Method for manufacturing anode for fluorine gas electrolytic synthesis
The anode effect in fluorine gas electrolysis is mitigated by depositing nickel fluoride on the anode surface through anodic polarization in a hydrogen fluoride and potassium hexafluoronicelate solution, ensuring stable and cost-effective fluorine gas production.
Patent Information
- Application Number
- PCT/JP2024/009408
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-31
AI Technical Summary
The anode effect, characterized by increased anode voltage and decreased current flow, occurs during fluorine gas electrolysis using a carbon electrode due to the formation of graphite fluoride, leading to unstable electrolysis processes.
An anode manufacturing method involving anodic polarization of a carbon-based anode in a solution containing hydrogen fluoride, metal fluoride, and potassium hexafluoronicelate (IV), which deposits nickel fluoride on the anode surface, reducing the occurrence of the anode effect by preventing graphite fluoride formation.
This method significantly reduces the frequency of anode effect occurrences, allowing for stable and high-current-density fluorine gas electrolysis, thereby lowering the manufacturing cost of fluorine gas.
Smart Images

Figure JP2024009408_31102024_PF_FP_ABST
Abstract
Description
Method for manufacturing anode for electrolytic synthesis of fluorine gas
[0001] The present invention relates to a method for producing an anode for electrolytic synthesis of fluorine gas.
[0002] Fluorine gas can be synthesized by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride. When electrolytically synthesizing fluorine gas, it has been common to use KF·2HF (a mixed molten salt of hydrogen fluoride and potassium fluoride, in which the molar ratio of hydrogen fluoride to potassium fluoride in the mixed molten salt is hydrogen fluoride:potassium fluoride=2:1) as the electrolyte solution and to use a carbon electrode as the anode, and to perform electrolysis at an electrolysis temperature of 80° C. to 100° C.
[0003] However, when a carbon electrode is used as an anode, a phenomenon in which the anode voltage increases during electrolysis and current flow decreases (hereinafter, sometimes referred to as the "anode effect") is likely to occur, which may prevent stable electrolysis from being performed continuously for a long period of time. This anode effect occurs when a discharge reaction of fluoride ions occurs on the surface of a carbon electrode, resulting in the formation of graphite fluoride ((CF)n) or the like, which has extremely low surface energy, on the surface of the carbon electrode, thereby making it difficult for the electrolyte to come into contact with the surface of the carbon electrode and reducing current flow. Patent Document 1 discloses an electrode in which a metal fluoride is supported in the pores of porous carbon as a carbon electrode that suppresses the anode effect. Patent Document 2 also discloses a technology in which a film containing a nickel potassium fluoride compound is coated on the surface of a carbon electrode to inhibit the formation of graphite fluoride.
[0004] Japanese Patent Publication No. 3037464 Japanese Patent Publication No. 5772102
[0005] There has been a demand for a technology for more sufficiently suppressing the occurrence of the anode effect when electrolysis of an electrolyte solution is performed using a carbon electrode as the anode. An object of the present invention is to provide a method for producing an anode that is less likely to cause the anode effect even when used in electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride to electrolyze fluorine gas.
[0006] In order to solve the above problems, one aspect of the present invention is as follows: [1] to [8]. [1] A method for producing an anode usable in electrolytically synthesizing fluorine gas by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride, the method comprising an anodizing step of immersing an anode base material having a carbon material as an anode and a cathode in an anode-producing mixed solution containing hydrogen fluoride, the anode base material containing hydrogen fluoride, and potassium hexafluoronickel(IV), and passing a current between the anode and the cathode to anodize the anode base material and cause nickel fluoride to adhere to the surface of the anode base material.
[0007] [2] The method for producing an anode for electrolytic synthesis of fluorine gas according to [1], wherein the concentration of potassium hexafluoronickelate (IV) in the anode production mixture is 500 ppm by mass or more and 5,000 ppm by mass or less. [3] In the anodization treatment, an anode current density is 0.01 A / cm 2 0.8A / cm or more 2 or less, and the amount of current per unit surface area of the anode substrate is 100 coulombs / cm 2 More than 5000 coulombs / cm 2 The method for producing an anode for electrolytic synthesis of fluorine gas according to [1] or [2] below.
[0008] [4] The method for producing an anode for electrolytic synthesis of fluorine gas according to any one of [1] to [3], wherein the nickel fluoride has nickel ions with a valence greater than 2. [5] The method for producing an anode for electrolytic synthesis of fluorine gas according to any one of [1] to [3], wherein the nickel fluoride is at least one of nickel trifluoride, nickel pentafluoride, and nickel tetrafluoride.
[0009] [6] The method for producing an anode for electrolytic synthesis of fluorine gas according to any one of [1] to [5], wherein the metal fluoride is at least one of potassium fluoride and cesium fluoride. [7] The method for producing an anode for electrolytic synthesis of fluorine gas according to any one of [1] to [6], wherein the ratio of the molar amount of the hydrogen fluoride to the molar amount of the metal fluoride contained in the anode production mixture is 1.6 or more and 3.2 or less. [8] The method for producing an anode for electrolytic synthesis of fluorine gas according to any one of [1] to [7], wherein the cathode is an electrode formed of at least one of iron, nickel, copper, and a copper-nickel alloy.
[0010] According to the present invention, it is possible to manufacture an anode that is less susceptible to the anode effect even when used in electrolytic synthesis of fluorine gas by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride.
[0011] 1 is a diagram illustrating an example of an electrolytic cell capable of carrying out the method for producing an anode for electrolytic synthesis of fluorine gas according to the present embodiment. FIG. 2 is a diagram illustrating a cyclic voltammogram obtained by cyclic voltammetry.
[0012] An embodiment of the present invention will be described below. Note that this embodiment is merely an example of the present invention, and the present invention is not limited to this embodiment. Furthermore, various modifications and improvements can be made to this embodiment, and such modifications and improvements can also be included in the present invention.
[0013] The method for producing an anode for electrolytic synthesis of fluorine gas according to this embodiment is a method for producing an anode usable for electrolytically synthesizing fluorine gas (F) by electrolyzing an electrolyte solution containing hydrogen fluoride (HF) and a metal fluoride, and includes an anodizing step in which an anode base material having a carbon material is immersed as an anode and a cathode in an anode-producing mixed solution containing hydrogen fluoride, the metal fluoride, and potassium hexafluoronickel(IV) (KNiF), and an electric current is passed between the anode (anode base material) and the cathode to anodize the anode base material and deposit nickel fluoride on the surface of the anode base material.
[0014] An anode manufactured by the method for manufacturing an anode for fluorine gas electrolytic synthesis according to this embodiment (hereinafter sometimes referred to as "anode for fluorine gas electrolytic synthesis according to this embodiment") has nickel fluoride attached to the surface of the anode base material by being anodized in the anodization treatment (for example, a nickel fluoride coating is formed on the surface of the anode base material). Therefore, the anode for fluorine gas electrolytic synthesis according to this embodiment is less likely to produce the anode effect even when used in electrolyzing fluorine gas by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride.
[0015] For example, when electrolytically synthesizing fluorine gas by electrolyzing an electrolyte (e.g., KF·2HF) containing hydrogen fluoride and a metal fluoride but not potassium hexafluoronickelate (IV), if the anode for electrolytic synthesis of fluorine gas according to this embodiment is used, the anode current density can be reduced to 0.01 A / cm 2 0.8A / cm or more 2 It is possible to perform electrolysis with the anode effect suppressed as described below. As a result, it is possible to reduce the frequency of interruptions or stops in the operation for electrolytic synthesis of fluorine gas, and it is also possible to perform electrolysis at a high current density, thereby reducing the cost of producing fluorine gas.
[0016] Here, the anode effect will be explained. When a carbon anode is anodized in an electrolyte containing hydrogen fluoride and a metal fluoride, fluoride ions (hereinafter referred to as "HF2 - ") occurs, generating fluorine atoms. The generated fluorine atoms couple to produce fluorine gas, but some of the fluorine atoms may bond with the carbon on the carbon anode, forming a water-repellent graphite fluoride film called a (CF)n film on the surface of the carbon anode. As a result, it becomes difficult for the electrolyte to come into contact with the surface of the carbon anode during electrolysis, making it difficult for the discharge reaction of fluoride ions to occur on the surface of the carbon anode. This increases the true current density, causing the anode voltage to rise and the current flow to decrease. This is the mechanism of the anode effect.
[0017] Patent Document 2 discloses a technique for coating the surface of a carbon electrode with a film other than a (CF)n film. That is, this technique involves applying a treatment for coating a nickel potassium fluoride compound-containing film to an electrode having a structure in which a part of the surface of a carbon substrate is coated with a conductive diamond layer and the other part is not coated with the conductive diamond layer, and coating only the surface not coated with the conductive diamond layer with the nickel potassium fluoride compound-containing film.
[0018] The surface of the carbon substrate is coated with a conductive diamond layer and a film containing a nickel potassium fluoride compound, such as potassium hexafluoronickelate (IV) (KNiF), making it difficult for a (CF)n coating to form on the surface.
[0019] Patent Document 2 describes the conditions for forming a nickel potassium fluoride compound-containing film, and states that it is preferable to adjust the nickel ion concentration in the electrolyte to 10 ppm to 5%, particularly 30 ppm to 1000 ppm, by adding nickel fluoride to the electrolyte or by dissolving nickel from the material of the electrolytic cell. Furthermore, the electrolysis conditions for the electrolyte include a current density of 0.001 A / cm 2 0.05A / cm or more 2 The electrolysis time is set to 0.1 to 10 hours.
[0020] In Patent Document 2, a current density of 0.05 A / cm 2 It is described that if the electrolysis time is higher than 10 hours, a graphite fluoride layer is likely to be formed before the nickel potassium fluoride compound-containing film is formed, which is undesirable, and that if the electrolysis time is longer than 10 hours, power consumption and productivity decrease, which is undesirable.
[0021] Therefore, as a method for allowing nickel ions to coexist in the electrolyte, a method of adding nickel fluoride (NiF2, molecular weight 96.7 g / mol) to the electrolyte was attempted. 100 g of KF·2HF solution was placed in a Teflon (registered trademark) sealed container housed in a thermostatic bath and maintained at 90°C, and 0.165 g of nickel fluoride powder was added to the KF·2HF solution so that the concentration of nickel (atomic weight 58.7 g / mol) in the KF·2HF solution was 1000 ppm by mass. The solution in the sealed container was then left at 90°C for 36 hours with occasional stirring. After leaving the solution, residual nickel fluoride powder was found at the bottom of the sealed container. After removing the residual nickel fluoride powder, the nickel concentration in the KF·2HF solution was measured by inductively coupled plasma atomic emission spectroscopy (ICP atomic emission spectroscopy), resulting in a concentration of 164 ppm by mass.
[0022] Furthermore, Patent Document 2 describes a method of dissolving nickel from the material of an electrolytic cell as a method of making nickel ions coexist in an electrolyte. If the material of the electrolytic cell is at a potential (a potential greater in the positive direction) than the dissolution potential of nickel (approximately 0.2 to 0.3 V vs. SEP), the nickel forming the electrolytic cell becomes ions and dissolves in the electrolyte.
[0023] To facilitate nickel dissolution, the nickel forming the electrolytic cell was used as the anode, and the KF·2HF electrolyte in the electrolytic cell was electrolyzed at a constant current at 85°C. The mass of the nickel anode was measured periodically during electrolysis to determine the amount of nickel lost. Electrolysis was continued until the amount of nickel lost reached a level where the nickel concentration in the KF·2HF electrolyte was 1,000 ppm by mass due to nickel dissolution. A sludge-like deposit was observed at the bottom of the electrolytic cell. After removing the sludge-like deposit, the nickel concentration in the KF·2HF electrolyte was measured by ICP atomic emission spectroscopy, resulting in a value of 282 ppm by mass.
[0024] As described above, methods for causing nickel ions to coexist in the electrolyte include adding nickel fluoride to the electrolyte and eluting nickel from the material of the electrolytic cell. However, it was found that with these methods, the concentration of nickel dissolved in the electrolyte is limited to approximately 200 to 300 ppm by mass.
[0025] In contrast, potassium hexafluoronickelate (IV) can be dissolved in anhydrous hydrogen fluoride at a concentration of 10% by mass or more. Although there are some variations depending on the temperature, the solubility of potassium hexafluoronickelate (IV) in KF·2HF is approximately 0.5% by mass, and the concentration of dissolved nickel is approximately 1,000 ppm by mass. Therefore, a larger amount of nickel electrolyte (divalent, trivalent, tetravalent nickel ions, etc.) can be dissolved in the KF·2HF electrolytic solution than in the method described in Patent Document 2.
[0026] Using the method of adding nickel fluoride to an electrolyte described in Patent Document 2, nickel fluoride was dissolved in a KF / 2HF solution to 160 ppm by mass, which is close to the saturated solubility, and the critical current density was measured, but it was found that the effect of suppressing the occurrence of the anode effect was poor. Details will be described later in Comparative Example 1. The critical current density is the current density before the electrolysis voltage suddenly rises. Since the phenomenon of the electrolysis voltage suddenly rising corresponds to the anode effect, it can be determined that the higher the critical current density, the less likely the electrode state is to cause the anode effect.
[0027] Next, the properties of the dissolved nickel electrolyte will be described. Patent Document 2 states that "by allowing nickel ions to coexist in the molten salt, the nickel ions form higher-order metal ions...", so it can be interpreted that nickel is dissolved in the electrolyte as divalent nickel ions.
[0028] Considering the mechanism by which potassium hexafluoronickelate (IV) is coated on the electrode in the technology disclosed in Patent Document 2, divalent nickel ions (NiF 2- ) diffuses to the surface of the electrode and reacts with the fluorine gas or fluorine atoms generated on the surface of the electrode, converting the divalent nickel ions into tetravalent nickel ions (NiF6 2-), which then diffuses back to the surface of the electrode. Potassium ions present near the electrode combine with tetravalent nickel ions and are deposited on the surface of the electrode, forming a coating of potassium hexafluoronickelate (IV).
[0029] Since the amount of divalent nickel ions dissolved in the KF·2HF electrolyte is about 200 to 300 ppm by mass, it is easy to predict that the amount of tetravalent nickel ions generated by reaction with fluorine gas or fluorine atoms will be very small. Therefore, it is believed that the formation of a potassium hexafluoronickelate (IV) film hardly occurs with the technology disclosed in Patent Document 2.
[0030] Another possible mechanism is that a discharge reaction of divalent nickel ions on the carbon surface forms a solid nickel fluoride (NiF2), and the nickel fluoride on the carbon surface reacts with the generated fluorine gas to form a high-valent nickel fluoride compound. However, since the reaction between nickel fluoride and fluorine gas to produce nickel tetrafluoride (NiF4) generally requires a high reaction temperature of 250 to 450°C, it is expected that nickel fluoride on the carbon electrode will hardly react with fluorine gas in the electrode reaction.
[0031] Regardless of the reaction route, dissolved divalent nickel ions must interact with fluorine gas produced in the electrode reaction to reach a high valence state, and unless fluorine gas is produced on the electrode, high valence nickel ions cannot be produced. The production of fluorine gas on the electrode surface also results in the formation of a (CF)n film.
[0032] In this embodiment, the properties of the nickel electrolyte dissolved in the anode production mixture are different from those in the technology disclosed in Patent Document 2, and therefore the action on the surface of the carbon electrode is also different. In the method for producing an anode for fluorine gas electrolysis according to this embodiment, the anode base material is anodized in an anode production mixture containing free hexafluoronickel(IV) ions, so that the hexafluoronickel(IV) ions directly react with the surface of the anode base material, regardless of the generation of fluorine gas by the electrode reaction. Therefore, the coating formed on the carbon surface exhibits properties completely different from those in the technology disclosed in Patent Document 2.
[0033] In order to allow free hexafluoronickel(IV) ions to be present in the anode production mixture, it is preferable that the amount of impurities that are easily oxidized in the anode production mixture be small. Examples of impurities that are easily oxidized include water, sulfuric acid derived from the raw materials, and silicon compounds. For example, if water is present in the anode production mixture, the hexafluoronickel(IV) ions oxidize the water, reducing the nickel in the hexafluoronickel(IV) ions to a low valence state, making it difficult to achieve the effects of the present invention.
[0034] In the method for producing an anode for fluorine gas electrolysis according to this embodiment, the anode production mixture contains potassium hexafluoronickel(IV), but a metal fluoride complex salt capable of liberating hexafluoronickel(IV) ions can also be used instead of potassium hexafluoronickel(IV). Examples of such metal fluoride complex salts include cesium hexafluoronickel(IV) and rubidium hexafluoronickel(IV).
[0035] When red crystalline powder potassium hexafluoronickelate (IV) is added to and dissolved in a clear KF·2HF solution, if water is present in the KF·2HF solution, the potassium hexafluoronickelate (IV) reacts with the water, causing the red color of the potassium hexafluoronickelate (IV) to disappear, resulting in a cloudy anode-making mixture. However, if free hexafluoronickel (IV) ions are present in the anode-making mixture, the anode-making mixture changes color from light pink to deep red as the concentration of hexafluoronickel (IV) ions increases. If free hexafluoronickel (IV) ions are not present in the anode-making mixture, the effects of the present invention are unlikely to be achieved.
[0036] The method for producing an anode for electrolytic synthesis of fluorine gas according to this embodiment can be carried out using, for example, an electrolytic cell. Examples of electrolytic cells include electrolytic cells used for electrolyzing fluorine gas by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride. Details will be described in the Examples, but an anode for electrolytic synthesis of fluorine gas according to this embodiment can be produced using, for example, an electrolytic cell made of Teflon as shown in FIG. 1.
[0037] The structure of the Teflon electrolytic cell shown in Fig. 1 will be briefly described. The electrolytic cell shown in Fig. 1 has a body 11 made of Teflon that contains an anode-producing mixed solution 10. The lid 12 of the body 11 is made of a transparent acrylic plate, allowing the color of the anode-producing mixed solution 10 inside the body 11 to be confirmed. A Teflon partition wall 13 is provided inside the electrolytic cell, and this partition wall 13 divides the gas phase inside the electrolytic cell into an anode-side gas phase and a cathode-side gas phase.
[0038] Although not shown in Fig. 1, an inert gas supply pipe is connected to the electrolytic cell for supplying an inert gas into the interior of the electrolytic cell so that the gas phase inside the electrolytic cell can be diluted with an inert gas such as nitrogen gas. Also connected to the electrolytic cell is a hydrogen fluoride supply pipe 31 for supplying hydrogen fluoride into the anode production mixed solution 10 in the main body 11. Furthermore, a fluorine gas extraction pipe 33 and a hydrogen gas extraction pipe 34 are connected to the electrolytic cell for extracting fluorine gas and hydrogen gas generated from the anode 21 and the cathode 22 from the electrolytic cell, respectively.
[0039] The electrolytic cell is further provided with an external heater (not shown) that can heat the anode manufacturing mixture 10 in the main body 11 to a temperature of, for example, 85° C. The electrolytic cell is further provided with a thermometer 32 such as a thermocouple that can measure the temperature of the anode manufacturing mixture 10 in the main body 11. The electrolytic cell is further provided with a stirring device (not shown) that can stir the anode manufacturing mixture 10 in the main body 11.
[0040] Furthermore, the anode manufacturing mixture 10 is a mixture containing hydrogen fluoride, a metal fluoride, and potassium hexafluoronickel(IV), for example, KF·2HF with potassium hexafluoronickel(IV) dissolved therein. The electrolytic cell includes an anode 21 and a cathode 22, both of which are immersed in the anode manufacturing mixture 10. The anode 21 is an anode substrate containing a carbon material, for example, a plate made of amorphous carbon. The cathode 22 is a metal plate made of a metal such as nickel. The electrolytic cell is installed in a dry box, which prevents water from the atmosphere from dissolving into the anode manufacturing mixture 10 in the main body 11.
[0041] [Dehydrated Electrolyte 1 Prepared by Dehydration Electrolysis 1] Using the electrolytic cell shown in Figure 1, dehydration electrolysis was carried out on an electrolyte solution that was a mixture of hydrogen fluoride and potassium fluoride. The anode current density was 0.3 A / cm 2 The electrolysis time was 2 hours. The anode was a conductive diamond electrode coated with conductive diamond. The anode had a square shape of 1 cm long and 1 cm wide.
[0042] Since conductive diamond has carbon bonds of sp3 orbitals, the (CF)n coating formed by the reaction of carbon of sp2 orbitals with fluorine gas is not formed on the surface of the conductive diamond electrode.Therefore, the conductive diamond electrode is an electrode that does not cause the anode effect.Therefore, if a conductive diamond electrode is used, dehydration electrolysis can be performed without causing the anode effect even in an electrolyte containing water.
[0043] The gas generated from the anode was diluted with nitrogen gas, and fluorine gas was absorbed and removed in a potassium iodide aqueous solution trap. The oxygen gas concentration in the gas discharged from the potassium iodide aqueous solution trap was measured by gas chromatography. As no oxygen gas was detected, it was determined that dehydration electrolysis was complete.
[0044] Because hydrogen fluoride is consumed by the electrolysis, hydrogen fluoride was intermittently supplied to the electrolyte during dehydration electrolysis so that the hydrogen fluoride concentration in the electrolyte was in the range of 40 mass % to 43 mass %. This operation is called dehydration electrolysis 1, and the electrolyte prepared by performing dehydration electrolysis 1 is called post-dehydration electrolyte 1.
[0045] [Potassium hexafluoronickel(IV)-added electrode 1] Potassium hexafluoronickel(IV) crystal powder was added to dehydrated electrolyte 1, and the concentration of potassium hexafluoronickel(IV) in dehydrated electrolyte 1 was set to 0.1% by mass. The concentration of nickel in dehydrated electrolyte 1 was 210 ppm by mass. Although potassium hexafluoronickel(IV) reacted slightly when potassium hexafluoronickel(IV) was added, all of the potassium hexafluoronickel(IV) crystal powder dissolved, and dehydrated electrolyte 1 assumed a light red color.
[0046] A portion of dehydrated electrolytic solution 1 (corresponding to the anode-producing mixed solution) in which potassium hexafluoronickel(IV) was dissolved was sampled, and the nickel concentration in dehydrated electrolytic solution 1 was measured by ICP atomic emission spectrometry. As a result, it was confirmed that the same amount of nickel as the added amount had dissolved.
[0047] A square carbon electrode (corresponding to an anode substrate) measuring 1 cm in length and 1 cm in width was immersed as an anode, and a metal cathode was also immersed in the dehydrated electrolyte 1 containing dissolved potassium hexafluoronickel (IV). A current of 0.1 A was then passed between the anode and cathode for 1 hour, thereby performing a surface treatment of the carbon electrode (corresponding to an anodization treatment).
[0048] The amount of current per unit surface area of the carbon electrode in this surface treatment was 360 coulombs / cm 2 The carbon electrode used was a brand new (unused for electrolysis) ABR grade electrode manufactured by SGL Carbon. The carbon electrode subjected to such a surface treatment is referred to as potassium hexafluoronickelate (IV)-added electrode 1. Unless otherwise specified, the "carbon electrode" hereinafter refers to a brand new (unused for electrolysis) ABR grade electrode manufactured by SGL Carbon.
[0049] [Patent Document 2 Retest Electrode 1] A rectangular nickel plate measuring 2 cm in length and 3 cm in width was immersed as an anode, and a metal cathode was also immersed in dehydrated electrolyte 1. Then, electrolysis was performed by passing a current of 0.6 A between the anode and cathode for 16 hours, and nickel was eluted from the nickel plate into dehydrated electrolyte 1. After electrolysis, dehydrated electrolyte 1 was pale yellow-green in color.
[0050] From the mass loss of the nickel plate, the nickel concentration in the dehydrated electrolyte 1 from which nickel had been eluted was calculated to be 1000 ppm by mass. However, a precipitate had formed in the dehydrated electrolyte 1 from which nickel had been eluted. When the nickel concentration in the dehydrated electrolyte 1 containing no precipitate was measured by ICP atomic emission spectroscopy, it was found to be 220 ppm by mass.
[0051] A square carbon electrode measuring 1 cm in length and 1 cm in width was immersed as an anode in the dehydrated electrolytic solution 1 into which nickel had been eluted, and a metal cathode was also immersed. Electrolysis was then performed by passing a current of 25 mA between the anode and cathode for 3 hours. This electrolysis resulted in the formation of a nickel potassium fluoride film on the surface of the carbon electrode. The amount of current per unit surface area of the carbon electrode during this electrolysis was 270 coulombs / cm.2 The current density in this electrolysis was 0.0025 A / cm 2 The carbon electrode on which the nickel potassium fluoride film was formed in this manner is the electrode described in Patent Document 2, and therefore this carbon electrode is referred to as Patent Document 2 Retest Electrode 1.
[0052] [Patent Document 2 Supplementary Test Electrode 2] A rectangular nickel plate measuring 2 cm in length and 3 cm in width was immersed as an anode in dehydrated electrolyte 1, and a metal cathode was also immersed. Electrolysis was performed by passing a current of 1 A between the anode and cathode for 26 hours, and nickel was eluted from the nickel plate into dehydrated electrolyte 1. After electrolysis, dehydrated electrolyte 1 was pale yellow-green (slightly greener than the color of dehydrated electrolyte 1 in the case of Patent Document 2 Supplementary Test Electrode 1).
[0053] From the mass loss of the nickel plate, the nickel concentration in the dehydrated electrolyte 1 from which nickel had been eluted was calculated to be 2700 ppm by mass. However, a precipitate had formed in the dehydrated electrolyte 1 from which nickel had been eluted. When the nickel concentration in the dehydrated electrolyte 1 containing no precipitate was measured by ICP atomic emission spectroscopy, it was found to be 280 ppm by mass.
[0054] A square carbon electrode measuring 1 cm in length and 1 cm in width was immersed as an anode in the dehydrated electrolytic solution 1 into which nickel had been eluted, and a metal cathode was also immersed. Electrolysis was then performed by passing a current of 25 mA between the anode and cathode for 3 hours. This electrolysis resulted in the formation of a nickel potassium fluoride film on the surface of the carbon electrode. The amount of current per unit surface area of the carbon electrode during this electrolysis was 270 coulombs / cm. 2 The current density in this electrolysis was 0.0025 A / cm 2 The carbon electrode on which the nickel potassium fluoride film was formed in this manner is the electrode described in Patent Document 2, and therefore this carbon electrode is referred to as Patent Document 2 Retest Electrode 2.
[0055] [Measurement of blank critical current density] A square carbon electrode measuring 1 cm in length and 1 cm in width was immersed as an anode and a metal cathode in the dehydrated electrolyte 1, and the critical current density was measured. Hereinafter, the critical current density measured by this method is referred to as the blank critical current density, and represents the critical current density when the electrode is not subjected to any treatment.
[0056] The critical current density was measured as follows: a direct current of 25 mA was first passed between the anode and cathode for 15 minutes, and then a direct current of 50 mA was passed for 15 minutes. The current was then increased by 25 mA every 15 minutes, and the current density before the electrolysis voltage suddenly increased was taken as the critical current density.
[0057] Since the phenomenon of a sudden rise in electrolysis voltage corresponds to the anode effect, it can be determined that the higher the critical current density, the less likely the electrode is to experience the anode effect. Unless otherwise specified, the critical current densities shown below are values obtained using this measurement method. After measuring the critical current density, remove the anode from the electrolytic cell.
[0058] Using the above measurement method, the critical current density (blank critical current density) of dehydrated electrolyte 1 containing no nickel ion species was measured. The carbon electrodes used in this measurement were unused for critical current density measurement or electrolysis. The carbon electrodes were replaced with new ones six times, and the critical current density was measured six times. The average value of these measurements was 0.29 A / cm. 2 The maximum value is 0.35 A / cm 2 The minimum value is 0.225 A / cm 2 It was.
[0059] [Measurement of critical current density of treated electrode] A method for measuring the critical current density of an anode produced by the method for producing an anode for electrolytic synthesis of fluorine gas according to this embodiment, without removing the anode from the anode production mixture used during production, is called critical current density measurement method A.
[0060] Furthermore, a method of measuring the critical current density by removing the anode manufactured by the manufacturing method for a fluorine gas electrolytic synthesis anode according to this embodiment from the anode manufacturing mixed solution used during manufacturing, and immersing it in dehydrated electrolyte 1 to which no nickel electrolyte has been added or in dehydrated electrolyte 1 to which no nickel electrolyte is present, is called critical current density measurement method B. The critical current density of the potassium hexafluoronickelate (IV)-added electrode 1 described above was measured by critical current density measurement method A. As a result, the critical current density was 0.575 A / cm 2 It was.
[0061] Furthermore, the potassium hexafluoronickelate (IV) added electrode 1 was produced twice, and the critical current density of each electrode was measured by the critical current density measurement method A. As a result, the critical current density was 0.575 A / cm 2 and 0.675 A / cm 2 As described above, the critical current density of the potassium hexafluoronickelate (IV) added electrode 1 was 2 to 3 times higher than the above-mentioned blank critical current density.
[0062] Next, the critical current density of the potassium hexafluoronickel(IV)-added electrode 1 was measured by critical current density measurement method B. That is, the potassium hexafluoronickel(IV)-added electrode 1 was removed from the anode-producing mixed solution used in producing the potassium hexafluoronickel(IV)-added electrode 1. Then, after dehydration, electrolytic solution 1 was prepared in another electrolytic cell having exactly the same structure as the electrolytic cell used in producing the potassium hexafluoronickel(IV)-added electrode 1, and the removed potassium hexafluoronickel(IV)-added electrode 1 was attached to the other electrolytic cell to measure the critical current density.
[0063] The measured critical current density was 0.550 A / cm 2 Therefore, it can be said that the surface-modified state of the potassium hexafluoronickelate (IV) added electrode 1 was maintained. The above-described series of electrode replacement operations were carried out in a glove box under a water-free nitrogen atmosphere.
[0064] Next, the critical current densities of supplementary test electrode 1 and supplementary test electrode 2 of Patent Document 2 were measured by critical current density measurement method A. The critical current density of supplementary test electrode 1 of Patent Document 2 was 0.300 A / cm 2 The color of the electrolyte remained light yellow-green and did not change, so it cannot be said that hexafluoronickel (IV) ions were present.
[0065] The critical current density of the retest electrode 2 in Patent Document 2 is 0.350 A / cm 2 The color of the electrolyte remained a light yellow-green and did not change, which does not indicate the presence of hexafluoronickel (IV) ions. The critical current densities of Patent Document 2 supplementary test electrode 1 and Patent Document 2 supplementary test electrode 2 were slightly higher than the average blank critical current density, but did not exceed the maximum blank critical current density.
[0066] As described above, it is clear that the anode manufactured by the method for manufacturing an anode for electrolytic synthesis of fluorine gas according to this embodiment is extremely unlikely to cause the anode effect. The mechanism by which this anode effect is suppressed is not clear, but it is expected that the presence of a fluorinating agent on the surface of the electrode is related to this.
[0067] The method for producing an anode for electrolytic synthesis of fluorine gas according to this embodiment will be described in more detail below. An example of an apparatus for carrying out the method for producing an anode for electrolytic synthesis of fluorine gas according to this embodiment is an electrolytic cell used for the electrolytic synthesis of fluorine gas. There are no particular limitations on the form of this electrolytic cell, and any electrolytic cell can be used as long as it is capable of electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride to generate fluorine gas.
[0068] Typically, the interior of an electrolytic cell is partitioned by a partition member such as a partition wall into an anode chamber in which an anode is placed and a cathode chamber in which a cathode is placed, so that fluorine gas generated at the anode and hydrogen gas generated at the cathode do not mix. Although the interior of an electrolytic cell is partitioned into an anode chamber in which an anode is placed and a cathode chamber in which a cathode is placed, the anode-producing mixed solution contained in the anode chamber and the anode-producing mixed solution contained in the cathode chamber are not isolated, and the anode-producing mixed solution contained in both chambers is often configured to be able to mix freely.
[0069] When the interior of the electrolytic cell has a structure that allows the anode production mixed solution contained in both the anode chambers to be freely mixed, potassium hexafluoronickelate (IV) may be contained in either the anode production mixed solution contained in the anode chamber or the anode production mixed solution contained in the cathode chamber.
[0070] The anode may be a carbonaceous electrode made of a carbon material such as diamond, diamond-like carbon, amorphous carbon, graphite, or glassy carbon, while the cathode may be a metal electrode made of a metal such as iron (Fe), nickel (Ni), copper (Cu), or a copper-nickel alloy (e.g., Monel (trademark)).
[0071] The anode-producing mixed solution contains hydrogen fluoride, a metal fluoride, and potassium hexafluoronickel(IV). The type of metal fluoride is not particularly limited, but an alkali metal fluoride is preferred, and at least one of potassium fluoride (KF) and cesium fluoride (CsF) is more preferred. One type of metal fluoride may be used alone, or two or more types may be used in combination. That is, potassium fluoride and cesium fluoride may be used in combination as the metal fluoride.
[0072] The ratio of the molar amount of hydrogen fluoride to the molar amount of metal fluoride contained in the anode-producing mixed solution ([molar amount of hydrogen fluoride] / [molar amount of metal fluoride]) is preferably 1.6 or more and 3.2 or less, and more preferably 1.9 or more and 3.0 or less. As the anode-producing mixed solution, for example, a solution obtained by dissolving potassium hexafluoronickelate (IV) in a mixed molten salt of hydrogen fluoride and potassium fluoride can be used. The molar ratio of hydrogen fluoride to potassium fluoride in the mixed molten salt of hydrogen fluoride and potassium fluoride can be, for example, hydrogen fluoride:potassium fluoride = 1.5 to 2.5:1. A typical mixed molten salt is KF·2HF with a hydrogen fluoride:potassium fluoride ratio of 2:1, and the melting point of this mixed molten salt is approximately 72°C.
[0073] Another example of a mixed solution for producing an anode is a mixed molten salt of hydrogen fluoride and cesium fluoride in which potassium hexafluoronickelate (IV) is dissolved. The molar ratio of hydrogen fluoride to cesium fluoride in the mixed molten salt of hydrogen fluoride and cesium fluoride can be, for example, hydrogen fluoride:cesium fluoride = 1.8 to 3.1:1. A typical mixed molten salt is CsF·2.4HF in which the ratio of hydrogen fluoride to cesium fluoride is 2.4:1, and the melting point of this mixed molten salt is approximately 16°C.
[0074] Because this anode-making mixed solution is corrosive, the inner surface of the electrolytic cell and other parts that come into contact with the anode-making mixed solution are preferably made of a metal such as iron, nickel, or Monel (trademark). Because the hydrogen fluoride in the anode-making mixed solution is consumed by electrolysis during anode production, it is preferable to supply hydrogen fluoride continuously or intermittently to the anode-making mixed solution, for example, during electrolysis during anode production. Hydrogen fluoride may be supplied to the anode-making mixed solution on the cathode chamber side of the electrolytic cell, or to the anode-making mixed solution on the anode chamber side.
[0075] When the hydrogen fluoride concentration in anode-production mixed solution is defined as a reference concentration by using KF·2HF (hydrogen fluoride concentration: 40.4 mass %) or CsF·2.4HF (hydrogen fluoride concentration: 24.0 mass %) as the mixed molten salt used in the anode-production mixed solution, the hydrogen fluoride concentration in the anode-production mixed solution is preferably controlled so that its fluctuation falls within a range of −5 mass % or more and +5 mass % or less of the reference concentration, more preferably controlled so that its fluctuation falls within a range of −2.5 mass % or more and +2.5 mass % or less of the reference concentration, and even more preferably controlled so that its fluctuation falls within a range of −1.5 mass % or more and +1.5 mass % or less of the reference concentration.
[0076] The anode-producing mixture can be obtained by mixing hydrogen fluoride, a metal fluoride, and potassium hexafluoronickelate (IV) (KNiF). Potassium hexafluoronickelate (IV) may be commercially available or prepared. Potassium hexafluoronickelate (IV) can be prepared by mixing potassium fluoride and nickel fluoride (NiF) in a molar ratio of 2:1 and treating the mixture at a temperature of 250°C to 450°C in a fluorine gas atmosphere.
[0077] Because potassium hexafluoronickelate(IV) is an oxidizing solid, it reacts with water to convert to potassium fluoride salt of trivalent nickel (KNiF) or potassium fluoride salt of divalent nickel (KNiF). Potassium pentafluoronickelate(III) (KNiF) and potassium tetrafluoronickelate(II) (KNiF) have lower solubility in the anode manufacturing mixture than potassium hexafluoronickelate(IV). Therefore, it is preferable to use potassium hexafluoronickelate(IV) with a low water content. The water content of potassium hexafluoronickelate(IV) is preferably 0.5% by mass or less, and more preferably 0.3% by mass or less.
[0078] The method for adding potassium hexafluoronickel(IV) to the anode-producing mixture is not particularly limited. Alternatively, the anode-producing mixture may be prepared by mixing a metal fluoride with liquid hydrogen fluoride in which potassium hexafluoronickel(IV) has been dissolved, or by mixing solid potassium hexafluoronickel(IV) with a mixture of hydrogen fluoride and a metal fluoride. Furthermore, a predetermined amount of potassium hexafluoronickel(IV) may be added all at once, or may be added in portions. The concentration of potassium hexafluoronickel(IV) in the anode-producing mixture is preferably 500 ppm by mass or more and 5000 ppm by mass or less, and more preferably 1000 ppm by mass or more and 4000 ppm by mass or less.
[0079] The anode production mixture may contain potassium hexafluoronickel(IV) in an amount exceeding the saturated solubility. If the anode production mixture contains potassium hexafluoronickel(IV) in an amount exceeding the saturated solubility, undissolved potassium hexafluoronickel(IV) solids will accumulate at the bottom of the electrolytic cell. However, when the method for producing an anode for fluorine gas electrolysis according to this embodiment is implemented, the nickel electrolyte in the anode production mixture becomes nickel fluoride and adheres to the surface of the anode base material, resulting in a decrease in the concentration of nickel electrolyte in the anode production mixture. If the anode production mixture contains potassium hexafluoronickel(IV) in an amount exceeding the saturated solubility, the undissolved potassium hexafluoronickel(IV) solids will dissolve as the nickel electrolyte concentration decreases, thereby maintaining the saturated solubility.
[0080] In the method for producing an anode for electrolytic synthesis of fluorine gas according to this embodiment, an electric current is passed between the anode (anode substrate) and the cathode to anodize the anode substrate, and nickel fluoride is deposited on the surface of the anode substrate. In this anodization, the anode current density is set to 0.01 A / cm 2 0.8A / cm or more 2 It is preferable that the current flow per unit surface area of the anode substrate is 100 coulombs / cm or less. 2 More than 5000 coulombs / cm 2 It is preferable that:
[0081] Anode current density is 0.01 A / cm 2 Even if the anode current density is less than 0.8 A / cm, there is no particular problem, and this can be addressed by extending the treatment time of the anodization treatment. 2 If the voltage is made larger, the anodization treatment can be completed in a short time, but if an increase in voltage is confirmed during the anodization treatment, it is preferable to take measures such as quickly stopping the supply of current to prevent the anode effect from occurring.
[0082] The anode current density was 0.05 A / cm 2 Excess 0.6A / cm 2It is more preferable that the anode current density is equal to or less than 1000 kJ / cm2. The anode current density may be a constant value, or may be gradually increased from a low value or gradually decreased from a high value. The method for changing the anode current density is not particularly limited.
[0083] The amount of current per unit surface area of the anode substrate is an important value because it is related to the amount of nickel fluoride that functions as a catalyst deposited on the surface of the anode substrate. The amount of current per unit surface area of the anode substrate is 100 coulombs / cm 2 Preferably, it is 5000 coulombs / cm or more. 2 Although there is no particular problem if the anode substrate is larger than this, the processing time for the anodization treatment will be longer. 2 More preferably, it is equal to or greater than this.
[0084] It is preferable to adjust the amount of current passed per unit surface area of the anode base material depending on the concentration of potassium hexafluoronickel(IV) in the anode-producing mixed solution. However, the amount of current passed may be increased when the concentration of potassium hexafluoronickel(IV) is low, and decreased when the concentration of potassium hexafluoronickel(IV) is high.
[0085] The concentration of nickel electrolyte (IV) ions in the anode production mixture during anodization can be measured by ICP atomic emission spectroscopy. To liberate hexafluoronickel (IV) ions in the anode production mixture, it is desirable that the amount of easily oxidizable impurities present in the anode production mixture be small. In particular, a small amount of water in the mixed molten salt before the addition of potassium hexafluoronickel (IV) is preferred, since this allows for a smaller amount of potassium hexafluoronickel (IV) to be added.
[0086] When removing water from the mixed molten salt by electrolysis (dehydration electrolysis), water can be removed by electrolysis using electrodes such as conductive diamond electrodes, nickel electrodes, carbon electrodes, etc. When removing water from the mixed molten salt by electrolysis using carbon electrodes, the carbon electrodes used for dehydration electrolysis can be used as the anode substrate in the method for producing an anode for fluorine gas electrolysis according to this embodiment. In this case, since a (CF)n coating is formed on the surface of the carbon electrode during dehydration electrolysis, the effect of anodization in the presence of hexafluoronickel(IV) ions is smaller than when a new carbon electrode is used, but it is not completely ineffective.
[0087] In the method for producing an anode for fluorine gas electrolysis according to this embodiment, a current is passed between the anode and the cathode to anodize the anode substrate, thereby depositing nickel fluoride on the surface of the anode substrate, and examples of this nickel fluoride include nickel fluorides having nickel ions with a valence greater than 2. Examples include at least one of nickel trifluoride (NiF), dinickel pentafluoride (NiF), and nickel tetrafluoride (NiF).
[0088] The present invention will be explained in more detail below with reference to examples and comparative examples. [Comparative Example 1] An anode for electrolytic synthesis of fluorine gas was manufactured using the Teflon electrolytic cell shown in Figure 1 described above. KF.2HF was used as the electrolyte, and 750 g of KF.2HF was placed in the body of the electrolytic cell. The electrolyte was heated to 85°C, and the anode and cathode were immersed in it. The cathode was a square nickel plate measuring 5 cm in length and 5 cm in width. The anode was a square diamond electrode measuring 1 cm in length and 1 cm in width, with a conductive diamond coating on its surface.
[0089] A current was passed between the anode and the cathode to perform dehydration electrolysis of the electrolyte. The anode current density was 0.3 A / cm 2The electrolysis time was 2 hours. The gas generated from the anode was diluted with nitrogen gas, and fluorine gas was absorbed and removed in a potassium iodide aqueous solution trap. The oxygen gas concentration in the gas discharged from the potassium iodide aqueous solution trap was measured by gas chromatography. As a result, no oxygen gas was detected, so it was determined that dehydration electrolysis was complete.
[0090] Since hydrogen fluoride in the electrolyte solution is consumed by the dehydration electrolysis, hydrogen fluoride was intermittently supplied to the electrolyte solution during the dehydration electrolysis so that the hydrogen fluoride concentration in the electrolyte solution was within the range of 40% by mass to 43% by mass. The electrolyte solution prepared by such an operation is referred to as post-dehydration electrolyte solution 1.
[0091] Next, 0.2 g of nickel fluoride was added to and dissolved in the dehydrated electrolytic solution 1 in the electrolytic cell. The concentration of nickel fluoride in the dehydrated electrolytic solution 1 was 270 ppm by mass, and the amount of nickel dissolved was 160 ppm by mass. The amount of nickel fluoride added was determined by measuring in advance the amount of nickel fluoride dissolved in KF 2HF at 85°C (details will be described later).
[0092] The color of the dehydrated electrolyte 1 in which nickel fluoride was dissolved was transparent. The nickel concentration in the dehydrated electrolyte 1 was also measured by ICP atomic emission spectroscopy, and the result was the same as that described above. A new carbon electrode was immersed as an anode in the dehydrated electrolyte 1 in which nickel fluoride was dissolved, and electrolysis was performed by passing a current of 25 mA between the anode and cathode for 3 hours. This electrolysis resulted in the formation of a nickel potassium fluoride film, as described in Patent Document 2, on the surface of the carbon electrode. This carbon electrode was a square with a length of 1 cm and a width of 1 cm. The anode current density in this electrolysis was 0.0025 A / cm 2 The current flow per unit surface area of the carbon electrode is 270 coulombs / cm 2 is.
[0093] Here, the method for measuring the amount of dissolved nickel fluoride described above will be explained. 100 g of KF·2HF was placed in a sealable Teflon container, a predetermined amount of nickel fluoride powder was added thereto, the container was sealed, and the container was left in a thermostatic chamber at 85°C for 36 hours. However, the contents of the container were occasionally stirred. After leaving it for 36 hours, the contents of the container were visually observed to confirm whether or not any nickel fluoride powder remained dissolved.
[0094] The solubility of nickel fluoride powder was investigated by varying the amount of nickel fluoride powder added. When nickel fluoride powder was added in an amount equivalent to or less than 320 ppm by mass, no residual nickel was observed. In contrast, when nickel fluoride powder was added in an amount greater than 320 ppm by mass, residual nickel was observed. After removing the residual nickel fluoride powder, the nickel concentration in KF-2HF was measured by ICP atomic emission spectroscopy, and the maximum nickel concentration was 200 ppm by mass.
[0095] [Comparative Example 2] The critical current density of the anode of Comparative Example 1 was measured in the electrolyte of Comparative Example 1 by Critical Current Density Measurement Method A, and was found to be 0.25 A / cm 2 This critical current density is within the range of the critical current density obtained in the blank experiment described above, so it cannot be said that the anode effect is suppressed. Furthermore, the color of the electrolyte does not indicate the presence of hexafluoronickel(IV) ions.
[0096] [Comparative Example 3] After the critical current density measurement in Comparative Example 2 was completed, the anode was removed from the electrolyte and, without washing with water, heated to 300°C using a high-temperature inert gas flow to volatilize the hydrogen fluoride component adsorbed on the carbon electrode. Thereafter, energy dispersive X-ray analysis was performed using a JEOL Ltd. JCM-7000 tabletop scanning electron microscope to confirm the presence of nickel on the surface of the carbon electrode, but nickel was not confirmed because it was below the detection limit.
[0097] Comparative Example 4 Dehydrated electrolyte 1 obtained in the same manner as in Comparative Example 1 was placed in the electrolytic cell shown in Fig. 1 , and an anode and a cathode were immersed in dehydrated electrolyte 1. The anode was a rectangular nickel plate measuring 2 cm in length and 3 cm in width, and the cathode was a nickel plate. Electrolysis was performed by passing a current of 1 A between the anode and cathode for 26 hours, and nickel was eluted from the nickel plate into dehydrated electrolyte 1.
[0098] From the mass loss of the nickel plate used as the anode, the nickel concentration in the dehydrated electrolyte 1 was calculated to be 2800 ppm by mass, but a precipitate was generated in the dehydrated electrolyte 1. When the nickel concentration in the dehydrated electrolyte 1 not containing the precipitate was measured by ICP atomic emission spectroscopy, it was 270 ppm by mass. The dehydrated electrolyte 1 after electrolysis was pale yellow-green in color.
[0099] After dehydration, the nickel was dissolved and a new carbon electrode was immersed as an anode in the electrolytic solution 1, and a current of 25 mA was passed between the anode and cathode for 10 hours to perform electrolysis. This electrolysis resulted in the formation of a nickel potassium fluoride film, as described in Patent Document 2, on the surface of the carbon electrode. This carbon electrode was a square, 1 cm long and 1 cm wide. The anode current density during this electrolysis was 0.0025 A / cm 2 The current flow per unit surface area of the carbon electrode is 900 coulombs / cm 2 is.
[0100] The carbon electrode on which the potassium nickel fluoride film was formed was dehydrated, removed from the electrolytic solution 1, and without washing with water, heated to 300°C in an inert gas to volatilize the hydrogen fluoride adsorbed on the carbon electrode. Thereafter, the presence of nickel on the surface of the carbon electrode was confirmed in the same manner as in Comparative Example 3, but nickel could not be confirmed because it was below the detection limit.
[0101] Comparative Example 5: Dehydrated electrolyte 1 obtained in the same manner as in Comparative Example 1 was placed in the electrolytic cell shown in FIG. 1, and nickel fluoride was added and dissolved therein. An anode was then immersed in dehydrated electrolyte 1 with nickel fluoride dissolved therein. This anode was a square carbon electrode measuring 1 cm in length and 1 cm in width. This carbon electrode was formed from highly oriented pyrolytic graphite (HOPG ZYH manufactured by Momentive) having a basal plane.
[0102] Cyclic voltammetry was then performed using Ni / NiF as the reference electrode, and a cyclic voltammogram was obtained. The potential scan rate was 0.4 mV / sec. The first run of the obtained cyclic voltammogram is shown in Figure 2. As can be seen from Figure 2, the current peaked at a potential near 5.5 V vs. Ni / NiF, and the current dropped sharply at potentials above that. This behavior corresponds to the anodic effect.
[0103] Comparative Example 6: Dehydrated electrolyte solution 1 obtained in the same manner as in Comparative Example 1 was placed in the electrolytic cell shown in Figure 1, and lithium fluoride (LiF) powder was added and dissolved therein. Lithium fluoride is an additive that is thought to be effective in suppressing the anode effect. The concentration of lithium fluoride in dehydrated electrolyte solution 1 was set to 1.0 mass%.
[0104] A new carbon electrode was immersed as an anode in this dehydrated electrolyte 1 containing dissolved lithium fluoride, and electrolysis was performed by passing a current of 0.05 A between the anode and cathode for 5 hours. This electrolysis resulted in a surface treatment of the carbon electrode. The carbon electrode was a square with a length of 1 cm and a width of 1 cm. The amount of current per unit surface area of the carbon electrode during this electrolysis was 900 coulombs / cm. 2 During the electrolysis, the dehydrated electrolyte 1 was stirred with a stirrer to prevent the lithium fluoride from settling.
[0105] After the surface treatment by electrolysis was completed, the critical current density was measured. That is, a direct current of 25 mA was first applied between the anode and the cathode for 15 minutes, and then the current was increased by 25 mA every 15 minutes. The current density before the electrolysis voltage suddenly increased was taken as the critical current density. As a result, the critical current density was 0.275 A / cm.2 It was.
[0106] The same procedure was repeated to measure the critical current density, which was 0.30 A / cm 2 These results show that the addition of lithium fluoride cannot suppress the anodic effect.
[0107] Comparative Example 7 Dehydrated electrolyte 1 obtained in the same manner as in Comparative Example 1 was placed in the electrolytic cell of Fig. 1, and potassium hexafluoronickel (IV) crystal powder was added and dissolved therein. The concentration of potassium hexafluoronickel (IV) in dehydrated electrolyte 1 was 0.3 mass%, and the amount of dissolved nickel was 630 mass ppm. Dehydrated electrolyte 1 after dissolution of potassium hexafluoronickel (IV) was red.
[0108] A new square carbon electrode measuring 1 cm in length and 1 cm in width was immersed as an anode in dehydrated electrolyte 1 containing dissolved potassium hexafluoronickelate (IV), and a metal cathode was also immersed in the electrolyte, and the anode was left for 6 hours without passing a current. The critical current density of the anode was then measured by critical current density measurement method B. The result was that the critical current density was 0.250 A / cm. 2 From this result, it can be seen that the effect of suppressing the anode effect cannot be obtained by simply immersing the carbon electrode in dehydrated electrolyte 1 in which potassium hexafluoronickelate (IV) has been dissolved.
[0109] Example 1 Dehydrated electrolyte 1 obtained in the same manner as in Comparative Example 1 was placed in the electrolytic cell shown in Figure 1, and potassium hexafluoronickel (IV) crystal powder was added and dissolved therein. The concentration of potassium hexafluoronickel (IV) in dehydrated electrolyte 1 was 0.3 mass%, and the amount of dissolved nickel was 630 mass ppm. Dehydrated electrolyte 1 after dissolution of potassium hexafluoronickel (IV) was red.
[0110] A dehydrated electrolytic solution 1 containing dissolved potassium hexafluoronickelate (IV) was used as an anode-producing mixture. A new carbon electrode was immersed in this anode-producing mixture as an anode (anode substrate), and a metal cathode was also immersed. Then, electrolysis was performed by passing a current of 0.1 A between the anode and the cathode for 6 hours. Through this electrolysis, nickel fluoride was formed on the surface of the carbon electrode, which was the anode substrate, to produce an anode for fluorine gas electrolysis. This carbon electrode was a square, 1 cm long and 1 cm wide. The anode current density during this electrolysis was 0.1 A / cm 2 The current per unit surface area of the carbon electrode is 2160 coulombs / cm 2 is.
[0111] The critical current density of the obtained anode for electrolytic synthesis of fluorine gas was measured by the critical current density measurement method A. The measurement was carried out twice, and the critical current density was 0.875 A / cm 2 and 0.825 A / cm 2 Table 1 shows the manufacturing conditions of the anode for electrolytic synthesis of fluorine gas and the measurement results of the critical current density.
[0112] Examples 2 to 4 Anodes for the electrolytic synthesis of fluorine gas were produced in the same manner as in Example 1, except that the concentration of potassium hexafluoronickelate (IV) in the dehydrated electrolytic solution 1, the time of electrolysis (pretreatment), and the amount of current applied during electrolysis were changed as shown in Table 1. The critical current density of the resulting anodes for the electrolytic synthesis of fluorine gas was measured by critical current density measurement method A. Each measurement was performed once. The production conditions for the anodes for the electrolytic synthesis of fluorine gas and the measurement results of the critical current density are summarized in Table 1.
[0113]
[0114] The results shown in Table 1 show that the critical current density tends to increase as the amount of dissolved potassium hexafluoronickelate (IV) increases, but the increase in critical current density roughly saturates at a concentration of 5,000 ppm by mass. Furthermore, the results of Examples 2 and 3 show that the critical current density increases as the amount of current applied during electrolysis increases, and that the critical current density increases significantly more than the blank critical current density.
[0115] Example 5 The anode for which the critical current density of Example 4 was measured was removed from the anode-producing mixture and heated to 300°C in an inert gas to volatilize the hydrogen fluoride adsorbed on the carbon electrode. Thereafter, the presence of nickel on the surface of the carbon electrode was confirmed in the same manner as in Comparative Example 3.
[0116] Example 6: Dehydrated electrolyte 1 obtained in the same manner as in Comparative Example 1 was placed in the electrolytic cell shown in FIG. 1, and potassium hexafluoronickel (IV) crystal powder was added and dissolved therein. The concentration of potassium hexafluoronickel (IV) in dehydrated electrolyte 1 was 0.1% by mass. An anode was then immersed in dehydrated electrolyte 1 with potassium hexafluoronickel (IV) dissolved therein. The anode was a square carbon electrode measuring 1 cm in length and 1 cm in width. The carbon electrode was formed of highly oriented pyrolytic graphite (HOPG ZYH manufactured by Momentive) with a basal plane.
[0117] Cyclic voltammetry was then performed using Ni / NiF as the reference electrode, and a cyclic voltammogram was obtained. The potential scanning rate was 0.4 mV / sec. The first run of the obtained cyclic voltammogram is shown in FIG. 2. As can be seen from FIG. 2, the current peaked at a potential near 5.5 V vs. Ni / NiF, and this peak current value was 2.7 times larger than the peak current value of Comparative Example 5. This result shows that although an anodic effect occurred, the addition of potassium hexafluoronickelate (IV) increased the current value that could be passed before the anodic effect occurred.
[0118] Furthermore, microscopic Raman spectroscopy revealed no difference in the peak intensities of the D and G bands between potassium hexafluoronickelate (IV) and nickel fluoride, suggesting that the amount of intercalation compound inserted remains unchanged between the two. Therefore, the difference in peak current value is thought to be due to the fact that the addition of potassium hexafluoronickelate (IV) causes nickel fluorides with valences higher than divalent to act as catalysts for the fluorine gas production reaction, thereby suppressing the formation of a (CF)n coating on the surface of the carbon electrode.
[0119] Example 7 An anode for electrolytic synthesis of fluorine gas was produced in the same manner as in Example 4. The critical current density of the obtained anode for electrolytic synthesis of fluorine gas was measured by the critical current density measurement method B, and was found to be 0.850 A / cm 2 It was.
[0120] Example 8 Dehydrated electrolyte 1 obtained in the same manner as in Comparative Example 1 was placed in the electrolytic cell of Fig. 1, and potassium hexafluoronickel (IV) crystal powder was added and dissolved therein. The concentration of potassium hexafluoronickel (IV) in dehydrated electrolyte 1 was 0.4 mass%, and the amount of dissolved nickel was 840 mass ppm. Dehydrated electrolyte 1 after dissolution of potassium hexafluoronickel (IV) was red.
[0121] Then, the dehydrated electrolytic solution 1 in which potassium hexafluoronickelate (IV) was dissolved was used as an anode-producing mixture, and a new carbon electrode was immersed as an anode (anode substrate) in this anode-producing mixture, along with a metal cathode. Then, electrolysis was performed by passing a current of 0.3 A between the anode and the cathode for 4.5 hours. Through this electrolysis, nickel fluoride was formed on the surface of the carbon electrode, which was the anode substrate, to produce an anode for fluorine gas electrolysis. This carbon electrode was a square, 1 cm long and 1 cm wide. The anode current density in this electrolysis was 0.3 A / cm 2 The current flow per unit surface area of the carbon electrode is 4860 coulombs / cm 2 is.
[0122] The completed anode for fluorine gas electrolytic synthesis (first anode for fluorine gas electrolytic synthesis) was removed from the electrolytic cell, and a new carbon electrode was immersed as an anode in dehydrated electrolyte 1 in which potassium hexafluoronickelate (IV) had been dissolved, and the same operation as above was carried out to produce an anode for fluorine gas electrolytic synthesis (second anode for fluorine gas electrolytic synthesis). The same operation was further repeated to sequentially produce third to sixth anodes for fluorine gas electrolytic synthesis, for a total of six anodes for fluorine gas electrolytic synthesis.
[0123] After the completed sixth anode for fluorine gas electrolysis was removed from the electrolytic cell, potassium hexafluoronickel (IV) crystal powder was further added and dissolved in the dehydrated electrolytic solution 1. The amount of potassium hexafluoronickel (IV) added was such that the concentration of potassium hexafluoronickel (IV) in the dehydrated electrolytic solution 1 increased by 0.1% by mass.
[0124] A new carbon electrode was immersed as an anode in dehydrated electrolyte 1 containing additional potassium hexafluoronickelate (IV), and electrolysis was performed by passing a current of 0.3 A between the anode and cathode for 4.5 hours. Nickel fluoride was formed on the surface of the carbon electrode, which served as the anode substrate, by this electrolysis, producing the seventh anode for electrolytic synthesis of fluorine gas. This carbon electrode was a square, 1 cm long and 1 cm wide. The anode current density in this electrolysis was 0.3 A / cm. 2 The current flow per unit surface area of the carbon electrode is 4860 coulombs / cm 2 is.
[0125] The critical current density of the seven anodes for fluorine gas electrolytic synthesis produced as described above was measured by critical current density measurement method B. The results are shown in Table 2. As can be seen from the results shown in Table 2, the critical current density of the first to sixth anodes for fluorine gas electrolytic synthesis tended to decrease in the order of production. This is thought to correspond to the gradual decrease in the concentration of hexafluoronickel(IV) ions in electrolyte 1 after dehydration, as the nickel electrolyte of potassium hexafluoronickel(IV) adheres to the surface of the electrode due to electrolysis.
[0126]
[0127] For the seventh anode for fluorine gas electrolysis, the critical current density recovered again. This suggests that the re-addition of potassium hexafluoronickel(IV) increased the concentration of hexafluoronickel(IV) ions in post-dehydration electrolyte 1, and that hexafluoronickel(IV) ions were attached to the surface of the carbon electrode by electrolysis.
[0128] At the time when the production of the sixth anode for fluorine gas electrolysis was completed, the color of the dehydrated electrolyte 1 was lighter than the initial red color but still remained red, which suggests that hexafluoronickel(IV) ions were still present but their concentration had decreased. Example 8 shows that a higher concentration of hexafluoronickel(IV) ions results in more hexafluoronickel(IV) ions adhering to the surface of the carbon electrode.
[0129] 10... Mixed liquid for anode production 11... Main body 13... Partition wall 21... Anode 22... Cathode
Claims
1. A method for producing an anode usable in electrolytically synthesizing fluorine gas by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride, the method comprising the steps of: immersing an anode base material having a carbon material as an anode and a cathode in an anode-producing mixed solution containing hydrogen fluoride, a metal fluoride, and potassium hexafluoronickel (IV), and passing an electric current between the anode and the cathode to anodize the anode base material, thereby depositing nickel fluoride on the surface of the anode base material.
2. The method for producing an anode for electrolytic synthesis of fluorine gas according to claim 1, wherein the concentration of the potassium hexafluoronickelate (IV) in the anode production mixture is 500 ppm by mass or more and 5,000 ppm by mass or less.
3. In the anodization, the anode current density is 0.01 A / cm 2 0.8A / cm or more 2 or less, and the amount of current per unit surface area of the anode substrate is 100 coulombs / cm 2 More than 5000 coulombs / cm 2 3. The method for producing an anode for electrolytic synthesis of fluorine gas according to claim 1 or 2, wherein the anode is:
4. The method for producing an anode for electrolytic synthesis of fluorine gas according to claim 1 or 2, wherein the nickel fluoride has nickel ions with a valence greater than two.
5. A method for producing an anode for electrolytic synthesis of fluorine gas according to claim 1 or 2, wherein the nickel fluoride is at least one of nickel trifluoride, nickel pentafluoride, and nickel tetrafluoride.
6. A method for producing an anode for electrolytic synthesis of fluorine gas according to claim 1 or 2, wherein the metal fluoride is at least one of potassium fluoride and cesium fluoride.
7. A method for producing an anode for electrolytic synthesis of fluorine gas according to claim 1 or 2, wherein the ratio of the molar amount of said hydrogen fluoride to the molar amount of said metal fluoride contained in said anode production mixture is 1.6 or more and 3.2 or less.
8. The method for producing an anode for electrolytic synthesis of fluorine gas according to claim 1 or 2, wherein the cathode is an electrode formed from at least one of iron, nickel, copper, and a copper-nickel alloy.
Citation Information
Patent Citations
Dewatering process of fluorine hydride
CN101423194A
Electrode for electrolytically synthesizing fluorine compound
JP2012193415A
Anode for electrolytic synthesis and method for manufacturing fluorine gas or fluorine-containing compound
WO2020026854A1