Method for manufacturing grain-oriented electrical steel sheet
By employing predictive modeling to optimize annealing conditions, the method ensures consistent forsterite coating properties in grain-oriented electrical steel sheets, addressing the challenge of inconsistent coatings and improving magnetic performance through uniform film adhesion evaluation.
Patent Information
- Application Number
- PCT/JP2024/015939
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-14
AI Technical Summary
Existing methods for manufacturing grain-oriented electrical steel sheets face challenges in achieving consistent forsterite coating properties over the entire length and width due to variations in decarburization annealing and finish annealing conditions, leading to inconsistent magnetic properties and difficulties in evaluating film adhesion non-destructively.
A method involving data collection on decarburized annealed sheet quality indices and finish annealing conditions, followed by predictive modeling using multiple regression or machine learning to optimize annealing separator composition and finish annealing conditions, ensuring uniform forsterite coating properties by adjusting O basis weight and Ti+V+Zr+Nb basis weight within specific ranges.
This approach allows for the stable production of grain-oriented electrical steel sheets with excellent coating properties over the entire length and width, enhancing magnetic performance and enabling non-destructive evaluation of film adhesion.
Smart Images

Figure JP2024015939_14112024_PF_FP_ABST
Abstract
Description
Manufacturing method of grain-oriented electrical steel sheet
[0001] The present invention relates to a method for manufacturing a grain-oriented electrical steel sheet having excellent coating properties over the entire length and width.
[0002] Grain-oriented electrical steel sheets are soft magnetic materials mainly used for iron cores of transformers, etc., and are required to have excellent magnetic properties, i.e., low iron loss and high magnetic flux density. Such grain-oriented electrical steel sheets are produced by hot-rolling a material containing inhibitor-forming components such as MnS, MnSe, or AlN, optionally annealing the hot-rolled sheet, cold-rolling once or twice or more times with intermediate annealing in between, decarburization annealing, applying an annealing separator mainly composed of MgO to the surface of the steel sheet, and then finish-annealing.
[0003] In the above-mentioned finish annealing, the SiO formed in the decarburization annealing 2 The oxide film mainly composed of MgO reacts with the annealing separator mainly composed of MgO to form a forsterite film. This forsterite film not only provides insulation to the steel sheet surface, but also improves the magnetic properties of the steel sheet by imparting tensile stress due to its low thermal expansion.
[0004] Therefore, forming a forsterite coating that has excellent coating properties, i.e., that has high adhesion over the entire length and width of the steel sheet, is extremely important in producing grain-oriented electrical steel sheets with excellent magnetic properties.
[0005] On the other hand, since the decarburization annealing is a continuous annealing in a highly oxidizing atmosphere, the oxidation level in the furnace is likely to fluctuate, which tends to cause variations in the quality of the decarburized annealed sheet, such as the amount and shape of the oxide film. Furthermore, if variations in the composition and roughness of the steel sheet surface occur in the process preceding the decarburization annealing, variations in the formation of the oxide film may also occur.
[0006] In addition, since the finish annealing is batch annealing in a coiled form, temperature variations tend to occur within the coil, which tends to cause variations in the coating properties.
[0007] To address these problems, Patent Document 1 proposes a technique of changing the components of an annealing separator in the longitudinal direction and width direction of a steel sheet and applying the changed composition.
[0008] Furthermore, conventionally, the coating adhesion of a forsterite coating has been evaluated by a bend peeling test. However, because this bend peeling test is a destructive test, it is impossible to measure the properties of the entire product. Therefore, even though the coating properties are prone to variation as described above, there has been a problem in that it is not possible to evaluate the coating adhesion over the entire length and width while taking such variation into account.
[0009] To address this problem, Patent Document 2 proposes a technique in which light is irradiated onto the surface of a steel sheet and the coating adhesion is evaluated based on the brightness.
[0010] Relisted No. 2020-196773 JP 2011-158328 A
[0011] However, the technique described in Patent Document 1 has problems such as high manufacturing costs, insufficient effectiveness, and still causing variations in coating properties.
[0012] Furthermore, the technology described in Patent Document 2 has the problem that the correlation between brightness and coating adhesion can be shifted even with slight changes in material components or manufacturing conditions, and coating adhesion cannot necessarily be evaluated sufficiently.
[0013] The present invention advantageously solves the above-mentioned problems by providing a method for manufacturing grain-oriented electrical steel sheets that can stably produce grain-oriented electrical steel sheets with excellent coating properties by non-destructively determining the coating properties over the entire length and width of the product steel sheets.
[0014] The gist of the present invention is as follows: 1. In a method for producing grain-oriented electrical steel sheet, a steel material for grain-oriented electrical steel sheet is hot-rolled, and then cold-rolled once or twice or more times with intermediate annealing in between, followed by decarburization annealing, and then an annealing separator mainly composed of MgO is applied to the surface of the steel sheet, followed by finish annealing to produce a finished sheet, the method comprises obtaining data on the quality index of the decarburization annealed steel sheet and the finish annealing conditions, and further obtaining data on the weight of O and the weight of Ti+V+Zr+Nb contained in the forsterite coating of the finished sheet, and using the actual values of each of the weights as objective variables, and determining the quality index of the decarburization annealed steel sheet, the annealing separator, and the final annealing conditions. a method for producing a grain-oriented electrical steel sheet, in which a prediction model for each basis weight is created by performing multiple regression analysis or machine learning using actual values of the agent composition and the finish annealing conditions as explanatory variables, and the prediction model for each basis weight is used to set the annealing separator composition and the finish annealing conditions according to the value of the decarburization-annealed sheet quality index at each position (m, n) (where 1≦m≦i, 1≦n≦j) obtained by dividing the steel sheet into i divisions in the longitudinal direction and j divisions in the width direction, so that the O basis weight and (Ti+V+Zr+Nb basis weight) / O basis weight at each position (m, n) fall within ranges determined by coating adhesion.
[0015] 2. The maximum number of the O basis weight of the product sheet is 1.00 g / m 2 or more, and the maximum number of (Ti+V+Zr+Nb weight) / O weight is 0.01 or more.
[0016] 3. The quality index of the decarburized annealed sheet is O concentration, Si concentration, P concentration, Mn concentration, SiO concentration, 2 Production amount, FeSiO 3 Amount of production, and Fe 2 SiO 4 3. The method for producing a grain-oriented electrical steel sheet according to 1 or 2, wherein at least one of the amounts of the grains produced is selected from the group consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24
[0017] 4. The method for producing a grain-oriented electrical steel sheet according to any one of items 1 to 3, wherein the annealing separator composition contains at least one of a Ti content, a V content, a Zr content, and a Nb content in the annealing separator.
[0018] 5. The finish annealing conditions are H 25. The method for producing a grain-oriented electrical steel sheet according to any one of 1 to 4, wherein the gas introduction temperature and / or the heating rate are 950 to 1100°C.
[0019] According to the present invention, it is possible to stably manufacture grain-oriented electrical steel sheets having excellent coating properties over the entire length and width.
[0020] 1 is a diagram showing the fluorescent X-ray Mn intensity of a decarburization-annealed sheet at each position (m, n) in a comparative example of the present invention. 2 is a diagram showing the fluorescent X-ray Mn intensity of a decarburization-annealed sheet at each position (m, n) in an inventive example of the present invention. 3 is a diagram showing the H intensity during finish annealing at each position (m, n) in a comparative example of the present invention. 2 1 is a diagram showing the temperature of the steel sheet surface when gas is introduced. 2 FIG. 1 is a diagram showing the temperature of the steel sheet surface when gas is introduced; FIG. 2 is a diagram showing the O weight of the product sheet at each position (m, n) in a comparative example of the present invention; FIG. 3 is a diagram showing the O weight of the product sheet at each position (m, n) in an inventive example of the present invention; FIG. 4 is a diagram showing the (Ti+V+Zr+Nb weight) / O weight of the product sheet at each position (m, n) in a comparative example of the present invention; and FIG. 5 is a diagram showing the (Ti+V+Zr+Nb weight) / O weight of the product sheet at each position (m, n) in an inventive example of the present invention.
[0021] First, we will explain the steel material composition of the grain-oriented electrical steel sheet (also simply referred to as steel sheet in this specification) used in the method for producing a grain-oriented electrical steel sheet according to one embodiment of the present invention. The steel material composition may be a conventionally known composition. Specifically, it is as follows. The remainder other than the following components is Fe and unavoidable impurities. C is an effective component for improving the texture, but a content of less than 0.01% by mass does not provide sufficient effects. On the other hand, if the content exceeds 0.1% by mass, decarburization becomes difficult and magnetic properties deteriorate. Therefore, the content is preferably in the range of 0.01 to 0.1% by mass. More preferably, the lower limit is 0.02% by mass and the upper limit is 0.08% by mass.
[0022] Si is an effective component for increasing resistivity and improving magnetic properties, but if the content is less than 1.0 mass%, sufficient effects cannot be obtained. On the other hand, if the content exceeds 5.0 mass%, cold rollability deteriorates significantly. Therefore, the content is preferably in the range of 1.0 to 5.0 mass%. More preferably, the lower limit is 2.0 mass% and the upper limit is 4.0 mass%.
[0023] Like Si, Mn increases resistivity and improves magnetic properties. It is also an effective component for improving hot ductility, but a content of less than 0.01% by mass does not provide sufficient effects. On the other hand, a content exceeding 0.5% by mass deteriorates magnetic properties. Therefore, the content is preferably in the range of 0.01 to 0.5% by mass. More preferably, the lower limit is 0.02% by mass and the upper limit is 0.2% by mass.
[0024] In addition, in the present disclosure, conventionally known MnS, MnSe, or AlN can be used as the inhibitor. When MnS or MnSe is used, it is preferable to add 0.01 to 0.5 mass% of Mn, 0.002 to 0.03 mass% of S, or 0.002 to 0.03 mass% of Se. On the other hand, when AlN is used, it is preferable to add 0.004 to 0.04 mass% of Al and 0.002 to 0.03 mass% of N. The above inhibitors may be used alone or in combination.
[0025] Furthermore, for the purpose of improving magnetic properties, one or more of the following may be added in mass %: B: 0.0001 to 0.005%, Ti: 0.001 to 0.01%, P: 0.005 to 0.1%, Cr: 0.01 to 0.5%, Ni: 0.01 to 1.5%, Cu: 0.01 to 0.5%, Nb: 0.002 to 0.08%, Mo: 0.005 to 0.1%, Sn: 0.005 to 0.5%, Sb: 0.005 to 0.5%, and Bi: 0.001 to 0.05%.
[0026] Next, a method for producing a grain-oriented electrical steel sheet according to one embodiment of the present invention will be described. First, a steel material for the grain-oriented electrical steel sheet, which has been adjusted to have the above-mentioned chemical composition, is hot-rolled, annealed as needed, cold-rolled once or twice or more times with intermediate annealing in between, and then decarburization-annealed.
[0027] Here, it is preferable that the decarburization annealing temperature be 750 to 950°C and the time be 80 to 200 seconds. If the annealing temperature is less than 750°C and the time is less than 80 seconds, decarburization may be difficult. On the other hand, if the annealing temperature is more than 950°C and the time is more than 200 seconds, the primary recrystallized grain size becomes coarse and secondary recrystallization is suppressed, which may result in deterioration of magnetic properties.
[0028] In addition, the oxidation resistance (PH) of the decarburization annealing 2 O / PH 2 ) is preferably in the range of 0.3 to 0.6. 2 O / PH 2 If the pH is less than 0.3, decarburization may be difficult. 2 O / PH 2 If the value exceeds 0.6, FeO is formed, which may deteriorate the coating properties.
[0029] In this embodiment, it is important to obtain data on the quality index of the decarburized annealed steel sheet (in this example, obtained by calculation or measurement) because this data contributes to determining the finish annealing conditions. The decarburized annealed steel sheet quality indexes include, for example, the O concentration, Si concentration, P concentration, and Mn concentration on the steel sheet surface, and SiO 2 Production amount, FeSiO 3 Amount of production and Fe 2 SiO 4 Furthermore, the ratio of any of the concentrations or amounts may be determined and used. When the quality index of the decarburized annealed sheet is obtained by measurement, it may be determined by measurement using X-ray fluorescence analysis, infrared spectroscopy, or the like, or when it is obtained by calculation, it may be calculated from the decarburization annealing conditions such as the annealing temperature, time, and oxidation degree.
[0030] Then, an annealing separator mainly composed of MgO is applied to the steel sheet surface. Here, at least one of Ti, Zr, V, and Nb compounds is added to the annealing separator to improve the coating properties. The total amount of these added is preferably 1 to 7 mass% in terms of each metal element. If the amount added is less than 1 mass%, sufficient effect cannot be obtained. On the other hand, if the amount added exceeds 7 mass%, the metal elements may penetrate into the steel, resulting in deterioration of magnetic properties. The type of compound is not limited. For example, oxides, hydroxides, borates, carbonates, nitrates, phosphates, sulfates, halides, etc. can be used. These compounds may be used alone or in combination. It is preferable to record the data on the composition of the applied annealing separator, as this data will be used later in creating a predictive model.
[0031] Furthermore, for the purpose of improving the coating properties and magnetic properties, conventionally known oxides, hydroxides, borates, carbonates, nitrates, phosphates, sulfates, and halides of Li, Na, Mg, Al, Si, K, Ca, Fe, Co, Ni, Cu, Sr, Ba, and lanthanoids may be added. These may be used alone or in combination.
[0032] The amount of each additive is preferably in the range of 0.01 to 15 parts by mass per 100 parts by mass of MgO. If the amount is less than 0.01 part by mass, sufficient effects cannot be obtained. On the other hand, if the amount is more than 15 parts by mass, excessive film formation or excessive suppression force may occur, which may result in deterioration of magnetic properties. Next, final annealing is performed. This final annealing can include secondary recrystallization annealing to promote secondary recrystallization and purification annealing to purify the inhibitor.
[0033] In the above-mentioned secondary recrystallization annealing, if the secondary recrystallization is to be completed during soaking, the annealing temperature is preferably 800 to 1000°C and the annealing time is preferably in the range of 5 to 200 hours. If the annealing temperature is less than 800°C or the annealing time is less than 5 hours, the secondary recrystallization may not be completed during soaking, and the magnetic properties may deteriorate. On the other hand, if the annealing temperature exceeds 1000°C or the annealing time exceeds 200 hours, the coil may buckle and the shape may deteriorate.
[0034] Furthermore, when secondary recrystallization is to be completed during heating, it is preferable that the heating rate from 700 to 1100°C is in the range of 2.5 to 50°C / h. If the heating rate is less than 2.5°C / h, the coil may buckle and the shape may deteriorate. On the other hand, if the heating rate exceeds 50°C / h, the secondary recrystallized grains may become finer, and the magnetic properties may deteriorate. Here, the annealing atmosphere is N 2 or an inert atmosphere of Ar.
[0035] In the purification annealing, the annealing temperature is preferably 1150 to 1250°C and the time is preferably in the range of 2 to 50 hours. If the annealing temperature is less than 1150°C or the annealing time is less than 2 hours, the purification may be insufficient. On the other hand, if the annealing temperature exceeds 1250°C or the annealing time exceeds 50 hours, the coil may buckle and the shape may deteriorate.
[0036] In addition, for the purpose of film formation and purifying, H 2 Gas is introduced. 2 By introducing the gas, the Fe oxide formed on the surface of the steel sheet is reduced, the oxidizing property in the furnace is increased, and the formation of the coating is promoted. 2 If the gas introduction temperature is less than 900°C, the inhibitor may decompose before the secondary recrystallization is completed, resulting in deterioration of the magnetic properties. 2 If the gas introduction temperature exceeds 1050° C., sufficient effect cannot be obtained.
[0037] In this embodiment, data on the finish annealing conditions of the steel sheet is acquired (in this example, acquired by calculation or measurement) because they directly affect the coating properties. 2 These are either or both of the gas introduction temperature and the heating rate between 950 and 1100° C. When the above-mentioned finish annealing conditions are obtained by measurement, they may be obtained by actual measurement using a thermocouple wound in a coil, or when they are obtained by calculation, they may be obtained by calculation from the finish annealing conditions such as the annealing temperature and time.
[0038] Furthermore, in this embodiment, it is important to obtain data on the O weight and Ti+V+Zr+Nb weight contained in the forsterite coating of the product sheet (obtained by measurement in this example), because the magnitude of the weight allows for a reproducible estimation of an index related to peeling resistance (coating adhesion), which is the most important of the coating properties, and this leads to non-destructive management of the coating properties of the steel sheet.
[0039] Regarding acquisition by measurement, a method for non-destructively measuring the basis weight of each element includes, for example, measuring the fluorescent X-ray intensity of each element and then converting it into the basis weight of each element using a calibration curve prepared in advance.
[0040] In the method according to this embodiment, first, data on the decarburization-annealed steel sheet quality index and the finish annealing conditions are obtained, and data on the O weight and Ti+V+Zr+Nb weight contained in the forsterite coating of the product steel sheet are also obtained. Next, a prediction model for each basis weight is created by performing multiple regression analysis or machine learning using the actual values of each basis weight as a response variable and the actual values of the decarburization-annealed steel sheet quality index, annealing separator composition, and finish annealing conditions as explanatory variables.
[0041] Furthermore, the steel sheet to be subjected to the manufacturing method of this embodiment is divided into i parts in the longitudinal direction and j parts in the width direction, and each part (m, n) (where 1≦m≦i, 1≦n≦j) is set. Then, using the prediction model for each basis weight, the annealing separator composition and the finish annealing conditions are substituted within a certain range for the decarburization annealed sheet quality index at each of the above-mentioned positions (m, n), and the annealing separator composition and the finish annealing conditions are set so that the maximum basis weight of O and the maximum value of (Ti+V+Zr+Nb basis weight) / O basis weight at each of the positions (m, n) fall within a range determined by coating adhesion.
[0042] That is, in this embodiment, when using the prediction model for each basis weight, the decarburization annealed sheet quality index, finish annealing conditions, and each basis weight of the product sheet at each position (m, n) (where 1≦m≦i, 1≦n≦j) obtained by dividing the steel sheet longitudinally into i parts and the steel sheet widthwise into j parts are used. Note that each position (m, n) refers to each divided region (portion) when the steel sheet is divided into i parts in the longitudinal direction, preferably 10 to 100 parts, and j parts in the steel sheet widthwise, preferably 5 to 20 parts.
[0043] Furthermore, when creating a prediction model for each of the coating weights, the decarburization-annealed sheet quality index and the finish annealing conditions for the steel sheet are obtained (e.g., derived by calculation or measurement), and the O coating weight and Ti+V+Zr+Nb coating weight contained in the forsterite coating of the product sheet are obtained (e.g., derived by measurement), the longitudinal direction of the steel sheet may be divided into i parts and the width direction of the steel sheet may be divided into j parts and the results may be obtained (e.g., by performing such calculation or measurement).
[0044] When the O, Si, P, and Mn concentrations on the surface of the decarburized annealed sheet are high, or when FeSiO 3 and Fe 2 SiO 4 When the amount of Fe-based oxides is large, such as those described above, excessive film formation occurs during final annealing, and the weight of O after final annealing increases. As a result, there is a risk that (weight of Ti + V + Zr + Nb) / weight of O becomes insufficient. 2 It is necessary to suppress the formation of a coating during finish annealing by increasing the gas introduction temperature and / or slowing the heating rate between 950 and 1100° C. Furthermore, it is necessary to increase the weight of Ti+V+Zr+Nb by reducing the weight of O and / or increasing the amounts of Ti, V, Zr, and Nb added to the annealing separator.
[0045] On the other hand, when the O, Si, P, and Mn concentrations on the surface of the decarburized annealed sheet are low or when FeSiO 3 and Fe 2 SiO 4 When the amount of Fe-based oxides is small, the formation of the coating during the final annealing may be insufficient, and the amount of O applied after the final annealing may be insufficient. 2It is necessary to promote film formation during finish annealing and increase the O coating weight by lowering the gas introduction temperature and / or increasing the heating rate between 950°C and 1100°C.
[0046] The model used for the machine learning in this embodiment is not limited, and a random forest or a neural network may be used.
[0047] Thereafter, if necessary, the sheet is subjected to an insulating coating, planarization annealing, and magnetic domain refinement treatment to obtain a finished sheet. Note that the fluorescent X-ray Ti intensity of the finished sheet may be measured according to the above-described procedure at any time before the sheet is subjected to finish annealing and obtained as a finished sheet.
[0048] Here, the maximum range of the O basis weight is 1.00 g / m 2 The maximum weight per unit area of O is preferably 1.00 g / m or more. 2 If the coating amount is less than 2.00 g / m, the amount of the coating formed will be too small, and the coating may be easily broken by external stress, resulting in insufficient adhesion. 2 The upper limit of the range of the maximum number of the O basis weight is not particularly limited, but it is set to 10.00 g / m because it will cause a decrease in the space factor. 2 Preferably less than this level.
[0049] Furthermore, the maximum range of the (Ti+V+Zr+Nb basis weight) / O basis weight is preferably 0.01 or more. If the value of the maximum number of the (Ti+V+Zr+Nb basis weight) / O basis weight is less than 0.01, there is a risk of insufficient coating adhesion. More preferably, it is 0.02 or more. Note that there is no particular upper limit to the range of the maximum number of the (Ti+V+Zr+Nb basis weight) / O basis weight, but since there is a risk of each metal element penetrating into the steel, it is preferably about 0.20 or less.
[0050] Although the reason why coating adhesion can be evaluated by the value of (Ti + V + Zr + Nb coating weight) / O coating weight of the finished steel sheet is not clear, the inventors believe as follows: The Ti, V, Zr, and Nb compounds added to the annealing separator decompose during finish annealing and are incorporated into the forsterite coating in the form of nitrides, oxides, etc., and segregate at grain boundaries, thereby increasing the strength of the coating. Therefore, it is believed that the greater the Ti + V + Zr + Nb coating weight relative to the amount of forsterite coating, the better the coating adhesion. Therefore, it is believed that the adhesion of the forsterite coating (coating adhesion) can be evaluated by measuring the (Ti + V + Zr + Nb coating weight) / O coating weight, which allows for estimation of such grain boundary segregation. In the above example, data on the decarburization-annealed steel sheet quality index and the finish annealing conditions are obtained by measurement or calculation, and data on the O weight and Ti + V + Zr + Nb weight contained in the forsterite coating of the product sheet are further obtained by measurement. However, the present disclosure is not limited to this case. For example, when past performance data exists, such a series of data can be obtained externally. For example, a series of data can be obtained via a computer's communication unit. Alternatively, such a series of data can be obtained by a person through transfer, etc. Furthermore, for example, in the case of finish annealing conditions, set value data can be obtained instead of calculation or measurement. As such, various modifications and variations are possible in the acquisition of data necessary to create a learning model.
[0051] Example 1 In this example, a general machine learning tool was used to create a prediction model for each basis weight by machine learning using a neural network, with the actual values of the O basis weight and Ti+V+Zr+Nb basis weight of the product sheet over the past two years as the objective variables, and the actual values of the decarburized annealed sheet quality index, annealing separator composition, and finish annealing conditions as the explanatory variables.
[0052] A steel material containing, by mass%, 0.03% C, 0.004% N, 0.007% Al, 3.4% Si, and 0.06% Mn, with the balance being Fe and unavoidable impurities, was subjected to slab heating at 1260°C, followed by hot rolling and further cold rolling. After that, the steel material was subjected to intermediate annealing at 1050°C for 1 minute and cold rolling again to form a cold-rolled sheet having a thickness of 0.23 mm. The steel sheet was then subjected to decarburization annealing in a wet hydrogen atmosphere at 840°C for 2 minutes. The steel sheet was then divided into 50 sections (i) at 100 m pitches in the longitudinal direction and into 10 sections (j) at 100 mm pitches in the width direction, and X-ray fluorescence analysis and infrared spectroscopy were performed at each position (m, n) (where 1≦m≦i, 1≦n≦j) along the steel sheet, to measure the intensity of each element and the amount of oxide generated at each position (m, n) of the steel sheet. Next, TiO 2 The annealing separator containing 3 parts by mass of N 2 After soaking in a gas atmosphere, the material is heated to a temperature of 950 to 1100°C at a heating rate of 15°C / h. 2 Gas was introduced, and soaking treatment was carried out at 1200° C. for 5 hours.
[0053] Here, the maximum number of basis weights of the product sheet O at each position (m, n) is 1.00 g / m 2 or more, and the maximum value of (Ti + V + Zr + Nb basis weight) / O basis weight is 0.01 or more. 2 Finish annealing was carried out under two conditions: one according to the present invention, in which the gas introduction temperature was adjusted within the range of 900 to 1050°C, and the other in which all 10 coils were uniformly set at 960°C. After that, a coating mainly made of phosphate was applied, and then flattening annealing was carried out at 850°C for 1 minute to produce a product sheet.
[0054] Fluorescent X-ray analysis was performed at each position (m, n) of the product sheet thus obtained, and the fluorescent X-ray intensities of O, Ti, V, Zr, and Nb were measured. These were converted into the respective basis weights using the calibration curves, and the maximum O basis weight was 1.00 g / m. 2The percentage of positions where the maximum value of (Ti+V+Zr+Nb weight) / O weight was 0.01 or more was determined. Here, in the following Tables 1-1 to 8-2, when the fluorescent X-ray Mn intensity at the end of the decarburized annealed sheet was high, the H 2 A comparison is shown between the case where the gas introduction temperature is changed to 980°C and the case where it is uniformly set to 960°C.
[0055]
[0056]
[0057]
[0058]
[0059]
[0060]
[0061]
[0062]
[0063]
[0064]
[0065]
[0066]
[0067]
[0068]
[0069]
[0070]
[0071] As shown in Tables 1-1 to 8-2 and Figures 1A, 1B, 2A, 2B, 3A, 3B, 4A, and 4B, the decarburization annealed sheet Mn fluorescent X-ray intensity at the steel sheet width direction end is high, and therefore, 2When the gas introduction temperature was changed to 980°C, excessive film formation on the upper part of the coil could be effectively prevented. As a result, the maximum basis weight of the product sheet O was 1.00 g / m 2 The percentage of positions where the maximum value of (Ti+V+Zr+Nb basis weight) / O basis weight was 0.01 or more increased (in the example of FIG. 4B, the percentage was 100%). 2 When the gas introduction temperature was uniformly set to 960°C, excessive film formation occurred on the upper part of the coil, and the maximum weight of the product sheet O was 1.00 g / m 2 Furthermore, the percentage of positions where the maximum number of (Ti+V+Zr+Nb basis weight) / O basis weight was 0.01 or more decreased (in the example of FIG. 4A, the percentage was 75.4%).
[0072] In this way, depending on the variation in the quality index of the decarburized annealed sheet, 2 When the gas introduction temperature was changed (example of the invention), the maximum number of the product sheet O basis weight was 1.00 g / m 2 The percentage of positions where the maximum number of (Ti+V+Zr+Nb basis weight) / O basis weight was 0.01 or more was 98.8% on average for 10 coils. 2 When the gas introduction temperature was uniformly set to 960° C. (comparison example), the ratio was 86.6% on average for the 10 coils.
[0073] Example 2 In this example, a general machine learning tool was used to create a prediction model for each basis weight by machine learning using a random forest, with the actual values of the O basis weight and Ti+V+Zr+Nb basis weight of the product sheet over the past two years as the objective variables, and the actual values of the decarburized annealed sheet quality index, the annealing separator composition, and the finish annealing conditions as the explanatory variables.
[0074] A material containing, by mass%, 0.07% C, 0.009% N, 0.022% Al, 3.4% Si, 0.07% Mn, and 0.02% Se, with the balance being Fe and unavoidable impurities, was slab heated at 1380°C, hot rolled, cold rolled, intermediate annealed at 1050°C for 1 minute, and cold rolled again to form a 0.23 mm cold-rolled sheet. The sheet was then decarburized and annealed in a wet hydrogen atmosphere at 840°C for 2 minutes, and then divided into 50 sections (i) at 100 m pitches in the longitudinal direction of the steel sheet and into 10 sections (j) at 100 mm pitches in the width direction of the steel sheet. X-ray fluorescence analysis and infrared spectroscopy were performed at each position (m, n) (where 1≦m≦i, 1≦n≦j) in the steel sheet, and the intensity of each element and the amount of oxide generated at each position (m, n) of the steel sheet were measured. Then, TiO 2 After applying an annealing separator containing 3 parts by mass of the above, the steel sheet was heated in the range of room temperature to 950°C at a heating rate of 15°C / h, and then heated in the range of 950 to 1100°C at a predetermined heating rate. 2 The gas was introduced at 950° C., and the mixture was soaked at 1200° C. for 5 hours.
[0075] Here, according to the quality index of the decarburization annealed sheet at each position (m, n), the maximum number of the product sheet O weight at each position (m, n) is 1.00 g / m 2 Finish annealing was performed in two cases: one where the heating rate from 950 to 1100°C was changed to 10 to 20°C / h for each of the 10 coils, and the other where the heating rate was uniformly set to 15°C / h for all 10 coils, so that the maximum value of (Ti + V + Zr + Nb basis weight) / O basis weight was 0.01 or more. A phosphate-based coating was then applied, and the product sheet was subjected to flattening annealing at 850°C for 1 minute to obtain a product sheet. X-ray fluorescence analysis was then performed at each position (m, n) of the product sheet, and the X-ray fluorescence intensities of O, Ti, V, Zr, and Nb were measured and converted to the respective basis weights using a calibration curve. The maximum O basis weight was 1.00 g / m. 2 The percentage of positions where the maximum number of (Ti+V+Zr+Nb basis weight) / O basis weight was 0.01 or more was determined.
[0076] When the heating rate is changed according to the variation in the quality index of the decarburized annealed sheet, the maximum number of O weights of the product sheet is 1.00 g / m 2The percentage of positions where the maximum value of (Ti+V+Zr+Nb basis weight) / O basis weight was 0.01 or more was 98.7% on average for 10 coils. In contrast, when the heating rate was set uniformly at 15°C / h, the percentage was 84.3% on average for 10 coils.
Claims
1. A method for producing grain-oriented electrical steel sheet, which comprises hot rolling a steel material for grain-oriented electrical steel sheet, cold rolling once or at least twice with intermediate annealing therebetween, decarburization annealing, applying an annealing separator mainly composed of MgO to the surface of the steel sheet, and then finish annealing to produce a finished sheet, comprises obtaining data on the quality index of the decarburization annealed sheet of the steel sheet and the finish annealing conditions, and further obtaining data on the O weight and Ti+V+Zr+Nb weight contained in the forsterite coating of the finished sheet, and using the actual values of each of the aforementioned weights as objective variables and the actual values of the decarburization annealed sheet quality index, the annealing separator composition, and the finish annealing conditions as explanatory variables, to create a prediction model for each weight by multiple regression analysis or machine learning, A manufacturing method for grain-oriented electrical steel sheet in which a prediction model for each of the aforementioned coating weights is used, and in accordance with the value of the decarburization annealed sheet quality index at each position (m, n) (where 1≦m≦i, 1≦n≦j) obtained by dividing the steel sheet into i parts in the longitudinal direction and j parts in the width direction, the annealing separator composition and finish annealing conditions are set so that the O coating weight and (Ti+V+Zr+Nb coating weight) / O coating weight at each position (m, n) are within ranges determined by coating adhesion.
2. The maximum number of O-area weight of the product plate is 1.00 g / m 2 and a maximum number of (Ti+V+Zr+Nb weight) / O weight is 0.01 or more.
3. The quality index of the decarburized annealed sheet is O concentration, Si concentration, P concentration, Mn concentration, SiO 2 Production amount, FeSiO 3 Amount of production, and Fe 2 SiO 4 The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, wherein at least one of the amounts of the grains produced is a grain boundary grain.
4. The method for producing grain-oriented electrical steel sheet according to claim 1 or 2, wherein the annealing separator composition is at least one of the Ti content, V content, Zr content and Nb content contained in the annealing separator.
5. The method for producing grain-oriented electrical steel sheet according to claim 3, wherein the annealing separator composition is at least one of the Ti content, V content, Zr content and Nb content contained in the annealing separator.
6. The finish annealing conditions are H 2 The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, wherein either or both of the gas introduction temperature and the heating rate are 950 to 1100°C.
7. The finish annealing conditions are H 2 The method for producing a grain-oriented electrical steel sheet according to claim 3, wherein either or both of the gas introduction temperature and the heating rate are 950 to 1100°C.
8. The finish annealing conditions are H 2 The method for producing a grain-oriented electrical steel sheet according to claim 4, wherein either or both of the gas introduction temperature and the heating rate are 950 to 1100°C.
9. The finish annealing conditions are H 2 The method for producing a grain-oriented electrical steel sheet according to claim 5, wherein either or both of the gas introduction temperature and the heating rate are 950 to 1100°C.
Citation Information
Patent Citations
Preparation of unidirectional silicon steel plate
JP1984193220A
Method for controlling amount of oxide film at decarburizing annealing for grain oriented silicon steel sheet
JP1996100220A
Forsterite film of grain oriented silicon steel sheet with high magnetic flux density and its formation
JP1997184017A
Oriented electrical steel sheet and method therefor
JP2016145419A
Method for determining finish annealing conditions for oriented electromagnetic steel sheet, and method for manufacturing oriented electromagnetic steel sheet using said determination method
WO2022186357A1