxidation. In the electrolytic cell, the negative electrode is the electrode connected to the negative pole of the power supply and obtains electrons to perform reduction.
[0063] The term "electrolyte" is called Electrolyte in English, which means the medium that provides ion exchange between the positive and negative electrodes of the battery.
[0064] The term "separator" in English refers to the thin membrane that separates the positive and negative electrodes during electrolysis to prevent contact and short circuits. Separators also allow electrolyte ions to pass through.
[0065] The term “SEI” is the abbreviation of “Solid Electrolyte Interphase”, which means an interface protective film or solid electrolyte interface (film), and refers to a passivation film layer with solid electrolyte properties.
[0066] The term "CEI" is an abbreviation for "Cathode Electrolyte Interphase", which means an interfacial protective film or cathode electrolyte interface (membrane), and refers to a passivation film layer with solid electrolyte properties.
[0067] At present, judging from the development of the market situation, materials such as lithium iron phosphate LiFePO4 are used as the first choice for positive electrode materials of electric vehicles or energy storage batteries due to their high safety and long cycle performance. However, materials such as LiFePO4 have the problem of low electrical conductivity, which leads to large impedance and polarization, affecting the cycle life, fast charging performance and energy efficiency of the battery. Therefore, materials such as LiFePO4 are usually carbon-coated to construct a conductive network of carbon materials on the surface of the positive electrode active material, thereby improving the electrical conductivity of the positive electrode material. However, the carbon materials coated on the surface of materials such as LiFePO4 often have defects or loose coating during the preparation process, causing the electrolyte to decompose at the interface between the positive electrode and the electrolyte and consume active lithium, resulting in an increase in electrolyte side reactions. Especially under high temperature conditions, the side reactions of the electrolyte will not only accelerate the consumption of active lithium, reducing the battery's electrochemical properties such as cycle stability, energy density, and rate performance, but may even cause the lithium-conducting channels of the carbon material coated on the surface of the positive electrode active material to become blocked or collapse, leading to the dissolution of metal ions in the positive electrode active material, ultimately causing the battery capacity to decay rapidly and further deteriorating the battery's electrochemical performance. In addition, during the battery's charge and discharge cycles, the serious side reactions caused by the contact between the positive and negative electrode materials and the electrolyte will also cause the SEI film on the negative electrode surface and the CEI film on the positive electrode surface to continuously rupture and repair during the cycle, resulting in a decrease in the battery's Coulombic efficiency and poor cycle performance.
[0068] In order to alleviate the side reaction problem of the electrolyte in the battery, the current method is mainly to introduce additives into the electrolyte to improve the performance of the electrolyte in high and low temperature environments. For example, in some known technologies, by adding additives such as vinylene carbonate, fluoroethylene carbonate, tris(trimethylsilyl) phosphate, vinyl ethylene carbonate, vinyl carboxylate, tris(trimethylsilyl) borate, cyclic sulfur-containing compounds, etc. to the electrolyte. Although it can improve the high and low temperature performance of the electrolyte in the battery and reduce side reactions to a certain extent; however, these electrolyte additives are mainly provided in combination, and the intrinsic relationship between the content of electrolyte additives and the characteristics of the electrode materials has not been specifically studied. If the amount of electrolyte additives is inappropriate, it is easy to cause the internal impedance of the battery to increase, resulting in increased polarization, thereby reducing the electrochemical performance of the battery.
[0069] Based on the above considerations, in order to solve the problem of side reactions between the electrolyte and the electrode materials, especially the decomposition of the electrolyte at the interface between the positive electrode and the electrolyte, which consumes active lithium and exacerbates the problem of side reactions such as metal ion dissolution that limit the performance of the battery. After in-depth research, the present application proposes a secondary battery, in which an additive is added to the electrolyte of the secondary battery, the additive includes a silane-type additive, the positive electrode active material includes an active material core and a carbon material coating layer, and the amount of the silane-type additive is determined according to the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material.
[0070] In such secondary batteries, the silane-type additive in the electrolyte has a more suitable oxidation potential than other additives. The oxygen-containing functional groups in the carbon material coating on the surface of the positive electrode active material preferentially react with the silane-type additive, resulting in the silane-type additive being preferentially oxidized at the positive electrode to produce silane and heteroatom-containing compounds, forming a CEI film. This effectively prevents the occurrence of catalytic side reactions between the active sites in the carbon material coating in the positive electrode active material and other components in the electrolyte, and inhibits the dissolution of metal ions in the positive electrode, thereby achieving the goals of reducing battery impedance, improving battery cycle performance, and improving high-temperature performance. In addition, the amount of the silane-type additive is determined based on the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material. The appropriate amount of the required additive is determined by the physical and chemical properties of the electrode material, thereby better ensuring the electrochemical performance of the secondary battery. Moreover, during the operation of the battery, the additives in the electrolyte may also form an SEI film on the surface of the negative electrode under the action of the negative electrode reduction potential, thereby better isolating the electrolyte from the electrode material, reducing the side reactions between the electrode material and the electrolyte, inhibiting the dissolution, deposition and reduction of metal ions in the electrode, and reducing the irreversible consumption of active metal ions.
[0071] For the convenience of description, the following embodiments of the present application are described by taking a secondary battery and its preparation method and application as an example.
[0072] In a first aspect, an embodiment of the present application provides a secondary battery, which includes a positive electrode 10, a negative electrode 20, a separator 30 and an electrolyte 40, wherein the positive electrode 10 contains a positive electrode active material 102, the positive electrode active material 102 includes an active material core and a carbon material coating layer, and the electrolyte 40 includes an electrolyte salt, an organic solvent and an additive, and the additive includes a silane-type additive; wherein the amount of the silane-type additive is determined according to the specific surface area of the positive electrode active material 102 and the content of the carbon material in the positive electrode active material 102.
[0073] The structure of the secondary battery provided in the embodiment of the present application includes at least the structure shown in FIG1 . The secondary battery includes a positive electrode 10, a negative electrode 20, a separator 30, and an electrolyte 40. The separator 30 is disposed between the positive electrode 10 and the negative electrode 20, and the electrolyte 40 is filled between the positive electrode 10 and the negative electrode 20 and infiltrates the separator 30. During charging, metal ions are released from the positive electrode active material 102 of the positive electrode, and after passing through the electrolyte 40 and the separator 30, are embedded in the negative electrode active material 202 of the negative electrode. During discharge, metal ions are released from the negative electrode active material 202 of the negative electrode, and after passing through the electrolyte 40 and the separator 30, are inserted into the positive electrode active material 102.
[0074] Thus, the secondary battery provided by the embodiments of the present application has at least the following advantages:
[0075] First, the electrolyte 40 additives include silane-type additives, which have a more suitable oxidation potential than other additives. Therefore, during the first charge and discharge process of the battery, the silane-type additive can preferentially react with active sites such as oxygen-containing functional groups in the carbon material (i.e., carbon material coating) on the surface of the positive electrode active material 102, and preferentially be oxidized to generate silane and heteroatom-containing compounds, forming a CEI film on the positive electrode surface. Passivate the reaction activity on the surface of the carbon material coating layer, inhibit the disorder of the carbon material coating layer, thereby effectively avoiding the active sites in the carbon material coating layer in the positive electrode active material 102 from contacting with other components in the electrolyte 40 to catalyze side reactions. And reduce the irreversible consumption of active metal ions, and reduce the risk of blockage or structural collapse of the metal ion conductive channel of the carbon material coating layer in the positive electrode active material 102, improve the degree of order of the carbon material coating layer, and ensure metal ion transmission. In addition, it can also inhibit the dissolution of metal ions in the positive electrode 10, thereby achieving the purpose of reducing battery impedance and improving battery cycle performance and improving high temperature performance.
[0076] Secondly, since the silane-type additive in the electrolyte 40 of the present application directly reacts with active sites such as oxygen-containing functional groups in the carbon material coating layer on the surface of the positive electrode active material 102 to form a CEI film, it can be seen that the amount of the silane-type additive is directly related to the physical and chemical properties such as the specific surface area of the positive electrode active material 102 and the content of the surface carbon material coating layer. Therefore, the amount of the silane-type additive in the embodiment of the present application is determined according to the specific surface area of the positive electrode active material 102 and the content of the carbon material (i.e., the carbon material coating layer) in the positive electrode active material 102. The reasonable amount of the required additive is determined by the physical and chemical properties of the electrode material, which can guide the design of the electrode material and the electrolyte 40. Avoid the problem that the improper amount of additive in the electrolyte 40 cannot effectively reduce the side reaction between the electrolyte 40 and the electrode material, reduce the internal resistance, etc., thereby better ensuring the electrochemical performance of the secondary battery.
[0077] Third, during battery operation, the additives in the electrolyte 40 may also form an SEI film on the negative electrode surface under the influence of the negative electrode reduction potential, thereby inhibiting the deposition and reduction of metal ions at the negative electrode to form dendrites that damage the negative electrode structure and the stability of the SEI film. This effectively isolates the electrolyte from the electrode material, reduces side reactions between the electrode material and the electrolyte, inhibits the dissolution, deposition and reduction of metal ions in the electrode, and reduces the irreversible consumption of active metal ions.
[0078] In some possible embodiments, in a secondary battery, the mass percentage of the silane additive in the electrolyte 40 is marked as f, in %, and the specific surface area of the positive electrode active material 102 is marked as a, in m. 2 / g, the mass percentage of the carbon material in the positive electrode active material 102 is marked as e, with the unit of %, so that Z = f / (a*e) satisfies 0.001≤Z≤15. In the relationship formula Z = f / (a*e) in the embodiment of the present application, Z is only used to express the stoichiometric relationship between the mass percentage of the silane-type additive, the specific surface area of the positive electrode active material 102, and the mass percentage of the carbon material. It does not have a special meaning in itself. When the units of the parameters f, a, and e are determined, the value of Z is only related to the numerical value and is no longer affected by the parameter units. In this case, since the silane-type additive has a more suitable oxidation potential than other additives, during the first charge and discharge process of the battery, the silane-type additive preferentially reacts with active sites such as oxygen-containing functional groups in the carbon material on the surface of the positive electrode active material 102, and is preferentially oxidized to generate silane and heteroatom-containing compounds to form a CEI film. Therefore, the larger the specific surface area of the positive electrode active material 102, the more active sites and defects on its surface. In addition, the more carbon material layers coated on the surface of the positive electrode active material 102, the more active sites and defects such as oxygen-containing functional groups in the carbon material. At this time, the more silane-type additives are needed to passivate the surface reaction activity of the carbon material coating layer. Therefore, according to the physical and chemical properties such as the specific surface area of the positive electrode active material 102 and the content of the carbon material coating layer on its surface, the reasonable amount of the silane-type additive can be calculated. Through specific research, it was found that after the amount of the silane-type additive is determined according to the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material, in the secondary battery (including various stages such as before formation, after formation, capacity separation, and after circulation), the mass percentage f (in %) of the silane-type additive in the electrolyte 40 is proportional to the specific surface area a (in m2) of the positive electrode active material 102. 2 / g) and the mass percentage e (in %) of the carbon material on its surface is calculated as Z = f / (a*e). When 0.001≤Z≤15 is satisfied, under this condition, the electrode material and the electrolyte 40 in the battery have a better matching effect, which can effectively reduce the side reaction between the electrolyte 40 and the electrode material, reduce the impedance and improve the battery cycle performance, and improve the high temperature performance of the battery.
[0079] In a specific embodiment, in the secondary battery at various stages such as before formation, after formation, capacity separation, and after cycling, the mass percentage f (in %) of the silane additive in the electrolyte 40 and the specific surface area a (in m2) of the positive electrode active material 102 are 2 / g) and the mass percentage e (in %) of the carbon material on its surface are calculated as Z=f / (a*e), and both satisfy 0.001≤Z≤15.
[0080] For example, the mass percentage f (in %) of the silane additive in the electrolyte 40 and the specific surface area a (in m2) of the positive electrode active material 102 are 2 / g) and the mass percentage content e (in %) of the carbon material on its surface are calculated as Z = f / (a*e), and Z satisfies 0.001~0.1, 0.1~0.2, 0.001~0.2, 0.02~15, 0.02~0.1, 0.1~0.5, 0.5~1, 1~2, 2~3, 3~4, 4~5, 5~6, 6~7, 7~8, 8~9, 9~10, 10~11, 11~12, 12~13, 13~14, 14~15, etc.
[0081] In addition, it can be understood that in the embodiment of the present application, the mass percentage of the silane type additive in the electrolyte 40 (in %) is proportional to the specific surface area a (in m2) of the positive electrode active material 102. 2 / g) and the mass percentage e (in %) of carbon material on its surface Z = f / (a*e) is applicable not only to the battery assembly process, but also to the battery before and after formation, capacity division or cycle operation. That is, after formation, capacity division or cycle operation, the specific surface area a (in m2) of the positive electrode active material is 2 The relationship Z = f / (a*e) between the carbon material coating content (in %) and the carbon material coating content (in %) thereof and the silane additive content (in %) still satisfies 0.001≤Z≤15 and is still within the range defined in the embodiments of the present application. It should be noted that the values of a, e, and f in the relationship may have a certain impact on material testing during actual battery formation, capacity separation, or cycling due to the formation of an interface film. Therefore, a certain measurement error may be allowed. Values within the error range may be understood as being within the range defined in the embodiments of the present application.
[0082] In some possible embodiments, the silane additive includes at least one of tris(trimethylsilane) phosphate (TMSP), tris(trimethylsilane) borate (TMSB), tris(trimethylsilane) phosphite, tris(triethylsilane) phosphate, tris(triethylsilane) borate, tris(triethylsilane) phosphite, tris(trifluoromethylsilane) phosphate, tris(trifluoromethylsilane) borate, tris(trifluoromethylsilane) phosphite, tris(trifluoroethylsilane) phosphate, tris(trifluoroethylsilane) borate, and tris(trifluoroethylsilane) phosphite. In this case, these silane additives have a more suitable oxidation potential than other additives. During the initial charge and discharge process of the battery, the silane additive preferentially reacts with active sites such as oxygen-containing functional groups in the carbon material on the surface of the positive electrode active material 102, passivating the reactivity of the carbon material coating layer, inhibiting the disordering of the carbon material coating layer, and preferentially being oxidized to form silanes and compounds containing heteroatoms such as phosphorus and boron, thereby forming a CEI film on the positive electrode surface. On the one hand, the CEI membrane can effectively prevent the active sites in the carbon material coating layer of the positive electrode active material 102 from contacting with other components in the electrolyte 40 to catalyze side reactions, reduce the irreversible consumption of active metal ions, maintain the structure of the carbon material coating layer as a metal ion conductive channel, and simultaneously inhibit the dissolution of metal ions from the positive electrode 10, thereby reducing battery impedance, improving battery cycle performance, and improving high-temperature performance. On the other hand, compounds containing heteroatoms such as phosphorus and boron in the CEI membrane have high electrical conductivity, which can improve the electrical conductivity of the CEI membrane, facilitate lithium ion transmission, and better enhance battery cycle performance, safety, and other characteristics.
[0083] In some possible embodiments, the weight percentage of the silane additive in the electrolyte 40 is 0.01% to 1.0%. At this added content, the silane additive can fully passivate the reactive sites and defects on the surface of the carbon material coating, forming a CEI film on the positive electrode surface. This effectively reduces disordering of the carbon material coating, improves ion transfer efficiency, reduces side reactions between the electrolyte 40 and the positive electrode material, reduces irreversible consumption of active metal ions, maintains the structure of the carbon material coating as a conductive metal ion channel, and inhibits metal ion dissolution from the positive electrode 10, thereby reducing battery impedance, improving battery cycle performance and safety, and improving high-temperature performance. Furthermore, this content of the silane additive ensures that the CEI film formed on the positive electrode surface has an appropriate thickness, effectively reducing side reactions between the positive electrode material and the electrolyte 40, improving battery cycle safety, and preventing an excessively thick CEI film from affecting battery impedance. For example, the mass percentage of the silane additive in the electrolyte 40 may be 0.01% to 0.05%, 0.05% to 0.1%, 0.1% to 0.2%, 0.2% to 0.3%, 0.3% to 0.4%, 0.4% to 0.5%, 0.5% to 0.6%, 0.6% to 0.7%, 0.7% to 0.8%, 0.8% to 0.9%, 0.9% to 1.0%, etc. In a specific embodiment, the mass percentage of the silane additive in the electrolyte 40 may be typically, but not limited to, 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 0.9%, 1.0%, or any value between 0.01% and 1.0%.
[0084] In some possible embodiments, the mass percentage of the carbon material in the positive electrode active material 102 is 0.5% to 5%. In this case, the content of the carbon material coating layer in the positive electrode active material 102 can ensure sufficient and complete coating of the active material core, improve the conductivity of the active material core, and help reduce internal resistance and polarization, thereby improving the battery's cycle life, fast charging performance, energy efficiency, and other characteristics. At the same time, this content of the carbon material coating layer also avoids the risk of excessive introduction of carbon material, which may lead to reduced capacity of the positive electrode active material 102, reduced coulombic efficiency, increased carrier migration and transmission paths, increased impedance, and increased side reactions. Exemplary, the mass percentage of the carbon material in the positive electrode active material 102 can be 0.5% to 1.0%, 1.0% to 1.5%, 1.5% to 2%, 2% to 2.5%, 2.5% to 3%, 3% to 3.5%, 3.5% to 4%, 4% to 4.5%, 4.5% to 5%, etc.
[0085] In some possible embodiments, the specific surface area of the positive electrode active material 102 is 0.1 m 2 / g~20m 2 / g. In this case, the larger the specific surface area of the positive electrode active material 102, the more conducive it is to the embedding and de-embedding of ions, which is beneficial to improving the rate performance of the battery. However, the larger the specific surface area of the positive electrode active material 102, the more side reactions there will be with the electrolyte 40, which is not conducive to improving the coulombic efficiency of the battery. Therefore, the specific surface area of the positive electrode active material 102 in the embodiment of the present application not only ensures that the ions have a larger active surface area for de-embedding during the charge and discharge process of the battery, but also helps to control the side reactions between the positive electrode active material 102 and the electrolyte 40. For example, the specific surface area of the positive electrode active material 102 can be 0.1m 2 / g~1m 2 / g, 0.2m 2 / g~0.8m 2 / g, 0.1m 2 / g~0.2m 2 / g, 0.2m 2 / g~0.3m 2 / g, 0.3m 2 / g~0.4m 2 / g, 0.4m 2 / g~0.5m 2 / g, 0.5m 2 / g~0.6m 2 / g, 0.6m 2 / g~0.7m 2 / g, 0.7m 2 / g~0.8m 2 / g, 0.8m 2 / g~0.9m 2 / g, 0.9m 2 / g~1.0m 2 / g, 1.0m 2 / g~2m 2 / g, 2m 2 / g~3m 2 / g、m 2 / g~4m 2 / g、4m 2 / g~5m 2 / g、5m 2 / g~6m 2 / g、6m 2 / g~7m 2 / g、7m 2 / g~8m 2 / g、8m 2 / g~9m 2 / g、9m 2 / g~10m 2 / g、10m 2 / g~11m 2 / g、11m 2 / g~12m 2 / g、12m 2 / g~13m 2 / g、13m 2 / g~14m 2 / g、14m 2 / g~15m 2 / g、15m 2 / g~16m 2 / g、16m 2 / g~17m 2 / g、17m 2 / g~18m 2 / g、18m 2 / g~19m 2 / g、19m 2 / g~20m 2 / g, etc.
[0086] In some possible implementations, the active material core includes at least one of metal oxides and polyanion salts. In this case, the active materials included in the core of the positive electrode active material 102 have characteristics such as high capacity and safety.
[0087] In some possible embodiments, the metal oxides include at least one of lithium cobaltate, lithium nickelate, lithium nickel cobalt manganeseate, lithium nickel cobalt aluminumate, lithium manganate, lithium nickel manganeseate, and lithium vanadate. Among them, lithium cobaltate (LiCoO2), lithium manganate (LiMnO2), and lithium nickelate (LiNiO2) all have an α-NaFeO2 crystal structure and belong to the hexagonal system. From the perspective of crystal structure, Li-O octahedrons and MO octahedrons (M is a transition metal element) alternate and stack on each other, so these materials are also called layered positive electrode materials. Lithium cobaltate (LCO) has the advantages of high discharge platform, high specific capacity, good cycle performance, and simple synthesis process. Lithium cobaltate is particularly suitable for small batteries, such as those used in digital products such as mobile phones, model airplanes, model cars, electronic cigarettes, smart wearables, etc., to meet the market development needs of intelligence, lightness, and miniaturization. Compared with traditional positive electrode materials such as lithium cobalt oxide, lithium manganese oxide (LiMnO2) has the advantages of abundant resources, low cost, no pollution, good safety, and good rate performance, making it an ideal positive electrode material for power batteries. However, lithium manganese oxide with a layered structure is a non-thermodynamically stable phase, while lithium manganese oxide with a spinel structure has advantages such as good structural stability and high power density. Compared with lithium cobalt oxide and lithium manganese oxide, lithium nickel oxide (LiNiO2) can achieve a higher actual capacity. At the same time, nickel has great application potential due to its abundant resources and low price. Lithium vanadate has the unique advantages of high specific capacity (up to about 300mAh / g) and low price. As a traditional lithium-ion battery positive electrode material, it has been widely studied. Lithium nickel cobalt manganese oxide replaces more than two-thirds of the cobalt in lithium cobalt oxide with relatively cheap nickel and manganese, and has a higher specific capacity and lower cost than single-unit positive electrode materials. Compared to other lithium-ion battery cathode materials such as lithium manganese oxide and lithium iron phosphate, nickel-cobalt manganese oxide and lithium cobalt oxide are very similar in electrochemical and processing properties, making nickel-cobalt manganese oxide a new battery material that is gradually replacing lithium cobalt oxide and becoming the next-generation lithium-ion battery material. As a high-nickel ternary material, lithium nickel cobalt aluminum oxide (NCA) boasts high specific capacity (up to 200 mAh / g or more), low price, and excellent cycling stability. The active material of lithium nickel manganese oxide often has a spinel structure, developed based on spinel lithium manganese oxide. Like lithium manganese oxide, it is a positive electrode material with three-dimensional lithium ion channels. Its reversible capacity is 146.7 mAh / g, similar to that of lithium manganese oxide, but its voltage platform is around 4.7 V, more than 15% higher than the 4 V voltage platform of lithium manganese oxide. Its cycling stability at high temperatures is also significantly improved compared to the original lithium manganese oxide.
[0088] In some possible embodiments, the polyanion salt includes at least one of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium nickel phosphate, lithium iron silicate, lithium iron fluorosulfate, lithium iron borate, and lithium iron titanate. In this case, the core of the polyanion salt positive electrode active material has a stable polyhedral framework structure, has better structural and thermodynamic stability, and can obtain higher cyclability and safety. Among them, the lithium iron phosphate positive electrode material is an olivine structure, belongs to the orthorhombic crystal system, and has the advantages of high reversible specific capacity (about 170.0mAh / g), stable charge and discharge platform, high safety, long cycle life, abundant resources and low price. Lithium manganese phosphate has high safety and stability similar to lithium iron phosphate, and its theoretical energy density is 21% higher than the latter. It is considered to be the most promising next-generation lithium-ion power battery positive electrode material. Manganese element is added to lithium iron phosphate to increase the voltage platform to obtain lithium manganese iron phosphate. The ionic radius of manganese ions (0.083nm) and iron ions (0.078nm) is close, making them miscible in any proportion. Therefore, by adding manganese to lithium iron phosphate and adjusting the ratio of its atomic number to iron (manganese to iron ratio), a high voltage platform can be achieved while also circumventing the inherent defects of lithium manganese phosphate. Lithium vanadium phosphate has two phases: a rhombohedral phase and a more thermodynamically stable monoclinic phase. In this phase, the tetrahedral PO4 and the octahedral VO6 are connected by sharing a vertex (oxygen atom), and a three-dimensional network structure is formed with V2(PO4)3 as the structural unit. Lithium ions fill the voids in the three-dimensional structure. As a result, lithium vanadium phosphate has good structural stability, three-dimensional lithium ion diffusion channels, high specific capacity, high redox potential, good high current charge and discharge performance, and abundant raw materials, meeting the power density requirements of the lithium-ion battery industry. The presence of the PO covalent bond in lithium vanadium phosphate not only improves its kinetic and thermodynamic stability but also weakens the VO covalent bond (i.e., the inductive effect), reducing the antibonding orbital energy of the vanadium ion, thereby raising its redox energy level. This gives lithium vanadium phosphate a higher discharge platform than vanadium oxide. Lithium cobalt phosphate inherits the advantages of lithium iron phosphate, such as safety, cycling stability, and low-current float charge resistance, but also significantly increases its voltage, reaching an operating voltage of 4.8V and an energy density of 800Wh / kg. Lithium nickel phosphate offers the advantage of high energy density. Lithium iron silicate can intercalate and deintercalate two lithium ions, with a theoretical specific capacity of up to 330mAh / g. Its high energy density has attracted considerable attention. Lithium ferrous fluorosulfate, a new sulfate polyanion material, not only offers outstanding advantages such as low cost and environmental friendliness, but also exhibits superior high-rate safety compared to cathode materials such as layered lithium cobalt oxide and spinel lithium manganese oxide. Furthermore, due to the presence of two lithium ions in its structure, its theoretical capacity is twice that of lithium iron phosphate.Lithium iron borate is a new type of polyanion positive electrode material with high specific capacity. In terms of structure, it has a smaller molar mass (BO3). 3- Replace (PO4) 3- , which can achieve a higher theoretical specific capacity (220mAh / g). At the same time, the structure of lithium iron borate makes it have better conductivity (conductivity is 3.9×10 -7 S / cm), with minimal volume change (approximately 2%) before and after charge and discharge, good reversibility, and excellent chemical and electrochemical stability. Lithium iron titanate has a theoretical capacity of 295 mAh / g, a moderate operating voltage, and is widely available, inexpensive, and environmentally friendly, making it a cathode material that has recently been researched.
[0089] In some possible embodiments, when the active material core comprises metal oxides, the specific surface area of the positive electrode active material 102 is 0.1 m 2 / g~1.0m 2 / g, satisfying 0.01≤Z≤15. Since metal oxide active materials have relatively small specific surface areas, when the active material core of the positive electrode active material 102 is a metal oxide, the specific surface area of the corresponding positive electrode active material 102 is also small, exemplarily 0.1m 2 / g~1.0m 2 / g. At this time, the mass percentage f (unit: %) of the silane additive in the electrolyte 40 and the specific surface area a (unit: m) of the positive electrode active material 102 are 2 The relationship between the mass percentage of the surface carbon material (a / g) and the mass percentage of the surface carbon material (e) is Z = f / (a*e), where Z satisfies 0.01≤Z≤15. Under this condition, side reactions between the electrolyte 40 and the electrode material can be effectively reduced, reducing impedance, improving battery cycle performance, and improving high-temperature performance.
[0090] In some possible embodiments, when the active material core comprises metal oxides, the specific surface area of the positive electrode active material 102 is 0.2 m 2 / g~0.8m 2 / g, and 0.02≤Z≤10. In this case, the side reaction between the electrolyte 40 and the electrode material can be more effectively reduced, the impedance can be reduced, the battery cycle performance can be improved, and the high temperature performance of the battery can be improved.
[0091] In some embodiments, the specific surface area of the positive electrode active material 102 including the metal oxide type active material core may be 0.1 m 2 / g~1m 2 / g, 0.2m 2 / g~1m 2 / g, 0.3m 2 / g~1m2 / g, 0.4m 2 / g~1m 2 / g, 0.5m 2 / g~1m 2 / g, 0.6m 2 / g~1m 2 / g, 0.7m 2 / g~1m 2 / g, 0.8m 2 / g~1m 2 / g, 0.9m 2 / g~1m 2 / g, 0.2m 2 / g~0.9m 2 / g, 0.2m 2 / g~0.8m 2 / g, 0.2m 2 / g~0.7m 2 / g, 0.2m 2 / g~0.6m 2 / g, 0.2m 2 / g~0.5m 2 / g, 0.2m 2 / g~0.4m 2 / g, 0.2m 2 / g~0.3m 2 / g, etc.
[0092] In some specific embodiments, the active material core includes a positive electrode active material 102 of a metal oxide type such as lithium cobalt oxide, lithium nickel cobalt manganese oxide, etc., and the specific surface area can be 0.1 m 2 / g, 0.15m 2 / g, 0.2m 2 / g, 0.35m 2 / g, 0.5m 2 / g, 0.65m 2 / g, 0.8m 2 / g, 1.0m 2 Typical but not limiting specific surface areas include 0.0541 square feet (0.001 square feet) and 0.001 square feet (0.001 square feet).
[0093] In some possible embodiments, when the active material core includes a polyanion salt, the specific surface area of the positive electrode active material 102 is 7 m 2 / g~20m 2 / g, satisfying 0.001≤Z≤0.2. Since polyanion salt active materials often have a polyhedral framework structure, they have a relatively large specific surface area. When the active material core of the positive electrode active material 102 is a polyanion salt, the corresponding specific surface area of the positive electrode active material 102 is also large, exemplarily 7m2 / g~20m 2 / g. At this time, the mass percentage f (unit: %) of the silane additive in the electrolyte 40 and the specific surface area a (unit: m) of the positive electrode active material 102 are 2 The relationship between the mass percentage of the surface carbon material (a / g) and the mass percentage of the surface carbon material (e) is Z = f / (a*e), where Z satisfies 0.001≤Z≤0.2. Under this condition, side reactions between the electrolyte 40 and the electrode material can be effectively reduced, reducing impedance, improving battery cycle performance, and improving high-temperature performance.
[0094] In some possible embodiments, when the active material core includes a polyanion salt, the specific surface area of the positive electrode active material 102 is 9 m 2 / g~15m 2 / g; and 0.002≤Z≤0.1. In this case, the side reaction between the electrolyte 40 and the electrode material can be more effectively reduced, the impedance can be reduced, the battery cycle performance can be improved, and the high temperature performance of the battery can be improved.
[0095] In some embodiments, the specific surface area of the positive electrode active material 102 including the polyanion salt may be 7 m 2 / g~20m 2 / g、8m 2 / g~19m 2 / g、9m 2 / g~18m 2 / g、10m 2 / g~17m 2 / g、11m 2 / g~16m 2 / g、12m 2 / g~15m 2 / g、13m 2 / g~14m 2 / g、7m 2 / g~10m 2 / g、10m 2 / g~13m 2 / g、13m 2 / g~15m 2 / g、15m 2 / g~18m 2 / g、18m 2 / g~20m 2 / g、9m 2 / g~15m 2 / g、10m 2 / g~14m 2 / g、11m 2 / g~13m2 / g, etc.
[0096] In some specific embodiments, the active material core includes a positive electrode active material 102 of a phosphate-based polyanion salt such as lithium iron phosphate, lithium manganese phosphate, or lithium manganese iron phosphate, and the specific surface area can be 7m 2 / g、9m 2 / g、10m 2 / g, 12.5m 2 / g、15m 2 / g、18m 2 / g, 20m 2 Typical but not limiting specific surface areas include 0.0541 square feet (0.001 square feet) and 0.001 square feet (0.001 square feet).
[0097] In some specific embodiments, when the active material core includes lithium iron phosphate positive electrode active material 102, the specific surface area of the positive electrode active material 102 is 7m 2 / g~20m 2 / g, Z=f / (a*e)wherein, Z satisfies 0.001≤Z≤0.2. For example, Z can be a value between 0.001 and 0.01, a value between 0.005 and 0.02, a value between 0.01 and 0.05, a value between 0.02 and 0.2, or a value between any two values. For example, the value of Z can be typically but not limited to 0.001, 0.005, 0.01, 0.02, 0.05, 0.1, 0.2, or any value between 0.001 and 0.2.
[0098] In some specific embodiments, when the active material core includes lithium manganese iron phosphate positive electrode active material 102, the specific surface area of the positive electrode active material 102 is 7m 2 / g~20m 2 / g, Z=f / (a*e)wherein, Z satisfies 0.001≤Z≤0.2. For example, Z can be a value between 0.001 and 0.01, a value between 0.005 and 0.02, a value between 0.01 and 0.05, a value between 0.02 and 0.2, or a value between any two values. For example, the value of Z can typically but not limitatively be 0.001, 0.005, 0.01, 0.02, 0.05, 0.1, 0.2, or any value between 0.001 and 0.2.
[0099] In some specific embodiments, when the active material core includes lithium cobalt oxide positive electrode active material 102, the specific surface area of the positive electrode active material 102 is 0.1 m 2 / g~1.0m 2 / g, Z=f / (a*e)wherein, Z satisfies 0.01≤Z≤15. For example, Z can be a value between 0.01 and 0.1, a value between 0.05 and 0.5, a value between 0.2 and 5, a value between 1 and 15, or a number between any two values. For example, the value of Z can be typically but not limited to 0.02, 0.05, 0.1, 0.2, 0.5, 0.1, 0.2, 0.5, 1.0, 2.0, 5.0, 7.0, 10.0, 12.5, 15.0, or any value between 0.02 and 15.
[0100] In some specific embodiments, when the active material core includes lithium nickel cobalt manganese positive electrode active material 102, the specific surface area of the positive electrode active material 102 is 0.1 m 2 / g~1.0m 2 / g, Z=f / (a*e)wherein, Z satisfies 0.01≤Z≤15. For example, Z can be a value between 0.01 and 0.1, a value between 0.05 and 0.5, a value between 0.2 and 5, a value between 1 and 15, or a number between any two values. For example, the value of Z can be typically but not limited to 0.02, 0.05, 0.1, 0.2, 0.5, 0.1, 0.2, 0.5, 1.0, 2.0, 5.0, 7.0, 10.0, 12.5, 15.0, or any value between 0.02 and 15.
[0101] In some possible embodiments, the peak intensity ratio of the D peak to the G peak of the positive electrode active material 102 in the Raman test is R=I D / I G , R value range is 0.6~1.3. In Raman test, D peak is caused by the defects of carbon material coating layer on the surface of positive electrode active material 102. If there are more material defects, D peak will be more obvious and stronger. R=I D / I G The larger the value, the more defects there are, the lower the degree of graphitization, the higher the degree of disorder of the carbon material coating layer, and the more unfavorable the ion migration and transmission. The D peak of the Raman test in the embodiment of the present application is the displacement range of 1300cm in the Raman spectrum of the positive electrode active material 102. -1 to 1400cm -1 The peak of D appears at 1350cm -1 The G peak is located near the radial breathing mode of the symmetrical stretching vibration of the sp2 carbon atoms in the aromatic ring (structural defect). The shift range of the G peak in the Raman spectrum of the positive active material 102 is 1530 cm -1 to 1630cm -1 The peak of G peak appears at 1580cm -1The D peak and the G peak correspond to disordered carbon and ordered graphitic carbon, respectively. Therefore, the intensity ratio of the D peak to the G peak (I D / I G ) can reflect the degree of defects and graphitization of the carbon material. A positive electrode active material 102 with an R value ranging from 0.6 to 1.3 ensures that there are suitable ion migration and transmission channels in the surface carbon material coating layer. For example, the peak intensity ratio R of the D peak to the G peak in the Raman test of the positive electrode active material 102 can be 0.6-1.2, 0.6-1.1, 0.6-1.0, 0.6-0.9, 0.6-0.8, 0.6-0.7, 0.7-1.2, 0.8-1.2, 0.9-1.1, 0.7-1.0, 0.8-1, etc.
[0102] In some possible embodiments, the peak intensity ratio R of the D peak to the G peak in the Raman spectrum of the positive electrode active material 102 is in the range of 0.8 to 1.2. In this case, the surface carbon material coating layer of the positive electrode active material 102 of the secondary battery can better balance improving the conductivity of the positive electrode active material core and achieving more suitable ion migration and transmission efficiency.
[0103] In addition, it is understood that after the battery is formed, capacity divided, or cycled, the peak intensity ratio R of the D peak to the G peak in the Raman test of the positive electrode active material 102 still ranges from 0.8 to 1.2, which is still within the range defined in the embodiments of the present application. It should be noted that the value of the peak intensity ratio R of the D peak to the G peak in the Raman test of the positive electrode active material 102, after actual battery formation, capacity divided, or cycled, is acceptable due to the formation of the interfacial film, which will have a certain impact on the carbon material coating on the surface of the positive electrode active material. The values within the error range can be understood as the range defined in the embodiments of the present application.
[0104] In some possible implementations, the carbon material of the coating layer on the surface of the positive electrode active material 102 may be any carbon material such as amorphous carbon, carbon nanotubes, graphene, graphite, carbon fiber, etc.
[0105] In some possible embodiments, the additive also includes vinylene carbonate. In this case, vinylene carbonate can undergo an electrochemical reaction on the surface of the negative electrode during the initial charge and discharge process of the secondary battery to form a solid electrolyte interface film, namely a SEI film, which effectively inhibits the embedding of solvent molecules and the bloating of the battery, thereby improving the battery capacity and life. Compared with other negative electrode additives, vinylene carbonate has a better SEI film formation effect on the negative electrode surface. At this time, the electrolyte 40 contains both positive electrode film-forming additives and negative electrode film-forming additives. During the operation of the battery, the negative electrode film-forming additives such as vinylene carbonate in the electrolyte 40 will form an SEI film on the surface of the negative electrode under the action of the negative electrode reduction potential, isolating the electrolyte 40 from contact with the negative electrode material, so as to inhibit the deposition and reduction of metal ions at the negative electrode to form dendrites that destroy the negative electrode structure and the stability of the SEI film. At the same time, positive electrode film-forming additives such as silane-type additives will form a CEI film on the positive electrode surface under the action of the positive electrode oxidation potential, passivate the active sites on the positive electrode surface, and inhibit the dissolution of metal ions in the positive electrode material, thereby effectively reducing the side reactions catalyzed by the contact between the electrolyte 40 and the positive electrode material.
[0106] In some possible embodiments, the mass percentage of vinylene carbonate in the electrolyte 40 is 0.1% to 5%. In this case, the mass percentage of vinylene carbonate in the electrolyte 40 is 0.1% to 5%, which fully ensures its film-forming effect on the surface of the negative electrode, forms a SEI film, isolates the contact between the electrolyte 40 and the negative electrode material, and inhibits the deposition and reduction of metal ions at the negative electrode to form dendrites that destroy the negative electrode structure and the stability of the SEI film. At the same time, it avoids the formation of an SEI with too high a thickness to increase the internal resistance of the battery. Exemplarily, the mass percentage of vinylene carbonate in the electrolyte 40 can be 0.1% to 0.5%, 0.5% to 1%, 1% to 2%, 2% to 3%, 3% to 4%, 4% to 5%, 2% to 3%, 3% to 5%, etc. In a specific embodiment, the mass percentage of vinylene carbonate in the electrolyte 40 can be 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, etc., which are typical but non-limiting contents.
[0107] In some possible embodiments, the electrolyte salt includes LiClO4, LiBF4, LiPF6, LiAsF6, LiCF3SO3, LiTDI, Li[(CF3SO2)2N], Li[(FSO2)2N], Li[(C m F 2m+1 SO2)(C n F 2n+1SO2)N], wherein m and n are natural numbers. In this case, these electrolytic salts can ensure high ionic conductivity of the electrolyte 40, and do not cause harmful side reactions with electrode materials, electrolyte 40, diaphragm 30, etc., and have good chemical stability. Among them, lithium hexafluorophosphate LiPF6 has suitable solubility and high ionic conductivity in non-aqueous solvents; it can form a stable passivation film on the surface of current collectors such as aluminum foil. In addition, it can cooperate with carbonate solvents to generate a stable SEI film on the surface of the negative electrode. Compared with LiPF6, lithium tetrafluoroborate LiBF4 has a wider operating temperature range, better stability at high temperatures and better low-temperature performance. Lithium perchlorate LiClO4 has a relatively high solubility and therefore exhibits relatively high ionic conductivity. Its room temperature ionic conductivity in carbonate organic solvents can reach 9mS / cm, and the electrochemical stability window can reach 5.1V vs.Li + / Li, has relatively good oxidation stability, this property also makes the electrolyte salt compatible with some high voltage positive electrode materials, thus exerting the high energy density of lithium-ion batteries. Lithium hexafluoroarsenate LiAsF6 has the same ionic conductivity as LiBF4, and at the same time, the electrochemical window can reach 6.3Vvs.Li + / Li, high electrochemical stability, and the electrolyte lithium salt is non-corrosive to the current collector. Lithium 4,5-dicyano-2-(trifluoromethyl)isopyrazole LiTDI: The isopyrazole ring promotes negative charge dissociation through resonance, while the two nitrile groups have an optimized electronegativity-to-weight ratio, further promoting positive charge dissociation. Furthermore, the CF3 group attached to the isopyrazole ring provides electrochemical stability and exceptional thermal stability. This makes the molecule an excellent choice for long-lasting lithium-ion batteries operating at high voltages and temperatures. This not only extends battery life and fast charging performance, but also addresses the purity and stability issues of high-capacity battery materials. Lithium bis(fluorosulfonyl)imide salt Li[(FSO2)2N] effectively reduces the low-temperature resistance of the SEI layer formed on the electrode surface at low temperatures, reducing capacity loss during storage, thereby providing high battery capacity and electrochemical performance. It can also be used as an electrolyte for primary batteries. Lithium trifluoromethanesulfonate LiCF3SO3 has excellent thermal stability, water absorption and decomposition, and cycle performance. Its stable anions can improve the structure and composition of the passivation layer between the electrolyte and the negative electrode material interface, which is beneficial to the stability of the electrolyte, passivation film, and electrode. Lithium bis(trifluoromethanesulfonyl)imide Li[(CF3SO2)2N] has high electrochemical stability and conductivity, and has a high voltage (above 4.2V). Asymmetric bis(fluorosulfonyl)imide lithium salt Li[(C m F 2m+1 SO2)(C n F 2n+1SO2)N] has suitable conductivity, high thermal stability and electrochemical stability, low probability of side reactions, and will not produce corrosive gases such as HF.
[0108] In some possible embodiments, the molar concentration of the electrolyte salt in the electrolyte 40 is 0.01 mol / L to 5.0 mol / L. In this case, the molar concentration of the electrolyte salt in the electrolyte 40 of 0.01 mol / L to 5.0 mol / L can ensure high ionic conductivity of the electrolyte 40. Exemplarily, the molar concentration of the electrolyte salt in the electrolyte 40 can be 0.01 mol / L to 0.05 mol / L, 0.05 mol / L to 0.1 mol / L, 0.1 mol / L to 0.3 mol / L, 0.3 mol / L to 0.5 mol / L, 0.5 mol / L to 0.8 mol / L, 0.8 mol / L to 1 mol / L, 1 mol / L to 2 mol / L, 2 mol / L to 3 mol / L, 3 mol / L to 4 mol / L, 4 mol / L to 5 mol / L, 2 mol / L to 4 mol / L, 3 mol / L to 5 mol / L, etc. In specific embodiments, the molar concentration of the electrolyte salt can be typical but non-limiting concentrations such as 0.01 mol / L, 0.1 mol / L, 0.5 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, 3.0 mol / L, 4.0 mol / L or 5.0 mol / L.
[0109] In some possible embodiments, the organic solvent includes at least one of a carbonate solvent, an ether solvent, and a carboxylate solvent. The organic solvent is an important component of the battery electrolyte 40 and plays an important role in dissolving electrolyte salts, additives, etc. It has an important impact on the solubility of the electrolyte salt, the conductivity of the electrolyte, the cycle efficiency, the reversible capacity and the safety of the battery. In this case, at least one organic solvent among the carbonate solvent, the ether solvent and the carboxylate solvent has good solubility for the electrolyte salt, and has low melting point, high boiling point, low vapor pressure, a wide operating temperature range, high dielectric constant and low viscosity, high conductivity and other characteristics. Among them, the lower dielectric constant of the ether solvent molecules allows the ions in the ether electrolyte 40 to attract more solvent molecules and release them during desolvation, causing a larger system entropy change and temperature coefficient. Exemplary, ether solvents include chain ethers such as 1,2-dimethoxypropane (DMP), dimethoxymethane (DMM), and ethylene glycol dimethyl ether (DME), and cyclic ethers such as tetrahydrofuran (THF) and 2-methyltetrahydrofuran (2-Me-THF). Carbonate solvents include cyclic carbonates such as propylene carbonate (PC) and ethylene carbonate (EC), as well as chain carbonates such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). Among them, cyclic carbonates EC, PC, etc. have a very high dielectric constant, which makes lithium salts easier to dissolve, but at the same time the viscosity is also very large, which makes the lithium ion migration rate lower. Chain carbonates DMC, DEC, EMC, etc. have a small dielectric constant and weak ability to dissolve lithium salts, but their low viscosity has good fluidity, which facilitates lithium ion migration. Among carboxylate solvents, cyclic carboxylate solvents, such as γ-butyrolactone (BL), have a relatively wide liquid temperature range. The resulting electrolyte 40 has a conductivity similar to that of EC+PC electrolyte 40 and, like carbonates, can also form a passivation film. However, BL readily decomposes in water, is highly toxic, and has a significantly lower cycling efficiency than organic carbonate solvents, making it rarely used in lithium-ion batteries. Linear carboxylates primarily include methyl formate (MF), methyl acetate (MA), methyl butyrate (MB), and ethyl propionate (EP). These esters have freezing points, on average, 20°C to 30°C lower than carbonates and have lower viscosities, thus improving the low-temperature performance of electrolyte 40.
[0110] In some possible embodiments, the electrolyte 40 further includes at least one auxiliary additive selected from the group consisting of biphenyl, fluorobenzene, trifluoromethylethylene carbonate, fluoroethylene carbonate, bisfluoroethylene carbonate, vinyl ethylene carbonate, 1,3-propane sultone, 1,4-butane sultone, 1,3-propylene sulfate, vinyl sulfate, vinyl sulfite, methylene methanedisulfonate, succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,3,6-hexanetrionitrile, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), and lithium difluorophosphate. In this case, the electrolyte 40 may further include auxiliary additives. By adding auxiliary additives, the stability of the CEI and SEI films can be further improved, the safety of the battery can be improved, the acid and water content in the electrolyte 40 can be controlled, and the conductivity and other properties of the electrolyte 40 can be improved. Among them, biphenyl can be used as an overcharge protection additive for electrolyte 40. It undergoes an oxidative electropolymerization reaction at an overcharge voltage of 4.5V to 4.6V, forming an electropolymer at the battery's positive electrode, which can effectively maintain the battery voltage in a relatively safe range. Fluorine-containing additives such as fluorobenzene, trifluoromethyl ethylene carbonate, fluoroethylene carbonate, bisfluoroethylene carbonate, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate, and lithium difluorophosphate can effectively improve the battery's thermal stability, ionic conductivity, and low-temperature performance. Sulfate and sulfonate additives such as 1,3-propane sultone, 1,4-butane sultone, 1,3-propylene sulfate, vinyl sulfate, vinyl sulfite, and methylene methanedisulfonate can form high-quality interfacial films on both the positive and negative electrodes, significantly improving the performance of lithium-ion batteries. Nitrile additives such as succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, and 1,3,6-hexanetricarbonitrile exhibit excellent stability and strong oxidation resistance at the positive electrode. Furthermore, the cyano group possesses strong coordination ability, allowing it to bind to active sites on the electrode surface (such as high-valent metal ions like nickel, cobalt, and manganese), shielding these active ions and reducing the electrode's decomposition of the electrolyte 40. Nitriles are inherently stable at the positive electrode, capable of complexing active ions and without forming a high-resistance surface film. Therefore, nitriles enhance the electrolyte 40's resistance to positive electrode oxidation, thereby increasing the electrolyte 40's cycle life at high voltages. Boron-containing additives such as lithium bis(oxalatoborate) and lithium difluorooxalatoborate, when applied to lithium-ion batteries with various positive electrode materials, can form a protective film on the positive electrode surface during battery cycling, stabilizing the electrode / electrolyte 40 interface and improving battery performance.
[0111] In some possible embodiments, the secondary battery includes a lithium-ion battery. A lithium-ion battery is a type of rechargeable battery that uses graphite or other carbon materials as the negative electrode and a lithium-containing compound as the positive electrode. It is a type of battery that uses lithium metal or lithium alloy as the positive / negative electrode material and uses a non-aqueous electrolyte solution. A lithium-ion battery is essentially a battery with a concentration difference. The positive and negative electrode materials have different electrochemical potentials and are separated by a separator 30. + From the intercalation material electrode with higher chemical potential to the electrode with lower potential, only lithium ions can move through the separator 30 in the electrolyte 40, and the charge compensation electrons can only move through the external circuit to form a current for output use. Discharge process: In a fully charged lithium-ion battery, lithium ions are embedded in the anode material. The anode (negative electrode) has many micropores, and lithium ions are embedded in the micropores of the negative electrode. During discharge, Li + Electrons move from the anode to the cathode through the diaphragm 30. Electrons cannot pass through the diaphragm 30 and can only move to the positive electrode through the negative electrode of the external circuit. Electrons are negatively charged, and the direction of electrons is from the negative electrode to the positive electrode, and the direction of current is from the positive electrode to the negative electrode. Charging process: When the battery is charged, lithium ions are generated on the cathode of the battery, and the generated lithium ions move to the anode through the electrolyte 40. The anode has many micropores, and the lithium ions that reach the anode are embedded in the anode micropores. The more lithium ions are embedded, the higher the charging capacity. Therefore, lithium-ion batteries mainly rely on the movement of lithium ions between the positive electrode 10 and the negative electrode 20 to work. During the charging and discharging process, Li + Insertion and deinsertion back and forth between the two electrodes: During charging, Li + It is deintercalated from the positive electrode and intercalated into the negative electrode through the electrolyte, and the negative electrode is in a lithium-rich state; the opposite is true during discharge.
[0112] In some possible embodiments, the negative electrode 20 contains at least one negative electrode active material 202 selected from carbon-based negative electrode materials, silicon-based negative electrode materials, and lithium titanate. The battery negative electrode active material 202 plays the role of storing and releasing energy in the secondary battery, and mainly affects the battery's initial efficiency, cycle performance, etc. The negative electrode active material 202 can be divided into two categories according to the different negative electrode active substances: carbon-based and non-carbon-based negative electrode materials. Among them, carbon-based materials can be divided into carbon-based negative electrode materials such as graphite (such as commercial graphite G49, AML906, QCG-H2), hard carbon, soft carbon and graphene. Among them, graphite negative electrode materials can be further divided into natural graphite, artificial graphite, composite graphite and mesophase carbon microbeads. Natural graphite and artificial graphite are the most widely used. Non-carbon-based materials are divided into non-carbon materials such as silicon-based negative electrode materials and lithium titanate. Among them, silicon-based negative electrode materials include silicon alone, compounds formed by silicon and non-metals, compounds formed by silicon and metals, etc.
[0113] In some possible embodiments, a secondary battery includes at least one of a battery cell, a battery module, and a battery pack. A battery cell refers to a single electrochemical cell containing positive and negative electrodes, which is the smallest unit of a power battery and also an electrical energy storage unit. The components of a battery cell include four main parts: a positive electrode 10, a negative electrode 20, an electrolyte 40, and a separator 30. A battery module refers to a plurality of battery cells encapsulated together in the same outer shell frame, which are connected to the outside through a unified boundary, thus forming a module. A battery pack refers to a plurality of battery cells or battery modules that are jointly controlled or managed by a battery management system (BMS) and a thermal management system. This unified whole is called a battery pack.
[0114] In some possible implementations, the embodiments of the present application have no particular limitation on the shape of the battery cell, which may be cylindrical, square, or any other shape.
[0115] In some embodiments, the outer packaging of a battery cell may include a housing and a cover. The positive electrode sheet, the negative electrode sheet, and the separator may be wound and / or laminated to form an electrode assembly. The electrode assembly is encapsulated in a housing. The electrolyte 40 is infiltrated into the electrode assembly. The number of electrode assemblies contained in a battery cell may be one or more, and can be adjusted based on actual needs. The composite separator 30 of the above-described embodiment is disposed between the positive and negative electrode sheets.
[0116] In some possible implementations, the battery cells according to the present application can be assembled into a battery module. A battery module can contain multiple battery cells, the specific number of which can be adjusted based on the application and capacity of the battery module. Within a battery module, multiple battery cells can be arranged sequentially along the length of the battery module. Of course, any other arrangement is also possible.
[0117] In some possible implementations, the battery module may further include a housing having a receiving space, and the plurality of battery cells are received in the receiving space.
[0118] In some possible implementations, the above-mentioned battery cells and / or battery modules may also be assembled into a battery pack, and the number of battery cells or battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0119] In some possible implementations, a battery pack may include a battery box and a plurality of battery modules disposed in the battery box. The plurality of battery modules may be arranged in the battery box in any manner.
[0120] The secondary battery in the above embodiments of the present application can be manufactured by the following method.
[0121] In a second aspect, as shown in FIG2 , an embodiment of the present application provides a method for preparing a secondary battery, comprising the following steps:
[0122] S10 obtains the positive electrode 10, the negative electrode 20 and the separator 30, wherein the positive electrode 10 contains a positive electrode active material 102, the positive electrode active material 102 includes an active material core and a carbon material coating layer;
[0123] S20. An electrolyte solution 40 is prepared comprising an electrolyte salt, an organic solvent and an additive; wherein the additive comprises a silane-type additive; determining the amount of the silane-type additive based on the specific surface area of the positive electrode active material 102 and the content of the carbon material in the positive electrode active material 102;
[0124] S30 . Assemble the positive electrode 10 , the negative electrode 20 , the separator 30 and the electrolyte 40 into a secondary battery.
[0125] Thus, the method for preparing a secondary battery provided in an embodiment of the present application comprises preparing an electrolyte 40 comprising an electrolyte salt, an organic solvent, and an additive, and then assembling the electrolyte 40 with the positive electrode 10, the negative electrode 20, and the separator 30 to obtain a secondary battery. The electrolyte contains a silane-type additive in an amount determined based on the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material. On the one hand, the silane-type additive can preferentially react with active sites such as oxygen-containing functional groups in the carbon material on the surface of the positive electrode active material 102, preferentially forming a CEI film on the positive electrode surface, passivating the reactivity of the carbon material coating surface, reducing the irreversible consumption of active metal ions, inhibiting the disordering of the carbon material coating, ensuring metal ion transmission channels, and thus improving battery cycle performance. On the other hand, the reasonable amount of the required additive is determined based on the physical and chemical properties of the electrode material, avoiding problems such as the inability to effectively reduce side reactions between the electrolyte 40 and the electrode material and reduce internal resistance due to improper additive dosage in the electrolyte 40, thereby better ensuring the electrochemical performance of the secondary battery.
[0126] In step S10, a positive electrode 10, a negative electrode 20, and a separator 30 are obtained. The positive electrode 10 contains a positive electrode active material 102, which includes an active material core and a carbon material coating. The positive electrode 10, the negative electrode 20, and the separator 30 can be purchased directly from commercial sources or prepared by methods known in the art.
[0127] In some possible implementations, the negative electrode 20 includes a negative electrode current collector 201 and a negative electrode material layer coated on the surface of the negative electrode current collector 201. In addition to the negative electrode active material 202, the negative electrode material layer may also include a certain amount of binder, conductive agent and other components.
[0128] In some possible implementations, the negative electrode active material 202 is a carbon-based material capable of accepting and releasing lithium ions, including but not limited to carbon-based negative electrode materials such as graphite (e.g., commercial graphite G49, AML906, QCG-H2), soft carbon (e.g., coke), and hard carbon; or silicon-based negative electrode materials such as silicon, compounds formed by silicon and non-metals, or compounds formed by silicon and metals; or negative electrode active material 202 such as lithium titanate. These are merely exemplary descriptions and are not specifically limited herein.
[0129] In some possible implementations, the negative electrode current collector 201 may be a metal foil, such as copper foil, gold foil, platinum foil, etc. This is only for illustrative purposes and is not specifically limited herein.
[0130] In some possible implementations, typical but non-limiting examples of the binder include sodium carboxymethylcellulose (CMC-Na), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), lithium polyacrylate (LiPAA), etc. These are merely exemplary and are not specifically limited herein.
[0131] In some possible implementations, the conductive agent may be typically but not limited to amorphous carbon, carbon nanotubes, carbon fibers, graphene, etc. This is merely an example and is not specifically limited herein.
[0132] In some possible implementations, the preparation of the negative electrode 20 includes the following steps: mixing the negative electrode active material 202 with a conductive agent such as conductive carbon black, a binder such as carboxymethyl cellulose and styrene-butadiene rubber, and a solvent such as water in a mass ratio of (80-99):(1-5):(2-10):100 to form a negative electrode mixed slurry, vacuum degassing, discharging, coating on a coating machine, and obtaining the negative electrode 20 after rolling, slitting, and die-cutting.
[0133] In some possible implementations, the positive electrode 10 includes a positive electrode current collector 101 and a positive electrode material layer coated on the surface of the positive electrode current collector 101. In addition to the positive electrode active material 102, the positive electrode material layer may also include a certain amount of binder, conductive agent and other components.
[0134] In some possible implementations, the positive electrode active material 102 in the positive electrode 10 includes an active material core and a carbon material coating layer. In this case, the carbon material coating layer can improve the conductivity of the active material core, which helps reduce internal resistance and polarization, and improve battery characteristics such as cycle life, fast charging performance, and energy efficiency.
[0135] In some possible embodiments, the mass percentage of the carbon material in the positive electrode active material 102 is 0.5% to 5%. In this case, the content of the carbon material coating layer in the positive electrode active material 102 can ensure sufficient and complete coating of the active material core, improve the conductivity of the active material core, and help reduce internal resistance and polarization, thereby improving battery cycle life, fast charging performance, energy efficiency, and other characteristics.
[0136] In some possible implementations, the active material core includes at least one of a metal oxide and a polyanion salt. In some specific embodiments, the metal oxide includes at least one of lithium cobaltate, lithium nickelate, lithium nickel cobalt manganeseate, lithium nickel cobalt aluminumate, lithium manganate, lithium nickel manganeseate, and lithium vanadate. In some specific embodiments, the polyanion salt includes at least one of lithium iron phosphate, lithium manganese phosphate, lithium iron manganese phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium nickel phosphate, lithium iron silicate, lithium ferrous fluorosulfate, lithium iron borate, and lithium iron titanate. In this case, the active materials included in the core of the positive electrode active material 102 have characteristics such as high capacity and safety.
[0137] In some possible embodiments, the specific surface area of the positive electrode active material 102 is 0.1 m 2 / g~20m 2 In this case, the specific surface area of the positive electrode active material 102 ensures a large active surface area for ion insertion and removal during the charge and discharge process of the battery, and is also conducive to controlling the side reactions between the positive electrode active material 102 and the electrolyte 40 .
[0138] In some possible implementations, the positive electrode current collector 101 may be a metal foil, such as aluminum foil, gold foil, platinum foil, etc. This is merely an example and is not specifically limited herein.
[0139] In some possible implementations, the binder may be typically but not limited to polyvinylidene fluoride (PVDF), acrylonitrile multipolymer, polyacrylic acid, hydroxypropyl methylcellulose, etc. This is only for illustrative purposes and is not specifically limited herein.
[0140] In some possible implementations, the conductive agent may be typically but not limited to amorphous carbon, carbon nanotubes, carbon fibers, graphene, etc. This is merely an example and is not specifically limited herein.
[0141] In some possible implementations, the preparation of the positive electrode 10 includes the following steps: preparing a positive electrode mixed slurry of the positive electrode active material 102 with a conductive agent such as conductive carbon black, a binder such as polyvinylidene fluoride, and a solvent such as N-methylpyrrolidone in a mass ratio of (80-99):(1-5):(2-10):100, vacuum degassing, discharging, coating on a coating machine, and obtaining the positive electrode 10 after rolling, slitting, and die-cutting.
[0142] In some possible implementations, in a secondary battery, the separator 30 can block the passage of electrons while allowing the passage of ions. Exemplary separators 30 include, but are not limited to, single-layer polypropylene (PP), single-layer polyethylene (PE), double-layer PP / PE, double-layer PP / PP, triple-layer PP / PE / PP, and ceramic-coated PE.
[0143] In step S20, an electrolyte solution 40 is prepared, comprising an electrolyte salt, an organic solvent, and an additive. The additive includes a silane-type additive, and the amount of the silane-type additive is determined based on the specific surface area of the positive electrode active material 102 and the carbon material content in the positive electrode active material 102. A typical but non-limiting step for preparing the electrolyte solution 40 includes preparing a mixed solution of the electrolyte salt, the organic solvent, and the additive to obtain the electrolyte solution 40.
[0144] In some possible embodiments, in the secondary battery, the mass percentage of the silane additive in the electrolyte 40 is marked as f, in %, and the specific surface area of the positive electrode active material 102 is marked as a, in m 2 / g, mark the mass percentage of carbon material in the positive electrode active material 102 as e, with a unit of %, so that Z = f / (a*e) satisfies 0.001≤Z≤15. In the relationship formula of Z = f / (a*e) in the embodiment of the present application, when the units of the parameters f, a, and e are determined, the value of Z is only related to the numerical value and is no longer affected by the parameter units. In this case, the amount of the silane-type additive is determined according to the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material, so that in the secondary battery at various stages such as before formation, after formation, capacity separation, and after circulation, the mass percentage f (in %) of the silane-type additive in the electrolyte 40 is equal to the specific surface area a (in m2) of the positive electrode active material 102. 2 The relationship between the mass percentage of the carbon material on its surface (a / g) and its mass percentage e (in %) is calculated as Z = f / (a*e), and both satisfy 0.001≤Z≤15. Under this condition, the electrode material and electrolyte 40 have a good matching effect, which can effectively reduce side reactions between the electrolyte 40 and the electrode material, reduce impedance, and improve battery cycle performance, thereby improving the battery's high-temperature performance.
[0145] In some possible embodiments, the silane-type additive includes at least one of tris(trimethylsilane) phosphate (TMSP), tris(trimethylsilane) borate (TMSB), tris(trimethylsilane) phosphite, tris(triethylsilane) phosphate, tris(triethylsilane) borate, tris(triethylsilane) phosphite, tris(trifluoromethylsilane) phosphate, tris(trifluoromethylsilane) borate, tris(trifluoromethylsilane) phosphite, tris(trifluoroethylsilane) phosphate, tris(trifluoroethylsilane) borate, and tris(trifluoroethylsilane) phosphite. In this case, these silane-type additives have a more suitable oxidation potential than other additives. During the first charge and discharge process of the battery, the silane-type additives preferentially react with active sites such as oxygen-containing functional groups in the carbon material on the surface of the positive electrode active material 102, passivate the reaction activity on the surface of the carbon material coating layer, inhibit the disorder of the carbon material coating layer, and are preferentially oxidized to generate silanes and compounds containing heteroatoms such as phosphorus and boron, forming a CEI film on the positive electrode surface.
[0146] In some possible embodiments, the mass percentage of the silane additive in the electrolyte 40 is 0.01% to 1.0%. In this case, the content of the silane additive ensures that the CEI film formed on the positive electrode surface has an appropriate thickness, which can effectively reduce the side reactions between the positive electrode material and the electrolyte 40, improve the battery cycle safety, and prevent the excessive thickness of the CEI film from affecting the battery impedance.
[0147] In some possible embodiments, the additive also includes vinylene carbonate. Compared to other negative electrode additives, vinylene carbonate has a better SEI film-forming effect on the negative electrode surface. In this case, vinylene carbonate can undergo an electrochemical reaction on the negative electrode surface during the initial charge and discharge process of the secondary battery to form a solid electrolyte interface film, or SEI film, effectively inhibiting the insertion of solvent molecules and battery bloating, thereby improving battery capacity and life.
[0148] In some possible embodiments, the weight percentage of vinylene carbonate in the electrolyte 40 is 0.1% to 5%. In this case, the vinylene carbonate fully ensures its film-forming effect on the surface of the negative electrode, forming a SEI film, isolating the electrolyte 40 from the negative electrode material, and inhibiting the deposition and reduction of metal ions at the negative electrode to form dendrites that damage the negative electrode structure and the stability of the SEI film.
[0149] In some possible embodiments, the electrolyte salt includes LiClO4, LiBF4, LiPF6, LiAsF6, LiCF3SO3, LiTDI, Li[(CF3SO2)2N], Li[(FSO2)2N], Li[(C m F 2m+1 SO2)(C n F2n+1 SO2)N], where m and n are natural numbers. In this case, these electrolytic salts can ensure high ionic conductivity of the electrolyte 40, do not cause harmful side reactions with the electrode materials, the electrolyte 40, the separator 30, etc., and have good chemical stability.
[0150] In some possible implementations, the molar concentration of the electrolyte salt in the electrolyte 40 is 0.01 mol / L to 5.0 mol / L. In this case, the concentration of the electrolyte salt can ensure high ionic conductivity of the electrolyte 40.
[0151] In some possible embodiments, the organic solvent includes at least one of a carbonate solvent, an ether solvent, and a carboxylate solvent. In this case, these organic solvents all have good solubility for electrolyte salts, and at the same time have low melting point, high boiling point, low vapor pressure, a wide operating temperature range, high dielectric constant and low viscosity, high conductivity and other characteristics. Among them, carbonate solvents include but are not limited to dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, trifluoromethyl ethylene carbonate, bis (2,2,2-trifluoroethyl) carbonate, (2,2,2-trifluoroethyl) methyl carbonate, etc. Ether solvents include but are not limited to tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, dimethoxymethane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis (2,2,2-trifluoroethyl) ether, etc. Carboxylate solvents include, but are not limited to, methyl formate, ethyl formate, ethyl acetate, propyl acetate, propyl propionate, methyl difluoroacetate, methyl trifluoroacetate, and the like.
[0152] In some possible embodiments, the electrolyte 40 further includes at least one auxiliary additive selected from the group consisting of biphenyl, fluorobenzene, trifluoromethyl ethylene carbonate, fluoroethylene carbonate, bisfluoroethylene carbonate, vinyl ethylene carbonate, 1,3-propane sultone, 1,4-butane sultone, 1,3-propylene sulfate lactone, vinyl sulfate, vinyl sulfite, methylene methanedisulfonate, succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,3,6-hexanetrionitrile, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), and lithium difluorophosphate.
[0153] In step S30, the method for assembling the positive electrode 10, negative electrode 20, separator 30, and electrolyte 40 into a secondary battery includes, but is not limited to: forming a core from the positive electrode 10, negative electrode 20, and separator 30 according to conventional processes, coating the core with an insulating film around the periphery and bottom, securing the core with tape, assembling the core into a shell, welding and sealing, baking at 80°C to 100°C, injecting electrolyte 40, impregnating, forming, and dividing the electrolyte, thereby obtaining a secondary battery. The core can be either a wound cell or a laminated cell.
[0154] In a third aspect, the present application provides an electrical device, which includes the above-mentioned secondary battery, or the secondary battery prepared by the above-mentioned method.
[0155] The electrical equipment provided in the embodiments of the present application includes the secondary battery with high safety performance and excellent electrochemical performance, thereby improving the safety and stability of the electrical equipment.
[0156] In some possible implementations, the electrical equipment may select the aforementioned secondary batteries such as battery cells, battery modules or battery packs according to its usage requirements.
[0157] In some possible implementations, the electrical device may be, but is not limited to, a mobile device, such as a mobile phone, a laptop computer, etc., or an electric vehicle, such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., or an electric train, a ship, a satellite, an energy storage system, etc.
[0158] In some specific embodiments, the electric device may be a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, etc. In order to meet the high power and high energy density requirements of such electric devices, the above-mentioned battery pack or battery module may be used.
[0159] In other specific embodiments, the power-consuming device may also be a recorder, radio, electronic learning machine, mobile phone, tablet computer, laptop computer, etc. Such power-consuming devices are generally required to be lightweight and thin, and can use the battery cells described in the above embodiments as a power source. For example, a schematic diagram of a mobile terminal 300 power-consuming device is shown in FIG3 .
[0160] Example
[0161] The following description will be made in conjunction with specific examples. The examples described below are exemplary and are intended only to explain the present application and are not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the examples, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used without manufacturer's indication are conventional products that can be purchased commercially.
[0162] The positive and negative electrode materials used in the lithium-ion batteries of the following examples and comparative examples of the present application include the following types. The materials used can be prepared according to known technologies or commercially available products.
[0163] Active material core of the positive electrode active material 102: LiFePO4 (LFP), LiFe 0.5 Mn 0.5PO4(LMFP), LiCoO2(LCO) or LiNi8Co1Mn1O2(NCM).
[0164] Negative electrode active material 202: graphite material.
[0165] Examples 1 to 22
[0166] Embodiments 1 to 22 of the present application respectively provide a lithium-ion battery, including a positive electrode 10, a negative electrode 20, a separator 30, and an electrolyte 40, wherein the separator 30 is disposed between the positive electrode 10 and the negative electrode 20, and the electrolyte 40 is filled between the positive electrode 10 and the negative electrode 20 and infiltrates the separator 30.
[0167] The positive electrode 10 contains a positive electrode active material 102, which includes an active material core and a carbon material coating layer. The material of the active material core and the mass percentage of the carbon material coating layer in the positive electrode active material 102, the specific surface area of the positive electrode active material 102, and the Raman test R=I of the positive electrode active material 102 in each embodiment are shown in FIG. D / I G The values of and other parameters are shown in Table 1 below.
[0168] The electrolyte 40 includes ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), lithium hexafluorophosphate (LiPF6), vinylene carbonate (VC) and a silane-type additive. The mass ratio of EC:EMC:DMC is 30:30:40, the molar concentration of lithium hexafluorophosphate is 1 mol / L, and the mass percentage of vinylene carbonate (VC) and the specific type and content of the silane-type additive (tris(trimethylsilyl)phosphate TMSP, tris(trimethylsilyl)borate TMSB) are shown in Table 1 below.
[0169] The preparation of lithium-ion batteries includes the following steps:
[0170] 1. Preparation of positive electrode 10: Weigh 2% polyvinylidene fluoride (PVDF), 2% conductive agent Super P, and 96% positive electrode active material 102 (see Table 1 below for details of different embodiments) in percentage by weight, add them to N-methylpyrrolidone (NMP) in sequence, stir and mix thoroughly, apply the slurry on an aluminum foil current collector, dry, cold press, and cut to produce positive electrode sheets.
[0171] 2. Preparation of negative electrode 20: Weigh 1.5% sodium carboxymethyl cellulose (CMC), 2.5% styrene-butadiene rubber (SBR), 1% Super P and 95% negative electrode active material 202 graphite in percentage by weight, add them to deionized water in sequence, stir and mix thoroughly, apply the slurry on a copper foil current collector, dry, cold press and cut to obtain negative electrode sheets.
[0172] 3. Preparation of electrolyte 40: Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of EC:EMC:DMC = 30:30:40, and lithium hexafluorophosphate (LiPF6) was added to the resulting mixture to a molar concentration of 1 mol / L. Vinylene carbonate (VC) and different types of silane-type additives (see Table 1 below for details of different embodiments) were then added to obtain electrolyte 40.
[0173] 4. Battery assembly: The positive electrode 10, negative electrode 20 and commercial PE separator 30 prepared above are made into a battery cell, which is packaged with a polymer and perfused with the electrolyte 40 prepared above. After infiltration, formation and volume separation, a 4Ah soft-pack lithium-ion battery is obtained.
[0174] Comparative Examples 1 to 4
[0175] Comparative Examples 1 to 4 of the present application respectively provide a lithium-ion battery, which differs from Example 1 in that: the active material core in the positive electrode active material 102, the specific surface area of the positive electrode active material 102, the mass percentage of the carbon material in the positive electrode active material 102, the vinylene carbonate (VC) content or the silane-type additive content, as shown in Table 1 below.
[0176] The following tests were carried out on the above embodiments and comparative examples respectively:
[0177] 1. The Z values for each Example and Comparative Example were calculated using the mass percentage f of the silane additive in the electrolyte 40, the specific surface area a of the positive electrode active material 102, and the mass percentage e of the carbon material on its surface, according to Z = f / (a*e). The calculation results are shown in Table 1 below.
[0178] 2. An area of 100 μm × 100 μm was selected on the positive electrode active material 102, and the positive electrode sheet within the area was scanned using a laser microconfocal Raman spectrometer to obtain the D peak and G peak of the carbon material on all positive electrode material particles within the area. The data was processed using LabSpec software to obtain the peak intensities of the D peak and G peak of the carbon material on each positive electrode active material particle 102, which are I(D) and I(G), respectively. The R value = I D / I G The value of is the average value of the ratio of I(D) to I(G) of the carbon layer on all particles of the positive electrode active material 102 measured within this range. The test results are shown in Table 1 below.
[0179] 3. The 55°C high temperature cycle performance and 60°C high temperature cycle performance of the lithium ion batteries prepared in the above embodiments and comparative examples were tested respectively. The test methods were carried out according to the following test examples:
[0180] ①55℃ high temperature cycle performance test:
[0181] The lithium-ion batteries prepared in the examples and comparative examples were placed in an oven at a constant temperature of 55±3°C and charged at a constant current of 1C to 3.65V (when the core of the positive electrode active material is LiFePO4), 4.1V (when the core of the positive electrode active material is LiFe 0.5 Mn 0.5 PO4), 4.5V (when the core of the positive electrode active material is LiCoO2), 4.25V (when the core of the positive electrode active material is LiNi8Co1Mn1O2), and then charge at a constant voltage until the current drops to 0.05C, and rest for 10 minutes. Then, discharge at a constant current of 1C to 2.5V (LiFePO4), 2.5V (LiFe 0.5 Mn 0.5 PO4), 3.0V (LiCoO2), 2.75V (LiNi8Co1Mn1O2), and so on for 500 cycles. The discharge capacity of the 1st and 500th cycles was recorded, and the capacity retention rate of the cycle was calculated as follows:
[0182] Capacity retention (%)=discharge capacity at the 500th cycle / discharge capacity at the 1st cycle×100%.
[0183] ②60℃ storage for 30 days performance test:
[0184] Under the condition of ambient temperature of 25±3℃, the battery is charged and discharged once at 0.2C / 0.2C, and the capacity of this time is the initial capacity; the battery is charged again at 0.2C constant current to 3.65V (LiFePO4), 4.1V (LiFe 0.5 Mn 0.5 PO4), 4.5V (LiCoO2), 4.25V (LiNi8Co1Mn1O2), and then charge at a constant voltage until the current drops to 0.05C. The charged battery is placed at 60°C for 30 days, then placed in an open circuit at room temperature for 2 hours, and discharged at a constant current of 0.2C to 2.5V (LiFePO4), 2.5V (LiFe 0.5 Mn 0.5 PO4), 3.0V (LiCoO2), 2.75V (LiNi8Co1Mn1O2), record it as the remaining capacity, and calculate the remaining capacity retention rate of the cycle record according to the following formula:
[0185] Record the remaining capacity retention rate (%) = remaining capacity / initial capacity × 100%.
[0186] The test results are shown in Table 1 below:
[0187] Table 1
[0188] As can be seen from the test results in Table 1 above, the lithium-ion batteries prepared in Examples 1 to 22 of the present application, the positive electrode active material 102 includes an active material core and a carbon material coating layer, the electrolyte 40 includes an electrolyte salt, an organic solvent and an additive, and the amount of the silane-type additive in the lithium-ion battery is such that Z=f / (a*e) in the battery satisfies 0.001≤Z≤15, wherein f is the mass percentage of the silane-type additive, a is the specific surface area of the positive electrode active material 102, and e is the mass percentage of the carbon material in the positive electrode active material 102. Through the reasonable combination of the electrode material and the electrolyte 40, the additive in the electrolyte 40 can form a CEI film on the positive electrode surface and a SEI film on the negative electrode surface during the first charge and discharge process, respectively, thereby inhibiting the dissolution of electrode metal ions, reducing the catalytic side reactions between the electrolyte 40 and the electrode material, reducing the battery impedance, and improving the battery cycle performance. The lithium-ion batteries of the embodiment all exhibit better capacity retention after 500 cycles at 55° C. and capacity retention after 30 days of storage at 60° C., thereby improving the high-temperature performance of the lithium-ion batteries.
[0189] This demonstrates that, given fixed parameters such as the specific surface area of vinylene carbonate (VC), the positive electrode active material 102, and the carbon coating layer content, the amount of the silane additive can be rationally designed based on Z = f / (a*e), satisfying 0.001 ≤ Z ≤ 15, leading to improved battery cycling and high-temperature energy storage performance. This is due to the fact that the silane additive preferentially reacts at the active sites of the carbon coating layer during the initial charge and discharge process, passivating the surface reactivity of the carbon coating layer and effectively preventing catalytic side reactions between the active sites on the carbon coating layer and the electrolyte 40. This reduces the irreversible consumption of active lithium and the blockage or structural collapse of the lithium-conducting channels in the carbon coating layer. This also facilitates the formation of an effective CEI film on the positive electrode surface, inhibiting the dissolution of positive electrode metal ions, thereby reducing impedance, improving battery cycling performance, and enhancing high-temperature performance.
[0190] Specifically, by comparing the comparative diagram of the 55°C high-temperature cycling performance test of the lithium-ion battery of Example 1 and Comparative Example 1 in Figure 4, and the test data of Examples 1 and 2 and Comparative Example 1, Comparative Example 9 and Comparative Example 2, Comparative Example 14 and Comparative Example 3, and Comparative Examples 19 and 20 and Comparative Example 4 in Table 1, it can be seen that the main difference is that the electrolyte 40 of the comparative example does not contain a silane-type additive. The high-temperature cycling performance and high-temperature storage performance of the lithium-ion batteries prepared in the comparative example both show lower performance. This indicates that if the electrolyte 40 does not contain a silane-type additive, the active sites of the carbon material coating layer on the surface of the positive electrode active material 102 cannot be passivated, resulting in an intensification of the side reaction with the electrolyte 40, leading to a deterioration of the battery's cycling performance and high-temperature storage performance.
[0191] By comparing the results of Example 13 and Example 21, it can be seen that when Z<0.001, the content of the silane-type additive is too small to completely passivate the active sites of the surface coating layer of the positive electrode active material 102, the inhibitory effect on the side reactions in the late stage of the battery cycle is weakened, the effect on the cycle improvement is small, and the storage performance deteriorates.
[0192] By comparing the test results of Example 13 and Example 22, it can be seen that when the core of the active material is LFP polyanion salt, as the value of Z increases, the content of the silane-type additive increases, the thickness of the passivation film will increase, thereby increasing the impedance and the charge and discharge polarization, which has a poor effect on improving the battery cycle and reduces the storage performance.
[0193] Finally, it should be noted that the above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any changes or substitutions within the technical scope disclosed in this application should be included in the scope of protection of this application. Therefore, the scope of protection of this application should be based on the scope of protection of the claims.
Claims
1. A secondary battery, characterized in that: The secondary battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode contains a positive electrode active material, the positive electrode active material comprises an active material core and a carbon material coating layer, the electrolyte comprises an electrolyte salt, an organic solvent and an additive, the additive comprises a silane-type additive; wherein the amount of the silane-type additive is determined according to the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material.
2. The secondary battery according to claim 1, wherein: In the secondary battery, the mass percentage of the silane additive in the electrolyte is marked as f, in %, and the specific surface area of the positive electrode active material is marked as a, in m 2 / g, the mass percentage of the carbon material in the positive electrode active material is marked as e, with the unit of %, so that Z=f / (a*e) satisfies 0.001≤Z≤15.
3. The secondary battery according to claim 1 or 2, characterized in that: The silane-type additive includes at least one of tris(trimethylsilane)phosphate, tris(trimethylsilane)borate, tris(trimethylsilane)phosphite, tris(triethylsilane)phosphate, tris(triethylsilane)borate, tris(triethylsilane)phosphite, tris(trifluoromethylsilane)phosphate, tris(trifluoromethylsilane)borate, tris(trifluoromethylsilane)phosphite, tris(trifluoroethylsilane)phosphate, tris(trifluoroethylsilane)borate, and tris(trifluoroethylsilane)phosphite.
4. The secondary battery according to claim 3, characterized in that: The mass percentage of the silane type additive in the electrolyte is 0.01% to 1.0%.
5. The secondary battery according to claim 3, characterized in that: The mass percentage of the carbon material in the positive electrode active material is 0.5% to 5%.
6. The secondary battery according to claim 3, characterized in that: The specific surface area of the positive electrode active material is 0.1 m 2 / g~20m 2 / g.
7. The secondary battery according to any one of claims 1, 2, 4 to 6, characterized in that: The active material core includes at least one of metal oxides and polyanion salts.
8. The secondary battery according to claim 7, characterized in that The metal oxides include at least one of lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium nickel manganese oxide, and lithium vanadate; and / or, The polyanion salts include at least one of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium nickel phosphate, lithium iron silicate, lithium ferrous fluorosulfate, lithium iron borate, and lithium iron titanate.
9. The secondary battery according to claim 8, characterized in that When the active material core includes the metal oxide, the specific surface area of the positive electrode active material is 0.1 m 2 / g~1.0m 2 / g, satisfying 0.01≤Z≤15.
10. The secondary battery according to claim 9, characterized in that When the active material core includes the metal oxide, the specific surface area of the positive electrode active material is 0.2 m 2 / g~0.8m 2 / g, satisfying 0.02≤Z≤10.
11. The secondary battery according to claim 8, wherein When the active material core includes the polyanion salt, the specific surface area of the positive electrode active material is 7 m 2 / g~20m 2 / g; satisfying 0.001≤Z≤0.
2.
12. The secondary battery according to claim 11, wherein: When the active material core includes the polyanion salt, the specific surface area of the positive electrode active material is 9 m 2 / g~15m 2 / g; satisfying 0.002≤Z≤0.
1.
13. The secondary battery according to any one of claims 1, 2, 4 to 6, 8 to 12, characterized in that: The peak intensity ratio of the D peak to the G peak of the positive electrode active material Raman test is R=I D / I G , R value range is 0.6~1.
3.
14. The secondary battery according to claim 13, characterized in that: The peak intensity ratio R of the D peak to the G peak in the Raman test of the positive electrode active material ranges from 0.8 to 1.
2.
15. The secondary battery according to any one of claims 1, 2, 4 to 6, 8 to 12, and 14, characterized in that: The additives also include vinylene carbonate.
16. The secondary battery according to claim 15, characterized in that: In the electrolyte, the mass percentage of the vinylene carbonate is 0.1% to 5%.
17. The secondary battery according to any one of claims 1, 2, 4 to 6, 8 to 12, 14 and 16, characterized in that: The electrolyte salt includes LiClO4, LiBF4, LiPF6, LiAsF6, LiCF3SO3, LiTDI, Li[(CF3SO2)2N], Li[(FSO2)2N], Li[(C m F 2m+1 SO2)(C n F 2n+1 SO2)N], wherein m and n are natural numbers.
18. The secondary battery according to claim 17, wherein: In the electrolyte solution, the molar concentration of the electrolyte salt is 0.01 mol / L to 5.0 mol / L.
19. The secondary battery according to any one of claims 1, 2, 4 to 6, 8 to 12, 14, 16, and 18, characterized in that: The organic solvent includes at least one of a carbonate solvent, an ether solvent, and a carboxylate solvent.
20. The secondary battery according to claim 19, wherein: The electrolyte also contains at least one auxiliary additive selected from the group consisting of biphenyl, fluorobenzene, trifluoromethylethylene carbonate, fluoroethylene carbonate, bisfluoroethylene carbonate, vinyl ethylene carbonate, 1,3-propane sultone, 1,4-butane sultone, 1,3-propylene sulfate, vinyl sulfate, vinyl sulfite, methylene disulfonate, succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,3,6-hexanetrinitrile, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), and lithium difluorophosphate.
21. The secondary battery according to any one of claims 1, 2, 4 to 6, 8 to 12, 14, 16, 18, and 20, characterized in that: The secondary battery includes a lithium ion battery.
22. The secondary battery according to any one of claims 1, 2, 4 to 6, 8 to 12, 14, 16, 18, and 20, characterized in that: The negative electrode contains at least one negative electrode active material selected from the group consisting of carbon-based negative electrode material, silicon-based negative electrode material, and lithium titanate.
23. The secondary battery according to any one of claims 1, 2, 4 to 6, 8 to 12, 14, 16, 18, and 20, characterized in that: The secondary battery includes at least one of a battery cell, a battery module, and a battery pack.
24. A method for preparing a secondary battery, characterized in that: The following steps are involved: Obtaining a positive electrode, a negative electrode and a separator, wherein the positive electrode contains a positive electrode active material, and the positive electrode active material includes an active material core and a carbon material coating layer; Preparing an electrolyte comprising an electrolyte salt, an organic solvent and an additive; wherein the additive comprises a silane-type additive; and determining the amount of the silane-type additive according to the specific surface area of the positive electrode active material and the content of the carbon material in the positive electrode active material; The positive electrode, the negative electrode, the separator and the electrolyte are assembled into a secondary battery.
25. The method for preparing a secondary battery according to claim 24, characterized in that: In the secondary battery, the mass percentage of the silane additive in the electrolyte is marked as f, in %, and the specific surface area of the positive electrode active material is marked as a, in m 2 / g, the mass percentage of the carbon material in the positive electrode active material is marked as e, with the unit of %, so that Z=f / (a*e) satisfies 0.001≤Z≤15.
26. The method for preparing a secondary battery according to claim 24 or 25, characterized in that: The silane-type additive includes at least one of tris(trimethylsilane)phosphate, tris(trimethylsilane)borate, tris(trimethylsilane)phosphite, tris(triethylsilane)phosphate, tris(triethylsilane)borate, tris(triethylsilane)phosphite, tris(trifluoromethylsilane)phosphate, tris(trifluoromethylsilane)borate, tris(trifluoromethylsilane)phosphite, tris(trifluoroethylsilane)phosphate, tris(trifluoroethylsilane)borate, and tris(trifluoroethylsilane)phosphite.
27. The method for preparing a secondary battery according to claim 26, characterized in that: The mass percentage of the silane type additive in the electrolyte is 0.01% to 1.0%.
28. The method for preparing a secondary battery according to claim 26, characterized in that: The mass percentage of the carbon material in the positive electrode active material is 0.5% to 5%.
29. The method for preparing a secondary battery according to claim 26, characterized in that: The specific surface area of the positive electrode active material is 0.1 m 2 / g~20m 2 / g.
30. An electrical equipment, characterized in that: The electrical device comprises a secondary battery as claimed in any one of claims 1 to 23, or a secondary battery prepared by the method as claimed in any one of claims 24 to 29.
Citation Information
Patent Citations
Secondary battery, preparation method thereof and electric equipment
CN118825369A
Non-aqueous electrolyte for lithium secondary battery, and lithium secondary battery comprising same
CN109075387A
Electrolyte and lithium ion battery
CN113675475A
Lithium ion battery
CN114447295A
Lithium ion battery
CN115939513A
Cited By
Battery cell, battery device and electric device
CN120545473A
Battery monomer, battery device and electric equipment
CN122393408A