Polymer coating material, preparation method therefor, and use thereof

By using a polymer coating material on the negative active material of a lithium-ion battery to form a polymer-conductive material hybrid coating layer, the problems of volume expansion and dispersion are solved, and the cycle performance and production efficiency of the lithium-ion battery are improved.

WO2024221284A1PCT designated stage expired Publication Date: 2024-10-31SHENZHEN YANYI NEW MATERIALS CO LTD

Patent Information

Application Number
PCT/CN2023/090918
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2023-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The negative active material of lithium-ion batteries expands severely in volume during the charge and discharge process, resulting in material separation and unstable structure, which affects the cycle performance and production efficiency of the battery. The slurry dispersion and liquid injection efficiency is low, which affects the production efficiency and performance of the battery. .

Method used

A polymer coating material containing active groups is combined with a conductive material to form a polymer-conductive material hybrid coating layer, which improves the hydrophilicity and conductivity of the negative active material, inhibits volume expansion, and improves dispersion and infiltration sex.

Benefits of technology

It significantly improves the liquid absorption efficiency and cycle performance of the negative electrode plate, extends the service life of the battery, and improves the production efficiency and performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023090918-FTAPPB-I100001
    Figure PCTCN2023090918-FTAPPB-I100001
  • Figure PCTCN2023090918-FTAPPB-I100002
    Figure PCTCN2023090918-FTAPPB-I100002
  • Figure PCTCN2023090918-FTAPPB-I100003
    Figure PCTCN2023090918-FTAPPB-I100003
Patent Text Reader

Abstract

The present application provides a polymer coating material, a preparation method therefor, and a use thereof. The polymer coating material comprises a combination of a polymer and a conductive material; the polymer contains an active group; the active group comprises a combination of a cyano group, a hydroxyl group, and a strongly hydrophilic group; and the strongly hydrophilic group comprises an amino group and / or a carboxyl group. The polymer coating material has excellent hydrophilicity and conductivity, and is used as a negative electrode active material modifier. On the one hand, the polymer coating material can improve the hydrophilicity of a negative electrode active material, improve the dispersity of the negative electrode active material in a negative electrode slurry, and improve the wettability and the electrolyte adsorption efficiency of a negative electrode sheet to an electrolyte; and on the other hand, the polymer coating material can inhibit the volume expansion of the negative electrode active material, and improve the conductivity to obtain a modified negative electrode active material having excellent hydrophilicity, dispersity, cycle performance, high capacity, and rate performance, thereby improving the production efficiency and the use performance of a lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

A polymer coating material and its preparation method and application Technical Field

[0001] The present application belongs to the technical field of lithium-ion battery materials, for example, a polymer coating material and its preparation method and application. Background Art

[0002] As a green and environmentally friendly new energy source, lithium-ion batteries offer advantages such as excellent reliability, high safety, compact size, and lightweight. They are currently widely used in a variety of fields, including digital products, electric vehicles, and military products. In recent years, to meet the demands of future electrification, particularly the further development of the digital product industry, represented by mobile phones, and the electric vehicle industry, lithium-ion batteries have faced significant challenges in improving their performance. Currently, the market demand for lithium-ion batteries is growing, and the requirements for their long cycle life are also increasing.

[0003] Lithium-ion batteries are typically assembled from a positive electrode, a negative electrode, a separator, and an electrolyte. The electrochemical performance of a battery is closely related to each component, with the positive and negative electrodes, in particular, having a decisive influence on the performance of lithium-ion batteries. Furthermore, the preparation processes of the positive and negative electrodes directly impact the production schedule and product performance of lithium-ion batteries. Conventional negative electrode sheet preparation methods involve mixing the negative electrode active material, a conductive agent, a binder, and a solvent (usually water) to form a negative electrode slurry. The negative electrode slurry is then coated onto a current collector and subjected to drying, roller pressing, and other processing steps to produce the negative electrode sheet. During the preparation of the negative electrode slurry, the slurry dispersion step is crucial in lithium-ion battery production, as the dispersion time of the negative electrode active material directly determines the production efficiency of the lithium-ion battery. However, the commonly used negative electrode active materials currently have a relatively hydrophobic surface, requiring a long time to disperse, which seriously affects battery production efficiency. Furthermore, if the negative electrode active material in the negative electrode slurry is poorly dispersed, the negative electrode sheet will be uneven, negatively impacting the performance of the lithium-ion battery.

[0004] Another important step in the production of lithium-ion batteries is injecting electrolyte into the battery. This involves injecting electrolyte into the battery after the positive and negative electrode sheets and separators are assembled into a cell and packaged (referred to as the "injection process"). During this process, the accuracy of the injection volume and the efficiency of the injection directly determine the consistency and production efficiency of the lithium-ion battery. Because the negative electrode sheets undergo winding, lamination, and extrusion during the preparation of the cell, the electrode sheet's liquid absorption efficiency is relatively low, requiring a long injection time and prone to uneven absorption, which seriously affects battery production efficiency and yield.

[0005] In addition to significant deficiencies in the negative electrode slurry dispersion and injection processes during lithium-ion battery production, the electrochemical performance of negative electrode active materials also has significant room for improvement. Current negative electrode active materials primarily include carbon-based and silicon-based materials. These materials undergo varying degrees of volume expansion during the charge and discharge process, with silicon-based materials experiencing particularly severe volume expansion. This can lead to pulverization and separation of the materials, damaging the battery electrode structure and making it difficult to form a stable SEI film. This results in continuous consumption of lithium ions and electrolyte, rapid battery cycle decay, and insufficient cycle stability.

[0006] Therefore, in order to improve the production efficiency of the slurry dispersion process and the liquid injection process and improve the cycle performance of lithium-ion batteries, developing anode materials with better performance is an urgent problem to be solved in this field.

[0007] Summary of the Invention

[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0009] The present application provides a polymer coating material, a preparation method thereof, and an application thereof. The polymer coating material has excellent hydrophilicity and electrical conductivity. As a modifier for negative electrode active materials, the polymer coating material can, on the one hand, improve the hydrophilicity of the negative electrode active material, thereby improving its dispersion performance in the negative electrode slurry, improving the production efficiency of the negative electrode slurry, and improving the wettability and liquid absorption efficiency of the negative electrode plate to the electrolyte; on the other hand, the polymer coating material can effectively inhibit the volume expansion of the negative electrode active material while improving the electrical conductivity, thereby obtaining a modified negative electrode active material with excellent hydrophilicity, dispersibility, cycle performance, high capacity and rate performance, thereby improving the production efficiency and performance of lithium-ion batteries.

[0010] This application adopts the following technical solutions:

[0011] In a first aspect, an embodiment of the present application provides a polymer coating material, wherein the polymer coating material comprises a combination of a polymer and a conductive material; the polymer contains active groups, wherein the active groups comprise a combination of cyano, hydroxyl and strongly hydrophilic groups, and the strongly hydrophilic groups comprise amino and / or carboxyl groups.

[0012] The polymer coating material provided in the embodiment of the present application includes a combination of a polymer containing an active group and a conductive material. As a negative electrode active material modifier, it can be coated on the surface of the negative electrode active material to form a modified negative electrode active material having a polymer-conductive material hybrid coating layer. The components of the polymer coating material and its technical effects are as follows: (1) The cyano group in the polymer has a strong adhesion to the negative electrode active material (such as graphite), so that the polymer coating material can be tightly coated on the surface of the negative electrode active material, inhibiting the volume expansion of the negative electrode active material during the charge and discharge process; (2) The polymer contains hydroxyl groups and strong hydrophilic groups and has good hydrophilicity. When the polymer coating material is coated on the surface of the negative electrode active material, the surface properties of the modified negative electrode active material are made more hydrophilic and easier to be evenly dispersed in the negative electrode slurry, which not only greatly shortens the slurrying time, but also improves the surface uniformity of the negative electrode plate; at the same time, due to this surface hydrophilicity, the negative electrode plate has a better wettability to the electrolyte. Good, can greatly improve the electrolyte infiltration speed of the negative electrode sheet, shorten the liquid absorption time, and improve the liquid absorption efficiency; (3) in the preparation process of the modified negative electrode active material, the hydroxyl group in the polymer reacts with the strong hydrophilic group (amino group and / or carboxyl group) by thermal cross-linking reaction, so that the coating layer on the surface of the modified negative electrode active material has strong water resistance while being hydrophilic, and will not fall off during the preparation process of the negative electrode slurry, so that the surface of the negative electrode active material has a stable coating layer, which inhibits the volume expansion of the negative electrode active material during the cycle; (4) The polymer coating material and the coating layer formed contain conductive materials, have good conductivity, can avoid the impedance degradation caused by the coating, and make the modified negative electrode active material have good conductivity and rate performance.

[0013] In summary, the embodiments of the present application, through the design of a polymer containing an active group and its compounding with a conductive material, make the polymer coating material have excellent hydrophilicity and conductivity, and can be used as a negative electrode active material modifier. On the one hand, it improves the hydrophilicity of the negative electrode active material, improves its dispersion performance in the negative electrode slurry, shortens the slurrying time, improves the production efficiency of the negative electrode slurry, and improves the wettability and liquid absorption efficiency of the negative electrode plate to the electrolyte; on the other hand, the polymer coating material can form a stable and reliable coating layer on the surface of the negative electrode active material, effectively inhibit the volume expansion of the negative electrode active material, and avoid the impedance degradation caused by the coating, and improve the conductive performance, thereby obtaining a modified negative electrode active material with excellent hydrophilicity, dispersibility, cycle performance, conductivity and rate performance, thereby improving the production efficiency of lithium-ion batteries and improving the cycle performance of lithium-ion batteries.

[0014] In one embodiment, the polymer is coated on the surface of the conductive material.

[0015] It should be noted that, in the polymer coating material, the coating of the conductive material by the polymer may be complete or partial.

[0016] In one embodiment, the mass percentage of the conductive material in the polymer coating material is 1-60%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or 55%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0017] As an optional technical solution in an embodiment of the present application, the weight percentage of the conductive material in the polymer coating material is 1-60%, so that the polymer coating material can form a stable polymer-conductive material hybrid coating layer on the surface of the negative electrode active material, inhibiting the volume expansion of the negative electrode active material during cycling, and improving the material's structural stability, cycling performance, and conductivity. If the conductive material content is too low, the improvement in conductivity is not significant, and the material may experience impedance degradation due to the coating. If the conductive material content is too high, the polymer coating effect is affected, resulting in the polymer coating material having a weak inhibitory effect on the volume expansion of the negative electrode active material, and failing to effectively improve the cycling performance.

[0018] In one embodiment, the conductive material includes any one of polythiophene, polypyrrole, polyaniline, carbon black, carbon nanotubes, carbon fibers, graphene, graphite, Ketjen black, and acetylene black, or a combination of at least two thereof.

[0019] As an optional technical solution of an embodiment of the present application, the strong hydrophilic group in the polymer includes a combination of amino and carboxyl groups, that is, the active group includes a combination of cyano, hydroxyl, amino and carboxyl groups.

[0020] In one embodiment, the molar percentage of cyano groups in the active group is 1-50%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0021] In one embodiment, the molar percentage of the hydroxyl group in the active group is 1-50%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0022] In one embodiment, the molar percentage of the strong hydrophilic group in the active group is 1-60%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or 55%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0023] In one embodiment, the molar percentage of the amino group in the active group is 1-20%, for example, it can be 2%, 3%, 5%, 7%, 9%, 10%, 11%, 13%, 15%, 17% or 19%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0024] In one embodiment, the molar percentage of the carboxyl group in the active group is 1-40%, for example, it can be 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35% or 38%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0025] As an optional technical solution of an embodiment of the present application, the active groups in the polymer include, by molar percentage, 1-50% cyano group, 1-50% hydroxyl group, 1-20% amino group, and 1-40% carboxyl group; thereby, on the one hand, the polymer has good hydrophilicity, so that the polymer coating material can improve the hydrophilicity and dispersion properties of the negative electrode active material, improve the production efficiency of the negative electrode slurry, and enhance the wettability and liquid absorption efficiency of the negative electrode electrode sheet to the electrolyte; on the other hand, a specific proportion of cyano groups enables the polymer to have good adhesion to the negative electrode active material, so that the polymer coating material is tightly coated on the surface of the negative electrode active material; at the same time, the hydroxyl group can undergo a thermal cross-linking reaction with the amino group and the carboxyl group to form a stable coating layer with good water resistance on the surface of the negative electrode active material, thereby inhibiting the volume expansion of the negative electrode active material during the charge and discharge process. If the active groups in the polymer are not a combination of cyano, hydroxyl, amino and carboxyl groups in a specific molar ratio, it will affect the coating and modification effect of the polymer coating material on the negative electrode active material, and it will be impossible to obtain a coating layer with hydrophilicity, water resistance and stability on the surface of the negative electrode active material, which will lead to the modified negative electrode active material being unable to take into account both good hydrophilicity and cycle stability.

[0026] In one embodiment, the polymerized monomers of the polymer include a combination of alkenyl nitrile monomers, hydroxyl-containing acrylate monomers, acrylamide monomers, and alkenyl carboxylic acid monomers.

[0027] In one embodiment, the polymerizable monomers include the following components in terms of molar percentage: 1-50% alkenyl nitrile monomers, 1-50% hydroxyl-containing acrylate monomers, 1-20% acrylamide monomers, and 1-40% alkenyl carboxylic acid monomers.

[0028] As an optional technical solution of the embodiment of the present application, the polymer is formed by copolymerizing alkenyl nitrile monomers, hydroxyl acrylate monomers, acrylamide monomers and alkenyl carboxylic acid monomers in a specific molar ratio, thereby making the obtained polymer contain four active groups: cyano, cyano, amino and carboxyl.

[0029] The molar percentage of the alkenyl nitrile monomer in the polymer monomer of the polymer is 1-50%, for example, 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%. etc.; the molar percentage of the hydroxyl-containing acrylate monomer is 1-50%, for example, 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%; the molar percentage of the acrylamide monomer is 1-20%, for example, 2%, 3%, 5%, 7%, 9%, 10%, 11%, 13%, 15%, 17% or 19%; the molar percentage of the alkenyl carboxylic acid monomer is 1-40%, for example, 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35% or 38%, and specific values ​​between the above points. Due to space limitations and for the sake of simplicity, the examples of this application will not exhaustively list the specific values ​​included in the above ranges.

[0030] In one embodiment, the alkenyl nitrile monomer includes any one of acrylonitrile, methacrylonitrile, and crotononitrile, or a combination of at least two thereof.

[0031] In one embodiment, the hydroxyl group-containing acrylic acid ester monomer includes any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate, or a combination of at least two thereof.

[0032] In one embodiment, the acrylamide monomer includes acrylamide and / or methacrylamide.

[0033] In one embodiment, the alkenyl carboxylic acid monomer includes any one of acrylic acid, methacrylic acid, and crotonic acid, or a combination of at least two thereof.

[0034] In a second aspect, an embodiment of the present application provides a method for preparing the polymer coating material as described in the first aspect, wherein the preparation method includes method A or method B;

[0035] The method A comprises: mixing a polymer solution with a conductive material to obtain the polymer coating material;

[0036] The method B comprises: mixing a polymer monomer solution with a conductive material and then performing a polymerization reaction to obtain the polymer coating material.

[0037] The preparation methods provided in the embodiments of this application include two categories: In Method A, a polymer is first obtained, and then the polymer solution is uniformly mixed with a conductive material to obtain the polymer-coated material. In Method B, a monomer solution of the polymer is uniformly mixed with a conductive material, and then a polymerization reaction is carried out to obtain the polymer-coated material. In Method B, because the polymerization reaction is carried out in the presence of a conductive material, the resulting polymer can be better coated on the surface of the conductive material.

[0038] In one embodiment, in method A, the preparation method of the polymer comprises: subjecting a polymerizable monomer to a polymerization reaction in the presence of an initiator to obtain the polymer.

[0039] In one embodiment, in method A, the initiator includes a water-soluble azo initiator and / or persulfate.

[0040] In one embodiment, in method A, the initiator is selected from any one of ammonium persulfate, potassium persulfate, or sodium persulfate, or a combination of at least two thereof.

[0041] In one embodiment, in method A, based on the mass of the polymerized monomer as 100%, the mass of the initiator is 0.05-5%, for example, it can be 0.08%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0042] In one embodiment, in method A, the polymerization reaction is carried out in the presence of a solvent, and the solvent preferably comprises water.

[0043] In one embodiment, in method A, the temperature of the polymerization reaction is 60-100°C, for example, it can be 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, 90°C, 92°C, 95°C or 98°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0044] In one embodiment, in method A, the polymerization reaction time is 0.5-12h, for example, it can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h or 11h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0045] In one embodiment, in method A, the solvent of the polymer solution comprises water.

[0046] In one embodiment, method B comprises: mixing a polymer monomer solution with a conductive material, and then performing a polymerization reaction in the presence of an initiator to obtain the polymer coating material.

[0047] In one embodiment, in method B, the solvent of the polymerization monomer solution includes water.

[0048] In one embodiment, in method B, the initiator includes a water-soluble azo initiator and / or persulfate, and may further optionally include any one or a combination of at least two of ammonium persulfate, potassium persulfate or sodium persulfate.

[0049] In one embodiment, in method B, based on the mass of the polymerized monomer as 100%, the mass of the initiator is 0.05-5%, for example, it can be 0.08%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0050] In one embodiment, in method B, the temperature of the polymerization reaction is 60-100°C, for example, it can be 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, 90°C, 92°C, 95°C or 98°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0051] In one embodiment, in method B, the polymerization reaction time is 0.5-12h, for example, it can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h or 11h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0052] In method A and method B, the polymerizable monomers include a combination of alkenyl nitrile monomers, hydroxyl-containing acrylate monomers, acrylamide monomers, and alkenyl carboxylic acid monomers.

[0053] In one embodiment, the polymerizable monomers include the following components in terms of molar percentage: 1-50% alkenyl nitrile monomers, 1-50% hydroxyl-containing acrylate monomers, 1-20% acrylamide monomers, and 1-40% alkenyl carboxylic acid monomers.

[0054] In a third aspect, an embodiment of the present application provides an application of the polymer coating material as described in the first aspect in a negative electrode active material.

[0055] In one embodiment, the polymer coating material is used as a negative electrode active material modifier in the negative electrode active material.

[0056] In a fourth aspect, an embodiment of the present application provides a modified negative electrode active material, which includes a negative electrode active material and a coating layer arranged on the surface of the negative electrode active material; the raw material of the coating layer is the polymer coating material described in the first aspect.

[0057] In one embodiment, the negative electrode active material includes a carbon-based material and / or a silicon-based material.

[0058] In one embodiment, the carbon-based material includes any one of graphite, carbon black, carbon nanotubes, carbon fibers, mesocarbon microbeads, and petroleum coke, or a combination of at least two thereof.

[0059] In one embodiment, the silicon-based material includes any one of nano-silicon, micro-silicon, porous silicon, amorphous silicon, and silicon oxide, or a combination of at least two thereof.

[0060] In one embodiment, based on the mass of the negative electrode active material as 100%, the mass of the polymer coating material is 1-10%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0061] In the embodiments of the present application, the mass of the polymer coating material is the total mass of the polymer and the conductive material, and the polymer is calculated based on the solid content and does not include any solvent / dispersant, etc.

[0062] As an optional technical solution of the embodiment of the present application, in the modified negative electrode active material, the mass of the polymer coating material is 1-10%, based on the mass of the negative electrode active material as 100%. The polymer coating material forms a uniform and stable polymer-conductive material hybrid coating layer on the surface of the negative electrode active material, which makes the modified negative electrode active material have good hydrophilicity, is easy to disperse evenly in the negative electrode slurry, shortens the slurry preparation time, and improves the wettability of the negative electrode electrode sheet to the electrolyte, shortens the liquid absorption time of the negative electrode electrode sheet, and improves the liquid absorption efficiency. At the same time, the formed polymer-conductive material hybrid coating layer can effectively inhibit the volume expansion of the negative electrode active material during cycling, significantly improves the structural stability and cycle performance of the material, and has good conductive properties. If the mass of the polymer coating material is too small, it will not form an effective coating and will not inhibit the volume expansion of the negative electrode active material. If the mass of the polymer coating material is too large, the thickness of the formed coating structure will be too high, which will increase the impedance of the modified negative electrode active material and deteriorate the conductivity and rate performance.

[0063] In one embodiment, the modified negative electrode active material is prepared by the following method, comprising: mixing the negative electrode active material with a polymer coating material dispersion to obtain a slurry; and drying the slurry to obtain the modified negative electrode active material.

[0064] In one embodiment, the solvent of the polymer coating material dispersion comprises water.

[0065] In one embodiment, the drying method is spray drying.

[0066] In one embodiment, the inlet temperature of the spray drying is 200-300°C, for example, it can be 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C or 290°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0067] In one embodiment, the outlet temperature of the spray drying is 100-200°C, for example, it can be 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or 190°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0068] In one embodiment, the spray drying pressure is 0.2-0.8 MPa, for example, it can be 0.25 MPa, 0.30 MPa, 0.35 MPa, 0.40 MPa, 0.45 MPa, 0.50 MPa, 0.55 MPa, 0.60 MPa, 0.65 MPa, 0.70 MPa or 0.75 MPa, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0069] In one embodiment, the feed rate of the slurry in the spray drying is 5-15 mL / min, for example, it can be 6 mL / min, 7 mL / min, 8 mL / min, 9 mL / min, 10 mL / min, 11 mL / min, 12 mL / min, 13 mL / min or 14 mL / min, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0070] As an optional technical solution of the embodiment of the present application, in the preparation process of the modified negative electrode active material, the negative electrode active material and the polymer coating material dispersion are first mixed evenly to obtain a slurry; the slurry is spray-dried, and the process is accompanied by high-temperature heat treatment (inlet temperature is 200-300°C, outlet temperature is 100-200°C), so that the hydroxyl group and the amino group / carboxyl group undergo a thermal cross-linking reaction, so that the coating layer on the surface of the modified negative electrode active material has hydrophilicity and also has good water resistance and coating stability based on the thermal cross-linking reaction. The coating layer will not fall off during the preparation process of the negative electrode slurry, and can play the role of improving hydrophilicity and inhibiting volume expansion in a long-lasting and stable manner.

[0071] In a fifth aspect, an embodiment of the present application provides a negative electrode material composition, which includes the modified negative electrode active material as described in the fourth aspect.

[0072] In one embodiment, the negative electrode material composition includes a modified negative electrode active material, a conductive agent, a binder, and optionally a thickener.

[0073] In one embodiment, based on 100 parts by mass of the modified negative electrode active material, the mass of the conductive agent is 0.1-5.0 parts, for example, it can be 0.1 parts, 0.3 parts, 0.5 parts, 0.7 parts, 0.9 parts, 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.5 parts, 2.8 parts, 3.0 parts, 3.2 parts, 3.5 parts, 3.8 parts, 4.0 parts, 4.2 parts, 4.5 parts or 4.8 parts, as well as specific point values ​​between the above points. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0074] In one embodiment, the binder includes styrene butadiene rubber (SBR).

[0075] In one embodiment, based on 100 parts by mass of the modified negative electrode active material, the mass of the binder is 0.1-5.0 parts, for example, it can be 0.1 parts, 0.3 parts, 0.5 parts, 0.7 parts, 0.9 parts, 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.5 parts, 2.8 parts, 3.0 parts, 3.2 parts, 3.5 parts, 3.8 parts, 4.0 parts, 4.2 parts, 4.5 parts or 4.8 parts, as well as specific point values ​​between the above points. Due to space limitations and for the sake of simplicity, the embodiments of the present application no longer exhaustively list the specific point values ​​included in the range.

[0076] In one embodiment, the thickening agent includes sodium carboxymethylcellulose (CMC).

[0077] In one embodiment, based on 100 parts by mass of the modified negative electrode active material, the mass of the thickener is 0.1-3.0 parts, for example, it can be 0.1 parts, 0.3 parts, 0.5 parts, 0.7 parts, 0.9 parts, 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.5 parts or 2.8 parts, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the embodiments of this application no longer exhaustively list the specific point values ​​included in the range.

[0078] In a sixth aspect, an embodiment of the present application provides a negative electrode plate, which includes a current collector and a coating disposed on the current collector, wherein the material of the coating includes the negative electrode material composition as described in the fifth aspect.

[0079] In the seventh aspect, an embodiment of the present application provides an electrochemical energy storage device, which includes at least one of the polymer coating material as described in the first aspect, the modified negative electrode active material as described in the fourth aspect, the negative electrode material composition as described in the fifth aspect, and the negative electrode plate as described in the sixth aspect.

[0080] In one embodiment, the electrochemical energy storage device includes any one of a lithium-ion battery, a sodium-ion battery, a supercapacitor, a fuel cell, or a solar cell, and a lithium-ion battery can be further selected.

[0081] This application has the following beneficial effects:

[0082] (1) The polymer coating material provided in the present application has excellent hydrophilicity and conductivity through the design of a polymer containing an active group and its compounding with a conductive material. It can be used as a modifier for negative electrode active materials. On the one hand, it improves the hydrophilicity of the negative electrode active material, improves its dispersion performance in the negative electrode slurry, shortens the slurrying time, improves the production efficiency of the negative electrode slurry, and improves the wettability and liquid absorption efficiency of the negative electrode plate to the electrolyte; on the other hand, the polymer coating material can form a stable and reliable coating layer on the surface of the negative electrode active material, effectively inhibits the volume expansion of the negative electrode active material, avoids the impedance degradation caused by the coating, and improves the conductive performance.

[0083] (2) In the modified negative electrode active material provided in the present application, the polymer coating material can form a stable polymer-conductive material hybrid coating layer on the surface of the negative electrode active material, so that the modified negative electrode active material has excellent hydrophilicity and dispersibility, cycle performance, conductivity and rate performance, thereby improving the production efficiency of lithium-ion batteries and improving the cycle performance of lithium-ion batteries.

[0084] (3) The present application designs and optimizes the components of the polymer coating material, so that the modified negative electrode active material can be used in negative electrode sheets and lithium-ion batteries. The negative electrode sheets have good wettability to the electrolyte, which significantly improves the liquid absorption efficiency of the negative electrode sheets and the production efficiency of the liquid injection process; at the same time, the coating layer on the surface of the negative electrode active material can effectively inhibit the volume expansion of the negative electrode active material without causing impedance degradation, so that the modified negative electrode active material has excellent cycle stability and conductivity, which significantly improves the cycle performance of the lithium-ion battery.

[0085] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION

[0086] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0087] As used herein, the terms "comprises," "including," "having," "containing" or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises a listed element is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0088] "Optionally" or "either" means that the subsequently described event or circumstance can or cannot occur, and that the description includes instances where the event occurs and instances where it does not.

[0089] The indefinite articles "a" and "an" before an element or component of the present application do not limit the quantity requirement (i.e., the number of times the element or component appears). Therefore, "a" or "an" should be interpreted as including one or at least one, and elements or components in the singular also include plural forms, unless the quantity clearly refers to only the singular form.

[0090] The terms "one embodiment," "some embodiments," "exemplarily," "specific examples," or "some examples" used herein mean that a specific feature, structure, material, or characteristic described in conjunction with the embodiment or example is included in at least one embodiment or example of the present application. In this document, the schematic descriptions of the above terms do not necessarily refer to the same embodiment or example.

[0091] Moreover, the technical features involved in each embodiment of the present application can be combined with each other as long as they do not conflict with each other.

[0092] In the following specific embodiments of the present application, the conductive materials and polymer monomers used are all commercially available products; the specific sources of the conductive materials are as follows:

[0093] Conductive carbon black (SP): brand: Arbon F-200GS, purchased from ASAHI CARBON CO LTD, Japan;

[0094] Polythiophene: brand Solar3, purchased from Shanghai Kaishefeng Industrial Co., Ltd.

[0095] Carbon fiber: brand VGCF-H, purchased from Showa Denko, Japan;

[0096] Carbon nanotubes: brand CN301C3, purchased from Kolon, South Korea;

[0097] Graphene: brand TA-001A, purchased from Shenzhen Turing Evolution Technology Co., Ltd.

[0098] Ketjen black: brand EC-300J, purchased from Lion of Japan.

[0099] Example 1

[0100] This embodiment provides a polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material.

[0101] Specifically, the polymer coating material includes a combination of conductive carbon black (SP) and a polymer, wherein the mass percentage of SP is 20%; the active groups of the polymer include a combination of cyano, hydroxyl, amino and carboxyl groups, and its polymerized monomers include, by mole percentage, 20% acrylonitrile, 40% hydroxyethyl acrylate, 15% acrylamide, and 25% acrylic acid.

[0102] The preparation method of the polymer coating material is as follows: 0.2 mol of acrylonitrile, 0.4 mol of hydroxyethyl acrylate, 0.15 mol of acrylamide, 0.25 mol of acrylic acid, ammonium persulfate (0.86 g, the mass of which is 1% of the total mass of the four monomers), SP (21.4 g, the mass of SP is 25% of the total mass of the four monomers) and 400 mL of deionized water are mixed evenly, and polymerization reaction is carried out at 85° C. for 5 hours to obtain the polymer coating material.

[0103] A modified negative electrode active material, comprising a negative electrode active material (artificial graphite) and a coating layer disposed on the surface of the negative electrode active material, wherein the raw material of the coating layer is the polymer coating material provided in this embodiment; the preparation method is as follows:

[0104] 5 parts by weight of polymer-coated material (based on solid content) was dispersed in 100 parts of water. 95 parts of artificial graphite was added while stirring at 1000 rpm and thoroughly mixed for 30 minutes to obtain a slurry. The slurry was spray-dried using the following parameters: inlet temperature of 250°C, outlet temperature of 150°C, feed rate of 10 mL / min, and air pressure of 0.5 MPa. After spraying, the collected particles constituted the modified negative electrode active material.

[0105] Example 2

[0106] This embodiment provides a polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material.

[0107] Specifically, the polymer coating material includes a combination of conductive carbon black (SP) and a polymer, wherein the mass percentage of SP is 25%; the active groups of the polymer include a combination of cyano, hydroxyl, amino and carboxyl groups, and its polymerized monomers include, by mole percentage, 20% acrylonitrile, 40% hydroxyethyl acrylate, 10% acrylamide, and 30% acrylic acid.

[0108] The preparation method of the polymer coating material comprises: uniformly mixing 0.2 mol of acrylonitrile, 0.4 mol of hydroxyethyl acrylate, 0.1 mol of acrylamide, 0.3 mol of acrylic acid, 0.86 g of ammonium persulfate (the mass of which is 1% of the total mass of the four monomers) and 400 mL of deionized water, and performing a polymerization reaction at 85° C. for 5 hours to obtain a polymer solution; and mixing the polymer solution with 28.6 g of SP so that the mass ratio of the polymer to the SP is 3:1, and uniformly mixing to obtain the polymer coating material.

[0109] A modified negative electrode active material, comprising a negative electrode active material (silicon dioxide) and a coating layer disposed on the surface of the negative electrode active material, wherein the raw material of the coating layer is the polymer coating material provided in this embodiment; the preparation method is as follows:

[0110] 5 parts by weight of polymer coating material (based on solid content) was dispersed in 100 parts of water. 95 parts of silicon oxide was added while stirring at 1000 rpm and thoroughly mixed for 30 minutes to obtain a slurry. The slurry was spray-dried using the following parameters: inlet temperature of 250°C, outlet temperature of 150°C, feed rate of 10 mL / min, and air pressure of 0.5 MPa. After spraying, the collected particles constituted the modified negative electrode active material.

[0111] Examples 3-15

[0112] A polymer coating material, a preparation method thereof, and a modified negative electrode active material using the polymer coating material. The only difference between these materials and Example 1 is the components and amounts of the polymer coating material, as shown in Table 1. "Content (%)" represents the mass percentage of the conductive material in the polymer coating material; "mol%" represents the molar percentage of the monomer in the polymerized monomer. The preparation methods for the polymer coating materials and the modified negative electrode active materials provided in Examples 3-15 are the same as those in Example 1.

[0113] Table 1

[0114] In Table 1, “--” represents that the component does not exist.

[0115] Comparative Example 1

[0116] This comparative example provides a polymer coating material, a preparation method thereof, and a modified negative electrode active material using the polymer coating material. The only difference between the polymer coating material and Example 1 is that the active group of the polymer does not contain a hydroxyl group, and the polymerized monomers thereof include, by mole percentage, 20% acrylonitrile, 40% ethyl acrylate, 15% acrylamide, and 25% acrylic acid. The other components, amounts, and preparation method of the polymer coating material are the same as those in Example 1.

[0117] A modified negative electrode active material, which differs from the modified negative electrode active material in Example 1 only in that the polymer coating material provided in this comparative example is used as the raw material of the coating layer; other components, amounts and preparation methods of the modified negative electrode active material are the same as those in Example 1.

[0118] Comparative Example 2

[0119] This comparative example provides a polymer coating material, a preparation method thereof, and a modified negative electrode active material using the polymer coating material. The only difference between the polymer coating material and Example 1 is that the active group of the polymer does not contain a cyano group, and the polymerized monomers thereof include, by mole percentage, 20% methyl acrylate, 40% hydroxyethyl acrylate, 15% acrylamide, and 25% acrylic acid. The other components, amounts, and preparation method of the polymer coating material are the same as those in Example 1.

[0120] A modified negative electrode active material, which differs from the modified negative electrode active material in Example 1 only in that the polymer coating material provided in this comparative example is used as the raw material of the coating layer; other components, amounts and preparation methods of the modified negative electrode active material are the same as those in Example 1.

[0121] Comparative Example 3

[0122] This comparative example provides a polymer coating material, a preparation method thereof, and a modified negative electrode active material using the polymer coating material. The only difference between the polymer coating material and Example 1 is that the active groups of the polymer do not contain carboxyl groups and amino groups, and the polymerized monomers thereof include, by mole percentage, 20% acrylonitrile, 40% hydroxyethyl acrylate, and 40% methyl acrylate. The other components, amounts, and preparation method of the polymer coating material are the same as those in Example 1.

[0123] A modified negative electrode active material, which differs from the modified negative electrode active material in Example 1 only in that the polymer coating material provided in this comparative example is used as the raw material of the coating layer; other components, amounts and preparation methods of the modified negative electrode active material are the same as those in Example 1.

[0124] Comparative Example 4

[0125] This comparative example is unmodified artificial graphite.

[0126] Comparative Example 5

[0127] This comparative example is unmodified silicon oxide.

[0128] Application Example 1-15, Comparative Application Example 1-5

[0129] A negative electrode plate comprises a current collector (Cu foil) and a coating disposed on the current collector, wherein the coating is made of a negative electrode material composition; the negative electrode material composition comprises a negative electrode active material, a conductive agent (conductive carbon black, SP), a binder (styrene-butadiene rubber, SBR), and a thickener (sodium carboxymethyl cellulose, CMC) in a mass ratio of 95:1.0:2.5:1.5; wherein the negative electrode active material is the modified negative electrode active material provided in Examples 1-15 and Comparative Examples 1-5, respectively.

[0130] Preparation of the negative electrode sheet: The negative electrode active material, SP, SBR and CMC were mixed in a mass ratio of 95:1.0:2.5:1.5, added to deionized water at a solid content of 40 wt%, and stirred thoroughly to prepare a uniform negative electrode slurry. After passing through a 100 mesh screen, the slurry was coated on the negative electrode current collector Cu foil, dried, and rolled with a roller at a speed of 10×10 4 The negative electrode sheet was obtained by rolling the negative electrode sheet with a unit length load of N / m.

[0131] A lithium-ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte, wherein the negative electrode sheet is the aforementioned negative electrode sheet; the preparation method of the lithium-ion battery is as follows:

[0132] (1) Preparation of positive electrode sheet: The positive electrode active material (lithium iron phosphate), conductive agent (conductive carbon black) and binder (polyvinylidene fluoride, PVDF) were mixed in a mass ratio of 95.5:2.0:2.5, added to NMP at a ratio of 50 wt% solid content, and stirred thoroughly to prepare a uniform positive electrode slurry. After passing through a 100 mesh sieve, the slurry was coated on the positive electrode current collector Al foil, dried, and rolled with a roller at 10 × 10 4 The positive electrode sheet is obtained by rolling the sample with a unit length load of N / m.

[0133] (2) Preparation of negative electrode sheet: as described above;

[0134] (3) Diaphragm: PE porous polymer film (Shenzhen Xingyuan Material Technology Co., Ltd.) was used as the diaphragm;

[0135] (4) Assembly of lithium-ion batteries: The positive electrode sheet, the separator, and the negative electrode sheet are wound in sequence to obtain a battery cell; the battery cell is encapsulated with an aluminum-plastic film, baked to remove water, and then injected with an electrolyte. After vacuum packaging, shelving, formation, secondary sealing, and shaping, the lithium-ion battery is obtained.

[0136] Performance testing:

[0137] (1) Fineness of negative electrode slurry

[0138] During the preparation of the negative electrode slurry, the fineness (μm) of the negative electrode active material after dispersion for 10 minutes was tested. The lower the fineness measured after 10 minutes, the better the dispersion performance of the negative electrode active material.

[0139] (2) Liquid absorption performance of the negative electrode

[0140] Add 1 mL of DMC electrolyte to the negative electrode to be tested. Start timing from the moment the DMC electrolyte contacts the electrode to the moment the electrolyte is completely absorbed by the electrode. Record the electrode absorption time, as shown in Table 2.

[0141] (3) Normal temperature cycle performance

[0142] The lithium-ion battery prepared above was charged to 4.2V at a constant current of 0.33C, then charged at a constant voltage to a cutoff current of 0.02C, and discharged at 0.33C to 2.5V; left for 5 minutes, charged to 4.2V at a constant current of 0.33C, then charged at a constant voltage to a cutoff current of 0.02C, and discharged at 0.33C to 2.5V, thus performing initial adjustment.

[0143] At 25°C, charge the initially conditioned lithium-ion battery at a constant current of 0.5C to 4.2V, then charge at a constant voltage to a cutoff current of 0.02C, rest for 5 minutes, and then discharge at a constant current of 1C to 2.5V, rest for 5 minutes. Measure the discharge capacity of the first cycle. Repeat this charge / discharge cycle for 100 cycles, measure the discharge capacity of the 100th cycle, and calculate the capacity retention rate at the 100th cycle using the following formula:

[0144] Capacity retention rate after 100 cycles (%) = 100% × 100th cycle discharge capacity / first cycle discharge capacity.

[0145] (4) Rate performance

[0146] At 25°C, charge the initially conditioned lithium-ion battery at a constant current of 0.5C to 4.2V, then charge it at a constant voltage to a cutoff current of 0.02C, let it rest for 5 minutes, then discharge it at a constant current of 1C to 2.5V, let it rest for 5 minutes, and measure the 1C discharge capacity. Then charge it at a constant current of 0.5C to 4.2V, then charge it at a constant voltage to a cutoff current of 0.02C, let it rest for 5 minutes, then discharge it at a constant current of 3C to 2.5V, let it rest for 5 minutes, and measure the discharge capacity at a 3C rate. 3C capacity retention (%) = 100% × 3C discharge capacity / 1C discharge capacity.

[0147] The test results are shown in Table 2.

[0148] Table 2

[0149] Combined with the performance test data in Table 2, it can be seen that compared with the negative electrode sheets and lithium-ion batteries prepared using conventional negative electrode active materials in Comparative Examples 4 and 5 (Comparative Example 4: artificial graphite; Comparative Example 5: silicon dioxide), the polymer coating material provided in Examples 1-7 of the present application is used as a negative electrode active material modifier, so that the prepared modified negative electrode active material has good hydrophilicity and dispersibility, and a fineness of 20-22 μm can be achieved after dispersion for 10 minutes, which can shorten the slurrying time, improve the wettability and liquid absorption efficiency of the negative electrode sheet to the electrolyte, and make the liquid absorption time 21-32 seconds. At the same time, the volume expansion of the negative electrode active material in the modified negative electrode active material is effectively suppressed, and while having excellent structural stability and cycle performance, the conductivity and rate performance of the material can also be improved. The capacity retention rate of the lithium-ion battery containing the carbon-based modified negative electrode active material (artificial graphite, Examples 1, 3-7) after 100 cycles at room temperature is ≥96.1%, and the 3C rate performance is ≥85.0%; the capacity retention rate of the lithium-ion battery containing the silicon-based modified negative electrode active material (silicon dioxide, Example 2) after 100 cycles at room temperature is ≥90%, and the 3C rate performance is ≥82.0%.

[0150] In the present application, by designing a polymer containing an active group and compounding it with a conductive material, the polymer coating material is coated on the surface of the negative electrode active material to form a stable polymer-conductive material hybrid coating layer, so that the modified negative electrode active material has good hydrophilicity and dispersibility. At the same time, the introduction of cyano groups makes the polymer and the negative electrode active material have good adhesion, and the hydroxyl group can undergo a thermal cross-linking reaction with the amino group and / or carboxyl group to form a stable coating layer with good water resistance on the surface of the negative electrode active material, which inhibits the volume expansion of the negative electrode active material during the charge and discharge process, and the coating layer will not fall off during the slurry preparation; at the same time, since the coating layer contains a conductive material, the impedance degradation caused by the coating is avoided, so that the modified negative electrode active material has excellent cycle performance, conductivity and rate performance. Combined with the effect data of Examples 1-15, it can be seen that by adjusting the component ratio of the conductive material and the polymer and the type and ratio of the active groups in the polymer, the cycle performance and rate performance of the modified negative electrode active material and the lithium ion battery containing it can be controlled and optimized. If the proportion of cyano groups in the polymer is too low (Example 8), the adhesion between the polymer and the negative electrode active material is reduced, the stability of the coating layer is insufficient, and the cycle performance is affected; if the proportion of cyano groups in the polymer is too high (Example 9), the hydrophilicity of the modified negative electrode active material is affected, resulting in a prolonged liquid absorption time of the negative electrode sheet. If the proportion of hydroxyl groups in the polymer is too high and the proportion of carboxyl and amino groups, which are strong hydrophilic groups, is too low (Example 10), or if the proportion of hydroxyl groups in the polymer is too low and the proportion of carboxyl and amino groups, which are strong hydrophilic groups, is too high (Example 11), the cross-linking of hydroxyl groups with carboxyl and amino groups during coating is insufficient, and partial detachment of the coating layer occurs during the preparation of the negative electrode slurry, affecting the cycle performance. If the amount of conductive material used is small (Example 14), the improvement effect on the conductive properties of the modified negative electrode active material is not obvious, resulting in a slightly lower rate performance of the battery; if the amount of conductive material used is too much (Example 15), it will affect the coating effect of the coating layer on the negative electrode active material and the inhibitory effect on the volume expansion of the negative electrode active material, resulting in a decrease in cycle performance.

[0151] The polymer of Comparative Example 1 does not contain hydroxyl groups, and the polymer of Comparative Example 3 does not contain carboxyl groups and amino groups, resulting in insufficient hydrophilicity of the modified negative electrode active material, slow liquid absorption rate of the negative electrode plate, and inability of the polymer coating material to undergo thermal cross-linking, resulting in low stability of the coating layer, which falls off during the preparation of the negative electrode slurry, and therefore cannot suppress volume expansion and pulverization, resulting in poor cycle performance; the polymer of Comparative Example 2 does not contain cyano groups, and although the hydrophilicity of the modified negative electrode active material is acceptable, due to insufficient adhesion between the polymer and the negative electrode active material, the coating layer is unstable and the cycle performance is poor.

[0152] The applicant declares that this application uses the above-mentioned embodiments to illustrate the polymer coating material, its preparation method, and application. However, this application is not limited to the above-mentioned embodiments, which does not mean that this application must rely on the above-mentioned embodiments in order to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent replacements for various raw materials in the product of this application, addition of auxiliary components, and selection of specific methods, etc., fall within the scope of protection and disclosure of this application.

Claims

1. A polymer coating material, comprising a combination of a polymer and a conductive material; the polymer contains active groups, the active groups comprising a combination of cyano, hydroxyl and strong hydrophilic groups, the strong hydrophilic groups comprising amino and / or carboxyl groups.

2. The polymer coating material according to claim 1, wherein The polymer is coated on the surface of the conductive material; Optionally, the mass percentage of the conductive material in the polymer coating material is 1-60%; Optionally, the conductive material includes any one of polythiophene, polypyrrole, polyaniline, carbon black, carbon nanotubes, carbon fibers, graphene, graphite, Ketjen black, and acetylene black, or a combination of at least two thereof.

3. The polymer coating material according to claim 1 or 2, wherein: The active groups include a combination of cyano, hydroxyl, amino and carboxyl groups; Optionally, the molar percentage of cyano groups in the active groups is 1-50%; Optionally, the molar percentage of hydroxyl groups in the active groups is 1-50%; Optionally, the molar percentage of amino groups in the active groups is 1-20%; Optionally, the molar percentage of carboxyl groups in the active groups is 1-40%.

4. The polymer coating material according to any one of claims 1 to 3, wherein: The polymerizable monomers of the polymer include a combination of alkenyl nitrile monomers, hydroxyl-containing acrylate monomers, acrylamide monomers and alkenyl carboxylic acid monomers; Optionally, the polymerizable monomers include the following components in terms of molar percentage: 1-50% of alkenyl nitrile monomers, 1-50% of hydroxyl-containing acrylate monomers, 1-20% of acrylamide monomers, and 1-40% of alkenyl carboxylic acid monomers; Optionally, the alkenyl nitrile monomer includes any one of acrylonitrile, methacrylonitrile, and crotononitrile, or a combination of at least two thereof; Optionally, the hydroxyl-containing acrylic ester monomers include hydroxyethyl acrylate, hydroxyethyl methacrylate, Any one of ester, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, or a combination of at least two thereof; Optionally, the acrylamide monomers include acrylamide and / or methacrylamide; Optionally, the alkenyl carboxylic acid monomer includes any one of acrylic acid, methacrylic acid, and crotonic acid, or a combination of at least two of them.

5. A method for preparing the polymer coating material according to any one of claims 1 to 4, wherein the preparation method comprises method A or method B; The method A comprises: mixing a polymer solution with a conductive material to obtain the polymer coating material; The method B comprises: mixing a polymer monomer solution of a polymer with a conductive material and then performing a polymerization reaction to obtain the polymer coating material.

6. A modified negative electrode active material, comprising a negative electrode active material and a coating layer disposed on the surface of the negative electrode active material; the raw material of the coating layer is the polymer coating material according to any one of claims 1 to 4; Optionally, the negative electrode active material includes a carbon-based material and / or a silicon-based material; Optionally, the carbon-based material includes any one of graphite, carbon black, carbon nanotubes, carbon fibers, mesocarbon microbeads, and petroleum coke, or a combination of at least two thereof; Optionally, the silicon-based material includes any one of nano silicon, micro silicon, porous silicon, amorphous silicon, silicon oxide, or a combination of at least two thereof; Optionally, based on 100% of the mass of the negative electrode active material, the mass of the polymer coating material is 1-10%.

7. The modified negative electrode active material according to claim 6, wherein The modified negative electrode active material is prepared by the following method, which includes: mixing the negative electrode active material with a polymer coating material dispersion to obtain a slurry; drying the slurry to obtain the modified negative electrode active material; Optionally, the drying method is spray drying; Optionally, the inlet temperature of the spray drying is 200-300°C; Optionally, the outlet temperature of the spray drying is 100-200°C; Optionally, the spray drying pressure is 0.2-0.8 MPa; Optionally, the feed rate of the slurry in the spray drying is 5-15 mL / min.

8. A negative electrode material composition, comprising the modified negative electrode active material according to claim 6 or 7; Optionally, the negative electrode material composition comprises a combination of a modified negative electrode active material, a conductive agent, a binder and optionally a thickener. 9 . A negative electrode plate, comprising a current collector and a coating disposed on the current collector, wherein a material of the coating comprises the negative electrode material composition according to claim 8 .

10. An electrochemical energy storage device, comprising at least one of the polymer coating material according to any one of claims 1 to 4, the modified negative electrode active material according to claim 6 or 7, the negative electrode material composition according to claim 8, and the negative electrode sheet according to claim 9; Optionally, the electrochemical energy storage device includes any one of a lithium-ion battery, a sodium-ion battery, a supercapacitor, a fuel cell or a solar cell, and a lithium-ion battery may further be selected.

Citation Information

Patent Citations

  • Modified composite material containing silicon-base material, preparation method thereof, and application thereof in lithium ion battery

    CN109301184A

  • Binder, negative pole piece and electrochemical device

    CN110233235A

  • Lithium ion battery

    CN114094165A

  • Binder composition for secondary battery

    CN114342125A

  • Binder composition for non-aqueous electrolyte secondary battery, slurry for secondary battery negative electrode, negative electrode for secondary battery, and secondary battery

    JP2020184414A

Cited By

  • Negative electrode, preparation method thereof and battery

    CN119725379A

  • Semi-conductive adhesive for cable semi-conductive shielding tape and preparation method of semi-conductive adhesive