Cyano functionalized organosiloxane compound, and preparation and use thereof

By using cyano-functionalized organosiloxane compounds as electrolyte additives in lithium-ion batteries, the insufficient performance of existing electrolytes in high energy density and high temperature cycling storage is solved, and the cycle life and safety of the battery is significantly improved. sex.

WO2024235358A1PCT designated stage expired Publication Date: 2024-11-21GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI

Patent Information

Application Number
PCT/CN2024/105690
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-17
Filing Date
2024-07-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing commercial carbonate electrolytes and electrolyte additives cannot fully meet the needs of electrochemical performance such as high-energy-density batteries, especially high-voltage applications and high-temperature cyclic storage, and cannot effectively improve the cycle life and safety of lithium-ion batteries.

Method used

Using cyano-functionalized organosiloxane compounds as electrolyte high-voltage/high-temperature additives or solvents for lithium-ion batteries or other electrochemical energy storage devices, the electrolytics that improve the electrode interface performance and compatibility are formed by combining with lithium salts and solvents. liquid, including specific chemical structures and preparation methods.

Benefits of technology

The cyano-functionalized organosiloxane compound forms a dense and stable protective film at the electrode interface, which improves the battery's high-temperature/high-pressure cycle life, discharge capacity and rate performance, reduces the flammability of the electrolyte, and enhances the battery's safety and Electrochemical properties such as high temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024105690_21112024_PF_FP_ABST
    Figure CN2024105690_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A cyano functionalized organosiloxane compound having a chemical structural formula as shown in formula 1-4. The compound is used as an electrolyte high-pressure / high-temperature additive or solvent of a lithium-ion battery or other electrochemical energy storage devices. A dense and stable protective film containing nitrogen and silicon is formed on the electrode interface, such that the interface performance and compatibility between the positive and negative electrodes and the electrolyte are improved, oxidative decomposition of the electrolyte is effectively inhibited, and electrochemical properties such as the cycle life, the discharge capacity and multiplier of the battery at high-temperature / high-pressure are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Cyano-functionalized organosiloxane compounds and their preparation and application Technical field:

[0001] The present invention relates to the technical field of electrochemical energy storage, and in particular to a cyano-functionalized organosiloxane compound and its preparation and application. Background technology:

[0002] Lithium-ion batteries are widely used in consumer electronics such as mobile phones and laptops due to their high specific energy, low self-discharge, lack of memory effect, and long cycle life. As lithium batteries are gradually being used in emerging industries such as electric vehicles and energy storage, their electrochemical and safety properties, including energy density and cycle life, currently cannot meet the technological requirements of these emerging industries. Cathode materials such as high-nickel ternary materials, lithium-manganese-rich materials, and high-voltage lithium cobalt oxide have high specific capacities and are increasingly common in high-energy-density power batteries and energy storage batteries. Research and development of high-energy-density lithium metal batteries is also booming and holds promise for practical application. However, existing commercial carbonate electrolytes and electrolyte additives cannot fully meet the practical application requirements of these high-energy-density batteries, especially in high-voltage applications and electrochemical properties such as high-temperature cycling and storage.

[0003] Therefore, researching and developing new electrolyte materials to meet and improve the application of electrochemical energy storage devices such as lithium-ion batteries is a long-term and urgent technical need.

[0004] Summary of the invention:

[0005] The purpose of the present invention is to provide a cyano-functionalized organosiloxane compound and its preparation and application.

[0006] The present invention is achieved through the following technical solutions:

[0007] The chemical structure is a cyano-functionalized organosiloxane compound represented by Formula 1, Formula 2, or Formula 3, or a cyano-functionalized organosiloxane isomer represented by Formula 4 or Formula 5:

[0008] wherein R1 is selected from a C1-C5 alkyl group; n1 is an integer from 0 to 5; n2 is an integer from 1 to 5, X is selected from a C2-C5 straight-chain alkylene group, Y is selected from a C2-C5 straight-chain alkylene group or a C2-C5 branched-chain alkylene group or -NR2CH2CH2CN, wherein R2 is a C2-C5 straight-chain or C2-C5 branched-chain alkylene group.

[0009] The preparation method of the cyano-functionalized organosiloxane compound comprises the following steps: under the protection of an inert gas, a double-bond imine nitrile or a double-bond nitrile compound is subjected to a hydrosilylation reaction with an alkoxysilane under platinum metal catalysis, the reaction temperature being 30-130° C. and the reaction time being 4-24 hours; the molar ratio of the double-bond imine nitrile or the double-bond nitrile compound to the alkoxysilane is 1:1.0-2.2; the alkoxysilane is any one of pentamethyldisiloxane, 1,1,3,3,5,5,5-heptamethyltrisiloxane or 1,1,1,3,5,5,5-heptamethyltrisiloxane; and the hydrosilylation reaction catalyst is selected from chloroplatinic acid or Karstedt's catalyst, and the amount added is 0.1-1 times the amount of the double-bond imine nitrile or the double-bond nitrile compound.

[0010] When R1 is selected from methyl, the specific synthetic route includes the following route:

[0011] The present invention also provides the use of a cyano-functionalized organosiloxane compound represented by Formula 1, Formula 2, or Formula 3, or a cyano-functionalized organosiloxane isomer represented by Formula 4 and Formula 5, in lithium-ion batteries or other electrochemical energy storage devices (such as sodium-ion batteries, potassium-ion batteries, lithium-sulfur batteries, supercapacitors, etc.). The cyano-functionalized organosiloxane compound or the cyano-functionalized organosiloxane isomer represented by Formula 4 and Formula 5 is used as a high-pressure or high-temperature additive or solvent for the electrolyte of a lithium-ion battery or other electrochemical energy storage device.

[0012] The lithium-ion battery electrolyte includes a lithium salt, a solvent, and the cyano-functionalized organosiloxane compound of the present invention or the cyano-functionalized organosiloxane isomers shown by Formula 4 and Formula 5 as an electrolyte additive. The concentration of the lithium salt in the electrolyte is 0.5-1.5 mol / L, and the amount of the cyano-functionalized organosiloxane compound or the cyano-functionalized organosiloxane isomers shown by Formula 4 and Formula 5 used is 0.1%-5% of the total mass of the lithium salt and the solvent. The solvent includes two or more of ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. The lithium salt is selected from one or more of lithium hexafluorophosphate (LiPF6), lithium dioxalatoborate (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium perchlorate (LiClO4), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI), and lithium bis(fluorosulfonyl imide) (LiFSI). The positive electrode material of the lithium-ion battery can use LiNi x Co y Mn z O2 (x+y+z=1, x≥0.6), lithium cobalt oxide (LCO), nickel cobalt aluminum and lithium manganese oxide (LMO) positive electrode material system; the lithium ion battery negative electrode material uses one of metallic lithium, graphite, lithium titanate or silicon-based system.

[0013] The present invention also protects a lithium-ion battery, comprising a positive electrode sheet containing a positive electrode active material, a negative electrode sheet containing a negative electrode active material, a lithium battery separator and a lithium-ion battery electrolyte, wherein the lithium-ion battery electrolyte comprises a lithium salt, a solvent and the cyano-functionalized organosiloxane compound or the cyano-functionalized organosiloxane isomers represented by Formula 4 and Formula 5.

[0014] The positive electrode material of lithium-ion batteries is LiNi x Co y Mn z O2 (x, y, z refer to the molar ratios of nickel, cobalt, and manganese, respectively, x+y+z=1, x≥0.6), any one of lithium cobalt oxide, nickel cobalt aluminum, and lithium manganese oxide; the negative electrode material of the lithium-ion battery is one of metallic lithium, graphite, lithium titanate, or a silicon-based system.

[0015] The beneficial effects of the present invention are as follows:

[0016] 1) The cyano-containing organosiloxane compound or the cyano-functionalized organosiloxane isomers represented by Formula 4 and Formula 5 can be used as a high-voltage / high-temperature additive for the electrolyte of lithium-ion batteries or other electrochemical energy storage devices (such as sodium-ion batteries, potassium-ion batteries, lithium-sulfur batteries, supercapacitors, etc.). It can decompose preferentially over the carbonate electrolyte, forming a dense and stable protective film containing nitrogen and silicon elements at the electrode interface, improving the interface performance and compatibility between the positive and negative electrodes and the electrolyte, effectively inhibiting the oxidative decomposition of the electrolyte, and improving the electrochemical properties of the battery such as the high-temperature / high-voltage cycle life, discharge capacity and rate.

[0017] 2) Cyano-containing organosiloxane compounds have a wide electrochemical window and can be used as electrolyte solvents and applied to high-energy lithium batteries. Their polyorganosiloxanes help reduce the flammability of the electrolyte and improve battery safety. The wide electrochemical window can be applied to high-voltage batteries. The highly polar cyano and siloxane groups help improve the compatibility between the electrolyte and the electrode and improve the high-temperature and other electrochemical properties of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] FIG1 is a hydrogen nuclear magnetic resonance spectrum of the compound of Example 1 of the present invention;

[0019] FIG2 is a carbon NMR spectrum of the compound of Example 1 of the present invention;

[0020] FIG3 is a silicon nuclear magnetic resonance spectrum of the compound of Example 1 of the present invention;

[0021] FIG4 is a hydrogen nuclear magnetic resonance spectrum of the compound of Example 2 of the present invention;

[0022] FIG5 is a carbon NMR spectrum of the compound of Example 2 of the present invention;

[0023] FIG6 is a hydrogen nuclear magnetic resonance spectrum of the compound of Example 2 of the present invention;

[0024] FIG7 is a hydrogen nuclear magnetic resonance spectrum of the compound of Example 3 of the present invention;

[0025] FIG8 is a carbon NMR spectrum of the compound of Example 3 of the present invention;

[0026] FIG9 is a silicon nuclear magnetic resonance spectrum of the compound of Example 3 of the present invention;

[0027] FIG10 is a hydrogen nuclear magnetic resonance spectrum of the compound of Example 4 of the present invention;

[0028] FIG11 is a carbon NMR spectrum of the compound of Example 4 of the present invention;

[0029] FIG12 is a silicon NMR spectrum of the compound of Example 4 of the present invention;

[0030] FIG13 is a hydrogen nuclear magnetic resonance spectrum of the compound of Example 5 of the present invention;

[0031] FIG14 is a carbon NMR spectrum of the compound of Example 5 of the present invention;

[0032] FIG15 is a silicon NMR spectrum of the compound of Example 5 of the present invention;

[0033] FIG16 is a hydrogen nuclear magnetic resonance spectrum of the compound of Example 6 of the present invention;

[0034] FIG17 is a carbon NMR spectrum of the compound of Example 6 of the present invention;

[0035] FIG18 is a silicon NMR spectrum of the compound of Example 6 of the present invention;

[0036] FIG19 is a hydrogen nuclear magnetic resonance spectrum of the cyano-functionalized organosiloxane isomers obtained in Example 7 of the present invention;

[0037] FIG20 is a carbon NMR spectrum of the cyano-functionalized organosiloxane isomers obtained in Example 7 of the present invention;

[0038] FIG21 is a silicon NMR spectrum of cyano-functionalized organosiloxane isomers obtained in Example 7 of the present invention;

[0039] FIG22 is a linear scanning curve of the compound of Example 1 of the present invention;

[0040] FIG23 is a linear scanning curve of the compound of Example 2 of the present invention;

[0041] FIG24 is a linear scanning curve of the compound of Example 3 of the present invention;

[0042] FIG25 is a linear scanning curve of the compound of Example 4 of the present invention;

[0043] FIG26 is a linear scanning curve of the compound of Example 5 of the present invention;

[0044] FIG27 is a linear scanning curve of the compound of Example 6 of the present invention;

[0045] FIG28 shows the room temperature cycling performance test of the electrolytes of Example 8, Example 11 and Comparative Example 1 on an NCM811 / Li battery at 4.3V;

[0046] FIG29 is a rate performance test of NCM811 / Li batteries using the electrolytes of Example 8 of the present invention and Comparative Example 1;

[0047] FIG30 is a rate performance test of LMO / Li batteries using the electrolytes of Example 8 of the present invention and Comparative Example 1;

[0048] FIG31 shows the high-temperature cycle performance test of LMO / Li batteries using the electrolytes of Example 8 of the present invention and Comparative Example 1;

[0049] FIG32 shows the room temperature cycling performance test of LMO / Li batteries using the electrolytes of Example 8 of the present invention and Comparative Example 1;

[0050] FIG33 shows the high temperature cycle performance of the Graphite / LCO battery using the electrolytes of Example 8 of the present invention and Comparative Example 1;

[0051] FIG34 shows the impedance test of the Graphite / LCO battery using the electrolytes of Example 8 of the present invention and Comparative Example 1;

[0052] FIG35 shows the cycling performance test of NCM811 / Li batteries using the electrolytes of Example 10 of the present invention and Comparative Example 1 at 4.5V and 55°C;

[0053] FIG36 shows the impedance test of LTO / Li batteries using the electrolytes of Example 9, Example 10, and Comparative Example 1 of the present invention;

[0054] FIG37 shows cycle tests of LMO / LTO soft-pack batteries using the electrolytes of Example 10 of the present invention and Comparative Example 1;

[0055] FIG35 shows the room temperature cycling performance test of NCM811 / Li batteries using the electrolytes of Example 10 of the present invention and Comparative Example 1;

[0056] FIG38 is a high-temperature storage capacity retention test of NCM622 / AG batteries using the electrolytes of Example 11 of the present invention and Comparative Example 2;

[0057] FIG39 shows a high-temperature storage gas generation test of NCM622 / AG batteries using the electrolytes of Example 11 of the present invention and Comparative Example 2;

[0058] FIG40 is an impedance test of the NCM811 / Li battery using the electrolytes of Example 12, Example 13 and Comparative Example 1 of the present invention.

[0059] Figure 41 is a room temperature cycle performance test of the NCM811 / Li battery of the electrolyte of Example 14 of the present invention and Comparative Example 1 at 4.5V. Specific implementation method:

[0060] The following is a further description of the present invention, but not a limitation of the present invention.

[0061] Example 1: Synthesis of cyano-functionalized organodisiloxane compound (TMSPAN)

[0062] Under an Ar atmosphere, a 25 mL two-necked flask was charged with 1,1,1,3,3-pentamethyldisiloxane (95.64 g, 0.646 mol), 3,3'-(allylnitrodiyl)dipropionitrile (70.23 g, 0.431 mol), and a catalytic amount of chloroplatinic acid. The reaction was allowed to proceed at 100°C for 5 h before terminating. After vacuum distillation (bp: 175°C, 2.5 mmHg), 110 g of a cyano-functionalized organodisiloxane compound (TMSPAN) was obtained.

[0063] TMSPAN: 1 H-NMR (400MHz, CDCl3) δ2.87(t,J=6.8Hz,4H),2.52(t,J=7.4Hz,2H),2.46(t, J=6.8Hz,4H),1.50-1.40(m,2H),0.53-0.44(m,2H),0.07(m,9H),0.06(s,6H); 13 C-NMR (100MHz, CDCl3) δ118.5,56.7,49.7,21.2,17.0,15.5,1.9,0.3. 29 Si-NMR (100MHz, CDCl3): δ7.3, 7.1. 1 H-NMR, 13 C-NMR and 29 Si-NMR spectra are shown in Figures 1 to 3.

[0064] Example 2: Synthesis of a cyano-functionalized organotrisiloxane compound (HMSPAN1)

[0065] Under Ar atmosphere, 1,1,1,3,5,5,5-heptamethyltrisiloxane (5 g, 22.51 mmol), compound 3,3'-(allyl nitrogen diyl)dipropionitrile (3.5 g, 21.44 mmol) and a catalytic amount of chloroplatinic acid were added in sequence to a 25 mL two-necked flask. The mixture was refluxed at 120 ° C for 15 h and HMSPAN1 was obtained by distillation under reduced pressure (bp: 178 ° C, 2 mmHg).

[0066] HMSPAN1: 1 H-NMR (400MHz, CDCl3): δ2.87(t,J=6.8Hz,4H),2.54-2.43(m,6H),1.50-1.38(m,2H),0.49-0.38(m,2H),0.09(s,18H),0.02(s,3H). 13 C-NMR (100MHz, CDCl3): δ118.5,56.4,49.6,20.8,16.9,14.6,1.7,0.4. 29 Si-NMR (100MHz,CDCl3):δ7.5,-22.0. 1 H-NMR, 13 C-NMR and 29 Si-NMR spectra are shown in Figures 4 to 6.

[0067] Example 3: Synthesis of a cyano-functionalized organotrisiloxane compound (HMSPAN2)

[0068] Under Ar atmosphere, 1,1,1,3,3,5,5-heptamethyltrisiloxane (45.8 g, 0.206 mol), compound 3,3'-(allyl nitrogen diyl) dipropionitrile (2 g, 0.196 mol) and a catalytic amount of Karstedt's reagent were added sequentially into a 100 mL two-necked flask. The reaction was carried out at 80°C for 5 h, and HMSPAN2 was obtained by distillation under reduced pressure (bp: 184°C, 1.05 mmHg).

[0069] HMSPAN2: 1 H-NMR (400MHz, CDCl3): δ2.86(t,J=6.8Hz,4H),2.52(t,J=7.2Hz,2H),2.46(t, J=6.8Hz,4H),1.51-1.42(m,2H),0.54-0.48(m,2H),0.08(s,15H),0.02(s,6H). 13 C-NMR (100MHz, CDCl3): δ118.5,56.8,49.7,21.1,17.0,15.4,1.8,1.2,0.2.29 Si-NMR (79.5MHz,CDCl3):δ7.2,7.1,-20.8. 1 H-NMR, 13 C-NMR and 29 Si-NMR spectra are shown in Figures 7 to 9.

[0070] Example 4: Synthesis of cyano-functionalized organosiloxane compound (MTSMCN)

[0071] Under Ar atmosphere, 1,1,1,3,5,5,5-heptamethyltrisiloxane (50.0 g, 0.225 mol) and 2-methyl-3-butenenitrile (19.2 g, 0.363 mol) were added in sequence into a 100 mL two-necked flask, followed by a certain amount of chloroplatinic acid. The mixture was reacted at 90 ° C for 24 h and distilled under reduced pressure to obtain the product (bp: 90 ° C, 1.35 mmHg).

[0072] MTSMCN: 1 H-NMR (400MHz, CDCl3): δ2.58-2.46(m,1H),1.58-1.50(m,2H),1.24(d,J=6.8Hz,3H),0.66-0.49(m,2H),0.05(s,18H),0.02(s,3H). 13 C-NMR (100MHz, CDCl3): δ122.7,28.1,28.0,17.4,14.7,1.6,0.6. 29 Si-NMR (100MHz,CDCl3):δ7.9,-23.3. 1 H-NMR, 13 C-NMR and 29 Si-NMR spectra are shown in Figures 10 to 12.

[0073] Example 5: Synthesis of Cyano-functionalized Organosiloxane Compound (TSMCN)

[0074] Under Ar atmosphere, 1,1,1,3,3,5,5-heptamethyltrisiloxane (50.0 g, 0.225 mol) and 2-methyl-3-butenenitrile (19.2 g, 0.363 mol) were added in sequence into a 100 mL two-necked flask, followed by a certain amount of chloroplatinic acid. The mixture was reacted at 90 ° C for 24 h and distilled under reduced pressure to obtain the product (bp: 90 ° C, 1.35 mmHg).

[0075] TSMCN: 1H-NMR (400MHz, CDCl3): δ2.63-2.52(m,1H),1.69-1.58(m,2H),1.31(d,J=7.2Hz,3H),0.82-0.59(m,2H),0.10(s,6H),0.09(s,9H),0.03(s,6H). 13 C-NMR (100MHz, CDCl3): δ122.9,28.5,28.2,17.5,15.6,1.7,1.1,0.1. 29 Si-NMR (100MHz,CDCl3):δ7.3,6.6,-20.6. 1 H-NMR, 13 C-NMR and 29 Si-NMR spectra are shown in Figures 13 to 15.

[0076] Example 6: Synthesis of a cyano-functionalized organosiloxane compound (BPDSPAN)

[0077] Under Ar atmosphere, 1,1,1,3,3-pentamethyldisiloxane (3.36 g, 22 mmol) and 3-(diallylamino)propionitrile (6.98 g, 47 mmol) were added in sequence into a 100 mL two-necked flask, and a certain amount of Karstedt's reagent was added. The reaction was carried out at 50°C for 24 h, and the product was distilled under reduced pressure (bp: 153°C, 0.90 mmHg).

[0078] BPDSPAN: 1 H-NMR (400MHz, CDCl3): δ2.79 (t, J = 7.2Hz, 2H), 2.45-2.36 (m, 6H), 1.47-1.38 (m, 4H), 0.50-0.43 (m, 4H), 0.05 (s, 18H), 0.03 (s, 12H). 13 C-NMR (100MHz, CDCl3): δ118.9,57.2,49.8,21.1,16.1,15.7,1.9,0.3. 29 Si-NMR (100MHz,CDCl3):δ7.4,7.3. 1 H-NMR, 13 C-NMR and 29 Si-NMR spectra are shown in Figures 16 to 18.

[0079] Example 7: Synthesis of Cyano-functionalized Organosiloxane Isomers (TSTCN)

[0080] Under Ar atmosphere, 1,1,1,3,5,5,5-heptamethyltrisiloxane (54.83 g, 0.246 mol) and butenenitrile (16.53 g, 0.246 mol) were added in sequence into a 100 mL two-necked flask, followed by a certain amount of chloroplatinic acid. The mixture was reacted at 90°C for 24 h, and then distilled under reduced pressure to obtain cyano-functionalized organosiloxane isomers, designated as TSTCN (bp: 82°C, 1.35 mmHg), consisting of TSTCN1 and TSTCN2; the ratio of TSTCN1 to TSTCN2 was 1:3.6.

[0081] TSTCN1: 1 H-NMR (400MHz, CDCl3): δ2.45 (dd, J=16.8, 4.4Hz, 1H), 2.11 (dd, J=16.8, 10.4 Hz,1H),1.10(d,J=7.6Hz,1H),0.98-0.88(m,1H),0.11(s,18H),0.06(s,3H). 13 C-NMR (100MHz, CDCl3) δ120.0,19.5,18.5,13.7,1.78,-2.4. 29 SiNMR (79.49MHz, CDCl3) δ8.6, 8.5, 24.9.

[0082] TSTCN2: 1 H-NMR (400MHz, CDCl3): δ2.35 (t, J=6.8Hz, 2H), 1.73-1.64 (m, 2H), 0.65-0.57 (m, 2H), 0.10 (s, 18H), -0.03 (s, 3H). 13 C-NMR (100MHz, CDCl3) δ119.8,20.3,19.9,17.0,1.80,-0.3. 29 Si-NMR (79.49MHz, CDCl3) δ7.6,-23.6.

[0083] NMR 1 H-NMR, 13 C-NMR and 29 Si-NMR spectra are shown in Figures 19 to 21.

[0084] Example 8:

[0085] The required basic electrolyte LB301 = 1M LiPF6 ethylene carbonate (EC) / dimethyl carbonate (DMC) / ethyl methyl carbonate (EMC) (1:1:1) is from Shanghai Xiaoyuan Energy Technology Co., Ltd., and 0.2 wt.% of the additive TMSPAN synthesized in Example 1 is added to the electrolyte, stirred evenly and set aside.

[0086] Example 9:

[0087] The required basic electrolyte LB301 = 1M LiPF6 EC / DMC / EMC (1:1:1) was obtained from Shanghai Xiaoyuan Energy Technology Co., Ltd. 0.5 wt.% of the additive HMSPAN1 synthesized in Example 2 was added to the electrolyte, stirred evenly and set aside.

[0088] Example 10:

[0089] The required basic electrolyte LB301 = 1M LiPF6 EC / DMC / EMC (1:1:1) was obtained from Shanghai Xiaoyuan Energy Technology Co., Ltd. 0.5 wt.% of the additive HMSPAN2 synthesized in Example 3 was added to the electrolyte, stirred evenly and set aside.

[0090] Example 11:

[0091] The required basic electrolyte LB301 = 1M LiPF6 EC / DMC / EMC (1:1:1) was obtained from Shanghai Xiaoyuan Energy Technology Co., Ltd. 2 wt.% of the additive MTSMCN synthesized in Example 4 was added to the electrolyte and stirred for use.

[0092] Example 12:

[0093] The required basic electrolyte LB301 = 1M LiPF6 EC / DMC / EMC (1:1:1) was obtained from Shanghai Xiaoyuan Energy Technology Co., Ltd. 2 wt.% of the additive TSMCN synthesized in Example 5 was added to the electrolyte and stirred for use.

[0094] Example 13:

[0095] The required basic electrolyte LB301 = 1M LiPF6 EC / DMC / EMC (1:1:1) was obtained from Shanghai Xiaoyuan Energy Technology Co., Ltd. 0.5 wt.% of the additive BPDSPAN synthesized in Example 6 was added to the electrolyte and stirred evenly for later use.

[0096] Example 14:

[0097] The required basic electrolyte LB301 = 1M LiPF6 EC / DMC / EMC (1:1:1) was obtained from Shanghai Xiaoyuan Energy Technology Co., Ltd. 0.5 wt.% of the additive TSTCN synthesized in Example 7 was added to the electrolyte and stirred evenly for later use.

[0098] Comparative Example 1:

[0099] Basic electrolyte LB301 = 1M LiPF6 EC / DMC / EMC (1:1:1), and no other additives are added to this basic electrolyte.

[0100] Comparative Example 2:

[0101] Commercial carbonate electrolyte.

[0102] Example 15: Electrode Preparation

[0103] The positive electrode material, conductive agent, binder, and solvent are mixed in a certain proportion, coated on aluminum foil, and dried to produce a positive electrode sheet. Similarly, the negative electrode material, conductive agent, binder, and solvent are mixed in a certain proportion, coated on copper foil, and dried to produce a negative electrode sheet.

[0104] The positive electrode material is LiNi x Co y Mn z Any one of O2 (x+y+z=1), LCO and lithium manganate; the negative electrode material is one of metallic lithium, graphite and lithium titanate.

[0105] Acetylene black is a conductive agent; the binder can be selected from vinylidene fluoride / hexafluoropropylene copolymer and polyvinylidene fluoride (PVDF); and the solvent can be selected from N-methylpyrrolidone (NMP) and acetone.

[0106] Button battery separators are generally selected from separators that can better soak into the electrolyte, such as polyethylene, polypropylene, or a mixture of the two.

[0107] Example 16: Battery Assembly and Performance Testing

[0108] CR2025 button cells were assembled in a glove box. The positive and negative electrodes were prepared according to Example 15. The electrolytes from Example 8, Example 10, Example 11, Example 12, Example 13, and Example 14 were used as test electrolytes. The cells were assembled in the following order: negative electrode shell, negative electrode sheet, electrolyte, separator, electrolyte, positive electrode sheet, and positive electrode shell. After assembly, the cells were left to rest for 12 hours to obtain a ternary NCM811 button cell.

[0109] In a glove box, CR2025 button cells were assembled. The positive and negative electrodes were prepared according to Example 15. The electrolyte of Example 8 was then added in the following order: negative electrode shell, negative electrode sheet, electrolyte, separator, electrolyte, positive electrode sheet, and positive electrode shell. After assembly, the cells were left to rest for 12 hours to obtain a lithium cobalt oxide button cell.

[0110] CR2025 button cells were assembled in a glove box. The positive and negative electrodes were prepared according to Example 15. The electrolytes of Example 8 and Example 10 were used as the battery test electrolytes. The cells were assembled in the following order: negative electrode shell, negative electrode sheet, electrolyte, separator, electrolyte, positive electrode sheet, and positive electrode shell. After assembly, the cells were allowed to stand for 12 hours to obtain a lithium manganese oxide button cell.

[0111] CR2025 button cells were assembled in a glove box. The positive and negative electrodes were prepared according to Example 15. The electrolytes of Example 9 and Example 10 were used as the battery test electrolytes. The cells were assembled in the following order: negative electrode shell, negative electrode sheet, electrolyte, separator, electrolyte, positive electrode sheet, and positive electrode shell. After assembly, the cells were allowed to stand for 12 hours to obtain a lithium titanate button cell.

[0112] Battery impedance test method: After the battery cycle is completed, the AC impedance EIS is tested on a Shanghai Chenhua electrochemical workstation with an amplitude of 5 mV and a frequency range of 0.01 Hz to 100 kHz.

[0113] FIG22 is a linear scan test curve of the compound of Example 1 of the present invention. It is found that the compound of Example 1 slowly begins to oxidatively decompose at 3.97 V, indicating that the cyano-functionalized organosiloxane compound can be used as a film-forming additive in batteries.

[0114] FIG23 is a linear scan test curve of the compound of Example 2 of the present invention. It is found that the compound of Example 2 slowly begins to oxidatively decompose at 4.05 V, indicating that the cyano-functionalized organosiloxane compound can be used as a film-forming additive in batteries.

[0115] FIG24 is a linear scan test curve of the compound of Example 3 of the present invention. It is found that the compound of Example 3 slowly begins to oxidatively decompose at 3.98 V, indicating that the cyano-functionalized organosiloxane compound can be used as a film-forming additive in batteries.

[0116] FIG25 is a linear scan test curve of the compound of Example 4 of the present invention. It is found that the compound of Example 4 begins to oxidatively decompose at 5.8 V, indicating that the compound of Example 4 can improve the stability of the electrolyte.

[0117] FIG26 is a linear scan test curve of the compound of Example 5 of the present invention. It is found that the additive compound of Example 5 itself begins to oxidatively decompose at 5.84V, indicating that the compound of Example 5 can improve the stability of the electrolyte.

[0118] FIG27 is a linear scan test curve of the compound of Example 6 of the present invention. It is found that the additive compound of Example 6 itself begins to oxidatively decompose at 3.67V, indicating that the compound of Example 6 can improve the stability of the electrolyte.

[0119] As shown in Figure 28, NCM811 and lithium sheets were used as the positive and negative electrodes, respectively, to assemble 2025 button-type batteries. Charge / discharge tests were conducted at Shenzhen Xinwei, with charge and discharge voltages ranging from 3-4.3V. The electrolyte batteries of Examples 8 and 11 were charged / discharged at a constant current of 1C. It was found that compared to the electrolyte battery of Comparative Example 1, the NCM811 / Li half-cells assembled with the electrolytes of Examples 8 and 11 showed improved room-temperature cycling performance, with capacity retention rates increasing from 88.2% to 93.3% (60 cycles) and from 90.4% to 99.4% (49 cycles), respectively.

[0120] FIG29 is a rate performance test of the electrolyte batteries of Example 8 of the present invention and Comparative Example 1. The NCM811 / Li battery assembled with the electrolyte of Example 8 exhibits higher capacity at different rates.

[0121] FIG30 shows the rate performance test of LMO / Li batteries assembled with the electrolytes of Example 8 of the present invention and Comparative Example 1. The LMO / Li battery assembled with the electrolyte of Example 8 exhibits relatively high capacity at high rates of 5C / 10C.

[0122] Figures 31-32 show 2025 button-type cells assembled using LMO and lithium sheets as the positive and negative electrodes, respectively. Charge / discharge tests were conducted at Shenzhen Xinwei, with charge and discharge voltages ranging from 3-4.3V. The cells assembled with the electrolyte of Example 8 were charged and discharged at a constant current of 1C. The high-temperature 60°C cycling performance of the LMO / Li half-cell assembled with the electrolyte of Example 8 was found to be improved, with capacity retention increasing from 91.7% to 93% (110 cycles). In Figure 32, the room-temperature cycling capacity of the LMO / Li half-cell assembled with the electrolyte of Example 8 was significantly improved.

[0123] Figure 33 shows a 2025 button-type battery assembled using LCO and graphite as the positive and negative electrodes, respectively. Charge / discharge testing was performed at Shenzhen Xinwei, with charge and discharge voltages ranging from 3 to 4.53V. The battery assembled with the electrolyte of Example 8 was charged and discharged at a constant current of 1C. The LCO / graphite full cell assembled with the electrolyte of Example 8 exhibited a slight improvement in capacity at 45°C compared to the cell assembled with the electrolyte of Comparative Example 1.

[0124] FIG34 shows impedance measurements of LCO / Graphite batteries assembled with the electrolytes of Example 8 and Comparative Example 1. The additive in the electrolyte of Example 8 is TMSPAN, synthesized in Example 1, which significantly reduces the impedance of the LCO / Graphite battery interface film.

[0125] Figure 35 shows a 2025 button-type battery assembled using NCM811 and lithium sheets as the positive and negative electrodes, respectively. Charge and discharge tests were conducted at Shenzhen Xinwei, with charge and discharge voltages ranging from 3 to 4.5V. The battery assembled with the electrolyte of Example 10 was charged and discharged at a constant current of 1C. The NCM811 / Li half-cell assembled with the electrolyte of Example 10 showed significantly improved cycling performance at a high voltage of 4.5V and a high temperature of 55°C.

[0126] Figure 36 shows the impedance test of LTO / Li half-cells assembled with the electrolytes of Examples 9 and 10 of the present invention and Comparative Example 1. The additive in the electrolyte of Example 9 is HMSPAN1 synthesized in Example 2, and the additive in the electrolyte of Example 10 is HMSPAN2 synthesized in Example 3. Both can significantly reduce the impedance of the lithium titanate battery interface film.

[0127] Figure 37 shows a 2.22Ah pouch cell assembled using LMO / LTO materials. The cell, assembled with the electrolyte of Example 10, was charged and discharged at 55°C at a constant current of 2C. The LMO / LTO pouch cell assembled with the electrolyte of Example 10 maintained its capacity after 170 cycles.

[0128] Figure 38 shows a 1Ah Pouch battery assembled using NCM622 / graphite material and stored at 85°C for 6 hours. The capacity retention and recovery rates of the Pouch battery assembled with the electrolyte of Example 11 are slightly improved.

[0129] Figure 39 shows a 1Ah Pouch cell assembled using NCM622 / graphite material and stored at 85°C for 6 hours. The expansion rate of the Pouch cell assembled with the electrolyte of Example 11 under hot and cold test conditions is significantly lower than that of Comparative Example 2. The electrolyte material of Example 6 can suppress high-temperature gas production in the cell.

[0130] FIG40 shows the impedance test of NCM811 / Li half-cells assembled with the electrolytes of Examples 12 and 13 of the present invention and Comparative Example 1. The electrolyte additives of Examples 12 and 13 can significantly reduce the impedance of the positive electrode material interface film.

[0131] Figure 41 shows a 2025 coin-shaped battery assembled using NCM811 and lithium sheets as the positive and negative electrodes, respectively. Charge and discharge tests were conducted at Shenzhen Xinwei, with a charge and discharge voltage of 3-4.5V. The battery assembled with the electrolyte of Example 14 was charged and discharged at a constant current of 1C. The cycling performance of the NCM811 / Li half-cell assembled with the electrolyte of Example 14 was found to be improved, with capacity retention increasing from 87.2% to 91.8%.

Claims

1. A cyano-functionalized organosiloxane compound having a chemical structure as shown in Formula 1, Formula 2 or Formula 3, or a cyano-functionalized organosiloxane isomer as shown in Formula 4 and Formula 5: in, R1 is selected from C1-C5 alkyl; n1 is an integer from 0 to 5; n2 is an integer from 1 to 5, X is selected from C2-C5 straight chain alkylene, Y is selected from C2-C5 straight chain alkylene or C2-C5 branched chain alkylene or -NR2CH2CH2CN, wherein R2 is C2-C5 straight chain or C2-C5 branched chain alkylene.

2. The method for preparing the cyano-functionalized organosiloxane compound according to claim 1, characterized in that: The method comprises the following steps: under the protection of inert gas, double-bond imine nitrile or double-bond nitrile compound respectively reacts with alkoxysilane under platinum metal catalysis for hydrosilylation reaction, the reaction temperature is 30-130°C, and the reaction time is 4-24h; the molar ratio of the double-bond imine nitrile or double-bond nitrile compound to the alkoxysilane is 1:1.0-2.2; the alkoxysilane is any one of pentamethyldisiloxane, 1,1,3,3,5,5,5-heptamethyltrisiloxane or 1,1,1,3,5,5,5-heptamethyltrisiloxane; and the hydrosilylation reaction catalyst is selected from chloroplatinic acid or Karstedt's catalyst, and the added amount is 0.1-1 times of the double-bond imine nitrile or double-bond nitrile compound.

3. Use of the cyano-functionalized organosiloxane compound represented by Formula 1, Formula 2 or Formula 3 or the cyano-functionalized organosiloxane isomers represented by Formula 4 and Formula 5 in lithium ion batteries, sodium ion batteries, potassium ion batteries, lithium sulfur batteries, and supercapacitors according to claim 1, characterized in that: The cyano-functionalized organosiloxane compound or the cyano-functionalized organosiloxane isomers represented by Formula 4 and Formula 5 are used as high-pressure or high-temperature additives or solvents for electrolytes of lithium-ion batteries, sodium-ion batteries, potassium-ion batteries, lithium-sulfur batteries, and supercapacitors.

4. The use according to claim 3, characterized in that: The lithium-ion battery electrolyte comprises a lithium salt, a solvent and the cyano-functionalized organosiloxane compound as claimed in claim 1 or the cyano-functionalized organosiloxane isomers represented by Formula 4 and Formula 5 as an electrolyte additive or solvent.

5. The use according to claim 4, characterized in that: The concentration of the lithium salt in the electrolyte is 0.5-1.5 mol / L, and the usage of the cyano-functionalized organosiloxane compound or the cyano-functionalized organosiloxane isomers represented by Formula 4 and Formula 5 is 0.1%-5% of the total mass of the lithium salt and the solvent.

6. The use according to claim 4, characterized in that: The solvent includes two or more of ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.

7. The use according to claim 4, characterized in that: The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium perchlorate, lithium bis(trifluoromethanesulfonylimide) and lithium bis(fluorosulfonylimide).

8. The use according to claim 3, characterized in that: The positive electrode material of lithium-ion batteries is LiNi x Co y Mn z O2, any one of lithium cobalt oxide, nickel cobalt aluminum and lithium manganese oxide; the negative electrode material of the lithium ion battery is one of metallic lithium, graphite, lithium titanate or silicon-based system, wherein x, y, z refer to the molar ratio of nickel, cobalt and manganese respectively, x+y+z=1, x≥0.

6.

9. A lithium ion battery, characterized in that: The invention comprises a positive electrode sheet containing a positive electrode active material, a negative electrode sheet containing a negative electrode active material, a lithium battery separator and a lithium ion battery electrolyte, wherein the lithium ion battery electrolyte comprises a lithium salt, a solvent and the cyano-functionalized organosiloxane compound as described in claim 1 or the cyano-functionalized organosiloxane isomers shown by formula 4 and formula 5.

10. The lithium ion battery according to claim 9, characterized in that: The positive electrode material of lithium-ion batteries is LiNi x Co y Mn z O2, lithium cobalt oxide, nickel cobalt aluminum and lithium manganese oxide; the negative electrode material of the lithium ion battery is one of metallic lithium, graphite, lithium titanate or silicon-based system; wherein x, y, z refer to the molar ratio of nickel, cobalt and manganese respectively, x+y+z=1, x≥0.6.

Citation Information

Patent Citations

  • Siloxane derivative electrolyte for lithium-ion battery and high-voltage lithium-ion battery

    CN105449278A

  • Electrolyte and lithium ion battery comprising same

    CN105810998A

  • Double-cyano functionalized organic silicon-amino electrolyte material

    CN106025358A

  • Functionalized silanes and electrolyte compositions and electrochemical devices containing same

    CN106795184A

  • Cyano-functionalized organosiloxane compound as well as preparation and application thereof

    CN116621867A

Cited By

  • Electrolyte, lithium ion battery and preparation method of lithium ion battery

    CN119994196A