Grain-oriented electromagnetic steel sheet and magnetic domain control method

By controlling strain distribution and optimizing energy ray irradiation conditions, the method addresses the challenge of varying strain intensity in grain-oriented electrical steel sheets, resulting in reduced iron loss and improved magnetic domain control, achieving lower core loss and enhanced magnetic properties.

WO2024225463A1PCT designated stage expired Publication Date: 2024-10-31NIPPON STEEL CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016535
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional methods for reducing iron loss in grain-oriented electrical steel sheets through magnetic domain subdivision do not achieve the expected results due to varying strain intensity caused by laser irradiation, making it difficult for domain walls to move and hinder the reduction of iron loss.

Method used

The method involves controlling the strain distribution by introducing compressive elastic stress through energy ray irradiation, ensuring a gradual change in compressive elastic stress along the plate thickness direction and optimizing energy ray irradiation conditions to maintain domain width refinement while facilitating domain wall mobility, with specific criteria for irradiation power density, beam diameter, and scanning speed.

Benefits of technology

This approach effectively reduces iron loss by ensuring domain walls can move more easily, achieving lower core loss while maintaining the domain width refinement, as evidenced by compressive elastic stress measurements and iron loss characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016535_31102024_PF_FP_ABST
    Figure JP2024016535_31102024_PF_FP_ABST
Patent Text Reader

Abstract

In this grain-oriented electromagnetic steel sheet, in a cross-section orthogonal to the extending direction of an irradiation mark of an energy ray and parallel to the sheet thickness direction, when a virtual line is drawn in the sheet thickness direction so as to include a position where compressive elastic stress measured by EBSD is 20 MPa or more, the degree of change in the compressive elastic stress on the virtual line is 4 MPa or less per 1 μm over the entire region in the sheet thickness direction.
Need to check novelty before this filing date? Find Prior Art

Description

Grain-oriented electrical steel sheet and magnetic domain control method

[0001] The present invention relates to a grain-oriented electrical steel sheet and a magnetic domain control method applicable in the manufacturing process of the grain-oriented electrical steel sheet. This application claims priority to Japanese Patent Application No. 2023-073595, filed on April 27, 2023, the contents of which are incorporated herein by reference.

[0002] Grain-oriented electrical steel sheets are soft magnetic materials primarily used as iron core materials in transformers. Therefore, grain-oriented electrical steel sheets are required to have magnetic properties, including high magnetization and low iron loss. Iron loss is the power loss consumed as thermal energy when an iron core is excited by an alternating current magnetic field. From an energy conservation perspective, iron loss should be as low as possible. The level of iron loss is influenced by factors such as magnetic susceptibility, sheet thickness, coating tension, impurity content, electrical resistivity, grain size, and magnetic domain size. Even though various technologies have been developed for grain-oriented electrical steel sheets, research and development continues to reduce iron loss in order to improve energy efficiency. Laser irradiation has been proposed as one method for reducing iron loss. This technology is believed to reduce eddy current loss by subdividing the magnetic domain width through laser irradiation.

[0003] For example, Patent Document 1 discloses a method for producing a steel sheet having a surface irradiated with a focused continuous wave laser beam while scanning the surface in a direction inclined from the rolling direction of the steel sheet, and a method for repeating the process while shifting the area scanned with the continuous wave laser beam at predetermined intervals, in which the average power of the continuous wave laser beam is represented as P (W), the scanning speed as Vc (mm / s), the predetermined interval as PL (mm), and the input energy Ua as Ua = P / (Vc × PL) (mJ / mm 2 ), 1.0 mm ≦ PL ≦ 3.0 mm, and 0.8 mJ / mm 2 ≦Ua≦2.0mJ / mm 2 Patent Document 1 discloses a method for manufacturing a grain-oriented electrical steel sheet in which magnetic domains are controlled by irradiation with laser light, which method is characterized by satisfying the following: Patent Document 1 shows that it is possible to easily reduce iron loss in both the L direction and the C direction of a grain-oriented electrical steel sheet while ensuring high productivity.

[0004] Furthermore, Patent Document 2 discloses a method for manufacturing a grain-oriented electrical steel sheet in which linear closure domains are formed at approximately regular intervals and approximately perpendicular to the rolling direction of the steel sheet by scanning and irradiating a continuous wave laser beam, thereby improving the iron loss characteristics. 00 It has been shown that grain-oriented electrical steel sheets with reduced iron loss can be obtained by setting the focusing diameter d [mm] of the irradiation beam in the rolling direction, the linear scanning velocity V [mm / s] of the laser beam, and the average laser output P [W] in the ranges of 0<d≦0.2 and 0.001≦P / V≦0.012.

[0005] Patent Document 3 discloses a method for improving the iron loss value of an electrical steel sheet by irradiating the surface of the grain-oriented electrical steel sheet with continuous wave laser light in a direction substantially perpendicular to the rolling direction, in which a circular spot of YAG focused by a flat-field lens is irradiated so as to satisfy predetermined conditions, thereby obtaining an extremely low iron loss value.

[0006] Patent Document 4 describes a steel sheet having a forsterite coating on the surface thereof, with Se-enriched areas in the coating or at least in the interface between the coating and the steel sheet, and the presence ratio of the enriched areas being 10,000 μm on the steel sheet surface in terms of area ratio. 2 This publication discloses a method for producing a grain-oriented electrical steel sheet, which comprises irradiating a grain-oriented electrical steel sheet having a grain size of 2% or more with an electron beam under conditions of a diameter of 0.05 mm to 0.5 mm, a scanning speed of 1.0 m / s or more, and an acceleration voltage of 30 kV or more to subdivide the magnetic domains of the grain-oriented electrical steel sheet.

[0007] Japanese Patent No. 4669565 Japanese Patent No. 4510757 Japanese Patent Application Laid-Open No. 63-83227 International Publication No. 2012 / 017669

[0008] Conventional techniques, including those mentioned above, can achieve a certain degree of iron loss reduction effect by reducing eddy current loss. However, as a result of investigations by the present inventors, it was found that conventional techniques do not achieve the iron loss reduction effect expected from the subdivision of magnetic domain width, and there is room for improvement.

[0009] Therefore, an object of the present invention is to provide a magnetic domain control method for realizing lower iron loss than conventionally in grain-oriented electrical steel sheets, and grain-oriented electrical steel sheets having lower iron loss than conventionally obtained by applying the magnetic domain control method.

[0010] The inventors investigated why conventional techniques have not achieved the iron loss reduction effect expected from the refinement of magnetic domain widths, and found that although the distortion caused by irradiation with a laser or the like is essential for reducing iron loss through irradiation with a laser or the like, the distortion caused by irradiation with a laser or the like varies greatly depending on the location, and in areas where the distortion strength differs greatly, the domain walls become less likely to move, thereby hindering the iron loss reduction effect.

[0011] Therefore, the inventors investigated how to control the strain distribution to facilitate domain wall movement and achieve low iron loss while maintaining the effect of dividing the magnetic domain width. As a result, the inventors discovered that the strain (compressive strain) caused by irradiation with an energy beam such as a laser can be evaluated as compressive elastic stress, and that gradual change in this compressive elastic stress facilitates domain wall movement, resulting in low iron loss.

[0012] The present invention has been made in view of the above findings. The gist of the present invention is as follows. [1] In a grain-oriented electrical steel sheet according to one aspect of the present invention, when a virtual line is drawn in the thickness direction of a cross section perpendicular to the extension direction of an irradiation mark of an energy ray and parallel to the thickness direction of the sheet so as to include a position where the compressive elastic stress measured by EBSD is 20 MPa or more, the degree of change in the compressive elastic stress on the virtual line is 4 MPa or less per μm throughout the thickness direction. [2] In the grain-oriented electrical steel sheet according to [1], the length of the irradiation mark of the energy ray in a direction perpendicular to the extension direction and the thickness direction is defined as the width W of the irradiation mark, and the widths W at five positions in one irradiation mark are defined as W 1 , W 2 , W 3 , W 4 , W 5 Then, the average value W can be expressed by the following formula (6): Ave. may satisfy the following formula (7):Ave. = (W 1 +W 2 +W 3 +W 4 +W 5 ) / 5 (6) 25≦W Ave. ≦200 (7) [3] A magnetic domain control method according to another aspect of the present invention is a method for controlling the magnetic domain of a grain-oriented electrical steel sheet by irradiating the sheet with an energy beam while scanning it in a direction intersecting the rolling direction of the grain-oriented electrical steel sheet, the unit being W / mm 2 The power density of the energy beam at Ip is expressed in mJ / mm 2 When the average irradiation energy density in the scanning direction of the energy beam is Ua, the beam diameter in mm in the scanning direction of the energy beam is d, and the scanning speed of the energy beam in m / s is v, the Ip, Ua, d, and v satisfy the following formulas (1) to (3): Ip≦1500 (1) Ua≧1.5 (2) d / v≧0.00010 (3) In the magnetic domain control method described in [4] and [3], the Ip and Ua may satisfy the following formulas (4) and (5): Ip≦1000 (4) Ua≧2.5 (5)

[0013] According to the above aspects of the present invention, it is possible to provide a magnetic domain control method for realizing lower iron loss than conventionally in a grain-oriented electrical steel sheet, and a grain-oriented electrical steel sheet having lower iron loss than conventionally obtained by applying the magnetic domain control method.

[0014] 1 is a diagram for explaining measurement positions of elastic stress distribution. FIG. 2 is a graph obtained by ImageJ, used for measuring the width of the irradiation mark of an energy beam, with the horizontal axis representing DISTANCE and the vertical axis representing GRAY VALUE.

[0015] A grain-oriented electrical steel sheet according to one embodiment of the present invention (grain-oriented electrical steel sheet according to this embodiment) and a magnetic domain control method applicable to the manufacture of grain-oriented electrical steel sheet (magnetic domain control method according to this embodiment) will be described.

[0016] [Grain-oriented electrical steel sheet] <Compressive elastic stress> As described above, when controlling the magnetic domains of a grain-oriented electrical steel sheet, strain (compressive strain) is introduced by irradiating the sheet with an energy beam such as a laser. However, in regions where the magnitude of the strain caused by the irradiation with the laser beam or the like varies, the domain walls are less likely to move, thereby hindering the iron loss reduction effect. Therefore, in the grain-oriented electrical steel sheet according to this embodiment, the degree of change in the magnitude of the strain caused by the irradiation with the energy beam is made gentler to facilitate the movement of the domain walls while maintaining the effect of subdividing the magnetic domain width. In this embodiment, compressive elastic stress is used as an indicator of the magnitude of this strain. Specifically, in the grain-oriented electrical steel sheet according to this embodiment, when an imaginary line is drawn in the sheet thickness direction so as to include a position where the compressive elastic stress measured by EBSD is 20 MPa or more in a cross section that is orthogonal to the extension direction of the energy beam irradiation marks (scanning direction of the energy beam) and parallel to the sheet thickness direction, the degree of change in the compressive elastic stress on the imaginary line is 4 MPa or less per μm throughout the entire region in the sheet thickness direction.

[0017] If the change in compressive elastic stress (hereinafter, unless otherwise specified, simply referring to elastic stress means compressive elastic stress) exceeds 4 MPa per 1 μm (if the difference in elastic stress between adjacent regions is large), the domain walls become difficult to move, and a sufficient iron loss reduction effect cannot be obtained. A change in elastic stress of 4 MPa or less per 1 μm throughout the entire thickness direction means that when comparing the elastic stress at any point on the imaginary line with the elastic stress at a position 1 μm away from that point in the thickness direction, the difference (absolute value) is 4 MPa or less. To reduce the change in elastic stress, the irradiation conditions of the energy beam can be adjusted, as described below.

[0018] The cross section for measuring the elastic stress is a cross section perpendicular to the extension direction of the energy beam irradiation mark and parallel to the thickness direction (ND), and the change in compressive elastic stress on a virtual line in the thickness direction that includes the position where the elastic stress is 20 MPa or more is measured for the following reason. That is, the elastic stress is introduced below the energy beam irradiation position, and when a region (sometimes referred to as a high elastic stress region) is formed under conventional irradiation conditions where the introduced elastic stress (compressive elastic stress) is 20 MPa or more, the change in elastic stress in the thickness direction is considered to be the largest. Simply reducing the change in elastic stress in other directions, such as the width direction, does not provide a sufficient magnetic domain refinement effect, nor does it provide a magnetic improvement effect. Since the elastic stress in the thickness direction is dominated by the energy beam introduction conditions, such as the beam shape, reducing the change in elastic stress in the width direction does not necessarily reduce the change in elastic stress in the thickness direction. Typically, magnetic domain control is performed by irradiating the surface of the grain-oriented electrical steel sheet with an energy beam such as a laser while scanning the beam in a direction substantially parallel to the width direction of the grain-oriented electrical steel sheet (for example, a direction at an angle of 75 to 105° with respect to the rolling direction). Therefore, the direction perpendicular to the direction in which the irradiation marks of the energy beam extend is often substantially parallel to the rolling direction.

[0019] If there is no region where the compressive elastic stress is 20 MPa or more (high elastic stress region), magnetic domain control will be insufficient. Therefore, the grain-oriented electrical steel sheet according to this embodiment is based on the premise that there is a high elastic stress region.

[0020] The elastic stress and the change in elastic stress in the thickness direction are determined by the following method. FIG. 1 shows the case where laser irradiation is performed in a direction perpendicular to the rolling direction (RD) (parallel to the width direction (TD)). In this case, as shown in FIG. 1, cross sections parallel to the rolling direction (RD) and the thickness direction (ND) are used as the measurement surfaces. Since elastic stress is introduced by irradiation with an energy beam, a region of this measurement surface, centered at the energy beam irradiation position IM, spanning the entire thickness direction and having a width twice the energy beam irradiation width IW, is used as the measurement region MR, and map measurement is performed using electron backscatter diffraction (EBSD). During map measurement, an electron beam is irradiated onto a sample with the measurement surface tilted 70 degrees with respect to the electron beam irradiation direction in steps of 1 μm or less to obtain an EBSD image. The obtained image is saved as 956 × 956 pixels, and strain calculation is performed using CrossCourt4 from BLG Vantage to calculate the elastic stress. This identifies a high elastic stress region R where an elastic stress (compressive elastic stress) of 20 MPa or more has been introduced. For measurement, the EBSD analysis surface must be subjected to surface treatment to remove mechanical strain due to polishing or cross-section processing. For example, a method can be used in which the analysis surface is mirror-polished and then the processed strain layer due to polishing is sputtered away with an argon ion beam. Then, a virtual line VL is drawn parallel to the thickness direction (ND) passing through this high elastic stress region R. At each measurement point on this virtual line VL, the strain intensity is compared with that at a measurement point moved 1 μm in the thickness direction. If the difference in elastic stress at all measurement points from a measurement point moved 1 μm in the thickness direction is 4 MPa or less, it is determined that the difference in elastic stress is 4 MPa or less per μm throughout the entire thickness direction. Typically, a region of high elastic stress is formed at a position slightly away from the surface below the irradiation position (toward the center of the thickness), but the reference position of the virtual line does not matter as long as the point has an elastic stress of 20 MPa or more.

[0021] Irradiation of energy rays for magnetic domain control is usually carried out multiple times at regular intervals so that the irradiation positions (determined by irradiation marks (which can be distinguished visually or by observing the surface magnetic domains) in the final grain-oriented electrical steel sheet) are parallel, as shown in Figure 1. If the above conditions are satisfied at at least one irradiation position, the effect at that position can be obtained, but from the perspective of improving the properties of the grain-oriented electrical steel sheet, it is preferable that the degree of change in elastic stress is as described above at all positions.

[0022] Furthermore, in the grain-oriented electrical steel sheet according to this embodiment, it is preferable that the irradiation marks are continuous and linear, and that the change in width of each irradiation mark is small. By making the change in width of the irradiation mark small, elastic stress is introduced in the sheet width direction without leakage or overlap, and a sufficient magnetic domain refinement effect is obtained, and as a result, a sufficient magnetic improvement effect is obtained. Specifically, the length in the direction perpendicular to the extension direction and the sheet thickness direction is defined as the width W of the irradiation mark, and the widths W at five points in each irradiation mark are defined as W 1 , W 2 , W 3 , W 4 , W 5 Then, the average value W can be expressed by the formula (6) Ave. It is preferable that W satisfies the following formula (7): Ave. = (W 1 +W 2 +W 3 +W 4 +W 5 ) / 5 (6) 25≦W Ave. ≦200 (7)

[0023] The width W of the irradiation scar is measured using a technique called reflection X-ray topography. The X-ray topography device used is a Rigaku XRTmicron, with a Cu target as the X-ray source. The diffraction plane during imaging is (310). The CCD resolution is 2.4 μm, and the digital resolution is 16-bit. Specifically, a 100 mm x 100 mm (× plate thickness) insulating coated material with energy beam irradiation scars is first prepared, and topography images of five fields of view on the same energy beam in the plate width direction are captured using SnapShot in high-resolution mode. The field diameter during imaging is 6-7 mm in the plate width direction and 7-8 mm in the rolling direction. Time delay integration (TDI) scanning may be performed in advance to determine the imaging location. Next, the specific irradiation scars are calculated from the captured topography images using image analysis software called ImageJ. Specifically, the topography image is developed on ImageJ, and the analysis range, ROI (Range of Interest) is set (pixel width and height are 2.406 μm). The ROI is rectangular, and its range is 646 pixels (equivalent to approximately 1.55 mm) in the rolling direction and 84 pixels (equivalent to approximately 0.20 mm) in the plate width direction. Hereinafter, the side parallel to the rolling direction will be referred to as the long side of the ROI, and the side parallel to the plate width direction will be referred to as the short side of the ROI. The ROI is set so that the irradiation mark fits within the rectangle. At this time, visual inspection is also acceptable, so set so that the irradiation mark is located at the center of the long side of the ROI. Once the ROI setting is complete, a graph is drawn within the ROI setting range, with the horizontal axis representing DISTANCE and the vertical axis representing GRAY VALUE. The graph drawing function is part of the functions of ImageJ and is used. This results in a spectrum with a negative peak, as shown in Figure 2. The gray scale is read at both ends of the spectrum, and their average value is calculated. Hereafter, this average value is referred to as I Ave. The negative peak intensity (minimum value of the spectrum) in the spectrum is called I Bottom Let's say. Ave. and I Bottom The difference is ΔI Height Here, I, which can be defined by the following equation (8), HHThe concept of (Half Height) is introduced. HH is the Gray Scale value corresponding to half the peak intensity. HH is defined as the distance between two points corresponding to I. HH  =I Height + (0.5 × I Height ) ... (8) According to this method, W (μm) in each of the five fields of view is measured, and each field of view is assigned a number from 1 to 5. That is, the widths W at the five points are designated as W 1 , W 2 , W 3 , W 4 , W 5 This W 1 , W 2 , W 3 , W 4 , W 5 Calculate the arithmetic mean of W Ave. Let's say.

[0024] <Thickness> There are no limitations on the thickness of the grain-oriented electrical steel sheet (the thickness of the base steel sheet excluding the glass coating and insulating coating, if any). A thinner thickness increases the effect of magnetic domain control, so a thickness of 0.15 mm to 0.23 mm is preferable.

[0025] <Chemical Composition> The chemical composition of the grain-oriented electrical steel sheet (the chemical composition of the base steel sheet excluding the glass coating and insulating coating, if any) is not limited and may be selected from known ranges depending on the properties required of the grain-oriented electrical steel sheet. For example, a chemical composition containing C: 0.010% or less, Si: 3.00 to 4.00%, Mn: 0.01 to 0.50%, N: 0.010% or less, sol. Al: 0.020% or less, S: 0.010% or less, P: 0.030% or less, Cr: 0 to 0.50%, Sn: 0 to 0.50%, Cu: 0 to 0.50%, Se: 0 to 0.020%, Sb: 0 to 0.50%, Mo: 0 to 0.10%, with the balance being Fe and impurities is exemplified.

[0026] <Glass Coating> The grain-oriented electrical steel sheet according to this embodiment may have a known glass coating formed on the surface of the base steel sheet. The glass coating is an inorganic coating mainly composed of magnesium silicate. The glass coating is formed by a reaction between an annealing separator containing magnesia (MgO) applied to the surface of the base steel sheet and the components of the surface of the base steel sheet during finish annealing, and has a composition derived from the components of the annealing separator and the base steel sheet ... 2 SiO 4 phase and MgAlO 4 In addition to these phases, precipitates may be contained in an amount of about 1% by area or less.

[0027] <Insulating Coating> In the grain-oriented electrical steel sheet according to this embodiment, a known insulating coating (tensioning insulating coating) may be formed on the surface of the base steel sheet or on the surface of the glass coating. The insulating coating imparts electrical insulation to the grain-oriented electrical steel sheet, thereby reducing eddy current loss and improving the iron loss characteristics of the grain-oriented electrical steel sheet (reducing iron loss). In addition to the electrical insulation described above, the insulating coating also provides various other properties, such as corrosion resistance, heat resistance, and slip resistance. Furthermore, the insulating coating has the function of applying tension to the grain-oriented electrical steel sheet. By applying tension to the grain-oriented electrical steel sheet and facilitating domain wall movement in the grain-oriented electrical steel sheet, the iron loss characteristics of the grain-oriented electrical steel sheet can be improved (reduced iron loss). The insulating coating is formed, for example, by applying a coating liquid mainly composed of metal phosphate and silica to the surface of the glass coating and baking it.

[0028] [Magnetic Domain Control Method] In the magnetic domain control method according to this embodiment, a grain-oriented electrical steel sheet is irradiated with an energy beam while scanning it in a direction intersecting the rolling direction (for example, a direction at an angle of 30 to 150°, preferably 75 to 105°, relative to the rolling direction), thereby controlling the magnetic domains of the grain-oriented electrical steel sheet. Conventional methods of inducing strain (and the resulting elastic stress) by using a temperature difference generated in the steel sheet during energy beam irradiation involve irradiating the steel sheet with a high-energy beam for a short period of time to induce elastic stress. This results in a large temperature difference in the steel sheet, resulting in localized areas with large elastic stress. In the magnetic domain control method according to this embodiment, energy beam irradiation is performed so that the irradiation time at each position is longer than under conventional general irradiation conditions, thereby inducing sufficient elastic stress (compressive elastic stress) while gradually changing the elastic stress. To achieve this, the power density of the energy beam is reduced, the average irradiation energy density is increased, and the time during which the energy beam is irradiated at one point on the steel sheet is prolonged. Specifically, in the magnetic domain control method according to this embodiment, the unit of W / mm is used. 2 The power density of the energy beam at Ip is expressed in mJ / mm 2 The energy beam is irradiated so that Ip, Ua, d, and v satisfy the following formulas (1) to (3), where Ua is the average irradiation energy density in the scanning direction of the energy beam, d is the beam diameter in mm, and v is the scanning speed of the energy beam in m / s. Ip≦1500 (1) Ua≧1.5 (2) d / v≧0.00010 (3), where d / v corresponds to the time (s) during which the energy beam is irradiated to a point on the steel sheet. If any one of formulas (1) to (3) is not satisfied, there is a concern that the degree of change in elastic stress in the sheet thickness direction will exceed 4 MPa per μm. There is no lower limit for Ip, but Ip may be 100 or more in order to effectively generate magnetic domain refinement. Although there is no upper limit for Ua, from the viewpoint of not deteriorating noise characteristics, Ua should be 5.0 or less, or 3.0 or less, since better noise characteristics can be obtained. There is no upper limit for d / v, but d / v may be 0.00100 or less.

[0029] As described above, in conventional methods for introducing elastic stress by the temperature difference that occurs in a steel sheet during energy beam irradiation, the energy beam has generally been irradiated for a short period of time. When a coating is formed on the surface of a grain-oriented electrical steel sheet, attempts have been made to widen the beam diameter to prevent the coating from breaking, but extending the irradiation time beyond the range where the coating is not deteriorated would reduce the elastic stress and also lead to reduced productivity, and this has not been considered. The present inventors focused on the degree of change in elastic stress and discovered that significant effects can be obtained by irradiating energy beams under the above-described conditions, which have not been set in the past.

[0030] It is preferable that Ip and Ua satisfy the following formulas (4) and (5): Ip≦1000 (4) Ua≧2.5 (5)

[0031] In the magnetic domain control method according to this embodiment, the energy beam is, for example, a laser or an electron beam. However, in the case of a pulsed wave, elastic stress changes in the scanning direction, and it is difficult to ensure a long irradiation time as in the magnetic domain control method according to this embodiment. Therefore, a continuous wave energy beam, such as a continuous wave laser, is used as the energy beam. For example, by using a continuous wave laser, it is possible to achieve a wavelength of 25 μm≦W Ave. It is possible to obtain a grain-oriented electrical steel sheet having irradiation marks that satisfy the following criteria:

[0032] The steel sheet subjected to magnetic domain control may be a known grain-oriented electrical steel sheet, and its manufacturing method is not particularly limited. That is, magnetic domain control may be performed on grain-oriented electrical steel sheets manufactured by any manufacturing method. A typical grain-oriented electrical steel sheet is manufactured by a manufacturing method including the following steps. a hot rolling process in which a steel billet such as a slab is heated and hot-rolled to form a hot-rolled steel sheet; a hot-rolled sheet annealing process in which the hot-rolled steel sheet is annealed; a pickling process in which the hot-rolled steel sheet after the hot-rolled sheet annealing process is pickled; a cold rolling process in which the hot-rolled steel sheet after the pickling process is cold-rolled once or multiple times with annealing in between to form a cold-rolled steel sheet; a decarburization annealing process in which the cold-rolled steel sheet is decarburized; a finish annealing process in which an annealing separator mainly composed of MgO powder is applied to the front and back surfaces of the cold-rolled steel sheet after the decarburization annealing process, which is the base steel sheet, and then dried and finish annealed to form a glass coating; and a coating forming process in which an insulating coating is formed on the glass coating. Furthermore, when obtaining a grain-oriented electrical steel sheet having the chemical composition exemplified above, taking into consideration that the contents of some elements change due to decarburization, finish annealing, and the like, a steel slab may be used that contains, in mass%, C: 0.010 to 0.200%, Si: 3.00 to 4.00%, sol. Al: 0.010 to 0.040%, Mn: 0.01 to 0.50%, N: 0.020% or less, S: 0.005 to 0.040%, P: 0.030% or less, Cu: 0 to 0.50%, Cr: 0 to 0.50%, Sn: 0 to 0.50%, Se: 0 to 0.020%, Sb: 0 to 0.50%, Mo: 0 to 0.10%, with the balance being Fe and impurities.

[0033] The grain-oriented electrical steel sheet of the present invention will be described in more detail using examples. The examples shown below are merely examples of the grain-oriented electrical steel sheet and the manufacturing method thereof according to the present invention, and the grain-oriented electrical steel sheet and the manufacturing method thereof according to the present invention are not limited to the examples below.

[0034] A grain-oriented electrical steel sheet having a thickness of 0.23 mm and consisting of 0.010% C, 3.30% Si, 0.10% Mn, 0.007% S, 0.030% acid-soluble Al, 0.008% N, 0.06% Sn, and the balance being Fe and impurities was subjected to magnetic domain control by laser irradiation, scanning in a direction perpendicular to the rolling direction at a pitch of 5 mm in the rolling direction under the conditions shown in Table 1. From the grain-oriented electrical steel sheet after magnetic domain control, multiple samples measuring 500 mm in the rolling direction including the irradiation position and 100 mm in the sheet width direction were cut out. The elastic stress distribution and magnetic properties of these samples were evaluated using the methods described below.

[0035] [Elastic Stress Distribution] A map measurement was performed using electron backscatter diffraction (EBSD) on a cross section parallel to the rolling direction (RD) and the thickness direction (ND), with the measurement area being a region extending across the entire thickness direction with a width twice the irradiation width of the energy beam centered on the irradiation position of one energy beam. For the map measurement, an electron beam was irradiated onto a sample with a cross section to be measured, tilted 70 degrees with respect to the irradiation direction of the electron beam, in steps of 2 μm or less, to obtain an EBSD image. The obtained image was saved as a 956 × 956 pixel image, and strain calculations were performed using CrossCourt4 from BLG Vantage to calculate the elastic stress in the rolling direction. The reference point for strain and elastic stress was the point farthest from the irradiation position of the energy beam within the measurement range of the cross section of the grain-oriented electrical steel sheet, or its vicinity (within a range of about 10 pixels). A measurement point where the compressive elastic stress was 20 MPa or more was selected, and the compressive elastic stress at each measurement point on a virtual line parallel to the thickness direction passing through that measurement point was compared with the compressive elastic stress at a point moved 1 μm in the thickness direction. However, in cases where there was no measurement point where the compressive elastic stress was 20 MPa or more (examples where "NO" is written in the "Is the maximum compressive elastic stress 20 MPa or more?" column in the table), the compressive elastic stress at each measurement point on a virtual line parallel to the thickness direction passing through the measurement point where the compressive elastic stress was maximum was compared with the compressive elastic stress at a point moved 1 μm in the thickness direction. If the maximum difference in elastic stress was 4 MPa or less, it was determined that the degree of change in elastic stress was small.

[0036] [Magnetic Properties] A sample of 60 mm wide x 300 mm long was taken from the center of the grain-oriented electrical steel sheet. The length of the sample was parallel to the rolling direction. Using this sample, the iron loss W at a frequency of 50 Hz and a maximum magnetic flux density of 1.7 T was measured in accordance with JIS C2556 (2015). 17/50 (W / kg) was measured. 17/50 If the iron loss was less than 0.740 W / Kg, it was determined to have low iron loss. Furthermore, using the above sample, the magnetic flux density (T) was determined by a single sheet magnetic property test (SST test) in accordance with JIS C2556 (2015). Specifically, a magnetic field of 800 A / m was applied to the sample to determine the magnetic flux density (T).

[0037]

[0038] As can be seen from Table 1, for Examples 1 to 8, in which magnetic domain control was performed under conditions where Ip, Ua, and d / v were within the ranges of the present invention, the maximum compressive elastic stress was 20 MPa or more and the difference in compressive elastic stress was 4 MPa or less. As a result, excellent iron loss characteristics were obtained. In contrast, in Comparative Examples 1 to 9, Ip, Ua, or d / v were outside the ranges of the present invention, and the maximum compressive elastic stress was less than 20 MPa or the maximum difference in compressive elastic stress exceeded 4 MPa. As a result, the iron loss characteristics were poor.

[0039] According to the present invention, it is possible to provide a magnetic domain control method for realizing lower iron loss than conventionally in grain-oriented electrical steel sheets, and grain-oriented electrical steel sheets having lower iron loss than conventionally obtained by applying the magnetic domain control method.

[0040] TD Plate width direction RD Rolling direction ND Plate thickness direction IM Irradiation position IW Irradiation width MR Measurement area R Area where compressive elastic stress is 20 MPa or more (high elastic stress area) VL Virtual line

Claims

1. A grain-oriented electrical steel sheet, characterized in that, in a cross section perpendicular to the extension direction of the energy beam irradiation marks and parallel to the sheet thickness direction, when a virtual line is drawn in the sheet thickness direction so as to include a position where the compressive elastic stress measured using EBSD is 20 MPa or more, the degree of change in the compressive elastic stress on the virtual line is 4 MPa or less per μm over the entire region in the sheet thickness direction.

2. The length of the irradiation mark of the energy beam in the direction perpendicular to the extension direction and the plate thickness direction is defined as the width W of the irradiation mark, and the widths W at five points in one irradiation mark are defined as W 1 , W 2 , W 3 , W 4 , W 5 Then, the average value W can be expressed by the following formula (6): Ave. The grain-oriented electrical steel sheet according to claim 1, characterized in that W satisfies the following formula (7). Ave. = (W 1 +W 2 +W 3 +W 4 +W 5 ) / 5 (6) 25≦W Ave. ≦200 (7) 3. A method for controlling the magnetic domains of a grain-oriented electrical steel sheet by scanning and irradiating the sheet with an energy beam in a direction intersecting the rolling direction of the sheet, the method being expressed in units of W / mm 2 The power density of the energy beam at 2 a beam diameter in the scanning direction of the energy beam in the unit of mm, and a scanning speed of the energy beam in the unit of m / s, v, the Ip, Ua, d, and v satisfy the following formulas (1) to (3): Ip≦1500 (1) Ua≧1.5 (2) d / v≧0.00010 (3) 4. The magnetic domain control method according to claim 3, wherein the Ip and the Ua satisfy the following expressions (4) and (5): Ip≦1000 (4) Ua≧2.5 (5)

Citation Information

Patent Citations

  • Improvement of iron loss value of electrical steel sheet

    JP1988083227A

  • Game machine

    JP2023073595A

  • Grain-oriented electrical steel sheet with excellent magnetic properties and its manufacturing method

    JP4510757B2

  • A method for manufacturing grain-oriented electrical steel sheets in which magnetic domains are controlled by laser irradiation.

    JP4669565B2

  • Grain-oriented electrical steel sheet, and method for producing same

    WO2012017669A1