Method for recycling lithium-ion battery

By using a system of carbon dioxide supply in the recovery process of lithium-ion batteries for pyrolysis, combining the synergistic effects of zeolite molecular sieve and bicarbonate, diluting organic gases and adsorbing carbon dioxide, solving the problems of explosion risks and high costs, and achieving safe and efficient recycling process.

WO2024229724A1PCT designated stage expired Publication Date: 2024-11-14GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
PCT/CN2023/093116
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Explosion accidents are prone to occur during the recycling process of existing lithium-ion batteries, and the use cost of inert gas is high, making it difficult to ensure safety and reduce carbon emissions.

Method used

The pyrolysis is carried out using a system containing carbon dioxide supply, carbon dioxide is released through a mixture of zeolite molecular sieve and bicarbonate, the organic gas is diluted, the risk of explosion is reduced, and carbon dioxide is adsorbed through zeolite molecular sieve to achieve recycling.

Benefits of technology

Reduces recycling costs, improves safety, ensures safety of the pyrolysis process, and achieves reduction of carbon emissions and regeneration of zeolite molecular sieves without increasing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023093116_14112024_PF_FP_ABST
    Figure CN2023093116_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery recycling. Disclosed is a method for recycling a lithium-ion battery. The method for recycling a lithium-ion battery provided in the present application comprises: pyrolyzing a crushed lithium-ion battery in air atmosphere, performing a thermal reaction thereon after the pyrolysis is finished, and screening same after the thermal reaction is finished to obtain an undersize black powder; collecting the gas generated by both the pyrolysis and the thermal reaction and condensing the gas to obtain an electrolyte component; and adding a carbon dioxide provider during the pyrolysis process, wherein the carbon dioxide provider comprises a zeolite molecular sieve or a mixture of a zeolite molecular sieve and a bicarbonate. The recycling method provided in the present application has high safety.
Need to check novelty before this filing date? Find Prior Art

Description

A method for recycling lithium-ion batteries Technical Field

[0001] The present application belongs to the technical field of battery recycling, and in particular relates to a method for recycling ion batteries. Background Art

[0002] With the development of new energy vehicles, sales of lithium-ion batteries have steadily increased. Using new energy vehicles can significantly conserve mineral energy and contribute to carbon emissions reductions. However, as power batteries are used, their performance inevitably degrades. When they degrade to 80% of their original performance, they no longer meet the standards for use in new energy vehicles. Consequently, a large number of retired power batteries will emerge over time. The safe and environmentally friendly disposal of these retired batteries has become a major challenge for the new energy industry.

[0003] Currently, used power batteries are typically discharged to below a safe voltage before being crushed. After crushing, the electrolyte is typically recovered or removed through pyrolysis. However, the carbonate organic solvents in the electrolyte are easily decomposed and volatile, with a low flash point and high flammability, making them prone to explosions during processing. Therefore, avoiding these types of accidents is crucial. Pyrolysis in an inert atmosphere is often used to avoid this, but the inert gas used is expensive, and the subsequent cost of recovering the inert gas is also relatively high, increasing the cost of the processing.

[0004] The recycling of used power batteries will inevitably produce escaped carbon dioxide in each process section and plant area. Compared with the concentrated carbon dioxide emitted during the pyrolysis process, the carbon dioxide released into the atmosphere during other process sections is difficult to collect and utilize. Therefore, it is very difficult to ensure the safety of the pyrolysis process while reducing carbon emissions from the entire process section.

[0005] Summary of the Invention

[0006] The purpose of this application is to overcome the shortcomings of the above-mentioned prior art and provide a low-cost, high-safety lithium-ion battery recycling method.

[0007] To achieve the above-mentioned objectives, the technical solution adopted in the present application is: a lithium-ion battery recycling method, which comprises the following steps: pyrolyzing the crushed lithium-ion battery, performing a thermal reaction after the pyrolysis, and screening after the thermal reaction to obtain black powder under the sieve; simultaneously collecting and condensing the gases generated by the pyrolysis and thermal reaction to obtain electrolyte components; adding a carbon dioxide provider during the pyrolysis process; the carbon dioxide provider comprises a zeolite molecular sieve or a mixture of a zeolite molecular sieve and a bicarbonate.

[0008] In a lithium-ion battery recycling method provided in the present application, by placing the crushed lithium-ion batteries in a system containing a carbon dioxide provider for pyrolysis, the use of inert gas can be avoided, thereby reducing recycling costs and achieving excellent economic benefits. The present application further specifies that the carbon dioxide provider includes a zeolite molecular sieve or a mixture of a zeolite molecular sieve and a bicarbonate. During the pyrolysis process, the zeolite molecular sieve and the bicarbonate continuously release carbon dioxide gas, thereby timely diluting the organic gas generated during the pyrolysis process of the lithium-ion battery to below the lower explosion concentration limit (typically a volume fraction of 5%), thereby ensuring the safety of the recycling process.

[0009] In one embodiment, the pyrolysis is performed in an air atmosphere.

[0010] The inventors have found that by adopting the technical solution of the present application, when pyrolysis is carried out in a system containing a carbon dioxide provider, there are no requirements for the pyrolysis system and it can be carried out directly in an air atmosphere, which reduces the operational requirements.

[0011] In one embodiment, the zeolite molecular sieve is at least one selected from JLOX-500 zeolite molecular sieve and 5A zeolite molecular sieve.

[0012] The inventors have found that when the zeolite molecular sieve is further selected as JLOX-500 zeolite molecular sieve and / or 5A zeolite molecular sieve, on the one hand, the two zeolite molecular sieves can release carbon dioxide more effectively in the presence of pyrolysis gas, thereby ensuring that the volume fraction of organic gas generated by the pyrolysis of lithium-ion batteries is lower during the recovery process, that is, the safety is better; on the other hand, the two zeolite molecular sieves can also be effectively used for the adsorption of carbon dioxide generated during the overall recovery process, especially the adsorption of carbon dioxide generated during the treatment of pyrolysis gas, thereby completing the regeneration of the zeolite molecular sieve while reducing carbon emissions, without increasing energy consumption.

[0013] In one embodiment, the cation in the bicarbonate salt is potassium ion, sodium ion or ammonium ion.

[0014] In one embodiment, the bicarbonate is selected from at least one of potassium bicarbonate and sodium bicarbonate.

[0015] The inventors have found that further selecting bicarbonate as the above type can have a good synergistic effect with the zeolite molecular sieve, effectively releasing carbon dioxide, reducing the volume fraction of explosive organic gas, and improving safety.

[0016] In one embodiment, the mass ratio of the carbon dioxide provider to the lithium-ion battery is zeolite molecular sieve: lithium-ion battery = 1: (50-100).

[0017] In one embodiment, the mass ratio of the carbon dioxide provider to the lithium-ion battery is zeolite molecular sieve: lithium-ion battery = 1: (70-90).

[0018] The inventors have studied that when the mass ratio of the carbon dioxide provider to the lithium-ion battery is selected to be 1:(50-100), especially 1:(70-90), on the one hand, it can ensure that the carbon dioxide produced by the carbon dioxide provider can fully and effectively dilute the organic gas produced by pyrolysis, making it far below the lower limit of the explosion concentration; on the other hand, it can also avoid the situation where the volume fraction and recovery rate of the explosive organic gas do not change much even if the carbon dioxide provider increases further. That is, while taking economic benefits into consideration at the same time, economic benefits and actual excellent results can be achieved within the mass ratio range provided in this application.

[0019] In one embodiment, in the mixture of zeolite molecular sieve and bicarbonate, the mass ratio of bicarbonate to zeolite molecular sieve is bicarbonate:zeolite molecular sieve=1:(5-20).

[0020] In one embodiment, in the mixture of zeolite molecular sieve and bicarbonate, the mass ratio of bicarbonate to zeolite molecular sieve is bicarbonate:zeolite molecular sieve=1:(9-15).

[0021] The inventors have found that when bicarbonate is added during the pyrolysis stage, it will decompose and produce carbon dioxide due to the high-temperature reaction, which can synergize with the zeolite molecular sieve to jointly improve the safety of the recovery process and reduce the volume fraction of organic gases produced by pyrolysis; at the same time, in the subsequent thermal reaction stage, the carbonate produced after the decomposition of bicarbonate can further absorb the HF produced in the thermal reaction process, which is beneficial to reducing environmental pollution; and the inventors have found that when the mass ratio of bicarbonate to zeolite molecular sieve is 1:(5-20), especially 1:(9-15), the synergistic effect of bicarbonate and zeolite molecular sieve is more obvious during the pyrolysis stage, and the volume fraction of explosive organic gases produced by pyrolysis can be more effectively diluted.

[0022] In one embodiment, the pyrolysis is performed by heating to 200-400° C. at a heating rate of 0.5-3° C. / min and keeping the temperature for 1-2 hours.

[0023] In one embodiment, the pyrolysis is performed by heating to 300-350° C. at a heating rate of 1-2° C. / min and keeping the temperature for 1-2 hours.

[0024] The inventors have studied that the heating rate and insulation temperature during the pyrolysis process will affect the safety of the recovery process. When heating to 200-400℃ at a heating rate of 0.5-3℃ / min and keeping warm for 1-2h, especially heating to 300-350℃ at a heating rate of 1-2℃ / min and keeping warm for 1-2h, safety can be improved.

[0025] In one embodiment, the thermal reaction is heating to 500-650° C. at a heating rate of 3-7° C. / min and keeping the temperature for 3-5 hours.

[0026] In one embodiment, the diameter of the crushed lithium-ion battery is 1-3 mm, and the crushing process is performed under a protective gas environment.

[0027] In one embodiment, the lithium-ion battery is a waste lithium-ion battery that is safely discharged and then crushed.

[0028] In one embodiment, the inert gas is selected from at least one of nitrogen, argon, and carbon dioxide.

[0029] Crushing under inert gas can further ensure the safety of the recovery process. Crushing it to a diameter of 1-3 mm can increase the surface area of ​​pyrolysis and thermal reactions on the one hand, and prevent it from entering the silo and mixing with the zeolite molecular sieve, which is not conducive to subsequent screening on the other hand.

[0030] In one embodiment, the condensation is water cooling, and the temperature of the water is 10-30°C.

[0031] In one embodiment, after the electrolyte components are obtained by condensing, the process further includes the steps of absorbing the uncondensed gas with alkaline solution and burning it.

[0032] In one embodiment, the alkali solution absorption is direct alkali solution absorption or spray absorption.

[0033] In one embodiment, the alkali solution is selected from at least one of a sodium bicarbonate aqueous solution, a potassium bicarbonate aqueous solution, a potassium hydroxide aqueous solution, and a sodium hydroxide aqueous solution with a concentration of 1-5 mol / L.

[0034] In one embodiment, the alkali solution is a sodium hydroxide aqueous solution with a concentration of 1-5 mol / L.

[0035] The inventors have found that the use of dilute alkali solution within the above concentration range can recover phosphorus pentafluoride produced in the pyrolysis stage and the thermal reaction stage, and the water vapor in the dilute alkali solution can further help prevent explosions.

[0036] In one embodiment, after combustion, the gas is further purified to obtain purified carbon dioxide, which is then adsorbed by a zeolite molecular sieve, thereby achieving regeneration of the zeolite molecular sieve and simultaneously achieving the effect of reducing carbon emissions.

[0037] In addition, the present application also provides a lithium-ion battery recovery device, which is a rotary kiln 11, and an air inlet 12 and an air outlet 13 are respectively provided on the left and right ends of one side of the rotary kiln 11. The rotary kiln 11 also includes a silo 14, which is a hollow cavity and is horizontally arranged along the central axis of the hollow cavity. One end of the silo 14 is opened as a zeolite molecular sieve inlet and outlet 15, and the air outlet 13 of the rotary kiln 11 is connected to the exhaust gas absorption device 16.

[0038] On the other hand, the present application also provides an application of the lithium-ion battery recycling device in lithium-ion battery recycling, which includes the following steps: placing the zeolite molecular sieve into the hollow cavity of the hopper 14, placing the crushed lithium-ion battery in the cavity of the non-hopper part of the rotary kiln 11, and then pyrolyzing; after the pyrolysis is completed, the zeolite molecular sieve is removed and a thermal reaction is carried out, and after the thermal reaction is completed, it is sieved to obtain black powder under the sieve; at the same time, the gases generated by the pyrolysis and thermal reaction are collected and condensed to obtain electrolyte components.

[0039] In one embodiment, hopper 14 is a perforated hopper with a pore diameter of 0.5-0.8 mm. Therefore, the diameter of the zeolite molecular sieve added in this application is 1-3 mm, ensuring that the zeolite molecular sieve does not leak from the pores in hopper 14. This further ensures that the zeolite molecular sieve does not physically contact the crushed lithium ions, facilitating subsequent screening. In one embodiment, the filling rate of the crushed lithium-ion batteries in the rotary kiln 11 is 5-25%.

[0040] Compared with the prior art, the present invention has the following advantages:

[0041] First, the present application provides a lithium-ion battery recycling method that conducts pyrolysis in an air stream under the action of a carbon dioxide provider. This allows the carbon dioxide provider to reduce the oxygen concentration in the pyrolysis system. Furthermore, the carbon dioxide generated by the carbon dioxide provider under pyrolysis conditions can promptly dilute the organic gases produced by pyrolysis to the lower limit of their explosive concentration, thereby reducing the possibility of explosion and ensuring the safety of the pyrolysis process. Furthermore, by introducing the carbon dioxide provider, the present application avoids the use of the currently widely used inert gas for the pyrolysis reaction, thereby reducing the cost of the recycling process and achieving excellent economic benefits.

[0042] Second, the zeolite molecular sieve in the carbon dioxide supply used in this application can be used to adsorb carbon dioxide gas generated in other stages or other processes in the plant after being taken out after use in the pyrolysis reaction stage. In particular, the carbon dioxide generated in the pyrolysis stage and the thermal reaction stage after tail gas treatment can be adsorbed and then placed in the pyrolysis reaction for use, thereby realizing the recycling of the zeolite molecular sieve and achieving the effect of carbon emission reduction without increasing energy consumption.

[0043] Third: The recovery method provided by the present application is simple to operate, does not require complex equipment, and the recovery process is highly safe. After the pyrolysis reaction stage is completed, the volume fraction of explosive organic gas is below 2.98%. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] FIG1 is a process flow chart of Example 1 of the present application;

[0045] FIG2 is a schematic diagram of a rotary kiln during the recovery process of Example 1 of the present application; 11-rotary kiln, 12-air inlet, 13-air outlet, 14-bin, 15-zeolite molecular sieve inlet and outlet, 16-tail gas absorption device. DETAILED DESCRIPTION

[0046] In order to better illustrate the purpose, technical solutions and advantages of this application, this application will be further described below in conjunction with specific embodiments.

[0047] Unless otherwise specified, the reagents, methods and equipment used in this application are conventional reagents, methods and equipment in the art.

[0048] Example 1

[0049] The present invention provides a method for recycling lithium-ion batteries. The specific process flow chart is shown in FIG1 , and the rotary kiln equipment used is shown in FIG2 . The specific recycling process includes the following steps:

[0050] (1) Add 10 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm into the silo of the rotary kiln (the silo pore size is 0.6 mm);

[0051] (2) Discharging and crushing waste lithium-ion batteries to a diameter of 2 mm under an argon atmosphere, then adding 700 g of the crushed lithium-ion batteries to the non-bin portion of a rotary kiln (filling rate of 14%), and then heating to 300 ° C at a heating rate of 1 ° C / min in an air atmosphere for 1.5 h to carry out a pyrolysis reaction;

[0052] (3) After the pyrolysis reaction is completed, the zeolite molecular sieve is removed and then heated to 550°C at a heating rate of 4°C / min and kept at this temperature for 3.5 h for thermal reaction;

[0053] (4) After the thermal reaction is completed, the product is broken up and sieved, and the black powder under the sieve is collected;

[0054] (5) Cooling the pyrolysis tail gas in step (2) and the thermal reaction tail gas in step (3) in water at a temperature of 25° C. and collecting the electrolyte components;

[0055] (6) The uncondensed portion of the gas in step (5) is sprayed and absorbed with a sodium bicarbonate aqueous solution having a concentration of 3 mol / L, and then the unabsorbed portion of the gas is collected and burned, and the burned gas is purified to obtain carbon dioxide, which is then adsorbed using the zeolite molecular sieve taken out in step (3).

[0056] Example 2

[0057] The present invention provides a method for recycling lithium-ion batteries. The specific recycling process includes the following steps:

[0058] (1) Add 10 g of 5A zeolite molecular sieve with a diameter of 1 mm into the silo of the rotary kiln (the silo pore size is 0.6 mm);

[0059] (2) Discharging and crushing waste lithium-ion batteries to a diameter of 2 mm under an argon atmosphere, 900 g of the crushed lithium-ion batteries were then added to the non-bin portion of a rotary kiln (filling rate of 18%), and then heated to 350°C in an air atmosphere at a heating rate of 2°C / min for 1 h to carry out a pyrolysis reaction;

[0060] (3) After the pyrolysis reaction is completed, the zeolite molecular sieve is removed and then heated to 600°C at a heating rate of 6°C / min and kept at this temperature for 3 h for thermal reaction;

[0061] (4) After the thermal reaction is completed, the product is broken up and sieved, and the black powder under the sieve is collected;

[0062] (5) Cooling the pyrolysis tail gas in step (2) and the thermal reaction tail gas in step (3) in water at a temperature of 10° C. and collecting the electrolyte components;

[0063] (6) The uncondensed gas in step (5) is sprayed and absorbed with a sodium bicarbonate aqueous solution having a concentration of 1 mol / L, and then the unabsorbed gas is collected and burned, and the burned gas is purified to obtain carbon dioxide, which is then adsorbed with the zeolite molecular sieve taken out in step (3).

[0064] Example 3

[0065] The present invention provides a method for recycling lithium-ion batteries. The specific recycling process includes the following steps:

[0066] (1) Add 10 g of JLOX-500 zeolite molecular sieve with a diameter of 3 mm into the silo of the rotary kiln (the silo pore size is 0.6 mm);

[0067] (2) Discharging and crushing waste lithium-ion batteries to a diameter of 2 mm under an argon atmosphere, then adding 500 g of the crushed lithium-ion batteries to the non-bin portion of a rotary kiln (filling rate of 10%), and then heating to 200 ° C at a heating rate of 0.5 ° C / min in an air atmosphere for 2 h to carry out a pyrolysis reaction;

[0068] (3) After the pyrolysis reaction is completed, the zeolite molecular sieve is removed and then heated to 500°C at a heating rate of 3°C / min and kept at this temperature for 5 h for thermal reaction;

[0069] (4) After the thermal reaction is completed, the product is broken up and sieved, and the black powder under the sieve is collected;

[0070] (5) Cooling the pyrolysis tail gas in step (2) and the thermal reaction tail gas in step (3) in water at a temperature of 25° C. and collecting the electrolyte components;

[0071] (6) The uncondensed portion of the gas in step (5) is sprayed and absorbed with a sodium bicarbonate aqueous solution having a concentration of 5 mol / L, and then the unabsorbed portion of the gas is collected and burned, and the burned gas is purified to obtain carbon dioxide, which is then adsorbed using the zeolite molecular sieve removed in step (3).

[0072] Example 4

[0073] The present invention provides a method for recycling lithium-ion batteries. The specific recycling process includes the following steps:

[0074] (1) Add 10 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm into the silo of the rotary kiln (the silo pore size is 0.6 mm);

[0075] (2) Discharging and crushing waste lithium-ion batteries to a diameter of 2 mm under an argon atmosphere, followed by adding 1000 g of the crushed lithium-ion batteries to the non-bin portion of a rotary kiln (filling rate of 20%), followed by heating to 400°C at a heating rate of 3°C / min in an air atmosphere for 1 h to carry out a pyrolysis reaction;

[0076] (3) After the pyrolysis reaction is completed, the zeolite molecular sieve is removed and then heated to 650°C at a heating rate of 7°C / min and kept at this temperature for 3 h for thermal reaction;

[0077] (4) After the thermal reaction is completed, the product is broken up and sieved, and the black powder under the sieve is collected;

[0078] (5) Cooling the pyrolysis tail gas in step (2) and the thermal reaction tail gas in step (3) in water at a temperature of 25° C. and collecting the electrolyte components;

[0079] (6) The uncondensed portion of the gas in step (5) is sprayed and absorbed with a sodium bicarbonate aqueous solution having a concentration of 3 mol / L, and then the unabsorbed portion of the gas is collected and burned, and the burned gas is purified to obtain carbon dioxide, which is then adsorbed using the zeolite molecular sieve taken out in step (3).

[0080] Example 5

[0081] The embodiment of the present application provides a lithium-ion battery recycling method, which differs from Example 1 only in step (1). Step (1) of this embodiment is: 9 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm and 1 g of sodium bicarbonate are added to the hopper of the rotary kiln (the hopper pores are 0.6 mm).

[0082] Example 6

[0083] The embodiment of the present application provides a method for recycling lithium-ion batteries, the only difference from Example 1 being step (1). Step (1) of this embodiment is as follows: 9.375 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm and 0.625 g of sodium bicarbonate are added to the hopper of the rotary kiln (the hopper pores are 0.6 mm).

[0084] Example 7

[0085] The embodiment of the present application provides a lithium-ion battery recycling method, which differs from Example 1 only in step (1). Step (1) of this embodiment is: adding 9.5 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm and 0.5 g of sodium bicarbonate to the hopper of the rotary kiln (the hopper pore is 0.6 mm).

[0086] Example 8

[0087] The embodiment of the present application provides a lithium-ion battery recycling method, which differs from Example 1 only in step (1). Step (1) of this embodiment is: 8.5 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm and 1.5 g of sodium bicarbonate are added to the hopper of the rotary kiln (the hopper pores are 0.6 mm).

[0088] Example 9

[0089] The embodiment of the present application provides a method for recycling lithium-ion batteries. The only difference between the embodiment 1 and the embodiment 1 is step (1). Step (1) of the embodiment is: 6 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm and 4 g of sodium bicarbonate are added to the hopper of the rotary kiln (the hopper pores are 0.6 mm).

[0090] Example 10

[0091] This embodiment of the present application provides a method for recycling lithium-ion batteries, the only difference between which is from Example 1 is that the zeolite molecular sieve used is type 4A zeolite molecular sieve.

[0092] Comparative Example 1

[0093] The comparative example of the present application provides a lithium-ion battery recycling method, which differs from Example 1 only in step (1). Step (1) of this comparative example is: 5 g of JLOX-500 zeolite molecular sieve with a diameter of 2 mm is added to the hopper of the rotary kiln (the hopper pore is 0.6 mm).

[0094] Comparative Example 2

[0095] The comparative example of the present application provides a lithium-ion battery recycling method, the only difference between which and Example 1 is step (2). In step (2) of the comparative example, the battery is heated to 300°C at a heating rate of 0.1°C / min and kept warm for 1.5 hours to carry out a pyrolysis reaction.

[0096] Comparative Example 3

[0097] The comparative example of the present application provides a method for recycling lithium-ion batteries, the only difference between which and Example 1 is step (2). In step (2) of the comparative example, the battery is heated to 300°C at a heating rate of 4°C / min and kept warm for 1.5 hours for a pyrolysis reaction.

[0098] Comparative Example 4

[0099] The comparative example of the present application provides a method for recycling lithium-ion batteries, the only difference between which and Example 1 is step (2). In step (2) of the comparative example, the battery is heated to 150°C at a heating rate of 1°C / min and kept warm for 1.5 hours for a pyrolysis reaction.

[0100] Comparative Example 5

[0101] The comparative example of the present application provides a method for recycling lithium-ion batteries, the only difference between which and Example 1 is step (2). In step (2) of the comparative example, the battery is heated to 500°C at a heating rate of 1°C / min and kept warm for 1.5 hours for a pyrolysis reaction.

[0102] Comparative Example 6

[0103] The comparative example of the present application provides a method for recycling lithium-ion batteries, the only difference between which and Example 1 is that in step (1), the zeolite molecular sieve is replaced by sodium bicarbonate.

[0104] Comparative Example 7

[0105] The comparative example of the present application provides a method for recycling lithium-ion batteries, and the specific recycling process includes the following steps:

[0106] (1) Discharging and crushing waste lithium-ion batteries to a diameter of 2 mm under an argon atmosphere, 700 g of the crushed lithium-ion batteries were then added to a rotary kiln (filling rate of 14%) and heated to 300 °C at a heating rate of 1 °C / min under an argon atmosphere for 1.5 h for pyrolysis reaction. The argon flow rate was 50 mL / min.

[0107] (3) After the pyrolysis reaction is completed, the mixture is heated to 550°C at a heating rate of 4°C / min and kept at this temperature for 3.5 h for thermal reaction;

[0108] (4) After the thermal reaction is completed, the product is broken up and sieved, and the black powder under the sieve is collected;

[0109] (5) Cooling the pyrolysis tail gas in step (2) and the thermal reaction tail gas in step (3) in water at a temperature of 25° C. and collecting the electrolyte components;

[0110] (6) The uncondensed gas in step (5) is sprayed and absorbed with a sodium bicarbonate aqueous solution having a concentration of 3 mol / L, and then the unabsorbed gas is collected and burned.

[0111] Effect Examples

[0112] This effect example verifies the volume fraction of the explosive organic gas in the system in step (2) of the recovery method provided in Examples 1-10 and Comparative Examples 1-7, as well as the recovery rate of the electrolyte components and the black powder under the sieve, wherein the volume fraction of the explosive organic gas is detected by a sensor; the obtained results are shown in Table 1;

[0113] Table 1

[0114] As can be seen from Table 1, when the technical solution of the present application is adopted, the volume fraction of the explosive organic gas after pyrolysis is maintained below 2.98% during the overall recovery process, which is lower than the lower explosion concentration limit, indicating that the recovery method provided by the present application is highly safe; in particular, in Examples 1-2 and Examples 5-6, the volume fraction of the explosive organic gas during the recovery process is maintained below 2.33%, which is far below the lower explosion concentration limit. As can be seen from Examples 1 and 10, the type of zeolite molecular sieve will affect the safety of the recovery process.

[0115] As can be seen from Example 1 and Comparative Example 1, when too little zeolite molecular sieve is added, the volume fraction of the explosive organic gas detected in step (2) shows a significant increasing trend, which is not conducive to the development of safe recovery. As can be seen from Example 1 and Comparative Examples 2-5, the heating rate and the holding temperature during the pyrolysis process will significantly affect the volume fraction of the explosive organic gas in the system. As can be seen from Example 1 and Comparative Example 6, when the carbon dioxide provided by the present invention is not adopted, the safety is reduced during the recovery process. In addition, Comparative Example 7 is a pyrolysis method using conventional inert gas protection, in which the volume of the inert gas used is 27L, and the market price of the inert gas is 90 yuan / 40L, that is, the cost of the inert gas for the recovery of Comparative Example 7 is 40 yuan. In fact, the reactor volume used in industry is relatively large. If a 200m 3 If a reactor is used, it would cost nearly 30w / time to fill the reactor with helium. However, the technical solution of the present application does not need to use helium, which can obviously reduce costs and improve economic benefits.

Claims

1. A method for recycling lithium-ion batteries, It is characterized in that The recovery method comprises the following steps: The crushed lithium-ion battery is pyrolyzed, a thermal reaction is carried out after the pyrolysis is completed, and the sieved material is screened to obtain black powder; at the same time, the gas generated by the pyrolysis and thermal reaction is collected and condensed to obtain the electrolyte component; Adding carbon dioxide as a provider during the pyrolysis process; The carbon dioxide provider includes zeolite molecular sieve or a mixture of zeolite molecular sieve and bicarbonate.

2. The recycling method according to claim 1, It is characterized in that The zeolite molecular sieve is selected from at least one of JLOX-500 zeolite molecular sieve and 5A zeolite molecular sieve.

3. The recycling method according to claim 1, It is characterized in that The cation in the bicarbonate is potassium ion, sodium ion or ammonium ion.

4. The recovery method according to claim 3, It is characterized in that The bicarbonate is selected from at least one of potassium bicarbonate and sodium bicarbonate.

5. The recycling method according to claim 1, It is characterized in that The mass ratio of the carbon dioxide provider to the lithium ion battery is carbon dioxide provider:lithium ion battery=1:(50-100).

6. The recovery method according to claim 5, It is characterized in that The mass ratio of the carbon dioxide provider to the lithium ion battery is carbon dioxide provider:lithium ion battery=1:(70-90).

7. The recycling method according to claim 1, It is characterized in that In the mixture of zeolite molecular sieve and bicarbonate, the mass ratio of bicarbonate to zeolite molecular sieve is bicarbonate:zeolite molecular sieve=1:(5-20).

8. The recovery method according to claim 7, It is characterized in that In the mixture of zeolite molecular sieve and bicarbonate, the mass ratio of bicarbonate to zeolite molecular sieve is bicarbonate:zeolite molecular sieve=1:(9-15).

9. The recycling method according to claim 1, It is characterized in that The pyrolysis is performed by heating to 200-400° C. at a heating rate of 0.5-3° C. / min and keeping the temperature for 1-2 hours.

10. The recycling method according to claim 9, It is characterized in that The pyrolysis is performed by heating to 300-350° C. at a heating rate of 1-2° C. / min and keeping the temperature for 1-2 hours.

11. The recycling method according to claim 1, It is characterized in that The thermal reaction is to heat to 500-650° C. at a heating rate of 3-7° C. / min and keep the temperature for 3-5 hours.

12. The recycling method according to claim 1, It is characterized in that The diameter of the crushed lithium-ion battery is 1-3 mm, and the crushing process is carried out under a protective gas environment.

13. The recycling method according to claim 1, It is characterized in that The condensation is water cooling, and the temperature of the water is 10-30°C.

14. The recycling method according to claim 1, It is characterized in that After the electrolyte components are condensed, the process also includes the steps of burning the uncondensed gas and absorbing the alkaline solution.

15. The recovery method according to claim 14, It is characterized in that The alkali solution is selected from at least one of a sodium bicarbonate aqueous solution, a potassium bicarbonate aqueous solution, a potassium hydroxide aqueous solution, and a sodium hydroxide aqueous solution with a concentration of 1-5 mol / L.

16. A lithium-ion battery recycling device, It is characterized in that The device is a rotary kiln (11), wherein an air inlet (12) and an air outlet (13) are respectively arranged at the left and right ends of one side of the rotary kiln (11), and the rotary kiln (11) further comprises a silo (14), wherein the silo (14) is a hollow cavity and is horizontally arranged along the central axis of the hollow cavity, and one end of the silo (14) is an opening for a zeolite molecular sieve inlet and outlet (15), and the air outlet (13) of the rotary kiln (11) is connected to a tail gas absorption device (16).

17. Use of the lithium ion battery recycling device according to claim 16 in lithium ion battery recycling, It is characterized in that The application comprises the following steps: placing a zeolite molecular sieve into a hollow cavity of a silo (14), placing a crushed lithium-ion battery in a cavity of a non-silo part of a rotary kiln (11), and then pyrolyzing the zeolite molecular sieve; after the pyrolysis is completed, taking out the zeolite molecular sieve and subjecting it to a thermal reaction, and after the thermal reaction is completed, sieving the sieve to obtain black powder; and at the same time, collecting and condensing the gases generated by the pyrolysis and thermal reaction to obtain electrolyte components.

18. The use according to claim 17, It is characterized in that In the rotary kiln (11), the filling rate of the crushed lithium-ion batteries is 5-25%.

Citation Information

Patent Citations

  • Method of pyrolysis in process of recovering and treating waste lithium batteries

    CN109719117A

  • System and method for recovering black powder from waste lithium batteries through multistage pyrolysis

    CN113161640A

  • Harmless and resourceful treatment method for waste lithium battery electrolyte

    CN114497794A

  • Charged crushing and electrolyte resourceful treatment method for waste lithium battery

    CN114552042A

  • Efficient dissociation method for positive electrode material and current collector of waste lithium battery

    CN114695995A

Cited By

  • Pyrolysis treatment system and method for waste lithium battery material

    CN120043346A

  • Pyrolysis processing system and method for waste lithium battery materials

    CN120043346B