Nonaqueous electrolytic solution and nonaqueous electrolyte secondary battery

The non-aqueous electrolyte with phosphorus-containing compounds addresses the degradation issue in batteries by forming a protective film on the positive electrode, enhancing cycle characteristics and safety through reduced oxidative decomposition and solvent vaporization.

WO2024225104A1PCT designated stage expired Publication Date: 2024-10-31PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015049
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-28
Filing Date
2024-04-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional non-aqueous electrolytes in batteries are prone to degradation, leading to increased internal resistance and decreased cycle characteristics due to oxidative decomposition at the electrolyte-positive electrode interface, which affects battery performance and longevity.

Method used

A non-aqueous electrolyte composition featuring a phosphorus-containing compound, such as Li3PO4, Na3PO4, or LiPO3F, insoluble in the solvent, dispersed in a non-aqueous solvent, which forms a protective film on the positive electrode surface, suppressing oxidative decomposition and allowing for self-repair, thereby enhancing cycle characteristics.

Benefits of technology

The proposed electrolyte configuration significantly improves battery cycle characteristics by reducing oxidative decomposition, maintaining performance over time, and ensuring better stability and safety by preventing solvent vaporization and self-heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015049_31102024_PF_FP_ABST
    Figure JP2024015049_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A nonaqueous electrolytic solution according to the present disclosure contains a nonaqueous solvent, an electrolyte dissolved in the nonaqueous solvent, and particles of a phosphorus-containing compound. The particles of the phosphorus-containing compound are insoluble in the nonaqueous solvent. The phosphorus-containing compound contains at least one selected from the group consisting of Li3PO4, Na3PO4, K3PO4, LiPO3, LiPO3F, metaphosphoric acid, and calcium phosphate. The nonaqueous electrolytic solution according to the present disclosure has fluidity at 25°C. A secondary battery 100 according to the present disclosure comprises a positive electrode 5, a negative electrode 6, and a nonaqueous electrolytic solution according to the present disclosure.
Need to check novelty before this filing date? Find Prior Art

Description

Nonaqueous electrolyte and nonaqueous electrolyte secondary battery

[0001] The present disclosure relates to a non-aqueous electrolyte solution and a non-aqueous electrolyte secondary battery.

[0002] As known to those skilled in the art, in conventional batteries, the electrolyte may be decomposed by the active material, which can cause disadvantages such as an increase in the internal resistance of the battery and a decrease in the cycle characteristics of the battery.

[0003] Patent Document 1 discloses a nonaqueous electrolyte secondary battery having a negative electrode and a positive electrode made of either metallic lithium or a non-graphitizable carbon material, and a nonaqueous electrolyte. Patent Document 1 discloses that a nonaqueous electrolyte secondary battery containing vinylene carbonate as a nonaqueous solvent has good cycle characteristics. Patent Document 2 discloses an ion secondary battery comprising a positive electrode made of a composite lithium oxide or composite sodium oxide, a negative electrode made of a material capable of retaining lithium or sodium, a separator, and an electrolyte made of a nonaqueous solvent, the electrolyte containing fluoroethylene carbonate and phosphorus compound particles.

[0004] JP 2005-268230 A JP 2012-018801 A

[0005] The present disclosure provides a nonaqueous electrolyte suitable for improving the cycle characteristics of a battery.

[0006] The non-aqueous electrolyte solution of the present disclosure includes: a non-aqueous solvent; an electrolyte dissolved in the non-aqueous solvent; and particles of a phosphorus-containing compound insoluble in the non-aqueous solvent, wherein the phosphorus-containing compound includes at least one selected from the group consisting of LiPO, NaPO, KPO, LiPO, LiPOF, metaphosphoric acid, and calcium phosphate, and has fluidity at 25°C.

[0007] According to the technology of the present disclosure, the cycle characteristics of the battery can be improved.

[0008] FIG. 1 is a schematic cross-sectional view showing an example of a nonaqueous electrolyte secondary battery according to the second embodiment.

[0009] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. The present disclosure is not limited to the following embodiments.

[0010] (Embodiment 1) The nonaqueous electrolyte solution of embodiment 1 includes a nonaqueous solvent, an electrolyte dissolved in the nonaqueous solvent, and particles of a phosphorus-containing compound insoluble in the nonaqueous solvent. The phosphorus-containing compound includes at least one selected from the group consisting of Li3PO4, Na3PO4, K3PO4, LiPO3, LiPO3F, metaphosphoric acid, and calcium phosphate. The nonaqueous electrolyte solution of embodiment 1 has fluidity at 25°C. When a battery using the nonaqueous electrolyte solution of embodiment 1 is operated, the particles of the phosphorus-containing compound dispersed in the nonaqueous electrolyte solution form a coating on the surface of the positive electrode. This can suppress oxidative decomposition of the solvent at the interface between the nonaqueous electrolyte solution and the positive electrode. Furthermore, even if the coating is damaged over time or due to repeated charge and discharge, the particles of the phosphorus-containing compound dispersed in the nonaqueous electrolyte solution can repair the coating. As a result, the nonaqueous electrolyte solution of the present disclosure can suppress oxidative decomposition of the solvent for a longer period of time than, for example, a battery assembled with a coating formed directly on the positive electrode. As described above, the nonaqueous electrolyte solution of the first embodiment can improve the cycle characteristics of the battery.

[0011] In the present disclosure, "having fluidity at 25°C" means having a viscosity of 20,000 mPa·s or less at 25°C. The nonaqueous electrolyte solution in embodiment 1 does not necessarily have to always have fluidity at 25°C, and may have, for example, thixotropy. For example, "having fluidity at 25°C" also includes a solution that exhibits a viscosity of more than 20,000 mPa·s at 25°C in a static state, but exhibits a viscosity of 20,000 mPa·s or less at 25°C when a force is applied, such as shearing due to stirring.

[0012] The viscosity of the nonaqueous electrolyte solution in embodiment 1 at 25°C may be, for example, 5000 mPa·s or less, 3000 mPa·s or less, or 1000 mPa·s or less. The lower limit of the viscosity of the nonaqueous electrolyte solution in embodiment 1 at 25°C is not particularly limited, and is, for example, 1.0 mPa·s or more. The nonaqueous electrolyte solution in embodiment 1 is, for example, liquid. Liquids also include sols. That is, the nonaqueous electrolyte solution in embodiment 1 may be a nonaqueous colloidal solution in which particles of a phosphorus-containing compound are dispersed.

[0013] In the present disclosure, "particles of a phosphorus-containing compound insoluble in a non-aqueous solvent" refers to particles of a phosphorus-containing compound that require 100 mL or more of non-aqueous solvent to dissolve 1 g at 25°C. That is, the solubility of the particles of the phosphorus-containing compound in 100 mL of non-aqueous solvent is 1 g or less. Here, "dissolution" means that the permeability of the solution obtained when the particles of the phosphorus-containing compound are dissolved in the non-aqueous solvent in a container does not change from the permeability of the solvent, i.e., the solution is not cloudy and no precipitate is observed on the bottom of the container after standing for 24 hours. For example, lithium difluorophosphate (LiPO2F2) is soluble in esters, and when the non-aqueous solvent contains an ester, it is not included in the particles of the phosphorus-containing compound of the present disclosure.

[0014] The particles of the phosphorus-containing compound may have a solubility of 0.1 g or less in 100 mL.

[0015] The calcium phosphate in the particles of the phosphorus-containing compound is, for example, hydroxyapatite.

[0016] The phosphorus-containing compound may include at least one selected from the group consisting of Li3PO4, Na3PO4, K3PO4, LiPO3, LiPO3F, and metaphosphoric acid.

[0017] The phosphorus-containing compound may contain Li3PO4. That is, the nonaqueous electrolyte solution of the present disclosure may contain Li3PO4 particles. According to the above configuration, the cycle characteristics of the battery can be improved.

[0018] In the non-aqueous electrolyte solution of embodiment 1, the content of the phosphorus-containing compound particles may be 0.1 vol% or more and 10 vol% or less. The content of the phosphorus-containing compound particles may be 0.1 vol% or more and 8 vol% or less, 0.5 vol% or more and 6 vol% or less, 1 vol% or more and 5 vol% or less, or 1 vol% or more and 4 vol% or less. The above configuration can improve the dispersibility of the phosphorus-containing compound particles and the fluidity of the non-aqueous electrolyte solution.

[0019] The content ratio of phosphorus-containing compound particles in the nonaqueous electrolyte in embodiment 1 can be determined, for example, by the following method. After measuring the volume of the nonaqueous electrolyte, the nonaqueous electrolyte is filtered to separate the particles. The separated particles are washed with a solvent such as dimethyl carbonate, and the washing solvent is evaporated and dried, after which the mass of the particles is measured. The volume of the particles is calculated from the specific gravity determined from the mass of the particles and the particle components. The particle components can be determined by various analytical methods such as inductively coupled plasma analysis (ICP), X-ray diffraction (XRD), infrared absorption spectroscopy (IR), and nuclear magnetic resonance analysis (NMR). In this way, the content ratio of phosphorus-containing compound particles in the nonaqueous electrolyte can be calculated. The volume of the nonaqueous electrolyte can also be calculated from the composition and mass. The composition of the nonaqueous electrolyte can be measured using a liquid chromatograph, gas chromatograph, etc.

[0020] The average particle diameter of the phosphorus-containing compound particles may be 1 nm or more and 500 nm or less. This configuration improves the dispersibility of the phosphorus-containing compound particles in the nonaqueous electrolyte, thereby enabling increased industrial productivity of the nonaqueous electrolyte. The average particle diameter of the phosphorus-containing compound particles may be 5 nm or more and 400 nm or less, or 10 nm or more and 300 nm or less. When the average particle diameter of the phosphorus-containing compound particles is 500 nm or less, in a battery using the nonaqueous electrolyte of the present disclosure, the phosphorus-containing compound particles may penetrate between the positive electrode active material particles arranged inside the positive electrode active material layer when the nonaqueous electrolyte permeates the positive electrode active material layer. Therefore, a coating of the phosphorus-containing compound is also formed on the surface of the positive electrode active material arranged inside the positive electrode active material layer, thereby suppressing oxidative decomposition of the solvent inside the positive electrode active material layer.

[0021] The average particle size of the particles of the phosphorus-containing compound may be equal to or smaller than the pore size of the separator of a battery using a nonaqueous electrolyte. According to the above configuration, the particles of the phosphorus-containing compound do not clog the pores of the separator, so that circulation of the electrolyte inside the electrode group is not hindered even during charge and discharge.

[0022] In the present disclosure, the average particle size refers to the median diameter (d50). The median diameter is the particle diameter at which the cumulative volume in the volume-based particle size distribution is equal to 50%. The volume-based particle size distribution can be determined by a laser diffraction scattering method using a commercially available laser diffraction measuring device.

[0023] The electrolyte may include, for example, a lithium salt. Examples of lithium salts include lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium perchlorate (LiClO), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bisperfluoroethylsulfonylimide (LiN(SO2C2F5)2), LiAsF6, LiCF3SO3, and lithium difluoro(oxalato)borate. The electrolyte may include at least one selected from the substances listed above as lithium salts. The lithium salt may include fluorine (F). The lithium salt may be LiPF6.

[0024] The concentration of the lithium salt in the nonaqueous electrolyte may be, for example, 0.5 mol / L or more and 2 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte having excellent ionic conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.

[0025] The non-aqueous solvent is not particularly limited, and for example, a cyclic carbonate, a chain carbonate, a cyclic carboxylic acid ester, or the like may be used.

[0026] Examples of the cyclic carbonate include propylene carbonate (PC) and ethylene carbonate (EC).

[0027] Examples of the chain carbonate ester include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC).

[0028] Examples of the cyclic carboxylic acid ester include γ-butyrolactone (GBL) and γ-valerolactone (GVL).

[0029] The nonaqueous solvent may be used alone or in combination of two or more. The nonaqueous solvent may contain ethylene carbonate. This can increase the solubility of an electrolyte such as a lithium salt in the nonaqueous solvent.

[0030] The nonaqueous electrolyte solution in embodiment 1 may further contain other substances than those described above. For example, the nonaqueous electrolyte solution in embodiment 1 may further contain an additive to improve the dispersibility of the phosphorus-containing compound particles. The additive is, for example, a fluorine-containing solvent. That is, the nonaqueous electrolyte solution in embodiment 1 may further contain a fluorine-containing solvent. With the above configuration, it is possible to reduce aggregation of the phosphorus-containing compound particles and the resulting sedimentation of the particles over time.

[0031] The fluorine-containing solvent may include a fluorinated ether, and the fluorinated ether may include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether.

[0032] The fluorine-containing solvent may contain a fluorinated cyclic ester. The fluorinated cyclic ester is a compound obtained by fluorinating a cyclic ester, for example, by substituting one or more hydrogen atoms bonded to a carbon atom constituting the cyclic structure of the cyclic ester with a fluorine atom. Due to the interaction between the fluorinated cyclic ester, the phosphorus-containing compound, and the lithium salt, the nonaqueous electrolyte of the present disclosure has improved dispersion stability, reducing particle aggregation and resulting particle sedimentation over time of the phosphorus-containing compound. A nonaqueous electrolyte with improved particle dispersibility can improve the industrial productivity of the nonaqueous electrolyte and the battery using the same. Furthermore, the nonaqueous electrolyte of embodiment 1 containing the fluorinated cyclic ester may be thixotropic and may gel over time when left standing. Based on the above, batteries containing the nonaqueous electrolyte of the present disclosure have less risk of leakage in the event of damage. Furthermore, the nonaqueous solvent is less likely to volatilize, thereby suppressing electrolyte evaporation and self-heating of the battery. Therefore, the nonaqueous electrolyte of the present disclosure can improve battery safety.

[0033] The number of carbon atoms in the fluorinated cyclic ester may be 3 or more and 10 or less, or 3 or more and 4 or less, or even 3. The fluorinated cyclic ester may include at least one selected from the group consisting of fluoroethylene carbonate, difluoroethylene carbonate, fluoropropylene carbonate, and trifluoropropylene carbonate. The fluorinated cyclic ester may include fluoroethylene carbonate. According to the above configuration, the nonaqueous electrolyte of the present disclosure has improved dispersion stability and can suppress sedimentation of particles of the phosphorus-containing compound. Furthermore, according to the above configuration, the nonaqueous electrolyte exhibits thixotropy, which can improve the safety of the battery.

[0034] The content of the fluorinated cyclic ester may be 0.1% by volume or more and 30% by volume or less relative to the total of the nonaqueous solvent and the fluorinated cyclic ester, 0.5% by volume or more and 30% by volume or less, 1.0% by volume or more and 28.0% by volume or less, 5.0% by volume or more and 25.0% by volume or less, or 10.0% by volume or more and 20.0% by volume or less relative to the total of the nonaqueous solvent and the fluorinated cyclic ester.

[0035] The nonaqueous electrolyte solution in the first embodiment can be produced, for example, by the following method.

[0036] A lithium salt is dissolved in a non-aqueous solvent. The resulting solution is mixed with particles of a phosphorus-containing compound, such as LiPO4 particles, and ZrO2 balls as a mixing medium in a ball mill. The mixing medium is removed from the resulting mixture to obtain the non-aqueous electrolyte solution of embodiment 1.

[0037] The method for producing the non-aqueous electrolyte is not limited to the above, and may be, for example, by dispersing particles of a phosphorus-containing compound in a non-aqueous solvent in which a lithium salt has been dissolved, using an ultrasonic homogenizer.

[0038] (Embodiment 2) A nonaqueous electrolyte secondary battery according to Embodiment 2 includes a positive electrode, a negative electrode, and the nonaqueous electrolyte solution according to Embodiment 1. By using the nonaqueous electrolyte solution according to Embodiment 1, the cycle characteristics of the secondary battery can be improved.

[0039] FIG. 1 is a schematic cross-sectional view showing an example of a nonaqueous electrolyte secondary battery according to Embodiment 2. The secondary battery 100 includes a container 1, an electrode group 4, and an electrolyte solution (not shown). The electrolyte solution is the nonaqueous electrolyte solution of Embodiment 1. The electrode group 4 has a wound structure. The electrode group 4 is housed in the container 1. The electrode group 4 includes a positive electrode 5, a negative electrode 6, and a pair of separators 7. The electrode group 4 is impregnated with the electrolyte solution. The opening of the container 1 is closed with a sealing plate 2. The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material layer 5b. One end of a positive electrode lead 5c is connected to the positive electrode 5. The other end of the positive electrode lead 5c is connected to the back surface of the sealing plate 2. An insulating packing 3 is disposed around the sealing plate 2. The negative electrode 6 includes a negative electrode current collector 6a and a negative electrode active material layer 6b. One end of the negative electrode lead 6c is connected to the negative electrode 6. The other end of the negative electrode lead 6c is connected to the bottom surface of the container 1. An insulating ring 8 is disposed on each of the upper and lower surfaces of the electrode group 4.

[0040] Each component of the secondary battery 100 will be specifically described below.

[0041] The positive electrode current collector 5a can be a sheet or film made of a metal material such as aluminum, stainless steel, titanium, or an alloy thereof. Aluminum and its alloys are suitable materials for the positive electrode current collector 5a because they are inexpensive and easy to form into thin films. The sheet or film may be porous or non-porous. Examples of the sheet or film include metal foil and metal mesh. A carbon material such as carbon may be applied to the surface of the positive electrode current collector 5a as a conductive auxiliary material.

[0042] The positive electrode active material layer 5b includes a positive electrode active material. The positive electrode active material may be a material capable of absorbing and releasing lithium ions. Examples of the positive electrode active material include lithium-containing transition metal oxides, lithium-containing transition metal phosphates, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides, and transition metal oxynitrides. In particular, using a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate as the positive electrode active material can reduce the manufacturing cost of the battery and increase the average discharge voltage. Examples of lithium-containing transition metal oxides include lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, and lithium nickel manganese oxide. Examples of lithium-containing transition metal phosphates include lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, and lithium nickel phosphate.

[0043] The positive electrode active material may contain lithium nickel oxide having a layered rock salt crystal structure. The proportion of Ni among metal elements other than Li contained in the lithium nickel oxide may be 50 atomic % or more. The lithium nickel oxide may also contain other transition metals. The lithium nickel oxide is useful for achieving a high operating voltage.

[0044] The lithium nickel oxide may be represented by the following composition formula (I): Element M1 is at least one selected from the group consisting of V, Co, and Mn. Element M2 is at least one selected from the group consisting of Mg, Al, Ca, Ti, Cu, Zn, and Nb. Composition formula (I) satisfies 0.9≦α≦1.10, −0.05≦β≦0.05, 0.5≦x1<1, 0≦x2≦0.5, and 0<1−x1−x2≦0.5.

[0045] Li α Ni x1 M1 x2 M2 (1-x1-x2) O 2+β ...(I)

[0046] The positive electrode active material layer 5b may contain other materials such as a conductive additive and a binder.

[0047] The conductive additive is used to reduce the resistance of the positive electrode 5. Examples of the conductive additive include a carbon material and a conductive polymer compound. Examples of the carbon material include carbon black, graphite, acetylene black, carbon nanotubes, carbon nanofibers, graphene, fullerene, and graphite oxide. Examples of the conductive polymer compound include polyaniline, polypyrrole, and polythiophene.

[0048] The binder is used to improve the binding property of the material constituting the positive electrode 5. As the binder, polymer materials such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, polytetrafluoroethylene, carboxymethyl cellulose, polyacrylic acid, styrene-butadiene copolymer rubber, polypropylene, polyethylene, and polyimide can be used.

[0049] The negative electrode current collector 6a may be a sheet or film made of a metal material such as stainless steel, nickel, copper, or an alloy thereof. The sheet or film may be porous or non-porous. Examples of the sheet or film include metal foil and metal mesh. A carbon material such as carbon may be applied to the surface of the negative electrode current collector 6a as a conductive auxiliary material.

[0050] The negative electrode active material layer 6b includes a negative electrode active material. The negative electrode active material can be a material capable of absorbing and releasing lithium ions. The negative electrode active material includes, for example, at least one selected from the group consisting of carbon materials and materials capable of forming an alloy with lithium. Examples of carbon materials include graphite. Examples of materials capable of forming an alloy with lithium include silicon, silicon-containing oxides, tin, zinc alloys, bismuth, and germanium. One type selected from these negative electrode active materials may be used, or two or more types may be used in combination.

[0051] The negative electrode active material layer 6b may contain at least one selected from the group consisting of graphite and silicon as the negative electrode active material. The negative electrode active material layer 6b may contain only graphite as the negative electrode active material. Graphite is recommended because it is resistant to deterioration even when repeatedly charged and discharged at a deep depth. Carbon materials other than graphite may also be used as the negative electrode active material. Silicon has a larger capacity than graphite and is therefore advantageous for increasing the capacity of the secondary battery 100.

[0052] The negative electrode active material layer 6b may contain other materials such as a conductive additive, a binder, etc. Materials that can be used as the conductive additive and binder for the positive electrode active material layer 5b can also be used for the negative electrode active material layer 6b.

[0053] The electrolyte is the nonaqueous electrolyte in embodiment 1. The electrolyte is impregnated into the positive electrode 5, the negative electrode 6, and the separator 7. The electrolyte may fill the internal space of the container 1. The electrolyte allows lithium ions to move between the positive electrode 5 and the negative electrode 6.

[0054] The average particle size of the particles of the phosphorus-containing compound contained in the electrolyte may be equal to or smaller than the pore size of the separator 7 .

[0055] The separator 7 has lithium ion conductivity. The material of the separator 7 is not particularly limited as long as it allows the passage of lithium ions. The material of the separator 7 can be at least one selected from the group consisting of a gel electrolyte, an ion exchange resin membrane, a semipermeable membrane, and a porous membrane. Using these materials for the separator 7 can sufficiently ensure the safety of the secondary battery 100. Examples of gel electrolytes include gel electrolytes containing fluororesins such as PVdF. Examples of ion exchange resin membranes include cation exchange membranes and anion exchange membranes. Examples of porous membranes include porous membranes made of polyolefin resins and porous membranes containing glass paper obtained by weaving glass fibers into a nonwoven fabric. Using the nonaqueous electrolyte of embodiment 1 in the secondary battery 100 suppresses oxidation of the separator 7 and reduces deterioration in the strength of the separator 7.

[0056] The container 1 is made of a metal such as aluminum or stainless steel, and may have a cylindrical shape or a rectangular tube shape.

[0057] The electrode group 4 may be wound into a cylindrical shape or an oval shape.

[0058] The shape of the secondary battery 100 is not particularly limited. In the present disclosure, as an example of the structure of the nonaqueous electrolyte secondary battery according to embodiment 2, the configuration example shown in FIG. 1 is described, i.e., a secondary battery in which an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween and an electrolyte solution are housed in an exterior body. However, the secondary battery according to the present disclosure is not limited to this configuration example. The secondary battery according to the present disclosure may have any shape, such as a cylindrical shape, a prismatic shape, a coin shape, a button shape, a laminate shape, or the like. Furthermore, as the electrode group in the secondary battery according to the present disclosure, instead of a wound-type electrode group, an electrode group of another shape, such as a stacked-type electrode group formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween, may be used.

[0059] The application of the nonaqueous electrolyte solution of the present disclosure is not limited to the secondary battery 100. In addition to lithium secondary batteries, the nonaqueous electrolyte solution of the present disclosure can be applied to various secondary batteries such as sodium secondary batteries and magnesium secondary batteries.

[0060] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.

[0061] (Technology 1) A non-aqueous electrolyte solution comprising: a non-aqueous solvent; an electrolyte dissolved in the non-aqueous solvent; and particles of a phosphorus-containing compound insoluble in the non-aqueous solvent, wherein the phosphorus-containing compound comprises at least one selected from the group consisting of Li3PO4, Na3PO4, K3PO4, LiPO3, LiPO3F, metaphosphoric acid, and calcium phosphate, and the non-aqueous electrolyte solution has fluidity at 25°C.

[0062] This configuration can improve the cycle characteristics of the battery.

[0063] (Technology 2) The nonaqueous electrolyte according to Technology 1, wherein the phosphorus-containing compound includes Li3PO4. With this configuration, the cycle characteristics of the battery can be improved.

[0064] (Technology 3) The nonaqueous electrolyte solution according to Technology 1 or 2, wherein the content of the particles in the nonaqueous electrolyte solution is 0.1% by volume or more and 10% by volume or less. With this configuration, the dispersibility of the phosphorus-containing compound particles and the fluidity of the nonaqueous electrolyte solution can be improved.

[0065] (Technology 4) The nonaqueous electrolyte solution according to any one of Technologies 1 to 3, wherein the particles have an average particle size of 1 nm or more and 500 nm or less. With this configuration, the dispersibility of the particles of the phosphorus-containing compound in the nonaqueous electrolyte solution is improved, making it possible to increase industrial productivity.

[0066] (Technology 5) The nonaqueous electrolyte according to any one of Technologies 1 to 4, further comprising a fluorine-containing solvent. With this configuration, the dispersibility of particles of the phosphorus-containing compound in the nonaqueous electrolyte is improved, making it possible to increase industrial productivity.

[0067] (Technology 6) The nonaqueous electrolyte according to Technology 5, wherein the fluorine-containing solvent includes a fluorinated ether. With this configuration, the dispersibility of particles of the phosphorus-containing compound in the nonaqueous electrolyte is improved, and industrial productivity can be increased.

[0068] (Technology 7) The nonaqueous electrolyte according to Technology 6, wherein the fluorinated ether includes 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether. With this configuration, the dispersibility of particles of the phosphorus-containing compound in the nonaqueous electrolyte is further improved, and industrial productivity can be increased.

[0069] (Technology 8) The nonaqueous electrolyte according to Technology 5, wherein the fluorine-containing solvent contains a fluorinated cyclic ester. This configuration can improve the dispersion stability of the nonaqueous electrolyte. This improves the dispersibility of particles of the phosphorus-containing compound in the nonaqueous electrolyte, making it possible to increase the industrial productivity of the nonaqueous electrolyte and batteries using the nonaqueous electrolyte.

[0070] (Technology 9) The nonaqueous electrolyte solution according to Technology 8, wherein the fluorinated cyclic ester includes at least one selected from the group consisting of fluoroethylene carbonate, difluoroethylene carbonate, fluoropropylene carbonate, and trifluoropropylene carbonate. With this configuration, dispersion stability can be further improved.

[0071] (Technology 10) The nonaqueous electrolyte according to Technology 8 or 9, wherein the content of the fluorinated cyclic ester is 0.1% by volume or more and 30% by volume or less with respect to the total of the nonaqueous solvent and the fluorinated cyclic ester. This configuration can improve the dispersibility of particles of the phosphorus-containing compound and the fluidity of the nonaqueous electrolyte.

[0072] (Technology 11) A non-aqueous electrolyte secondary battery comprising: a positive electrode; a negative electrode; and the non-aqueous electrolyte solution according to any one of Technologies 1 to 10.

[0073] This configuration can improve cycle characteristics.

[0074] The present disclosure will be described in more detail below using examples. The following examples are merely examples of embodiments, and are not intended to limit the scope of the present disclosure.

[0075] <Samples 1-1 to 1-5> (Sample 1-1) (Preparation of Nonaqueous Electrolyte) Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of EC:EMC:DMC = 20:5:75 to prepare a nonaqueous solvent. LiPF6 was dissolved in the obtained nonaqueous solvent to a concentration of 1 mol / L to obtain a solution. 15 g of the obtained solution, 1.2 g of Li3PO4 particles (average particle diameter 10 μm) as particles of a phosphorus-containing compound, and 70 g of ZrO2 balls (average particle diameter 0.5 mm) as mixing media were placed in a ball mill and mixed at 300 rpm for 2 hours. The average particle diameter of the Li3PO4 particles after mixing was 50 nm. The supernatant of the obtained mixture was removed by sucking up the ZrO2 balls with a dropper, and the nonaqueous electrolyte of Sample 1-1 was obtained. In the non-aqueous electrolyte of Sample 1-1, 4% by volume of Li3PO4 particles were dispersed. The non-aqueous electrolyte of Sample 1-1 had fluidity at 25°C.

[0076] (Sample 1-2) EC, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (ASAHIKLIN AE-3000 manufactured by AGC Corporation), EMC, and DMC were mixed in a volume ratio of EC:AE-3000:EMC:DMC = 15:5:5:75 to prepare a non-aqueous solvent. A non-aqueous electrolyte solution of Sample 1-2 was obtained in the same manner as Sample 1-1, except that the obtained non-aqueous solvent was used.

[0077] (Sample 1-3) A nonaqueous electrolyte solution of Sample 1-3 was obtained in the same manner as Sample 1-1, except that 0.6 g of Li3PO4 particles (average particle size 10 μm) was charged into the ball mill as particles of the phosphorus-containing compound.

[0078] (Sample 1-4) A nonaqueous electrolyte solution of Sample 1-4 was obtained in the same manner as Sample 1-1, except that 0.3 g of Li3PO4 particles (average particle size 10 μm) was charged into the ball mill as particles of the phosphorus-containing compound.

[0079] (Sample 1-5) EC, EMC, and DMC were mixed in a volume ratio of EC:EMC:DMC = 20:5:75 to prepare a nonaqueous solvent. LiPF was dissolved in the obtained nonaqueous solvent to a concentration of 1 mol / L to obtain the nonaqueous electrolyte solution of Sample 1-5. That is, the nonaqueous electrolyte solution of Sample 1-5 was prepared in the same manner as Sample 1-1, except that it did not contain particles of a phosphorus-containing compound.

[0080] [Evaluation of Dispersion Stability of Nonaqueous Electrolyte] The nonaqueous electrolytes of Samples 1-1 to 1-4 were each placed in a transparent glass container and left to stand for 72 hours, and the dispersion state of the Li3PO4 particles was visually confirmed. As a result of the evaluation, in the nonaqueous electrolytes of Samples 1-1, 1-3, and 1-4, some particles settled after 6 hours, and deposits were confirmed on the bottom of the container. In the nonaqueous electrolyte of Sample 1-2, particles did not settle even after 72 hours, and no deposits were confirmed on the bottom of the container. The time at which sedimentation was confirmed is shown in Table 1.

[0081] [Preparation of Test Cells] Test cells using the nonaqueous electrolyte solutions of Samples 1-1 to 1-5 were prepared according to the following procedure.

[0082] Li(Ni) 0.6 Co 0.2 Mn 0.2 A positive electrode slurry was prepared by adding N-methyl-2-pyrrolidone (NMP) to a positive electrode active material having a composition of acetylene black (AB), polyvinylidene fluoride (PVDF), and acetylene black (AB). The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF=96:2:2.

[0083] The positive electrode slurry was applied to the surface of an aluminum foil (1.45 cm x 1.45 cm), the coating was dried, and then rolled to form a positive electrode active material layer. In this way, a positive electrode was obtained.

[0084] Laminate half-cells were fabricated using a positive electrode, a Li metal foil (2 cm × 2 cm, 200 μm thick) as a counter electrode, a separator, and the nonaqueous electrolytes of Samples 1-1 to 1-5. A polyethylene separator (Celgard, #2320) was used as the separator.

[0085] As a result of the above, evaluation cells of Samples 1-1 to 1-5 were obtained.

[0086] [Cycle Test] A cycle test was carried out on the evaluation cells of Samples 1-1 to 1-5 according to the following procedure. The evaluation cells of Samples 1-1 to 1-5 were charged at a constant current of 0.3 C at an ambient temperature of 55°C until the voltage reached 4.7 V. Thereafter, they were discharged at a constant current of 0.3 C until the voltage reached 2.5 V. The above-described charge and discharge constituted one cycle, and this cycle was repeated 43 times to evaluate the capacity retention rate. The evaluation results are shown in Table 1.

[0087] [Evaluation of Separator Strength] For the evaluation cells of Samples 1-1 to 1-5, a trickle test was carried out in the following manner, and then a separator puncture test was carried out.

[0088] (Trickle Test) The evaluation cells of Samples 1-1 to 1-5 were charged at a constant current of 0.3 C at an ambient temperature of 55° C. until the voltage reached 4.7 V, and then the voltage of 4.7 V was maintained for 72 hours.

[0089] (Separator Puncture Test) After the trickle test, the evaluation cells for Samples 1-1 to 1-5 were disassembled, and the separators were removed. A 20 mm x 20 mm test piece was cut from the removed separator. Five of the above test pieces were prepared for each sample. The test piece was fixed in a jig, and a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm was pierced from the side that had been located on the positive electrode side at a test speed of 50 ± 5 mm / min, and the maximum force [N] until the needle penetrated was measured. The above measurements were performed on all test pieces, and the average value was taken as the separator strength. The evaluation results are shown in Table 1. A similar piercing test was performed on the separator before the trickle test, and the separator strength was 4.0 N.

[0090] In Table 1, the capacity retention rate is a relative value when the capacity of each test cell at the first cycle is set to 100%. The separator strength retention rate is the ratio (%) of the separator strength after the trickle test for Samples 1-1 to 1-5 to the separator strength (4.0 N) before the trickle test.

[0091]

[0092] (Discussion) In the cycle test, the secondary batteries of Samples 1-1 to 1-4 had improved capacity retention rates compared to the secondary battery of Sample 1-5. After the trickle test, the separator of Sample 1-5 showed a decrease in strength compared to before the test, whereas the separators of Samples 1-1 to 1-4 showed almost no decrease in strength. Here, the strength of the separator decreases as the number of double bonds increases due to the dehydrogenation reaction caused by oxidation. These results demonstrate that oxidation of the solvent and separator was suppressed in the evaluation cells of Samples 1-1 to 1-4. The nonaqueous electrolyte of Sample 1-2 had better dispersion stability than the nonaqueous electrolytes of Samples 1-1, 1-3, and 1-4.

[0093] <Samples 2-1 to 2-9> (Sample 2-1) Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were used as the nonaqueous solvent. Fluoroethylene carbonate (FEC) was used as the fluorinated cyclic ester. EC, FEC, EMC, and DMC were mixed in a volume ratio of EC:FEC:EMC:DMC = 10:10:5:75 to prepare a solvent. LiPF6 was dissolved in the resulting solvent to a concentration of 1 mol / L to obtain a solution. 15 g of the resulting solution, 0.3 g of Li3PO4 particles (average particle diameter 10 μm) as phosphorus-containing compound particles, and 70 g of ZrO2 balls (average particle diameter 0.5 mm) as mixing media were placed in a ball mill and mixed at 300 rpm for 2 hours. The average particle diameter of the Li3PO4 particles after mixing was 50 nm. The supernatant liquid of the resulting mixture was sucked up with a dropper to remove the ZrO2 balls, yielding a nonaqueous electrolyte solution of Sample 2-1, in which 1% by volume of Li3PO4 particles were dispersed.

[0094] The viscosity of the non-aqueous electrolyte of Sample 2-1 at 25°C was measured using a rheometer (MCR72 manufactured by Anton Paar) at a shear rate of 1000 s -1 The viscosity of the nonaqueous electrolyte of Sample 2-1 at 25° C. was 4.95 mPa·s.

[0095] (Sample 2-2) FEC, EMC, and DMC were mixed in a volume ratio of FEC:EMC:DMC=20:5:75 to prepare a solvent. A nonaqueous electrolyte solution of Sample 2-2 was obtained in the same manner as Sample 2-1, except that the obtained solvent was used.

[0096] The viscosity of the nonaqueous electrolyte of Sample 2-2 at 25° C. measured in the same manner as Sample 2-1 was 4.21 mPa·s.

[0097] (Sample 2-3) A nonaqueous electrolyte solution of Sample 2-3 was obtained in the same manner as Sample 2-1, except that 1.2 g of Li3PO4 particles (average particle size 10 μm) were charged into the ball mill as particles of the phosphorus-containing compound.

[0098] The viscosity of the nonaqueous electrolyte of Sample 2-3 at 25° C. measured in the same manner as Sample 2-1 was 9.21 mPa·s.

[0099] (Sample 2-4) A nonaqueous electrolyte solution of Sample 2-4 was obtained in the same manner as Sample 2-2, except that 1.2 g of Li3PO4 particles (average particle size 10 μm) were charged into the ball mill as particles of the phosphorus-containing compound.

[0100] The viscosity of the nonaqueous electrolyte of Sample 2-4 at 25° C. measured in the same manner as Sample 2-1 was 9.25 mPa·s.

[0101] (Sample 2-5) A nonaqueous electrolyte solution of Sample 2-5 was obtained in the same manner as Sample 2-1, except that 1.8 g of Li3PO4 particles (average particle diameter 10 μm) were charged into the ball mill as particles of the phosphorus-containing compound.

[0102] The viscosity of the nonaqueous electrolyte of Sample 2-5 at 25° C. measured in the same manner as Sample 2-1 was 13.52 mPa·s.

[0103] (Sample 2-6) A nonaqueous electrolyte solution of Sample 2-6 was obtained in the same manner as Sample 2-2, except that 1.8 g of Li3PO4 particles (average particle diameter 10 μm) were charged into the ball mill as particles of the phosphorus-containing compound.

[0104] The viscosity of the nonaqueous electrolyte of Sample 2-6 at 25° C. measured in the same manner as Sample 2-1 was 14.46 mPa·s.

[0105] (Sample 2-7) EC, EMC, and DMC were mixed in a volume ratio of EC:EMC:DMC = 20:5:75 to prepare a solvent. A nonaqueous electrolyte solution of Sample 2-7 was obtained in the same manner as Sample 2-1, except that the obtained solvent was used. In Sample 2-7, no fluorinated cyclic ester was used.

[0106] The viscosity of the nonaqueous electrolyte of Sample 2-7 at 25° C. measured in the same manner as Sample 2-1 was 4.24 mPa·s.

[0107] (Sample 2-8) A nonaqueous electrolyte solution of Sample 2-8 was obtained in the same manner as Sample 2-7, except that 1.2 g of Li3PO4 particles (average particle diameter 10 μm) were charged into the ball mill as particles of the phosphorus-containing compound.

[0108] The viscosity of the nonaqueous electrolyte of Sample 2-8 at 25° C. measured in the same manner as Sample 2-1 was 8.06 mPa·s.

[0109] (Sample 2-9) A nonaqueous electrolyte solution of Sample 2-9 was obtained in the same manner as Sample 2-7, except that 1.8 g of Li3PO4 particles (average particle diameter 10 μm) were charged into the ball mill as particles of the phosphorus-containing compound.

[0110] The viscosity of the nonaqueous electrolyte of Sample 2-9 at 25° C. measured in the same manner as Sample 2-1 was 11.38 mPa·s.

[0111] [Evaluation of Dispersion Stability of Nonaqueous Electrolyte] The nonaqueous electrolyte solutions of Samples 2-1 to 2-9 were each placed in a container and left to stand for 12 hours, and the dispersion state of the Li3PO4 particles was visually confirmed. As a result of the evaluation, in the nonaqueous electrolyte solutions of Samples 2-1 to 2-6, particles did not settle even after 12 hours, and the nonaqueous electrolyte solution was in a single phase state. In the nonaqueous electrolyte solutions of Samples 2-7 to 2-9, particles settled after 12 hours, and the nonaqueous electrolyte solution separated into two phases. The results are shown in Table 1. Furthermore, after the above-mentioned standing, the nonaqueous electrolyte solutions of Samples 1-1 to 1-6 were in a gel state. From the above, it was confirmed that the nonaqueous electrolyte solutions of Samples 2-1 to 2-6 have thixotropy.

[0112]

[0113] <Samples 2-10 to 2-11> (Sample 2-10) A nonaqueous electrolyte solution of Sample 2-10 was obtained in the same manner as Sample 2-3, except that the concentration of LiPF6 in the solution was changed to 1.3 mol / L.

[0114] (Sample 2-11) EC, FEC, EMC, and DMC were mixed in a volume ratio of EC:FEC:EMC:DMC = 10:10:5:75 to prepare a solvent. LiPF was dissolved in the resulting solvent to a concentration of 1.3 mol / L to obtain the nonaqueous electrolyte solution of Sample 2-11. That is, the nonaqueous electrolyte solution of Sample 2-11 was prepared in the same manner as Sample 2-10, except that it did not contain particles of a phosphorus-containing compound.

[0115] [Preparation of Evaluation Cells] Evaluation cells using the nonaqueous electrolyte solutions of Samples 2-10 and 2-11 were prepared by the following procedure.

[0116] LiNi 0.5 Mn 0.5 A positive electrode slurry was prepared by adding N-methyl-2-pyrrolidone (NMP) to a positive electrode active material having a composition of O, acetylene black (AB), and polyvinylidene fluoride (PVDF). The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF=96:2:2.

[0117] The positive electrode slurry was applied to the surface of an aluminum foil (1.45 cm x 1.45 cm), the coating was dried, and then rolled to form a positive electrode active material layer. In this way, a positive electrode was obtained.

[0118] Cells were fabricated using graphite electrodes as the positive and negative electrodes, separators, and the nonaqueous electrolytes of Samples 2-10 and 2-11, respectively. A three-layer separator (PP / PE / PP) was used as the separator.

[0119] As a result of the above, evaluation cells of samples 2-10 and 2-11 were obtained.

[0120] [Thermal Behavior Evaluation (ARC Evaluation)] The evaluation cell was evaluated for the presence or absence of self-heating and gas generation using a runaway reaction measurement device (Accelerated Rate Calorimeter: ARC, manufactured by NETZCH) under the following conditions. Measurement start temperature: 80°C, Holding time: 20 min, Heat generation detection temperature: 0.02°C / min, Temperature rise rate: 5°C, Battery voltage: 4.0 V, State of charge. If no temperature rise above the heat generation detection temperature is detected for 20 minutes from the measurement start temperature, the temperature is raised to the next step and measurement is performed again. If a temperature rise above the heat generation detection temperature is detected, it is determined that self-heating has started, and the temperature at that time is taken as the self-heating start temperature. The presence or absence of gas generation after maintaining the self-heating start temperature for 20 minutes was confirmed.

[0121] For the evaluation cell of Sample 2-10, no self-heating or gas generation was observed when ARC evaluation was performed up to 200° C. For the evaluation cell of Sample 2-11, self-heating and gas generation were observed.

[0122]

[0123] (Discussion) As can be seen from Table 2, the nonaqueous electrolytes of Samples 2-1 to 2-6 did not precipitate LiPO particles and had excellent dispersion stability. As can be seen from Table 3, the cell of Sample 2-10 containing the nonaqueous electrolyte of the present disclosure did not experience self-heating or gas generation. Therefore, the cell of Sample 2-10 had superior safety to the cell of Sample 2-11.

[0124] The technology of the present disclosure is useful for, for example, lithium ion secondary batteries.

Claims

1. A non-aqueous electrolyte comprising: a non-aqueous solvent; an electrolyte dissolved in the non-aqueous solvent; and particles of a phosphorus-containing compound insoluble in the non-aqueous solvent, wherein the phosphorus-containing compound comprises at least one selected from the group consisting of Li3PO4, Na3PO4, K3PO4, LiPO3, LiPO3F, metaphosphoric acid, and calcium phosphate, and the non-aqueous electrolyte has fluidity at 25°C.

2. The nonaqueous electrolyte according to claim 1, wherein the phosphorus-containing compound comprises Li3PO4.

3. The non-aqueous electrolyte according to claim 1, wherein the content of said particles in said non-aqueous electrolyte is 0.1 volume % or more and 10 volume % or less.

4. The nonaqueous electrolyte according to claim 1, wherein the particles have an average particle size of 1 nm or more and 500 nm or less.

5. The nonaqueous electrolyte according to claim 1, further comprising a fluorine-containing solvent.

6. The nonaqueous electrolyte according to claim 5, wherein the fluorine-containing solvent comprises a fluorinated ether.

7. The nonaqueous electrolyte of claim 6, wherein the fluorinated ether comprises 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether.

8. The nonaqueous electrolyte according to claim 5, wherein the fluorine-containing solvent comprises a fluorinated cyclic ester.

9. The nonaqueous electrolyte according to claim 8, wherein the fluorinated cyclic ester comprises at least one selected from the group consisting of fluoroethylene carbonate, difluoroethylene carbonate, fluoropropylene carbonate, and trifluoropropylene carbonate.

10. The non-aqueous electrolyte according to claim 8, wherein the content of the fluorinated cyclic ester is 0.1 vol % or more and 30 vol % or less with respect to the total of the non-aqueous solvent and the fluorinated cyclic ester.

11. A nonaqueous electrolyte secondary battery comprising: a positive electrode; a negative electrode; and the nonaqueous electrolyte solution according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Non-aqueous liquid electrolyte secondary cell

    JP2005268230A

  • Secondary battery

    JP2012018801A

  • Lithium secondary battery

    JP1998189043A

  • Nonaqueous electrolyte secondary battery and its manufacturing method

    JP2005071641A

  • Nonaqueous electrolyte secondary battery

    JP2012109240A