Nb- and ti-containing ultrahigh-strength cold-rolled dual-phase steel, and preparation method therefor

By adding Nb and Ti elements to the high-strength steel plate, and using pickling cold rolling and critical zone annealing, a fine ferrite and martensite structure is formed, which solves the problem of insufficient plastic toughness and formability of the high-strength steel plate. It achieves high tensile strength and yield strength improvement, and is suitable for the lightweight and safety performance requirements of automotive steel.

WO2024222303A1PCT designated stage expired Publication Date: 2024-10-31SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
PCT/CN2024/082116
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-03-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

When the existing high-strength steel plate has a strength level above 800MPa, its plasticity and formability are significantly reduced, and it is prone to cracking, wrinkling, springback and other forming defects, and its tensile strength is low, making it difficult to meet the requirements of lightweight and lightweight automotive steel. Safety performance requirements.

Method used

Ultra-high strength cold-rolled dual-phase steel containing Nb and Ti is used. Through reasonable chemical composition design and preparation process, fine ferrite and martensite microstructures are formed, and pickling, cold rolling and Critical zone annealing treatment controls the grain size and phase transition point to improve the mechanical properties of the material.

Benefits of technology

It has achieved a tensile strength of 1219-1644MPa, a yield strength of 546-1049MPa, and an elongation after break of 7.00%-9.87%, which significantly improves the mechanical properties and plasticity of the steel plate and is suitable for the manufacture of automotive safety structural parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082116_31102024_PF_FP_ABST
    Figure CN2024082116_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are an Nb- and Ti-containing ultrahigh-strength cold-rolled dual-phase steel, and a preparation method therefor. The matrix structure of the dual-phase steel comprises ferrite and martensite, and the dual-phase steel comprises the following components in percentage by mass: 0.19%-0.21% of C, 0.25%-0.27% of Si, 3.1%-3.3% of Mn, 0.04%-0.05% of Nb, 0.02%-0.03% of Ti, 0.18%-0.2% of Mo, 0.05%-0.07% of Al, and the balance of Fe and inevitable impurities. The preparation method for the dual-phase steel comprises: component design, smelting, forging, hot rolling, pickling, cold rolling, and intercritical annealing. The dual-phase steel of the present invention has ultrahigh strength, maintains good ductility, has a tensile strength of 1219-1644 MPa, a yield strength of 546-1049 MPa and a percentage elongation after fracture of 7.00%-9.87%, and is suitable for manufacturing automobile safety structural members.
Need to check novelty before this filing date? Find Prior Art

Description

Ultra-high strength cold-rolled dual-phase steel containing Nb and Ti and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of ultra-high strength automobile steel plates, and in particular to an ultra-high strength cold-rolled dual-phase steel containing Nb and Ti and a preparation method thereof. Background Art

[0002] In recent years, driven by the rapid growth of the automotive industry, China has ranked first in the world in both automobile production and sales for many consecutive years. Although the growth rate of automobile production and sales has slowed due to the dual impact of slowing domestic economic growth and the transformation and upgrading of the domestic economy, the automotive industry still has room for development, especially in the new energy vehicle sector, which is being vigorously developed by the country. Production and sales are expected to continue to grow for some time to come. With the development of the automotive and steel industries, the research and development requirements and standards for automotive steel are constantly evolving. Faced with fierce competition from other emerging materials, advanced automotive steel materials are developing towards higher strength, higher ductility, lower cost, and easier processing and forming.

[0003] However, as the strength of advanced high-strength steel increases, especially for high-strength steels with strength levels above 800 MPa, the plasticity, toughness, and formability of these steels decrease significantly, making them more susceptible to forming defects such as cracking, wrinkling, and springback during the forming process. To this end, researchers from various countries have made significant technological progress in recent years in the areas of process fundamentals, metallurgy, materials processing, mechanism research, and deep processing applications of high-performance advanced high-strength steels. Major research areas focus on alloy composition, microstructure, heat treatment processes, coating and plating, deep processing technologies, digital simulation, and big data analysis.

[0004] Whether from the perspective of performance or from the perspective of comprehensive cost, in the foreseeable future of the next 30 to 50 years, high-strength steel plates will be the preferred material for meeting the requirements of lightweight vehicle bodies and improving vehicle safety performance. Future high-quality automotive steel should have both ultra-high strength and good plasticity.

[0005] Chinese patent CN114606449A, "High Strength-Plasticity Product, Low Yield Ratio DP980 Cold-Rolled Dual-Phase Steel and Its Production Method," published on June 10, 2022, states that the steel plate composition is C: 0.11%-0.14%, Si: 0.10%-0.15%, Mn: 2.22%-2.24%, P ≤ 0.014%, S ≤ 0.003%, Mo: 0.13%-0.16%, Cr: 0.27%-0.31%, Al: 0.17%-0.21%, Ti: 0.03%-0.05%, and the remainder is Fe and unavoidable impurities. This method incorporates multiple alloying elements, but the tensile strength level is low and the plasticity is average, leaving significant room for improvement in mechanical properties.

[0006] In addition, the Chinese patent CN113584393A "A Duplex Steel with a Tensile Strength of 780MPa and Its Production Method" published on November 2, 2021, has a steel plate composition of C: 0.06%-0.10%, Si: less than 1.0%, Mn+Cr: 2.0%-2.8%, Nb+Ti: 0.03%-0.08%, Al: 0.02%-0.08%, P: less than 0.03%, S: less than 0.008%, N: less than 0.006%, and the rest is Fe and unavoidable impurities. The duplex steel prepared by this method has a yield strength ratio of 0.65-0.80, which can significantly reduce the springback during the stamping process of parts, but the tensile strength is only 780MPa, and there is a lot of room for improvement.

[0007] Summary of the Invention

[0008] In response to the problems in the above background, the present invention aims to provide an ultra-high strength cold-rolled dual-phase steel and a preparation method thereof, which can reduce the thickness of the steel plate while meeting the strength requirements of the steel plate for automobiles, thereby providing an effective measure for lightweighting automobiles.

[0009] In order to solve the above problems, the technical solutions adopted by the present invention are as follows:

[0010] An ultra-high strength cold-rolled dual-phase steel has a microstructure of fine ferrite + martensite, with a martensite volume fraction of 38%-80%, a ferrite volume fraction of 20%-62%, and a ferrite grain size of 1.28-1.75μm. It also contains a small amount of finely dispersed nanoscale second-phase particles, and the second-phase particle size is generally less than 20nm.

[0011] Disclosed is an ultra-high strength cold-rolled dual-phase steel, the chemical composition and mass fraction of which, calculated by percentage, meet the following conditions: C: 0.19%-0.21%, Si: 0.25%-0.27%, Mn: 3.1%-3.3%, Nb: 0.04%-0.05%, Ti: 0.02%-0.03%, Mo: 0.18%-0.2%, Al: 0.05%-0.07%, and the remainder being Fe and unavoidable impurities.

[0012] In the composition design of the ultra-high strength cold-rolled dual-phase steel described in the present invention, the functions of each element are as follows:

[0013] C: Carbon is a solid solution strengthening element, ensuring the material's high strength. The carbon content in duplex steel is generally 0.03%-0.23%. When the carbon content is too low, the austenite content is low when heated within the same critical region (ferrite and austenite), which reduces the volume fraction of martensite obtained after quenching and is not conducive to achieving high strength. However, if the carbon content is too high, the material's weldability will be reduced. Therefore, the carbon content should be designed to be as low as possible while still meeting strength requirements.

[0014] Si: Silicon is a solid solution strengthening element. On the one hand, it can improve the strength of the material. On the other hand, it can accelerate the segregation of carbon into the austenite, purify the ferrite, and thus improve the performance of the finished product.

[0015] Mn: Manganese is an element that strongly improves the hardenability of austenite. Austenite containing an appropriate amount of Mn can achieve the desired structure by varying the rapid cooling termination temperature, thereby obtaining products with different properties. At the same time, Mn can also dissolve in ferrite to form solid solution strengthening.

[0016] Nb and Ti: Niobium and titanium are carbonitride precipitation elements that can refine grains and precipitate carbonitrides, thereby improving material strength. Both of them have significant grain refinement and precipitation strengthening effects. More importantly, low Nb and Ti contents will weaken the strengthening effect, while high Nb and Ti contents will not only increase the size of the precipitated phase but also increase costs. Therefore, the present invention requires that the Nb and Ti contents be controlled at 0.04%-0.05% and 0.02%-0.03%, respectively.

[0017] Mo: Molybdenum is a medium-strong carbide-forming element. It increases the A3 and A1 temperatures, moves the GS line to the upper left, delays the transformation of proeutectoid ferrite, and promotes the formation of acicular ferrite and bainite. In the production of thick-gauge steel plates, it can significantly improve the uneven microstructure and performance along the thickness direction caused by uneven cooling rate and deformation.

[0018] Al: Trace amounts of Al can purify molten steel and refine grains during the smelting and forging process.

[0019] The above-mentioned method for preparing an ultra-high strength cold-rolled dual-phase steel containing Nb and Ti specifically comprises the following preparation steps:

[0020] (1) Casting: According to the chemical composition ratio of the above-mentioned duplex steel, iron ore, quicklime, ferromolybdenum, ferrotitanium, ferroniobium, alumina, iron-silicon alloy, and iron-manganese alloy are placed in an oxidizing atmosphere furnace to smelt and cast the ingot;

[0021] (2) Forging: The above-mentioned ingot is heated to 1220-1280°C and kept at this temperature for 2-3 hours to dissolve all the elements C, Si, Mn, Nb, Ti, Mo, and Al, and then forging is started at a forging temperature of 1150-1200°C to obtain a forged ingot;

[0022] (3) Hot rolling: The forging blank is heated to 1210-1270°C and kept at this temperature for 2-3 hours. The starting rolling temperature is 1100-1200°C and the finishing rolling temperature is 850-950°C. After rolling, the steel plate is taken out and air-cooled to room temperature to obtain a hot-rolled plate with a thickness of 3.7-4 mm.

[0023] (4) Pickling and cold rolling: The hot-rolled plate is pickled and cold-rolled, and the oxide scale after the hot rolling and pickling process is polished. The cold rolling reduction rate is 40%-60%, the number of cold rolling passes is 5-8 times, and the thickness of the cold-rolled plate after cold rolling is 1.8-1.9 mm;

[0024] (5) Intercritical Annealing: The cold-rolled sheet was subjected to intercritical annealing. The phase transition points of the steel sheet were measured using a Gleeble 3800 thermal simulator, indicating Ac1 = 705°C and Ac3 = 838°C. The intercritical annealing temperature was set at 735-775°C, and the annealing time was 8-12 min. The heating process was carried out in a tubular furnace. After the furnace temperature was raised to 735-775°C, the cold-rolled sheet was placed in the tube furnace. The heating rate was 5-20°C / s, and the steel was kept at this temperature for 8-12 min before oil quenching to obtain the dual-phase steel.

[0025] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0026] (1) The ultra-high strength cold-rolled dual-phase steel of the present invention adopts a reasonable composition design. Controlling the appropriate carbon content (0.19%-0.21% wt) not only ensures sufficient strength but also provides good plasticity and welding performance; controlling the appropriate Si (0.25%-0.27% wt) and Mn (3.1-3.3% wt) contents not only ensures the formation of the dual-phase structure and gives it good hardenability, but also plays a role in solid solution strengthening; adding a small amount of microalloying elements Nb (0.04%-0.05% wt), Ti (0.02%-0.03% wt), Mo (0.18%-0.2% wt), Al (0.05%-0.07% wt), on the basis of the original C-Si-Mn dual-phase steel, by adding a small amount of microalloying elements, can simultaneously play a role in grain refinement and precipitation strengthening.

[0027] (2) In the preparation process of the present invention, a suitable cold rolling reduction rate (50%), intercritical annealing temperature (735-775°C) and annealing time of 8-12 minutes are used. The purpose of cold rolling at a reduction rate of 40%-60% is to refine the original bainite grains to the greatest extent possible, and the annealing time of about 10 minutes is to avoid grain coarsening while obtaining a dual-phase structure. The dual-phase steel prepared by this method not only ensures sufficiently fine grains but also maintains a high martensite volume fraction (38%-80%) in the dual-phase structure, which can maximize the mechanical properties of the cold-rolled dual-phase steel.

[0028] (3) The ultra-high strength cold-rolled dual-phase steel obtained by the present invention has a tensile strength of 1219-1644 MPa, a yield strength of 546-1049 MPa, and an elongation after fracture of 7.00%-9.87%.

[0029] (4) The present invention can effectively refine the grains by adding Mo, Nb, Ti, and Al elements to conventional C-Si-Mn dual-phase steel; and by controlling the appropriate critical zone annealing temperature and annealing time during the preparation process, it can ensure a sufficiently high martensite volume fraction and thus provide sufficiently high strength while maintaining good plasticity, so that the final product can be used as a suitable steel component for automobiles. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] FIG1 shows engineering stress-strain curves of ultra-high strength cold-rolled dual-phase steels prepared in Examples 1-3 of the present invention;

[0031] FIG2 is a graph showing thermal expansion curves of the ultra-high strength cold-rolled dual-phase steels prepared in Examples 1-3 of the present invention;

[0032] FIG3 is a scanning electron microscope image (SEM) of the ultra-high strength cold-rolled dual-phase steel prepared in Example 1 of the present invention;

[0033] FIG4 is a scanning electron microscope photograph (SEM) of the ultra-high strength cold-rolled dual-phase steel prepared in Example 2 of the present invention;

[0034] FIG5 is a scanning electron microscope photograph (SEM) of the ultra-high strength cold-rolled dual-phase steel prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0035] To facilitate understanding of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technical personnel in this field without making creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] A method for preparing ultra-high strength cold-rolled dual-phase steel containing Nb and Ti, comprising the following steps:

[0038] (1) According to the chemical composition ratio of the duplex steel in Table 1 below, iron ore, quicklime, ferromolybdenum, ferrotitanium, ferroniobium, alumina, ferrosilicon alloy, and ferromanganese alloy are placed in an oxidizing atmosphere furnace to smelt and cast the ingot;

[0039] (2) heating the above-mentioned ingot to 1220-1280°C and keeping the temperature for 2-3 hours to dissolve all the elements C, Si, Mn, Nb, Ti, Mo, and Al, and then starting forging at a forging temperature of 1150-1200°C to obtain a forged ingot;

[0040] (3) heating the forging billet to 1210-1270°C and holding the temperature for 2-3 hours, starting the rolling process at 1100-1200°C, and finishing the rolling process at 850-950°C. After rolling, the steel plate is removed and air-cooled to room temperature to obtain a hot-rolled plate having a thickness of 3.7-4 mm.

[0041] (4) pickling and cold rolling the hot-rolled plate, grinding the oxide scale after the hot rolling and pickling process, the cold rolling reduction rate is 40%, the number of cold rolling passes is 5-8 times, and the thickness of the cold-rolled plate after cold rolling is 1.8-1.9 mm;

[0042] (5) The cold-rolled sheet is subjected to intercritical annealing in a tubular furnace. The furnace temperature is raised to 775°C and the cold-rolled sheet is placed therein. The heating rate is 5-20°C / s. The sheet is kept at this temperature for 8 minutes and then oil quenched to obtain the duplex steel.

[0043] Example 2

[0044] A method for preparing ultra-high strength cold-rolled dual-phase steel containing Nb and Ti, comprising the following steps:

[0045] (1) According to the chemical composition ratio of the duplex steel in Table 1 below, iron ore, quicklime, ferromolybdenum, ferrotitanium, ferroniobium, alumina, ferrosilicon alloy, and ferromanganese alloy are placed in an oxidizing atmosphere furnace to smelt and cast the ingot;

[0046] (2) heating the above-mentioned ingot to 1220-1280°C and keeping the temperature for 2-3 hours to dissolve all the elements C, Si, Mn, Nb, Ti, Mo, and Al, and then starting forging at a forging temperature of 1150-1200°C to obtain a forged ingot;

[0047] (3) heating the forging billet to 1210-1270°C and holding the temperature for 2-3 hours, starting the rolling process at 1100-1200°C, and finishing the rolling process at 850-950°C. After rolling, the steel plate is removed and air-cooled to room temperature to obtain a hot-rolled plate having a thickness of 3.7-4 mm.

[0048] (4) pickling and cold rolling the hot-rolled plate, grinding the oxide scale after the hot rolling and pickling process, the cold rolling reduction rate is 50%, the number of cold rolling passes is 5-8 times, and the thickness of the cold-rolled plate after cold rolling is 1.8-1.9 mm;

[0049] (5) The cold-rolled sheet is subjected to intercritical annealing in a tubular furnace. The furnace temperature is raised to 755°C and the cold-rolled sheet is placed therein. The heating rate is 5-20°C / s. The sheet is kept at this temperature for 10 minutes and then oil quenched to obtain the dual-phase steel.

[0050] Example 3

[0051] A method for preparing ultra-high strength cold-rolled dual-phase steel containing Nb and Ti, comprising the following steps:

[0052] (1) According to the chemical composition ratio of the duplex steel in Table 1 below, iron ore, quicklime, ferromolybdenum, ferrotitanium, ferroniobium, alumina, ferrosilicon alloy, and ferromanganese alloy are placed in an oxidizing atmosphere furnace to smelt and cast the ingot;

[0053] (2) heating the above-mentioned ingot to 1220-1280°C and keeping the temperature for 2-3 hours to dissolve all the elements C, Si, Mn, Nb, Ti, Mo, and Al, and then starting forging at a forging temperature of 1150-1200°C to obtain a forged ingot;

[0054] (3) heating the forging billet to 1210-1270°C and holding the temperature for 2-3 hours, starting the rolling process at 1100-1200°C, and finishing the rolling process at 850-950°C. After rolling, the steel plate is removed and air-cooled to room temperature to obtain a hot-rolled plate having a thickness of 3.7-4 mm.

[0055] (4) pickling and cold rolling the hot-rolled plate, grinding the oxide scale after the hot rolling and pickling process, the cold rolling reduction rate is 60%, the number of cold rolling passes is 5-8 times, and the thickness of the cold-rolled plate after cold rolling is 1.8-1.9 mm;

[0056] (5) The cold-rolled sheet is subjected to intercritical annealing in a tubular furnace. The furnace temperature is raised to 735°C and the cold-rolled sheet is placed therein. The heating rate is 5-20°C / s. The sheet is kept at this temperature for 12 minutes and then oil quenched to obtain the dual-phase steel.

[0057] Table 1 is a list of chemical components of the above embodiments of the present invention;

[0058] Table 2 shows the cold rolling and intercritical annealing process parameters of the above embodiments of the present invention;

[0059] Table 3 shows the microstructure and mechanical properties of the dual-phase steels prepared in the above embodiments of the present invention.

[0060] Table 1 Chemical composition of Examples 1 to 3

[0061] Table 2 Cold rolling and intercritical annealing process parameters of Examples 1 to 3

[0062] The mechanical properties of the dual-phase steels prepared in Examples 1 to 3 were tested, and the test results are shown in Table 3.

[0063] Table 3 Microstructure and mechanical properties of dual-phase steels prepared in Examples 1 to 3

[0064] As shown in Tables 1-3, the cold-rolled dual-phase steel sheets produced using the composition design, cold rolling, and heat treatment processes of the present invention exhibit excellent mechanical properties, with tensile strength reaching 1644 MPa, yield strength reaching 1049 MPa, yield strength ratios ranging from 44.8% to 63.8%, elongations after fracture ranging from 7.00% to 9.87%, and strength-ductility products ranging from 10.7 to 12.1 GPa·%. Furthermore, the dual-phase steels produced in Examples 1-3 exhibit suitable microstructures, with a martensite volume fraction ranging from 38% to 80% and a ferrite grain size ranging from 1.30 to 1.75 μm. The ultra-high-strength cold-rolled dual-phase steels produced in each example exhibit excellent performance and are suitable for the manufacture of automotive safety structural components, demonstrating promising application value and prospects.

[0065] Figure 1 shows the engineering stress-strain curves of the ultra-high-strength cold-rolled dual-phase steels prepared in Examples 1-3 of the present invention. As can be seen, as the martensite volume fraction increases, the yield strength of the examples increases, the tensile strength increases, and the yield strength ratio also increases. The elongation after fracture first decreases and then increases, and the strength-ductility product also decreases and then increases. When the martensite volume fraction is 80%, Example 1 achieves a maximum yield strength of 1049 MPa and a maximum tensile strength of 1644 MPa.

[0066] Figure 2 shows the thermal expansion curves of the ultra-high-strength cold-rolled dual-phase steels prepared in Examples 1-3 of the present invention. It can be seen that the phase transformation points for the three examples in this alloy composition are Ac1 = 705°C, Ac3 = 838°C, and Ms = 372°C. The dual-phase steel undergoes an austenitic transformation when heated above 705°C, which ends at 838°C, transforming into a fully austenitic structure. Upon rapid cooling to 372°C, the martensitic transformation begins.

[0067] Figure 3 is a SEM image of the ultra-high strength cold-rolled dual-phase steel prepared in Example 1 of the present invention. It can be seen that when the martensite volume fraction is 80%, the average ferrite grain size is 1.30 μm. At this time, the matrix structure of the dual-phase steel is continuous martensite.

[0068] Figure 4 is a SEM image of the ultra-high strength cold-rolled dual-phase steel prepared in Example 2 of the present invention. It can be seen that when the martensite volume fraction is 66%, the average ferrite grain size is 1.28 μm. At this time, the matrix structure of the dual-phase steel is still continuous martensite.

[0069] Figure 5 is a SEM image of the ultra-high-strength cold-rolled dual-phase steel produced in Example 3 of the present invention. It shows that at a martensite volume fraction of 38%, the average ferrite grain size is 1.75 μm. At this point, the matrix of the dual-phase steel is continuous ferrite, with numerous nanoscale (less than 20 nm) second-phase particles visible within the ferrite matrix.

[0070] It should be noted that the embodiments listed above are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments. Similar changes or modifications made therewith are directly derived from the contents disclosed by those skilled in the art or can be easily associated with them, and should all fall within the scope of protection of the present invention. In addition, the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.

Claims

1. An ultra-high strength cold-rolled dual-phase steel containing Nb and Ti, characterized in that: The formula includes: C, Si, Mn, Nb, Ti, Mo, Al and Fe, and the mass percentages of each component are: C: 0.19%-0.21%, Si: 0.25%-0.27%, Mn: 3.1%-3.3%, Nb: 0.04%-0.05%, Ti: 0.02%-0.03%, Mo: 0.18%-0.2%, Al: 0.05%-0.07%, and the rest is Fe and unavoidable impurities.

2. The ultra-high strength cold-rolled dual-phase steel containing Nb and Ti according to claim 1, characterized in that: The formula includes: C, Si, Mn, Nb, Ti, Mo, Al and Fe, and the mass percentages of each component are: C: 0.198%, Si: 0.268%, Mn: 3.259%, Nb: 0.045%, Ti: 0.027%, Mo: 0.193%, Al: 0.06%, and the rest are Fe and unavoidable impurities.

3. The method for preparing the ultra-high strength cold-rolled dual-phase steel containing Nb and Ti according to claim 1, characterized in that: The specific steps include: (1) Casting: smelting the ingot according to the chemical composition mass percentage of claim 1; (2) Forging: The above-mentioned ingot is heated to dissolve all the elements C, Si, Mn, Nb, Ti, Mo and Al, and then forging is started to obtain a forged ingot; (3) Hot rolling: rolling the forged billet under heating, taking out the steel plate after rolling and air cooling it to room temperature to obtain a hot-rolled plate; (4) Pickling and cold rolling: pickling and cold rolling the hot-rolled sheet, grinding the oxide scale on the surface of the material after hot rolling and pickling, and obtaining a cold-rolled sheet; (5) Intercritical region annealing: The above-mentioned cold-rolled sheet is subjected to intercritical region annealing treatment. The heating process is carried out in a tubular furnace. After the furnace temperature is raised to the set intercritical region annealing temperature, the cold-rolled sheet is placed in the tube for annealing treatment, heat preservation, and oil quenching to obtain the dual-phase steel.

4. The method for preparing a Nb-Ti-containing ultra-high strength cold-rolled dual-phase steel according to claim 3, characterized in that: The temperature of heating the ingot in step (2) is 1220-1280°C and kept warm for 2-3h; the temperature of forging the ingot in step (2) is 1150-1200°C.

5. The method for preparing a Nb-Ti-containing ultra-high strength cold-rolled dual-phase steel according to claim 3, characterized in that: The forging billet in step (3) is rolled in a heated state, specifically: the forging billet is heated to 1210-1270°C and kept warm for 2-3h, the starting rolling temperature is 1100-1200°C, and the final rolling temperature is 850-950°C.

6. The method for preparing a Nb-Ti-containing ultra-high strength cold-rolled dual-phase steel according to claim 3, characterized in that: In step (4), the cold rolling reduction rate is 40%-60%, the number of cold rolling passes is 5-8 times, and the thickness of the cold rolled plate after cold rolling is 1.8-1.9 mm.

7. The method for preparing ultra-high strength cold-rolled dual-phase steel containing Nb and Ti according to claim 3, characterized in that: In step (5), the critical region annealing temperature is set to 735-775° C. and the annealing time is set to 8-12 min.

8. The method for preparing ultra-high strength cold-rolled dual-phase steel containing Nb and Ti according to claim 3, characterized in that: The heating rate of the tubular furnace in step (5) is 5-20°C / s.

9. The method for preparing ultra-high strength cold-rolled dual-phase steel containing Nb and Ti according to claim 3, characterized in that: The final microstructure of the dual-phase steel is fine ferrite + martensite, in which the volume fraction of martensite is 38%-80%, the volume fraction of ferrite is 20%-62%, the ferrite grain size is 1.28-1.75μm, and it also contains finely dispersed nanoscale second phase particles, and the second phase particle size is less than 20nm.

10. The method for preparing ultra-high strength cold-rolled dual-phase steel containing Nb and Ti according to claim 3, characterized in that: The tensile strength of the finally obtained dual-phase steel is 1219-1644 MPa, the yield strength is 546-1049 MPa, and the elongation after fracture is 7.00%-9.87%.

Citation Information

Patent Citations

  • Ultra high strength steel plate having excellent workability, and production method for same

    CN102869801A

  • Hot-rolled martensite steel and production method thereof

    CN103334057A

  • 1300 MPa-grade ultrahigh-strength cold-rolled steel sheet for automobile and production method of 1300 MPa-grade ultrahigh-strength cold-rolled steel sheet

    CN109628846A

  • High-strength galvanized steel sheet, and method for manufacturing same

    CN111433380A

  • Ultrahigh-strength cold-rolled dual-phase steel containing Nb and Ti and preparation method of ultrahigh-strength cold-rolled dual-phase steel

    CN116590614A

Cited By

  • Nb-Ti-containing cold roll steel and preparation method thereof

    CN122235567A