Additive, electrolyte comprising same, and lithium ion battery
By using [3-(N,N-dimethylamino)propyl]trimethoxysilane and sulfonylsilane compounds as electrolyte additives in lithium-ion batteries, a stable interface film is formed, which solves the problem of high-temperature cycling of lithium-ion batteries. and the problem of reduced storage performance, taking into account low-temperature performance and rate performance, and avoiding the carcinogenic risks of traditional additives.
Patent Information
- Application Number
- PCT/CN2023/127352
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-10-27
- Publication Date
- 2024-10-31
AI Technical Summary
The cycle performance and storage performance of existing lithium-ion batteries decrease at high temperatures, and commonly used additives are detrimental to low-temperature performance and rate performance, and some carcinogenic chemicals are harmful to environmental protection and human health.
[3-(N,N-Dimethylamino)propyl]trimethoxysilane and sulfonylsilane compounds are used as electrolyte additives to form a stable interface film to capture H2O, PF5 and HF, reduce positive electrode corrosion, and improve High temperature performance, taking into account both low temperature performance and rate performance.
It effectively reduces the corrosion of the positive electrode by HF, inhibits the high-temperature gas production of the battery, improves the high-temperature storage and cycle performance, and improves the low-temperature performance and rate performance.
Smart Images

Figure CN2023127352_31102024_PF_FP_ABST
Abstract
Description
An additive, an electrolyte containing the same, and a lithium-ion battery
[0001] This application is based on the Chinese application with CN application number 202310478312.2 and application date April 28, 2023, and claims its priority. The disclosed content of the CN application is again introduced as a whole into this application. Technical Field
[0002] The present invention relates to the technical field of lithium ion batteries, and in particular to an additive, an electrolyte containing the additive, and a lithium ion battery. Background Art
[0003] Lithium-ion secondary batteries, with their advantages such as high operating voltage, long cycle life, and fast charge and discharge speeds, have gradually established a broad market and play a vital role in small electronic products such as mobile phones, computers, and power tools. However, with the continuous development of electronic products, the market is placing higher demands on the range of power tools. Currently, increasing the operating voltage and improving the nickel content are two common methods to improve the range of power tools.
[0004] However, during battery operation, side reactions between the electrolyte and the negative electrode surface can easily cause battery bloating. Water reacts with lithium salts in the electrolyte to generate HF, which corrodes the positive electrode, leading to a decrease in the battery's high-temperature cycling and storage performance. Prior art uses additives to suppress gas production in battery cells. However, while conventional sulfur-containing additives such as 1,3-propane sultone (PS) and methylene methanedisulfonate (MMDS) have some effect, these additives are not conducive to improving the battery's low-temperature performance and rate capability. Furthermore, PS is a carcinogenic chemical, which is environmentally unfriendly and poses significant risks to human health.
[0005] Summary of the Invention
[0006] The main purpose of the present invention is to provide an additive, an electrolyte containing the additive and a lithium ion battery, so as to solve the problem in the prior art that the battery cannot have both low temperature performance and rate performance.
[0007] To achieve the above object, according to one aspect of the present invention, an additive is provided, which includes [3-(N,N-dimethylamino)propyl]trimethoxysilane and a sulfonylsilane compound, wherein the sulfonylsilane compound has a structure shown in formula (I):
[0008] Among them, R1 represents F, C1~C 20 Straight or branched alkyl, C1~C 20 Alkyl substituted amino, substituted or unsubstituted C6~C 20Aryl, cyano, F-substituted C1~C 20 Any one of the straight-chain or branched-chain alkyl groups;
[0009] R2 represents a substituted or unsubstituted imidazole group, C1 to C 20 Straight or branched chain alkyl, F-substituted C1~C 20 Straight or branched alkyl, C1~C 20 Alkoxy, C2~C 20 Carboxylate group, F substituted C2~C 20 Carboxylate group, C4~C 20 Heteroaryl, C2~C 20 Any one of the diethylene glycol groups;
[0010] R3, R4, and R5 each independently represent H, F, Cl-C 20 Straight or branched chain alkyl, F-substituted C1~C 20 Straight chain or branched alkyl, substituted or unsubstituted C6~C 20 Any one of the aryl groups.
[0011] Furthermore, R1 represents F, a primary amino group, a tertiary amino group, a C1-C 10 Any one of the straight-chain or branched alkyl groups; R2 represents a C4-C6 heteroaryl, a C1-C 10 Straight or branched alkyl, F-substituted C2~C 10 Carboxylate group, C2~C 20 R3, R4, R5 each independently represent a C1 to C6 straight chain or branched alkyl group, an unsubstituted C6 to C 20 Any one of the aryl groups.
[0012] Furthermore, R1 represents any one of F, primary amino group, tertiary amino group, and trifluoromethyl group; R2 represents any one of imidazole group, ethyl group, difluoroacetate group, and diethylene glycol group; R3, R4, and R5 each independently represent any one of methyl group, ethyl group, isopropyl group, and phenyl group.
[0013] Furthermore, the sulfonylsilane compound is selected from one or more of the following structures:
[0014] Furthermore, the sulfonylsilane compound is selected from combination of combination of combination of combination of Any combination of .
[0015] In order to achieve the above-mentioned object, according to one aspect of the present invention, an electrolyte is provided, which includes a lithium salt, an electrolyte additive and a solvent, and the electrolyte additive includes the above-mentioned additive provided in this application.
[0016] Furthermore, the concentration of lithium salt in the electrolyte is 0.5 to 1.5 M; and the additive is 0.1 to 5 wt % of the electrolyte weight.
[0017] Furthermore, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium dioxalatoborate, lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide.
[0018] Furthermore, the solvent includes one or more of chain and cyclic carbonates and carboxylates.
[0019] Furthermore, the electrolyte further comprises a functional additive, and the functional additive accounts for 0.2 to 10 wt % of the electrolyte.
[0020] Furthermore, the functional additives include at least one of a circulation additive, a low-temperature additive, a high-temperature additive, a flame retardant additive, and an anti-overcharge additive.
[0021] According to another aspect of the present invention, a lithium-ion battery is provided, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the electrolyte comprises the above-mentioned electrolyte provided in the present application.
[0022] Applying the technical solution of the present invention, the additive of the present application includes both silane groups and sulfonyl groups. The silane group can capture H2O, PF5 and HF from the electrolyte, reducing damage to the positive electrode structure, and the sulfonyl group can form a dense and thinner interface film. The additive of the present application can have a lower HOMO and a higher LUMO, and can preferentially oxidize and reduce on the surface of the positive and negative electrodes to form a stable interface film, effectively isolating the electrolyte and the positive and negative electrodes, avoiding oxidation reactions between the electrolyte and the positive and negative electrodes, reducing the generation of HF, thereby reducing HF corrosion of the positive electrode, and inhibiting the gas production of the battery at high temperature, thereby improving the high-temperature storage and high-temperature cycle performance of the battery. At the same time, the interface film formed is dense and rich in inorganic substances, which can take into account both low-temperature performance and rate performance. DETAILED DESCRIPTION
[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the embodiments.
[0024] As analyzed in the background technology, however, due to the side reaction between the electrolyte and the surface of the negative electrode during the operation of the battery, it is easy to cause the battery to swell, and the reaction of water with the lithium salt in the electrolyte will also generate HF to corrode the positive electrode, thereby causing the high-temperature cycle performance and high-temperature storage performance of the battery to decrease. In the prior art, additives are used to suppress the gas production of battery cells. However, although conventional sulfur-containing additives such as 1,3-propane sultone (PS) and methylene disulfonate (MMDS) have certain effects, the above additives are not conducive to improving the low-temperature performance and rate performance of the battery, and PS is a carcinogenic chemical, which is not conducive to environmental protection and has great harm to human health. In order to solve the above problems, the present application provides an additive, an electrolyte comprising the same, and a lithium-ion battery.
[0025] In a typical embodiment of the present application, an additive is provided, which includes [3-(N,N-dimethylamino)propyl]trimethoxysilane and a sulfonylsilane compound, wherein the sulfonylsilane compound has a structure shown in formula (I):
[0026] Among them, R1 represents F, C1~C 20 Straight or branched alkyl, C1~C 20 Alkyl substituted amino, substituted or unsubstituted C6~C 20 Aryl, C1~C 20 Alkyl-substituted cyano, F-substituted C1~C 20 Any one of the straight-chain or branched alkyl groups; R2 represents a substituted or unsubstituted imidazole group, a C1-C 20 Straight or branched chain alkyl, F-substituted C1~C 20 Straight or branched alkyl, C1~C 20 Alkoxy, C2~C 20 Carboxylate group, F substituted C2~C 20 Carboxylate group, C4~C 20 Heteroaryl, C2~C 20 Any one of the diethylene glycol groups; R3, R4, R5 each independently represent H, F, C1~C 20 Straight or branched chain alkyl, F-substituted C1~C 20 Straight chain or branched alkyl, substituted or unsubstituted C6~C 20 Any one of the aryl groups.
[0027] The additives of the present application include [3-(N,N-dimethylamino)propyl]trimethoxysilane and sulfonylsilane compounds. [3-(N,N-dimethylamino)propyl]trimethoxysilane is easier to oxidize than the solvent to form CEI, and is also easier to reduce to form SEI, which is beneficial to reduce the corrosion of HF on the positive electrode. Sulfonylsilane compounds include both silane and sulfonyl groups. The silane group can capture H2O, PF5 and HF from the electrolyte to reduce damage to the positive electrode structure, and the sulfonyl group can form a denser and thinner interface film. The additives of the present application can have a lower HOMO and a higher LUMO, and can preferentially oxidize and reduce on the surface of the positive and negative electrodes to form a stable interface film, effectively isolating the electrolyte and the positive and negative electrodes, avoiding oxidation reactions between the electrolyte and the positive and negative electrodes, reducing the generation of HF, thereby reducing the corrosion of HF on the positive electrode, and inhibiting the gas production of the battery at high temperature, thereby improving the high-temperature storage and high-temperature cycle performance of the battery. At the same time, the interface film formed is dense and rich in inorganic substances, which can take into account both low-temperature performance and rate performance.
[0028] In order to further suppress the gas generation of the battery cell, in some embodiments, R1 represents F, a primary amine group, a tertiary amine group, a C1-C 10 Any one of the straight-chain or branched alkyl groups; R2 represents a C4-C6 heteroaryl, a C1-C 10 Straight or branched alkyl, F-substituted C2~C 10 Carboxylate group, C2~C 20 R3, R4, R5 each independently represent a C1 to C6 straight chain or branched alkyl group, an unsubstituted C6 to C 20 Any one of the aryl groups.
[0029] In order to further improve the high-temperature storage and high-temperature cycle performance of the battery while taking into account the low-temperature performance and rate performance, R1 represents any one of F, primary amino group, tertiary amino group, and trifluoromethyl group; R2 represents any one of imidazole group, ethyl group, difluoroacetate group, and diethylene glycol group; R3, R4, and R5 each independently represent any one of methyl group, ethyl group, isopropyl group, and phenyl group.
[0030] In some embodiments, the additive is selected from one or more of the following structures:
[0031] In order to further improve the high temperature storage and high temperature cycle performance of the battery while taking into account the low temperature performance and rate performance, in some embodiments, the above additives are selected from combination of combination of combination of combination of Any combination of .
[0032] In another typical embodiment of the present application, an electrolyte is provided. The electrolyte includes a lithium salt, an additive, and a solvent. The electrolyte additive includes the above-mentioned additive.
[0033] When the electrolyte including the above additives is used in a battery, it has good high-temperature storage performance and high-temperature cycle performance, while taking into account low-temperature performance and rate performance.
[0034] In order to improve the conductivity of the electrolyte and avoid an increase in electrolyte viscosity due to an excessively high lithium salt concentration, in some embodiments, the lithium salt concentration in the electrolyte is 0.5 to 1.5 M; for example, it can be 0.5 M, 0.75 M, 1 M, 1.25 M, or 1.5 M.
[0035] In some embodiments, the additive comprises 0.1 to 5 wt % of the electrolyte. If the additive content is too high, the film will be too thick, affecting the capacity and rate capability, while also increasing the cost. If the additive content is too low, the interface film cannot be formed on the positive and negative electrode surfaces of the battery, thereby affecting the high-temperature cycling performance and high-temperature storage performance of the battery.
[0036] The present application does not particularly limit the type of lithium salt, and any lithium salt commonly used in the art can be applied to the present application. In some embodiments, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium difluorooxalatophosphate (LiODFP), lithium bis(fluorosulfonyl imide) (LiFSI), and lithium bis(trifluoromethylsulfonyl imide) (LiTFSI).
[0037] The present application has no particular restrictions on the type of solvent, and all commonly used solvents in the art can be applied to the present application. In order to improve the solubility of additives and lithium salts, in some embodiments, the solvent includes one or more of chain and cyclic carbonates and carboxylates. Cyclic carbonate solvents include but are not limited to ethylene carbonate (EC), fluoroethylene carbonate (FEC), and propylene carbonate (PC); chain carbonate solvents include but are not limited to dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC); carboxylate solvents include but are not limited to propyl acetate (PA), ethyl acetate (EA), and propyl propionate (PP).
[0038] In some embodiments, functional additives may be added to the electrolyte according to product requirements. The functional additives include at least one of a recycling additive, a low-temperature additive, a high-temperature additive, a flame retardant additive, and an overcharge prevention additive. The functional additives may be present in an amount of 0.2 to 10 wt % of the electrolyte.
[0039] In some embodiments, the functional additive includes at least one of fluoroethylene carbonate, vinyl sulfate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphate, tris(pentafluorophenyl)borane, lithium difluorophosphate, 3-hexylthiophene, hexafluorocyclotriphosphazene, and tris(hexafluoroisopropyl)phosphate.
[0040] In another typical embodiment of the present application, a lithium-ion battery is provided, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the electrolyte comprises the above-mentioned electrolyte.
[0041] The lithium-ion battery comprising the above electrolyte has good high-temperature storage performance and high-temperature cycle performance, while taking into account both low-temperature performance and rate performance.
[0042] The positive electrode active material in the positive electrode can be selected from LiNi 1-x-y-z Co x Mn y Al z One of O2, lithium nickel manganese oxide, lithium cobalt oxide, lithium-rich manganese-based solid solution, lithium manganese oxide or lithium iron phosphate, wherein 0≤x≤1, 0≤y≤1, 0≤z≤1, and 0≤x+y+z≤1.
[0043] The negative electrode active material of the negative electrode can be selected from artificial graphite, coated natural graphite, silicon-carbon negative electrode, silicon negative electrode or lithium titanate.
[0044] The present application is further described in detail below with reference to specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application.
[0045] The compounds used in the examples of this application are shown in Table 1.
[0046] Table 1
[0047] Example 1
[0048] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:DEC:EMC=1:1:2, and 1M lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, and then 0.5% of compound 1 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0049] Example 2
[0050] Ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of EC:PC:DEC:EMC=1:1:1:2, and 0.8M lithium hexafluorophosphate (LiPF6) and 0.2M lithium bis(fluorosulfonyl)imide (LiFSI) were added. After the lithium salt was completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, 3% compound 1 and [3-(N,N-dimethylamino)propyl]trimethoxysilane were added to obtain an electrolyte.
[0051] Example 3
[0052] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a mass ratio of EC:DEC:EMC=1:2:1, and after mixing, 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added. After the lithium salt was completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, 0.5% compound 2 and [3-(N,N-dimethylamino)propyl]trimethoxysilane were added to obtain an electrolyte.
[0053] Example 4
[0054] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a mass ratio of EC:DEC:EMC=1:2:1, and after mixing, 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) were added. After the lithium salt was completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, and then 0.5% compound 3 and [3-(N,N-dimethylamino)propyl]trimethoxysilane were added to obtain an electrolyte.
[0055] Example 5
[0056] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of EC:DEC:EMC=1:1:2, and 1M lithium hexafluorophosphate (LiPF6) was added after mixing. After the lithium salt was completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, and 0.5% compound 4 and [3-(N,N-dimethylamino)propyl]trimethoxysilane were added to obtain an electrolyte.
[0057] Example 6
[0058] Ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:PC:DEC:EMC=1:1:1, and after mixing, 0.7M lithium hexafluorophosphate (LiPF6) and 0.3M lithium bis(fluorosulfonyl)imide (LiFSI) are added. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, 0.3% 3-hexylthiophene, 0.5% compound 1, 3% compound 4 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0059] Example 7
[0060] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:DEC:EMC=1:1:1, and after mixing, 0.8M lithium hexafluorophosphate (LiPF6) and 0.2M lithium difluorooxalatoborate (LiODFB) are added. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, 0.3% 3-hexylthiophene, 0.5% compound 2, 2% compound 3 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0061] Example 8
[0062] Ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and propyl propionate (PP) are mixed in a mass ratio of EC:DEC:EMC:PP=1:1:1:1, and 1M lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, 0.3% 3-hexylthiophene, 1% compound 2, 2.5% compound 4 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0063] Example 9
[0064] Ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and propyl propionate (PP) are mixed in a mass ratio of EC:DEC:EMC:PP=1:1:1:1, and 1M lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, 0.3% 3-hexylthiophene, 0.5% compound 1, 1.5% compound 3, 0.8% compound 4, and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0065] Example 10
[0066] Ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and propyl propionate (PP) are mixed in a mass ratio of EC:DEC:EMC:PP=1:1:1:1, and 1M lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, 0.3% 3-hexylthiophene, 1% compound 2, 0.6% compound 3, 1.5% compound 4, and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0067] Example 11
[0068] Ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:PC:DEC:EMC=1:1:1, and after mixing, 0.7 mol of lithium hexafluorophosphate (LiPF6) and 0.3 mol of lithium bis(fluorosulfonyl)imide (LiFSI) are added. After the lithium salt is completely dissolved, 1% of lithium difluorophosphate, 3% of fluoroethylene carbonate, 1% of vinyl sulfate, 2% of hexafluorocyclotriphosphazene, 0.3% of 3-hexylthiophene, 0.5% of compound 1, 3% of compound 2 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0069] Example 12
[0070] Ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:PC:DEC:EMC=1:1:1, and after mixing, 0.7 mol of lithium hexafluorophosphate (LiPF6) and 0.3 mol of lithium bis(fluorosulfonyl)imide (LiFSI) are added. After the lithium salt is completely dissolved, 1% of lithium difluorophosphate, 3% of fluoroethylene carbonate, 1% of vinyl sulfate, 2% of hexafluorocyclotriphosphazene, 0.3% of 3-hexylthiophene, 0.5% of compound 1, 3% of compound 3 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0071] Example 13
[0072] Ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and propyl propionate (PP) are mixed in a mass ratio of EC:DEC:EMC:PP=1:1:1:1, and 1 mol of lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 1% of lithium difluorophosphate, 3% of fluoroethylene carbonate, 1% of vinyl sulfate, 2% of hexafluorocyclotriphosphazene, 0.3% of 3-hexylthiophene, 0.5% of compound 1, 1.5% of compound 2, 0.8% of compound 3 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0073] Example 14
[0074] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:DEC:EMC=1:1:2, and 1M lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, and then 4% of compound 1 and [3-(N,N-dimethylamino)propyl]trimethoxysilane are added to obtain an electrolyte.
[0075] Comparative Example 1
[0076] The difference from Example 1 is that Compound 1 is not contained. The remaining raw materials and preparation methods are the same as those in Example 1.
[0077] Comparative Example 2
[0078] The difference from Example 6 is that it does not contain Compound 1 and Compound 4. The remaining raw materials and preparation methods are the same as those in Example 6.
[0079] Comparative Example 3
[0080] The difference from Example 9 is that it does not contain Compound 1, 3 and Compound 4. The remaining raw materials and preparation methods are the same as those of Example 9.
[0081] Comparative Example 4
[0082] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:DEC:EMC=1:1:2, and 1 mol of lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 1% lithium difluorophosphate, 3% fluoroethylene carbonate, 1% vinyl sulfate, 2% hexafluorocyclotriphosphazene, and 0.5% MMDS are added to obtain an electrolyte.
[0083] Comparative Example 5
[0084] The difference from Example 1 is that [3-(N,N-dimethylamino)propyl]trimethoxysilane is not contained.
[0085] Preparation of positive electrode: ternary material LiNi0 0.7 C0 0.1 Mn 0.2 The conductive agent Super P, the adhesive PVDF and the carbon nanotube (CNT) are mixed evenly in a mass ratio of 97.2:1.8:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for the current collector. The coating amount is 340g / m 2 , dried at 85°C and then cold pressed; then striped and sliced, and then baked at 85°C in vacuum for 4 hours to make lithium-ion battery positive electrodes that meet the requirements.
[0086] Preparation of negative electrode sheet: Artificial graphite is mixed with conductive agent Super P, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) in a mass ratio of 94.5:1.5:1.5:2.5 to form a slurry, which is then mixed evenly. The mixed slurry is then coated on both sides of the copper foil, dried, and rolled to obtain the negative electrode sheet, which is then baked at 85°C in a vacuum for 4 hours to produce a lithium-ion battery negative electrode sheet that meets the requirements.
[0087] Preparation of lithium-ion batteries: The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are laminated to form a lithium-ion battery with a thickness of 0.5 mm, a width of 5 mm and a length of 8 mm, and a capacity of 3 Ah. The battery is vacuum-baked at 85°C for 48 hours and the electrolyte of the above embodiments and comparative examples is injected to complete the battery production.
[0088] The electrical performance of the 3Ah soft-pack lithium-ion batteries assembled in Examples 1 to 15 and Comparative Examples 1 to 4 was tested. The specific testing method is as follows:
[0089] (1) Initial DC resistance (DCR) test
[0090] After capacity separation, the experimental batteries of Examples 1 to 15 and Comparative Examples 1 to 4 were each charged to a state of charge (SOC) of 50%. After resting for 30 minutes, the sampled voltage V0 at the start of discharge was recorded. Subsequently, the experimental batteries were discharged at a current of 3C for 10 seconds, and the sampled voltage V1 at the end of discharge was recorded. The initial DC discharge resistance DCR of the experimental batteries was calculated as (V1-V0) / I.
[0091] (2) Cycle performance test
[0092] Under 45°C test conditions, the experimental batteries in Examples 1 to 15 and Comparative Examples 1 to 4 were subjected to charge and discharge cycle performance tests at a charge and discharge rate of 1C. The charge and discharge voltage range was set to 2.8-4.25V. The high-temperature cycle was repeated for 800 cycles, and the DCR was measured every 100 cycles. The capacity retention rate and DCR growth rate were recorded.
[0093] (3) High temperature shelf test
[0094] The experimental battery was charged and discharged at a rate of 0.33C for 3 weeks at room temperature, and the average discharge capacity was taken as C1. It was then charged to 100% SOC, placed at 60°C for 7 days, and placed at room temperature for 6 hours. It was discharged at a rate of 0.33C, and the discharge capacity was taken as C2. It was then charged and discharged for another 3 weeks, and the average discharge capacity was taken as C3. C2 divided by C1 is the capacity retention rate, and C3 divided by C1 is the capacity recovery rate.
[0095] (4) Low temperature test
[0096] The experimental battery was charged and discharged at a rate of 1C for 3 weeks at room temperature, and the average value was taken as C1. It was then charged to 100% SOC, placed at -20℃ for 10h, and discharged at 1C to 2.8V. The discharge capacity was recorded as C2. C1 divided by C2 is the low-temperature discharge retention rate.
[0097] (5) Rate test
[0098] The experimental battery was charged and discharged at a 1C rate for 3 weeks at room temperature, and the average value was taken as C1. It was then charged to 100% SOC and discharged to 2.8V at 3C. The discharge capacity was recorded as C2. C1 divided by C2 is the 3C rate discharge capacity retention rate.
[0099] Table 2
[0100] As can be seen from Table 2,
[0101] 1) Comparing the initial DCR results of the lithium-ion batteries in Examples 1 to 14 with those in Comparative Examples 1 to 5, it can be seen that compared with traditional functional additives, the additives of the present invention can effectively reduce the initial DCR and the growth of DCR during the cycle, thereby improving high-temperature cycling.
[0102] 2) Comparing the high-temperature storage and volume expansion rate results of the electrolytes and experimental batteries in Examples 1 to 14 with those in Comparative Examples 1 to 5, it can be seen that the additives and electrolytes of the present invention can inhibit battery cell gas production compared to conventional functional additives, thereby improving the retention and recovery rate of high-temperature storage.
[0103] 3) Comparison of the low-temperature and rate test results of the electrolytes and experimental batteries in Examples 1 to 14 and Comparative Examples 1 to 5 shows that the additives and electrolytes of the present invention can improve the low-temperature discharge performance and rate performance compared to conventional additives.
[0104] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: the additives of the present application include both silane groups and sulfonyl groups. The silane group can capture H2O, PF5, and HF from the electrolyte, reducing damage to the positive electrode structure, and the sulfonyl group can form a dense and thinner interface film. The additives of the present application can form a stable interface film on the surface of the positive and negative electrodes, effectively isolating the electrolyte and the positive and negative electrodes, avoiding oxidation reactions between the electrolyte and the positive and negative electrodes, reducing the generation of HF, thereby reducing HF corrosion of the positive electrode, and inhibiting the gas production of the battery at high temperatures, thereby improving the high-temperature storage and high-temperature cycle performance of the battery, while taking into account low-temperature performance and rate performance.
[0105] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention are intended to be within the scope of protection of the present invention.
Claims
1. An additive, It is characterized in that The additive includes [3-(N,N-dimethylamino)propyl]trimethoxysilane and a sulfonyl silane compound, wherein the sulfonyl silane compound has a structure shown in formula (I): Among them, R 1 Indicates F, C 1 ~C 20 Straight or branched alkyl, C 1 ~C 20 Alkyl substituted amine, substituted or unsubstituted C 6 ~C 20 Aryl, cyano, F-substituted C 1 ~C 20 Any one of the straight chain or branched chain alkyl groups; R 2 represents a substituted or unsubstituted imidazolyl group, C 1 ~C 20 Straight or branched alkyl, C substituted by F 1 ~C 20 Straight or branched alkyl, C 1 ~C 20 Alkoxy, C 2 ~C 20 carboxylate group, F-substituted C 2 ~C 20 The carboxylate group, C 4 ~C 20 Heteroaryl, C 2 ~C 20 Any one of the diethylene glycol groups; R 3 , R 4 , R 5 Each independently represents H, F, C 1 ~C 20 Straight or branched alkyl, C substituted by F 1 ~C 20 A straight chain or branched alkyl, substituted or unsubstituted C 6 ~C 20 Any one of the aromatic groups.
2. The additive according to claim 1, It is characterized in that The R 1 represents F, primary amine, tertiary amine, F-substituted C 1 ~C 10 Any one of the straight chain or branched chain alkyl groups; The R 2 Represents C 4 ~C 6 Heteroaryl, C 1 ~C 10 Straight or branched alkyl, C substituted by F 2 ~C 10 The carboxylate group, C 2 ~C 20 Any one of the diethylene glycol groups; The R 3 , the R 4 , the R 5 Each independently represents C 1 ~C 6 Straight-chain or branched alkyl, unsubstituted C 6 ~C 20 Any one of the aromatic groups.
3. The additive according to claim 1, It is characterized in that The R 1 represents any one of F, a primary amino group, a tertiary amino group, and a trifluoromethyl group; The R 2 represents any one of an imidazolyl group, an ethyl group, a difluoroacetate group, and a diethylene glycol group; The R 3 , the R 4 , the R 5 Each independently represents any one of a methyl group, an ethyl group, an isopropyl group, and a phenyl group.
4. The additive according to claim 1, It is characterized in that The sulfonyl silane compound is selected from one or more of the following structures:
5. The additive according to claim 1, It is characterized in that The sulfonyl silane compound is selected from combination of combination of combination of combination of Any combination of .
6. An electrolyte comprising a lithium salt, an electrolyte additive and a solvent, It is characterized in that The electrolyte additive includes the additive according to any one of claims 1 to 5.
7. The electrolyte according to claim 6, It is characterized in that The lithium salt concentration in the electrolyte is 0.5-1.5 M; the additive is 0.1-5 wt % of the electrolyte weight.
8. The electrolyte according to claim 6, It is characterized in that The lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium bis(fluorosulfonyl imide) salt, and lithium bis(trifluoromethylsulfonyl imide).
9. The electrolyte according to claim 6, It is characterized in that The solvent includes one or more of chain and cyclic carbonates and carboxylates.
10. The electrolyte according to claim 6, It is characterized in that The electrolyte further comprises a functional additive, and the functional additive accounts for 0.2 to 10 wt % of the electrolyte.
11. The electrolyte according to claim 10, It is characterized in that The functional additives include at least one of a circulation additive, a low-temperature additive, a high-temperature additive, a flame retardant additive, and an anti-overcharge additive.
12. A lithium ion battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte. It is characterized in that The electrolyte includes the electrolyte according to claim 6.
Citation Information
Patent Citations
An additive, an electrolyte including the additive, and a lithium-ion battery.
CN116190795B
Electrolytic solutions and battery
CN101197455A
Lithium ion electrolyte and preparation method and application thereof
CN112768771A
Electrolyte and electrochemical device
CN113396496A
Additive, electrolyte containing additive and lithium ion battery
CN116190795A
Cited By
Battery electrolyte film-forming additive, battery electrolyte and application thereof
CN119381564A