Positive electrode sheet and preparation method therefor, secondary battery, and electrical device

By introducing a carbon cladding layer into the positive electrode active material and controlling the particle size distribution, the problem of influence of micropowder and large particles is solved, the circulation stability and high-temperature performance of the material are improved, and a more uniform electrochemical reaction is achieved.

WO2024234544A1PCT designated stage expired Publication Date: 2024-11-21CONTEMPORARY AMPEREX TECHNOLOGY CO LTD +1

Patent Information

Application Number
PCT/CN2023/124793
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2023-10-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the content of micropowder and ultra-large single crystal particles in the olivine phosphate-based positive electrode active material, resulting in a cycle life attenuation and affecting the particle uniformity and mechanical integrity of the material.

Method used

Using phosphate-based positive electrode active material containing carbon cladding, the primary particle size is controlled to be above 80nm and below 180nm by compaction granulation, sintering and pulverization, and the secondary particle size is distributed within a suitable range to reduce the micropowder and The proportion of large particles improves the circulation stability of the material.

Benefits of technology

It significantly improves the cycle life and high-temperature storage performance of the positive electrode active material, slows down the cycle life attenuation and side reaction rate of small particles, and enhances the chemical mechanical stability and electrochemical performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023124793_21112024_PF_FP_ABST
    Figure CN2023124793_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a positive electrode sheet and a preparation method therefor, a secondary battery, and an electrical device. The positive electrode sheet comprises a current collector and a positive electrode film layer located on at least one side of the current collector. The positive electrode film layer comprises a positive electrode active material. The positive electrode active material comprises a base material and a carbon coating layer located on the surface of the base material. The base material has a structural general formula of LizFexMn(1-x-y)MyPO4, where 1≤z≤1.1, 0.5≤x≤1, and 0≤y≤0.1, and M is selected from at least one of Ti, V, and Mg. At least a portion of the positive electrode active material comprises primary particles. The particle size distribution of primary particles having a primary particle size of 80 nm or more and less than 180 nm in the positive electrode active material is less than or equal to 10%. In a cross section cut after the positive electrode active material is prepared into an electrode sheet, the number of particles in a (250±5)μm2 region having a primary particle size of 1500 nm or more is not more than 15. The primary particle size distribution concentration in the positive electrode active material in the provided positive electrode sheet is significantly increased, and the cyclic performance of the battery is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode sheet and preparation method thereof, secondary battery and electric device

[0001] Cross-references

[0002] This application refers to Chinese Patent Application No. 202310542575.5 filed on May 15, 2023, entitled “Positive Electrode Active Material and Preparation Method Thereof, Positive Electrode Sheet, Secondary Battery and Electrical Device,” which is incorporated herein by reference in its entirety. Technical Field

[0003] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode plate and a preparation method thereof, a secondary battery and an electrical device. Background Art

[0004] Olivine phosphate-based cathode materials are widely used in secondary batteries due to their stable structure and excellent cycle life. As energy storage applications increase the performance requirements for secondary batteries, improving the cycle performance of olivine phosphate-based cathode materials is a pressing scientific and technological challenge in this field. One factor affecting the cycle performance of cathode active materials is the presence of fine powders in the materials, which rapidly degrades cycle life and thus hinders further improvement.

[0005] At present, the most common method to improve the micropowder in positive electrode active materials is to optimize the production process and equipment to reduce the generation of micropowder particles during the mixing or transportation of materials. Although this can reduce the generation of micropowder particles to a certain extent, the effect is minimal. Alternatively, a cyclone separation device is used to remove micropowder particles from the material, but the effect is not good, especially for nanomaterials of lithium iron phosphate or lithium manganese iron phosphate, which is difficult to achieve effective separation at a high yield.

[0006] In addition, the presence of ultra-large single crystal particles in the positive electrode active material affects the mechanical integrity of the positive electrode active material particles and also affects the cycle performance of the positive electrode active material.

[0007] Therefore, it is urgent to improve the content of micropowder and ultra-large single crystal particles in the positive electrode active material to improve the particle uniformity of the positive electrode active material.

[0008] Summary of the Invention

[0009] The present application aims to solve at least one of the technical problems existing in the background art. To this end, one object of the present application is to provide a positive electrode plate, which comprises a phosphate-based positive electrode active material. Compared with current conventional phosphate-based positive electrode active nanomaterials, this material has a significantly different primary particle distribution, with a more uniform distribution and a smaller proportion of micropowder and large particles, which can improve the cycling and high-temperature storage performance of the phosphate-based positive electrode active material.

[0010] The first aspect of the present application is to provide a positive electrode sheet, comprising a current collector and a positive electrode film layer located on at least one side of the current collector, wherein the positive electrode film layer comprises a positive electrode active material, wherein the positive electrode active material comprises a substrate and a carbon coating layer located on the surface of the substrate, wherein the substrate has a structural formula Li z Fe x Mn (1-x-y) M y PO4, wherein 0.5≤x≤1, 0≤y≤0.1, 1≤z≤1.1; M is selected from at least one of Ti, V, and Mg; at least a portion of the positive electrode active material comprises primary particles, and the particle size distribution of the primary particles having a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is less than or equal to 10%.

[0011] The positive electrode active material in the positive electrode plate provided in the present application has a primary particle size distribution of primary particles with a primary particle size of more than 80 nm and less than 180 nm in the positive electrode active material powder controlled within an appropriate range, which helps to reduce or slow down the cycle life decay of small-particle positive electrode active substances in the positive electrode active material, slow down the rate of side reactions between the surface of the micropowder and the electrolyte, and thus improve the cycle life of the positive electrode active material.

[0012] In some embodiments, the particle size distribution of primary particles with a primary particle size of 80 nm to 180 nm in the positive electrode active material is less than or equal to 8.5%, and optionally less than 8%, 6%, 5%, or 2%.

[0013] In some embodiments, the primary particles of the positive electrode active material with a primary particle size of 1500 nm or more are substantially 250 μm in the cross section of the positive electrode sheet. 2 The number of particles in the area does not exceed 15, optionally, in the basic 250μm 2 The number of particles in the area does not exceed 12, 8 or 6, optionally 250 μm 2 When measuring, it can have 5μm 2 The region is selected from the cross-sectional end face of the electrode piece, and the method of preparing the positive electrode active material into the electrode piece is well known in the art.

[0014] Primary particles with a primary particle size of more than 1500nm are prone to particle breakage or pulverization during the circulation of positive electrode active materials, reducing the mechanical integrity of the positive electrode active material particles and thus leading to loss of active material. Controlling the particle size distribution of primary particles with a primary particle size of more than 1500nm in the positive electrode active material powder within an appropriate range helps to improve the chemical mechanical stability of the positive electrode active material and improve the electrochemical performance, thereby improving the cycle stability of the positive electrode active material. Excessively large primary particle size causes the particles to break during the cycle, resulting in loss of electrical contact between the crushed particles, which is also an important cause of capacity decay during battery use. The fresh interface generated by the crushing will accelerate the dissolution of metal ions, leading to a decrease in cycle life.

[0015] In some embodiments, the primary particles with a primary particle size of 100 nm or more and 1500 nm or less are (250±5) μm in the cross section of the cathode active material after the cathode active material is prepared into an electrode sheet. 2 The particle size distribution index in the region is less than or equal to 0.45, and can be optionally less than or equal to 0.36, wherein the particle size distribution index refers to the ratio of the standard deviation of the primary particle size of the primary particles divided by the average primary particle size.

[0016] Primary particles with a primary particle size of more than 100nm and less than 1500nm have excellent particle size consistency, which makes the discharge behavior of each particle tend to be consistent during the battery cycle. The possibility of overcharging and over-discharging of each particle during the charge and discharge process is reduced, which is beneficial to ensure the structural stability of the positive electrode active material and improve the battery's room temperature cycle performance and high temperature cycle performance.

[0017] In some embodiments, the positive electrode active material includes secondary particles, and the particle size distribution of the secondary particles satisfies: (Dv90-Dv10) / Dv50≤3.

[0018] In the positive electrode active material, the particle size distribution of the secondary particles is within a suitable range, which helps to improve the particle size uniformity of the positive electrode active material.

[0019] In some embodiments, the secondary particles have a Dv50 of 0.45-1.5 μm, optionally 0.6-1.5 μm.

[0020] In the positive electrode active material, the particle size of the secondary particles is within a suitable range. During the charge and discharge process, the secondary particles will not or will reduce structural damage caused by excessive lithium deintercalation, or the polarization degree of the secondary particles during the charge and discharge process is reduced, which helps to make the current density on the surface of the secondary particles more uniform, thereby making the capacity of the positive electrode active material more fully utilized.

[0021] In some embodiments, in the general formula of the positive electrode active material provided by the present application, 0.6 < x ≤ 1, 0 ≤ y < 0.1, 1 ≤ z ≤ 1.1, optionally 0.8 ≤ x ≤ 1, 0.004 ≤ y ≤ 0.008, 1 ≤ z ≤ 1.08.

[0022] In some embodiments, in the positive electrode active material provided by the present application, the mass content of the M element in the positive electrode active material is 1000 ppm - 6000 ppm, optionally 1500 ppm - 5000 ppm.

[0023] The mass content of the M element in the positive electrode active material within a suitable range helps to improve the structural stability of the positive electrode active material.

[0024] The second aspect of the present application provides a method for preparing a positive electrode sheet, and the preparation method specifically includes:

[0025] Compaction granulation: Compacting and granulating raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, an M source, and a shaping aid to obtain compacted and formed particles;

[0026] Sintering: Filling the compacted and formed particles and sintering the compacted and formed particles to obtain secondary particles;

[0027] Crushing: Crushing the secondary particles to obtain a positive electrode active material;

[0028] Coating: Coating a positive electrode slurry containing the positive electrode active material on at least one side of a current collector to form a positive electrode sheet,

[0029] wherein the positive electrode active material includes a substrate and a carbon coating layer on the surface of the substrate, and the substrate has a structural general formula Li z Fe x Mn (1-x-y) M y PO4, where 0.5 ≤ x ≤ 1, 0 ≤ y ≤ 0.1, 1 ≤ z ≤ 1.1; M is selected from at least one of Ti, V, and Mg;

[0030] At least a part of the positive electrode active material includes primary particles, and the particle size distribution of primary particles with a primary particle size above 80 nm and below 180 nm in the positive electrode active material is less than or equal to 1

[0031] The number of primary particles with a primary particle size above 1500 nm in the cross-section (250 ± 5) μm 2 of the cut positive electrode sheet does not exceed 15.

[0032] Controlling the particle size distribution of primary particles with a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material powder within the above range helps to reduce or slow down the cycle life attenuation of small-particle positive electrode active substances in the positive electrode active material, thereby improving the cycle life of the positive electrode active material.

[0033] In some embodiments, the particle size distribution of primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material is less than or equal to 8.5%, and can be 8%, 6%, 5%, 4%, or less than 2%. The smaller the particle size distribution of primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material, the more conducive it is to improving the cycle life of the positive electrode active material and helping to maintain the stability of the cycle life of the positive electrode active material.

[0034] In some embodiments, the positive electrode active material in the positive electrode sheet prepared by the method has a primary particle size of 1500 nm or more and a particle size of (250±5) μm in the cross section after the electrode sheet is cut. 2 The number of particles in the area does not exceed 15, optionally, in the basic 250μm 2 The number of particles in the area does not exceed 12, 8 or 6.

[0035] Controlling the particle size distribution of primary particles with a primary particle size of more than 1500 nm in the positive electrode active material powder within the above range helps to improve the chemical mechanical stability of the positive electrode active material and improve the electrochemical performance, thereby improving the cycle stability of the positive electrode active material.

[0036] In some embodiments, the average particle size of the compacted granules in the compaction and granulation step is 3 mm to 30 mm.

[0037] Compacting the formed particles within a suitable range helps to improve the uniformity of different raw materials inside the particles. At the same time, the pores between the particles are conducive to eliminating the reducing gas generated by the decomposition of the carbon source during the preparation process. The uniformity of carbon at different positions in the sintering device (such as the crucible) is improved. At the same time, after compaction, the carbon source precursor will not flow significantly at high temperature, resulting in stratification at height.

[0038] In some embodiments, the compacted shaped particles have a compacted density of 1.0 g / cm 3 Above, optional 1.2-3.0g / cm 3 .

[0039] The compaction density of the compacted particles is controlled within a suitable range, which helps to increase the filling volume during the preparation process, thereby increasing the sintering capacity.

[0040] In some embodiments, the preparation method comprises: filling compacted shaped particles to a filling height of 5 cm to 30 cm, and sintering the compacted shaped particles to obtain secondary particles;

[0041] Optionally, the filling height is 8cm-20cm.

[0042] The filling height of the compacted particles during the sintering process is within an appropriate range, which helps to timely discharge the reducing gas generated by the decomposition of the carbon source during the sintering process, while accelerating heat transfer and avoiding uneven decomposition of the carbon source in the compacted particles at different positions in the sintering device, thereby improving the consistency of particle growth while taking into account production capacity.

[0043] In some embodiments, the preparation method includes pulverizing the secondary particles to a Dv50 of 0.45 μm to 1.5 μm, optionally 0.6 μm to 1.5 μm. By pulverizing the secondary particles to a particle size within the aforementioned range, the secondary particles are prevented from, or have reduced structural damage due to excessive lithium insertion and extraction during charge and discharge, or the polarization of the secondary particles during charge and discharge is reduced, thereby facilitating full utilization of the capacity of the positive electrode active material.

[0044] In some embodiments, the preparation method includes: pulverizing the secondary particles so that their particle size distribution satisfies: (Dv90 - Dv10) / Dv50 ≤ 3; alternatively, pulverizing the secondary particles so that their particle size distribution satisfies: 1 ≤ (Dv90 - Dv10) / Dv50 ≤ 3. Pulverizing the secondary particles so that their particle size distribution falls within the aforementioned range helps improve the particle size uniformity and cycle stability of the positive electrode active material.

[0045] In some embodiments, the compaction and granulation step specifically includes:

[0046] The raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M, forming aid and solvent are ground to obtain slurry; the slurry is dried and then compacted and granulated to obtain compacted and formed particles.

[0047] First, the grinding process reduces the size of existing oversized primary particles, reducing their content in the raw materials and helping to reduce the size distribution of oversized primary particles in the prepared positive electrode active material. This also reduces the particle size of different raw materials, helping to obtain more uniform nanometer-scale primary particles. This also improves the uniformity of the mixing of different raw materials, contributing to the uniformity of different components in the prepared positive electrode active material. Furthermore, the drying process creates appropriate pores between the raw material particles, facilitating the discharge of reducing gases generated by the decomposition of the carbon source during sintering.

[0048] In some embodiments, the sintering temperature in the sintering step is 600° C.-800° C.; and / or the constant temperature sintering time in the sintering step is 2 h-12 h.

[0049] The sintering temperature and / or sintering time are controlled within a suitable range so that the compacted particles are fully sintered, and thus the positive electrode active material has excellent structural parameters.

[0050] In some embodiments, the compaction and granulation step specifically includes:

[0051] (1-1) mixing initial reactants including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, and an M source uniformly and then pre-sintering the mixture to obtain an initial product;

[0052] (1-2) mixing and grinding an intermediate reactant including an initial product, a carbon source, and a molding aid to obtain an intermediate product;

[0053] (2) compacting and granulating the intermediate product to obtain compacted granules,

[0054] Wherein, the mass content of the carbon source in the step (1-1) is 2%-5%, based on the total mass of the initial reactants.

[0055] A small amount of carbon source in the pre-sintering process can play a reducing role, allowing the initial reactants to be fully mixed and reacted, improving the uniformity and completeness of the reaction, and obtaining an initial product with excellent particle size uniformity. The pre-sintering treatment allows the ultrafine particles in the initial reactants to pre-react, reducing the content of small particles in the raw materials and improving the particle size uniformity of the material. At the same time, the intermediate reactant containing the initial product, carbon source and forming aid is further ground to refine large particles, reduce the content of oversized primary particles in the raw materials, and further improve the particle size uniformity of the material, providing a material basis for the subsequent preparation of positive electrode active materials with excellent particle size uniformity.

[0056] In summary, the pre-sintering treatment can improve the particle size uniformity of the initial reactants, so that the intermediate product undergoing compaction and granulation has excellent particle size uniformity, which helps to improve the uniformity of different components in the prepared positive electrode active material.

[0057] In some embodiments, the Dv50 of the intermediate product is 0.45 μm-1.25 μm, and the D V 10 is greater than or equal to 0.15μm.

[0058] Control the Dv50 and D V 10 Within a suitable range, it is beneficial to control the mass content of small particles of the positive electrode active material, which can improve the structural stability of the positive electrode active material and improve the cycle performance of the battery.

[0059] The third aspect of the present application provides a secondary battery, comprising a negative electrode sheet and a positive electrode sheet provided by the first aspect of the present application or a positive electrode sheet prepared by the preparation method provided by the second aspect.

[0060] A fourth aspect of the present application provides an electrical device, comprising the secondary battery provided in the third aspect of the present application.

[0061] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar components or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in this application and should not be construed as limiting the scope of this application.

[0063] FIG1 is a schematic diagram of sintering of compacted shaped particles in a sintering device in the present application;

[0064] FIG2 is a scanning electron microscope (SEM) photograph of the positive electrode active material in Example 1 of the present application;

[0065] FIG3 is a scanning electron microscope photograph of a cross-section of the positive electrode active material prepared as a positive electrode sheet in Example 1 of the present application, taken by argon ion beam cutting; the electron microscope scale in FIG3A is 2 μm; the electron microscope scale in FIG3B is 500 nm;

[0066] FIG4 is a scanning electron microscope photograph of a cross section of the positive electrode active material prepared as a positive electrode sheet in Comparative Example 1 of the present application, taken by argon ion beam cutting. The electron microscope scale in FIG4A is 1 μm; the electron microscope scale in FIG4B is 200 nm.

[0067] FIG5 is a cycle performance test curve of the secondary battery in Example 1 and Comparative Example 1 of the present application at 25° C. and 60° C.;

[0068] FIG6 is a schematic diagram of a secondary battery cell according to an embodiment of the present application;

[0069] FIG7 is an exploded view of the secondary battery cell according to an embodiment of the present application shown in FIG6 ;

[0070] FIG8 is a schematic diagram of a battery module according to an embodiment of the present application;

[0071] FIG9 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0072] FIG10 is an exploded view of the battery pack according to one embodiment of the present application shown in FIG9 ;

[0073] 11 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application;

[0074] 12 is a SEM photograph of a cross section of a secondary battery in one embodiment of the present application;

[0075] FIG13 is a scanning electron microscope photograph of the cross section of the positive electrode piece after argon ion beam cutting in Example 15 of the present application.

[0076] Description of reference numerals:

[0077] 1. Battery pack; 2. Upper box; 3. Lower box; 4. Battery module; 5. Secondary battery; 5. Casing; 5. Electrode assembly; 5. Cover plate; 6. Compacted pellets; 7. Sagger. DETAILED DESCRIPTION

[0078] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.

[0079] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0080] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0081] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0082] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0083] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0084] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0085] positive electrode active material

[0086] Multiple factors can affect the cycle performance of positive electrode active materials, such as the residual alkali content on the surface of the material, the integrity of the crystal structure of the material, the content of micropowder in the material, and the water content adsorbed on the surface of the material. Among them, the content of micropowder, that is, the proportion of small particles in all particles, is an important factor restricting the further improvement of battery cyclability. This is because in the synthesis reaction of positive electrode active materials, the embedding energy barrier of lithium ions in particles with smaller particle sizes is lower and the reaction activity is higher, resulting in the transition of lithium ions into lithium in the micropowder, the Li content in the small particles of micropowder is excessive, and the Li content in other particles with a particle size larger than the particle size of the micropowder is insufficient, that is, the lithium distribution is uneven. During the charging process, due to polarization, the small particles are always excessively delithiated and the structure is destroyed, and the side reactions between the small particles and the electrolyte in the charged state are more intense, and more obvious at high temperatures, resulting in a faster decay of the cycle life of the small particles. Therefore, controlling the content of micropowder in the positive electrode active material helps to improve the cycle performance in energy storage devices (e.g., secondary batteries).

[0087] The present application provides a carbon-coated (@C) phosphate-based positive electrode active material, including the general formula Li z Fe x Mn (1-x- y) M y At least one of the compounds shown in PO4@C, wherein 0.5≤x≤1, 0≤y≤0.1, and 1≤z≤1.1; M is selected from at least one of Ti, V, and Mg; at least a portion of the positive electrode active material comprises primary particles, and the particle size distribution of the primary particles having a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is less than or equal to 10%.

[0088] In this article, the term "positive electrode active material" may be "Li z Fe x Mn (1-x-y) M y PO4@C” indicates.

[0089] In this article, the term "positive electrode active material, including the general formula Li z Fe x Mn (1-x-y) M y At least one of the compounds shown in PO4@C and the term "positive electrode active material includes a substrate and a carbon coating layer located on the surface of the substrate, the substrate having a structural formula Li z Fe x Mn (1-x-y) M y PO4” is the same expression.

[0090] In some embodiments, the particle size distribution of primary particles with a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is less than or equal to 9.5%, 9%, 8.5%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1%, or the particle size distribution of primary particles with a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is selected from 0.1%-10%, 0.5%-10%, 1%-10%, 0.1%-8%, 0.1%-6%, 0.1%-4%, 0.1%-3%, 0.1%-2%, 0.1%-1%, 0.3%-5%, 0.8%-3%, or 0.1%-1.5%.

[0091] The term "primary particle" is also called a single crystal particle. Usually, a single small crystal grain is called a primary particle. In some cases, even if it is an amorphous particle, when there are original particles and agglomerated particles, the original particles can also be called primary particles.

[0092] Agglomerates between multiple primary particles or particles form aggregates called "secondary particles." The forces that cause particles to aggregate can be physical bonds (such as van der Waals forces) or chemical bonds (such as bridging oxygen bonds). Agglomeration can be achieved through external pressure or by the aid of additional substances (such as adhesive chemicals). The size of these secondary particles is called the "secondary particle size."

[0093] Herein, the term "primary particle size" refers to the particle size of primary particles.

[0094] In this application, the terms "micropowder", "small particles" and "micropowder small particles" have the same meaning, and refer to particles with a particle size of more than 80 nm and less than 180 nm, and the particles include primary particles and secondary particles.

[0095] The term "particle size distribution" refers to the percentage of particles within a certain particle size or a certain particle size range in the total number of powder particles.

[0096] The particle size distribution can be determined by a commonly used detection method in the art, such as a laser particle size analyzer, to determine the particle size distribution of the powder particles.

[0097] The particle size distribution can also be measured by the long diameter statistical method, which can measure the particle size of the active material in the electrode membrane. In some embodiments, the electrode can be cut perpendicular to the electrode plane (for example, a relatively large plane) using an argon ion beam, and the exposed section is photographed using a scanning electron microscope. The diameter of the equivalent circle is calculated according to the cross-sectional area of ​​each particle. Particles below 80nm are difficult to distinguish one by one when photographed using a scanning electron microscope. In this case, particles below 80nm can be excluded from the statistics when measuring the particle size distribution using the equivalent circle diameter statistical method.

[0098] In the positive electrode active material provided in the present application, the particle size distribution of primary particles with a primary particle size of more than 80 nm and less than 180 nm in the positive electrode active material powder is controlled within 10%, which helps to reduce the number of micropowders whose structures are destroyed due to excessive delithiation during charging, reduce the side reactions between micropowders and electrolytes, delay the cycle life attenuation of the positive electrode active material, and thus improve the cycle life of the positive electrode active material.

[0099] As mentioned above, the high activity of micropowders in the reaction leads to uneven lithium distribution in the cathode active material, which also affects the surface condition of the cathode active material. When the powder content is too high, the alkalinity of the cathode active material increases due to the high lithium content, which increases side reactions with the binder, deteriorating the processability of the slurry and causing a rapid increase in slurry viscosity. In severe cases, gelation may occur. Maintaining the micropowder particle size distribution within an appropriate range also helps improve the processability of the cathode active material.

[0100] In some embodiments, the particle size distribution of primary particles with a primary particle size of 80 nm to 180 nm in the positive electrode active material is less than or equal to 8.5%, and optionally less than 8%, 6%, 5%, or 2%.

[0101] Controlling the particle size distribution of primary particles with a primary particle size of more than 80nm and less than 180nm in the positive electrode active material powder to less than 8.5% can further reduce the possibility of side reactions between the micropowder and the electrolyte, and improve the battery's room temperature cycle capacity retention rate and high temperature cycle capacity retention rate.

[0102] In some embodiments, the positive electrode active material has a primary particle size of 1500 nm or more and a primary particle size of 250 μm or more. 2 The number of particles in the area does not exceed 15, optionally, in the area of ​​250 μm 2 The number of particles in the area does not exceed 12, 10, 9, 8, 7, 6, 5, 4, 3, or 2. "Basic" indicates the measurement error or the degree of fluctuation during measurement, which can be selected as 5μm 2The "region" refers to the region in the cross section of the cathode active material after it is prepared into a pole piece. The region is used to measure the number of large particles. The method of preparing a cathode active material into a pole piece is well known in the art.

[0103] In some embodiments, the positive electrode active material can be prepared into a pole piece according to the method disclosed in Example 1. In some embodiments, the positive electrode material powder and polyvinylidene fluoride (PVDF) binder can be mixed in a mass ratio of 95:5, and N-methylpyrrolidone is used as a solvent to prepare a pole piece, which is cold pressed to a compaction density of 2.2 g / cm 3 .

[0104] In some embodiments, the primary particles of the positive electrode active material having a primary particle size of 1500 nm or more are substantially 250 μm. 2 The number of particles in the area does not exceed 0-2, 0-3, 1-2, 1-3, 2-3, 0-4, 2-4, 3-4, 0-5, 2-5, 0-6, 5-6, 6-8, 8-14.

[0105] In some embodiments, the primary particles of the positive electrode active material having a primary particle size of 1500 nm or more are substantially 250 μm. 2 The number of particles in the area does not exceed 0-2, 0-3, 1-2, 1-3, 2-3, 0-4, 2-4, 3-4, 0-5, 2-5, 0-6, 5-6, 6-8, 8-12.

[0106] The number of particles with a primary particle size of 1500nm or larger can be counted using a scanning electron microscope (SEM). For example, an argon ion beam is used to cut the electrode perpendicular to its large surface, exposing the end face. The end face is photographed using an SEM, and the particle size is counted using the equivalent circle area method. The number of large particles can be determined using a single measurement or by averaging multiple measurements.

[0107] Primary particles with a primary particle size of more than 1500nm are also called "large particles", "ultra-large single crystal particles" or "ultra-large primary particles". During the cycle process, the positive electrode material undergoes a deformation process of repeated expansion and contraction. Due to deformation, the ultra-large primary particles undergo intergranular cracks during the cycle, which in turn causes severe pulverization of the ultra-large primary particles. This seriously reduces the mechanical integrity of the primary and secondary particles, aggravates the penetration of the electrolyte, and leads to a large loss of positive electrode active materials (for example, lithium ions). At the same time, the presence of intergranular cracks also causes electrical contact failure, aggravating capacity polarization loss. Correspondingly, the continuous generation of new electrode / electrolyte interfaces also leads to a sharp deterioration in the chemical and mechanical properties of the positive electrode active materials during long cycles.

[0108] Controlling the particle size distribution of primary particles with a primary particle size of 1500 nm or greater within an appropriate range within the cathode active material powder can effectively prevent particle breakage, alleviate surface degradation, and suppress intergranular cracking, thereby enhancing chemical-mechanical stability and improving electrochemical performance. This suppresses interfacial degradation and overall mechanical disintegration, enhancing chemical-mechanical stability, and ultimately improving the cycling stability of the cathode active material.

[0109] In some embodiments, the primary particles with a primary particle size of 100 nm or more and 1500 nm or less are (250±5) μm in the cross section of the cathode active material after the cathode active material is prepared into an electrode sheet. 2 The particle size distribution index in the region is less than or equal to 0.45, wherein the particle size distribution index refers to the ratio of the standard deviation of the primary particle diameters of the primary particles divided by the average primary particle diameter.

[0110] In some embodiments, the primary particles with a primary particle size of 100 nm or more and 1500 nm or less are (250±5) μm in the cross section of the cathode active material after the cathode active material is prepared into an electrode sheet. 2 The particle size distribution index within the region may be selected from any one of less than or equal to 0.45, less than or equal to 0.40, less than or equal to 0.35, less than or equal to 0.3, less than or equal to 0.25, and less than or equal to 0.20.

[0111] In some embodiments, the primary particles with a primary particle size of 100 nm or more and 1500 nm or less are (250±5) μm in the cross section of the cathode active material after the cathode active material is prepared into an electrode sheet. 2 The particle size distribution index in the region is less than or equal to 0.36, wherein the particle size distribution index refers to the ratio of the standard deviation of the primary particle diameters of the primary particles divided by the average primary particle diameter.

[0112] In some embodiments, the primary particles with a primary particle size of 100 nm or more and 1500 nm or less are (250±5) μm in the cross section of the cathode active material after the cathode active material is prepared into an electrode sheet. 2 The particle size distribution index within the region may be selected from any one of less than or equal to 0.36, less than or equal to 0.3, less than or equal to 0.25, and less than or equal to 0.20.

[0113] The particle size distribution index has a well-known meaning in the art and can be measured by test methods and test instruments well-known in the art. The particle size distribution index is an important parameter for measuring the uniformity of particle size. The lower the particle size distribution index, the smaller the particle size deviation value, and the higher the particle size uniformity. As an example test method, the electrode is cut open perpendicularly to the large surface of the electrode using an argon ion beam to expose the cross section, and the cross section is photographed using a scanning electron microscope. The particle size of the positive electrode active material is statistically analyzed using the equivalent circle area statistical method.

[0114] The particle size distribution index (PDI) is the standard deviation of the particle size divided by the average particle size.

[0115] Where σ is the standard deviation of particle size, x i is the particle size value, is the average particle size, n is the total number of particles counted, and the average particle size is the total particle size value divided by the total number of particles counted.

[0116] Average particle size The total particle size of primary particles with a primary particle size of 100 nm or more and 1500 nm or less divided by the number of primary particles with a primary particle size of 100 nm or more and 1500 nm or less,

[0117] Particle size x i The particle size of primary particles is between 100 nm and 1500 nm.

[0118] The total number of particles n is (250±5) μm in the cross section of the positive electrode sheet. 2 The number of primary particles with a primary particle size of 100 nm or more and 1500 nm or less within the region.

[0119] Primary particles with a primary particle size of more than 100nm and less than 1500nm have excellent particle size consistency, which makes the discharge behavior of each particle tend to be consistent during the battery cycle. The possibility of overcharging and over-discharging of each particle during the charge and discharge process is reduced, which is beneficial to ensure the structural stability of the positive electrode active material and improve the battery's room temperature cycle performance and high temperature cycle performance.

[0120] In some embodiments, the positive electrode active material includes secondary particles, and the particle size distribution of the secondary particles satisfies: (Dv90-Dv10) / Dv50≤3, optionally less than or equal to 2.9, 2.8, 2.6, 2.5, 2.4, 2.3, 2.2, 1.4, 1.5, or 1.2. Alternatively, 1≤(Dv90-Dv10) / Dv50≤3.

[0121] In the positive electrode active material, the particle size distribution of the secondary particles is within a suitable range, which helps to improve the particle size uniformity of the positive electrode active material and further enhance the cycle performance.

[0122] In some embodiments, the Dv50 of the secondary particles is 0.45 - 1.5 μm, optionally 0.5 - 1.5 μm, 0.8 - 1.5 μm, 0.7 - 1.5 μm, 1 - 1.5 μm, 0.45 - 1.3 μm, 0.45 - 1.0 μm, 0.5 - 1.0 μm, 0.6 - 1.5 μm or 0.7 - 1.5 μm, or any value within the range.

[0123] In the positive electrode active material, the particle size of the secondary particles is within a suitable range. During charge and discharge, the secondary particles will not or reduce the structural damage caused by excessive lithium deintercalation and intercalation. In addition, it helps to reduce the polarization degree of the secondary particles during charge and discharge, helps to make the current density on the surface of the secondary particles more uniform, so as to fully exert the capacity of the positive electrode active material and improve the cycle performance.

[0124] In the positive electrode active material provided by the present application, while reducing the particle size distribution of fine powder and large particles, the concentration degree of the particle size distribution of the positive electrode active material is significantly improved.

[0125] In some embodiments, the positive electrode active material may be one or more of lithium iron phosphate or lithium iron manganese phosphate with an olivine structure and their modified compounds, which can improve the rate performance of the battery while enhancing the cycle performance and storage performance of the battery. The working voltage of the battery using these positive electrode active materials is not high, generally ≤ 4.35V, so the cycle performance and storage performance of the battery can be further improved.

[0126] In some embodiments, in the positive electrode active material provided by the present application, 0.6 < x ≤ 1, 0 ≤ y < 0.1, 1 ≤ z ≤ 1.1, optionally 0.8 ≤ x ≤ 1, 0.004 ≤ y ≤ 0.008, and 1 ≤ z ≤ 1.08.

[0127] In some embodiments, in the positive electrode active material provided by the present application, the mass content of the M element in the positive electrode active material is selected from 1000 ppm to 6000 ppm, optionally 1000 ppm to 5500 ppm, 1000 ppm to 5000 ppm, 1500 ppm to 6000 ppm, 1500 ppm to 5000 ppm, 2000 ppm to 6000 ppm, 2500 ppm to 6000 ppm, or 2000 ppm to 5500 ppm, or any value within the range.

[0128] In some embodiments, the M includes Ti. In some embodiments, the M includes V. In some embodiments, the M includes Mg.

[0129] The main body of the anion part of the positive electrode active material is a phosphate matrix, and the metal matrix is mainly composed of iron, manganese, or a combination of both. By introducing divalent or polyvalent M cations, lithium ions are intercalated and deintercalated in the matrix of the olivine structure composed of cations including M and anions including phosphoric acid, which helps to improve the structural stability of the positive electrode active material.

[0130] Preparation method of positive electrode active material

[0131] The present application provides a preparation method of a carbon-coated (@C) phosphate-based positive electrode active material, and the positive electrode active material includes at least one of the compounds represented by the general formula Li z Fe x Mn (1-x-y) M y PO4@C, where 0.5 ≤ x ≤ 1, 0 ≤ y ≤ 0.1, 1 ≤ z ≤ 1.1; M is selected from at least one of Ti, V, and Mg.

[0132] In the positive electrode active material of some embodiments, 0.6 < x ≤ 1, 0 ≤ y < 0.1, optionally 0.8 ≤ x ≤ 1, 0.004 ≤ y ≤ 0.008, 1 ≤ z ≤ 1.08. In some embodiments, the M is selected from Ti. In some embodiments, the M is selected from V. In some embodiments, the M is selected from Mg.

[0133] In the positive electrode active material of some embodiments, the mass content of the M element in the positive electrode active material is 1000 ppm - 6000 ppm, optionally 1000 ppm - 5500 ppm, 1000 ppm - 5000 ppm, 1500 ppm - 6000 ppm, 1500 ppm - 5000 ppm, 2000 ppm - 6000 ppm, 2500 ppm - 6000 ppm, or 2000 ppm - 5500 ppm, or any value within the range.

[0134] The main body of the anion part of the positive electrode active material is a phosphate matrix, and the metal matrix is mainly composed of iron, manganese, or a combination of both. By introducing divalent or polyvalent M cations, lithium ions are intercalated and deintercalated in the matrix of the olivine structure composed of cations including M and anions including phosphoric acid, which helps to improve the structural stability of the positive electrode active material.

[0135] In some embodiments, the positive electrode active material can be one or several of lithium iron phosphate or lithium iron manganese phosphate with an olivine structure and their modified compounds, which can improve the rate performance of the battery while enhancing the cycle performance and storage performance of the battery. The working voltage of the battery using these positive electrode active materials is not high, generally ≤ 4.35V, so the cycle performance and storage performance of the battery can be further improved.

[0136] The preparation method provided in this application comprises the following steps:

[0137] Raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, an M source and a molding aid are mixed uniformly and then compacted and granulated to obtain compacted molded particles.

[0138] Generally speaking, a compacted particle is an actual particle group composed of particles of different sizes and shapes. Compared with an imaginary particle group composed of uniform spherical particles, if the particle diameters of the two are the same, the diameter of the spherical particles is the average particle diameter of the actual particle group (compacted particle). For spherical particles, there is no doubt that the spherical diameter is the particle diameter of the particle, but in reality, there are no real spherical particles, and the shape of the actual particles is very complex. For convenience, this application uses an equivalent particle size to describe the particle size (particle size) or average particle size of irregular particles. It can be understood that when the physical properties or physical behavior of a particle is closest to a homogeneous sphere of a certain diameter, the diameter (or combination) of the sphere is taken as the equivalent particle size of the measured particle.

[0139] The average particle size can be determined using a particle size determination method or instrument commonly used in the art, including but not limited to a laser particle size analyzer or an ultrasonic particle size analyzer. The average particle size can be a linear average diameter, an area average diameter, a volume average diameter, a weight average diameter, or a specific surface area average diameter. The average particle size herein refers to the volume average diameter. When an equivalent particle size is used to describe particle size, the average particle size herein may also refer to the volume equivalent diameter.

[0140] In some embodiments, the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, lithium oxide, lithium chloride, lithium nitrate, and lithium sulfate. Optionally, the lithium source includes lithium carbonate.

[0141] In some embodiments, the iron source includes at least one of ferric phosphate, ferrous hydroxide, ferrous nitrate, ferrous phosphate, ferrous pyrophosphate, ferrous carbonate, ferrous chloride, ferrous oxalate, ferric chloride, ferric hydroxide, ferric nitrate, ferric citrate, and ferric oxide. Optionally, the iron source includes ferric oxide.

[0142] In some embodiments, the manganese source includes at least one of manganese dioxide, manganese trioxide, manganese tetraoxide, manganese oxalate, manganese acetate, or manganese nitrate.

[0143] In some embodiments, the phosphorus source includes at least one of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, iron phosphate, lithium dihydrogen phosphate, and lithium phosphate. Optionally, the phosphorus source includes ammonium dihydrogen phosphate.

[0144] In some embodiments, the carbon source includes at least one of sucrose, glucose, citric acid, fructose, lactose, porous graphene, activated carbon, activated carbon fiber, mesoporous carbon, carbon nanotubes, carbon molecular sieves, asphalt and polyethylene glycol. Optionally, the carbon source includes sucrose.

[0145] In some embodiments, the M source is selected from at least one of oxides, hydroxides, oxalates, acetates, chlorides, nitrates or phosphates of Ti, V, and Mg. Optionally, the M source includes one or more of titanium dioxide, magnesium hydroxide, and vanadium pentoxide.

[0146] The molding aid is selected from a polymer that can be dissolved or dispersed in water or alcohol. In some embodiments, the molding aid includes at least one of polypropylene, starch, phenolic resin, polyurethane, melamine resin, polyethylene, stearic acid, PVC, polyacrylonitrile, natural rubber, styrene-butadiene rubber, and butadiene rubber. Optionally, the molding aid includes starch.

[0147] The molding aid can further improve the integrity of the compacted particles during the sintering process, enhance the mechanical stability of the compacted particles during the sintering process, and avoid structural collapse of the particles during the sintering process.

[0148] In some embodiments, raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, an M source, and a molding aid are ground; optionally, the raw materials are ground to a Dv50 of 0.3-1.5 μm, 0.3-1.0 μm, 0.3-0.8 μm, 0.35-0.6 μm, or 0.35-0.9 μm. The raw materials can be ground using a grinding device such as a ball mill, a sand mill, or a mechanical mill.

[0149] In some embodiments, water, an alcohol solvent, or a homogeneous and stable mixed solution of the two can be added and mixed with the raw materials before grinding. The alcohol solvent includes but is not limited to methanol, ethanol, and ethylene glycol, and can be a mixture of one or more different alcohol solvents.

[0150] In some embodiments, the molding aid in the raw materials can be dissolved or dispersed in water, alcohol solvent, or a uniform and stable mixed solution of the two, and mixed with other components in the raw materials as the solvent or solution is added.

[0151] After grinding, the size of the oversized primary particles decreases, reducing their content in the raw materials and helping to reduce the size distribution of the oversized primary particles in the prepared positive electrode active material. This also reduces the particle size of different raw materials, helping to obtain more uniform nanometer-scale primary particles. This also improves the uniformity of the mixing of different raw materials, helping to improve the uniformity of the different components in the prepared positive electrode active material.

[0152] In some embodiments, the ground raw material is dried, or alternatively, spray dried. In some embodiments, the microspheres formed by spray drying have a particle size Dv50 of 5-50 μm, or alternatively, 5-40 μm, 8-30 μm, 10-25 μm, or 10-20 μm.

[0153] The raw materials processed by spray drying are spherical with good fluidity, and there are appropriate pores between the raw material particles, which are conducive to the discharge of reducing gases generated by the decomposition of the carbon source during the sintering process.

[0154] In some embodiments, the raw material after the spray drying process is compacted and granulated.

[0155] In some embodiments, raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, an M source, and a molding aid are compacted and granulated to obtain compacted granules having an average particle size of 3 mm to 30 mm, optionally 5 mm to 25 mm, 5 mm to 20 mm, 5 mm to 15 mm, 10 mm to 15 mm, 10 mm to 20 mm, or 10 mm to 25 mm. The average particle size can also be selected from any value of 7.5 mm, 12.5 mm, 17.5 mm, 22.5 mm, or 27.5 mm, or a range between any two values.

[0156] When the average particle size of the compacted granules is less than 3mm, the pores formed by the bridges between the granules are small, and the improvement in gas removal is not significant. When the average particle size of the compacted granules is greater than 30mm, the uniformity of the nanoparticles within a single compacted granule cannot be guaranteed, and the gas removal capacity of a single compacted granule is significantly reduced. Compacting the granules within the appropriate range helps improve the uniformity of the different raw materials within the granules, and the pores between the granules are conducive to removing the reducing gases generated by the decomposition of the carbon source during the preparation process.

[0157] In some embodiments, the compacted granules obtained by compaction granulation have a compaction density of 1.0 g / cm 3 Above, optional 1.2-3.0g / cm 3 .

[0158] The compaction density of the compacted particles is controlled within a suitable range, which helps to increase the filling volume during the preparation process, thereby increasing the sintering capacity.

[0159] In some embodiments, the preparation method includes: packing the compacted granules to a packing height of 5 cm to 30 cm, and sintering the compacted granules to obtain secondary granules. Optionally, the packing height is 8 cm to 30 cm, 8 cm to 20 cm, 5 cm to 25 cm, 5 cm to 20 cm, 10 cm to 30 cm, 10 cm to 25 cm, or 10 cm to 20 cm.

[0160] FIG1 shows a schematic diagram of the sintering of compacted particles in a filling component of a sintering device, such as a sagger. The sagger 7 is generally made of graphite material, and is used to fill the compacted particles 6. At this time, pores can be formed between the compacted particles 6, and the reducing gas and other gaseous substances generated by the decomposition of the carbon source during the sintering process can be discharged from the pores in the direction indicated by the arrow in FIG1 . The rising gas can transfer heat to the compacted particles 6 on the top layer of the sagger 7. When the gas is not discharged smoothly, the temperature of each part of the sagger 7 is uneven, and the content of reducing gas on the top layer of the sagger 7 may be high. The filling height of the compacted particles within an appropriate range is helpful to timely discharge the reducing gas and other gaseous unwanted substances during the sintering process, while accelerating the heat transfer and avoiding the uneven decomposition of the carbon source in the compacted particles at different positions in the sintering device, which can improve the consistency of particle growth; at the same time, it takes into account production capacity.

[0161] In some embodiments, after filling and compacting the formed particles, the porosity between the particles is 5%-20%. Optionally, the porosity is selected from 5%-15%, 10%-20%, 10%-15%, 8%-20%, 12%-20% or 8%-17%.

[0162] In some embodiments, the compacted particles are sintered in an inert gas atmosphere. The inert gas may include one or more of nitrogen, carbon dioxide, and helium. Optionally, the inert gas is selected from nitrogen.

[0163] In some embodiments, the compacted shaped particles are sintered within a sintering temperature range of 600°C-800°C. Optionally, the sintering temperature is selected from 650°C-800°C, 680°C-800°C, 700°C-800°C, 600°C-780°C, 600°C-750°C, 620°C-800°C or 640°C-720°C.

[0164] In some embodiments, the compacted particles are sintered at a sintering temperature range of 600°C-800°C for 2-12 hours, optionally sintered at the sintering temperature for 2-10 hours, 4-12 hours, 2-10 hours, 4-8 hours, 6-12 hours, 6-10 hours or 6-8 hours.

[0165] In some embodiments, during the sintering process, the heating rate is controlled at 1°C-5°C / min to the sintering temperature. Optionally, the heating rate is selected from 2°C-5°C / min, 3°C-5°C / min, 2°C-4°C / min or 2°C-3°C / min; or, the heating rate is selected from 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, or a range between any two of the above values.

[0166] In the preparation method provided herein, the raw material mixture is compacted and granulated before sintering. This facilitates the timely discharge of reducing gases from the decomposition of the carbon source during the sintering process, preventing uneven decomposition of the carbon source at different locations in the sintering apparatus. This also ensures that the compacted particles at different locations in the sintering apparatus are heated evenly. After sintering, the carbon content in the surface, middle, and bottom particles tends to be consistent, resulting in a substantially consistent growth-retarding effect on the raw material particles during the sintering reduction process, and improving the uniformity of the carbon content in the primary particle nanomaterial.

[0167] In some embodiments, the preparation method includes: crushing the secondary particles obtained after sintering so that their Dv50 is 0.45μm-1.5μm, optionally, crushing to a Dv50 selected from 0.5-1.5μm, 0.8-1.5μm, 0.7-1.5μm, 1-1.5μm, 0.45-1.3μm, 0.45-1.0μm, 0.5-1.0μm, 0.6-1.5μm or 0.7-1.5μm.

[0168] D V 50 is too small, the overall particle size is low, the proportion of small particles increases, and the surface stability of the material decreases; D V If 50 is too large, the overall particle size is low, the proportion of large particles increases, and the particle breakage effect increases during the circulation process, which is not conducive to improving material stability.

[0169] Crushing the secondary particles to an appropriate particle size range prevents or reduces structural damage to the secondary particles due to excessive lithium insertion and removal during charge and discharge. This also helps reduce the polarization of the secondary particles during charge and discharge, making the current density on the surface of the secondary particles more uniform and improving the stability of the material, thereby fully utilizing the capacity of the positive electrode active material and enhancing cycle performance.

[0170] In some embodiments, the preparation method includes: crushing the secondary particles so that their particle size distribution satisfies: (Dv90-Dv10) / Dv50≤3, optionally, less than or equal to 2.9, 2.8, 2.6, 2.5, 2.4, 2.3, 2.2, 2, 1.8, 1.4, 1.2, or 1.5. Alternatively, crushing the secondary particles so that their particle size distribution satisfies: 1≤(Dv90-Dv10) / Dv50≤3.

[0171] In the positive electrode active material, the particle size distribution of the secondary particles is within a suitable range, which helps to improve the particle size uniformity of the positive electrode active material and further enhance the cycle performance.

[0172] In some embodiments, the preparation method includes crushing the sintered secondary particles so that at least a portion of the obtained positive electrode active material includes primary particles, and the particle size distribution of primary particles with a primary particle size of more than 80nm and less than 180nm in the positive electrode active material is less than or equal to 10%.

[0173] In some embodiments, the particle size distribution of primary particles with a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is less than or equal to 9.5%, 9%, 8.5%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1%, or the particle size distribution of primary particles with a primary particle size of greater than 50 nm and less than 200 nm in the positive electrode active material is selected from 0.1%-10%, 0.5%-10%, 1%-10%, 0.1%-8%, 0.1%-6%, 0.1%-4%, 0.1%-3%, 0.1%-2%, 0.1%-1%, 0.3%-5%, 0.8%-3%, or 0.1%-1.5%.

[0174] In the positive electrode active material prepared by the preparation method provided in the present application, the particle size distribution of the micropowder is significantly reduced, the side reaction between the micropowder and the electrolyte is reduced, the cycle life attenuation of the positive electrode active material is delayed, and the cycle life of the positive electrode active material is improved.

[0175] At the same time, the positive electrode active material prepared by the method reduces the particle size distribution of the micropowder, reduces the side reaction between the positive electrode active material and the binder, and improves the processing performance of the positive electrode active material.

[0176] In some embodiments, the secondary particles are crushed so that the primary particle size of the obtained positive electrode active material is less than 1500 nm and the primary particle size is less than 250 μm. 2 The number of particles in the area does not exceed 15, optionally within 250μm 2 The number of particles in the area does not exceed 12, 10, 9, 8, 7, 6, 5, 4, 3, or 2.

[0177] The positive electrode active material prepared by this method significantly reduces the particle size distribution of oversized primary particles, improving the mechanical integrity of the primary and secondary particles, and delaying the penetration of electrolyte into the positive electrode active material and the loss of positive electrode active substances (e.g., lithium ions) during cycling. Furthermore, it reduces electrical contact failure and capacity polarization loss caused by intergranular cracks in oversized primary particles, thereby improving the chemical, mechanical, and cycling performance of the positive electrode active material.

[0178] In some embodiments, the preparation method does not include multiple compaction granulation.

[0179] The preparation method provided in this application has a simple process flow, high reproducibility, and relatively low cost, which is conducive to industrial mass production.

[0180] In some embodiments, the preparation method comprises:

[0181] Raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source and forming aid are mixed with water, alcohol or mixed solvent, ground, dried and compacted to obtain compacted particles; the compacted particles are filled, sintered and crushed to obtain positive electrode active material.

[0182] In some embodiments, the preparation method comprises:

[0183] Mixing raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source and a molding aid with water, an alcohol or a mixed solvent, grinding, drying, and compacting to obtain compacted particles with an average particle size controlled in the range of 3 mm to 30 mm;

[0184] Filling the compacted particles to a filling height of 5 cm to 30 cm with a porosity of 5% to 20%, and sintering;

[0185] The secondary particles obtained by pulverizing and sintering are pulverized to a Dv50 of 0.45 μm-1.5 μm and / or 1≤(Dv90-Dv10) / Dv50≤3 to obtain a positive electrode active material.

[0186] In some embodiments, the preparation method comprises:

[0187] Compacting and granulating: Compacting and granulating raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M source and molding aid to obtain compacted and molded particles;

[0188] Sintering: filling the compacted particles and sintering the compacted particles to obtain secondary particles;

[0189] Crushing: Crushing the secondary particles to obtain a positive electrode active material.

[0190] In some embodiments, the preparation method comprises:

[0191] Compacting and granulating: grinding raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M, forming aid and solvent to obtain slurry; drying the slurry and then compacting and granulating to obtain compacted granules;

[0192] Sintering: filling the compacted particles and sintering the compacted particles to obtain secondary particles;

[0193] Crushing: Crushing the secondary particles to obtain a positive electrode active material.

[0194] First, the grinding process reduces the size of existing oversized primary particles, reducing their content in the raw materials and helping to reduce the size distribution of oversized primary particles in the prepared positive electrode active material. This also reduces the particle size of different raw materials, helping to obtain more uniform nanometer-scale primary particles. This also improves the uniformity of the mixing of different raw materials, contributing to the uniformity of different components in the prepared positive electrode active material. Furthermore, the drying process creates appropriate pores between the raw material particles, facilitating the discharge of reducing gases generated by the decomposition of the carbon source during sintering.

[0195] In some embodiments, the compaction and granulation step specifically includes:

[0196] (1-1) mixing initial reactants including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, and an M source uniformly and then pre-sintering the mixture to obtain an initial product;

[0197] (1-2) mixing and grinding an intermediate reactant including an initial product, a carbon source, and a molding aid to obtain an intermediate product;

[0198] (2) compacting and granulating the intermediate product to obtain compacted granules,

[0199] Wherein, the mass content of the carbon source in the step (1-1) is 2%-5%, based on the total mass of the initial reactants.

[0200] In some embodiments, based on the total mass of the initial reactants, the mass content of the carbon source in step (1-1) can be any value among 2%, 3%, 4%, 5%, or a range between any two values.

[0201] A small amount of carbon source in the pre-sintering process can play a reducing role, allowing the initial reactants to be fully mixed and reacted, improving the uniformity and completeness of the reaction, and obtaining an initial product with excellent particle size uniformity. The pre-sintering treatment allows the ultrafine particles in the initial reactants to pre-react, reducing the content of small particles in the raw materials and improving the particle size uniformity of the material. At the same time, the intermediate reactant containing the initial product, carbon source and forming aid is further ground to refine large particles, reduce the content of oversized primary particles in the raw materials, and further improve the particle size uniformity of the material, providing a material basis for the subsequent preparation of positive electrode active materials with excellent particle size uniformity.

[0202] In summary, the pre-sintering treatment can improve the particle size uniformity of the initial reactants, so that the intermediate product undergoing compaction and granulation has excellent particle size uniformity, which helps to improve the uniformity of different components in the prepared positive electrode active material.

[0203] In some embodiments, the Dv50 of the intermediate product is 0.45 μm-1.25 μm, and the D V 10 is greater than or equal to 0.15μm.

[0204] In some embodiments, the Dv50 of the intermediate product can be any value selected from 0.45 μm, 0.55 μm, 0.65 μm, 0.75 μm, 0.85 μm, 0.95 μm, 1.05 μm, 1.15 μm, 1.25 μm, or a range between any two values.

[0205] In some embodiments, the D of the intermediate product V 10 can be selected as any one of greater than or equal to 0.15 μm, greater than or equal to 0.16 μm, greater than or equal to 0.17 μm, greater than or equal to 0.18 μm, greater than or equal to 0.19 μm, and greater than or equal to 0.20 μm.

[0206] Control the Dv50 and D V 10 Within an appropriate range, it is beneficial to control the mass content of small particles of the positive electrode active material, further improve the particle size uniformity of the positive electrode active material, improve the structural stability of the positive electrode active material, and improve the cycle performance of the battery.

[0207] The present application also provides a positive electrode active material prepared by the method.

[0208] The present application also provides the use of the positive electrode active material prepared by the method in a secondary battery.

[0209] Positive electrode

[0210] The positive electrode sheet of the present application includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector and comprising a positive electrode active material in any embodiment. For example, the positive electrode current collector has two surfaces that are opposed in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.

[0211] In the secondary battery of the present application, the positive electrode film layer generally comprises a positive electrode active material and an optional binder and an optional conductive agent. The positive electrode film layer is generally formed by coating the positive electrode slurry on the positive electrode current collector, drying, and cold pressing. The positive electrode slurry is generally formed by dispersing the positive electrode active material, the optional conductive agent, the optional binder, and any other components in a solvent and stirring them evenly. The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto. The type and content of the conductive agent and the binder are not specifically limited and can be selected according to actual needs. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0212] In the secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, the positive electrode current collector may be aluminum foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.

[0213] Preparation method of positive electrode sheet

[0214] The present application provides a method for preparing a positive electrode sheet, the preparation method specifically comprising:

[0215] Compacting and granulating: Compacting and granulating raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M source and molding aid to obtain compacted and molded particles;

[0216] Sintering: filling the compacted particles and sintering the compacted particles to obtain secondary particles;

[0217] Crushing: crushing the secondary particles to obtain positive electrode active materials;

[0218] Coating: coating the positive electrode slurry containing the positive electrode active material on at least one side of the current collector to form a positive electrode sheet,

[0219] The positive electrode active material includes a substrate and a carbon coating layer located on the surface of the substrate, and the substrate has a structural formula of Li z Fe x Mn(1-xy)M yPO4, wherein 0.5≤x≤1, 0≤y≤0.1, 1≤z≤1.1; M is selected from at least one of Ti, V, and Mg;

[0220] At least a portion of the positive electrode active material comprises primary particles, and the primary particles having a primary particle size of 80 nm or more and 180 nm or less account for less than or equal to 10% of the particle size distribution in the positive electrode active material;

[0221] The primary particles with a primary particle size of 1500nm or more are (250±5)μm in the cross section of the positive electrode sheet. 2 The number of particles in the area does not exceed 15.

[0222] The positive electrode plate obtained by the above preparation method has a positive electrode active material whose primary particle size is greater than 1500nm and whose primary particle size is greater than 80nm and less than 180nm, and the particle size distribution of the primary particles is controlled within an appropriate range, which can improve the cycle stability of the positive electrode active material, improve the cycle stability of the positive electrode plate, and improve the room temperature and high temperature cycle performance of the battery.

[0223] In some embodiments, the average particle size of the compacted granules in the compacting and granulating step is 3 mm to 30 mm. In some embodiments, the average particle size of the compacted granules in the compacting and granulating step can be any value selected from 3 mm, 5 mm, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, or a range between any two values.

[0224] Compacting the formed particles within a suitable range helps to improve the uniformity of different raw materials inside the particles. At the same time, the pores between the particles are conducive to removing the reducing gas generated by the decomposition of the carbon source during the preparation process, and the uniformity of carbon at different positions in the sintering device (such as the crucible) is improved.

[0225] In some embodiments, the compacted shaped particles have a compacted density of 1.0 g / cm 3 Above, or 1.2-3.0g / cm 3 .

[0226] In some embodiments, the compacted density of the compacted shaped particles may be 1.0 g / cm 3 , 1.2g / cm 3 , 1.4g / cm 3 , 1.6g / cm 3 , 1.8g / cm 3 , 2.0g / cm 3 , 2.2g / cm 3 , 2.4g / cm 3 , 2.6g / cm 3 , 2.8g / cm3 , 3.0g / cm 3 Any value in , or a range between any two values.

[0227] The compaction density of the compacted particles is controlled within a suitable range, which helps to increase the filling volume during the preparation process, thereby increasing the sintering capacity.

[0228] In some embodiments, the sintering step is specifically to fill the compacted particles to a filling height of 5 cm to 30 cm, and sinter the compacted particles to obtain secondary particles.

[0229] In some embodiments, the sintering step is specifically filling the compacted particles to a filling height of 8cm-30cm, 8cm-20cm, 5cm-25cm, 5cm-20cm, 10cm-30cm, 10cm-25cm or 10cm-20cm.

[0230] The filling height of the compacted particles during the sintering process is within an appropriate range, which helps to timely discharge the reducing gas generated by the decomposition of the carbon source during the sintering process, while accelerating heat transfer and avoiding uneven decomposition of the carbon source in the compacted particles at different positions in the sintering device, thereby improving the consistency of particle growth while taking into account production capacity.

[0231] In some embodiments, the pulverizing step is specifically to pulverize the secondary particles so that their Dv50 is 0.45 μm-1.5 μm; and pulverize the secondary particles so that their particle size distribution satisfies: (Dv90-Dv10) / Dv50≤3.

[0232] In some embodiments, the pulverizing step is specifically to pulverize the secondary particles so that their Dv50 can be any value among 0.45 μm, 0.5 μm, 0.7 μm, 0.9 μm, 1.0 μm, 1.2 μm, 1.4 μm, 1.5 μm, or a range between any two values.

[0233] In some embodiments, the secondary particles are crushed so that their particle size distribution satisfies any one of: (Dv90-Dv10) / Dv50≤3, (Dv90-Dv10) / Dv50≤2.5, (Dv90-Dv10) / Dv50≤2, and (Dv90-Dv10) / Dv50≤1.5.

[0234] Crushing the secondary particles to make their particle size distribution within the above range is helpful to improve the particle size uniformity and cycle stability of the positive electrode active material.

[0235] In some embodiments, the sintering temperature in the sintering step is 600° C.-800° C.; and / or the constant temperature sintering time in the sintering step is 2 h-12 h.

[0236] In some embodiments, the sintering temperature may be any value selected from 600° C., 650° C., 700° C., 750° C., 800° C., or a range between any two values.

[0237] In some embodiments, the sintering time may be any value selected from 2 h, 4 h, 6 h, 8 h, 10 h, 12 h, or a range between any two values.

[0238] The sintering temperature and / or sintering time are controlled within a suitable range so that the compacted particles are fully sintered, and thus the positive electrode active material has excellent structural parameters.

[0239] In some embodiments, the compaction and granulation step specifically includes:

[0240] (1) Grinding raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, M, a molding aid, and a solvent to obtain a slurry; and drying the slurry and then compacting and granulating it to obtain compacted molded particles.

[0241] First, the grinding process reduces the size of existing oversized primary particles, reducing their content in the raw materials and helping to reduce the size distribution of oversized primary particles in the prepared positive electrode active material. This also reduces the particle size of different raw materials, helping to obtain more uniform nanometer-scale primary particles. This also improves the uniformity of the mixing of different raw materials, contributing to the uniformity of different components in the prepared positive electrode active material. Furthermore, the drying process creates appropriate pores between the raw material particles, facilitating the discharge of reducing gases generated by the decomposition of the carbon source during sintering.

[0242] In some embodiments, the compaction and granulation step specifically includes:

[0243] (1-1) mixing initial reactants including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, and an M source uniformly and then pre-sintering the mixture to obtain an initial product;

[0244] (1-2) mixing and grinding an intermediate reactant including an initial product, a carbon source, and a molding aid to obtain an intermediate product;

[0245] (2) compacting and granulating the intermediate product to obtain compacted granules,

[0246] Wherein, the mass content of the carbon source in the step (1-1) is 2%-5%, based on the total mass of the initial reactants.

[0247] In some embodiments, based on the total mass of the initial reactants, the mass content of the carbon source in step (1-1) can be any value among 2%, 3%, 4%, 5%, or a range between any two values.

[0248] A small amount of carbon source in the pre-sintering process can play a reducing role, allowing the initial reactants to be fully mixed and reacted, improving the uniformity and completeness of the reaction, and obtaining an initial product with excellent particle size uniformity. The pre-sintering treatment allows the ultrafine particles in the initial reactants to pre-react, reducing the content of small particles in the raw materials and improving the particle size uniformity of the material. At the same time, the intermediate reactant containing the initial product, carbon source and forming aid is further ground to refine large particles, reduce the content of oversized primary particles in the raw materials, and further improve the particle size uniformity of the material, providing a material basis for the subsequent preparation of positive electrode active materials with excellent particle size uniformity.

[0249] In summary, the pre-sintering treatment can improve the particle size uniformity of the initial reactants, so that the intermediate product undergoing compaction and granulation has excellent particle size uniformity, which helps to improve the uniformity of different components in the prepared positive electrode active material.

[0250] In some embodiments, the Dv50 of the intermediate product is 0.45 μm-1.25 μm, and the D V 10 is greater than or equal to 0.15μm.

[0251] In some embodiments, the Dv50 of the intermediate product can be any value selected from 0.45 μm, 0.55 μm, 0.65 μm, 0.75 μm, 0.85 μm, 0.95 μm, 1.05 μm, 1.15 μm, 1.25 μm, or a range between any two values.

[0252] In some embodiments, the D of the intermediate product V 10 can be selected as any one of greater than or equal to 0.15 μm, greater than or equal to 0.16 μm, greater than or equal to 0.17 μm, greater than or equal to 0.18 μm, greater than or equal to 0.19 μm, and greater than or equal to 0.20 μm.

[0253] Control the Dv50 and D V 10 Within an appropriate range, it is beneficial to control the mass content of small particles of the positive electrode active material, further improve the particle size uniformity of the positive electrode active material, improve the structural stability of the positive electrode active material, and improve the cycle performance of the battery.

[0254] secondary batteries

[0255] The present application provides a secondary battery, which includes a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte in any embodiment.

[0256] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0257] In the secondary battery of the present application, the negative electrode film layer generally includes a negative electrode active material, an optional binder, an optional conductive agent, and other optional auxiliary agents.

[0258] In some embodiments, the negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, mesophase microcarbon beads, silicon-based materials, and tin-based materials.

[0259] The negative electrode film layer is usually formed by coating the negative electrode slurry on the negative electrode current collector, drying it, and cold pressing it. The negative electrode slurry is usually formed by dispersing the negative electrode active material, optional conductive agent, optional binder, and other optional additives in a solvent and stirring them evenly. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto. The type and content of the conductive agent and binder are not specifically limited and can be selected according to actual needs. As an example, the conductive agent may include one or more of superconducting carbon, carbon black (such as acetylene black, Ketjen black, etc.), carbon dots, carbon nanotubes, graphene, and carbon nanofibers. As an example, the binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (such as polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). Other optional additives may include thickeners (such as sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials, etc.

[0260] In the secondary battery of the present application, the negative electrode film layer may be disposed on one side of the negative electrode current collector, or may be disposed on both sides of the negative electrode current collector. For example, the negative electrode current collector has two opposite sides in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite sides of the negative electrode current collector.

[0261] In the secondary battery of the present application, the type of negative electrode current collector is not specifically limited and can be selected according to actual needs.

[0262] In the secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, the negative electrode current collector may be a copper foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0263] It should be noted that the negative electrode film parameters (e.g., thickness, compaction density, etc.) given in this application refer to the parameters of the negative electrode film layer on a single side of the negative electrode current collector. When the negative electrode film layer is provided on both sides of the negative electrode current collector, the parameters of the negative electrode film layer on either side that meet the requirements of this application are considered to fall within the scope of protection of this application. The ranges for negative electrode film thickness, compaction density, etc. described in this application refer to the parameters of the negative electrode film layer after cold pressing and used in battery assembly.

[0264] In addition, in the secondary battery of the present application, the negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) disposed between the negative electrode current collector and the negative electrode film layer. In other embodiments, the negative electrode plate described in the present application also includes a protective layer covering the surface of the negative electrode film layer.

[0265] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0266] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.

[0267] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0268] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0269] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0270] In the secondary battery of the present application, there is no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0271] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0272] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0273] The present application has no particular limitation on the shape of the battery, which can be cylindrical, square, or any other shape. For example, FIG6 shows a secondary battery 5 with a square structure as an example.

[0274] In some embodiments, referring to Figure 7, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0275] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0276] Figure 8 shows an example battery module 4. Referring to Figure 8 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0277] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0278] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0279] Figures 9 and 10 illustrate an example battery pack 1. Referring to Figures 9 and 10 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0280] Electrical devices

[0281] The present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0282] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0283] Figure 11 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0284] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0285] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

[0286] Example

[0287] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0288] 1. Preparation of batteries

[0289] Example 1

[0290] 1) Preparation of positive electrode active materials

[0291] Lithium carbonate, ferric oxide, ammonium dihydrogen phosphate, and titanium dioxide were weighed separately to achieve a Li:Fe:P ratio of 1.01:0.99:1.01 and a titanium dioxide:lithium carbonate ratio of 1:105. Water was added and mixed to form a slurry. Sucrose (8% by mass of the total solid raw materials) and starch (1% by mass of the total solid raw materials) were added to the slurry. The solids content of the slurry was 40%.

[0292] The mixed slurry was ground by a ball mill to a Dv50 of about 0.5 μm, and then spray-dried (the negative pressure of the high-speed spray dryer was -650 to -200 Pa, the inlet temperature was 300°C to 360°C, and the outlet temperature was 100°C to 140°C). The powder obtained by spray drying was compacted and granulated using a granulator, with an average particle size of about 10 mm and a compacted density of 1.2 to 1.5 g / cm 3The granulated reactants are loaded into a graphite crucible with a loading depth of 12 cm. The crucible filled with the reactants is placed in a kiln for sintering. The heating rate is controlled at 3°C / min, the holding temperature is controlled at 750°C, and the holding time is 6-8 hours. After the material is cooled, it is pulverized by a jet mill or a mechanical mill until the Dv50 is about 1.1 μm to obtain the positive electrode active material LiFe 0.995 Ti 0.005 PO4@C, where the Ti element content in the positive electrode active material is 1500ppm.

[0293] 2) Preparation of positive electrode sheet

[0294] 2.0 wt% polyvinylidene fluoride binder was fully dissolved in N-methylpyrrolidone (NMP), and then 1.0 wt% Super P, 0.5 wt% carbon nanotubes and 96.5 wt% of the above-mentioned positive electrode active material were added and stirred to obtain a positive electrode slurry. The slurry was evenly coated on the surface of the current collector aluminum foil and then transferred to a vacuum drying oven for complete drying. The dried electrode was rolled and punched to obtain a positive electrode sheet with a compaction density of 2.35 g / cm 3 .

[0295] 3) Preparation of negative electrode sheet

[0296] The active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in the solvent deionized water in a weight ratio of 96.7:1.3:0.8:1.2, and mixed evenly to prepare the negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.

[0297] 4) Electrolyte

[0298] In an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm), organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed uniformly in a volume ratio of 3:7, and LiPF6 lithium salt was dissolved in the organic solvent to prepare a solution with a mass content of 12.5% ​​to obtain an electrolyte.

[0299] 5) Isolation film

[0300] Polypropylene film is used as the isolation film.

[0301] 6) Preparation of batteries

[0302] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play an isolating role, and then wound to obtain an electrode assembly; the electrode assembly is placed in a battery case, and after drying, the electrolyte is injected, and then the process is sequentially carried out through the steps of standing, hot and cold pressing, formation, shaping, and capacity testing to obtain the lithium battery product of Example 1.

[0303] The preparation methods of Examples 2 to 10 are similar to those of Example 1, and the specific parameter adjustments are shown in Table 1.

[0304] The preparation method of Example 11 is similar to that of Example 1, except that magnesium hydroxide is used, and the mass ratio of magnesium hydroxide to lithium carbonate is 0.73:105.

[0305] The preparation method of Example 12 is similar to that of Example 1, except that vanadium pentoxide is used, and the mass ratio of vanadium pentoxide to lithium carbonate is 1.138:105.

[0306] The preparation method of Example 13 is similar to that of Example 1, but no doping elements are added to the raw materials. Specific parameters are shown in Table 1.

[0307] The preparation method of Example 14 is similar to that of Example 1, but the preparation process of the positive electrode active material is adjusted, as follows:

[0308] 1) Preparation of positive electrode active materials

[0309] Compaction granulation:

[0310] (1) Lithium carbonate, ferric oxide, ammonium dihydrogen phosphate and titanium dioxide were weighed separately, so that the mass ratio of Li:Fe:P elements was 1.01:0.99:1.01, and the mass ratio of titanium dioxide to lithium carbonate was 1:105. After adding water and mixing, a slurry was obtained, and sucrose with a mass fraction of 2% of all solid raw materials was added. The solid content in the slurry was 40%. The mixed slurry was ground in a ball mill until the Dv50 was about 0.5μm, and spray dried (the negative pressure of the high-speed spray dryer was -320Pa, the inlet temperature was 320℃, and the outlet temperature was 110℃). The dried material was loaded into a sagger and sintered in a kiln. The heating rate was controlled at 5℃ / min, the holding temperature was controlled at 750℃, and the holding time was 6 hours.

[0311] (2) After the material is cooled, it is pulverized by mechanical grinding. The pulverized material, sucrose and starch are mixed with water to obtain a slurry, wherein the mass fraction of sucrose is 6% and the mass fraction of starch is 2% based on the total mass of the solid matter of the slurry. The slurry obtained above is ground by a ball mill until the Dv50 of the slurry (i.e., the intermediate product in Table 1) is 0.5μm and the Dv10 is 0.12μm, and then spray dried (the negative pressure of the high-speed spray dryer is -320Pa, the inlet temperature is 320℃, and the outlet temperature is 110℃).

[0312] (3) The dried powder was compacted and granulated, with an average particle size of about 10 mm and a compacted density of 1.6 g / cm 3 .

[0313] Sintering: The granulated reactants are loaded into a graphite sagger to a depth of 12 cm. The sagger filled with the reactants is placed in a kiln for sintering. The heating rate is controlled at 3°C / min, the holding temperature is controlled at 750°C, and the holding time is 6 hours.

[0314] Crushing: After the material is cooled, it is crushed by air jet mill or mechanical mill until the Dv50 is 1μm to obtain the positive electrode active material LiFe 0.995 Ti 0.005 PO4@C, where the Ti element content in the positive electrode active material is 1500ppm.

[0315] The preparation methods of Examples 15 and 16 are similar to those of Example 14. For specific preparation parameters, please refer to Table 1.

[0316] Comparative Example 1

[0317] The preparation method of the battery of Comparative Example 1 is similar to that of the battery of Example 1, except that no compaction molding is performed and no molding additives are added, and the sintering reaction is directly performed after the spraying is completed.

[0318] Comparative Example 2

[0319] The preparation method of the battery of Comparative Example 2 is similar to that of the battery of Example 1, except that no compaction molding additive is added.

[0320] The preparation methods of Comparative Examples 3 to 6 are similar to those of Example 1, and the specific parameter adjustments are shown in Table 1.

[0321] The preparation method of the battery of Comparative Example 7 is similar to that of the battery of Example 1, but the preparation method of the active material is adjusted as follows:

[0322] A) Anhydrous ferric phosphate and lithium carbonate were weighed in a molar ratio of 1:0.5, and 0.2 wt% of titanium dioxide was mixed as an ion doping additive. Pure water was then added to form a slurry, which was then ball milled.

[0323] B) Transfer the ball-milled slurry into a sand mill for sand grinding to control the particle size of the sand-milled product. V 50 is 0.8μm.

[0324] C) adding 5 wt % glucose as an organic carbon source to the sand-milled slurry, maintaining the slurry temperature at 80° C. to 85° C. (specifically 80° C.), slowly stirring for 2 h, and spray drying to obtain a carbon-coated lithium iron phosphate precursor powder.

[0325] D) The precursor powder was transferred into a sintering furnace and heated from room temperature to 380°C at a heating rate of 10°C / min under a nitrogen atmosphere and held at that temperature for 4 hours. The precursor powder was then sintered at a heating rate of 10°C / min to 700°C for 10 hours, and then naturally cooled to obtain a sintered powder.

[0326] E) The sintered material is crushed by air jet mill to control the particle size D V 10 range is 0.41μm; D V 50 Particle size range is 1.08μm; D V The particle size range is 3.3 μm, and then it is sieved and iron is removed by electric current to obtain a carbon-coated lithium iron phosphate positive electrode active material (the mass percentage of carbon coated on the surface of the lithium iron phosphate material is 1.35%).

[0327] 2. Performance Testing

[0328] 1. Volume average particle size Dv10, D50, Dv90 test

[0329] Equipment model: Malvern 2000 (MasterSizer 2000) laser particle size analyzer, reference standard process: GB / T19077-2016 / ISO 13320:2009.

[0330] Specific test process: Take an appropriate amount of the sample to be tested (the sample concentration is sufficient to ensure 8-12% shading), add 20ml of deionized water, and ultrasonicate for 5 minutes (53KHz / 120W) to completely disperse the sample. Then, measure the sample according to GB / T19077-2016 / ISO 13320:2009 standard.

[0331] 2. Morphology test

[0332] The positive electrode active materials prepared in the examples and comparative examples were tested using a ZEISS sigma 300 scanning electron microscope, and the sample morphologies were observed with reference to the standard JY / T010-1996.

[0333] 3. Determination of primary particle size in positive electrode sheets

[0334] The electrode is cut open perpendicular to the electrode surface using an argon ion beam to expose the cross section, which is then photographed using a SEM.

[0335] Use equivalent circle area to calculate particle size

[0336] Taking FIG12 as an example, FIG12 shows an SEM image of a cross section of an electrode piece. The double arrows in the figure show the major diameters of the primary particles in the positive electrode piece, and the particle sizes of the primary particles are measured and counted.

[0337] The particle size in this patent is the area equivalent circle diameter, and the area of ​​each particle can be obtained by statistics using graphics software.

[0338] 4. Primary particles with a primary particle size of more than 100nm and less than 1500nm are (250±5)μm in the cross section of the positive electrode sheet. 2 Particle size distribution index within the region

[0339] The electrode was cut open perpendicularly to its large surface using an argon ion beam to expose the cross section, which was then photographed using a scanning electron microscope. The particle size of the active material was statistically analyzed using the equivalent circle area method, as shown in Figure 13.

[0340] The particle size distribution index (PDI) is the standard deviation of the particle size divided by the average particle size.

[0341] Where σ is the standard deviation of particle size, x i is the particle size value, x i is the average particle size, n is the total number of particles counted,

[0342] Average particle size The total particle size of primary particles with a primary particle size of 100 nm or more and 1500 nm or less divided by the number of primary particles with a primary particle size of 100 nm or more and 1500 nm or less,

[0343] Particle size x i The particle size of primary particles is between 100 nm and 1500 nm.

[0344] The total number of particles n is (250±5) μm in the cross section of the positive electrode sheet. 2The number of primary particles with a primary particle size of 100 nm or more and 1500 nm or less within the region.

[0345] 5. Battery performance test

[0346] 1) Capacity retention test at 25°C

[0347] The capacity retention test procedure is as follows: At 25°C, the prepared battery is charged at a constant current of 1C to 3.65V, then charged at a constant voltage of 3.65V until the current drops to 0.05C, and then discharged at 1C to 2.5V. The resulting capacity is recorded as the initial capacity (C0). The above steps are repeated for the same battery, and the discharge capacity of the battery after the nth cycle (Cn) is recorded at the same time. The battery capacity retention rate after each cycle is Pn = Cn / C0 × 100%. The capacity retention rate is measured after 1000 cycles under the above test conditions.

[0348] 2) Capacity retention test at 60°C

[0349] The capacity retention test process is as follows: at 60°C, the prepared battery is charged at a constant current of 1C to 3.65V, then charged at a constant voltage of 3.65V until the current drops to 0.05C, and then discharged at 1C to 2.5V. The resulting capacity is recorded as the initial capacity (C0). The above steps are repeated for the same battery, and the discharge capacity of the battery after the nth cycle (Cn) is recorded at the same time. The battery capacity retention rate after each cycle is Pn = Cn / C0 × 100%. The capacity retention rate after 1000 cycles is measured under the above test conditions.

[0350] 6. Determination of the content of doping elements Ti, V, and Mg

[0351] According to methods known in the art, a mixed acid of HF, HNO3 and HCl was prepared for sample dissolution so that titanium, vanadium and Mg in the positive electrode material were fully dissolved in the solution, and Ti, V and Mg elements were determined by inductively coupled plasma atomic emission spectroscopy.

[0352] 7. Evaluation of carbon distribution uniformity

[0353] Take the uncrushed material after sintering and cooling, and divide the material into three layers according to the height of the material filled in the graphite sagger. Take samples, and determine the carbon content with reference to the determination method of carbon content in GB / T 33822-2017 (infrared carbon-sulfur tester). Calculate the average carbon content of the materials in the upper, middle and lower layers, and calculate the range (i.e., the difference between the maximum and minimum values) based on the average carbon content of the materials in the upper, middle and lower layers.

[0354] The sintered, cooled and pulverized material was taken and the carbon content of the prepared positive electrode active material was determined by referring to the determination method of carbon content in GB / T 33822-2017 (infrared carbon-sulfur tester).

[0355] When the ratio of the extreme difference to the carbon content of the positive electrode active material does not exceed 10%, the uniformity of the carbon distribution is judged to be good; when the ratio of the two is greater than 10% and does not exceed 20%, the uniformity of the carbon distribution is judged to be good; when the ratio of the two is greater than 20% and does not exceed 30%, the uniformity of the carbon distribution is judged to be poor; when the ratio of the two is greater than 30%, the uniformity of the carbon distribution is judged to be poor.

[0356] 3. Analysis of test results of various embodiments and comparative examples

[0357] FIG2 shows an SEM image of the positive electrode active material prepared in Example 1. It can be seen that the primary particle size distribution of the positive electrode active material is very uniform, and the content of fine powder and large particles is low.

[0358] Figures 3A and 3B show scanning electron microscope photos of the argon ion beam cut section of the positive electrode sheet prepared in Example 1. It can be clearly observed that the uniform particle size distribution is very low. The content of micropowder and large particles in the positive electrode active material is extremely low. The number of nanoparticles with a diameter of less than 80nm accounts for less than 2%, and the number of particles with a diameter of more than 1500nm accounts for less than 250μm. 2 The quantity inside is 2 pieces.

[0359] FIG4A and FIG4B show scanning electron microscope photos of the cross section of the positive electrode sheet prepared in Comparative Example 1 cut by an argon ion beam, in which a large number of fine powders and oversized primary particles can be clearly observed.

[0360] FIG13 shows a scanning electron microscope photograph of a cross section of the positive electrode active material of Example 15 after being prepared into a positive electrode sheet by argon ion beam cutting. It can be clearly observed that the particle size of the primary particles has good uniformity.

[0361] Table 1 shows the parameters of the positive electrode active materials and batteries prepared in the examples and comparative examples. Table 2 shows the particle size Dv50 (μm), particle size distribution concentration (Dv90-Dv10) / Dv50, fine powder size distribution (% of fine powder with a particle size of 80-180 nm), number of large particles (250 μm) and the number of large particles (100 μm). 2 The number of primary particles with a diameter of 1500nm or more in the area), the particle size distribution index (the number of primary particles with a primary particle size of 100nm or more and 1500nm or less in the cross section of the positive electrode sheet within 250μm) 2 The results of the particle size distribution index within the region), carbon distribution uniformity evaluation results, and 1000-cycle capacity retention rate test results of secondary batteries at 25°C and 60°C were analyzed.

[0362] Table 1

[0363] Table 2

[0364] According to the above results, the particle size distribution of large particles and small particles in the positive electrode active materials of Examples 1 to 16 is reduced, and the uniformity of the charge and discharge reaction and the cycle performance of the positive electrode active materials are significantly improved.

[0365] FIG5 shows the cycle curves of Example 1 and Comparative Example 1 at 25° C. and 60° C. (two samples were measured in parallel). It can be seen that the cycle performance of the secondary battery prepared in Example 1 is significantly improved under normal temperature and high temperature conditions compared with the secondary battery prepared in Comparative Example 1.

[0366] The positive electrode sheet in Examples 1-16 includes a current collector and a positive electrode film layer located on at least one side of the current collector, the positive electrode film layer includes a positive electrode active material, the positive electrode active material includes a substrate and a carbon coating layer located on the surface of the substrate, at least a portion of the positive electrode active material includes primary particles, the primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material have a particle size distribution of less than or equal to 10%; and the primary particles with a primary particle size of 1500 nm or more are (250 ± 5) μm in the cross section of the positive electrode sheet. 2 The number of particles in the region does not exceed 15. Compared with Comparative Example 7, in Examples 1-16, compared with the positive electrode active material in the prior art, the particle size distribution of primary particles with a primary particle size of 80 nm or more and 180 nm or less is 35%, and the primary particles with a primary particle size of 1500 nm or more are (250 ± 5) μm in the cross section of the positive electrode sheet. 2 The number of particles in the area is 25. Compared with Comparative Example 7, the use of the positive electrode active material and positive electrode plate of the present application can improve the cycle capacity retention rate of the battery at room temperature and high temperature, and improve the room temperature and high temperature cycle performance of the battery. Compared with Comparative Examples 1-7, the use of the positive electrode active material and positive electrode plate of the present application can improve the room temperature cycle capacity retention rate and high temperature cycle capacity retention rate of the battery, and improve the room temperature and high temperature cycle performance of the battery.

[0367] From the comparison between Examples 1, 3, 4, 8, 9, 11-16 and Examples 2, 5-7, 10, it can be seen that the primary particles in the positive electrode active material with a primary particle size of more than 100 nm and less than 1500 nm are (250±5) μm in the cross section of the positive electrode sheet. 2The particle size distribution index in the region is less than or equal to 0.45, which can further improve the room temperature cycle performance and high temperature cycle performance of the battery. From the comparison of Examples 4, 15-16 with Examples 1-3, 5-14, it can be seen that the primary particles in the positive electrode active material with a primary particle size of more than 100nm and less than 1500nm are (250±5)μm in the cross section of the positive electrode sheet. 2 The particle size distribution index in the region is less than or equal to 0.36, which can further improve the normal temperature cycle capacity retention rate and high temperature cycle capacity retention rate of the battery.

[0368] Examples 1 to 3 adjusted the average particle size of the compacted granulation. Compared with Comparative Examples 3 to 4, the average particle size of the compacted granulation was within the range of 3-30 mm. The material had good air permeability during sintering, the particles were evenly heated, the carbon content was uniform, and the battery cycle performance was significantly improved. Both too small and too large an average particle size of the compacted granulation is detrimental to controlling the fine powder size distribution and the number of large particles.

[0369] In Examples 4 and 5, the height of the compacted particles during sintering was adjusted. The filling height was within the range of 5-30 cm. The material had good air permeability during sintering, the particles were heated evenly, the carbon was evenly distributed, the particle growth consistency was good, and the battery cycle performance was significantly improved. This was conducive to obtaining good production capacity.

[0370] Examples 6 to 8 adjusted the Dv50 value of the positive electrode active material after the pulverization treatment. Compared with Comparative Example 6, the Dv50 value is in the range of 0.45-1.5μm, and the particle size of the positive electrode active material is small, which contains at least some nano-scale primary particles, which is conducive to the release and embedding of active material lithium ions; at the same time, the (Dv90-Dv10) / Dv50 of the obtained positive electrode active material powder is less than 3, and the particle size distribution concentration is high. Both too small and too high Dv50 can lead to deterioration of cycle performance. If Dv50 is too small, the overall particle size is low, the proportion of small particles increases, and the surface stability of the material is reduced; if Dv50 is too large, the overall particle size is low, the proportion of large particles increases, and the particle crushing effect during the cycle increases, which is not conducive to improving the stability of the material.

[0371] The compaction density of the compaction granulation was adjusted in Example 9 and Example 10, and the compaction density was 1-2.5 g / cm 3 Compared with Comparative Examples 1 and 2, the compaction density is too low or no compaction molding process is performed, which is not conducive to the uniformity of particle size and carbon distribution.

[0372] Examples 11 to 13 adjust the reaction raw materials of the doping elements. It can be seen that the preparation method provided in this application can be applied to phosphate-based positive electrode active materials with different doping elements as well as those without doping elements. The doped phosphate-based positive electrode active material prepared using magnesium hydroxide and vanadium pentoxide has a particle size distribution and electrical properties similar to those of the doped phosphate-based positive electrode active material prepared using titanium dioxide. The phosphate-based positive electrode active material prepared in the examples without doping elements also has good particle size distribution and electrical properties.

[0373] Compared with Comparative Example 1, the positive electrode active materials prepared without compaction and granulation in Examples 1 to 13 exhibited low particle size distribution concentration and poor carbon content uniformity. Compared with Comparative Example 5, the addition of a molding aid to the raw materials helped improve the particle size distribution concentration and, due to improved chemical and mechanical properties, also contributed to improved battery cycling performance.

[0374] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A positive electrode sheet, characterized in that: The invention comprises a current collector and a positive electrode film layer located on at least one side of the current collector, wherein the positive electrode film layer comprises a positive electrode active material, wherein the positive electrode active material comprises a substrate and a carbon coating layer located on the surface of the substrate, wherein the substrate has a structural formula Li z Fe x Mn (1-x-y) M y PO4, wherein 1≤z≤1.1, 0.5≤x≤1, 0≤y≤0.1; M is selected from at least one of Ti, V, and Mg; At least a portion of the positive electrode active material includes primary particles, and the particle size distribution of the primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material is less than or equal to 10%; The primary particles with a primary particle size of 1500 nm or more are (250 ± 5) μm in the cross section of the positive electrode sheet. 2 The number of particles in the area does not exceed 15.

2. The positive electrode sheet according to claim 1, characterized in that: The particle size distribution of primary particles having a primary particle diameter of 80 nm or more and 180 nm or less in the positive electrode active material is 8.5% or less.

3. The positive electrode sheet according to claim 1 or 2, characterized in that: In the positive electrode active material, the primary particles with a primary particle size of 1500 nm or more are (250±5) μm in the cross section of the positive electrode sheet. 2 The number of particles in the area does not exceed 12.

4. The positive electrode sheet according to any one of claims 1 to 3, characterized in that: The primary particles with a primary particle size of 100 nm or more and 1500 nm or less are (250±5) μm in the cross section of the positive electrode sheet. 2 The particle size distribution index in the region is less than or equal to 0.45, and can be less than or equal to 0.

36. The particle size distribution index refers to the ratio of the standard deviation of the primary particle sizes of the primary particles divided by the average primary particle size.

5. The positive electrode sheet according to any one of claims 1 to 4, characterized in that: The positive electrode active material includes secondary particles, and the particle size distribution of the secondary particles satisfies: (Dv90-Dv10) / Dv50≤3.

6. The positive electrode sheet according to claim 5, characterized in that: The Dv50 of the secondary particles is 0.45-1.5 μm.

7. The positive electrode sheet according to any one of claims 1 to 6, characterized in that: 0.6 <x≤1,0≤y<0.1,1≤z≤1.1; The mass content of the M element in the positive electrode active material is 1000ppm-6000ppm.

8. A method for preparing a positive electrode sheet, characterized in that: The preparation method specifically comprises: Compacting and granulating: Compacting and granulating raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M source and molding aid to obtain compacted and molded particles; Sintering: filling the compacted particles, and sintering the compacted particles to obtain secondary particles; Crushing: crushing the secondary particles to obtain positive electrode active materials; Coating: coating a positive electrode slurry containing the positive electrode active material on at least one side of the current collector to form a positive electrode sheet, The positive electrode active material includes a substrate and a carbon coating layer located on the surface of the substrate, and the substrate has a structural formula of Li z Fe x Mn (1-x-y) M y PO4, wherein 0.5≤x≤1, 0≤y≤0.1, 1≤z≤1.1; M is selected from at least one of Ti, V, and Mg; At least a portion of the positive electrode active material includes primary particles, and the particle size distribution of the primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material is less than or equal to 10%; The primary particles with a primary particle size of 1500 nm or more are (250 ± 5) μm in the cross section of the positive electrode sheet. 2 The number of particles in the area does not exceed 15.

9. The preparation method according to claim 8, characterized in that: The average particle size of the compacted particles in the compacting and granulating step is 3 mm to 30 mm.

10. The preparation method according to claim 8 or 9, characterized in that: The compacted density of the compacted particles is 1.0 g / cm 3 Above, or 1.2-3.0g / cm 3 .

11. The preparation method according to any one of claims 8 to 10, characterized in that: The sintering step specifically includes filling the compacted particles to a filling height of 5 cm to 30 cm, and sintering the compacted particles to obtain secondary particles.

12. The preparation method according to any one of claims 8 to 11, characterized in that: The pulverizing step specifically comprises pulverizing the secondary particles so that their Dv50 is 0.45 μm-1.5 μm; The secondary particles are crushed so that their particle size distribution satisfies: (Dv90-Dv10) / Dv50≤3.

13. The preparation method according to any one of claims 8 to 12, characterized in that: The sintering temperature in the sintering step is 600° C.-800° C.; and / or the constant temperature sintering time in the sintering step is 2 h-12 h.

14. The preparation method according to any one of claims 8 to 13, characterized in that: The compaction granulation step specifically comprises: The raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M, molding aid and solvent are ground to obtain slurry; the slurry is dried and then compacted and granulated to obtain compacted and molded particles.

15. The preparation method according to any one of claims 8 to 13, characterized in that: The compaction granulation step specifically comprises: (1-1) mixing initial reactants including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, and an M source uniformly and then pre-sintering the mixture to obtain an initial product; (1-2) mixing and grinding the intermediate reactants including the initial product, the carbon source and the molding aid to obtain an intermediate product; (2) compacting and granulating the intermediate product to obtain compacted granules, Wherein, the mass content of the carbon source in the step (1-1) is 2%-5%, based on the total mass of the initial reactants.

16. The preparation method according to claim 15, characterized in that: The Dv50 of the intermediate product is 0.45 μm-1.25 μm, and the D V 10 is greater than or equal to 0.15μm.

17. A secondary battery, characterized in that: The invention comprises a negative electrode sheet, a separator, an electrolyte and a positive electrode sheet according to any one of claims 1 to 7 or a positive electrode sheet prepared by the preparation method according to any one of claims 8 to 16.

18. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 17.

Citation Information

Patent Citations

  • Positive electrode active materials and their preparation methods, positive electrode sheets, secondary batteries and electrical devices

    CN116259736B

  • Method for industrially producing lithium-iron-phosphate positive pole material

    CN102881902A

  • Secondary battery and preparation method thereof

    CN115513515A

  • Positive electrode active material and preparation method thereof, positive electrode plate, secondary battery and electric device

    CN116259736A

  • Data acquisition system for golf game using earphone case

    KR1020220107098A

Cited By

  • A lithium iron phosphate kiln external conveying production line

    CN119755983A

  • Composite positive electrode material and preparation method thereof, positive plate and secondary battery

    CN119833595A

  • Lithium ion secondary battery, battery device, power utilization device, preparation method of positive active material and preparation method of positive pole piece

    CN120072865A

  • Secondary battery and electric device

    CN121394518A

  • Positive electrode sheets, batteries, energy storage devices, and power consumption devices