Stainless steel vapor chamber processing method and vapor chamber

The porous copper plating is formed by electrodeposition on the stainless steel vapor chamber, which solves the problem of reduced heat transfer performance caused by the thickness compression of the liquid absorbing core, achieves efficient phase change heat dissipation and improved stability, and meets the heat dissipation needs of modern miniaturized electronic equipment. .

WO2024222249A1PCT designated stage expired Publication Date: 2024-10-31DONGGUAN LINGYI PRECISION MFG TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/081179
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-12
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

In the process of ultra-thinning of existing vapor chambers, the thickness compression of the liquid-absorbing core causes a decrease in heat transfer performance, which cannot meet the heat dissipation needs of modern miniaturized electronic equipment.

Method used

A porous copper coating is formed through electrodeposition as a liquid-absorbing core. The hydrogen bubble template method is used to cover the stainless steel with an electroplated copper coating. Combined with low-temperature oxidation and vacuum heating, a porous copper coating with high porosity and high specific surface area is formed to achieve efficient phase change. heat dissipation.

Benefits of technology

It realizes the ultra-thin stainless steel vapor chamber, improves the heat dissipation performance and stability, and meets the heat dissipation needs of modern miniaturized electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024081179_31102024_PF_FP_ABST
    Figure CN2024081179_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A stainless steel vapor chamber processing method and a vapor chamber, relating to the technical field of heat exchange. The stainless steel vapor chamber processing method comprises the following steps: connecting a stainless steel upper cover to a first copper body; immersing the first copper body, a second copper body, and the stainless steel upper cover into an electrolyte, the electrolyte comprising CuSO4 and H2SO4; electrically connecting a negative electrode of a power supply to the first copper body, and electrically connecting a positive electrode of the power supply to the second copper body; starting the power supply, and electroplating on a nickel plating layer of the stainless steel upper cover by means of a hydrogen bubble template method to form a porous copper plating layer; performing low-temperature oxidation on the stainless steel upper cover and the porous copper plating layer; and performing vacuum heating on the stainless steel upper cover and the porous copper plating layer. According to the stainless steel vapor chamber processing method, electro-deposition is performed on the stainless steel upper cover to form the porous copper plating layer to serve as a liquid suction core, efficient phase change heat dissipation is achieved, the thickness of the porous copper plating layer can be controlled, and the processing requirement is met.
Need to check novelty before this filing date? Find Prior Art

Description

Stainless steel soaking plate processing method and soaking plate Technical Field

[0001] The present invention relates to the field of heat exchange technology, and in particular to a stainless steel vapor chamber processing method and the vapor chamber. Background Art

[0002] The heat spreader has excellent thermal conductivity, and has the advantages of large heat transfer area, good temperature uniformity and high reliability. It is the primary way to solve the heat dissipation problem of electronic equipment.

[0003] In order to meet the heat dissipation needs of modern miniaturized electronic devices in the 5G era, ultra-thin vapor chambers are a research hotspot in the industry and academia. Currently, the vapor chamber wick structure can be a single structure such as micro-grooves, powder sintering, foam metal, wire mesh sintering, or a composite structure composed of two types of single structures. However, the composite structure is thicker, and the single-structure wick structure is usually difficult to fully control its porosity, capillary pressure, permeability and overall size. These factors determine the excellent capillary performance of the ultra-thin vapor chamber wick, among which the capillary performance of the wick plays a decisive role in the performance of the vapor chamber. However, as the vapor chamber design becomes thinner and thinner, the thickness of the wick is continuously compressed, which leads to a sharp decline in the heat transfer performance of the vapor chamber and the inability to guarantee the heat dissipation effect of the vapor chamber.

[0004] Summary of the Invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for processing a stainless steel vapor chamber, which can form a porous copper coating as a liquid wick through electrodeposition to achieve efficient phase change heat dissipation.

[0006] The present invention also provides a heat sink made by using the stainless steel heat sink processing method.

[0007] According to the first embodiment of the present invention, a method for processing a stainless steel vapor chamber comprises the following steps:

[0008] Connect the stainless steel upper cover to the first copper body;

[0009] Immersing the first copper body, the second copper body and the stainless steel upper cover in an electrolyte containing CuSO4 and H2SO4;

[0010] Electrically connecting the positive electrode of a power supply to the first copper body, and electrically connecting the negative electrode of the power supply to the second copper body;

[0011] Starting the power supply, and electroplating a porous copper coating on the nickel coating of the stainless steel upper cover by a hydrogen bubble template method;

[0012] Low-temperature oxidation of the stainless steel upper cover and the porous copper plating layer;

[0013] The stainless steel upper cover and the porous copper plating layer are vacuum heated.

[0014] According to the stainless steel heat sink processing method of the embodiment of the present invention, there are at least the following beneficial effects: the surface of the stainless steel upper cover is plated with a nickel coating, the stainless steel upper cover is connected to the first copper body so that the stainless steel upper cover is electrically connected to the first copper body, the stainless steel upper cover, the first copper body and the second copper body are immersed in an electrolyte, the electrolyte contains CuSO4 and H2SO4, the positive electrode of the power supply is electrically connected to the first copper body, and the negative electrode of the power supply is electrically connected to the second copper body, so that after the power supply is started, a copper coating can be electroplated on the nickel coating of the stainless steel upper cover. In addition to the reduction reaction of copper ions, a hydrogen evolution reaction is also included in the copper electrodeposition process. Hydrogen bubbles are precipitated from the nickel coating of the stainless steel upper cover. Using the hydrogen bubbles as templates, a deposition layer cannot be formed at the position occupied by the bubbles. Copper ions are reduced and deposited only in the gaps between the hydrogen bubbles as templates. Due to the fast deposition rate, the copper ions around the copper deposit are quickly exhausted. In addition, the continuous precipitation of hydrogen interrupts the diffusion of reactive ions from the electrolyte to the ion depletion area. Therefore, copper can only be deposited in the gas. The porous copper plating layer is continuously grown in the gaps between the bubbles, and finally a porous copper plating layer with a self-supporting structure of high porosity and high specific surface area is obtained. The porous copper plating layer has efficient flow of liquid working medium and low permeability. A super-hydrophilic porous copper plating layer is integrated on the surface of the stainless steel upper cover as a liquid absorption core to achieve efficient phase change heat dissipation. The thickness of the porous copper plating layer can be controlled by controlling the time of starting the power supply, so that the thickness of the porous copper plating layer can be accurately controlled. After the electroplating is completed, the stainless steel upper cover and the porous copper plating layer are first placed in an oxygen environment and heated at a low temperature, and then the stainless steel upper cover and the porous copper plating layer are placed in a vacuum environment and heated, so that an oxide film can be formed on the surface of the stainless steel upper cover to improve the corrosion resistance of the stainless steel upper cover, and the structural stability of the copper plating layer can be enhanced to further improve the working stability of the heat spreader. The porous copper plating layer is formed as a liquid absorption core by electroplating on the stainless steel upper cover through the stainless steel heat spreader processing method, so that efficient phase change heat dissipation can be achieved, and the thickness of the porous copper plating layer can be controlled to meet the processing requirements.

[0015] According to some embodiments of the present invention, "starting the power supply, and electroplating a porous copper plating layer on the nickel plating layer of the stainless steel upper cover by a hydrogen bubble template method" includes the following steps: adjusting the electrolyte to 25°C; starting the power supply for 25 seconds, the power supply outputting a current with a current density of 0.5A / cm2, and electroplating the porous copper plating layer on the nickel plating layer of the stainless steel upper cover by a hydrogen bubble template method.

[0016] According to some embodiments of the present invention, “immersing the first copper body, the second copper body and the stainless steel upper cover in an electrolyte containing CuSO4 and H2SO4” includes the following steps: immersing the first copper body, the second copper body and the stainless steel upper cover in the electrolyte consisting of 0.2 mol / L CuSO4, 1 mol / L H2SO4 and sodium dodecyl sulfate.

[0017] According to some embodiments of the present invention, the step of "vacuum heating the stainless steel upper cover and the porous copper coating" also includes the following steps: placing the stainless steel lower cover on the side of the stainless steel upper cover electroplated with the porous copper coating; pressing the stainless steel upper cover and the stainless steel lower cover together; and laser welding the stainless steel upper cover and the stainless steel lower cover to encapsulate the porous copper coating.

[0018] According to some embodiments of the present invention, “vacuum heating the stainless steel upper cover and the porous copper plating” includes the following steps: placing the stainless steel upper cover and the stainless steel lower cover in a vacuum environment; heating the stainless steel upper cover and the stainless steel lower cover to 850° C. for 120 minutes.

[0019] According to some embodiments of the present invention, "low-temperature oxidation of the stainless steel cover and the porous copper coating" includes the following steps: placing the stainless steel cover and the porous copper coating in an aerobic environment; heating the stainless steel cover and the porous copper coating to 500°C for 120 minutes.

[0020] According to some embodiments of the present invention, both the first copper body and the second copper body may be phosphor copper and brass.

[0021] According to some embodiments of the present invention, the step of "connecting the stainless steel upper cover to the first copper body" further includes the following steps: immersing the stainless steel upper cover in acetone; immersing the stainless steel upper cover in ethanol; immersing the stainless steel upper cover in deionized water; and immersing the stainless steel upper cover in 100 ml / L hydrochloric acid solution.

[0022] According to some embodiments of the present invention, the step of "connecting the stainless steel upper cover to the first copper body" also includes the following steps: immersing the stainless steel upper cover in deionized water; electroplating to form a nickel plating layer on the surface of the stainless steel upper cover; and immersing the stainless steel upper cover in deionized water again.

[0023] According to the second aspect of the embodiment of the present invention, the heat sink includes a stainless steel top cover and a heat dissipation copper plating; the stainless steel top cover includes a stainless steel body and a nickel plating, and the nickel plating is arranged on one side of the stainless steel body; the heat dissipation copper plating is arranged on the nickel plating, and a plurality of micropores are provided on the surface of the heat dissipation copper plate.

[0024] The heat spreader according to the embodiment of the present invention has at least the following beneficial effects: the heat spreader can be manufactured according to the stainless steel heat spreader processing method of the embodiment of the first aspect above, the surface of the stainless steel upper cover is plated with a nickel coating, the stainless steel upper cover is connected to the first copper body, so that the stainless steel upper cover and the first copper body are electrically connected, the stainless steel upper cover, the first copper body and the second copper body are immersed in an electrolyte, the electrolyte contains CuSO4 and H2SO4, the positive electrode of the power supply is electrically connected to the first copper body, and the negative electrode of the power supply is electrically connected to the second copper body, so that after starting the power supply, the stainless steel upper cover can be electrically connected to the first copper body. The nickel plating layer of the cover is electroplated with a copper plating layer. In addition to the reduction reaction of copper ions, the copper electrodeposition process also includes a hydrogen evolution reaction. Hydrogen bubbles are precipitated from the nickel plating layer of the stainless steel cover. Using hydrogen bubbles as templates, no deposit layer can be formed at the position occupied by the bubbles. Copper ions can only be reduced and deposited in the gaps between the hydrogen bubbles as templates. Due to the fast deposition rate, the copper ions around the copper deposits are quickly depleted. In addition, the continuous precipitation of hydrogen interrupts the diffusion of reactive ions from the electrolyte to the ion depletion area. Therefore, copper can only grow continuously in the gaps between the bubbles. , and finally a porous copper plating with a self-supporting structure of high porosity and high specific surface area is obtained. The porous copper plating has efficient flow of liquid working medium and low permeability. A super-hydrophilic porous copper plating is integrated on the surface of the stainless steel cover as a liquid absorption core to achieve efficient phase change heat dissipation. The thickness of the porous copper plating can be controlled by controlling the time of starting the power supply, so that the thickness of the porous copper plating can be accurately controlled. Among them, since the heat dissipation copper plating is arranged on the nickel plating layer, the surface of the heat dissipation copper sheet is provided with a number of micropores, and the multi-layer copper plating is the heat dissipation copper plating. After the electroplating is completed, The stainless steel upper cover and the heat dissipation copper plating are first placed in an oxygen environment and heated at a low temperature, and then the stainless steel upper cover and the heat dissipation copper plating are placed in a vacuum environment and heated, so that an oxide film can be formed on the surface of the stainless steel upper cover to improve the corrosion resistance of the stainless steel upper cover, and the structural stability of the copper plating can be strengthened to further improve the working stability of the heat sink; the heat dissipation copper plating is formed by electroplating on the stainless steel upper cover through the stainless steel heat sink processing method as a liquid absorption core, so as to realize efficient phase change heat dissipation, and the thickness of the heat dissipation copper plating can be controlled to meet the processing requirements.

[0025] Additional aspects and advantages of the present invention will be set forth in part in the description which follows and, in part, will be obvious from the description which follows, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the following description of the embodiments with reference to the accompanying drawings, in which:

[0027] FIG1 is a schematic flow chart of a method for processing a stainless steel soaking plate according to the present invention. DETAILED DESCRIPTION

[0028] The following describes embodiments of the present invention in detail. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended only to explain the present invention and are not to be construed as limiting the present invention.

[0029] In the description of the present invention, it should be understood that descriptions involving orientations, such as up, down, left, right, front, and back, etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the present invention.

[0030] In the description of the present invention, unless otherwise clearly defined, terms such as setting, installing, and connecting should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in the present invention based on the specific content of the technical solution.

[0031] 1 , a method for processing a stainless steel vapor chamber according to a first embodiment of the present invention includes the following steps:

[0032] S100, connecting the stainless steel upper cover to the first copper body;

[0033] S200, immersing the first copper body, the second copper body and the stainless steel upper cover in an electrolyte containing CuSO4 and H2SO4;

[0034] S300, electrically connecting the positive electrode of the power supply to the first copper body, and electrically connecting the negative electrode of the power supply to the second copper body;

[0035] S400, starting the power supply, and electroplating a porous copper plating layer on the nickel plating layer of the stainless steel upper cover by a hydrogen bubble template method;

[0036] S500, low temperature oxidation stainless steel cover and porous copper plating;

[0037] S600, vacuum heated stainless steel cover and porous copper plating.

[0038] The surface of the stainless steel cover is plated with nickel. The stainless steel cover is connected to the first copper body so that the stainless steel cover is electrically connected to the first copper body. The stainless steel cover, the first copper body and the second copper body are immersed in an electrolyte. The electrolyte contains CuSO4 and H2SO4. The positive pole of the power supply is electrically connected to the first copper body, and the negative pole of the power supply is electrically connected to the second copper body. After the power is turned on, a copper layer can be electroplated on the nickel layer of the stainless steel cover. In addition to the reduction reaction of copper ions, a hydrogen evolution reaction is also included in the copper electrodeposition process. Hydrogen bubbles are precipitated from the nickel layer of the stainless steel cover. Using the hydrogen bubbles as templates, no deposition layer can be formed at the position occupied by the bubbles. Copper ions can only be reduced and deposited in the gaps between the hydrogen bubbles as templates. Due to the fast deposition rate, the copper ions around the copper deposit are quickly exhausted. In addition, the continuous precipitation of hydrogen interrupts the diffusion of reactive ions from the electrolyte to the ion depletion area. Therefore, copper can only grow continuously in the gaps between the bubbles. A porous copper plating layer with a self-supporting structure having high porosity and high specific surface area is obtained, the porous copper plating layer has efficient flow of liquid working fluid and low permeability, a super-hydrophilic porous copper plating layer is integrally constructed on the surface of the stainless steel upper cover as a liquid absorption core, so as to achieve efficient phase change heat dissipation, and the thickness of the porous copper plating layer can be controlled by controlling the time of starting the power supply, so that the thickness of the porous copper plating layer can be accurately controlled; after the electroplating is completed, the stainless steel upper cover and the porous copper plating layer are first placed in an oxygen environment and heated at a low temperature, and then the stainless steel upper cover and the porous copper plating layer are placed in a vacuum environment and heated, so that an oxide film can be formed on the surface of the stainless steel upper cover to improve the corrosion resistance of the stainless steel upper cover, and the structural stability of the copper plating layer can be enhanced, so as to further improve the working stability of the heat spreader; a porous copper plating layer is formed by electroplating on the stainless steel upper cover as a liquid absorption core by a stainless steel heat spreader processing method, so as to achieve efficient phase change heat dissipation, and the thickness of the porous copper plating layer can be controlled to meet the processing requirements.

[0039] In some embodiments of the present invention, “S400, starting the power supply, and electroplating a porous copper coating on the nickel coating of the stainless steel cover by a hydrogen bubble template method” includes the following steps:

[0040] Adjust the electrolyte to 25°C;

[0041] The power supply was turned on for 25 seconds, and the power supply output current density was 0.5 A / cm2. A porous copper plating layer was electroplated on the nickel plating layer of the stainless steel upper cover by a hydrogen bubble template method.

[0042] By controlling the temperature of the electrolyte, the temperature of the first copper body, the second copper body and the stainless steel upper cover can be controlled, thereby controlling the temperature environment during the electroplating process and ensuring the stability of the electroplating process;

[0043] By controlling the start-up time of the power supply and the current output by the power supply, the electroplating time and efficiency can be controlled, thereby controlling the porous copper plating layer so that the porous copper plating layer can meet the ultra-thin processing requirements of the heat sink.

[0044] In some embodiments of the present invention, “S200, immersing the first copper body, the second copper body, and the stainless steel upper cover in an electrolyte containing CuSO4 and H2SO4” includes the following steps:

[0045] The first copper body, the second copper body and the stainless steel upper cover are immersed in an electrolyte consisting of 0.2 mol / L CuSO4, 1 mol / L H2SO4 and sodium lauryl sulfate.

[0046] By immersing the first copper body, the second copper body and the stainless steel upper cover in an electrolyte, since the electrolyte contains CuSO4 and H2SO4, which can provide a chemical environment for electrodepositing copper, sodium dodecyl sulfate, a chemical reducing agent, is introduced into the electrochemical deposition process, which can induce the coating to grow in the direction of instantaneous nucleation to obtain an electrodeposited coating sample, thereby improving the efficiency of electroplating.

[0047] In some embodiments of the present invention, the step of “S600, vacuum heating the stainless steel upper cover and the porous copper plating layer” may include the following steps:

[0048] Place the stainless steel lower cover on the side of the stainless steel upper cover electroplated with the porous copper layer;

[0049] Press-fit the stainless steel upper cover and the stainless steel lower cover;

[0050] Laser weld the stainless steel upper and lower covers to encapsulate the porous copper plating.

[0051] The porous copper plating is located between the stainless steel upper cover and the stainless steel lower cover, the stainless steel upper cover and the stainless steel lower cover are pressed against each other, and the stainless steel upper cover and the stainless steel lower cover are fixedly welded together by laser welding, so that the porous copper plating can be encapsulated between the stainless steel upper cover and the stainless steel lower cover to protect the porous copper plating.

[0052] In some embodiments of the present invention, “S600, vacuum heating the stainless steel upper cover and the porous copper plating layer” includes the following steps:

[0053] placing the stainless steel upper cover and the stainless steel lower cover under a vacuum environment;

[0054] The stainless steel upper cover and the stainless steel lower cover are heated to 850° C. for 120 minutes.

[0055] By vacuum heating the stainless steel upper cover and the stainless steel lower cover, the wrinkle deformation caused by the stainless steel welding can be smoothed out, and the porous copper plating layer can be further strengthened to improve the structural strength of the porous copper plating layer.

[0056] In some embodiments of the present invention, “S500, low temperature oxidation stainless steel upper cover and porous copper plating layer” includes the following steps:

[0057] placing the stainless steel cover and the porous copper coating in an oxygen environment;

[0058] Heat the stainless steel cover and the porous copper coating to 500°C for 120 minutes.

[0059] Placing the stainless steel upper cover and the porous copper plating layer in an oxygen environment can form an oxide film on the surfaces of the stainless steel upper cover and the stainless steel lower cover, thereby improving the corrosion resistance of the stainless steel upper cover and the stainless steel lower cover.

[0060] In some embodiments of the present invention, both the first copper body and the second copper body may be phosphor copper or brass.

[0061] Specifically, the first copper body is brass, and the second copper body is phosphor copper. Phosphor copper serves as the anode and brass serves as the cathode. The grains of phosphor copper are small and evenly distributed. During electroplating, the anode film is formed quickly and evenly, and the copper ion release is stable. The copper plating formed after electroplating is brighter and more uniform. Brass has a high thermal conductivity and good heat conduction efficiency, which can conduct heat more efficiently.

[0062] In some embodiments of the present invention, the step of “connecting the stainless steel upper cover to the first copper body” further includes the following steps:

[0063] Immerse the stainless steel cover in acetone;

[0064] Immerse the stainless steel cover in ethanol;

[0065] Immerse the stainless steel cover in deionized water;

[0066] Immerse the stainless steel cover in 100ml / L hydrochloric acid solution.

[0067] By immersing the stainless steel cover in acetone, ethanol and hydrochloric acid solution, the oil and oxide layer on the surface of the stainless steel cover can be removed, thereby improving the stability of subsequent electroplating; by immersing the stainless steel cover in deionized water, the acetone and ethanol attached to the stainless steel cover can be cleaned.

[0068] In some embodiments of the present invention, the step of “connecting the stainless steel upper cover to the first copper body” further includes the following steps:

[0069] Immerse the stainless steel cover in deionized water;

[0070] Electroplating a nickel layer on the surface of the stainless steel upper cover;

[0071] Immerse the stainless steel cover in deionized water again.

[0072] The stainless steel upper cover can be cleaned by immersing it in deionized water. The stainless steel upper cover is electroplated with a nickel layer, which can make the stainless steel upper cover have better corrosion resistance. Specifically, the nickel-plated part of the stainless steel upper cover is immersed in the electrolyte to prevent H2SO4 in the electrolyte from corroding the stainless steel upper cover.

[0073] 1 , a heat spreader according to an embodiment of the second aspect of the present invention comprises a stainless steel upper cover and a heat dissipating copper coating; the stainless steel upper cover comprises a stainless steel main body and a nickel coating, the nickel coating being disposed on one side of the stainless steel main body; the heat dissipating copper coating being disposed on the nickel coating, and a plurality of micropores being disposed on the surface of the heat dissipating copper sheet.

[0074] The heat spreader can be made according to the stainless steel heat spreader processing method of the first embodiment of the above-mentioned first aspect. The surface of the stainless steel upper cover is plated with a nickel coating. The stainless steel upper cover is connected to the first copper body so that the stainless steel upper cover is electrically connected to the first copper body. The stainless steel upper cover, the first copper body and the second copper body are immersed in an electrolyte. The electrolyte contains CuSO4 and H2SO4. The positive pole of the power supply is electrically connected to the first copper body, and the negative pole of the power supply is electrically connected to the second copper body. After the power is started, a copper coating can be electroplated on the nickel coating of the stainless steel upper cover. In addition to the reduction reaction of copper ions, a hydrogen evolution reaction is also included in the copper electrodeposition process. Hydrogen bubbles are precipitated from the nickel coating of the stainless steel upper cover. Using the hydrogen bubbles as templates, a deposition layer cannot be formed at the position occupied by the bubbles. Copper ions are reduced and deposited only in the gaps between the hydrogen bubbles as templates. Due to the fast deposition rate, the copper ions around the copper deposit are quickly depleted. In addition, the continuous precipitation of hydrogen interrupts the diffusion of reactive ions from the electrolyte to the ion depletion area. Therefore, copper can only grow continuously in the gaps between the bubbles, and finally a copper layer with high porosity and A porous copper plating with a high specific surface area and a self-supporting structure has high efficiency in liquid flow and low permeability. A super-hydrophilic porous copper plating is integrated on the surface of the stainless steel upper cover as a liquid absorption core to achieve efficient phase change heat dissipation. The thickness of the porous copper plating can be controlled by controlling the time of starting the power supply, so that the thickness of the porous copper plating can be accurately controlled. Since the heat dissipation copper plating is arranged on the nickel plating, the surface of the heat dissipation copper sheet is provided with a plurality of micropores, and the multi-layer copper plating is the heat dissipation copper plating. After the electroplating is completed, the stainless steel upper cover and the heat dissipation copper plating are first placed in an oxygen environment and heated at a low temperature, and then the stainless steel upper cover and the heat dissipation copper plating are placed in a vacuum environment and heated, so that an oxide film can be formed on the surface of the stainless steel upper cover to improve the corrosion resistance of the stainless steel upper cover, and the structural stability of the copper plating can be enhanced to further improve the working stability of the heat spreader. The heat dissipation copper plating is formed as a liquid absorption core by electroplating on the stainless steel upper cover through a stainless steel heat spreader processing method, so that efficient phase change heat dissipation can be achieved, and the thickness of the heat dissipation copper plating can be controlled to meet the processing requirements.

[0075] Throughout this specification, reference to terms such as "one embodiment," "some embodiments," "illustrative embodiments," "examples," "specific examples," or "some examples" means that a specific feature, structure, material, or characteristic described in conjunction with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, illustrative uses of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0076] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to the embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the claims and their equivalents.

Claims

1. A method for processing a stainless steel soaking plate, characterized in that: The following steps are involved: Connect the stainless steel upper cover to the first copper body; Immersing the first copper body, the second copper body and the stainless steel upper cover in an electrolyte containing CuSO4 and H2SO4; The positive electrode of the power supply is electrically connected to the first copper body, and the negative electrode of the power supply is electrically connected to the second copper body; Starting the power supply, and electroplating a porous copper coating on the nickel coating of the stainless steel upper cover by a hydrogen bubble template method; Low temperature oxidation of the stainless steel upper cover and the porous copper plating layer; The stainless steel upper cover and the porous copper plating layer are vacuum heated.

2. The method for processing a stainless steel soaking plate according to claim 1, characterized in that: “Starting the power supply to electroplate a porous copper coating on the nickel coating of the stainless steel cover by a hydrogen bubble template method” includes the following steps: The electrolyte is adjusted to 25°C; The power supply is started for 25 seconds, and the power supply outputs a current with a current density of 0.5 A / cm2. The porous copper coating is formed by electroplating on the nickel coating of the stainless steel cover by a hydrogen bubble template method.

3. The method for processing a stainless steel soaking plate according to claim 1, characterized in that: "immersing the first copper body, the second copper body and the stainless steel upper cover in an electrolyte, wherein the electrolyte comprises CuSO4 and H2SO4", comprises the following steps: The first copper body, the second copper body and the stainless steel upper cover are immersed in the electrolyte, wherein the electrolyte consists of 0.2 mol / L CuSO4, 1 mol / L H2SO4 and sodium dodecyl sulfate.

4. The method for processing a stainless steel soaking plate according to claim 1, characterized in that: The step of "vacuum heating the stainless steel cover and the porous copper coating" includes the following steps: Placing the stainless steel lower cover on the side of the stainless steel upper cover electroplated with the porous copper plating layer; Pressing the stainless steel upper cover and the stainless steel lower cover together; The stainless steel upper cover and the stainless steel lower cover are laser welded to encapsulate the porous copper plating layer.

5. The method for processing a stainless steel soaking plate according to claim 4, characterized in that: "Vacuum heating of stainless steel cover and porous copper coating" includes the following steps: placing the stainless steel upper cover and the stainless steel lower cover in a vacuum environment; The stainless steel upper cover and the stainless steel lower cover are heated to 850° C. for 120 minutes.

6. The method for processing a stainless steel soaking plate according to claim 1, characterized in that: "Low-temperature oxidation of the stainless steel upper cover and the porous copper coating" includes the following steps: Placing the stainless steel upper cover and the porous copper plating layer in an aerobic environment; The stainless steel upper cover and the porous copper plating layer are heated to 500° C. for 120 minutes.

7. The method for processing a stainless steel soaking plate according to claim 1, characterized in that: The first copper body and the second copper body may both be phosphor copper and brass.

8. The method for processing a stainless steel soaking plate according to claim 1, characterized in that: The step of "connecting the stainless steel upper cover to the first copper body" also includes the following steps: Immersing the stainless steel upper cover in acetone; Immersing the stainless steel upper cover in ethanol; Immersing the stainless steel upper cover in deionized water; The stainless steel upper cover is immersed in 100 ml / L hydrochloric acid solution.

9. The method for processing a stainless steel soaking plate according to claim 8, characterized in that: The step of "connecting the stainless steel upper cover to the first copper body" also includes the following steps: Immersing the stainless steel upper cover in deionized water; Electroplating a nickel plating layer on the surface of the stainless steel upper cover; The stainless steel upper cover is immersed in deionized water again.

10. A heat sink, characterized in that: include: The stainless steel upper cover comprises a stainless steel body and a nickel-plated layer, wherein the nickel-plated layer is arranged on one side of the stainless steel body; The heat dissipation copper plated layer is arranged on the nickel plated layer, and a plurality of micropores are arranged on the surface of the heat dissipation copper plate.

Citation Information

Patent Citations

  • Preparation method of three-dimensional micrometer level porous copper thin film

    CN103132111A

  • Preparation method of vapor chamber upper cover plate and vapor chamber

    CN112458503A

  • Vapor chamber and modified manufacturing method thereof

    CN115915699A

  • Stainless steel vapor chamber machining method and vapor chamber