Solid electrolyte capacitor and method for manufacturing same

The solid electrolytic capacitor design with a high glycerin content electrolyte and ester-bond-free epoxy resin effectively addresses electrolyte leakage issues, ensuring reliable performance in high-temperature environments by using a solid electrolyte and resin barrier to minimize evaporation.

WO2024225389A1PCT designated stage expired Publication Date: 2024-10-31NIPPON CHEMI CON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016279
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Electrolytic capacitors face significant electrolyte leakage, especially in high-temperature environments, due to evaporation and transpiration, leading to reduced capacitance and shortened lifespan, as existing sealing methods are not effective in completely confining the electrolyte.

Method used

A solid electrolytic capacitor design featuring a dielectric film on the anode body, a solid electrolyte layer with a high boiling point liquid component, and a resin member covering the case opening, where the electrolyte solution contains 30 wt% or more glycerin, and the resin member is made of epoxy resin without ester bonds, enhancing the barrier properties and reducing evaporation.

Benefits of technology

The solution significantly suppresses electrolyte leakage, even at high temperatures, by utilizing a high glycerin content in the electrolyte solution and an ester-bond-free epoxy resin, thereby extending the capacitor's lifespan and maintaining capacitance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016279_31102024_PF_FP_ABST
    Figure JP2024016279_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are an electrolyte capacitor having an enhanced electrolyte loss-preventing effect, and a method for manufacturing the same. An electrolyte layer is interposed between an anode body and a cathode body. The electrolyte layer includes a solid electrolyte layer and an electrolyte. The anode body, the cathode body, and the electrolyte layer are housed in a case, and at least a part of the opening side of the case is covered with a resin member. The electrolyte contains glycerin that accounts for 30 wt% or more of the total amount of solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Solid electrolytic capacitor and its manufacturing method

[0001] The present invention relates to a solid electrolytic capacitor having a solid electrolyte layer and an electrolytic solution, and a method for manufacturing the same.

[0002] Electrolytic capacitors have anodes and cathodes made of valve metals such as tantalum or aluminum. The anodes are enlarged by shaping the valve metal into a sintered body or etched foil, and the enlarged surfaces are coated with a dielectric film. An electrolyte is interposed between the anode and cathode foils.

[0003] The electrolyte is in close contact with the uneven surface of the anode foil and functions as the true cathode. The electrolyte also repairs the dielectric film. However, over time, the electrolyte evaporates and escapes from the electrolytic capacitor. As a result, the capacitance of the electrolytic capacitor decreases over time as it dries up, eventually reaching the end of its life.

[0004] Therefore, the anode body, cathode body, and electrolyte are housed in a bottomed outer case. The opening of the outer case is sealed with a sealant. The sealant contains an elastomer such as butyl rubber and is crimped to fit tightly to the opening of the case. This sealant confines the electrolyte within the case, suppressing the amount of evaporation and extending the life of the electrolytic capacitor.

[0005] However, the electrolyte is not completely contained within the case, but gradually permeates the sealing body and volatilizes to the outside of the electrolytic capacitor. Therefore, in some cases, the opening of the case is covered from above the sealing body with a resin layer that has lower electrolyte permeability than the elastomer (see, for example, Patent Document 1). This resin layer further enhances the gas barrier properties. In some cases, the opening of the case is sealed with a single sealing body in which an elastomer layer and a resin layer are laminated.

[0006] Japanese Unexamined Patent Publication No. 60-245106

[0007] In recent years, electrolytic capacitors have been increasingly used in high-temperature environments, such as in automotive applications, at temperatures of 170° C. In high-temperature environments, the electrolyte is more likely to escape from the electrolytic capacitor, and therefore there is a demand for electrolytic capacitors that suppress the amount of electrolyte loss even in high-temperature environments.

[0008] The present invention has been proposed to solve the above-mentioned problems, and an object of the present invention is to provide an electrolytic capacitor and a manufacturing method thereof that are more effective in suppressing the loss of electrolyte.

[0009] In order to solve the above-described problems, the electrolytic capacitor of the present embodiment includes an anode body having a dielectric coating, a cathode body facing the anode body, an electrolyte layer interposed between the anode body and the cathode body and containing a solid electrolyte layer and an electrolyte solution, a case accommodating the anode body, the cathode body, and the electrolyte layer, and a resin member covering at least a portion of an open side of the case, wherein the electrolyte solution contains glycerin accounting for 30 wt % or more of a total amount of solvent.

[0010] The electrolyte may further include ethylene glycol, sulfolane, polyethylene glycol, or a combination thereof.

[0011] The resin member may include an epoxy resin or an acrylic resin.

[0012] The resin member may include an epoxy resin.

[0013] The resin member may contain the epoxy resin having no ester bond.

[0014] The resin member may contain an amine-based hardener or a phenol-based hardener in addition to the epoxy resin.

[0015] The solid electrolyte layer may contain a high-boiling liquid component having a boiling point of 150° C. or higher and having a hydroxyl group.

[0016] The high boiling point liquid component may be ethylene glycol, diethylene glycol, glycerin, diglycerin, polyethylene glycol, or a combination thereof.

[0017] In order to solve the above-described problems, a method for manufacturing an electrolytic capacitor according to the present embodiment includes the steps of forming a dielectric film on a surface of an anode body, forming a solid electrolyte layer between the anode body and the cathode body, accommodating the anode body, the cathode body, and the solid electrolyte layer in a case, impregnating the anode body, the cathode body, and the solid electrolyte layer with an electrolyte solution containing 30 wt % or more of glycerin relative to a total amount of a solvent, and covering at least a portion of an opening side of the case with a resin member.

[0018] According to the present invention, the amount of electrolyte leaking from the solid electrolytic capacitor can be reduced.

[0019] 1 is a graph showing the relationship between the amount of omission of each solvent composition of the electrolyte and the glycerin ratio in the solvent in a solid electrolytic capacitor having a resin member; 2 is a graph showing a partial range of the relationship between the amount of omission of each solvent composition of the electrolyte and the glycerin ratio in the solvent in a solid electrolytic capacitor having a resin member; 3 is a graph showing the relationship between the amount of omission of each solvent composition of the electrolyte and the glycerin ratio in the solvent in a solid electrolytic capacitor without a resin member; 4 is a scatter plot showing the correlation between the amount of omission of the resin member and the weight change rate.

[0020] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the embodiments described below.

[0021] (Overall Configuration) The solid electrolytic capacitor according to this embodiment is a passive element that obtains capacitance through the dielectric polarization of a dielectric film and stores and discharges electric charge. This solid electrolytic capacitor is a so-called hybrid type that uses both a solid electrolyte layer and an electrolytic solution. Hereinafter, a hybrid type solid electrolytic capacitor will be simply referred to as a solid electrolytic capacitor.

[0022] A solid electrolytic capacitor comprises an anode body, a cathode body, an electrolyte layer, and a separator. The anode body has a dielectric film formed on its surface. The cathode body faces the dielectric film and faces the anode body. The electrolyte layer is interposed between the anode body and the cathode body, contacts the dielectric film, and serves as the true cathode of the solid electrolytic capacitor. This electrolyte layer is composed of a solid electrolyte layer and an electrolytic solution. The separator is interposed between the anode body and the cathode body, isolating them and preventing short circuits.

[0023] The solid electrolytic capacitor has a cylindrical outer case with one open end and the other closed end, and the anode body, cathode body, electrolyte layer, and separator are housed inside the outer case. The open end of the outer case is covered with an elastic member and a resin member. An anode lead is connected to the anode body, and a cathode lead is connected to the cathode body, and the anode lead and cathode lead extend through the elastic member and the resin member. The solid electrolytic capacitor is electrically connected to a mounted circuit via the anode lead and cathode lead.

[0024] (Anode Body) In such solid electrolytic capacitors, the anode body base material is made of a valve metal. In wound-type solid electrolytic capacitors, the anode body is a long strip of elongated valve metal. In stacked-type solid electrolytic capacitors, the anode body is a flat plate of elongated valve metal, a molded body of valve metal powder shaped into a flat plate, or a sintered body of valve metal powder. Valve metals include aluminum, tantalum, niobium, niobium oxide, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. The purity of the anode body is preferably 99.9% or higher, but impurities such as silicon, iron, copper, and magnesium may be contained.

[0025] A surface-expanding layer is formed on one or both sides of the anode body. The surface-expanding layer can be an etched layer formed by etching a substrate, a sintered layer formed by sintering valve metal powder onto a substrate, or a vapor-deposited layer formed by vapor-depositing valve metal particles onto a substrate. That is, the surface-expanding layer has a porous structure consisting of tunnel-like pits, spongy pits, or voids between densely packed powder or particles.

[0026] Tunnel-shaped etching pits are holes dug in the foil thickness direction. These tunnel-shaped etching pits are typically formed by passing a direct current in an acidic aqueous solution containing halogen ions, such as hydrochloric acid. The spongy etching pits turn the surface-expanding layer into a sponge-like layer with fine, interconnected voids. These spongy etching pits are formed by passing an alternating current in an acidic aqueous solution containing halogen ions, such as hydrochloric acid.

[0027] The sintered layer is produced by obtaining a powder of a valve action metal of the same or different type as the foil body by a milling method, atomization method, melt spinning method, rotating disk method, rotating electrode method, etc., forming a paste with a binder or solvent, applying it to the foil body, drying it, and heating and sintering it in a vacuum or reducing atmosphere, etc. The atomization method may be any of water atomization method, gas atomization method, and water gas atomization method. The vapor deposition layer is produced by, for example, resistance heating vapor deposition method or electron beam heating vapor deposition method. This vapor deposition layer is formed by heating and vaporizing a valve action metal of the same or different type as the foil body by resistance heat or electron beam energy, and depositing the vapor of valve action metal particles on the surface of the foil body.

[0028] The dielectric coating is formed on one or both sides of the anode body, following the irregularities of the surface-expanding layer. The dielectric coating is typically an oxide coating formed on the surface layer of the anode body. If the anode body is made of aluminum, it is an aluminum oxide layer formed by oxidizing the surface of the surface-expanding layer. In the chemical conversion treatment to form the dielectric coating, a voltage is applied to the anode body in a chemical conversion solution until the desired withstand voltage is achieved. The chemical conversion solution is a solution free of halogen ions, such as a phosphoric acid-based chemical conversion solution such as ammonium dihydrogen phosphate, a boric acid-based chemical conversion solution such as ammonium borate, or an adipic acid-based chemical conversion solution such as ammonium adipate.

[0029] (Cathode Body) In the case of a wound-type solid electrolytic capacitor, the cathode body is preferably a foil made of a valve metal and stretched. The purity of the cathode body is preferably 99% or higher. The cathode body may have a surface-expanding layer formed thereon, as with the anode body, or a plain foil without a surface-expanding layer may be used as the cathode body. The cathode body may have a natural oxide film or a thin oxide film (approximately 1 to 10 V) formed by chemical conversion treatment. The natural oxide film is formed by the cathode body reacting with oxygen in the air. Furthermore, the cathode body may have a layer made of metal nitride, metal carbide, or metal carbonitride formed thereon by vapor deposition, or a carbon-containing layer formed on the surface.

[0030] Alternatively, in the case of a stacked solid electrolytic capacitor, the cathode body is preferably a laminate of a metal layer and a carbon layer. The carbon layer of the cathode body is disposed facing the anode body. The carbon layer is formed by applying a paste onto the electrolyte layer after the electrolyte layer is formed on the anode body, and then curing the paste by heating. The metal layer is, for example, a silver layer, and is formed by applying a paste onto the carbon layer and then curing the paste by heating.

[0031] (Electrolyte Layer) (Electrolyte Solution) The solvent for the electrolyte solution contains glycerin at a ratio of 30 wt % or more of the total amount of solvent. The solvent other than glycerin is not particularly limited, and a protic polar solvent or an aprotic polar solvent can be used. Typical examples of protic polar solvents include polyhydric alcohols and oxyalcohol compounds, such as ethylene glycol, propylene glycol, diethylene glycol, and polyethylene glycol. Typical examples of aprotic polar solvents include sulfones and lactones, such as sulfolane, γ-butyrolactone, δ-valerolactone, ethylene carbonate, and propylene carbonate.

[0032] In a solid electrolytic capacitor having a resin layer, when the solvent for the electrolyte contains glycerin at a ratio of 30 wt% or more of the total amount of solvent, the amount of electrolyte that evaporates from the solid electrolytic capacitor is significantly improved compared to when the glycerin content is less than 30 wt% of the total amount of solvent. Furthermore, when the resin layer is omitted from the solid electrolytic capacitor, no significant change in the amount of evaporating is observed at the 30 wt% boundary, and the measure of making the glycerin content 30 wt% or more of the total amount of solvent is useful for solid electrolytic capacitors having a resin layer.

[0033] The solvent other than glycerin is preferably ethylene glycol, sulfolane, polyethylene glycol, or two or more of these, which further improves the amount of electrolyte solution that evaporates from the solid electrolytic capacitor.

[0034] The electrolytic solution may contain an electrolyte in addition to glycerin and a protic or aprotic polar liquid. The electrolyte is typically a salt of an organic acid, a salt of an inorganic acid, or a salt of a complex compound of an organic acid and an inorganic acid, and may be used alone or in combination of two or more. An acid that becomes an anion and a base that becomes a cation may be added separately to the liquid.

[0035] Examples of organic acids that can serve as anion components include carboxylic acids such as oxalic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, maleic acid, adipic acid, benzoic acid, toluic acid, enanthic acid, malonic acid, 1,6-decanedicarboxylic acid, 1,7-octanedicarboxylic acid, azelaic acid, resorcylic acid, phloroglucinic acid, gallic acid, gentisic acid, protocatechuic acid, pyrocatechuic acid, trimellitic acid, and pyromellitic acid, as well as phenols and sulfonic acids. Examples of inorganic acids that can serve as anion components include boric acid, phosphoric acid, phosphorous acid, hypophosphorous acid, carbonic acid, and silicic acid. Examples of composite compounds of organic and inorganic acids include borodisalicylic acid.

[0036] Furthermore, examples of at least one salt of an organic acid, an inorganic acid, or a complex compound of an organic acid and an inorganic acid include ammonium salts, quaternary ammonium salts, quaternized amidinium salts, amine salts, sodium salts, and potassium salts. Examples of quaternary ammonium ions of quaternary ammonium salts include tetramethylammonium, triethylmethylammonium, and tetraethylammonium. Examples of quaternized amidinium salts include ethyldimethylimidazolinium and tetramethylimidazolinium. Examples of amine salts include salts of primary amines, secondary amines, and tertiary amines. Examples of primary amines include methylamine, ethylamine, and propylamine. Examples of secondary amines include dimethylamine, diethylamine, ethylmethylamine, and dibutylamine. Examples of tertiary amines include trimethylamine, triethylamine, tributylamine, ethyldimethylamine, and ethyldiisopropylamine.

[0037] Furthermore, other additives can also be added to the electrolyte solution. Examples of additives include complex compounds of boric acid and polysaccharides (mannite, sorbite, etc.), complex compounds of boric acid and polyhydric alcohols, borate esters, nitro compounds (o-nitrobenzoic acid, m-nitrobenzoic acid, p-nitrobenzoic acid, o-nitrophenol, m-nitrophenol, p-nitrophenol, p-nitrobenzyl alcohol, etc.), phosphate esters, and alkyl phosphate esters. These may be used alone or in combination of two or more.

[0038] The electrolyte solution is impregnated into the voids of the capacitor element formed by the solid electrolyte layer. The capacitor element is an assembly consisting of an anode body, a cathode body, and an electrolyte layer. The electrolyte solution may be impregnated by immersing the capacitor element in a tank of the electrolyte solution, or the capacitor element may be impregnated with the electrolyte solution inside an outer case. In the impregnation process, a decompression treatment or a pressurization treatment may be performed as necessary; for example, the pressure inside the capacitor element may be reduced and the electrolyte may be pressurized.

[0039] (Solid electrolyte layer) The solid electrolyte layer includes a conductive polymer. The conductive polymer is a self-doped conjugated polymer doped with an internal dopant molecule, or an externally doped conjugated polymer doped with an external dopant molecule. The conjugated polymer is obtained by chemical oxidative polymerization or electrolytic oxidative polymerization of a monomer having a π-conjugated double bond or a derivative thereof. The dopant or external dopant molecule is an acceptor that easily accepts electrons into the conjugated polymer, or a donor that easily donates electrons, which allows the conductive polymer to exhibit high conductivity.

[0040] The presence of this solid electrolyte layer allows the proportion of glycerin to be 30 wt % or more of the total amount of solvent. That is, an electrolyte solution in which glycerin accounts for 30 wt % or more of the total amount of solvent has high viscosity and therefore high resistivity. However, the solid electrolyte layer has such high conductivity that it can offset the high resistivity of the electrolyte solution and reduce the effect of the electrolyte solution on the internal resistance of the solid electrolytic capacitor.

[0041] As the conjugated polymer, any known polymer can be used without any particular limitation. Examples include polypyrrole, polythiophene, polyfuran, polyaniline, polyacetylene, polyphenylene, polyphenylene vinylene, polyacene, polythiophene vinylene, etc. These conjugated polymers may be used alone or in combination of two or more types, or may even be a copolymer of two or more types of monomers.

[0042] Among the above conjugated polymers, preferred are conjugated polymers obtained by polymerizing thiophene or a derivative thereof, and preferred are conjugated polymers obtained by polymerizing 3,4-ethylenedioxythiophene (i.e., 2,3-dihydrothieno[3,4-b][1,4]dioxin), 3-alkylthiophene, 3-alkoxythiophene, 3-alkyl-4-alkoxythiophene, 3,4-alkylthiophene, 3,4-alkoxythiophene, or derivatives thereof. The thiophene derivative is preferably a compound selected from thiophenes having substituents at the 3rd and 4th positions, and the substituents at the 3rd and 4th positions of the thiophene ring may form a ring together with the carbon atoms at the 3rd and 4th positions. The alkyl group or alkoxy group preferably has 1 to 16 carbon atoms.

[0043] In particular, a polymer of 3,4-ethylenedioxythiophene, known as EDOT, i.e., poly(3,4-ethylenedioxythiophene), known as PEDOT, is particularly preferred. Furthermore, a substituent may be added to 3,4-ethylenedioxythiophene. For example, an alkylated ethylenedioxythiophene having an alkyl group having 1 to 5 carbon atoms added as a substituent may be used. Examples of alkylated ethylenedioxythiophenes include methylated ethylenedioxythiophene (i.e., 2-methyl-2,3-dihydro-thieno[3,4-b][1,4]dioxin), ethylated ethylenedioxythiophene (i.e., 2-ethyl-2,3-dihydro-thieno[3,4-b][1,4]dioxin), butylated ethylenedioxythiophene (i.e., 2-butyl-2,3-dihydro-thieno[3,4-b][1,4]dioxin), and 2-alkyl-3,4-ethylenedioxythiophene.

[0044] Any known dopant can be used without any particular limitation. A single dopant may be used, or two or more dopants may be used in combination. Furthermore, a polymer or a monomer may be used. Examples of dopants include inorganic acids such as polyanions, boric acid, nitric acid, and phosphoric acid, and organic acids such as acetic acid, oxalic acid, citric acid, tartaric acid, squaric acid, rhodizonic acid, croconic acid, salicylic acid, p-toluenesulfonic acid, 1,2-dihydroxy-3,5-benzenedisulfonic acid, methanesulfonic acid, trifluoromethanesulfonic acid, borodisalicylic acid, bisoxalateborate acid, sulfonylimide acid, dodecylbenzenesulfonic acid, propylnaphthalenesulfonic acid, and butylnaphthalenesulfonic acid.

[0045] Examples of the polyanion include a substituted or unsubstituted polyalkylene, a substituted or unsubstituted polyalkenylene, a substituted or unsubstituted polyimide, a substituted or unsubstituted polyamide, and a substituted or unsubstituted polyester, and include a polymer consisting only of a structural unit having an anionic group, and a polymer consisting of a structural unit having an anionic group and a structural unit not having an anionic group. Specific examples of the polyanion include polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyacryl sulfonic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropane sulfonic acid), polyisoprene sulfonic acid, polyacrylic acid, polymethacrylic acid, and polymaleic acid.

[0046] The solid electrolyte layer may contain a liquid component having a hydroxy group and a high boiling point of 150°C or higher. This high boiling point liquid component improves the chemical conversion properties of the dielectric film and increases the withstand voltage of the solid electrolytic capacitor. Examples of the high boiling point liquid component having a hydroxy group and a boiling point of 150°C or higher include ethylene glycol, diethylene glycol, glycerin, diglycerin, polyethylene glycol, and combinations of two or more of these.

[0047] Here, the conductive polymer may be attached by impregnating a conductive polymer liquid into the anode body, the separator, or both of them, or further into the cathode body or the capacitor element, and then drying the liquid. The conductive polymer liquid is a dispersion or solution in which a conductive polymer is dispersed or dissolved in a dispersion medium or solvent. A liquid component having a hydroxy group and a high boiling point of 150°C or higher may also serve as the dispersion medium or solvent for the conductive polymer liquid. Even if the conductive polymer liquid is volatilized in the drying step, the high boiling point liquid component can remain in the solid electrolyte layer.

[0048] (Separator) Examples of separators include cellulose papers such as kraft, Manila hemp, esparto, hemp, and rayon, and mixtures thereof; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and derivatives thereof; polytetrafluoroethylene resins, polyvinylidene fluoride resins, vinylon resins; polyamide resins such as aliphatic polyamides, semi-aromatic polyamides, and wholly aromatic polyamides; polyimide resins, polyethylene resins, polypropylene resins, trimethylpentene resins, polyphenylene sulfide resins, acrylic resins, and polyvinyl alcohol resins, and these resins can be used alone or in combination. Note that if the anode body and cathode body can be insulated by the solid electrolyte layer and the solid electrolyte layer can maintain its shape without a separator, the separator can be omitted.

[0049] (Elastic Member) The elastic member seals the open end of the outer case. The outer case is made of metal, such as aluminum, an aluminum alloy containing aluminum and manganese, or stainless steel. An elastic member is inserted into the open end of the outer case, and the elastic member is tightly attached by crimping, which bends the outer case inward. This elastic member tightly attaches to the crimped outer case due to its elastic force, preventing the electrolyte from leaking out from between the elastic member and the outer case. It is also possible to cover the open side of the outer case with a resin member without using an elastic member.

[0050] The elastic member includes an elastomer. Examples of the elastomer include isobutylene isoprene rubber (also called butyl rubber), ethylene propylene diene rubber (also called EPDM), styrene butadiene rubber, isoprene rubber, fluororubber, acrylic rubber, nitrile rubber, and natural rubber. These elastomers are produced by vulcanization such as resin vulcanization, peroxide vulcanization, sulfur vulcanization, quinoid vulcanization, and polyol vulcanization, and also include thermoplastic elastomers. One or more types of elastomers may be used.

[0051] Examples of vulcanizing agents include benzoyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, and alkylphenol formaldehyde resins. Examples of crosslinking accelerators include zinc oxide, magnesium oxide, lead peroxide, dibenzothiazyl, disulfide, 1,2-polybutadiene, triallyl cyanurate, metal salts of methacrylic acid and acrylic acid, and ester stearic acid N,N'-metaphenyl dimaleic acid. The initial crosslink density of the elastomer can be adjusted by using one or more of these vulcanizing agents and crosslinking accelerators in combination, and by selecting an appropriate one for each type of elastomer.

[0052] The elastic member may contain carbon and inorganic fillers in addition to the elastomer. The addition of carbon and inorganic fillers makes the elastomer less susceptible to cleavage, thereby suppressing softening of the elastic member. Examples of inorganic fillers include talc, mica, silica, kaolin, titania, alumina, and mixtures thereof, with flat-shaped talc and mica being preferred. Flat-shaped inorganic fillers are suitable for promoting crosslinking and adjusting crosslink density. Furthermore, the elastic member may have a hard synthetic resin plate or metal plate in addition to the elastomer layer, and may be a laminate of the elastomer layer and the hard synthetic resin plate or metal plate.

[0053] (Resin Member) The resin member covers the opening side of the outer case and suppresses evaporation of the electrolyte. The resin member also serves as a heat insulating layer during a reflow process, etc., improving the heat resistance of the solid electrolytic capacitor. The resin member is preferably disposed so as to cover the outer surface of the elastic member, and can suppress evaporation of the electrolyte that permeates the elastic member. Alternatively, the resin member may be provided on the elastic member and laminated together with an elastomer layer. The resin member may not cover the entire opening of the outer case, and may have some uncovered areas, such as the lead-out areas of the anode lead and the cathode lead.

[0054] This resin member is formed on the opening side of the exterior case by pouring it in liquid form onto the outer surface of the elastic member after the elastic member is installed and solidifying. Examples of resin materials for the resin member include thermosetting resins, thermoplastic resins, and ultraviolet-curing resins. Specific examples of resin materials include epoxy resins, silicone resins, allyl resins, polybutylene terephthalate resins, polycarbonate resins, polyethylene terephthalate resins, acrylic resins, phenolic resins, polyamide resins, alkyd resins, and urethane resins. The epoxy resin may be a two-component epoxy resin using an acid anhydride, or a one-component epoxy resin.

[0055] Among these, epoxy resin is preferred as the resin material for the resin member. Epoxy resin is a thermosetting resin or ultraviolet-curing resin, even in the category of synthetic resins, and does not soften with heat like thermoplastic resin, nor does it melt even when exposed to a high-temperature environment. Among thermosetting resins, epoxy resin, silicone resin, allyl resin, etc. have heat resistance of 150°C or higher. Among these, epoxy resin also has gas barrier properties and suppresses oxidative degradation of conductive polymers.

[0056] The resin material for the resin member is preferably an epoxy resin without an ester bond in its chemical structure. Water is present in the electrolyte, either intentionally or during the production process. If the epoxy resin has an ester bond in its chemical structure, when the electrolyte comes into contact with the resin member, the ester bond reacts with water, causing the epoxy resin to hydrolyze. Furthermore, if a compound with a hydroxy group is present in the electrolyte, the carbonyl group generated by hydrolysis and this compound will undergo an esterification reaction. The epoxy resin reacted with water or a compound with a hydroxy group will dissolve into the electrolyte in the solid electrolytic capacitor, increasing the ESR of the solid electrolytic capacitor. Therefore, the resin material for the resin member is preferably an epoxy resin without an ester bond in its chemical structure.

[0057] Epoxy resins that do not have an ester bond in their chemical structure include amine-cured epoxy resins and phenol-cured epoxy resins. Amine-cured epoxy resins are epoxy resins cured with an amine-curing agent and contain an amine-curing agent and an epoxy resin in their chemical structure. Phenol-cured epoxy resins are epoxy resins cured with a phenol-based curing agent and contain a phenol-based curing agent and an epoxy resin in their chemical structure. Amine-cured epoxy resins are produced by the reaction and bonding of amino groups and epoxy groups, and have ether bonds but no ester bonds. Phenol-cured epoxy resins are produced by the reaction and bonding of phenolic hydroxy groups and epoxy groups, and have ether bonds but no ester bonds.

[0058] The epoxy resins contained in phenol-cured epoxy resins and amine-cured epoxy resins are epoxy oligomers with two or more reactive epoxy groups at the terminals. These epoxy resins undergo an addition reaction with an acid anhydride curing agent, crosslinking the epoxy resin molecules and converting them from a liquid to a solid resin. Typical examples of epoxy resins include bisphenol A diglycidyl ether, a condensation product of bisphenol A and epichlorohydrin. Other examples of epoxy resins include other glycidyl-type epoxy resins and alicyclic epoxides such as 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate.

[0059] Examples of glycidyl epoxy resins include bisphenol-type resins obtained by glycidylating bisphenols, such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethylbisphenol A, tetramethylbisphenol F, tetramethylbisphenol AD, tetramethylbisphenol S, tetrabromobisphenol A, tetrachlorobisphenol A, and tetrafluorobisphenol A.

[0060] Glycidyl epoxy resins include epoxy resins obtained by glycidylating dihydric phenols, such as biphenol, dihydroxynaphthalene, and 9,9-bis(4-hydroxyphenyl)fluorene.

[0061] Glycidyl epoxy resins include epoxy resins obtained by glycidylating trisphenols. Examples of triphenols include 1,1,1-tris(4-hydroxyphenyl)methane and 4,4-(1-(4-(1-(4-hydroxyphenyl)-1-methylethyl)phenyl)ethylidene)bisphenol.

[0062] Glycidyl epoxy resins include epoxy resins obtained by glycidylating tetrakisphenols, such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane.

[0063] The glycidyl epoxy resin may be a novolac epoxy resin obtained by glycidylating novolacs, such as phenol novolac, cresol novolac, bisphenol A novolac, brominated phenol novolac, and brominated bisphenol A novolac.

[0064] Examples of glycidyl type epoxy resins include epoxy resins obtained by glycidylating polyhydric phenols, and aliphatic ether type epoxy resins obtained by glycidylating polyhydric alcohols such as glycerin and polyethylene glycol.

[0065] Examples of glycidyl-type epoxy resins include ether ester-type epoxy resins obtained by glycidylating hydroxycarboxylic acids, ester-type epoxy resins obtained by glycidylating polycarboxylic acids, glycidyl compounds of amine compounds, and amine-type epoxy resins. Examples of hydroxycarboxylic acids include p-oxybenzoic acid and β-oxynaphthoic acid. Examples of polycarboxylic acids include phthalic acid and terephthalic acid. Examples of amine compounds include 4,4-diaminodiphenylmethane and m-aminophenol. Examples of amine-type epoxy resins include triglycidyl isocyanurate.

[0066] The phenolic curing agent contained in the phenolic cured epoxy resin may be a bifunctional phenol or a polyfunctional phenol. Examples of the bifunctional phenol include hydroquinone, resorcinol, bisphenol F, biphenol, tetrabromobisphenol A, and naphthalenediol. Examples of the polyfunctional phenol include phenol novolac resin.

[0067] Examples of amine-based curing agents contained in amine-based cured epoxy resins include aliphatic polyamines, aromatic polyamines, and modified amines. Examples of aliphatic polyamines include diethylenetriamine and triethylenetetramine. Examples of aromatic polyamines include metaphenylenediamine, diaminodiphenylmethane, and diaminodiphenylsulfone. Examples of modified amines include amine adducts and ketimines.

[0068] The solid electrolytic capacitor will be described in more detail below based on examples, but the present invention is not limited to the following examples.

[0069] (Examples 1 to 18) Various solid electrolytic capacitors were fabricated. The various solid electrolytic capacitors had the following in common. First, an anode body and a cathode body were fabricated using aluminum foil. Both the anode body and the cathode body were subjected to AC etching to enlarge the surface, and spongy etching pits were formed. A dielectric film was formed on the foil surface of the anode body and the cathode body by chemical conversion treatment. In the chemical conversion treatment process for the anode body, a chemical conversion voltage of 66 V was applied and then maintained for 10 minutes. In the chemical conversion treatment process for the cathode body, a chemical conversion voltage of 3 V was applied and then maintained for 10 minutes.

[0070] Lead wires were connected to each of the anode and cathode bodies, and the anode and cathode foils were wound facing each other with a manila paper separator interposed between them. The wound body had a diameter of 10 mm and a height of 10 mm. Repair and chemical conversion were performed by passing a voltage of 56.5 V and a current density of 10 mA through the wound body in an aqueous solution of ammonium dihydrogen phosphate at a liquid temperature of 90°C for 10 minutes.

[0071] The wound body was first impregnated with a conductive polymer liquid. The conductive polymer liquid was a dispersion of poly(3,4-ethylenedioxythiophene) (PEDOT / PSS) doped with polystyrene sulfonic acid (PSS). PEDOT / PSS was added at a ratio of 1.2 wt% to the total conductive polymer liquid. Ethylene glycol was also added to the conductive polymer liquid at a ratio of 10 wt% to the conductive polymer dispersion. The wound body was impregnated with this conductive polymer liquid for 10 minutes at room temperature and in a reduced pressure environment of -0.3 MPa.

[0072] After the wound body was removed from the conductive polymer solution, it was further dried by being left to stand for 30 minutes in a temperature environment of 150° C. As a result, an electrolyte layer containing the conductive polymer and ethylene glycol was formed on the dielectric film of the anode body.

[0073] Next, the wound body was impregnated with an electrolyte solution. The electrolyte solution was allowed to penetrate the wound body for 10 minutes at room temperature and in a reduced pressure environment of -0.3 MPa. This produced a capacitor element consisting of an anode body, a cathode body, a separator, and an electrolyte layer. The capacitor element was housed in an outer case, and the open end of the outer case was sealed with an elastic member. The elastic member and the outer case were tightly attached by crimping. The elastic member was made of butyl rubber.

[0074] After sealing the exterior case with the elastic member, a resin was poured onto the outer surface of the elastic member and allowed to harden to form a resin member covering the outer surface of the elastic member. The poured resin was an amine-based cured epoxy resin with no ester bonds in its chemical structure.

[0075] The various solid electrolytic capacitors differ in the solvent of the electrolyte, but all of them have in common that 5 wt % of ammonium azelaate is added to the total amount of the electrolyte.

[0076] Among the various solid electrolytic capacitors, the first group has an electrolyte solvent composed of glycerin and ethylene glycol, with the glycerin ratio in the solvent varying. Among the various solid electrolytic capacitors, the second group has an electrolyte solvent composed of glycerin and sulfolane, with the glycerin ratio in the solvent varying. Among the various solid electrolytic capacitors, the third group has an electrolyte solvent composed of glycerin and polyethylene glycol, with the glycerin ratio in the solvent varying. Among the various solid electrolytic capacitors, the fourth group has an electrolyte solvent composed of glycerin and γ-butyrolactone, with the glycerin ratio in the solvent varying.

[0077] Each solid electrolytic capacitor was left at 170°C for 560 hours, and the amount of electrolyte lost was measured based on the weight difference before and after storage. The amounts of electrolyte lost for each solid electrolytic capacitor are shown in Tables 1 to 4 below.

[0078] (Table 1)

[0079] (Table 2)

[0080] (Table 3)

[0081] (Table 4)

[0082] Based on Tables 1 to 4 above, the relationship between the amount of leaching for each solvent composition of the electrolyte and the glycerin ratio in the solvent is shown in the graphs of Figures 1 and 2. In Figures 1 and 2, the square plots represent Group 1 containing ethylene glycol, the triangle plots represent Group 2 containing sulfolane, the diamond plots represent Group 3 containing polyethylene glycol, and the circle plots represent Group 4 containing γ-butyrolactone. Figure 2 shows an enlarged view of the range of leaching amounts from 8 mg to 20 mg in the graph of Figure 1.

[0083] 1 and 2, when at least a portion of the open side of the case is covered with a resin member, the amount of electrolyte leakage increases in the range where the glycerin ratio in the electrolyte solvent is low, with the border being 30 wt%, while the amount of electrolyte leakage is suppressed in the range where the glycerin ratio is high, with the border being 30 wt%. This tendency was confirmed to be remarkable when the electrolyte solvent was composed of glycerin and ethylene glycol, sulfolane, or polyethylene glycol.

[0084] Furthermore, when the solvent of the electrolyte is composed of glycerin and ethylene glycol, sulfolane or polyethylene glycol, the amount of electrolyte lost is kept particularly low.

[0085] Here, various solid electrolytic capacitors serving as reference examples were fabricated, and the amount of electrolyte loss was measured. The various solid electrolytic capacitors serving as reference examples were identical to the respective examples and comparative examples, including the composition of the electrolyte, except that the resin member was omitted. The various solid electrolytic capacitors serving as reference examples were left at a temperature of 170°C for 560 hours, and the amount of electrolyte loss was measured based on the weight difference before and after leaving the capacitors. The results are shown in Figure 3.

[0086] FIG. 3 is a graph showing the relationship between the amount of leakage for each solvent composition of the electrolyte solution of the Reference Example and the glycerin ratio in the solvent, in which the plots with square marks are the first group containing ethylene glycol, the plots with triangle marks are the second group containing sulfolane, the plots with diamond marks are the third group containing polyethylene glycol, and the plots with circle marks are the fourth group containing γ-butyrolactone.

[0087] As shown in Figure 3, when the resin member is omitted, there is no specific glycerin ratio that changes the tendency of the amount of electrolyte leakage, and the amount of electrolyte leakage is in line with the glycerin ratio. Therefore, it was confirmed that when at least a portion of the open side of the case is covered with a resin member, if the glycerin ratio in the electrolyte solvent is 30 wt % or more, the amount of electrolyte leakage from the solid electrolytic capacitor is significantly suppressed.

[0088] Examples 19 to 24 In Examples 1 to 18, an amine-based cured epoxy resin having no ester bond in its chemical structure was used as the resin member. Next, the type of resin member was changed and the weight change rate was measured for combinations of various resin members and various electrolyte solvents.

[0089] In Examples 19 to 21 and Comparative Examples 9 and 10, an acid anhydride-based cured epoxy resin having an ester bond in its chemical structure was used as the resin component. The solvent of the electrolyte solution in Examples 19 to 21 and Comparative Examples 9 and 10 was composed of glycerin and ethylene glycol, and the ratio of glycerin in the solvent was different. In Example 19, the solvent was entirely glycerin, in Example 20, the solvent contained 40 wt% of glycerin, in Example 21, the solvent contained 30 wt% of glycerin, in Comparative Example 9, the solvent contained 25 wt% of glycerin, and in Comparative Example 10, the solvent was entirely ethylene glycol.

[0090] In Examples 22 to 24 and Comparative Examples 11 and 12, acrylic resin was used as the resin member. The solvent of the electrolyte solution in Examples 22 to 24 and Comparative Examples 11 and 12 was composed of glycerin and ethylene glycol, and the ratio of glycerin in the solvent was different. In Example 22, the solvent was entirely glycerin, in Example 23, the solvent contained 40 wt% of glycerin, in Example 24, the solvent contained 30 wt% of glycerin, in Comparative Example 11, the solvent contained 25 wt% of glycerin, and in Comparative Example 12, the solvent was entirely ethylene glycol.

[0091] The weight change rate is the weight of the resin member changed due to the electrolyte solution absorbed into the resin member. In a temperature environment of 170 ° C, 0.5 g of the resin member was immersed in 5 mL of electrolyte solution solvent and left to stand for 48 hours. After 48 hours, the resin member was removed from the electrolyte solution solvent, excess liquid was wiped off from the surface, and the weight of the resin member after immersion was measured. The initial weight of the resin member was also measured before this 49-hour immersion test. Then, the initial weight was subtracted from the weight after immersion, and the percentage of the difference relative to the initial weight was calculated as the weight change rate.

[0092] Here, this weight change rate has a high correlation with the amount of electrolyte lost. As shown in Table 1 above, the weight change rate was measured along with the amount of electrolyte lost for Examples 1, 4, and 5 and Comparative Examples 1 and 2. Figure 4 is a scatter diagram plotting the weight change rate along with the amount of electrolyte lost for Examples 1, 4, and 5 and Comparative Examples 1 and 2. As shown in Figure 4, there is a high correlation between the weight change rate and the amount of electrolyte lost. In other words, the amount of electrolyte lost can be confirmed from the weight change rate.

[0093] The weight change rates of Examples 1, 4, and 5, Examples 19 to 24, and Comparative Examples 9 to 12 are shown in Table 5 below. (Table 5)

[0094] As shown in Table 5 above, even when various resins such as acid anhydride-based cured epoxy resin or acrylic resin are used as the resin component, the weight change rate is high in the range where the glycerin ratio in the solvent is low, with the boundary being 30 wt%, and the weight change rate is low in the range where the glycerin ratio is high. Since there is a high correlation with the amount of electrolyte loss, in other words, even when various resins such as acid anhydride-based cured epoxy resin or acrylic resin are used as the resin component, the amount of electrolyte loss is high in the range where the glycerin ratio in the solvent is low, with the boundary being 30 wt%, and the amount of electrolyte loss is low in the range where the glycerin ratio is high.

[0095] Therefore, it was confirmed that when at least a portion of the opening side of the case is covered with a resin member, if the glycerin ratio in the solvent of the electrolyte is 30 wt % or more, the amount of electrolyte leakage from the solid electrolytic capacitor is significantly suppressed regardless of the type of resin member.

[0096] Furthermore, as shown in Table 5 above, the weight change rate of the two types of epoxy resins is about one-third of that of the acrylic resin. This confirms that when covering at least a portion of the opening side of the case with a resin member, the loss of electrolyte from the solid electrolytic capacitor can be further suppressed by including 30 wt % or more of glycerin in the solvent for the electrolyte and using epoxy resin as the resin member.

[0097] Furthermore, as shown in Table 5 above, when comparing the weight change rates of amine-cured epoxy resins and acid anhydride-cured epoxy resins, the amine-cured epoxy resins are even better. Amine-cured epoxy resins have a chemical structure without ester bonds, while acid anhydride-cured epoxy resins have a chemical structure with ester bonds. This confirms that when covering at least a portion of the opening side of the case with a resin member, the loss of electrolyte from the solid electrolytic capacitor can be most significantly suppressed by including 30 wt % or more of glycerin in the solvent for the electrolyte and using an epoxy resin without ester bonds as the resin member.

Claims

1. A solid electrolytic capacitor comprising: an anode body having a dielectric film; a cathode body facing the anode body; an electrolyte layer interposed between the anode body and the cathode body and including a solid electrolyte layer and an electrolyte solution; a case accommodating the anode body, the cathode body, and the electrolyte layer; and a resin member covering at least a portion of an opening side of the case, wherein the electrolyte solution includes glycerin accounting for 30 wt % or more of a total amount of solvent.

2. The solid electrolytic capacitor according to claim 1, wherein the electrolyte further comprises ethylene glycol, sulfolane, polyethylene glycol, or a combination thereof.

3. The solid electrolytic capacitor according to claim 1 or 2, wherein the resin member contains an epoxy resin or an acrylic resin.

4. The solid electrolytic capacitor according to claim 3, wherein the resin member contains an epoxy resin.

5. The solid electrolytic capacitor according to claim 4, wherein the resin member contains an epoxy resin having no ester bond.

6. The solid electrolytic capacitor according to claim 4, wherein the resin member contains an amine-based hardener or a phenol-based hardener in addition to the epoxy resin.

7. The solid electrolytic capacitor according to claim 1 or 2, wherein the solid electrolyte layer contains a high-boiling point liquid component having a boiling point of 150° C. or higher and containing a hydroxyl group.

8. The solid electrolytic capacitor according to claim 7, wherein the high boiling point liquid component is ethylene glycol, diethylene glycol, glycerin, diglycerin, polyethylene glycol or a combination thereof.

9. A method for manufacturing a solid electrolytic capacitor comprising the steps of: forming a dielectric film on a surface of an anode body; forming a solid electrolyte layer between the anode body and the cathode body; housing the anode body, the cathode body, and the solid electrolyte layer in a case; impregnating the anode body, the cathode body, and the solid electrolyte layer with an electrolyte solution containing 30 wt % or more of glycerin based on a total amount of solvent; and covering at least a portion of an opening side of the case with a resin member.

Citation Information

Patent Citations

  • Electrolytic capacitor

    JP2016082053A

  • Electrolytic capacitor

    WO2018123525A1

  • Electrolytic capacitor

    WO2021193291A1

  • Solid electrolytic capacitor

    WO2023054502A1