Coin-shaped lithium primary battery
The coin-shaped lithium primary battery incorporates a boron-containing positive electrode mixture with optimized graphite dimensions to prevent moisture-induced internal resistance increases, maintaining battery performance and extending shelf life by forming a conductive film that reacts with water, addressing the issue of moisture ingress and film formation on the negative electrode.
Patent Information
- Application Number
- PCT/JP2024/001672
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-01-22
- Publication Date
- 2024-11-21
AI Technical Summary
Coin-type lithium primary batteries experience a significant increase in internal resistance during storage due to moisture ingress, which forms an inert film on the negative electrode, leading to reduced battery performance.
A coin-shaped lithium primary battery design featuring a positive electrode with manganese dioxide, graphite, a binder, and a boron compound, where the thickness and average length of the graphite are optimized to suppress the formation of non-conductive films by promoting the formation of a boron-containing conductive film that sacrificially reacts with water, thereby maintaining low internal resistance.
The optimized design effectively suppresses the increase in internal resistance due to moisture, ensuring stable battery performance over long-term storage, thus extending the battery's shelf life and suitability for small devices and memory backups.
Smart Images

Figure JP2024001672_21112024_PF_FP_ABST
Abstract
Description
Coin-type lithium primary battery
[0001] The present disclosure relates to coin-type lithium primary batteries.
[0002] Patent Document 1 proposes a "non-aqueous battery including an active metal negative electrode, a positive electrode, and an ion-conductive electrolyte solution containing a solute dissolved in a non-aqueous electrolyte, the solute being a salt of a first component which is a halide of an element selected from the group consisting of Al, Sb, Zr, and P, and a second component which is a halide, sulfide, sulfite, oxide, or carbonate of calcium or an alkali metal selected from the group consisting of Li, Na, and K, wherein the active metal negative electrode has a surface layer of a boron-containing material."
[0003] Patent Document 2 proposes "a lithium primary battery comprising a positive electrode made of manganese dioxide, a negative electrode made of lithium or a lithium alloy, and an electrolyte, characterized in that the manganese dioxide is manganese dioxide to which boron has been added, and the electrolyte contains butylene carbonate as a solvent."
[0004] Patent Document 3 proposes "a nonaqueous electrolyte battery including a positive electrode, a negative electrode, and an electrolyte, wherein the positive electrode comprises a positive electrode mixture including electrolytic manganese dioxide as an active material, expanded graphite as a conductive agent, and a binder, and the ratio of the median diameter of the expanded graphite to the median diameter of the electrolytic manganese dioxide is 1.5 to 3."
[0005] JP 59-117070 A JP 2007-134270 A JP 2019-102152 A
[0006] Although coin-type lithium primary batteries have a sealed structure, their internal resistance (IR) increases significantly during storage. The main cause of this increase in IR is the phenomenon in which moisture from the outside reacts with the negative electrode, forming an inert film on the negative electrode surface. Because coin-type batteries have a small internal volume, the concentration of moisture that enters can easily increase, leading to the formation of an inert film in a short period of time and a significant increase in IR.
[0007] In view of the above, one aspect of the present disclosure relates to a coin-type lithium primary battery including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte solution, wherein the positive electrode includes manganese dioxide, graphite, a binder, and a boron compound, and wherein a thickness T (mm) of the positive electrode and an average length DL (mm) of a major axis of the graphite satisfy formula (1): 0.02≦T (mm)×DL (mm)≦0.12.
[0008] The coin-type lithium primary battery according to the present disclosure can suppress an increase in internal resistance caused by moisture penetration during storage.
[0009] FIG. 1 is a longitudinal cross-sectional view of a coin-type lithium primary battery according to one embodiment of the present disclosure.
[0010] Hereinafter, embodiments of the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be exemplified, but other numerical values, materials, etc. may be applied as long as the effects of the present disclosure are obtained. Note that components other than those characteristic of the present disclosure may be components of known secondary batteries. In this specification, when a "range from numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B. In the following description, when a lower limit and an upper limit are exemplified for numerical values of specific physical properties, conditions, etc., any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit.
[0011] The present disclosure encompasses any combination of two or more claims arbitrarily selected from the appended claims, i.e., any combination of two or more claims arbitrarily selected from the appended claims may be combined unless a technical contradiction arises.
[0012] A coin-type lithium primary battery according to an embodiment of the present disclosure includes a power generating element including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte solution. The power generating element is hermetically housed in a predetermined exterior body.
[0013] The positive electrode is formed by press-molding a positive electrode mixture into a predetermined shape. The positive electrode mixture contains manganese dioxide, graphite, a binder, and a boron compound. The positive electrode has a pellet or cylindrical (disk) shape corresponding to the shape of the coin-type lithium primary battery. The thickness T of the positive electrode is not particularly limited, but is, for example, 400 μm or more and 2000 μm or less.
[0014] The negative electrode is formed, for example, by processing a metal sheet or metal foil into a predetermined shape. At least one of lithium metal and a lithium alloy can be used for the metal sheet. Examples of lithium alloys include lithium-aluminum alloys, lithium-tin alloys, lithium-silicon alloys, and lithium-lead alloys. The negative electrode has a disk shape that matches the shape of a coin-type lithium primary battery. A foil of lithium metal or a lithium alloy may be punched into a circle and used as the negative electrode.
[0015] The exterior body includes, for example, a case having a bottom plate and side portions rising from the periphery of the bottom plate and having a first terminal surface on its outer surface, a sealing plate having a top plate and periphery portions extending from the top plate to the inside of the side portions of the case and having a second terminal surface on its outer surface, and a gasket interposed and compressed between the side portions and the periphery. The edge of the side portion of the case is crimped to the sealing plate via the gasket.
[0016] Within the exterior, the following three reactions are primarily occurring competitively on the surface of the negative electrode: (A) A reaction to form a non-conductive film (A) caused by a reaction between invading moisture and the negative electrode surface; (B) A reaction to form an intermediate film (B) caused by a reaction between a boron compound and manganese dioxide, which produces a boron-containing intermediate, and the negative electrode surface; and (C) A reaction to form a film (C) caused by a reaction between a boron-containing product produced from the boron-containing intermediate and the negative electrode surface.
[0017] The boron-containing intermediate can exist in various forms, but is thought to be an ionic species generated by the decomposition of a boron compound by the catalytic action of manganese dioxide. The intermediate film (B) formed by the reaction of the boron-containing intermediate with the negative electrode surface has lower resistance than the non-conductive film (A) derived from water resulting from the reaction of moisture with the negative electrode surface, and can suppress an increase in internal resistance (IR), but this is not sufficient.
[0018] The boron-containing product may exist in various forms, but analysis shows that it is primarily Li 2 BO 2 Cation, LiBO 2 It is believed that the boron-containing product exists in the electrolyte as an ionic species such as an anion. Hereinafter, the boron-containing product is also referred to as "LBO ion."
[0019] The film (C) formed by the reaction of LBO ions with the negative electrode surface suppresses an increase in IR by sacrificially reacting with water. In other words, it is believed that the film (C) repeatedly forms and disappears. Therefore, the film (C) has little effect on the battery reaction and suppresses the formation of a water-derived non-conductive film. The inclusion of a boron compound in the positive electrode ensures a continuous supply of LBO ions necessary for repairing the film (C). This significantly suppresses an increase in internal resistance due to moisture entering the battery during storage.
[0020] Here, the thickness T (mm) of the positive electrode and the average length DL (mm) of the major axis of the graphite satisfy the following formula (1): 0.02≦T (mm)×DL (mm)≦0.12.
[0021] The product of T and DL (T·DL) in mm is 0.02 or more, or may be 0.04 or more, or may be 0.05 or more. The larger T·DL is, the thicker the positive electrode is and the flatter the graphite particles are.
[0022] The boron compound moves through the electrolyte in the positive electrode while repeatedly coming into contact with manganese dioxide. The basal surfaces of the flat-shaped graphite particles act as a barrier to the movement of the boron compound. Because the boron compound moves around the graphite particles, its migration path within the positive electrode becomes longer. This increases the opportunities for contact between the boron compound and manganese dioxide, and a larger amount of the boron compound is converted into a boron-containing intermediate, which then converts to LBO ions before reaching the negative electrode surface. As a result, the above-mentioned (C) "reaction of forming a good conductor film by reaction of the boron-containing product generated from the boron-containing intermediate with the negative electrode surface" becomes more dominant. In other words, the larger the T·DL, the more dominant the above-mentioned reaction (C) becomes.
[0023] Since the separator contains an abundant amount of electrolyte, the boron-containing product that reaches the electrolyte in the separator can quickly reach the surface of the negative electrode.
[0024] On the other hand, T·DL is 0.12 or less, and may be 0.10 or less, or 0.09 or less. If T·DL is too large, the positive electrode becomes excessively thick or the graphite particles become excessively flattened. If T·DL is too large, the migration path of LBO ions within the positive electrode becomes too long, and the above-mentioned (A) "reaction of forming a non-conductive film due to the reaction between infiltrated moisture and the negative electrode surface" becomes more dominant. In other words, if T·DL is too large, it is difficult to suppress an increase in the IR of the battery.
[0025] Graphite has a basal plane and an edge plane. The basal plane is the plane that determines the length of the long axis of graphite. The edge plane is the end face of the layer structure and is much shorter than the basal plane. In other words, most graphite particles have a flat shape with a long axis and a short axis. The average length of the long axis (DL) and the average length of the short axis (DW) can be measured, for example, using a scanning electron microscope (SEM) image of the cross section of the positive electrode by the following procedure. The aspect ratio of graphite is defined as the ratio of DL / DW.
[0026] (1) Randomly select 200 or more graphite particles from the SEM image.
[0027] (2) Determine the rectangle min with the smallest area that surrounds each particle.
[0028] (3) The length of the long side of the rectangle min is measured as the length of the long axis (dL) of the particle.
[0029] (4) The length of the short side of the rectangle min is measured as the length of the minor axis (dW) of the particle.
[0030] (5) The length (dL) of the long side of the rectangles (min) of 200 or more particles is averaged to obtain the average length (DL) of the major axis. DL is generally 10 μm to 100 μm, and may be 20 μm to 80 μm.
[0031] (6) The lengths of the short sides (dW) of the rectangles (min) of 200 or more particles are averaged to obtain the average length of the minor axis (DW). DW is generally 0.1 μm to 5 μm, but may be 0.5 μm to 4 μm, or 1 μm to 3 μm.
[0032] (7) The aspect ratio is calculated as the ratio of DL / DW. The aspect ratio is generally 2 to 1000, and may be 5 to 800.
[0033] Graphite acts as a conductive additive. When the positive electrode mixture contains graphite, a sufficient electron conduction path is ensured in the positive electrode, ensuring sufficient output.
[0034] The graphite may contain expanded graphite. The expanded graphite particles have a flat shape. Expanded graphite is prepared, for example, by inserting sulfuric acid between layers of the basal plane of graphite and then foaming. Expanded graphite has a large interplanar spacing in the c-axis direction perpendicular to the basal plane, and is therefore prone to exfoliation and flattening. The interplanar spacing (d002) of the (002) plane of expanded graphite determined by powder X-ray diffraction using CuKα radiation may be, for example, 3.37 Å or more. The crystallite size Lc(002) in the c-axis direction may be, for example, 500 Å or less. Note that the expanded graphite contains a trace amount of residual sulfate ions (SO 3 - ) is included.
[0035] The interplanar spacing (d002) can be determined from the Bragg equation (λ=2d×sin θ) by X-ray diffraction.
[0036] λ: wavelength of CuKα radiation (= 0.15418 nm) d: average interplanar spacing d002 of the (002) plane θ: angle (rad) of 1 / 2 of 2θ at the peak position determined by the centroid method The crystallite size Lc(002) can be calculated from the half width of the X-ray diffraction peak assigned to the (002) plane using Scherrer's formula (D(nm) = 0.9 × λ / (β × cos θ)).
[0037] λ = CuKα wavelength, β = half-width (rad) of the peak, θ = 1 / 2 angle (rad) of 2θ at the peak position determined by the centroid method. The graphite content contained in the positive electrode (i.e., positive electrode mixture) is preferably, for example, 1% by mass or more and 10% by mass or less, and more preferably 1% by mass or more and 5% by mass or less. If the graphite content is 1% by mass or more, the migration path of the boron compound or boron-containing intermediate becomes sufficiently long, allowing a sufficient amount of LBO ions to reach the negative electrode surface. If the graphite content is 10% by mass or less, the migration path of the boron compound or boron-containing intermediate does not become excessively long, preventing the formation of a water-derived non-conductor film from becoming dominant. Furthermore, if the graphite content is 1% by mass or more and 10% by mass or less, the positive electrode capacity can be ensured while also sufficiently ensuring its function as a conductive additive. The content of expanded graphite in the graphite is, for example, 80% by mass or more, or may be 90% by mass or more, or may be 100%.
[0038] The boron compound is a source of LBO ions. The boron compound may be, for example, at least one selected from the group consisting of boron oxides and lithium-containing boron oxides. Regardless of the type of boron compound, the final boron-containing product is LBO ions (Li 2 BO 2 Cation, LiBO 2 It is believed that ionic species such as anions are generated in the electrolyte. In particular, LiBO 2 It is highly likely that ionic species having the structure LiBO are generated, and the film on the negative electrode surface also contains LiBO. 2 It appears to maintain its structure.
[0039] The presence of LBO ions can be considered by, for example, inferring the state of boron elements in the film by time-of-flight secondary ion mass spectrometry (TOF-SIMS).
[0040] Examples of the boron compound to be mixed in the positive electrode mixture include B 2 O 3 , Li 2 B4 O 7 , Li 3 BO 3 and LiBO 2 At least one selected from the group consisting of these can be used. All of these are suitable as a source of LBO ions. Among them, B 2 O 3 and LiBO 2 At present, it is believed that at least one selected from the group consisting of the following is most suitable as a source of LBO ions.
[0041] The content of the boron compound contained in the positive electrode is, for example, 0.5% by mass or more and 5% by mass or less, and may be 0.8% by mass or more and 3% by mass or less. A boron compound content of 0.5% by mass or more is sufficient to continuously supply the LBO ions necessary for repairing the coating (C). This significantly suppresses an increase in internal resistance due to moisture penetration into the battery during storage. A boron compound content of 5% by mass or less can maximize the effect of suppressing an increase in internal resistance while ensuring sufficient positive electrode capacity.
[0042] The ratio Ve / (Vp+Vs), i.e., Ve / Vt, based on the volume Ve of the electrolyte in the battery and the total volume Vt of the void volume Vp of the positive electrode and the void volume Vs of the separator, is preferably 0.9 or more and 1.5 or less, and more preferably 1.0 or more and 1.2 or less.
[0043] When the volume Ve of the electrolyte in the battery is large and the Ve / Vt ratio exceeds 1.5, a portion of the electrolyte may be present outside the power-generating element without being impregnated into the positive electrode, separator, and negative electrode. Furthermore, boron compounds eluted from the positive electrode into the electrolyte may migrate through the electrolyte present outside the power-generating element and reach the negative electrode surface. Therefore, the boron compound or boron-containing intermediate before being converted to LBO ions may react on the negative electrode surface, resulting in insufficient formation of a film derived from LBO ions. On the other hand, when the volume Ve of the electrolyte in the battery is small and the Ve / Vt ratio is less than 0.9, the migration of LBO ions in the positive electrode slows, the non-conductive film formation reaction (A) becomes dominant, and it may be difficult to suppress an increase in the IR of the battery.
[0044] The volume Ve of the electrolyte in the battery can be calculated from the mass of the electrolyte contained in the battery and the specific gravity of the electrolyte. The mass of the electrolyte can be calculated by disassembling the battery, drying the power generating element, and then calculating the mass difference between the mass of the battery before disassembly and the mass of the battery after disassembly and drying.
[0045] The pore volume Vp of the positive electrode can be measured, for example, by the following procedure using a scanning electron microscope (SEM) image of the cross section of the positive electrode.
[0046] (1) An SEM image including a cross section of a positive electrode (positive electrode mixture) having a sufficient size is taken.
[0047] (2) By image processing, the area Se occupied by the electrolyte or voids in the area Sp of the cross section of a given positive electrode (positive electrode mixture) is determined.
[0048] (3) The void volume of the positive electrode, Vp, is calculated as Vp=Sp×Se / Sp.
[0049] The void volume Vs of the separator can be measured, for example, by the following procedure using a scanning electron microscope (SEM) image of the separator cross section.
[0050] (1) An SEM image including a cross section of a separator having a sufficient size is taken.
[0051] (2) By image processing, the area Sse occupied by the electrolyte or voids in the cross-sectional area Ss of a given separator is determined.
[0052] (3) The void volume of the separator is calculated as Vs = Ss × Sse / Ss.
[0053] The electrolyte contains a non-aqueous solvent and a solute (salt). The solute concentration in the electrolyte is, for example, 0.3 mol / L to 2 mol / L. As the non-aqueous solvent, propylene carbonate, ethylene carbonate, 1,2-dimethoxyethane, etc. can be used. These can be used alone or in combination of two or more. As the solute, LiClO 4 , LiPF 6 , LiBF 4, LiCF3SO3, LiN(CF3SO2)2, etc. can be used. These may be used alone or in combination of two or more.
[0054] The manganese dioxide may be electrolytic manganese dioxide. The electrolytic manganese dioxide may be neutralized with an alkali and then calcined. For example, the electrolytic manganese dioxide may be calcined in air or oxygen at 300 to 450°C for approximately 6 to 12 hours. Calcination volatilizes water, promotes crystallization, and also reduces the specific surface area. This improves the structural stability and water-resistant reactivity of the manganese dioxide. When using uncalcined electrolytic manganese dioxide, the crystallinity may be increased by adjusting the conditions during electrolysis to reduce the specific surface area.
[0055] The volume-based median diameter (D50) of manganese dioxide measured with a laser diffraction / scattering measuring device is, for example, 20 μm to 50 μm, or may be 20 μm to 45 μm, or may be 20 μm to 35 μm. When the median diameter of manganese dioxide is 20 μm or more, the opportunity for contact between graphite and the boron compound in the positive electrode increases, and the number of contact points between active materials also increases. On the other hand, when the median diameter of manganese dioxide is 50 μm or less, the pressure required to form the positive electrode mixture is reduced, making it easier to increase the packing density.
[0056] Examples of binders that can be used include fluororesins, rubber particles, and acrylic resins. Examples of fluororesins that can be used include polytetrafluoroethylene (hereinafter also referred to as "PTFE"), tetrafluoroethylene-hexafluoropropylene copolymers, and polyvinylidene fluoride. Examples of rubber particles that can be used include styrene butadiene rubber (SBR) and modified acrylonitrile rubber. Examples of acrylic resins include ethylene-acrylic acid copolymers. One type of binder may be used alone, or two or more types may be used in combination.
[0057] Among the binders, fibrous fluororesin is preferred. The fibrous fluororesin does not excessively coat the surface of the manganese dioxide and does not significantly inhibit contact between the surface of the manganese dioxide and the electrolyte (and further the boron compound or boron-containing intermediate). The fibrous fluororesin may be a fluororesin that does not dissolve in N-methyl-2-pyrrolidone (NMP) and disperses as particles. The fibrous fluororesin may be a fluororesin that fibrillates due to pressure applied to the positive electrode mixture when preparing the positive electrode.
[0058] Among fibrous fluororesins, for example, PTFE is preferred. PTFE is a fluororesin consisting of tetrafluoroethylene units (-CF 2 CF 2 The PTFE is a fluororesin containing tetrafluoroethylene units as a main component. The PTFE has a tetrafluoroethylene unit content of, for example, 90 mol % or more, and may have a weight average molecular weight Mw of, for example, 200,000 to 800,000.
[0059] The content of the binder contained in the positive electrode is, for example, 1% by mass or more and 10% by mass or less, and may be 1% by mass or more and 5% by mass or less. If the content of the binder is 1% by mass or more, it is possible to ensure sufficient positive electrode capacity while ensuring sufficient strength of the positive electrode. If the content of the binder contained in the positive electrode is 10% by mass or less, it is possible to maximize the effect of suppressing an increase in internal resistance while ensuring sufficient positive electrode capacity. The content of PTFE in the binder is, for example, 80% by mass or more, or may be 90% by mass or more, or may be 100%.
[0060] The separator may be made of any material that can prevent short-circuiting between the positive and negative electrodes and retain the electrolyte. Examples include woven fabrics, nonwoven fabrics, and microporous films made of polyolefin, polyester, etc. Polypropylene nonwoven fabrics are particularly preferred.
[0061] 1 is a longitudinal cross-sectional view of a coin-type lithium primary battery according to an embodiment of the present disclosure. The coin-type battery 11 includes an exterior body composed of a case 3, a sealing plate 8, and a gasket 7. The case 3 is a cylindrical, shallow-bottomed battery can having a bottom plate 3a and a side portion 3b that rises from the periphery of the bottom plate 3a via a first bend 9. The sealing plate 8 has a top plate 8a and a peripheral portion 8b that extends from the top plate 8a to the inside of the side portion 3b of the case 3. The end 3t (opening end) of the side portion 3b of the case 3 is bent inward at a second bend 10 and crimped to the peripheral portion 8b of the sealing plate 8 via the gasket 7, thereby sealing the gap between the case 3 and the sealing plate 8.
[0062] The exterior housing contains a power generating element. The power generating element includes a positive electrode 4, a negative electrode 5, a separator 6, and an electrolyte. In the illustrated example, the positive electrode 4 is disposed so as to face the bottom plate portion 3a of the case 3. Therefore, the outer surface of the bottom plate portion 3a functions as a positive electrode terminal surface. On the other hand, the negative electrode 5 is disposed so as to face the top plate portion 8a of the sealing plate 8. Therefore, the outer surface of the top plate portion 8a functions as a negative electrode terminal surface.
[0063] Although an example of a coin-type lithium primary battery has been described above, the shape of the battery is not particularly limited. The thickness and diameter of the battery are also not particularly limited. The coin-type lithium primary battery also includes a button-type lithium primary battery.
[0064] (Additional Note) The above description discloses the following techniques.
[0065] (Technology 1) A coin-type lithium primary battery comprising: a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte; wherein the positive electrode comprises manganese dioxide, graphite, a binder, and a boron compound; and wherein a thickness T (mm) of the positive electrode and an average length DL (mm) of the major axis of the graphite satisfy the following formula: 0.02≦T (mm)×DL (mm)≦0.12.
[0066] (Technology 2) The coin-type lithium primary battery according to Technology 1, wherein the graphite includes expanded graphite.
[0067] (Technology 3) The coin-type lithium primary battery according to Technology 1 or 2, wherein the content of the graphite contained in the positive electrode is 1% by mass or more and 10% by mass or less.
[0068] (Technology 4) The coin-type lithium primary battery according to any one of Technologies 1 to 3, wherein the boron compound is at least one selected from the group consisting of boron oxides and lithium-containing boron oxides.
[0069] (Technology 5) The boron compound is B 2 O 3 , Li 2 B 4 O 7 , Li 3 BO 3 and LiBO 2 5. The coin-type lithium primary battery according to any one of claims 1 to 4, wherein the lithium primary battery is at least one selected from the group consisting of:
[0070] (Technology 6) The coin-type lithium primary battery according to any one of Technologies 1 to 5, wherein the content of the boron compound contained in the positive electrode is 0.5% by mass or more and 5% by mass or less.
[0071] (Technology 7) The coin-type lithium primary battery according to any one of Technologies 1 to 6, wherein the ratio of the volume of the electrolyte solution to (the pore volume of the positive electrode plus the pore volume of the separator) is 0.9 or more and 1.5 or less.
[0072] (Technology 8) The coin-type lithium primary battery according to any one of Technologies 1 to 7, wherein the binder contains a fibrous fluororesin.
[0073] (Technology 9) The coin-type lithium primary battery according to Technology 8, wherein the fluororesin contains polytetrafluoroethylene.
[0074] <Examples> The present disclosure will be specifically described below based on examples. However, the present invention is not limited to the following examples. In these examples, a coin-type lithium primary battery having a structure as shown in FIG. 1 was fabricated.
[0075] Example 1 (1) Positive Electrode As a positive electrode active material, calcined electrolytic manganese dioxide was prepared by calcining electrolytic manganese dioxide in air at 400°C for 10 hours. A mixture of 95 parts by mass of calcined manganese dioxide, 2 parts by mass of expanded graphite (the average major axis length (DL): 0.06 mm, determined by the method described above after disassembling the prepared battery), and 1 part by mass of LiBO was used. 2 These were dry-mixed. Next, an aqueous dispersion containing 2 parts by mass of PTFE was added to the resulting mixed powder, followed by wet-mixing. The resulting mixture was dried to obtain a positive electrode mixture. The positive electrode mixture was tableted into a cylindrical shape with a diameter of 15 mm and a thickness (T) of 0.35 mm (T·DL = 0.021) to produce a positive electrode. The cylindrical positive electrode pellets were dried at 250 ° C for 8 hours.
[0076] (2) Negative Electrode A lithium metal foil having a thickness of 0.15 mm was punched into a circle having a diameter of 16 mm to prepare a negative electrode.
[0077] (3) Electrolyte: A non-aqueous solvent consisting of a mixture of propylene carbonate and 1,2-dimethoxyethane in a volume ratio of 2:1, containing lithium perchlorate (LiClO) as a solute. 4 ) was dissolved at a concentration of 1.0 mol / L to obtain an electrolyte solution.
[0078] (4) Case A case having a bottom plate diameter of 20 mm and a side portion 1b height of 1.1 mm was fabricated by drawing SUS430 (thickness 250 μm) having a nickel plating layer 3 μm thick on its surface.
[0079] (5) Sealing Plate A sealing plate 8 having a top plate portion 8a with a diameter of 17 mm was produced by pressing SUS430 (thickness: 250 μm) having a nickel plating layer with a thickness of 3 μm on its surface.
[0080] (6) Assembly of a Coin Battery A polypropylene gasket was placed on the sealing plate. The negative electrode was attached to the inside of the top plate of the sealing plate. Next, a 300 μm thick polypropylene nonwoven fabric was placed on top of the negative electrode as a separator. Then, the positive electrode was placed on the separator. Then, the electrolyte was poured into the sealing plate. A sealant consisting of blown asphalt and mineral oil was applied to the inside of the side of the case in advance, and the case was placed on the sealing plate. After that, the side edge of the case was bent inward and crimped to the periphery of the sealing plate via the gasket to produce a coin battery (Battery E1).
[0081] The thickness of the assembled battery was 1.2 mm. The assembled battery (approximately 3.5 V) was pre-discharged by a predetermined amount so that the battery voltage would be 3.2 V. The battery capacity after pre-discharge was 230 mAh when the discharge capacity was measured up to 2 V after constant resistance discharge (15 kΩ).
[0082] The ratio of the volume of the electrolyte (Ve) in the battery to the void volume of the positive electrode (Vp) plus the void volume of the separator (Vs) was Ve / (Vp+Vs)=Ve / Vt=1.2.
[0083] Examples 2 to 8 Batteries E2 to E8 were produced in the same manner as in Example 1, except that the battery diameter, battery thickness, positive electrode thickness (T), average length of the major axis of the expanded graphite (DL), and T·DL were changed as shown in Table 1A.
[0084] Comparative Examples 1 to 5 Batteries R1 to R5 were produced in the same manner as in Example 1, except that the battery diameter, battery thickness, positive electrode thickness (T), average length of the major axis of the expanded graphite (DL), and T·DL were changed as shown in Table 1B.
[0085] [Battery Evaluation] Ten batteries of each type were stored for 100 days at 60° C. and a relative humidity of 90%. After storage, the AC internal resistance was measured at room temperature under conditions of a voltage amplitude of 0.2 V and a frequency of 100 Hz.
[0086] Long-term storage of coin batteries at room temperature can be accelerated by storing them in a storage environment of 60°C and 90% relative humidity. Storing them in this environment for 100 days is said to be equivalent to storing them at room temperature for 10 years. The average values calculated for 10 batteries are shown in Tables 1A and 1B.
[0087]
[0088] Table 1A shows that the internal resistance is maintained low when 0.02≦T·DL≦0.12 is satisfied. This is thought to be because more boron compounds are converted to LBO ions before reaching the negative electrode surface, rather than moisture reaching the negative electrode surface and reacting with them.
[0089]
[0090] Table 1B shows that the internal resistance significantly increases when T DL < 0.02 or 0.12 < T DL, which is thought to be because the reaction between moisture and the negative electrode surface is more dominant than the reaction between LBO ions and the negative electrode surface.
[0091] Examples 9 to 12 Batteries E9 to E12 were produced and evaluated in the same manner as in Example 5, except that the total mass of the expanded graphite and manganese dioxide was kept constant and the content of the expanded graphite was changed as shown in Table 2. The results are shown in Table 2.
[0092]
[0093] Table 2 shows that the content of expanded graphite contained in the positive electrode (positive electrode mixture) is preferably 1% by mass to 10% by mass.
[0094] Examples 13 to 15 Batteries E13 to E15 were fabricated and evaluated in the same manner as in Example 5, except that the type of boron compound was changed as shown in Table 3. The results are shown in Table 2.
[0095]
[0096] Table 3 shows that the effect of suppressing the increase in internal resistance can be obtained regardless of the type of boron compound contained in the positive electrode (positive electrode mixture), and that among the boron compounds, LiBO 2 This shows that the effect of
[0097] Examples 16 and 17 Batteries E16 and E17 were produced and evaluated in the same manner as in Example 5, except that the type of graphite was changed to flake graphite or graphene each having a major axis length DL of 0.04 mm as shown in Table 4. The results are shown in Table 4.
[0098]
[0099] Table 4 shows that expanded graphite is highly effective as graphite to be contained in the positive electrode (positive electrode mixture).
[0100] Examples 18 to 21 Batteries E18 to E21 were fabricated and evaluated in the same manner as in Example 5, except that the Ve / Vt ratio was changed as shown in Table 5. The results are shown in Table 5.
[0101]
[0102] Table 5 shows that the Ve / Vt ratio is preferably within the range of 0.9 to 1.5.
[0103] Example 22 A battery E22 was produced and evaluated in the same manner as in Example 5, except that the binder was changed to tetrafluoroethylene-hexafluoropropylene copolymer (FEP) as shown in Table 6. The results are shown in Table 6.
[0104]
[0105] Table 6 shows that it is preferable to use fibrous PTFE as the binder.
[0106] As described above, the coin-type lithium primary battery according to the present disclosure suppresses an increase in internal resistance even after long-term storage at room temperature in an unused state. This makes it possible to extend the recommended usage period of the battery, and is of great industrial value. Furthermore, the coin-type lithium primary battery is suitable for use as a power source for small devices, memory backup, etc.
[0107] 3 Case 3a Bottom plate portion 3b Side portion 3t End portion 4 Positive electrode 5 Negative electrode 6 Separator 7 Gasket 8 Sealing plate 8a Top plate portion 8b Peripheral edge portion 9 First curved portion 10 Second curved portion 11 Coin-type lithium primary battery
Claims
1. A coin-type lithium primary battery comprising: a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte; wherein the positive electrode comprises manganese dioxide, graphite, a binder, and a boron compound; and wherein a thickness T (mm) of the positive electrode and an average length DL (mm) of the major axis of the graphite satisfy the following formula: 0.02≦T (mm)×DL (mm)≦0.
12.
2. The coin-type lithium primary battery according to claim 1, wherein the graphite comprises expanded graphite.
3. The coin-type lithium primary battery according to claim 1, wherein the content of the graphite in the positive electrode is 1% by mass or more and 10% by mass or less.
4. The coin-type lithium primary battery according to claim 1, wherein the boron compound is at least one selected from the group consisting of boron oxides and lithium-containing boron oxides.
5. The boron compound is B 2 O 3 , Li 2 B 4 O 7 , Li 3 B.O. 3 and LiBO 2 The coin-type lithium primary battery according to any one of claims 1 to 4, wherein the lithium primary battery is at least one selected from the group consisting of:
6. The coin-type lithium primary battery according to any one of claims 1 to 4, wherein the content of the boron compound in the positive electrode is 0.5% by mass or more and 5% by mass or less.
7. The coin-type lithium primary battery according to any one of claims 1 to 4, wherein a ratio (Ve / (Vp+Vs) based on the volume Ve of the electrolyte, the void volume Vp of the positive electrode, and the void volume Vs of the separator is 0.9 or more and 1.5 or less.
8. The coin-type lithium primary battery according to any one of claims 1 to 4, wherein the binder contains a fibrous fluororesin.
9. The coin-type lithium primary battery according to claim 8, wherein the fluororesin includes polytetrafluoroethylene.
Citation Information
Patent Citations
Preparation method of MnO2 doped with non-metal ion B3 +
CN110277551A
Lithium primary cell, its anodic active material and production of manganese dioxide used as this anodic active material
JP1990175886A
Nonaqueous electrolyte battery
JP1997129228A
Nonaqueous electrolyte battery
JP1999339794A
Lithium battery
JP2002334703A