Electrolyte solution production method and fluorine gas production method

By adding an alkali metal salt of hexafluoronicel(IV) acid to the electrolyte solution, the method effectively reduces water concentration, preventing the anode effect and enabling efficient fluorine gas production, addressing the inefficiencies of existing techniques.

WO2024224840A1PCT designated stage expired Publication Date: 2024-10-31RESONAC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009407
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for producing fluorine gas by electrolysis using a carbonaceous electrode are hindered by the anode effect, which occurs when water is present, leading to increased water concentration and inefficiencies, requiring time-consuming and labor-intensive techniques to reduce water concentration in the electrolyte solution.

Method used

Adding an alkali metal salt of hexafluoronicel(IV) acid to a mixture of hydrogen fluoride and inorganic fluoride with high water concentration to dehydrate the solution, reducing water content to 100 mass ppm or less, thereby preventing the anode effect and enabling efficient fluorine gas production.

Benefits of technology

This method allows for the production of an electrolyte solution with low water concentration through simple and rapid operations, resulting in economic and efficient generation of fluorine gas with minimal impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

Provided is an electrolyte solution production method capable of producing, in a short time by a simple operation, an electrolyte solution having a low water concentration. This electrolyte solution production method produces an electrolyte solution for generating fluorine gas through electrolysis using a carbonaceous electrode as an anode, the method comprising a dehydration step for adding an alkali metal salt of hexafluoronickelate (IV) to a mixture containing hydrogen fluoride and an inorganic fluoride and having a water concentration of more than 100 ppm by mass and 1% by mass or less so as to achieve water concentration of 100 ppm by mass or less.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte manufacturing method and fluorine gas manufacturing method

[0001] The present invention relates to a method for producing an electrolyte solution and a method for producing fluorine gas.

[0002] Fluorine gas can be synthesized by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride. A carbonaceous electrode is usually used as the anode when electrolyzing the electrolyte solution. However, if water is present in the electrolyte solution, an insulating film is likely to form on the surface of the anode, which may cause a phenomenon known as the anode effect, in which the electrolysis voltage rises sharply. Therefore, it is preferable that the water concentration of the electrolyte solution is as low as possible.

[0003] Patent Document 1 discloses a technique for reducing the water concentration of an electrolyte by blowing an inert gas into the electrolyte. Patent Document 2 discloses a technique for generating fluorine gas by electrolyzing the electrolyte using nickel electrodes and then reacting the generated fluorine gas with water to remove the water. Generally, as disclosed in Patent Document 3, a technique is often adopted in which electrolysis is performed at a low current density using carbonaceous electrodes to electrolyze water, and then the current density is increased to perform electrolysis to synthesize fluorine gas.

[0004] Japanese Patent Publication No. 2515, 1995 Japanese Patent Publication No. 3089432 Japanese Patent Publication No. 5520280

[0005] Although it is possible to reduce the water concentration of an electrolyte solution by the techniques disclosed in Patent Documents 1 to 3, the operations are time-consuming and require a long time, and therefore a technique that can reduce the water concentration of an electrolyte solution by a simple operation and in a short time has been desired. An object of the present invention is to provide a method for producing an electrolyte solution with a low water concentration by a simple operation and in a short time, and a method for producing fluorine gas that can economically produce fluorine gas.

[0006] In order to solve the above problems, one aspect of the present invention is as follows: [1] to [6] [1] A method for producing an electrolyte solution for generating fluorine gas by electrolysis using a carbonaceous electrode as an anode, the method comprising a dehydration step of adding an alkali metal hexafluoronickelate (IV) to a mixture containing hydrogen fluoride and an inorganic fluoride and having a water concentration of more than 100 ppm by mass and not more than 1% by mass, to reduce the water concentration to not more than 100 ppm by mass.

[0007] [2] The method for producing an electrolytic solution according to [1], wherein the alkali metal hexafluoronickelate (IV) is at least one of potassium hexafluoronickelate (IV), cesium hexafluoronickelate (IV), and rubidium hexafluoronickelate (IV).

[0008] [3] The method for producing an electrolytic solution according to [1] or [2], wherein the inorganic fluoride is at least one of potassium fluoride, cesium fluoride, rubidium fluoride, and ammonium fluoride. [4] The method for producing an electrolytic solution according to any one of [1] to [3], wherein the amount of the alkali metal hexafluoronickelate (IV) added is 100 ppm by mass or more and 10% by mass or less of the mass of the mixture.

[0009] [5] A method for producing fluorine gas, comprising an electrolysis step of electrolyzing the electrolyte solution produced by the method for producing an electrolyte solution according to any one of [1] to [4] in an electrolytic cell using an anode and a cathode to generate fluorine gas. [6] The method for producing fluorine gas according to [5], wherein the anode is a carbonaceous electrode having at least one of graphite, glassy carbon, and amorphous carbon.

[0010] The method for producing an electrolyte solution according to the present invention is capable of producing an electrolyte solution having a low water concentration by a simple operation in a short time. The method for producing fluorine gas according to the present invention is capable of producing fluorine gas economically.

[0011] An embodiment of the present invention will be described below. Note that this embodiment is merely an example of the present invention, and the present invention is not limited to this embodiment. Furthermore, various modifications and improvements can be made to this embodiment, and such modifications and improvements can also be included in the present invention.

[0012] It is known that water (HO) in the electrolyte causes the anode effect in the synthesis of fluorine gas (F) by electrolysis of an electrolyte. As a result of extensive research into methods for removing water from the electrolyte, the inventors discovered that the water concentration in the electrolyte can be reduced by adding an additive, leading to the completion of the present invention.

[0013] That is, the method for producing an electrolytic solution according to this embodiment is a method for producing an electrolytic solution for generating fluorine gas by electrolysis using a carbonaceous electrode as an anode, and includes a dehydration step of adding an alkali metal hexafluoronickel(IV) salt to a mixture containing hydrogen fluoride (HF) and an inorganic fluoride and having a water concentration of more than 100 ppm by mass and not more than 1% by mass, thereby reducing the water concentration to not more than 100 ppm by mass. The method for producing fluorine gas according to this embodiment also includes an electrolysis step of electrolyzing the electrolytic solution produced by the method for producing an electrolytic solution according to this embodiment in an electrolytic cell using an anode and a cathode to generate fluorine gas.

[0014] Since alkali metal hexafluoronickel(IV) salt is easily soluble in a mixture containing hydrogen fluoride and an inorganic fluoride and has oxidizing power, the alkali metal hexafluoronickel(IV) salt reacts with water in the electrolyte to decompose the water, thereby reducing the water concentration of the electrolyte. Therefore, when producing fluorine gas by electrolyzing an electrolyte containing alkali metal hexafluoronickel(IV) salt, the anode effect is unlikely to occur.

[0015] By adding an alkali metal hexafluoronickelate (IV), the water concentration of the electrolytic solution can be reduced, so the dehydration step in the method for producing an electrolytic solution according to this embodiment is an extremely simple operation, and dehydration can be carried out in a short time. Furthermore, since dehydration of the electrolytic solution can be carried out by a simple operation in a short time, the method for producing fluorine gas according to the present invention can produce fluorine gas economically.

[0016] The method for producing an electrolytic solution according to this embodiment and the method for producing fluorine gas according to this embodiment will be described in further detail below. [Electrolytic Solution] The electrolytic solution to be electrolyzed in the method for producing fluorine gas according to this embodiment contains hydrogen fluoride and an inorganic fluoride, and has a water concentration of 100 mass ppm or less. This electrolytic solution can be produced by the method for producing an electrolytic solution according to this embodiment. That is, the electrolytic solution can be produced by adding an alkali metal hexafluoronickel(IV) salt to a mixture containing hydrogen fluoride and an inorganic fluoride and having a water concentration of more than 100 mass ppm and 1 mass % or less, followed by dehydration, thereby reducing the water concentration to 100 mass ppm or less.

[0017] The type of inorganic fluoride is not particularly limited, but metal fluorides are preferred, and at least one of potassium fluoride (KF), cesium fluoride (CsF), and rubidium fluoride (RbF) is more preferred. Furthermore, ammonium fluoride (NH4F) can be used as the inorganic fluoride. When ammonium fluoride is used as the inorganic fluoride, nitrogen trifluoride (NF3) is generated by electrolysis of the electrolyte. The inorganic fluorides may be used alone or in combination of two or more.

[0018] When nitrogen trifluoride is produced together with fluorine gas, an electrolyte solution containing at least one of potassium fluoride, cesium fluoride, and rubidium fluoride, ammonium fluoride, and hydrogen fluoride is used, and the ratio of the molar amount of hydrogen fluoride to the molar amount of inorganic fluoride contained in the electrolyte solution ([molar amount of hydrogen fluoride] / [molar amount of inorganic fluoride]) is preferably 1.6 or more and 3.2 or less, more preferably 1.9 or more and 3.0 or less.

[0019] The electrolyte may be, for example, a mixed molten salt of hydrogen fluoride and potassium fluoride. The molar ratio of hydrogen fluoride to potassium fluoride in the mixed molten salt of hydrogen fluoride and potassium fluoride may be, for example, hydrogen fluoride:potassium fluoride = 1.5 to 2.5: 1. A typical electrolyte is KF·2HF, where the ratio of hydrogen fluoride to potassium fluoride is 2:1, and the melting point of this mixed molten salt is approximately 72°C.

[0020] Another example of the electrolyte solution is a mixed molten salt of hydrogen fluoride and cesium fluoride. The molar ratio of hydrogen fluoride to cesium fluoride in the mixed molten salt of hydrogen fluoride and cesium fluoride can be, for example, hydrogen fluoride:cesium fluoride = 1.8 to 3.1:1. A typical electrolyte solution is CsF·2.4HF, where the ratio of hydrogen fluoride to cesium fluoride is 2.4:1, and the melting point of this mixed molten salt is approximately 16°C.

[0021] Because hydrogen fluoride in the electrolyte is consumed by electrolysis, hydrogen fluoride may be continuously or intermittently supplied to the electrolyte during electrolysis. Hydrogen fluoride may be supplied to the electrolyte on the cathode chamber side of the electrolytic cell, or to the electrolyte on the anode chamber side. Taking the hydrogen fluoride concentration in a KF·2HF electrolyte (hydrogen fluoride concentration: 40.4 mass%) or CsF·2.4HF electrolyte (hydrogen fluoride concentration: 24.0 mass%) as a reference concentration, the hydrogen fluoride concentration in the electrolyte is preferably controlled to vary within a range of −5 mass% to +5 mass% of the reference concentration, more preferably −2.5 mass% to +2.5 mass% of the reference concentration, and even more preferably −1.5 mass% to +1.5 mass% of the reference concentration.

[0022] [Water Concentration of Electrolyte] Solid KF / HF, KF, and CsF typically contain several hundred ppm by mass of water, while hydrogen fluoride typically contains 100 to 200 ppm by mass of water. Water also adheres to the interior of the preparation equipment for preparing the electrolyte and the interior of the electrolytic cell in which the electrolyte is electrolyzed. Furthermore, the electrolyte may come into contact with the atmosphere during the electrolyte operation process, and the electrolyte may absorb water from the atmosphere. For these reasons, an electrolyte produced by mixing hydrogen fluoride and an inorganic fluoride contains water, and its water concentration is typically greater than 100 ppm by mass and less than or equal to 1% by mass.

[0023] Therefore, in this embodiment, as described above, an alkali metal hexafluoronickel(IV) salt is added to a mixture containing hydrogen fluoride and an inorganic fluoride and having a water concentration of more than 100 ppm by mass and not more than 1% by mass, followed by dehydration to reduce the water concentration to not more than 100 ppm by mass, thereby producing an electrolyte solution with a low water concentration.

[0024] For example, when the electrolyte is KF·2HF, a low-water-concentration electrolyte can be produced by mixing solid KF·HF or solid KF with liquid or gaseous hydrogen fluoride to prepare the mixture, adding an alkali metal hexafluoronickel(IV) acid salt thereto, and dehydrating the mixture.

[0025] Furthermore, when the electrolyte is CsF·2.4HF, an electrolyte with a low water concentration can be produced by mixing solid CsF with liquid or gaseous hydrogen fluoride to prepare the mixture, adding an alkali metal hexafluoronickel(IV) acid salt thereto, and dehydrating the mixture.

[0026] Even if the water concentration of a mixture containing hydrogen fluoride and an inorganic fluoride exceeds 1% by mass, it is possible to reduce the water concentration by adding an alkali metal hexafluoronickel(IV) salt. However, if the water concentration of the mixture is 1% by mass or less, the amount of nickel fluoride (NiF) produced as a by-product by the reaction of the alkali metal hexafluoronickel(IV) salt with water is small, making it difficult for nickel fluoride to deposit on the bottom of the electrolytic cell. Furthermore, considering the accuracy of the method for measuring the water concentration of the electrolyte, there is a risk that a water concentration of less than 100 ppm by mass cannot be accurately measured.

[0027] Here, an example of a method for measuring the moisture concentration of an electrolyte will be described, taking the case where the electrolyte is KF·2HF as an example. The moisture concentration of an electrolyte can be measured, for example, using a moisture analyzer having the following configuration. The moisture analyzer includes a cylindrical nickel heating section, a gas supply pipe for supplying an inert gas such as nitrogen gas into the cylindrical heating section, a heater such as an electric heater for heating the cylindrical heating section, a thermometer such as a thermocouple for measuring the temperature inside the cylindrical heating section, and an analyzer such as an FT-IR analyzer for analyzing the gas discharged from the cylindrical heating section. This moisture analyzer is installed inside a glove box maintained at low humidity.

[0028] The mass of the measured electrolyte sample is placed in a platinum boat-shaped tray, which is then placed inside the cylindrical heating section. An inert gas is then supplied into the cylindrical heating section through a gas supply pipe. The cylindrical heating section is pressurized by the inert gas to maintain its airtightness. The cylindrical heating section is then heated by a heater while a constant flow of inert gas is supplied to the cylindrical heating section through the gas supply pipe. The cylindrical heating section is heated in stages from room temperature to 350°C.

[0029] The gas evaporated from the sample by heating is discharged from the cylindrical heating section together with the inert gas and sent to the FT-IR analyzer. Continuous analysis is then performed by the FT-IR analyzer, and the absorption wave number is 1400 cm. -1 From 1899 cm -1The water concentration is quantified from the intensity of the peak in the range, and the total amount of evaporated water is calculated from the integrated value of the period from when the water peak is detected until it is no longer detected. The water concentration of the electrolyte can be calculated from the total amount of evaporated water and the mass of the sample.

[0030] The water concentration of the electrolyte solution (the mixture) measured by the above measurement method varies depending on the method for preparing the electrolyte solution (method for mixing hydrogen fluoride and inorganic fluoride), the atmosphere during preparation of the electrolyte solution (the atmosphere during mixing hydrogen fluoride and inorganic fluoride), and the preparation scale of the electrolyte solution (the amount of the mixture prepared). For example, when the amount of the electrolyte solution prepared is about several liters, the water concentration of the electrolyte solution can be made to be more than 100 ppm by mass and not more than 500 ppm by mass by preparing the electrolyte solution in a dry box. Furthermore, when the amount of the electrolyte solution prepared is 500 L or more and 1000 L or less on an industrial scale, the water concentration of the electrolyte solution before pre-electrolysis is 0.2 mass% or more and 1.0 mass% or less.

[0031] [Pre-electrolysis] As will be described later in the section on Examples, pre-electrolysis is performed on an electrolytic solution as a preliminary step to main electrolysis, which is electrolysis for producing fluorine gas. Studies were conducted to determine under what conditions pre-electrolysis can be performed in a stable manner in which the electrolysis voltage is unlikely to increase.

[0032] The interior of the electrolytic cell where electrolysis takes place is divided by a partition wall into an anode chamber containing an anode and a cathode chamber containing a cathode. Sixteen amorphous carbon electrodes (30 cm wide, 45 cm long, and 5 cm thick) manufactured by SGL Carbon are installed as anodes, and nickel (Ni) punched plates are installed as cathodes. The electrolytic cell is made of mild steel, as it is electrically connected to the cathode and cathodically protected. The partition wall separating the anode chamber and cathode chamber is also made of nickel.

[0033] 560 L of an electrolyte (molten salt) prepared by mixing 434 kg of hydrogen fluoride and 630 kg of potassium fluoride was placed inside the electrolytic cell. The anode and cathode were then immersed in the electrolyte. The electrolysis temperature was controlled to 85 to 95°C. Hydrogen fluoride could be intermittently supplied to the electrolyte in the electrolytic cell so that the hydrogen fluoride concentration in the electrolyte was 39 to 42% by mass. Furthermore, before the start of electrolysis, the electrolyte was sampled from the electrolytic cell, and the water concentration of the electrolyte was measured using the method described above, which was found to be 0.8% by mass.

[0034] The temperature of the electrolyte was set to 85°C, and a constant current was applied to two of the 16 amorphous carbon electrodes. When the current was gradually increased, the current reached 250 A (current density 0.072 A / cm 2 ), the electrolysis voltage exceeded 12 V, so electrolysis was stopped. The amount of current flowing at this time was 1.3 kAh. From this result, it was confirmed that when the water concentration of the electrolyte solution was 0.8 mass %, stable electrolysis could not be performed at a high current density, and that dehydration of the electrolyte solution was necessary before the main electrolysis.

[0035] The concentration of carbon dioxide in the anode gas (fluorine gas) generated by this electrolysis was measured with an FT-IR analyzer and found to be 3,800 ppm by volume. Since oxygen gas (O2) is generated when water in the electrolyte is electrolyzed, the concentration of oxygen gas could be tracked, but because it is difficult to accurately analyze oxygen gas in fluorine gas, the concentration of carbon dioxide (CO2) was tracked instead of oxygen gas.

[0036] The temperature of the electrolyte was set to 85°C, and a current of 875 A (current density 0.036 A / cm) was applied to the remaining 14 amorphous carbon electrodes that were not electrified. 2 A constant current of 30 kAh was applied for 34 hours. The carbon dioxide concentration in the anode gas generated by this electrolysis was measured using an FT-IR analyzer and found to be 130 ppm by volume. The water concentration of the sampled electrolyte was 400 ppm by mass.

[0037] The 14 amorphous carbon electrodes were subsequently used, and the current was gradually increased to 2625 A (current density 0.108 A / cm2 ) was applied, and electrolysis was performed with the temperature of the electrolyte at 85° C. The electrolysis voltage at this time was 9 V, and after 300 hours of continued electrolysis, the electrolysis voltage gradually increased and reached 12 V, so the electrolysis was stopped.

[0038] The electrolyte and electrodes in this electrolytic cell were replaced with new ones. The water concentration of the electrolyte sampled from the electrolytic cell before the start of electrolysis was 0.75% by mass. The temperature of the electrolyte was set to 85°C, and a current of 1000 A (current density 0.036 A / cm) was applied to 16 amorphous carbon electrodes. 2 A constant current of 100 kAh was applied for 100 hours to perform 100 kAh pre-electrolysis. The carbon dioxide concentration in the anode gas generated by this pre-electrolysis was measured using an FT-IR analyzer and found to be 50 ppm by volume or less. In addition, the water concentration of the electrolyte sampled after pre-electrolysis had decreased to 100 ppm by mass or less.

[0039] Following the preliminary electrolysis, the main electrolysis was carried out, and the applied constant current was gradually increased to 3000 A, and the current density was set to 0.108 A / cm 2 The electrolysis voltage at this time was 9 V. After 1000 hours of continued electrolysis, the electrolysis voltage began to gradually increase and reached 12 V, so the electrolysis was stopped.

[0040] It was speculated that the cause of this voltage increase was the use of the amorphous carbon electrodes in the main electrolysis, which were also used in the dehydration electrolysis (pre-electrolysis), which involves electrolysis at a low current density.When an electrolyte with a high water concentration is electrolyzed, an oxide film is formed on the carbon surface of the amorphous carbon electrode, and this film is thought to affect the main electrolysis.

[0041] Therefore, the electrolyte and amorphous carbon electrodes in the electrolytic cell were replaced with new ones. The water concentration of the electrolyte sampled from the electrolytic cell before the start of electrolysis was 0.72 mass%. Two of the 16 amorphous carbon electrodes were used for pre-electrolysis. The temperature of the electrolyte was set to 85°C, and a current of 125 A (current density 0.036 A / cm) was applied to the two amorphous carbon electrodes. 2A constant current of 100 kAh was applied for 800 hours to perform 100 kAh pre-electrolysis. The carbon dioxide concentration in the anode gas generated by this pre-electrolysis was measured using an FT-IR analyzer and found to be 50 ppm by volume or less. In addition, the water concentration of the electrolyte sampled after pre-electrolysis had decreased to 100 ppm by mass or less.

[0042] Using 14 amorphous carbon electrodes not used in the pre-electrolysis, the electrolysis was carried out following the pre-electrolysis, and the applied constant current was gradually increased to 3000 A, and the current density was set to 0.108 A / cm 2 The temperature of the electrolytic solution was 85° C. The electrolysis voltage at the start of electrolysis was 9 V. After 1000 hours of continued electrolysis, the electrolysis voltage was 10.5 V, and the electrolysis voltage did not increase to 12 V.

[0043] Analysis of the behavior of the carbon dioxide concentration in the anode gas and the water concentration in the electrolyte during dehydration electrolysis showed that the logarithm of the carbon dioxide concentration and the logarithm of the water concentration had a good linear relationship with the logarithm of the amount of current applied. When the type of electrolyte was KF·2HF and the amount was 560 L, if the water concentration of the electrolyte before electrolysis was 0.7 to 0.8 mass%, electrolysis at 100 kAh resulted in a current density of 0.036 A / cm. 2 During electrolysis at this temperature, the carbon dioxide concentration in the anode gas becomes 50 ppm by volume or less, and the water concentration in the electrolyte decreases to 100 ppm by mass or less.

[0044] If the water concentration of the electrolyte solution is reduced to 100 ppm by mass or less, the increase in electrolysis voltage can be suppressed even when new amorphous carbon electrodes are used, and therefore pre-electrolysis can be defined as electrolysis in which the water concentration of the electrolyte solution is reduced to 100 ppm by mass or less. The amount of current applied in pre-electrolysis varies depending on the amount of water contained in the initial electrolyte solution and the amount of electrolyte solution.

[0045] [Alkali Metal Hexafluoronickel(IV)] Alkali metal hexafluoronickel(IV) reacts with water, so when alkali metal hexafluoronickel(IV) is added to an electrolyte, the water in the electrolyte is decomposed, and the water concentration of the electrolyte is reduced.

[0046] Furthermore, the products produced by the reaction of alkali metal hexafluoronickel(IV) with water are oxygen gas and nickel fluoride, which do not inhibit the electrolysis of the electrolyte. Therefore, the method for producing fluorine gas according to this embodiment can efficiently produce fluorine gas.

[0047] Furthermore, hydrogen chloride (HCl), hydrogen bromide (HBr), hydrogen iodide (HI), etc. are not produced by the reaction of alkali metal hexafluoronickel(IV) with water, and therefore chlorine molecules (Cl), bromine molecules (Br), iodine molecules (I), etc. are unlikely to be produced by electrolysis. Therefore, the fluorine gas produced by the fluorine gas production method according to this embodiment has few impurities and is highly pure.

[0048] The type of alkali metal hexafluoronickelate (IV) is not particularly limited, but examples include potassium hexafluoronickelate (IV) (KNiF), cesium hexafluoronickelate (IV) (CsNiF), and rubidium hexafluoronickelate (IV) (RbNiF). One type of alkali metal hexafluoronickelate (IV) may be used alone, or two or more types may be used in combination.

[0049] Potassium hexafluoronickel(IV) dissolves quickly in KF·2HF, with a high solubility of approximately 3000 mass ppm. Therefore, water can be removed from the electrolyte in a short time. Furthermore, cesium hexafluoronickel(IV) and rubidium hexafluoronickel(IV) have relatively large molecular weights, so they require a relatively large amount to be added to the electrolyte. However, potassium hexafluoronickel(IV) has a relatively small molecular weight, so its amount can be kept relatively small.

[0050] Instead of alkali metal hexafluoronickel(IV), a metal fluoride complex of a metal other than nickel can be used to decompose water in the electrolyte. For example, alkali metal hexafluoromanganate(IV) such as potassium hexafluoromanganate(IV) (KMnF) or alkali metal hexafluorocobaltate(IV) such as potassium hexafluorocobaltate(IV) (KCoF) can also be used.

[0051] Furthermore, even if a metal fluoride such as antimony trifluoride (SbF), silver difluoride (AgF), or cobalt trifluoride (CoF) is used instead of an alkali metal hexafluoronickel(IV), water in the electrolyte can be decomposed in the same manner as when an alkali metal hexafluoronickel(IV) is used.

[0052] The amount of alkali metal hexafluoronickelate (IV) to be added to a mixture containing hydrogen fluoride and an inorganic fluoride varies depending on the amount of water contained in the mixture, and it is preferable to add alkali metal hexafluoronickelate (IV) in a number of moles that is 1 to 1.2 times the number of moles of water contained in the mixture.

[0053] In general, the amount of alkali metal hexafluoronickel(IV) to be added to a mixture containing hydrogen fluoride and an inorganic fluoride is preferably 100 ppm by mass or more and 10% by mass or less, more preferably 300 ppm by mass or more and 9% by mass or less, and even more preferably 600 ppm by mass or more and 8% by mass or less, of the mass of the mixture.

[0054] The timing for adding the alkali metal hexafluoronickel(IV) acid salt to the mixture containing hydrogen fluoride and inorganic fluoride is not particularly limited, but it is preferable to charge the mixture into an electrolytic cell, measure the water concentration, add the alkali metal hexafluoronickel(IV) acid salt in an amount according to the measurement result, dehydrate the mixture, and then start electrolysis.

[0055] The alkali metal hexafluoronickel(IV) salt may be commercially available or prepared by mixing potassium fluoride, cesium fluoride, or rubidium fluoride with nickel fluoride (NiF) in a molar ratio of 2:1 and treating the mixture at a temperature of 250° C. to 450° C. in a fluorine gas atmosphere.

[0056] [Electrolytic Cell] There are no particular limitations on the type of electrolytic cell used in the method for producing an electrolytic solution according to this embodiment, and any electrolytic cell can be used as long as it can electrolyze the electrolytic solution to generate fluorine gas or nitrogen trifluoride (hereinafter, sometimes referred to as "fluorine gas, etc.") Since the electrolytic solution is corrosive, the parts of the electrolytic cell that come into contact with the electrolytic solution, such as the inner surface, are preferably made of a metal such as iron (Fe), nickel, or Monel (trademark).

[0057] If the components constituting the electrolytic cell and immersed in the electrolytic solution contain iron, which is a source of iron ions, or copper (Cu), which is a source of copper ions, they will dissolve in the electrolytic solution unless they are cathodic protected. Therefore, it is preferable not to use materials containing iron or copper for the components constituting the electrolytic cell and immersed in the electrolytic solution. If cathodic protection is provided, there is no particular problem. Typically, the interior of the electrolytic cell is divided by a partition member such as a partition wall into an anode chamber in which an anode is disposed and a cathode chamber in which a cathode is disposed, so that fluorine gas, etc. generated at the anode and hydrogen gas (H2) generated at the cathode do not mix.

[0058] The anode may be a carbonaceous electrode made of a carbon material such as diamond, diamond-like carbon, amorphous carbon, graphite, or glassy carbon. In addition to the carbonaceous electrodes, the anode may also be a nickel electrode made of nickel, a copper-nickel alloy (e.g., Monel™), or a metal electrode made of other metals. The cathode may be a metal electrode made of iron, nickel, copper, a copper-nickel alloy (e.g., Monel™), or a metal.

[0059] The present invention will be described in more detail below with reference to examples and comparative examples. [Comparative Example 1] The interior of the electrolytic cell is partitioned by a partition wall into an anode chamber containing an anode and a cathode chamber containing a cathode. Sixteen amorphous carbon electrodes (30 cm wide, 45 cm long, and 5 cm thick) manufactured by SGL Carbon Co., Ltd. are installed as anodes, and nickel punched plates are installed as cathodes. The electrolytic cell is electrically connected to the cathode for cathodic protection, and is therefore made of mild steel. The partition wall separating the anode chamber and cathode chamber is also made of nickel.

[0060] 560 L of an electrolyte (molten salt) prepared by mixing 217 kg of hydrogen fluoride and 847 kg of acidic potassium fluoride (KF HF) was placed inside the electrolytic cell. The anode and cathode were then immersed in the electrolyte. The electrolysis temperature was controlled to 85 to 95°C. Before the start of electrolysis, the electrolyte was sampled from the electrolytic cell, and the water concentration of the electrolyte was measured using the method described above, which was 0.8% by mass. Electrolysis was performed while intermittently supplying hydrogen fluoride to the electrolyte in the electrolytic cell so that the hydrogen fluoride concentration of the electrolyte during electrolysis was 39% by mass or more and 42% by mass or less.

[0061] First, the temperature of the electrolyte was set to 85°C, and the current density was set to 0.036 A / cm 2 Electrolysis was initiated by applying a constant current of 1,000 A to all 16 amorphous carbon electrodes and the cathode at 1000 kA, and pre-electrolysis (dehydration electrolysis) was performed for 100 hours until the cumulative current flow reached 100 kAh. This pre-electrolysis reduced the carbon dioxide concentration in the anode gas to 50 ppm by volume or less, and the water concentration in the electrolyte to 100 ppm by mass or less.

[0062] Next, the electrolysis (production of fluorine gas) was carried out following the pre-electrolysis. That is, the applied constant current was gradually increased to 3000 A, and the current density was 0.108 A / cm. 2 The electrolysis voltage at this time was 9 V. After 1000 hours of continued electrolysis, the electrolysis voltage began to gradually increase and reached 12 V, so the electrolysis was stopped.

[0063] [Comparative Example 2] An electrolytic cell and an electrolytic solution similar to those in Comparative Example 1 were prepared. The water concentration of the electrolytic solution before the start of pre-electrolysis was 0.75 mass %. The temperature of the electrolytic solution was 85°C, and the current density was 0.036 A / cm 2 Electrolysis was initiated by applying a constant current of 125 A to two of the 16 amorphous carbon electrodes and the cathode, and pre-electrolysis (dehydration electrolysis) was performed for 800 hours until the cumulative current flow reached 100 kAh. This pre-electrolysis reduced the carbon dioxide concentration in the anode gas to 50 ppm by volume or less, and the water concentration in the electrolyte to 100 ppm by mass or less.

[0064] Next, the pre-electrolysis was followed by the main electrolysis (production of fluorine gas). That is, the temperature of the electrolytic solution was set to 85°C, and a current was applied to the 14 amorphous carbon electrodes and the cathode that had not been used in the pre-electrolysis. The applied constant current was gradually increased to 2625 A, and the current density was set to 0.108 A / cm. 2 The electrolysis voltage at this time was 9 V. After continuing the electrolysis for 1000 hours, the electrolysis voltage was 10.5 V.

[0065] [Comparative Example 3] An electrolytic cell and an electrolytic solution similar to those in Comparative Example 1 were prepared. The water concentration of the electrolytic solution before the start of pre-electrolysis was 0.7 mass %. The temperature of the electrolytic solution was 85°C, and the current density was 0.036 A / cm 2 Electrolysis was initiated by applying a constant current of 125 A to two of the 16 amorphous carbon electrodes and the cathode, and pre-electrolysis (dehydration electrolysis) was carried out for 240 hours until the cumulative current flow reached 30 kAh. This pre-electrolysis reduced the carbon dioxide concentration in the anode gas to 140 ppm by volume and the water concentration in the electrolyte to 430 ppm by mass.

[0066] Next, the pre-electrolysis was followed by the main electrolysis (production of fluorine gas). That is, the temperature of the electrolytic solution was set to 85°C, and a current was applied to the 14 amorphous carbon electrodes and the cathode that had not been used in the pre-electrolysis. The applied constant current was gradually increased to 2625 A, and the current density was set to 0.108 A / cm. 2 The electrolysis voltage at this time was 9 V. After 340 hours of continued electrolysis, the electrolysis voltage reached 12 V, so the electrolysis was stopped.

[0067] Comparative Example 4 The interior of the electrolytic cell was partitioned by a partition wall into an anode chamber containing an anode and a cathode chamber containing a cathode. An amorphous carbon electrode (1 cm wide, 1 cm long) manufactured by SGL Carbon was installed as the anode, and a nickel plate (5 cm wide, 5 cm long) was installed as the cathode. The electrolytic cell was made of Teflon (registered trademark). The partition wall separating the anode chamber and the cathode chamber was also made of Teflon (registered trademark).

[0068] In a glove box filled with nitrogen gas having a dew point of −80° C. or lower, 434 g of hydrogen fluoride and 630 g of potassium fluoride were mixed to prepare 0.56 L of an electrolyte solution. The prepared electrolyte solution was then placed in the electrolytic cell installed in the glove box, and the anode and cathode were immersed in the electrolyte solution.

[0069] The electrolysis temperature was controlled at 85 to 95°C. Before the start of electrolysis, the electrolyte solution was sampled from the electrolytic cell, and the water concentration of the electrolyte solution was measured by the above-mentioned method, which was found to be 200 ppm by mass. Electrolysis was performed while intermittently supplying hydrogen fluoride to the electrolyte solution in the electrolytic cell so that the hydrogen fluoride concentration of the electrolyte solution during electrolysis was 39% by mass or more and 42% by mass or less.

[0070] The temperature of the electrolyte was 85°C, and the current density was 0.025 A / cm 2 A constant current was applied to the amorphous carbon electrode and the cathode to start electrolysis, and the current density of the applied current was increased to 0.025 A / cm every 15 minutes. 2 The current density was increased to 0.225 A / cm 2 The electrolysis voltage rose sharply at

[0071] Example 1 An electrolytic cell and electrolytic solution similar to those in Comparative Example 1 were prepared. The water concentration of the electrolytic solution before the start of electrolysis was 0.7% by mass. Since the amount of water contained in the electrolytic solution was 413 mol, an equimolar amount of potassium hexafluoronickelate (IV), i.e., 104 kg of potassium hexafluoronickelate (IV), was added to the electrolytic cell. The amount of potassium hexafluoronickelate added was 9.7% by mass of the mass of the mixture of hydrogen fluoride and potassium fluoride.

[0072] The electrolyte solution thus prepared was left to stand overnight, and the water concentration of the electrolyte solution was measured. The temperature of the electrolyte solution was set to 85°C, and the current density was set to 0.108 A / cm. 2 Electrolysis was performed by applying a constant current of 3000 A to all 16 amorphous carbon electrodes and the cathode at 1000 Hz. The electrolysis voltage at this time was 9 V. After continuing the electrolysis for 1000 hours, the electrolysis voltage was 10 V.

[0073] [Example 2] An electrolytic cell and an electrolytic solution similar to those in Comparative Example 1 were prepared. The water concentration of the electrolytic solution before the start of pre-electrolysis was 0.75 mass %. The temperature of the electrolytic solution was 85°C, and the current density was 0.036 A / cm 2 Electrolysis was initiated by applying a constant current of 125 A to two of the 16 amorphous carbon electrodes and the cathode, and pre-electrolysis (dehydration electrolysis) was carried out for 240 hours until the cumulative current flow reached 30 kAh. This pre-electrolysis reduced the carbon dioxide concentration in the anode gas to 120 ppm by volume, and the water concentration in the electrolyte to 390 ppm by mass.

[0074] Since the amount of water contained in the electrolytic solution after the preliminary electrolysis was 23 mol, an equimolar amount of potassium hexafluoronickel(IV), i.e., 5.8 kg of potassium hexafluoronickel(IV), was added to the electrolytic cell. The amount of potassium hexafluoronickel(IV) added was 0.54 mass% of the mass of the mixture of hydrogen fluoride and potassium fluoride. After leaving the electrolytic solution prepared in this manner overnight, the water concentration of the electrolytic solution was measured and found to have decreased to 100 mass ppm or less.

[0075] Next, the pre-electrolysis was followed by the main electrolysis (production of fluorine gas). That is, the temperature of the electrolytic solution was set to 85°C, and a current was applied to the 14 amorphous carbon electrodes and the cathode that had not been used in the pre-electrolysis. The applied constant current was gradually increased to 2625 A, and the current density was set to 0.108 A / cm. 2 The electrolysis voltage at this time was 9 V. After continuing the electrolysis for 1000 hours, the electrolysis voltage was 10.2 V.

[0076] Example 3 An electrolytic cell and electrolytic solution similar to those in Comparative Example 4 were prepared. The water concentration of the electrolytic solution before the start of electrolysis was 200 ppm by mass. Since the amount of water contained in the electrolytic solution was 0.0118 mol, an equimolar amount of potassium hexafluoronickelate (IV), i.e., 3.0 g of potassium hexafluoronickelate (IV), was added to the electrolytic cell. The amount of potassium hexafluoronickelate added was 0.28% by mass of the mixture of hydrogen fluoride and potassium fluoride.

[0077] The electrolyte solution thus prepared was left to stand overnight, and the water concentration of the electrolyte solution was measured. The temperature of the electrolyte solution was set to 85°C, and the current density was set to 0.225 A / cm. 2 Electrolysis was performed by applying a constant current of 6250 A to the amorphous carbon electrode and the cathode at 1000 V. Electrolysis was performed while intermittently supplying hydrogen fluoride to the electrolyte in the electrolytic cell so that the hydrogen fluoride concentration in the electrolyte during electrolysis was 39% by mass or more and 42% by mass or less. The electrolysis voltage at this time was 9.3 V. Electrolysis was continued for 100 hours, but the electrolysis voltage did not increase.

[0078] Example 4 360 g of gaseous hydrogen fluoride was blown into 1,140 g of cesium fluoride contained in a 1 L Teflon (registered trademark) container to make the total amount 1,500 g. The water concentration of the mixture thus obtained was measured and found to be 350 ppm by mass.

[0079] Since the amount of water contained in this mixture was 0.0291 mol, an equimolar amount of cesium hexafluoronickel(IV), i.e., 12.8 g of cesium hexafluoronickel(IV), was added to the container. The amount of cesium hexafluoronickel(IV) added was 0.85 mass% of the mass of the mixture of hydrogen fluoride and cesium fluoride. After leaving the electrolyte solution prepared in this way overnight, the water concentration of the electrolyte solution was measured and found to have decreased to 100 mass ppm or less.

Claims

1. A method for producing an electrolyte for generating fluorine gas by electrolysis using a carbonaceous electrode as an anode, comprising a dehydration step of adding an alkali metal salt of hexafluoronickel(IV) to a mixture containing hydrogen fluoride and an inorganic fluoride and having a water concentration of more than 100 ppm by mass and not more than 1% by mass, thereby reducing the water concentration to 100 ppm by mass or less.

2. The method for producing an electrolyte solution according to claim 1, wherein the alkali metal hexafluoronickelate (IV) is at least one of potassium hexafluoronickelate (IV), cesium hexafluoronickelate (IV), and rubidium hexafluoronickelate (IV).

3. The method for producing an electrolyte solution according to claim 1, wherein the inorganic fluoride is at least one of potassium fluoride, cesium fluoride, rubidium fluoride, and ammonium fluoride.

4. The method for producing an electrolyte solution according to claim 1, wherein the amount of the alkali metal salt of hexafluoronickel (IV) acid added is 100 ppm by mass or more and 10% by mass or less of the mass of the mixture.

5. A method for producing fluorine gas, comprising an electrolysis step of electrolyzing the electrolyte produced by the method for producing an electrolyte according to any one of claims 1 to 4 in an electrolytic cell using an anode and a cathode to generate fluorine gas.

6. The method for producing fluorine gas according to claim 5, wherein the anode is a carbonaceous electrode having at least one of graphite, glassy carbon and amorphous carbon.

Citation Information

Patent Citations

  • Dewatering process of fluorine hydride

    CN101423194A

  • Method of electrolytically synthesizing nitrogen trifluoride

    JP2010018849A

  • Anode for electrolytic synthesis and method for manufacturing fluorine gas or fluorine-containing compound

    WO2020026854A1