Cross-linked polymer solid electrolyte, and preparation method therefor and use thereof

By using crosslinked polymer solid electrolytes in lithium-ion batteries, the problems of high impedance and low ionic conductivity of conventional solid electrolytes are solved, high ionic conductivity and low interface impedance are achieved, and the cycle stability of lithium-ion batteries is improved and Security.

WO2024230010A1PCT designated stage expired Publication Date: 2024-11-14SHENZHEN UNIV

Patent Information

Application Number
PCT/CN2023/114795
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2023-08-24
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The impedance of conventional solid electrolytes is large and the ionic conductivity is low, which leads to internal microcracks caused by positive and negative electrode expansion and contraction in the later stage of circulation, which fails rapidly and has poor circulation stability performance.

Method used

By dissolving the lithium salt in an organic solvent, adding cyclic ether monomers, initiators and crosslinking agents, a crosslinking polymer solid electrolyte is formed, and it is allowed to solidify while standing, forming a crosslinking polymer solid electrolyte with low impedance and high ionic conductivity. , the crosslinking agent is used to enhance structural stability and thermal stability and reduce crystallinity.

Benefits of technology

The solid electrolyte with high ionic conductivity, low interface impedance and high stability is achieved, which improves the safety and cycle stability of the battery, allowing it to discharge large-scale like liquid electrolyte, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023114795_14112024_PF_FP_ABST
    Figure CN2023114795_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of new energy materials. Disclosed are a cross-linked polymer solid electrolyte, and a preparation method therefor and the use thereof. The preparation method for the cross-linked polymer solid electrolyte comprises: dissolving a lithium salt into an organic solvent to obtain a liquid electrolyte solution; adding a cyclic ether monomer, an initiator and a cross-linking agent to the liquid electrolyte solution, and uniformly stirring the mixture to obtain a quasi-solid electrolyte precursor; and leaving the quasi-solid electrolyte precursor liquid to stand so as to obtain a cross-linked polymer solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-linked polymer solid electrolyte and its preparation method and application

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 10, 2023, with application number 202310519392.1 and invention name “Cross-linked polymer solid electrolyte and its preparation method and application”, the entire contents of which are incorporated by reference into the application. Technical Field

[0002] The present application relates to the technical field of new energy materials, and in particular to a cross-linked polymer solid electrolyte and a preparation method and application thereof. Background Art

[0003] Lithium-ion batteries are currently widely used in electronic devices, new energy electric vehicles, and large-scale energy storage. Conventional lithium-ion batteries use flammable liquid electrolytes, which pose potential safety risks. In the event of a puncture, impact, or high temperature, electrolyte leakage can occur, leading to safety accidents. Therefore, non-flammable solid electrolytes are beginning to replace liquid electrolytes.

[0004] However, conventional solid-state electrolytes have large impedance and low ionic conductivity. When used in batteries, they cause a large number of internal microcracks to form in the later stages of the battery cycle due to the continuous expansion and contraction of the positive and negative electrodes, resulting in rapid battery failure and poor cycle stability.

[0005] The above content is only used to assist in understanding the technical solution of this application and does not constitute an admission that the above content is prior art. Technical issues

[0006] The main purpose of this application is to provide a cross-linked polymer solid electrolyte and its preparation method and application, aiming to solve the technical problems of conventional solid electrolytes such as large impedance and low ionic conductivity. Technical Solutions

[0007] To achieve the above objectives, the present application provides a method for preparing a cross-linked polymer solid electrolyte, the method comprising the following steps:

[0008] dissolving lithium salt in an organic solvent to obtain a liquid electrolyte;

[0009] adding a cyclic ether monomer, an initiator, and a cross-linking agent into the liquid electrolyte and stirring until uniform, to obtain a quasi-solid electrolyte precursor liquid;

[0010] The quasi-solid electrolyte precursor liquid is allowed to stand to obtain a cross-linked polymer solid electrolyte.

[0011] Optionally, the lithium salt includes one or more of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium iodide (LiI), lithium bis(oxalatoborate) (LiBOB) and lithium hexafluoroarsenate (LiAsF6), wherein the concentration of the lithium salt is at least 0.1 mol / L and not more than 10 mol / L.

[0012] Optionally, the organic solvent includes one or more of ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), N,N-dimethylformamide (DMF), toluene, N-methylpyrrolidone and 4-methyl-1,3-dioxolane.

[0013] Optionally, the cyclic ether monomer includes one or more of 1,3-dioxolane (DOL), polyethylene glycol dimethyl ether (NHD), fluoroethylene carbonate (FEC) and vinylene carbonate (VC).

[0014] Optionally, the initiator includes one or more of lithium hexafluorophosphate (LiPF6), tin fluoride (SnF4), magnesium trifluoromethanesulfonate (Mg(OTf)2), 1-hydroxycyclohexyl phenyl ketone, Lewis acid and aluminum trifluoromethanesulfonate (Al(OTf)3), wherein the concentration of the initiator is at least 0.1 mol / L and not more than 5 mol / L.

[0015] Optionally, the cross-linking agent includes one or more of pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, Y-glycidyl ether silyl propyl sesquioxane and trimethylolpropane triglycidyl ether, wherein the content of the cross-linking agent is at least 1 wt.% and not more than 30 wt.%.

[0016] Optionally, the volume ratio of the organic solvent to the cyclic ether monomer is 1:10 to 10:1.

[0017] Optionally, the standing temperature of the quasi-solid electrolyte precursor liquid is at least 15° C. and not more than 60° C., and the standing time is at least 0.5 h and not more than 72 h.

[0018] The present application also provides a cross-linked polymer solid electrolyte, which is prepared by the above-mentioned cross-linked polymer solid electrolyte preparation method.

[0019] The present application also provides an application of a cross-linked polymer solid electrolyte, wherein the cross-linked polymer solid electrolyte is prepared by the above-mentioned preparation method of the cross-linked polymer solid electrolyte, and the application of the cross-linked polymer solid electrolyte in the preparation of a lithium metal battery.

[0020] The present application discloses a cross-linked polymer solid electrolyte and its preparation method and application, which comprises the following steps: dissolving a lithium salt in an organic solvent to obtain a liquid electrolyte; then adding a cyclic ether monomer, an initiator and a cross-linking agent to the liquid electrolyte and stirring until uniform, thereby obtaining a quasi-solid electrolyte precursor liquid; then allowing the quasi-solid electrolyte precursor liquid to stand, so that the quasi-solid precursor liquid gradually solidifies, and obtaining a cross-linked polymer solid electrolyte with low impedance and high ionic conductivity; in the present application, the addition of the initiator causes the cyclic ether monomer to undergo in situ ring-opening polymerization to form a linear polymer, and the added cross-linking agent connects with the cyclic ether monomer through the ring opening, further causing the linear polymer to cross-link to form a huge three-dimensional hybrid cross-linked network, thereby enhancing the structural stability; and the hybridization improves the thermal stability of the solid electrolyte, reduces the crystallinity of the polymer matrix, and thereby improves the ionic conductivity of the solid electrolyte, ultimately obtaining a solid polymer electrolyte with high ionic conductivity, low interfacial impedance and high stability. The preparation method is simple and can utilize the existing liquid electrolyte production process without increasing equipment investment, so it has industrial prospects. It reduces hydrogen bonds through cross-linking, thereby increasing the activity of polymer chain segments, improving the ionic conductivity of the solid electrolyte, and significantly reduces the impedance of the electrolyte through the synergistic effect between the components, so that the solid electrolyte can be discharged at a high rate like a liquid electrolyte, so that the solid electrolyte maintains good interface contact with the battery electrodes, and improves the safety and cycle stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] FIG1 is a schematic flow chart of a method for preparing a cross-linked polymer solid electrolyte according to an embodiment of the present application;

[0022] FIG2 is an AC impedance test diagram of the embodiment and comparative example of the present application;

[0023] FIG3 is a test diagram of the relationship between ionic conductivity and temperature in Example 1 of the present application;

[0024] FIG4 is a test diagram of the relationship between ionic conductivity and temperature in Example 2 of the present application;

[0025] FIG5 is a test diagram of the relationship between ionic conductivity and temperature in Example 3 of the present application;

[0026] FIG6 is a graph showing the stability performance test of the symmetrical batteries prepared in Example 1 and Comparative Example 1 of the present application;

[0027] FIG7 is a graph showing the stability performance test of the symmetrical batteries prepared in Example 2 and Comparative Example 1 of the present application;

[0028] FIG8 is a graph showing the stability performance of symmetrical batteries prepared in Example 3 and Comparative Example 1 of the present application;

[0029] FIG9 is a graph showing the cycle performance test of the battery prepared in Example 1 of the present application;

[0030] FIG10 is a graph showing the cycle performance test of the battery prepared in Example 2 of the present application;

[0031] FIG11 is a graph showing the cycle performance test of the battery prepared in Example 3 of the present application;

[0032] FIG12 is a diagram of the first cycle charge and discharge test of the battery prepared in Example 1 of the present application;

[0033] FIG13 is a graph showing the lithium ion migration number of Comparative Example 1 of the present application;

[0034] FIG14 is a graph showing the lithium ion transference number of Example 1 of the present application;

[0035] FIG15 is a graph showing the lithium ion transference number of Example 2 of the present application;

[0036] FIG16 is a graph showing the lithium ion transference number of Example 3 of the present application;

[0037] FIG17 is a linear sweep voltammogram of Examples 1-3 of the present application;

[0038] FIG18 is a schematic diagram of the polymer network structure of Example 1 of the present application;

[0039] FIG19 is a schematic diagram of the polymer network structure of Example 2 of the present application;

[0040] Figure 20 is a schematic diagram of the polymer network structure of Example 3 of the present application.

[0041] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. Best Mode for Carrying Out the Invention

[0042] To make the purpose, technical solutions and advantages of the examples of the present application clearer, the technical solutions in the examples of the present application will be described clearly and completely below. Where specific conditions are not specified in the examples, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0043] In addition, the meaning of "and / or" appearing throughout the text includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by this application. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0044] Lithium-ion batteries are used in every aspect of our lives, such as mobile phones, computers, electric vehicles, and various power tools. However, safety risks and battery life issues have driven the search for new batteries with enhanced safety and high specific energy. Conventional lithium-ion batteries often use electrolytes, using organic ethers or esters to dissolve lithium salts. The addition of film-forming protective agents ensures safe, long-lasting cycling of lithium-ion batteries. Among the numerous liquid organic electrolytes, carbonates are a class of organic solvents with high dielectric constants and wide electrochemical windows, making them one of the most widely used solvents in lithium-ion batteries. Commonly used organic solvents include diethyl carbonate, ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. However, these organic solvents are volatile and flammable, posing significant safety risks. Furthermore, the addition of organic electrolytes increases the proportion of inactive materials in the battery, reducing the overall specific energy of the lithium-ion battery. Large amounts of organic ester or ether electrolytes can easily short-circuit within the battery, potentially causing fires and serious safety incidents.

[0045] To further increase battery specific energy and address overall battery safety risks, non-flammable solid electrolytes are beginning to replace liquid electrolytes. However, conventional solid electrolytes have high impedance and low ionic conductivity (approximately 10-7 S cm-1). Consequently, when used in batteries, these electrolytes can cause numerous internal microcracks in the later stages of the battery cycle due to the continuous expansion and contraction of the positive and negative electrodes. This can lead to rapid battery failure and poor cycling stability.

[0046] In view of this, the present application proposes a cross-linked polymer solid electrolyte and its preparation method and application, which comprises dissolving a lithium salt in an organic solvent to obtain a liquid electrolyte; then adding a cyclic ether monomer, an initiator and a cross-linking agent to the liquid electrolyte and stirring until uniform; the addition of the initiator causes the monomer to undergo in situ ring-opening polymerization to form a linear polymer, and the addition of the cross-linking agent further causes the linear polymer to cross-link into a three-dimensional network polymer, thereby obtaining a quasi-solid electrolyte precursor liquid; then the quasi-solid electrolyte precursor liquid is allowed to stand, so that the quasi-solid precursor liquid gradually solidifies to obtain a cross-linked polymer solid electrolyte; the preparation method is simple in process and can utilize the existing liquid electrolyte production process without increasing equipment investment, and has industrial prospects; hydrogen bonds are reduced by cross-linking, thereby increasing the activity of the polymer chain segments, thereby improving the ionic conductivity of the solid electrolyte, and the synergistic effect between the components significantly reduces the impedance of the electrolyte, so that the solid electrolyte can be discharged at a high rate like a liquid electrolyte, so that the solid electrolyte maintains good interfacial contact with the battery electrodes, and improves the safety and cycle stability of the battery.

[0047] A first aspect of an embodiment of the present application provides a method for preparing a cross-linked polymer solid electrolyte, the preparation method comprising the following steps:

[0048] Step S10, dissolving lithium salt in an organic solvent to obtain a liquid electrolyte;

[0049] Lithium salt is added to an organic solvent and stirred until the lithium salt is completely dissolved to obtain a liquid electrolyte.

[0050] In one feasible embodiment, the lithium salt includes one or more of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium iodide (LiI), lithium bis(oxalatoborate) (LiBOB) and lithium hexafluoroarsenate (LiAsF6), wherein the concentration of the lithium salt is at least 0.1 mol / L and not more than 10 mol / L.

[0051] For example, if applied to other metal batteries, the metal salt can be adaptively modified, and the lithium salt can be replaced with the metal salt of the corresponding metal battery; for sodium ion batteries, the lithium salt can be replaced with the sodium salt, and so on.

[0052] In another feasible embodiment, the organic solvent includes one or more of ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), N,N-dimethylformamide (DMF), 1,2-dimethoxypropane (DMP), toluene, N-methylpyrrolidone and 4-methyl-1,3-dioxolane.

[0053] Optionally, the organic solvent includes one or more of ethylene glycol dimethyl ether (DME) and 1,2-dimethoxypropane (DMP).

[0054] Step S20, adding a cyclic ether monomer, an initiator, and a cross-linking agent to the liquid electrolyte and stirring until uniform, to obtain a quasi-solid electrolyte precursor liquid;

[0055] Cyclic ether monomers, initiators and cross-linking agents are added into liquid electrolyte and stirred until uniform to obtain a quasi-solid electrolyte precursor liquid.

[0056] In one feasible embodiment, the cyclic ether monomer includes one or more of 1,3-dioxolane (DOL), polyethylene glycol dimethyl ether (NHD), fluoroethylene carbonate (FEC) and vinylene carbonate (VC).

[0057] Optionally, the cyclic ether monomer includes: 1,3-dioxolane (DOL).

[0058] In another feasible embodiment, the initiator includes one or more of lithium hexafluorophosphate (LiPF6), tin fluoride (SnF4), magnesium trifluoromethanesulfonate (Mg(OTf)2), 1-hydroxycyclohexyl phenyl ketone, Lewis acid and aluminum trifluoromethanesulfonate (Al(OTf)3), wherein the concentration of the initiator is at least 0.1 mol / L and not more than 5 mol / L.

[0059] Optionally, the initiator includes lithium hexafluorophosphate (LiPF6).

[0060] In another feasible embodiment, the cross-linking agent includes: one or more of pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, γ-glycidyl ether silyl propyl sesquioxane and trimethylolpropane triglycidyl ether, wherein the content of the cross-linking agent is at least 1 wt.% and not more than 30 wt.%.

[0061] Optionally, the cross-linking agent includes: pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether and Y-glycidyl ether silylpropyl sesquioxane.

[0062] In this embodiment, the cross-linking agent can serve as a cross-linking center, forming a unit structure by connecting to the cyclic ether monomer through ring opening, and then connecting with the countless units formed to form a huge three-dimensional hybrid cross-linking network.

[0063] In another feasible embodiment, the volume ratio of the organic solvent to the cyclic ether monomer is 1:10 to 10:1.

[0064] Optionally, the volume ratio of the organic solvent to the cyclic ether monomer is 1:5 to 5:1.

[0065] Optionally, the volume ratio of the organic solvent to the cyclic ether monomer is 1:2 to 2:1.

[0066] Optionally, the volume ratio of the organic solvent to the cyclic ether monomer is 1:1.

[0067] In this embodiment, cyclic ether monomers are used to provide flexibility and interfacial compatibility, and the addition of an initiator allows the cyclic ether monomers to undergo in situ ring-opening polymerization, thereby forming a linear polymer. The addition of a cross-linking agent further allows the linear polymer to be cross-linked into a three-dimensional network polymer, thereby enhancing the structural stability. The hybridization of silicon atoms in the cross-linking agent improves the thermal stability of the solid electrolyte, reduces the crystallinity of the polymer matrix, and thereby improves the ionic conductivity of the solid electrolyte, ultimately obtaining a solid polymer electrolyte with high ionic conductivity, low interfacial impedance, and high stability.

[0068] Step S30 , allowing the quasi-solid electrolyte precursor liquid to stand to obtain a cross-linked polymer solid electrolyte.

[0069] The quasi-solid electrolyte precursor liquid is allowed to stand and gradually solidify to obtain a cross-linked polymer solid electrolyte.

[0070] In one feasible embodiment, the standing temperature of the quasi-solid electrolyte precursor liquid is at least 15° C. and not more than 60° C., and the standing time is at least 0.5 h and not more than 72 h.

[0071] In this embodiment, a liquid electrolyte is obtained by dissolving a lithium salt in an organic solvent; a cyclic ether monomer, an initiator and a cross-linking agent are then added to the liquid electrolyte and stirred until uniform, thereby obtaining a quasi-solid electrolyte precursor liquid; the quasi-solid electrolyte precursor liquid is then allowed to stand, so that the quasi-solid precursor liquid gradually solidifies, and a cross-linked polymer solid electrolyte with low impedance and high ionic conductivity is obtained; in this application, the addition of the initiator causes the cyclic ether monomer to undergo in situ ring-opening polymerization to form a linear polymer, and the addition of the cross-linking agent further cross-links the linear polymer into a three-dimensional network polymer, thereby enhancing the structural stability, and the hybridization of silicon atoms in the cross-linking agent improves the thermal stability of the solid electrolyte, reduces the crystallinity of the polymer matrix, and thereby improves the ionic conductivity of the solid electrolyte, ultimately obtaining a solid polymer electrolyte with high ionic conductivity, low interfacial impedance and high stability. The preparation method is simple and can utilize the existing liquid electrolyte production process without increasing equipment investment, so it has industrial prospects. It reduces hydrogen bonds through cross-linking, thereby increasing the activity of polymer chain segments, improving the ionic conductivity of the solid electrolyte, and significantly reduces the impedance of the electrolyte through the synergistic effect between the components, so that the solid electrolyte can be discharged at a high rate like a liquid electrolyte, so that the solid electrolyte maintains good interface contact with the battery electrodes, and improves the safety and cycle stability of the battery.

[0072] A second aspect of the present invention provides a cross-linked polymer solid electrolyte, wherein the cross-linked polymer solid electrolyte is prepared by the following method:

[0073] dissolving lithium salt in an organic solvent to obtain a liquid electrolyte;

[0074] adding a cyclic ether monomer, an initiator, and a cross-linking agent into the liquid electrolyte and stirring until uniform, to obtain a quasi-solid electrolyte precursor liquid;

[0075] The quasi-solid electrolyte precursor liquid is allowed to stand to obtain a cross-linked polymer solid electrolyte.

[0076] Optionally, the lithium salt includes one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium iodide, lithium bisoxalatoborate and lithium hexafluoroarsenate, wherein the concentration of the lithium salt is at least 0.1 mol / L and not more than 10 mol / L.

[0077] Optionally, the organic solvent includes one or more of ethylene glycol dimethyl ether, tetrahydrofuran, N,N-dimethylformamide, 1,2-dimethoxypropane (DMP), toluene, N-methylpyrrolidone and 4-methyl-1,3-dioxolane.

[0078] Optionally, the cyclic ether monomer includes one or more of 1,3-dioxolane, polyethylene glycol dimethyl ether, fluoroethylene carbonate and vinylene carbonate.

[0079] Optionally, the initiator includes one or more of lithium hexafluorophosphate, tin fluoride, magnesium trifluoromethanesulfonate, 1-hydroxycyclohexyl phenyl ketone, Lewis acid and aluminum trifluoromethanesulfonate, wherein the concentration of the initiator is at least 0.1 mol / L and not more than 5 mol / L.

[0080] Optionally, the cross-linking agent includes one or more of pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, Y-glycidyl ether silyl propyl sesquioxane and trimethylolpropane triglycidyl ether, wherein the content of the cross-linking agent is at least 1 wt.% and not more than 30 wt.%.

[0081] Optionally, the volume ratio of the organic solvent to the cyclic ether monomer is 1:10 to 10:1.

[0082] Optionally, the standing temperature of the quasi-solid electrolyte precursor liquid is at least 15° C. and not more than 60° C., and the standing time is at least 0.5 h and not more than 72 h.

[0083] A third aspect of the present application provides an application of a cross-linked polymer solid electrolyte, wherein the cross-linked polymer solid electrolyte is used in the preparation of a lithium metal battery; wherein the cross-linked polymer solid electrolyte is prepared by the following method:

[0084] dissolving lithium salt in an organic solvent to obtain a liquid electrolyte;

[0085] adding a cyclic ether monomer, an initiator, and a cross-linking agent into the liquid electrolyte and stirring until uniform, to obtain a quasi-solid electrolyte precursor liquid;

[0086] The quasi-solid electrolyte precursor liquid is allowed to stand to obtain a cross-linked polymer solid electrolyte.

[0087] Optionally, the lithium salt includes one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium iodide, lithium bisoxalatoborate and lithium hexafluoroarsenate, wherein the concentration of the lithium salt is at least 0.1 mol / L and not more than 10 mol / L.

[0088] Optionally, the organic solvent includes one or more of ethylene glycol dimethyl ether, tetrahydrofuran, N,N-dimethylformamide, toluene, N-methylpyrrolidone and 4-methyl-1,3-dioxolane.

[0089] Optionally, the cyclic ether monomer includes one or more of 1,3-dioxolane, polyethylene glycol dimethyl ether, fluoroethylene carbonate and vinylene carbonate.

[0090] Optionally, the initiator includes one or more of lithium hexafluorophosphate, tin fluoride, magnesium trifluoromethanesulfonate, 1-hydroxycyclohexyl phenyl ketone, Lewis acid and aluminum trifluoromethanesulfonate, wherein the concentration of the initiator is at least 0.1 mol / L and not more than 5 mol / L.

[0091] Optionally, the cross-linking agent includes one or more of pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, Y-glycidyl ether silyl propyl sesquioxane and trimethylolpropane triglycidyl ether, wherein the content of the cross-linking agent is at least 1 wt.% and not more than 30 wt.%.

[0092] Optionally, the volume ratio of the organic solvent to the cyclic ether monomer is 1:10 to 10:1.

[0093] Optionally, the standing temperature of the quasi-solid electrolyte precursor liquid is at least 15° C. and not more than 60° C., and the standing time is at least 0.5 h and not more than 72 h.

[0094] In order to make the details and operations of the above embodiments of the present application clearly understood by those skilled in the art, as well as to significantly demonstrate the advanced performance of the cross-linked polymer solid electrolyte and its preparation method and application in the embodiments of the present application, the above technical solutions are illustrated by multiple embodiments below.

[0095] Example 1

[0096] 1 mol / L lithium bis(trifluoromethanesulfonyl)imide was dissolved in ethylene glycol dimethyl ether (DME) to obtain a liquid electrolyte;

[0097] 1,3-dioxolane (DOL) with a volume ratio of 1:1 to DME, 2 mol / L lithium hexafluorophosphate (LiPF6), and 5 wt.% pentaerythritol glycidyl ether were added to the liquid electrolyte in batches and stirred until uniform to obtain a quasi-solid electrolyte precursor liquid;

[0098] The quasi-solid electrolyte precursor solution was allowed to stand at 25 °C for 20 h to obtain a cross-linked polymer solid electrolyte.

[0099] Example 2

[0100] The steps are the same as those in Example 1, except that the cross-linking agent added is polyethylene glycol diglycidyl ether.

[0101] Example 3

[0102] The steps are the same as those in Example 1, except that the organic solvent added is 1,2-dimethoxypropane (DMP), and the cross-linking agent added is Y-glycidyl ether silyl propyl sesquioxane.

[0103] Comparative Example 1

[0104] The steps are the same as those in Example 1, except that no cross-linking agent is added.

[0105] Furthermore, in order to verify the progress of the embodiments of the present application, the following performance tests were conducted on each embodiment and comparative example:

[0106] 1. Ionic conductivity and impedance test:

[0107] The prepared electrolyte was sandwiched between two stainless steel sheets and encapsulated in a CR2032 button cell. The electrochemical impedance spectroscopy (EIS) test of the assembled "steel sheet|electrolyte|steel sheet" battery was performed using a Shanghai Chenhua Electric CHI760e chemical workstation. The electrolyte thickness was 50 μm, the amplitude was 5 mV, and the frequency range was 10-10 6 Hz. The results are shown in Figure 2 and Table 1:

[0108] Table 1

[0109]

[0110] According to the AC impedance diagram in FIG2 and the impedance data in Table 1, the impedance of the solid electrolyte prepared in Examples 1-3 of the present application is about 2Ω, which has a very small impedance; and the ionic conductivity is 1.1×10 -3 S cm -1 Compared with the solid electrolyte prepared in Comparative Example 1, the ionic conductivity is increased by one order of magnitude, and the solid electrolyte has higher ionic conductivity.

[0111] 2. Test of the relationship between ionic conductivity and temperature:

[0112] The electrolyte prepared in Examples 1-3 was sandwiched between two stainless steel sheets and encapsulated in a CR2032 button cell. The electrochemical impedance spectroscopy (EIS) test of the assembled “steel sheet|electrolyte|steel sheet” battery was performed using a Shanghai Chenhua Electric CHI760e chemical workstation. The electrolyte thickness was 50 μm, the amplitude was 5 mV, and the frequency range was 10-10 6 Hz, experimental temperature 25-80℃, the results are shown in Figure 3-5.

[0113] According to the contents of Figures 3-5, the ionic conductivity of the cross-linked polymeric solid electrolytes prepared in Examples 1-3 gradually increases with increasing temperature, has a linear relationship with temperature, and can maintain stable ionic conductivity at a relatively high temperature (80°C).

[0114] 3. Stability performance test of the prepared symmetrical battery:

[0115] Battery assembly: The solid electrolytes of Examples 1-3 and Comparative Example 1 were assembled into lithium batteries in the order of negative electrode shell, spring, gasket, lithium metal, diaphragm, precursor liquid, lithium iron phosphate, lithium metal, and positive electrode shell; after assembly, they were pressed and sealed, and the batteries were left at room temperature for 24 hours to ensure in-situ solidification of the precursor liquid; after standing, a 1C rate performance test was performed, and the test results are shown in Figures 6-8, (a) is the voltage change curve of the cycle 0-800 h, and (b) is a local enlarged view of 795-800 h in (a).

[0116] According to Figure 6-8, at 1 mA / cm 2At current densities, the solid-state symmetrical cells prepared in Examples 1-3 were capable of charge and discharge at extremely low overpotentials. Even after cycling for 800 h, the voltage polarization remained stable, demonstrating very stable lithium deposition and dissolution behavior. Therefore, the cross-linked polymeric solid electrolyte prepared in this application, when used in batteries, exhibited excellent stability. In contrast, the solid-state symmetrical cell prepared in Comparative Example 1 exhibited a higher overpotential, reaching approximately 420 mV at 800 h. This continued increase in overpotential indicates an increase in uneven lithium plating / deplating during cycling.

[0117] 4. Cycle performance test of the prepared battery:

[0118] Positive electrode preparation: 0.4 g lithium iron phosphate, 0.05 g conductive carbon black, and 0.05 g polyvinylidene fluoride were added to 1.5 mL of N-methylpyrrolidone (NMP). The mixture was stirred at room temperature for 24 hours, then coated on a 20-μm-thick aluminum foil and dried in a vacuum at 80°C for 24 hours. The electrode was cut into 14 mm diameter discs. The active material lithium iron phosphate loading was 2.0 mg cm –2 .

[0119] Battery Assembly: The solid electrolytes prepared in Examples 1-3 were assembled into batteries in the order of negative electrode shell, spring, gasket, lithium metal, separator, precursor liquid, lithium iron phosphate, positive electrode, and positive electrode shell. After assembly, the batteries were pressed and sealed. The batteries were left to stand at room temperature for 24 hours to ensure in situ solidification of the precursor liquid to produce lithium iron phosphate | polymer solid electrolyte | lithium (LFP | SPE | Li) batteries. After standing, 1C rate performance testing was performed. The test results are shown in Figures 9-11.

[0120] 9-11 , the cross-linked polymer solid electrolyte batteries prepared in Examples 1-3 have excellent cycle performance. After 300 cycles, the capacities are 144.4 mAh / g, 144.9 mAh / g, and 140.4 mAh / g, respectively. Therefore, the cross-linked polymer electrolyte batteries prepared in this application have excellent cycle stability and high capacity.

[0121] 5. First cycle charge and discharge test of the prepared battery:

[0122] An LFP | SPE | Li battery prepared using the cross-linked polymer solid electrolyte according to Example 1 was subjected to first-cycle charge and discharge tests, with the results shown in FIG12 . FIG12 shows that the prepared polymer solid electrolyte battery exhibits a stable first-cycle charge and discharge platform at a 1C rate and has a relatively high first-cycle capacity of 165 mA / g (theoretical 170 mAh / g).

[0123] 6. Lithium ion migration number test:

[0124] The cross-linked polymer solid electrolytes prepared in Examples 1-3 and Comparative Example 1 were tested for lithium ion migration numbers, and the test results are shown in Figures 13-16. Referring to Figure 13, the lithium ion migration number of Comparative Example 1 is 0.34; referring to Figure 14, the lithium ion migration number of Example 1 is 0.81; referring to Figure 15, the lithium ion migration number of Example 2 is 0.55; and referring to Figure 16, the lithium ion migration number of Example 3 is 0.88. Therefore, the cross-linked polymer solid electrolyte prepared in this application has the effect of limiting anions, thereby reducing the polarization of battery charge and discharge, and facilitating the transfer of lithium ions.

[0125] 7. Electrochemical stability window test:

[0126] The cross-linked polymer solid electrolytes prepared in Examples 1-3 were subjected to electrochemical stability window testing using linear sweep voltammetry (LSV), and the test results are shown in Figure 17. As shown in Figure 17, the electrochemical stability window of Example 1 is 5.2 V, the electrochemical stability window of Example 2 is 5.2 V, and the electrochemical stability window of Example 3 is 5.3 V; therefore, the cross-linked polymer solid electrolytes prepared in this application have high-voltage stability.

[0127] In this application, Example 1 uses LiPF6 as an initiator and pentaerythritol glycidyl ether as a crosslinker and crosslinking center to design and synthesize a polymer network through in situ ring-opening polymerization. Referring to Figure 18, LiPF6 is added to DOL, and LiPF6 partially decomposes into lithium fluoride and phosphorus pentafluoride. As a strong Lewis acid and key initiator of polymerization, the above decomposition products enable it to proceed smoothly at room temperature; then phosphorus pentafluoride first combines with a small amount of water to form a complex, and then converts into an ion pair H + (PF5OH) - , becoming the initial active species of cationic polymerization, and triggering the ring opening of DOL to become a monomer active species; then the DOL molecule continues to insert ion pairs to make the polymer chain grow; then pentaerythritol glycidyl ether (cross-linker) opens the ring, so that its 4 epoxy groups are opened and connected to 8 DOL chains to form a unit structure, and then countless units are connected to form a huge three-dimensional hybrid cross-linked network, which provides rigidity and high cycle stability for the prepared cross-linked polymer solid electrolyte; and through the flexibility of the ether bond in pentaerythritol glycidyl ether, it exhibits a very low glass transition temperature, which is conducive to the movement of polymer chain segments, thereby making the cross-linked polymer solid electrolyte behave as an amorphous electrolyte material with high ionic conductivity.

[0128] Example 2: Using LiPF6 as an initiator and polyethylene glycol diglycidyl ether as a crosslinker and crosslinking center, a polymer network was designed and synthesized via in situ ring-opening polymerization. Referring to Figure 19, LiPF6 was added to DOL, where it partially decomposed into lithium fluoride and phosphorus pentafluoride. As a strong Lewis acid and key initiator for polymerization, the above decomposition products enabled the polymerization to proceed smoothly at room temperature. Furthermore, phosphorus pentafluoride first combined with a small amount of water to form a complex, which was then converted into an ion pair H + (PF5OH) - , becoming the initial active species of cationic polymerization, and triggering the ring opening of DOL to become a monomer active species; then the DOL molecule continues to insert ion pairs to make the polymer chain grow; then polyethylene glycol diglycidyl ether (cross-linker) opens the ring, so that its two epoxy groups are opened and connected to four DOL chains to form a unit structure, and then countless units are connected to form a huge three-dimensional hybrid cross-linked network, which provides rigidity and high cycle stability for the prepared cross-linked polymer solid electrolyte; and through the flexibility of the ether bond in polyethylene glycol diglycidyl ether, it exhibits a very low glass transition temperature, which is conducive to the movement of polymer chain segments, thereby making the cross-linked polymer solid electrolyte behave as an amorphous electrolyte material with high ionic conductivity.

[0129] Example 3: Using LiPF6 as an initiator and Y-glycidyl ether silyl propane as a crosslinker and crosslinking center, a polymer network was designed and synthesized via in situ ring-opening polymerization. Referring to Figure 20, LiPF6 was added to DOL, where it partially decomposed into lithium fluoride and phosphorus pentafluoride. As a strong Lewis acid and key initiator for polymerization, the above decomposition products enabled the polymerization to proceed smoothly at room temperature. Phosphorus pentafluoride then first combined with a small amount of water to form a complex, which was then converted into an ion pair H + (PF5OH) - , becoming the initial active species of cationic polymerization, and triggering the ring opening of DOL to become a monomer active species; then the DOL molecule continues to insert ion pairs to make the polymer chain grow; then Y-glycidyl ether silyl propane (cross-linker) opens the ring, so that its 8 vertices are connected to 16 DOL chains to form a unit structure, and then countless units are connected to form a huge three-dimensional hybrid cross-linked network, which provides rigidity and high cycle stability for the prepared cross-linked polymer solid electrolyte; and through the flexibility of the Si-O-Si bond in Y-glycidyl ether silyl propane, it exhibits a very low glass transition temperature, which is conducive to the movement of polymer chain segments, thereby making the cross-linked polymer solid electrolyte behave as an amorphous electrolyte material with high ionic conductivity.

[0130] The above are only preferred embodiments of the present application and are not intended to limit the scope of the present invention. Those skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of the present invention.

Claims

1. A method for preparing a cross-linked polymer solid electrolyte, wherein: The preparation method comprises the following steps: dissolving a lithium salt in an organic solvent to obtain a liquid electrolyte; Adding a cyclic ether monomer, an initiator and a cross-linking agent into the liquid electrolyte and stirring until uniform, to obtain a quasi-solid electrolyte precursor liquid; The quasi-solid electrolyte precursor liquid is allowed to stand to obtain a cross-linked polymer solid electrolyte.

2. The method for preparing a cross-linked polymer solid electrolyte according to claim 1, wherein: The lithium salt includes: one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium iodide, lithium bis(oxalatoborate) and lithium hexafluoroarsenate, wherein the concentration of the lithium salt is at least 0.1 mol / L and not more than 10 mol / L.

3. The method for preparing a cross-linked polymer solid electrolyte according to claim 1, wherein: The organic solvent includes one or more of ethylene glycol dimethyl ether, tetrahydrofuran, N,N-dimethylformamide, toluene, N-methylpyrrolidone and 4-methyl-1,3-dioxolane.

4. The method for preparing a cross-linked polymer solid electrolyte according to claim 1, wherein: The cyclic ether monomers include one or more of 1,3-dioxolane, polyethylene glycol dimethyl ether, fluoroethylene carbonate and vinylene carbonate.

5. The method for preparing a cross-linked polymer solid electrolyte according to claim 1, wherein: The initiator includes one or more of lithium hexafluorophosphate, tin fluoride, magnesium trifluoromethanesulfonate, 1-hydroxycyclohexyl phenyl ketone, Lewis acid and aluminum trifluoromethanesulfonate, wherein the concentration of the initiator is at least 0.1 mol / L and not more than 5 mol / L.

6. The method for preparing a cross-linked polymer solid electrolyte according to claim 1, wherein: The cross-linking agent includes one or more of pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, Y-glycidyl ether silyl propyl sesquioxane and trimethylolpropane triglycidyl ether, wherein the content of the cross-linking agent is at least 1 wt.% and not more than 30 wt.%.

7. The method for preparing a cross-linked polymer solid electrolyte according to claim 1, wherein: The volume ratio of the organic solvent to the cyclic ether monomer is 1:10 to 10:

1.

8. The method for preparing a cross-linked polymer solid electrolyte according to claim 1, wherein: The standing temperature of the quasi-solid electrolyte precursor liquid is at least 15° C. and not more than 60° C., and the standing time is at least 0.5 h and not more than 72 h.

9. A cross-linked polymer solid electrolyte, wherein: The cross-linked polymer solid electrolyte is prepared by the method according to any one of claims 1 to 6.

10. An application of a cross-linked polymer solid electrolyte, wherein: The cross-linked polymer solid electrolyte is prepared by the method according to any one of claims 1 to 6, and the cross-linked polymer solid electrolyte is used in the preparation of a lithium metal battery.

Citation Information

Patent Citations

  • Preparation method of gel electrolyte for lithium-sulfur battery

    CN105789694A

  • Asymmetric solid electrolyte and preparation method thereof as well as solid lithium battery and preparation method thereof

    CN114614079A

  • Solid polymer electrolyte and battery preparation method thereof

    CN115732754A

  • In-situ cured solid-liquid mixed electrolyte and lithium ion battery

    CN115911574A

  • Cross-linked polymer solid electrolyte as well as preparation method and application thereof

    CN116259833A

Cited By

  • Solid electrolyte precursor solution, solid electrolyte, battery and preparation method thereof

    CN119092812A