Method for producing joined substrate and method for producing semiconductor device

By ensuring substrates have a surface roughness of 1 nm or less and a contact angle of 70° or less, the method addresses bonding defects in semiconductor substrates, resulting in high-quality bonded substrates and reliable semiconductor devices with reduced voids and peeling issues.

WO2024237048A1PCT designated stage expired Publication Date: 2024-11-21SHIN ETSU HANDOTAI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016180
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-04-25
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Bonding defects occur during the direct bonding of semiconductor substrates due to inadequate surface roughness and surface free energy, leading to incomplete bonding and reduced quality of the bonded substrate.

Method used

The method involves preparing substrates with an average surface roughness (Ra) of 1 nm or less and a contact angle with water of 70° or less, adjusting the surface free energy by sputtering a material different from the base material to ensure appropriate bonding conditions, thereby reducing bonding defects and achieving high-quality bonding interfaces.

Benefits of technology

This approach significantly reduces bonding defects, resulting in high-quality bonded substrates with reliable semiconductor devices that minimize peeling or voids at the bonding interface, enhancing the reliability and performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016180_21112024_PF_FP_ABST
    Figure JP2024016180_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is a method for producing a joined substrate by directly joining the surfaces of two substrates to each other, said method comprising: a step for preparing two substrates, with an average surface roughness Ra and surface free energy of the surfaces to be directly joined being used as criteria; and a step for directly joining the two substrates prepared. In the step for preparing the two substrates, the substrates are prepared such that the surfaces to be directly joined have an average surface roughness Ra of 1 nm or less and such that a contact angle between water and the surfaces to be directly joined, which serves as an index of the surface free energy, is not more than 70°. The present invention thus provides a joined substrate production method that makes it possible to reduce the occurrence of joining defects in a joining technique.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a bonded substrate and method for manufacturing a semiconductor device

[0001] The present invention relates to a method for manufacturing a bonded substrate and a method for manufacturing a semiconductor device, and more particularly to a method for manufacturing a bonded substrate manufactured by bonding, for example, SiC wafers, GaN substrates, etc., and a method for manufacturing a semiconductor device.

[0002] SiC and GaN have a wider band gap than Si, which gives them high dielectric breakdown strength, and also high thermal conductivity, making them promising semiconductor materials for various semiconductor devices such as power devices and high-frequency devices. In addition, bonding semiconductor substrates has been used to improve heat dissipation characteristics.

[0003] For example, Non-Patent Document 1 reports that in devices using SiC, the SiC substrate and the subsequent epitaxial growth account for half of the cost, and points out that reducing the cost of the substrate is extremely important. + A method of performing ion implantation and substrate peeling has been proposed. + A method is disclosed in which ion-implanted single-crystal and polycrystalline SiC substrates are bonded together, and then the single-crystal and polycrystalline SiC substrates are separated. + It describes a method for producing the semiconductor device by the separation technique of the above, and describes a method for epitaxially growing InGaN after polishing or dry etching the surface.

[0004] Furthermore, apart from SiC, Non-Patent Document 2 proposes and discloses that a diamond substrate is bonded to a GaN substrate to improve heat dissipation characteristics.

[0005] Non-Patent Document 3 mentions the surface free energy in these substrate bondings, stating that when solids come into contact with each other, atoms form bonds between the contacting surfaces, reducing the surface free energy and lowering the energy of the entire solid, which is the driving force for bonding. It also states that a requirement for bonding is that the surface roughness (Ra: average surface roughness) of the substrates must be less than 1 nm.

[0006] JP 2016-018890 A JP 2013-513963 A

[0007] Iwamuro, "Progress in High Performance and High Reliability of SiC MOSFETs," Proceedings of the Wide Bandgap Semiconductor Society Special Open Symposium, Wide Bandgap Semiconductor Society, 2022. Shuichi Hiza, Kunihiko Nishimura, Eiji Yagyu, Mikio Yamamukai, "Development of GaN-HEMTs Using Diamond Heat Dissipation Substrates," Applied Physics, 90, (3), 167 (2021). Tadashi Suga, "Room Temperature Bonding by Surface Activation and Its Mechanism," Applied Physics, 89, (9), 498 (2020).

[0008] Based on this knowledge about the surface roughness at the time of substrate bonding, polishing and processing are performed to an Ra of 1 nm or less, but in reality, bonding defects may occur.

[0009] The present invention has been made to solve the above problems, and has an object to provide a method for manufacturing a bonded substrate that can reduce the occurrence of bonding defects in bonding technology.

[0010] In order to achieve the above object, the present invention provides a method for manufacturing a bonded substrate by directly bonding the surfaces of two substrates together, comprising the steps of preparing the two substrates based on an average surface roughness Ra and surface free energy of the surfaces to be directly bonded, and directly bonding the two prepared substrates, wherein in the step of preparing the two substrates, substrates are prepared whose surfaces to be directly bonded have an average surface roughness Ra of 1 nm or less and whose surfaces to be directly bonded have a contact angle with water of 70° or less, which serves as an index of the surface free energy.

[0011] Thus, in addition to setting the Ra of the directly bonded surfaces to 1 nm or less, the present invention also takes into consideration the surface free energy. It is thought that if the surface free energy is too low, the substrates will repel each other and become unable to be bonded. Therefore, by preparing two substrates with a surface free energy of at least a moderate level (specifically, using the contact angle with water as an index, a contact angle of 70° or less) and directly bonding them, it is possible to reduce bonding defects, particularly those that result in partial failure within the wafer plane (bonding interface). This makes it possible to provide high-quality bonded substrates.

[0012] In this case, in the step of preparing the two substrates, a material different from the substrate can be sputtered onto the surface of the base material, thereby preparing a substrate in which the surface free energy of the surface to be directly bonded has been adjusted.

[0013] In this way, even if the contact angle with water on the surface of a base material prepared for direct bonding exceeds 70°, a sputtered layer can be formed by the above-described sputtering, and the surface free energy on the surface of the sputtered layer can be adjusted, thereby preparing a substrate having a surface with a contact angle with water of 70° or less.

[0014] The present invention also provides a method for manufacturing a semiconductor device, characterized in that the semiconductor device is manufactured using a bonded substrate manufactured by the above-described method for manufacturing a bonded substrate of the present invention.

[0015] The semiconductor device manufactured in this manner has a high-quality bonded substrate, and therefore peeling or the like does not occur at the bonded interface, resulting in a high-quality and highly reliable semiconductor device.

[0016] As described above, the method for manufacturing a bonded substrate of the present invention makes it possible to reduce bonding defects during substrate bonding. Furthermore, the method for manufacturing a semiconductor device of the present invention makes it possible to provide a high-quality, highly reliable product.

[0017] Fig. 1 is a flow diagram showing an example of a method for manufacturing a bonded substrate and a method for manufacturing a semiconductor device according to the present invention. Fig. 2 is an explanatory diagram showing two substrates used in the method for manufacturing a bonded substrate according to the present invention, and an example of a bonded substrate obtained by directly bonding the two substrates. Fig. 3 is an explanatory diagram showing examples of contact angles (approximately 120° and 70° or less). Fig. 4 is an explanatory diagram showing another example of two substrates used in the method for manufacturing a bonded substrate according to the present invention. Fig. 5 is a graph showing contact angles on the surfaces of each substrate. Fig. 6 is an observation diagram of voids in Comparative Example 1.

[0018] As mentioned above, there has been a problem of poor bonding when directly bonding substrates, such as semiconductor substrates. After extensive research into this problem, the inventors have discovered that it is important to consider not only the surface roughness (Ra) of the substrates to be bonded, but also the surface free energy. As described in Atsushi Toyoda, "Technology of Adhesive Memos and Sticky Notes," Journal of the Japan Society for Precision Engineering, 89, (3), 233 (2023), this phenomenon is similar to that observed when Post-it notes are bonded. Furthermore, surface free energy is related to contact angle (Shinichiro Imabayashi, "Effect of Surface Roughness on the Wettability of Solid Surfaces," Review of Polarography, 115, 54, (2) (2008)). Therefore, surface free energy can be evaluated using the contact angle as an evaluation index. Therefore, more specifically, the inventors have found that if the surfaces have an Ra of 1 nm or less and a contact angle with water of 70° or less, bonding defects can be significantly reduced, and a method for manufacturing a bonded substrate with higher quality and reliability can be provided, and have completed the present invention. Furthermore, as a result of extensive research into the above-mentioned problems, the inventors have found that by using the above-mentioned bonded substrate, a semiconductor device with higher quality and reliability can be provided, and have completed the present invention.

[0019] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited thereto. First, FIG. 2 shows two substrates used in the method for manufacturing a bonded substrate of the present invention and a bonded substrate obtained by directly bonding the two substrates. As shown in FIG. 2 , the two substrates prepared are a support substrate 1 and a bond substrate 2. Furthermore, a bonded substrate 3 is produced by directly bonding one surface 11 of the support substrate 1 to one surface 21 of the bond substrate 2. The bonded portion between the surfaces 11 and 21 is a bonding interface 31. The types of the support substrate 1 and the bond substrate 2 are not particularly limited, and can be, for example, semiconductor substrates. More specifically, they can be silicon substrates or compound semiconductor substrates such as SiC substrates and GaN substrates. They can also be single-crystal substrates or polycrystalline substrates. The size and shape of the substrate are also not particularly limited, and can be, for example, a circular substrate with a diameter of 200 mm. They can also be 300 mm or even 450 mm in diameter. Since larger sizes generally lead to more bonding defects, the present invention is more effective in reducing such bonding defects.

[0020] The surface 11 of the support substrate 1 and the surface 21 of the bond substrate 2, which are actually directly bonded to each other, both have an average surface roughness Ra (hereinafter simply referred to as Ra) of 1 nm or less. The Ra value is more preferably 0.9 nm or less, and furthermore, 0.8 nm or less. The smaller the Ra value, the more preferable it is, and the lower limit can be set to 0 nm.

[0021] The method for measuring the average surface roughness Ra is not particularly limited and can be determined on a case-by-case basis. Ra can be measured using a commercially available measuring device. For example, Ra can be a measurement calculated from point cloud data measured with a confocal laser microscope (such as the OPTELICS manufactured by Lasertec) at a viewing angle of 100 μm. Alternatively, Ra can be a measurement obtained using a Keyence VK-X100 series laser microscope at a measurement length of 4 mm. If necessary, measurements can be taken at multiple locations (for example, five locations) to obtain an average value.

[0022] In addition to the above Ra requirement, both surfaces 11, 21 must have an appropriate surface free energy (hereinafter simply referred to as SFE). Here, the SFE is expressed using the contact angle between the surfaces 11, 21 and water as an index of SFE. A specific condition for the contact angle is 70° or less. The contact angle value can be more preferably 66° or less, further 62° or less, 59° or less, or 53° or less. The smaller the contact angle value, the better, and the closer to 0° the better. This is because a good bonding interface 31 can be obtained more reliably.

[0023] For an explanation of the contact angle, refer to Figure 3. A water droplet 102 is attached to a substrate 101 to be measured. The angle formed between the liquid surface of this water droplet 102 and the surface of the substrate 101 to be measured is the contact angle 103. In the upper diagram of Figure 3, the contact angle 103 is about 120°, but in the case of the support substrate 1 and bond substrate 2 of the present invention, the contact angle is 70° or less, as described above. An example of a contact angle of 70° or less is shown in the lower diagram of Figure 3. The larger the SFE, the greater the wettability, the smaller the contact angle, and the more suitable it is for bonding.

[0024] The method for measuring the contact angle is not particularly limited and can be determined on a case-by-case basis. The contact angle can be measured using a commercially available measuring device (for example, a contact angle meter PCA-11 manufactured by Kyowa Interface Science Co., Ltd.). For example, a 2.0 μL droplet of pure water can be dispensed onto a surface at one location from a syringe 104 shown in the upper diagram of FIG. 3, and the contact angle can be determined by image analysis. If necessary, measurements can be taken at multiple locations (for example, five locations) rather than at one location, and the average value can be calculated.

[0025] If the Ra is greater than 1 nm or the contact angle is greater than 70° for both the surface 11 of the support substrate 1 and the surface 21 of the bond substrate 2, the support substrate 1 and the bond substrate 2 cannot be directly bonded, or even if they are directly bonded, partial unbonded portions (voids) are likely to occur at the bonding interface 31 of the bonded substrate 3. On the other hand, if both the Ra and the contact angle satisfy the above conditions, direct bonding is possible, and an extremely good bonding interface 31 with very few or no voids can be obtained. Furthermore, the smaller the Ra and the contact angle, the more reliably the good bonding interface 31 can be obtained.

[0026] As described above, the support substrate 1 and the bond substrate 2 can be made of a base material of a single material such as a silicon substrate, a SiC substrate, or a GaN substrate, but they can also be configured to have a layer of a different material on the surface of such a base material.

[0027] FIG. 4 shows another example of two substrates (support substrate 1 and bond substrate 2). In the example of FIG. 4, a sputtered layer 5 is formed on the surface of the substrate 4 by sputtering a material different from the substrate 4. The entire structure of the substrate 4 and the sputtered layer 5 corresponds to the support substrate 1 and the bond substrate 2. In this case, the surface 51 of the sputtered layer 5 corresponds to the surface 11 of the support substrate 1 and the surface 21 of the bond substrate 21. That is, the surface 51 of the sputtered layer 5 satisfies the above-mentioned numerical conditions for Ra and contact angle. For example, the substrate 4 can be a SiC substrate or a GaN substrate, and the sputtered layer 5 can be a Si layer, but these materials are not particularly limited. An advantage of such a structure is that, even if the surface of the substrate 4 does not satisfy the above-mentioned conditions for Ra and contact angle, the surface can be modified by forming the sputtered layer 5 to obtain a good surface 51 that satisfies the above-mentioned conditions. The sputtered layer 5 is not limited to a single layer, and may be multiple layers. In this case, the Ra and contact angle of the outermost layer must be within the ranges specified in the present invention. Furthermore, the method for forming the layer is not limited to sputtering, and various known methods may be used.

[0028] The following describes a method for manufacturing a bonded substrate and a method for manufacturing a semiconductor device according to the present invention using the support substrate 1 and bond substrate 2 shown in Fig. 2 (or Fig. 4). Fig. 1 shows the flow of the method for manufacturing a bonded substrate and a semiconductor device according to the present invention. Overall, the method comprises the steps of preparing two substrates (step 1), directly bonding the two substrates (manufacturing a bonded substrate) (step 2), and manufacturing a semiconductor device using the bonded substrate (step 3).

[0029] Each step is described below. (Step 1: Preparation of Two Substrates) First, two substrates to be directly bonded are prepared. When preparing these substrates, the Ra and SFE of the surfaces to be directly bonded are used as criteria. More specifically, as described above, substrates are prepared having surfaces with an Ra of 1 nm or less and a contact angle with water (an index of SFE) of 70° or less. That is, a support substrate 1 having a surface 11 shown in FIG. 2 and a bond substrate 2 having a surface 21 are prepared, which satisfy both the Ra and contact angle conditions. Note that the support substrate 1 and the bond substrate 2 may be prepared from a single material, or may be prepared from a base material 4 and a sputtered layer 5 made of a different material, as shown in FIG. 4. For example, a surface condition that satisfies the Ra and contact angle conditions can be adjusted by preparing single-crystal or polycrystalline substrates, polishing them as needed using various polishing devices such as a double-sided polisher or a single-sided polisher, or forming the sputtered layer 5 by sputtering using a target.

[0030] (Step 2: Direct Bonding of Two Substrates) The surface 11 of the support substrate 1 and the surface 21 of the bond substrate 2 (the bond substrate 2 is shown upside down in FIGS. 1 and 2) are bonded together in an opposing relationship to directly bond these surfaces to produce a bonded substrate 3. Because both of the surfaces 11 and 21 to be directly bonded satisfy the above-mentioned conditions for Ra and contact angle, the occurrence of bonding defects can be reduced, and a good bonded substrate 3 with very few voids (or no voids) at the bonded interface 31 can be obtained.

[0031] At this time, if necessary, the bonding strength may be improved by subjecting the bonded substrate 3 to a heat treatment. If it is necessary to thin the bond substrate portion after bonding, this may be done using an existing known technique such as an ion implantation delamination method.

[0032] (Step 3: Manufacturing a Semiconductor Device Using Bonded Substrate) Next, a semiconductor device 6 is manufactured using the bonded substrate 3 manufactured as described above. The desired device can be obtained by appropriately performing various processes such as heat treatment, oxide film formation, etching, and photoresist treatment on the bond substrate portion of the bonded substrate 3. By using the bonded substrate 3, the number of epitaxial growth processes required to manufacture the device layer can be eliminated or reduced, and the semiconductor device 6 can be manufactured at low cost. Furthermore, since the bonded substrate 3 manufactured by the manufacturing method of the present invention has a good and high-quality bonded interface 31, the semiconductor device 6 manufactured can also be of high quality and highly reliable. In other words, reliability can be maintained without concerns about peeling or the like.

[0033] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. (Examples 1-3, Comparative Example 1) A 4H-SiC single crystal substrate having a diameter of 200 mm, a thickness of 355 μm, an n-type, a resistivity of 10 Ω·cm, and an off-angle of 4° relative to the (0001) plane was prepared as a bond substrate. The surface of this substrate was polished using silica as an abrasive, thereby planarizing the surface to an average roughness Ra of 0.8 nm. Ra was a measured value calculated from point cloud data at a viewing angle of 100 μm measured using an OPTELICS manufactured by Lasertec.

[0034] Next, the following substrates were prepared as support substrates. First, a 4H—SiC single crystal substrate identical to the bond substrate was prepared. Furthermore, a poly-SiC substrate of the same size as the bond substrate was prepared. The surfaces of each substrate were polished in the same manner as above to flatten the surface to an Ra of 0.8 nm. Furthermore, a 4H—SiC single crystal substrate identical to the bond substrate was prepared, and its surface was polished in the same manner as above to flatten the surface to an Ra of 0.8 nm, followed by silicon sputtering. The Ra of the surface of the sputtered layer was 0.8 nm. Furthermore, a poly-SiC substrate of the same size as the bond substrate was prepared, and its surface was polished in the same manner as above to flatten the surface to an Ra of 0.8 nm, followed by silicon sputtering. The Ra of the surface of the sputtered layer was 0.8 nm.

[0035] The contact angles of the surfaces of these substrates, (1) 4H—SiC single crystal substrate (for bond substrate, support substrate), (2) poly-SiC substrate (for support substrate), (3) silicon-sputtered 4H—SiC single crystal substrate (for support substrate), and (4) silicon-sputtered poly-SiC substrate (for support substrate), were measured using a contact angle meter PCA-11 manufactured by Kyowa Interface Science Co., Ltd. (using 2 μl of water). Measurements were taken at five locations and the average value was calculated. The contact angle measurement results are shown in FIG. 5. As shown in FIG. 5, only the poly-SiC substrate (2) had a large contact angle of 83°, indicating a small surface free energy. On the other hand, the contact angle of the 4H—SiC single crystal substrate (1) was 53°, while the contact angles of the silicon-sputtered 4H—SiC single crystal substrate (3) and the silicon-sputtered poly-SiC substrate (4) were small, at 62°, indicating a relatively large surface free energy.

[0036] Next, direct bonding of these substrates was attempted in the following combinations: (Example 1) (1) + (1): 4H—SiC single crystal substrates together Ra: both 0.8 nm Contact angles: both 53° (Example 2) (1) + (3): 4H—SiC single crystal substrate and silicon-sputtered 4H—SiC single crystal substrate Ra: both 0.8 nm Contact angles: (1) 53°, (3) 62° (Example 3) (1) + (4): 4H—SiC single crystal substrate and silicon-sputtered poly-SiC substrate Ra: both 0.8 nm Contact angles: (1) 53°, (4) 62° (Comparative Example 1) (1) + (2): 4H—SiC single crystal substrate and poly-SiC substrate Ra: both 0.8 nm Contact angles: (1) 53°, (2) 83°

[0037] Here, assuming that condition A is [Ra is 1 nm or less] and condition B is [contact angle is 70° or less], bonding was possible in Examples 1-3, which satisfied both conditions A and B. Furthermore, when confirmed with an ultrasonic microscope, no areas within the wafer surface (the bonding interface of the bonded substrates) where bonding was not possible were confirmed. On the other hand, bonding was possible in Comparative Example 1, which satisfied condition A but not condition B. However, it was confirmed with an ultrasonic microscope that there were areas within the wafer surface where bonding was not possible. Figure 6 shows an observation diagram of voids, which are areas of poor bonding.

[0038] In the following, (1) 4H—SiC single crystal substrates, (2) poly-SiC substrates, (3) silicon-sputtered 4H—SiC single crystal substrates, and (4) silicon-sputtered poly-SiC substrates with various Ra and contact angles were prepared, and direct bonding was attempted by combining these (Examples 4-6, Comparative Example 2). Direct bonding was attempted under the following conditions. (Example 4) (1) + (1): 4H—SiC single crystal substrates Ra: both 0.9 nm Contact angles: both 56° (Example 5) (1) + (3): 4H—SiC single crystal substrate and silicon-sputtered 4H—SiC single crystal substrate Ra: both 0.9 nm Contact angles: (1) 56°, (3) 66° (Example 6) (1) + (4): 4H—SiC single crystal substrate and silicon-sputtered poly-SiC substrate Ra: both 0.9 nm Contact angles: (1) 56°, (4) 66° (Comparative Example 2) (1) + (2): 4H—SiC single crystal substrate and poly-SiC substrate Ra: both 0.9 nm Contact angles: (1) 56°, (2) 86°

[0039] In Examples 4-6, which satisfied both conditions A and B, bonding was possible. Furthermore, when checked with an ultrasonic microscope, no voids were confirmed within the wafer surface. On the other hand, in Comparative Example 2, which satisfied condition A but did not satisfy condition B, bonding was possible. However, the ultrasonic microscope confirmed the presence of voids within the wafer surface. The number of voids was greater and their size was larger than in Comparative Example 1.

[0040] (Examples 7-9, Comparative Example 3) Direct bonding was attempted under the following conditions: (Example 7) (1) + (1): 4H—SiC single crystal substrates together Ra: 1.0 nm for both Contact angles: 59° for both (Example 8) (1) + (3): 4H—SiC single crystal substrate and silicon-sputtered 4H—SiC single crystal substrate Ra: 1.0 nm for both Contact angles: (1) 59°, (3) 70° (Example 9) (1) + (4): 4H—SiC single crystal substrate and silicon-sputtered poly-SiC substrate Ra: 1.0 nm for both Contact angles: (1) 59°, (4) 70° (Comparative Example 3) (1) + (2): 4H—SiC single crystal substrate and poly-SiC substrate Ra: 1.0 nm for both Contact angles: (1) 59°, (2) 89°

[0041] In Examples 7-9, which satisfied both conditions A and B, bonding was possible. Furthermore, when checked with an ultrasonic microscope, no voids were confirmed within the wafer surface. On the other hand, in Comparative Example 3, which satisfied condition A but did not satisfy condition B, bonding was possible. However, the ultrasonic microscope confirmed the presence of voids within the wafer surface. The number of voids was even greater than in Comparative Example 2, and they were also larger in size.

[0042] Comparative Examples 4-7 Direct bonding was attempted under the following conditions. (Comparative Example 4) (1) + (1): 4H—SiC single crystal substrates together Ra: 1.2 nm for both Contact angles: 62° for both (Comparative Example 5) (1) + (3): 4H—SiC single crystal substrate and silicon-sputtered 4H—SiC single crystal substrate Ra: (1) 1.2 nm, (3) 1.0 nm Contact angles: (1) 62°, (3) 70° (Comparative Example 6) (1) + (4): 4H—SiC single crystal substrate and silicon-sputtered poly-SiC substrate Ra: (1) 1.2 nm, (4) 1.0 nm Contact angles: (1) 62°, (4) 70° (Comparative Example 7) (1) + (2): 4H—SiC single crystal substrate and poly-SiC substrate Ra: (1) 1.2 nm, (2) 1.0 nm Contact angles: (1) 62°, (2) 89°

[0043] Neither Comparative Example 4-6, which satisfied condition B but not condition A, nor Comparative Example 7, which did not satisfy both conditions A and B, could be bonded.

[0044] In addition, GaN single crystal substrates, poly-GaN substrates, silicon-sputtered GaN single crystal substrates, and silicon-sputtered poly-GaN substrates with various Ra and contact angles were prepared, and direct bonding was attempted by combining these. As a result, when both conditions A and B were satisfied, bonding was possible, and no voids were observed within the wafer surface. On the other hand, when even one of conditions A and B was not satisfied, bonding was not possible, or even if bonding was possible, numerous voids were observed within the wafer surface.

[0045] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. A method for manufacturing a bonded substrate by directly bonding the surfaces of two substrates together, comprising the steps of preparing the two substrates based on the average surface roughness Ra and surface free energy of the surfaces to be directly bonded, and directly bonding the two substrates prepared, wherein in the step of preparing the two substrates, substrates are prepared whose surfaces to be directly bonded have an average surface roughness Ra of 1 nm or less, and whose surfaces to be directly bonded have a contact angle with water of 70° or less, which is an index of the surface free energy.

2. The method for manufacturing a bonded substrate as described in claim 1, characterized in that in the step of preparing the two substrates, a substrate is prepared in which the surface free energy of the surface to be directly bonded is adjusted by sputtering a material different from the base material onto the surface of the base material.

3. A method for manufacturing a semiconductor device, comprising the steps of: manufacturing the semiconductor device using a bonded substrate manufactured by the method for manufacturing a bonded substrate according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for manufacturing SOI substrate

    JP2010034523A

  • Semiconductor substrate structure and power semiconductor device

    JP2019210162A

  • Composite substrate, and manufacturing method thereof

    JP2021018998A

  • Semiconductor substrate, manufacturing method thereof, and semiconductor device