Surface-treated metal material and bonded body

The surface-treated metal material with a silane film and adhesive resin layer addresses the reliability issues in adhesive bonding by enhancing adhesion and durability, ensuring robust bonding in transportation equipment, even in challenging conditions.

WO2024237085A1PCT designated stage expired Publication Date: 2024-11-21KOBE STEEL LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016677
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-14
Filing Date
2024-04-30
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Adhesive bonding in transportation equipment faces challenges with strength reliability, particularly in high-temperature, high-humidity environments and under stress, where adhesion between metal and adhesive decreases, leading to corrosion and peeling, and existing surface treatment techniques fail to provide adequate long-term adhesive durability.

Method used

A surface-treated metal material with a silane film formed on the metal base, characterized by a specific absorption spectrum and surface roughness, which enhances adhesion and corrosion resistance, and an adhesive resin layer applied on the silane film to improve bonding strength and durability.

Benefits of technology

The surface-treated metal material exhibits excellent adhesive strength and durability with resins, maintaining bonding integrity even in harsh environments, and the joined body shows improved resistance to water ingress and corrosion, ensuring long-term adhesive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016677_21112024_PF_FP_ABST
    Figure JP2024016677_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a surface-treated metal material which is used for adhesive bonding and is capable of further improving bonding durability; and a bonded body which comprises this surface-treated metal material. This surface-treated metal material is obtained by providing at least a part of the surface of a metal base material with a silane film, wherein: when parallel polarized light having an angle of incidence of 75° is incident on the surface of the silane film and the absorption spectrum is measured by Fourier transform infrared spectroscopy, the surface-treated metal material has an absorption peak in a wavenumber region of 1,250 (cm-1) to 1,150 (cm-1); and if the surface roughness is measured with a laser microscope in any given three 1 mm × 1 mm measurement areas in the surface of the silane film, the aspect ratio is 0.5 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Surface-treated metal materials and joints

[0001] The present invention relates to a surface-treated metal material and a joined body including the surface-treated metal material.

[0002] In the field of transportation such as automobiles, ships and aircraft, adhesive joining is used as a joining technique between dissimilar materials such as steel and lightweight materials (aluminum alloys, titanium alloys, carbon fiber, etc.) from the viewpoint of weight reduction. Also, adhesive joining is attracting attention as an alternative to welding from the viewpoint of improving productivity and workability in response to on-site issues such as a lack of successors for welders, skill transfer, and improving the working environment.

[0003] On the other hand, adhesive bonding has issues with strength reliability during long-term use. It is known that adhesive bonding is more susceptible to strength degradation than welding or bolting in high-temperature, high-humidity environments, and environments where stresses such as fatigue and creep act in combination. In adhesive bonding, adhesion between the adhesive and the metal substrate is important. Insufficient adhesion between the metal material surface and the adhesive allows water to penetrate the interface between the metal and the resin. This results in corrosion of the metal surface and delamination at the interface, significantly reducing adhesive strength. Therefore, improving the adhesion between the metal and the adhesive resin prevents water penetration at the adhesive interface. Furthermore, to prevent water from easily changing the metal surface even if water does penetrate, it is necessary to modify the surface of the metal material to create a surface condition suitable for adhesion.

[0004] To solve the above problems, various surface treatment techniques have been proposed. For example, Patent Document 1 discloses an aqueous composition containing tetraalkyl silicate or its monomeric or oligomeric hydrolysis product and a hydrated oxide sol such as silica sol. By treating metal materials such as aluminum, steel, and titanium with the aqueous composition, the initial adhesion and long-term adhesion stability of coating films such as adhesives formed thereon can be improved.

[0005] Japan Special Publication No. 10-510307

[0006] However, even when the surface treatment technique described in Patent Document 1 is used, the adhesive strength with the resin, such as the adhesive, is significantly reduced after a long-term wet deterioration test, and therefore the required adhesive durability cannot be obtained.

[0007] The present invention has been made in consideration of the above problems, and aims to provide a surface-treated metal material that has excellent adhesive strength with resins such as adhesives and can further improve adhesive durability with resins, and a joined body including this surface-treated metal material.

[0008] The above object of the present invention is achieved by the following configuration [1] relating to a surface-treated metal material.

[0009] [1] A surface-treated metal material having a silane coating on at least a part of the surface of a metal substrate, wherein when parallel polarized light is incident on the surface of the silane coating at an incident angle of 75° and an absorption spectrum is measured by Fourier transform infrared spectroscopy, the absorption spectrum is 1250 (cm -1 ) or more 1150 (cm -1 ) or less, and when the surface roughness of the surface of the silane coating is measured by a laser microscope in a measurement range of 1 mm x 1 mm at any three points on the surface of the silane coating, the aspect ratio is 0.5 or more.

[0010] Furthermore, preferred embodiments of the present invention relating to surface-treated metal materials relate to the following [2] and [3].

[0011] [2] The surface-treated metal material according to [1], characterized in that an adhesive resin layer is provided on the surface of the silane coating.

[0012] [3] The surface-treated metal material according to [1] or [2], characterized in that the absorbance at the absorption peak is 0.003 or more.

[0013] The above object of the present invention can be achieved by the following constitutions [4] and [5] relating to the bonded body.

[0014] [4] A joined body including the surface-treated metal material according to any one of [1] to [3], wherein a first member and a second member are joined via an adhesive resin layer, one of the first member and the second member is the surface-treated metal material, and the silane coating of the surface-treated metal material and the adhesive resin layer are bonded together.

[0015] [5] A joined body including the surface-treated metal material according to any one of [1] to [3], wherein a first member and a second member are joined together via an adhesive resin layer, and both the first member and the second member are the surface-treated metal material having the metal base material made of the same or different metal materials, and the silane coating of the first member and the silane coating of the second member are bonded together by the adhesive resin layer.

[0016] According to the present invention, it is possible to provide a surface-treated metal material that has excellent adhesive strength with resins such as adhesives and can further improve adhesive durability with resins, and a joined body including this surface-treated metal material.

[0017] Fig. 1 is a graph showing an absorption spectrum with the vertical axis representing absorbance and the horizontal axis representing wavenumber. Fig. 2A is a side view showing the shape of the bonded body. Fig. 2B is a plan view showing the shape of the bonded body.

[0018] The present inventors have conducted extensive research into metal materials that can improve the adhesive strength and durability of resins, even for poorly adhesive metal materials such as stainless steel and titanium. As a result, they have found that the above-mentioned problems can be solved by appropriately controlling the absorption spectrum and surface roughness of the surface of a silane coating. The surface-treated metal materials according to embodiments of the present invention will be described in detail below.

[0019] [Surface-treated metal material] The surface-treated metal material according to this embodiment is a metal substrate having a silane coating formed on at least a portion of the surface thereof. The metal substrate and the silane coating will be described in more detail below.

[0020] <Metal Substrate> The metal substrate may be any member made of metal, and there are no particular limitations on its type or shape. Examples of metals include steel sheets, various plated steel sheets, pure aluminum or aluminum alloys, pure titanium or titanium alloys, stainless steel, copper or copper alloys, and the like. In particular, known aluminum alloys, such as Al-Mg alloys, Al-Mg-Si alloys, Al-Zn-Mg alloys, Al-Si alloys, and Al-Cu alloys, can be used. Known titanium alloys, such as α-titanium alloys, β-titanium alloys, and α+β-titanium alloys, can be used. Known stainless steels, such as austenitic stainless steels, ferritic stainless steels, martensitic stainless steels, and duplex stainless steels, can be used.

[0021] <Silane Coating> The silane coating is provided on at least a portion of the surface of the substrate, and specifically, is a surface treatment coating containing an organic silane compound. The silane coating containing the silane compound has excellent bonding properties with adhesives and excellent corrosion resistance, so that the silane coating can maintain excellent bonding strength when adhesively bonded to other members.

[0022] A silane coating can be formed, for example, by applying an aqueous solution containing silicon oxide to the surface of a substrate. Silicon oxide is activated by dissolving it in an aqueous solution and can self-polymerize through a sol-gel reaction. Furthermore, a substrate made of titanium or a titanium alloy has a native oxide coating formed thereon. Therefore, by applying an aqueous solution of silicon oxide to the oxide coating on the surface of the substrate, the titanium oxide coating reacts with the silicon oxide, and the silicon oxide molecules also polymerize with each other, allowing the formation of a silane coating with excellent bonding strength to the substrate in a desired region on the surface of the substrate.

[0023] In addition, silane coatings have high mutual solubility with machine oils such as processing oil and press oil, and organic compounds such as adhesives, and therefore have excellent bonding properties with adhesives. Furthermore, silane coatings can mitigate the effects of machine oils such as processing oil and press oil even when they are attached, preventing a decrease in adhesion durability due to oil application and achieving excellent corrosion resistance.

[0024] (Absorption Spectrum by Fourier Transform Infrared Spectroscopy) When a silane coating is formed on the surface of a metal substrate, silicon-oxygen bonds are inevitably formed in the region where the silane coating is formed. In this embodiment, as an indicator of whether a silane coating has been reliably formed, a method is used in which parallel polarized light is incident on the surface of the silane coating at an incident angle of 75° and the absorption spectrum is measured by Fourier Transform Infrared Spectroscopy (FT-IR).

[0025] 1 is a graph showing an absorption spectrum in which the vertical axis represents absorbance and the horizontal axis represents wavenumber. -1 ) or more 1150 (cm -1 1.) In the wave number region below 1000 Hz, there is an absorption peak as indicated by the arrow in Figure 1. Therefore, by observing the presence or absence of an absorption peak in the above wave number region, it is possible to determine whether or not a silane film has been formed.

[0026] If the absorbance at the absorption peak is 0.003 or more, the presence or absence of a silane coating can be determined more reliably. -1 ) or more 1150 (cm -1 When the compound has an absorption peak in a wave number region of 0.003 or less, the absorbance of the peak is preferably 0.003 or more.

[0027] (Surface Roughness) If the surface shape of a metal substrate is uniformly rough, the metal treatment solution is uniformly retained on the surface of the metal substrate during surface treatment to form a silane coating. As a result, a silane coating with a uniform film thickness is formed, resulting in a silane coating with excellent performance. If the surface shape of the metal substrate is uneven, the metal treatment solution may remain in some areas, such as deep grooves, resulting in a thick silane coating only in the grooves, making it impossible to obtain a silane coating with good performance. Furthermore, if a silane coating is formed with a uniform thickness, the stress applied to the interface when stress is applied to the adhesive bond can be uniformly distributed. In this way, reducing the force applied per unit area can ultimately stabilize the bond strength. Note that the thickness of the silane coating on the surface-treated metal material according to this embodiment is only a few nanometers, so the surface shape of the metal substrate is similarly reflected on the surface of the surface-treated metal material. Therefore, in this embodiment, the surface roughness is defined as the surface roughness of the surface of the surface-treated metal material.

[0028] The surface roughness of the surface-treated metal material can be defined using the surface roughness defined in ISO 25178. In this embodiment, the presence or absence of a silane coating with excellent performance is determined based on Str (aspect ratio of surface texture) when the surface roughness is measured using a laser microscope in a measurement range of 1 mm x 1 mm at three arbitrary locations on the surface of the silane coating. Str takes a value between 0 and 1, and a value close to 0 indicates the presence of streaks and the like, and the surface shape is unevenly rough. On the other hand, a value close to 1 indicates that the surface shape is uniformly rough, independent of direction, and therefore, in this embodiment, Str is preferably close to 1.

[0029] If the aspect ratio is less than 0.5, the surface shape of the metal substrate will be significantly uneven, making it impossible to form a silane coating with a uniform thickness, and therefore it will be impossible to obtain a silane coating with excellent performance. Therefore, the aspect ratio obtained by the above measurement method is set to 0.5 or more, preferably 0.7 or more, and more preferably 0.8 or more.

[0030] One method for uniformly roughening the surface of a surface-treated metal material is to blast the metal substrate. Specifically, the aspect ratio Str can be adjusted by selecting the type of blast material.

[0031] The surface-treated metal material according to this embodiment, configured as described above, has a silane coating provided on at least a portion of the surface of a metal substrate, and the absorption spectrum and aspect ratio of the surface of the silane coating are specified, resulting in a silane coating that has excellent adhesion to the metal substrate and excellent durability.

[0032] Furthermore, the silane coating has high mutual solubility with machine oils such as processing oil and press oil, and organic compounds such as adhesives, and therefore has excellent bonding strength with adhesives. Furthermore, the silane coating can mitigate the effects of machine oils such as processing oil and press oil, even if they are attached, thereby preventing a decrease in adhesion durability due to oil application and achieving excellent corrosion resistance. Therefore, when the surface-treated metal material obtained by the manufacturing method according to this embodiment is adhesively bonded to another member, excellent bonding strength can be maintained for a long period of time.

[0033] <Adhesive Resin Layer> The surface-treated metal material according to this embodiment may further have an adhesive resin layer on the surface of the silane coating. As described above, by having an adhesive resin layer on the surface of the silane coating, which has excellent bondability to adhesives and durability, it is possible to simplify the process of adhesively joining the surface-treated metal material according to this embodiment to similar surface-treated metal materials or other members.

[0034] The method for forming an adhesive resin layer on at least a portion of the surface of the silane coating is not particularly limited. For example, an adhesive sheet made in advance from an adhesive resin material may be attached to the surface of the silane coating, or the adhesive resin material may be sprayed or applied to the surface of the silane coating.

[0035] In the present invention, the resin constituting the adhesive resin layer is not particularly limited, and adhesive resins that have conventionally been used to bond titanium or titanium alloy materials can be used, such as epoxy resins, urethane resins, nitrile resins, nylon resins, acrylic resins, etc. The thickness of the adhesive resin layer is also not particularly limited, but from the viewpoint of improving adhesive strength, it is preferably 10 to 500 μm, and more preferably 50 to 400 μm.

[0036] [Method for Producing Surface-Treated Metal Material] The surface-treated metal material according to this embodiment can be produced, for example, as follows.

[0037] <Blasting Process> First, a blasting process is performed on at least a portion of the surface of a metal substrate. Specifically, abrasive grains or a solution containing abrasive grains are projected onto the surface at high speed using compressed air, a motor, or the like. This process removes and cleans contaminants, deposits, and oxide films present on the surface of the metal substrate, forming an uneven shape on the surface region of the metal substrate and allowing the aspect ratio to be adjusted.

[0038] (Type of blasting) The type of blasting in the blasting process is not particularly limited, and either a dry blasting method or a wet blasting method may be used, with similar effects being obtained using either method. For example, using a dry blasting method is preferable from an economical perspective because the equipment is small and versatile. Furthermore, using a wet blasting method reduces heat input to the surface of the metal substrate 1, suppressing the residue of abrasive grains, and is therefore preferable from the perspective of dust prevention and processing stability. Furthermore, the type of abrasive grains is not particularly limited, and commercially available abrasive grains may be used.

[0039] <Deposition step> Next, a metal treatment solution containing a silane compound is applied to the surface area of ​​the metal substrate that has been subjected to the blast treatment. In the deposition step, the metal treatment solution is applied so that an appropriate amount of the main component, mainly the silane compound, is present on the surface of the metal substrate, and examples of the method include spraying, showering, roll coating, brush application, and immersion treatment. Specific examples of the metal treatment solution will be described later.

[0040] <Drying Step> The solvent is then evaporated from the metal treatment solution applied to the surface of the metal substrate, and the metal substrate is dried to promote the reaction between the silane compound and the oxide film and the polymerization of the silane compounds themselves. This results in the formation of a silane film on at least a portion of the surface of the metal substrate, allowing the production of a surface-treated metal material. The drying temperature is not particularly limited, but a temperature of approximately 50 to 100°C, for example, is preferred, as it provides a good balance between productivity and energy consumption. Note that the step of applying the metal treatment solution to the surface of the substrate and the step of drying the surface of the substrate may be repeated two or three times to improve the integrity of the silane film and maximize the adhesive effect between the substrate and the silane film.

[0041] <Adhesive Resin Layer Forming Step> The surface-treated metal material according to this embodiment preferably further has an adhesive resin layer on its surface. Specifically, after the drying step, an adhesive resin layer is formed on the surface of the silane coating. As described above, by forming an adhesive resin layer on the surface of the silane coating, which has excellent adhesive bonding properties and durability, the steps for adhesively bonding the surface-treated metal material to similar surface-treated metal materials or other members can be simplified.

[0042] The method for forming the adhesive resin layer is not particularly limited, but for example, an adhesive sheet made in advance from an adhesive resin material may be attached to the surface of the silane coating, or the adhesive resin material may be sprayed or applied to the surface of the silane coating.

[0043] In the present invention, the resin constituting the adhesive resin layer is not particularly limited, and adhesive resins that have conventionally been used to bond titanium or titanium alloy materials can be used, such as epoxy resins, urethane resins, nitrile resins, nylon resins, acrylic resins, etc. The thickness of the adhesive resin layer is also not particularly limited, but from the viewpoint of improving adhesive strength, it is preferably 10 to 500 μm, and more preferably 50 to 400 μm.

[0044] Hereinafter, metal treatment solutions for forming silane films will be described with specific examples.

[0045] (Metal Treatment Solution) The metal treatment solution may be any solution containing a silane compound. For example, a solvent containing 50% to 99.99% by mass of water and 0% to 50% by mass of an organic solvent can be used. The mass of water relative to the total mass of the solution is more preferably 50% to 99.95% by mass. Note that, from the viewpoint of reducing volatile organic compounds (VOCs) and reducing the risk of explosion, it is preferable that the main component of the solvent is water. However, in order to reduce the surface tension of the metal treatment solution, improve water wettability and coatability, and improve the drying speed, the following organic solvents may be included, for example.

[0046] When an organic solvent is used, various water-soluble solvents such as various alcohols and polyethers, for example, methanol, ethanol, propyl alcohol, butanol (including isomers), glycol solvents, and their ethers can be used.

[0047] The metal treatment solution preferably contains a silane compound in a content of 0.01% by mass or more and 1% by mass or less, and the silane compound preferably includes an alkyl silicate or its oligomer and a hydrolyzate or polymer of an organosilane compound. The concentration of the silane compound relative to the total mass of the metal treatment solution is more preferably 0.05% by mass or more and 0.5% by mass or less. The concentration of the silane compound can be adjusted based on factors such as the amount of the metal treatment solution to be applied to the surface of the metal substrate. Specifically, the silane compound contained in the metal treatment solution preferably includes an alkyl silicate or its oligomer in a content of 0.005% by mass or more and less than 1% by mass, and a hydrolyzate or polymer of an organosilane compound in a content of 0.005% by mass or more and less than 1% by mass.

[0048] When the specific metal treatment solution described above is applied to at least a portion of the surface of a metal substrate, an alkyl silicate or its oligomer is introduced onto the surface of the substrate, forming a composite oxide film of the metal and silicon that constitute the metal substrate. Then, in a subsequent drying process, a silane film composed of the organosilane compound is formed, in which the organosilane compound and the composite oxide film are chemically bonded. In this way, a surface-treated metal material can be obtained that has excellent adhesive bonding properties, excellent corrosion resistance, and is resistant to deterioration in adhesive strength even when exposed to a high-temperature, humid environment, and has excellent adhesion durability. Furthermore, the use of the metal treatment solution allows surface treatment with the alkyl silicate or its oligomer and surface treatment with the organosilane compound to be performed in a single step, thereby simplifying the production of surface-treated metal materials with excellent adhesion durability and reducing capital investment and production costs.

[0049] The pH of the metal treatment solution is preferably 2 or higher and 7 or lower. A pH higher than 7 is undesirable because the alkyl silicate or its oligomer is more likely to polymerize excessively, potentially reducing the storage stability of the solution. Furthermore, as the polymerization of the alkyl silicate or its oligomer progresses, the resulting coating becomes thicker, causing internal breakdown of the silane coating when stress is applied, making it impossible to obtain high adhesive strength. Therefore, the pH of the metal treatment solution is preferably 7 or lower, and more preferably 6 or lower from the viewpoint of the stability of the alkyl silicate.

[0050] On the other hand, if the pH of the metal treatment solution is lower than 2, the dissolution of the substrate surface will be intense, resulting in a non-uniform coating, making it difficult to achieve stable adhesive performance. Therefore, the pH of the metal treatment solution is preferably 2 or higher, and in consideration of reactivity with the metal oxide coating, a pH of 3 or higher is more preferable. The pH of the metal treatment solution can be appropriately adjusted by adding an acid such as hydrochloric acid, sulfuric acid, nitric acid, or acetic acid.

[0051] The concentration of alkyl silicate or its oligomer in the metal treatment solution is preferably 0.005% by mass or more and less than 1% by mass. If the concentration of alkyl silicate or its oligomer in the metal treatment solution is 1% by mass or more, the resulting coating may become thick and its strength may decrease. Therefore, the concentration of alkyl silicate or its oligomer in the metal treatment solution is preferably less than 1% by mass, more preferably less than 0.5% by mass, and even more preferably less than 0.2% by mass.

[0052] On the other hand, if the concentration of alkyl silicate or its oligomer in the metal treatment solution is less than 0.005% by mass, the concentration of alkyl silicate or its oligomer is too low, making it impossible to form a sufficient composite oxide film of the metal and silicon that constitutes the metal substrate, and there is a risk that sufficient adhesion durability will not be obtained. Therefore, the concentration of alkyl silicate or its oligomer in the metal treatment solution is preferably 0.005% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.02% by mass or more.

[0053] Furthermore, the concentration of the organosilane compound in the metal treatment solution is preferably 0.005% by mass or more and less than 1% by mass. If the concentration of the organosilane compound in the metal treatment solution is 1% by mass or more, the resulting coating may become thick and its strength may decrease. Furthermore, the stability of the solution may also decrease. Therefore, the concentration of the organosilane compound in the metal treatment solution is preferably less than 1% by mass, more preferably less than 0.5% by mass, and even more preferably less than 0.2% by mass.

[0054] On the other hand, if the concentration of the organosilane compound in the metal treatment solution is less than 0.005% by mass, the concentration is too low, making it impossible to form a sufficient surface treatment film containing the organosilane compound, and sufficient adhesion durability cannot be obtained. Therefore, the concentration of the organosilane compound in the metal treatment solution is preferably 0.005% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.02% by mass or more.

[0055] When the mass of alkyl silicate or its oligomer contained as the silane compound in the metal treatment solution is X and the mass of the hydrolyzate or polymer of the organosilane compound is Y, the ratio of X to Y is preferably 4:1 to 1:4. Furthermore, the ratio of X to Y is more preferably 2:1 to 1:2. In order to control the polymerization of these substances and stabilize the metal treatment solution, the metal treatment solution preferably contains 1 mass % or less of an acid relative to the total mass of the silane compound.

[0056] In order to exhibit sufficient adhesion durability in a silane coating composed of an alkyl silicate or its oligomer and a hydrolyzate or polymer of an organic silane compound, it is preferable to adjust the coating amount to an optimum range. 2 If the coating amount of the silane coating is less than 20 mg / m, the metal surface cannot be sufficiently covered with the coating, and it may be difficult to obtain the desired adhesion durability. 2 If the coating amount of the silane coating exceeds 0.1 mg / m, the silane coating becomes bulky, resulting in insufficient adhesion of the silane coating to the metal substrate, which may cause breakage originating from the silane coating, making it difficult to obtain the desired adhesive strength. 2 20mg / m or more 2 It is preferable that the concentration is 0.5 mg / m or less. 2 15mg / m or more 2 By preparing a metal treatment solution with the ratio of X to Y in the metal treatment solution designed to fall within the above range, a preferred coating amount of the silane coating can be achieved.

[0057] The type of alkyl silicate or its oligomer contained in the metal treatment solution is not particularly limited, but silicates, tetraalkoxy orthosilicates, or their oligomers are preferred from the viewpoint of not producing by-products that may cause corrosion of the coating or deterioration of the adhesive resin after the reaction. Among these, tetraethyl orthosilicate (TEOS) or its polymers (oligomers) are preferred because they are neutral and do not leave any alkali residue after the silane coating is formed. Polymers include oligomers. Here, the alkyl silicates or their oligomers may be used alone or in combination of two or more.

[0058] The type of organosilane compound contained in the metal treatment solution is not particularly limited, but the organosilane compound may include a silane compound having multiple hydrolyzable trialkoxy groups in the molecule, its hydrolysate, or a polymer thereof. Silane compounds having multiple hydrolyzable trialkoxy groups in the molecule not only form dense siloxane bonds by self-polymerization, but also have high reactivity with metal oxides, forming chemically stable bonds, thereby further enhancing the durability of the silane coating. Furthermore, silane coatings have high mutual solubility with machine oils such as processing oil and press oil, and organic compounds such as adhesives. Therefore, even if machine oils such as processing oil and press oil adhere to the coating, the effects of such oils can be mitigated, thereby preventing a decrease in adhesion durability due to oil application. The type of the silane compound is not particularly limited, but from an economical viewpoint, a silane compound having two hydrolyzable trialkoxysilyl groups in the molecule (bissilane compound) is preferred, and for example, bistrialkoxysilylethane, bistrialkoxysilylbenzene, bistrialkoxysilylhexane, bistrialkoxysilylpropylamine, bistrialkoxysilylpropyltetrasulfide, etc. can be used. In particular, from the viewpoints of versatility, economical efficiency, and aqueous solution stability, it is preferable to use bistrialkoxysilylethane, and it is even more preferable to use bistriethoxysilylethane (BTSE). Here, as the organic silane compound, only one type may be used alone, or two or more types may be used in combination.

[0059] In addition, the organic silane compound may contain a silane coupling agent having a reactive functional group capable of chemically bonding with an organic resin component, its hydrolyzate, or its polymer.For example, a silane coupling agent having a reactive functional group such as an amino group, an epoxy group, a methacrylic group, a vinyl group, or a mercapto group can be used alone or in combination with a silane compound to form a chemical bond between the coating and the resin, thereby further improving adhesion durability.The functional group of the silane coupling agent is not limited to those described above, and silane coupling agents having various functional groups can be appropriately selected and used depending on the adhesive resin used. Specific preferred examples of the silane coupling agent include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(N-aminoethyl)-aminopropyltrimethoxysilane, 3-(N-aminoethyl)-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, etc. Here, as the silane coupling agent, only one type may be used alone, or two or more types may be used in combination.

[0060] In this embodiment, if the metal treatment solution contains particulate inorganic compounds with a diameter of 10 nm or more (hereinafter simply referred to as "particulate inorganic compounds"), an additional process, such as water washing, is required to remove the silane coating after the silane coating is formed. Furthermore, the silane coating formed may be thick, potentially reducing the adhesive strength and durability. Therefore, it is preferable that the metal treatment solution is substantially free of particulate inorganic compounds. Note that "the metal treatment solution is substantially free of particulate inorganic compounds" does not necessarily mean that the solution is completely free of particulate inorganic compounds; it is acceptable for the solution to contain particulate inorganic compounds at impurity levels. Specifically, it is acceptable for the metal treatment solution to contain up to 0.05% by mass of particulate inorganic compounds relative to the total amount of the metal treatment solution. Examples of particulate inorganic compounds include sols of inorganic oxides such as silica and alumina. The diameter of the particulate inorganic compounds refers to the diameter measured by observing the solid content of the treatment solution after drying using a transmission electron microscope (TEM) or by measuring the diluted treatment solution using a liquid particle counter.

[0061] In addition to the alkyl silicate or its oligomer, and the organosilane compound, the metal treatment solution may further contain, as necessary, one or more stabilizers, adjuvants, etc. For example, the metal treatment solution may contain, as a stabilizer, an organic compound such as a carboxylic acid having 1 to 4 carbon atoms, e.g., formic acid or acetic acid, or an alcohol having 1 to 4 carbon atoms, e.g., methanol or ethanol.

[0062] The metal treatment solution may be prepared, for example, by the following preparation method, but is not limited thereto. First, an organosilane compound and a small amount of acetic acid as a catalyst are added to a mixture of water and an alcohol such as ethanol, and the organosilane compound is sufficiently hydrolyzed to form an aqueous solution of the organosilane compound. Next, an aqueous solution of an alkyl silicate or its oligomer is prepared by a similar method, and these two solutions are mixed and then diluted with water to a predetermined concentration to prepare the metal treatment solution. Furthermore, since alkyl silicates and their oligomers are basic and easily polymerized, when a basic compound is used as the organosilane compound, it is preferable to neutralize the organosilane solution with acetic acid or the like before preparing the solution to avoid excessive polymerization of the alkyl silicate or its oligomer when the solutions are mixed.

[0063] [Jointed Structure] The joined structure according to this embodiment includes the surface-treated metal material. Specifically, the joined structure includes a first member and a second member joined together via an adhesive resin layer. At least one of the first member and the second member may be the surface-treated metal material, and the silane coating of the surface-treated metal material is bonded to the adhesive resin layer.

[0064] The bonded structure according to this embodiment configured as described above is less likely to lose adhesive strength and has excellent adhesive durability even when exposed to a high-temperature, humid environment. As described above, only one of the first member and the second member may be the surface-treated metal material according to the present invention, or both may be the surface-treated metal material according to the present invention. When only one of the first members (the first member) is a surface-treated metal material, the other member (the second member) may be a metal material that has not been surface-treated, a resin molded body that has not been surface-treated, or the like. As the surface-treated metal material, various metal materials can be used, including titanium or titanium alloy material, aluminum or aluminum alloy material, copper or copper alloy material, and stainless steel material.

[0065] Furthermore, as the resin molded body, for example, a fiber-reinforced plastic molded body formed from various fiber-reinforced plastics such as glass fiber reinforced plastic (GFRP), carbon fiber reinforced plastic (CFRP), boron fiber reinforced plastic (BFRP), aramid fiber reinforced plastic (AFRP, KFRP), polyethylene fiber reinforced plastic (DFRP), and Zylon fiber reinforced plastic (ZFRP) can be used. By using these fiber-reinforced plastic molded bodies, it is possible to reduce the weight of the joined body while maintaining a certain level of strength.

[0066] In addition to the above-mentioned fiber-reinforced plastics, the resin molded body may also be made of non-fiber-reinforced engineering plastics such as polypropylene (PP), acrylic-butadiene-styrene copolymer (ABS) resin, polyurethane (PU), polyethylene (PE), polyvinyl chloride (PVC), nylon 6, nylon 6,6, polystyrene (PS), polyethylene terephthalate (PET), polyamide (PA), polyphenylene sulfide (PPS), polybutylene terephthalate (PBT), and polyphthalamide (PPA).

[0067] When both the first member and the second member are surface-treated metal materials according to the present invention, the types of metal substrates may be the same or different, and various combinations of metal substrates can be used.

[0068] [Method for Manufacturing Bonded Structure] The bonded structure according to this embodiment can be manufactured by a conventionally known method. For example, an adhesive resin layer may be formed by a known method in the region where the silane coating is formed, and another member may be bonded to the adhesive resin layer so as to come into contact with the adhesive resin layer. The method for forming the adhesive resin layer is not particularly limited. As described above, an adhesive sheet made of an adhesive resin material may be used, or the adhesive resin material may be sprayed or applied to the surface of the silane coating.

[0069] In the above-described embodiment, an example of a surface-treated metal material on which an adhesive resin layer for producing a bonded body is formed is shown, but the present invention is not limited to the above example, and may also be a surface-treated metal material on which a coating film made of paint is formed on at least a portion of the silane coating. In a surface-treated metal material on which a coating film is formed, the adhesion between the stainless steel substrate and the silane coating is excellent, and the bonding between the silane coating and the paint is also excellent, so that the effect of preventing peeling of the paint can be obtained.

[0070] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples and can be practiced with modifications within the scope of the present invention, all of which are included in the technical scope of the present invention. Furthermore, the various production conditions below are merely examples, and the present embodiment is not limited to the following conditions.

[0071] [Manufacturing of Test Materials] <Preparation of Substrates> First, plates made of various metal materials were cut to a length of 100 mm in the longitudinal direction and a width of 25 mm to prepare two metal substrates for each test condition. The types of metal materials are as follows: Aluminum alloy (JIS A7075): plate thickness 3.8 mm Aluminum alloy (JIS A5052): plate thickness 2 mm Pure titanium (JIS Class 1): plate thickness 1.2 mm Stainless steel (JIS SUS304): plate thickness 1 mm

[0072] <Blast Treatment> Next, the evaluation range of the metal substrate was set to 10 mm from the longitudinal end and 25 mm in the width direction, and the substrates of Invention Examples Nos. 1 to 5 and Comparative Examples Nos. 4, 9, and 10 were subjected to dry or wet blast treatment within the evaluation range, followed by rinsing with water for 1 minute. The treatment conditions for the blast treatment were as follows. Note that Comparative Examples Nos. 1 to 3 and 5 to 8, which were not subjected to blast treatment, were only washed with acetone.

[0073] (Dry blasting conditions) Dry blasting equipment: Shot blasting equipment (NAB-3K) manufactured by Nissanki Co., Ltd. Abrasive material: White Morundum abrasive grains: WA#150 manufactured by Showa Denko K.K. Blast pressure: 0.7 (MPa)

[0074] (Wet blasting conditions) Wet blasting equipment: BABY Blast II (model: MBBII-25) manufactured by Maco Corporation Abrasive material: White Morundum abrasive grains manufactured by Showa Denko K.K.: WA#150, WA#320 Air pressure: 0.12 MPa Gun movement speed: 10 mm / sec

[0075] <Formation of silane coating> The substrates of Invention Examples No. 1 to 5 and Comparative Examples No. 5 to 8 were then immersed for 10 seconds at room temperature in a metal treatment solution containing the following silicon compound 1 and silicon compound 2, and then removed from the solution. A silane coating was formed by drying for 60 seconds at 100°C in a fan drying oven, and test materials were obtained.

[0076] (Metal Treatment Solution) Silicon Compound 1: Bistriethoxysilylethane (BTSE) 0.1 g Silicon Compound 2: Tetraethylorthosilicate (TEOS) 0.1 g Ethanol 2.0 g Acetic acid 0.001 g Water 97.8 g

[0077] [Measurement of the surface of the test material] <Measurement of Str (aspect ratio)> For the surface of each test material (surface of the silane coating), the surface roughness was measured in a measurement range of 1 mm x 1 mm at three arbitrary positions (position 1, position 2, position 3) using a laser microscope (Keyence shape analysis laser microscope VK-X150 / 160). The measurement conditions were as follows: the magnification of the objective lens was 20x, the aspect ratio was measured, and the average value of the three positions was calculated.

[0078] <Measurement of absorption spectrum by FT-IR> The absorption spectrum of the surface of each test material (surface of the silane coating) was measured using FT-IR (Fourier transform infrared spectrophotometer: Nicolet Magna-750 spectrometer). Specifically, parallel polarized light was incident at an incident angle of 75°, and the absorption spectrum was measured. -1 ) or more 1150 (cm -1) The presence or absence of absorption peaks in the following wave number ranges was measured. For those with peaks, the absorbance was measured. The manufacturing conditions of the test materials, as well as the measurement results of the aspect ratio and absorbance, are shown in Table 1 below.

[0079] [Manufacturing of Bonded Test Specimen] The two test pieces were then bonded together with an adhesive to obtain a bonded test piece (bonded body). Fig. 2A is a side view showing the shape of the bonded test piece, and Fig. 2B is a plan view thereof. As shown in Figs. 2A and 2B , an adhesive resin layer 35 was formed in the evaluation range on the surface of test piece 31b (second member), and test piece 31a (first member) having the same configuration as test piece 31b was placed on top of this adhesive resin layer 35. The overlap length was 10 mm, and test pieces 31a and 31b were placed so that only a region 10 mm from the end of test piece 31a overlapped with test piece 31b.

[0080] For Invention Examples 1-5 and Comparative Examples 5-8, a silane coating was formed in the evaluation area. Therefore, the 10 mm x 25 mm areas where the silane coating was formed were arranged facing each other, with adhesive resin layers 35 interposed between them. A structural thermosetting epoxy resin adhesive was used as the adhesive resin layer material. A small amount of glass beads (particle size 250 μm) was added to the adhesive resin material to adjust the thickness of the adhesive resin layer 35 to 250 μm. After stacking and arranging the specimens as described above, they were dried at room temperature for 30 minutes and then heated at 180°C for 30 minutes for a thermal curing treatment. The specimens were then left to stand at room temperature for 24 hours to prepare bonded specimens (bonded specimens).

[0081] For Comparative Examples 1 to 3 and 5 to 8, the specimens were arranged with the acetone-cleaned surfaces facing each other, with adhesive resin layer 35 interposed therebetween, and bonded specimens were prepared in the same manner as above. For Comparative Examples 4, 9, and 10, the specimens were arranged with the blast-treated surfaces facing each other, with adhesive resin layer 35 interposed therebetween, and bonded specimens were prepared in the same manner as above.

[0082] [Evaluation of Bonded Test Specimens] <Degradation Test> A degradation test was carried out on some of the obtained bonded test specimens to evaluate adhesion durability. The degradation test consisted of immersing the bonded test specimens in a 5% NaCl solution at 40°C for the period shown in Table 1 below.

[0083] <Tensile Test> A tensile test was performed on the resulting bonded specimen to evaluate its adhesiveness. The tensile conditions were as follows: both ends of the bonded specimen were pulled in the tensile direction indicated by the arrows in FIG. 2A at a tensile speed of 50 mm / min until fracture. The fracture surfaces of the surface-treated metal material 31a (first member) and the surface-treated metal material 31b (second member) were then observed, and the area of ​​the region where interfacial peeling occurred between the surface-treated metal material 31a and the adhesive resin layer (interfacial peeling area of ​​the first member) and the area of ​​the contact surface between the surface-treated metal material 31a and the adhesive resin layer (adhesion area of ​​the first member) were measured. Similarly, the area of ​​the region where interfacial peeling occurred between the surface-treated metal material 31b and the adhesive resin layer (interfacial peeling area of ​​the second member) and the area of ​​the contact surface between the surface-treated metal material 31b and the adhesive resin layer (adhesion area of ​​the second member) were measured. The cohesive failure rate was then calculated using the following formula (2). The conditions of the degradation test and the calculation results of the cohesive failure rate are shown in Table 1 below.

[0084] Cohesive failure rate (%)=100−{(interfacial peeling area of ​​first member / adhesion area of ​​first member)×100+(interfacial peeling area of ​​second member / adhesion area of ​​second member)×100} (2)

[0085]

[0086] As shown in Table 1 above, Invention Examples Nos. 1 to 5 are examples using specimens with a silane coating on the surface, and because the average aspect ratio was within the range specified in the present invention and the absorption peak was in a predetermined range, they showed an excellent cohesive failure rate regardless of the type of substrate. Furthermore, even after immersion in a NaCl solution, they showed an excellent cohesive failure rate, indicating excellent adhesion durability.

[0087] On the other hand, in Comparative Example No. 1, a silane coating was not formed, the average aspect ratio was outside the range specified by the present invention, and there was no absorption peak in the specified range, resulting in a low cohesive failure rate after the degradation test. In Comparative Example No. 2, a silane coating was not formed, and the average aspect ratio was outside the range specified by the present invention, resulting in a low cohesive failure rate after the degradation test. In Comparative Example No. 3, a silane coating was not formed, and there was no absorption peak in the specified range, resulting in a low cohesive failure rate even when immersion in the degradation test was not performed. In Comparative Example No. 4, a silane coating was not formed, and there was no absorption peak in the specified range, resulting in a low cohesive failure rate after the degradation test.

[0088] Comparative Examples 5, 6, and 8 had a silane coating and an absorption peak in the specified range, but the average aspect ratio was outside the range specified by the present invention, resulting in a low cohesive failure rate after the degradation test. Comparative Example 7 had a silane coating and an absorption peak in the specified range, but the average aspect ratio was outside the range specified by the present invention, resulting in a low cohesive failure rate even when the degradation test was not performed by immersion. Comparative Examples 9 and 10 had an average aspect ratio within the range specified by the present invention, but no silane coating was formed, resulting in no absorption peak in the specified range, resulting in a low cohesive failure rate after the degradation test.

[0089] Although various embodiments have been described above, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can conceive of various modifications or alterations within the scope of the claims, and it is understood that these also naturally fall within the technical scope of the present invention. Furthermore, the components of the above embodiments may be combined in any manner as long as they do not deviate from the spirit of the invention.

[0090] This application is based on a Japanese patent application filed on May 15, 2023 (Patent Application No. 2023-080411) and a Japanese patent application filed on February 14, 2024 (Patent Application No. 2024-020418), the contents of which are incorporated by reference into this application.

[0091] 31a: Surface-treated metal material (first member) 31b: Surface-treated metal material (second member) 35: Adhesive resin layer

Claims

1. A surface-treated metal material having a silane coating on at least a portion of the surface of a metal substrate, wherein when parallel polarized light having an incident angle of 75° is incident on the surface of the silane coating and the absorption spectrum is measured by Fourier transform infrared spectroscopy, the absorption spectrum is 1250 (cm -1 ) or more 1150 (cm -1 ) or less, and when the surface roughness of the surface of the silane coating is measured by a laser microscope in a measurement range of 1 mm x 1 mm at any three points on the surface of the silane coating, the aspect ratio is 0.5 or more.

2. The surface-treated metal material according to claim 1, characterized in that an adhesive resin layer is provided on the surface of the silane coating.

3. The surface-treated metal material according to claim 1, wherein the absorbance at the absorption peak is 0.003 or more.

4. A bonded body including the surface-treated metal material according to any one of claims 1 to 3, characterized in that a first member and a second member are bonded together via an adhesive resin layer, one of the first member and the second member is the surface-treated metal material, and the silane film of the surface-treated metal material is bonded to the adhesive resin layer.

5. A bonded body comprising the surface-treated metal material according to any one of claims 1 to 3, characterized in that a first member and a second member are bonded together via an adhesive resin layer, the first member and the second member are both surface-treated metal materials having metal base materials made of the same or different metal materials, and the silane coating of the first member and the silane coating of the second member are bonded together by the adhesive resin layer.

Citation Information

Patent Citations

  • surface treatment composition

    JP1998510307A

  • Image forming apparatus, and image forming system

    JP2023080411A

  • Drive circuit and display device using the same

    JP2024020418A

  • Aluminum alloy article, aluminum alloy member, and method for producing the same

    JP2013083005A

  • Underlayer treatment solution, method for manufacturing organic coated galvanized steel pipe using the same and organic coated galvanized steel pipe

    JP2016108629A