Zinc germanate / carbon composite anode material, preparation method therefor, and use thereof
Through the design of zinc germanate/carbon composite anode material, combining zinc germanate wire array with carbon fiber material and filling with nanocarbon gel, the problem of volume expansion of germanium-based materials during lithium ion deintercalation is solved, and the stability of the material is improved and battery performance.
Patent Information
- Application Number
- PCT/CN2023/095825
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-28
AI Technical Summary
The volume expansion and structural failure of germanium-based anode material during the lithium ion deintercalation process lead to low cyclic stability, affecting its application value.
Using zinc germanate/carbon composite anode material, the composite structure formed by combining the zinc germanate wire array with two-dimensional planar carbon fiber material, and filling the zinc germanate wire array with nanocarbon gel and coating lithium supplement agent. Laser beam modification is used to form a wire array material of consistent thickness to increase conductivity and battery performance.
The capacity, first-time Coulomb efficiency and rate performance of zinc germanate/carbon composite anode material is improved, the volume effect during lithium ion deintercalation is alleviated, and the structural stability and battery cycling performance of the material are enhanced.
Smart Images

Figure CN2023095825_28112024_PF_FP_ABST
Abstract
Description
Zinc germanate / carbon composite negative electrode material and its preparation method and application Technical Field
[0001] The present disclosure belongs to the technical field of lithium-ion batteries, and particularly relates to a zinc germanate / carbon composite negative electrode material and a preparation method and application thereof. Background Art
[0002] As we all know, electrode materials are one of the key factors affecting the electrochemical performance of lithium-ion batteries. Therefore, developing suitable high-performance electrode materials is an important strategy to improve the performance of lithium-ion batteries. Traditional embedded graphite anode materials cannot further improve the energy density of lithium-ion batteries due to their ultra-low discharge capacity. New conversion and alloy anode materials have become candidates for the next generation of high-energy-density anode materials due to their multi-electron reactions and high theoretical capacity.
[0003] Germanium, with its abundant resources, low cost, high theoretical lithium storage capacity, and suitable lithium deintercalation voltage, is a promising material for commercial applications. However, unlike carbon anode materials, germanium repeatedly contracts and expands during lithium deintercalation and insertion, which can easily lead to loss of electrical contact and deactivation of the anode material, significantly reducing the application value of germanium-based anode materials. The key to improving their cycling stability is to develop a suitable electrode system to mitigate the volume expansion and structural damage caused by lithium ion deintercalation and insertion.
[0004] Summary of the Invention
[0005] The present disclosure aims to at least address the technical problems existing in the aforementioned prior art. To this end, the present disclosure proposes a zinc germanium oxide / carbon composite anode material, its preparation method, and its application. By combining a germanium-based anode material with a carbon material, a highly stable array-type zinc germanium oxide / carbon composite anode material is synthesized. Compared to traditional graphite anode materials, this composite offers greater capacity, higher first coulombic efficiency, and greater rate capability.
[0006] According to one aspect of the present disclosure, a zinc germanate / carbon composite negative electrode material is proposed, which includes a base material and a zinc germanate wire array attached to the surface of the base material, wherein the base material is a two-dimensional planar carbon fiber material, the zinc germanate wire array is filled with gel B, and the surface of the zinc germanate wire array is covered with a coating C.
[0007] In some embodiments of the present disclosure, the base material is at least one of a carbon fiber membrane, a carbon fiber sheet, a carbon fiber felt, a graphite fiber sheet, a graphite fiber membrane, a polymer carbonized fiber membrane, or a polymer carbonized fiber sheet. Alternatively, the carbon fiber membrane is a spun carbon fiber membrane, and the carbon fiber sheet is a spun carbon fiber sheet. Alternatively, the base material is at least one of a graphite fiber sheet, a graphite fiber membrane, or a polymer carbonized fiber membrane.
[0008] In some embodiments of the present disclosure, the carbon content in the base material is ≥80 wt %.
[0009] In some embodiments of the present disclosure, the nanocarbon material is selected from at least one of carbon nanofibers, carbon nanoclusters, oligo-walled carbon nanotubes, single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes. As a conductive agent, the nanocarbon material can improve electrical conductivity.
[0010] In some embodiments of the present disclosure, the lithium supplement is at least one of n-butyl lithium, lithium carbonate, lithium fluoride, biphenyl lithium, lithium powder, lithium oxide or lithium sulfide.
[0011] In some embodiments of the present disclosure, the thickness of the zinc germanate / carbon composite negative electrode material is 0.5-65 μm.
[0012] In some embodiments of the present disclosure, the gel B contains nanocarbon materials. Adding nanocarbon materials to the gel B can improve electrical conductivity.
[0013] In some embodiments of the present disclosure, the coating film C contains a lithium replenisher. The coating film C contains a lithium replenisher, which can improve the initial coulombic efficiency of the battery.
[0014] The present disclosure also provides a method for preparing the zinc germanate / carbon composite negative electrode material, comprising the following steps:
[0015] S1: mixing a substrate material with solution A, heating to perform a seeding reaction, separating the solid from the liquid, and washing the resulting solid to obtain a seeding substrate with a zinc germanium oxide filament array attached to the surface; the solution A is an aqueous solution of zinc formate and germanium hydroxide;
[0016] S2: Flattening the seeding substrate, irradiating the surface of the zinc germanium filament array with a laser beam to make the thickness of the zinc germanium filament array uniform, and washing to obtain a modified seeding substrate;
[0017] S3: placing the modified seeding substrate in gel B for ultrasonic treatment, and then coating the surface of the zinc germanium wire array on one side of the modified seeding substrate with coating C, drying and cold pressing to obtain the zinc germanium oxide / carbon composite negative electrode material; the coating C forms the coating film C after drying.
[0018] The principle of the inoculation reaction in step S1 is as follows: when first heated, zinc formate hydrolyzes to produce hydroxide ions, and germanium hydroxide separates germanium ions and hydroxide ions. When the temperature rises, water molecules are removed to obtain germanium oxide. Germanium oxide and zinc ions gradually generate zinc germanate particles in an alkaline environment and deposit on the surface of the substrate material. As the dehydration time increases, germanium ions deposit on the zinc germanate particles, gradually forming columnar zinc germanate. Due to the high concentration difference of germanium ions associated with the boundary of the columnar zinc germanate, zinc germanate particles are gradually formed and deposited on the columnar zinc germanate, turning the columnar zinc germanate into nanowire zinc germanate. The deposited zinc germanate particles are then used as seeds to promote the growth of zinc germanate micro-nanowires, gradually forming long-fiber zinc germanate, and multiple long-fiber zinc germanate wire arrays.
[0019] In step S2, the lowest point in the layer of the zinc germanium filament array is used as the reference point for thickness (the lowest point in the layer refers to the height of the shortest zinc germanium filament in the zinc germanium filament array). A high-power-density laser beam is used to translate the zinc germanium filament array parallel to the two-dimensional plane of the inoculation substrate. At high temperature, the zinc germanium filament array material is pyrolyzed and detached at the contact point with the laser beam. In this way, the surface of the zinc germanium filament array of varying lengths on the inoculation substrate is modified by laser cutting to make the thickness of the zinc germanium filament array uniform.
[0020] In some embodiments of the present disclosure, in step S1, the germanium hydroxide is at least one of germanium dihydroxide or germanium tetrahydroxide.
[0021] In some embodiments of the present disclosure, in step S1 , the thickness of the base material is 0.5-30 μm.
[0022] In some embodiments of the present disclosure, in step S1, the molar volume ratio of zinc formate, germanium hydroxide and water in the solution A is (1-3) mol: (4.5-12) mol: (10-30) L.
[0023] In some embodiments of the present disclosure, in step S1, the heating temperature is 150-280° C., the heating time is 10-30 hours, and the generated gas is extracted during the heating process.
[0024] In some embodiments of the present disclosure, in step S1, the washing is performed using an organic solvent, and the organic solvent is at least one of methanol, ethanol, acetone or ethylene glycol.
[0025] In some embodiments of the present disclosure, in step S1, the inoculation reaction is followed by cooling with water at 0-5°C.
[0026] In some embodiments of the present disclosure, in step S2, the thickness of the zinc germanium filament array after the laser beam translation irradiation is 1-95 μm.
[0027] In some embodiments of the present disclosure, in step S2, the rinsing is to use deionized water to rinse away excess zinc germanium filaments adhering to the gaps between the zinc germanium filament arrays. The excess zinc germanium filaments between the zinc germanium filament arrays are zinc germanium filaments that fall off after the laser beam is translated and irradiated.
[0028] In some embodiments of the present disclosure, in step S3, the gel B is formed by mixing the nano-carbon material, the first binder, and the first solvent in a mass ratio of (0.8-5): (0.1-3): (6-9).
[0029] In some embodiments of the present disclosure, in step S3, the first binder is at least one of styrene-butadiene latex, chitosan, polyethylene glycol, or polyvinylidene fluoride.
[0030] In some embodiments of the present disclosure, in step S3, the first solvent is at least one of polyacrylamide or glutaraldehyde.
[0031] In some embodiments of the present disclosure, in step S3, after the ultrasonic treatment, the amount of gel B contained in the modified seeding substrate is 1%-12% of the mass of the modified seeding substrate.
[0032] In some embodiments of the present disclosure, in step S3, the coating C comprises a second binder, a third binder, the lithium replenisher, and a second solvent, wherein the mass ratio of the second binder, the third binder, and the lithium replenisher is (2-6):(3-10):(0.01-0.05). Optionally, the second solvent is N-methylpyrrolidone.
[0033] In some embodiments of the present disclosure, in step S3, the second binder is at least one of polyfurfuryl alcohol or polyethylene glycol.
[0034] In some embodiments of the present disclosure, in step S3, the third binder is at least one of sodium alginate, lithium alginate, sodium carboxymethyl cellulose, carboxymethyl cellulose, polyacrylic acid, sodium polyacrylate, or lithium polyacrylate. The second binder and the third binder are hydroxyl-containing and carboxyl-containing binders, respectively, which can synergistically enhance viscosity.
[0035] In some embodiments of the present disclosure, in step S3, the coating amount of the coating C accounts for 0.5%-2.0% of the mass of the modified seeding substrate.
[0036] The present disclosure also provides a negative electrode plate, comprising a current collector and the zinc germanate / carbon composite negative electrode material disposed on a surface of the current collector.
[0037] The present disclosure also provides a method for preparing the negative electrode sheet, which comprises spreading the zinc germanate / carbon composite negative electrode material flat on a current collector with an adhesive, drying, and cold pressing to obtain the negative electrode sheet.
[0038] In some embodiments of the present disclosure, the binder is at least one of sodium carboxymethyl cellulose, guar gum, styrene-butadiene rubber, polyacrylic acid, polytetrafluoroethylene, polyimide, polyvinyl alcohol, or polyacrylonitrile.
[0039] In some embodiments of the present disclosure, the amount of the binder used is 0.8%-5% of the mass of the zinc germanate / carbon composite negative electrode material.
[0040] According to the embodiments of the present disclosure, there are at least the following beneficial effects:
[0041] 1. Compared with the graphite negative electrode material obtained by mixing powdered graphite negative electrode material with a binder, in the negative electrode material in the shape of a wire array disclosed in the present invention, larger pores are left between the fibers or micro-nanowires on the seeding substrate, which is conducive to the flow, infiltration and retention of the electrolyte, shortens the lithium ion transmission distance, etc., and provides sufficient space to alleviate the volume effect during germanium alloying.
[0042] 2. The present invention uses laser cutting and modification, a fast and precise processing method, to maintain the same length of each fiber or micro-nanowire on the inoculated substrate, so that the prepared wire array type zinc germanium oxide / carbon composite negative electrode material has a consistent thickness, so that this alloy type negative electrode material (wire array type zinc germanium oxide / carbon composite negative electrode material) has a consistent orientation when the endpoint begins to be lithiated, avoiding the situation where the degree of lithiation is uneven due to inconsistent orientation, and some surface areas are not lithiated.
[0043] 3. Each tiny unit of the zinc germanium oxide wire array disclosed herein is a micro-nano long rod of zinc germanium oxide. Since there are pores between each long rod of zinc germanium oxide, and more circumferential stress and less longitudinal stress are generated during the lithiation (lithiation) process, the lateral expansion size of the long rod of zinc germanium oxide is much larger than the longitudinal size, and the outer wall expansion is greater than the inner wall expansion. The outer wall of the long rod of zinc germanium oxide is more likely to expand, which requires a buffer material to accommodate the release of stress. Therefore, by adding a filler gel B with low rheology to the zinc germanium oxide wire array, the release of the outer wall stress and the expansion stress of the inner wall can be accommodated, thereby effectively alleviating the volume change of the long rod of zinc germanium oxide and improving the structural stability of the long rod of zinc germanium oxide or the wire array. In addition, there are many pores between the wire array type zinc germanium oxide / carbon composite negative electrode materials, and the compaction density of the resulting negative electrode sheet is too small. The internal resistance of the battery increases significantly during the charge and discharge cycle, which reduces the electrical performance. Therefore, more pore filler gel B is left between the wire arrays to increase the density of the wire array type zinc germanium oxide / carbon composite negative electrode material itself, thereby designing the compaction density of the negative electrode sheet within a reasonable range.
[0044] 4. The present invention performs a coating treatment (coating C) on the surface of the wire array to form a thin film with a high viscosity modulus. The thin film does not undergo side reactions when in contact with the electrolyte, has high flexibility, and will not crack during the cutting of the electrode. Therefore, on the one hand, it acts as a protective layer to prevent the material from breaking during germanium alloying, resulting in fragments penetrating the SEI film, diaphragm or excessive polarization at the negative electrode point. On the other hand, it acts as a buffer layer for the entire wire array when it expands due to alloying, reducing the decline of battery capacity and the reduction of battery life. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] The present disclosure is further described below with reference to the accompanying drawings and embodiments, wherein:
[0046] FIG1 is a SEM image of the modified zinc germanium filament array graphite fiber membrane in step (2) of Example 3 of the present disclosure. DETAILED DESCRIPTION
[0047] The following will clearly and completely describe the concept and technical effects of the present disclosure in conjunction with embodiments to fully understand the purpose, features and effects of the present disclosure.
[0048] Example 1
[0049] This embodiment prepares an array-type zinc germanate / carbon composite negative electrode material and a negative electrode plate. The specific process is as follows:
[0050] (1) Inoculation: A two-dimensional planar graphite fiber membrane with a thickness of 18.5 μm was placed in a reactor, and solution A (mixed according to 1 mol of zinc formate, 4.5 mol of germanium dihydroxide, and 10 L of deionized water) was added. The mass ratio of solution A to the graphite fiber membrane was 2:1. The mixture was heated at 230 °C for 24 h and stirred to perform an inoculation reaction. The mixture was cooled to room temperature in deionized water at 2 °C. After solid-liquid separation, the solid was washed with ethanol to obtain a graphite fiber membrane inoculated with a zinc germanium filament array.
[0051] (2) Modification: The graphite fiber membrane seeded with the zinc germanium filament array is flattened, and the lowest point in the zinc germanium filament array layer is used as the reference point for thickness. A high-power density laser beam is used to translate the zinc germanium filament array parallel to the two-dimensional plane of the seeding substrate, so that the zinc germanium filament array material is pyrolyzed and detached at the contact site with the laser beam. The excess zinc germanium filaments adhering to the gaps between the filament arrays are then rinsed with deionized water to obtain a zinc germanium filament array graphite fiber membrane with uniform thickness (modified seeding substrate);
[0052] (3) Filling gel and coating: The zinc germanium wire array graphite fiber membrane is placed in gel B (mixed by carbon nanofibers, styrene-butadiene latex and glutaraldehyde in a mass ratio of 2:1.5:7), ultrasonically filled, and gel B is filled between the wire arrays. After ultrasonic treatment, the amount of gel B contained in the zinc germanium wire array graphite fiber membrane is 0.05 of the mass of the zinc germanium wire array graphite fiber membrane. Then, coating C (mixed by polyfurfuryl alcohol with high viscosity modulus, sodium alginate and lithium carbonate in a mass ratio of 2:3.5:0.02, and the solvent is N-methylpyrrolidone) is coated on the zinc germanium wire array surface on one side of the zinc germanium wire array graphite fiber membrane. The coating amount is 0.01 of the zinc germanium wire array graphite fiber membrane. After drying and rolling at room temperature, an array-type zinc germanium wire / carbon composite negative electrode material with a thickness of 10 μm is obtained.
[0053] (4) Sheet preparation: The uncoated surface of the array-type zinc germanium oxide / carbon composite negative electrode material is spread flat on a current collector with a binder (sodium carboxymethyl cellulose, styrene-butadiene rubber, and polyacrylonitrile mixed in a mass ratio of 1:1.5:2.5). The amount of binder used is 0.008 of the mass of the array-type zinc germanium oxide / carbon composite negative electrode material. After drying and rolling at room temperature until the coating thickness is 5 μm, the array-type zinc germanium oxide / carbon composite negative electrode sheet is obtained.
[0054] Example 2
[0055] This embodiment prepares an array-type zinc germanate / carbon composite negative electrode material and a negative electrode plate. The specific process is as follows:
[0056] (1) Inoculation: A two-dimensional planar graphite fiber membrane with a thickness of 18.5 μm was placed in a reactor, and solution A (mixed according to 1.5 mol zinc formate, 6 mol germanium dihydroxide, and 12 L deionized water) was added. The mass ratio of solution A to graphite fiber membrane was 3:1. The mixture was heated at 245 °C for 18 h and stirred to carry out the inoculation reaction. The mixture was cooled to room temperature in deionized water at 2 °C. After solid-liquid separation, the solid was washed with ethanol to obtain a graphite fiber membrane inoculated with a zinc germanium filament array.
[0057] (2) Modification: The graphite fiber membrane seeded with the zinc germanium filament array is flattened, and the lowest point in the zinc germanium filament array layer is used as the reference point for thickness. A high-power density laser beam is used to translate the zinc germanium filament array parallel to the two-dimensional plane of the seeding substrate, so that the zinc germanium filament array material is pyrolyzed and detached at the contact site with the laser beam. The excess zinc germanium filaments adhering to the gaps between the filament arrays are then rinsed with deionized water to obtain a zinc germanium filament array graphite fiber membrane with uniform thickness (modified seeding substrate);
[0058] (3) Filling gel and coating: The zinc germanium wire array graphite fiber membrane is placed in gel B (mixed by carbon nanofiber, styrene-butadiene latex and glutaraldehyde in a mass ratio of 3:2:8), ultrasonically filled, and gel B is filled between the wire arrays. After ultrasonic treatment, the amount of gel B contained in the zinc germanium wire array graphite fiber membrane is 0.08 of the mass of the zinc germanium wire array graphite fiber membrane. Then, coating C (mixed by polyfurfuryl alcohol, sodium alginate and lithium carbonate in a mass ratio of 3:4.5:0.018, and the solvent is N-methylpyrrolidone) is coated on the zinc germanium wire array surface on one side of the zinc germanium wire array graphite fiber membrane. The coating amount is 0.01 of the zinc germanium wire array graphite fiber membrane. After drying and rolling at room temperature, an array-type zinc germanium wire array / carbon composite negative electrode material with a thickness of 10 μm is obtained.
[0059] (4) Sheet preparation: The uncoated surface of the array-type zinc germanium oxide / carbon composite negative electrode material was spread flat on a current collector with a binder (sodium carboxymethyl cellulose, styrene-butadiene rubber, and polyacrylonitrile mixed in a mass ratio of 1:1.5:2.5). The amount of binder used was 0.008 of the mass of the array-type zinc germanium oxide / carbon composite negative electrode material. After drying and roller pressing at room temperature to a coating thickness of 5 μm, the array-type zinc germanium oxide / carbon composite negative electrode sheet was obtained.
[0060] Example 3
[0061] This embodiment prepares an array-type zinc germanate / carbon composite negative electrode material and a negative electrode plate. The specific process is as follows:
[0062] (1) Inoculation: A two-dimensional planar graphite fiber membrane with a thickness of 18.5 μm was placed in a reactor, and solution A (mixed according to 1.8 mol zinc formate, 6 mol germanium dihydroxide, and 15 L deionized water) was added. The mass ratio of solution A to graphite fiber membrane was 4:1. The mixture was heated at 175 °C for 30 h and stirred to perform an inoculation reaction. The mixture was cooled to room temperature in deionized water at 2 °C. After solid-liquid separation, the solid was washed with ethanol to obtain a graphite fiber membrane inoculated with a zinc germanium filament array.
[0063] (2) Modification: The graphite fiber membrane seeded with the zinc germanium filament array was flattened, and the lowest point in the zinc germanium filament array layer was used as the reference point for thickness. A high-power density laser beam was used to translate the zinc germanium filament array parallel to the two-dimensional plane of the seeding substrate, so that the zinc germanium filament array material was pyrolyzed and fell off at the contact point with the laser beam. The excess zinc germanium filaments adhering to the gaps between the filament arrays were then rinsed with deionized water to obtain a zinc germanium filament array graphite fiber membrane (modified seeding substrate) with uniform thickness (26 μm);
[0064] (3) Filling gel and coating: The zinc germanium wire array graphite fiber membrane is placed in gel B (mixed by carbon nanofiber, styrene-butadiene latex and glutaraldehyde in a mass ratio of 1:2.5:6.5), ultrasonically filled, and gel B is filled between the wire arrays. After ultrasonic treatment, the amount of gel B contained in the zinc germanium wire array graphite fiber membrane is 0.1 of the mass of the zinc germanium wire array graphite fiber membrane. Then, coating C (mixed by polyfurfuryl alcohol, sodium alginate and n-butyl lithium in a mass ratio of 3.5:4.5:0.03, and the solvent is N-methylpyrrolidone) is coated on the zinc germanium wire array surface on one side of the zinc germanium wire array graphite fiber membrane. The coating amount is 0.01 of the zinc germanium wire array graphite fiber membrane. After drying and rolling at room temperature, an array-type zinc germanium wire array / carbon composite negative electrode material with a thickness of 10 μm is obtained.
[0065] (4) Sheet preparation: The uncoated surface of the array-type zinc germanium oxide / carbon composite negative electrode material is spread flat on a current collector with a binder (sodium carboxymethyl cellulose, styrene-butadiene rubber, and polyacrylonitrile mixed in a mass ratio of 1:1.5:2.5). The amount of binder used is 0.008 of the mass of the array-type zinc germanium oxide / carbon composite negative electrode material. After drying and rolling at room temperature until the coating thickness is 5 μm, the array-type zinc germanium oxide / carbon composite negative electrode sheet is obtained.
[0066] Example 4
[0067] This embodiment prepares an array-type zinc germanate / carbon composite negative electrode material and a negative electrode plate. The specific process is as follows:
[0068] (1) Inoculation: A two-dimensional planar polymer carbon fiber membrane with a thickness of 8.5 μm was placed in a reactor, and solution A (mixed according to 1.0 mol zinc formate, 6 mol germanium dihydroxide, and 20 L deionized water) was added. The mass ratio of solution A to graphite fiber membrane was 3:1. The mixture was heated at 264 °C for 12 h and stirred to perform an inoculation reaction. The mixture was cooled to room temperature in deionized water at 4 °C. After solid-liquid separation, the solid was washed with ethanol to obtain a graphite fiber membrane inoculated with a zinc germanium oxide filament array.
[0069] (2) Modification: The graphite fiber membrane seeded with the zinc germanium filament array is flattened, and the lowest point in the zinc germanium filament array layer is used as the reference point for thickness. A high-power density laser beam is used to translate the zinc germanium filament array parallel to the two-dimensional plane of the seeding substrate, so that the zinc germanium filament array material is pyrolyzed and detached at the contact site with the laser beam. The excess zinc germanium filaments adhering to the gaps between the filament arrays are then rinsed with deionized water to obtain a zinc germanium filament array graphite fiber membrane with uniform thickness (modified seeding substrate);
[0070] (3) Filling gel and coating: The zinc germanium wire array graphite fiber membrane is placed in gel B (mixed by carbon nanofibers, styrene-butadiene latex and glutaraldehyde in a mass ratio of 3.5:2.5:9), ultrasonically filled, and gel B is filled between the wire arrays. After ultrasonic treatment, the amount of gel B contained in the zinc germanium wire array graphite fiber membrane is 0.03 of the mass of the zinc germanium wire array graphite fiber membrane. Then, coating C (mixed by polyfurfuryl alcohol, sodium alginate and n-butyl lithium in a mass ratio of 5.5:7.5:0.042, and the solvent is N-methylpyrrolidone) is coated on the zinc germanium wire array surface on one side of the zinc germanium wire array graphite fiber membrane. The coating amount is 0.01 of the zinc germanium wire array graphite fiber membrane. After drying and rolling at room temperature, an array-type zinc germanium wire array / carbon composite negative electrode material with a thickness of 10 μm is obtained.
[0071] (4) Sheet preparation: The uncoated surface of the array-type zinc germanium oxide / carbon composite negative electrode material is spread flat on a current collector with a binder (sodium carboxymethyl cellulose, styrene-butadiene rubber, and polyacrylonitrile mixed in a mass ratio of 1:1.5:2.5). The amount of binder used is 0.008 of the mass of the array-type zinc germanium oxide / carbon composite negative electrode material. After drying and rolling at room temperature until the coating thickness is 5 μm, the array-type zinc germanium oxide / carbon composite negative electrode sheet is obtained.
[0072] Example 5
[0073] This embodiment prepares an array-type zinc germanate / carbon composite negative electrode material and a negative electrode plate. The specific process is as follows:
[0074] (1) Inoculation: A two-dimensional planar polymer carbon fiber membrane with a thickness of 8.5 μm was placed in a reactor, and solution A (mixed according to 3 mol of zinc formate, 12 mol of germanium tetrahydroxide, and 20 L of deionized water) was added. The mass ratio of solution A to graphite fiber membrane was 4.5:1. The mixture was heated at 264 °C for 12 h and stirred to carry out the inoculation reaction. The mixture was cooled to room temperature in deionized water at 4 °C. After solid-liquid separation, the solid was washed with ethanol to obtain a graphite fiber membrane inoculated with a zinc germanium oxide wire array.
[0075] (2) Modification: The graphite fiber membrane seeded with the zinc germanium filament array is flattened, and the lowest point in the zinc germanium filament array layer is used as the reference point for thickness. A high-power density laser beam is used to translate the zinc germanium filament array parallel to the two-dimensional plane of the seeding substrate, so that the zinc germanium filament array material is pyrolyzed and detached at the contact site with the laser beam. The excess zinc germanium filaments adhering to the gaps between the filament arrays are then rinsed with deionized water to obtain a zinc germanium filament array graphite fiber membrane with uniform thickness (modified seeding substrate);
[0076] (3) Filling gel and coating: The zinc germanium wire array graphite fiber membrane is placed in gel B (mixed by carbon nanofibers, styrene-butadiene latex and glutaraldehyde in a mass ratio of 5:3:8.5), ultrasonically filled, and gel B is filled between the wire arrays. After ultrasonic treatment, the amount of gel B contained in the zinc germanium wire array graphite fiber membrane is 0.12 of the mass of the zinc germanium wire array graphite fiber membrane. Then, coating C (mixed by polyfurfuryl alcohol, sodium alginate and n-butyl lithium in a mass ratio of 6:8:0.5, and the solvent is N-methylpyrrolidone) is coated on the zinc germanium wire array surface on one side of the zinc germanium wire array graphite fiber membrane. The coating amount is 0.01 of the zinc germanium wire array graphite fiber membrane. After drying and rolling at room temperature, an array-type zinc germanium wire array / carbon composite negative electrode material with a thickness of 10 μm is obtained.
[0077] (4) Sheet preparation: The uncoated surface of the array-type zinc germanium oxide / carbon composite negative electrode material is spread flat on a current collector with a binder (sodium carboxymethyl cellulose, styrene-butadiene rubber, and polyacrylonitrile mixed in a mass ratio of 1:1.5:2.5). The amount of binder used is 0.008 of the mass of the array-type zinc germanium oxide / carbon composite negative electrode material. After drying and rolling at room temperature until the coating thickness is 5 μm, the array-type zinc germanium oxide / carbon composite negative electrode sheet is obtained.
[0078] Comparative Example 1
[0079] The difference between this comparative example and Example 1 is that the modification of step (2) is not performed.
[0080] Comparative Example 2
[0081] The difference between this comparative example and Example 3 is that the coating in step (3) is not performed.
[0082] Comparative Example 3
[0083] The difference between this comparative example and Example 3 is that the gel filling in step (3) is not performed.
[0084] Test example
[0085] 1. The array-type zinc germanium oxide / carbon composite negative electrode sheets of Examples 1-5 and Comparative Examples 1-3 were placed in a vacuum oven for drying. In the half-cell, a dried array-type zinc germanium oxide / carbon composite negative electrode sheet was used on the negative electrode side, a lithium metal sheet was used as the counter electrode on the positive electrode side, the separator was Celgard 2400, and the electrolyte was 1M LiPF6 in EC, DMC, and DEC (volume ratio of 1:1:1).
[0086] 2. First, punch the dried electrode and weigh it on an electronic analytical balance with a precision of 1 / 100,000. Then, assemble it in a glove box, where the water and oxygen content is kept below 0.5 ppm. Place the electrode into the CR2025 positive electrode casing, then add two drops of electrolyte. Place a 19mm diameter separator and add another drop of electrolyte. Next, place the lithium sheet, gasket, and spring in order, aligning their centers as closely as possible to the center of the battery. Finally, close the negative electrode casing and seal the pre-assembled battery in a battery packaging machine to complete the button cell assembly.
[0087] 3. Compaction density = surface density / thickness of negative electrode sheet (excluding thickness of current collector); expansion rate of negative electrode sheet = (thickness of negative electrode sheet after filling - thickness of negative electrode sheet after drying) / thickness of negative electrode sheet after drying * 100%.
[0088] 4. The charge and discharge performance of the prepared half-cell was tested at 100mA / g using the CT2001A battery testing system.
[0089] Table 1 Compacted density and expansion rate of negative electrode sheets of Examples 1-5 and Comparative Examples 1-3
[0090] Table 2 Initial efficiency and capacity retention of button batteries prepared in Examples 1-5 and Comparative Examples 1-3
[0091] Combining Table 1 and Table 2, it can be seen that compared with Comparative Examples 1-3, Examples 1-5 have a higher compaction density, better initial coulombic efficiency, and better capacity retention, and the appearance of the negative electrode sheet at the 500th cycle remains good with no cracks. Compared with Example 3, the gel is not filled, resulting in a higher material expansion rate. After multiple cycles, the material structure is damaged, which ultimately results in poor cycle performance (as can be seen from the capacity retention at the 500th cycle). Comparative Example 1 has not been modified, and the initial coulombic efficiency, capacity retention, and appearance of the negative electrode sheet at the 500th cycle are all worse than those of Examples 1-5. In short, after modification, gel filling, coating, and other treatments, the electrical performance of the negative electrode sheets of Examples 1-5 has been improved.
Claims
1. A zinc germanate / carbon composite negative electrode material, characterized in that: The zinc germanate / carbon composite negative electrode material includes a base material and a zinc germanate wire array attached to the surface of the base material, the base material is a two-dimensional planar carbon fiber material, the zinc germanate wire array is filled with gel B, and the surface of the zinc germanate wire array is covered with a coating C.
2. The zinc germanate / carbon composite negative electrode material according to claim 1, characterized in that: The base material is at least one of a carbon fiber film, a carbon fiber sheet, a carbon fiber felt, a graphite fiber sheet, a graphite fiber film, a polymer carbonized fiber film or a polymer carbonized fiber sheet.
3. The zinc germanate / carbon composite negative electrode material according to claim 1, characterized in that: The carbon content of the base material is ≥80wt%.
4. The zinc germanate / carbon composite negative electrode material according to claim 1, characterized in that: The nano-carbon material is selected from at least one of carbon nanofibers, carbon nanoclusters, few-walled carbon nanotubes, single-walled carbon nanotubes, double-walled carbon nanotubes or multi-walled carbon nanotubes.
5. The zinc germanate / carbon composite negative electrode material according to claim 1, characterized in that: The lithium supplement agent is at least one of n-butyl lithium, lithium carbonate, lithium fluoride, biphenyl lithium, lithium powder, lithium oxide or lithium sulfide.
6. The zinc germanate / carbon composite negative electrode material according to claim 1, characterized in that: The thickness of the zinc germanate / carbon composite negative electrode material is 0.5-65 μm.
7. The zinc germanate / carbon composite negative electrode material according to claim 1, characterized in that: The gel B contains nanocarbon material.
8. The zinc germanate / carbon composite negative electrode material according to claim 1, characterized in that: The coating film C contains a lithium supplement agent.
9. The method for preparing the zinc germanate / carbon composite negative electrode material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: mixing the substrate material with solution A, heating for inoculation reaction, separating the solid from the liquid, washing the obtained solid, and obtaining an inoculation substrate with a zinc germanate wire array attached to the surface; the solution A is an aqueous solution of zinc formate and germanium hydroxide; S2: Flatten the inoculated substrate, and use a laser beam to translate and illuminate the surface of the zinc germanate wire array. The zinc germanate wire array has a uniform thickness and after washing, a modified seeding substrate is obtained; S3: placing the modified seeding substrate in gel B for ultrasonic treatment, and then coating the coating C on the surface of the zinc germanate wire array on one side of the modified seeding substrate, and drying and cold pressing to obtain the zinc germanate / carbon composite negative electrode material; the coating C forms the coating film C after drying.
10. The preparation method according to claim 9, characterized in that: In step S1, the thickness of the base material is 0.5-30 μm.
11. The preparation method according to claim 9, characterized in that: In step S1, the molar volume ratio of zinc formate, germanium hydroxide and water in the solution A is (1-3) mol: (4.5-12) mol: (10-30) L; and the mass ratio of the solution A to the substrate material is (2-5):
1.
12. The preparation method according to claim 9, characterized in that: In step S1, the heating temperature is 150-280°C, and the heating time is 10-30h.
13. The preparation method according to claim 9, characterized in that: In step S1, the washing is performed using an organic solvent, and the organic solvent is at least one of methanol, ethanol, acetone or ethylene glycol.
14. The preparation method according to claim 9, characterized in that: In step S2, the thickness of the zinc germanate filament array after the laser beam translation irradiation is 1-95 μm.
15. The preparation method according to claim 9, characterized in that: In step S2, the rinsing is: using deionized water to rinse away the excess zinc germanate wires adhering to the gaps between the zinc germanate wire arrays.
16. The preparation method according to claim 9, characterized in that: In step S3, the gel B is formed by mixing the nano-carbon material, the first binder and the first solvent in a mass ratio of (0.8-5): (0.1-3): (6-9).
17. The preparation method according to claim 16, characterized in that: In step S3, the first binder is at least one of styrene-butadiene latex, chitosan, polyethylene glycol or polyvinylidene fluoride.
18. The preparation method according to claim 16, characterized in that: In step S3, the first solvent is at least one of polyacrylamide or glutaraldehyde.
19. The preparation method according to claim 9, characterized in that: In step S3, after the ultrasonic treatment, the amount of gel B contained in the modified seeding substrate is 1%-12% of the mass of the modified seeding substrate.
20. The preparation method according to claim 9, characterized in that: In step S3, the coating C comprises a second binder, a third binder, a lithium supplement agent and a second solvent, and the mass ratio of the second binder, the third binder and the lithium supplement agent is (2-6): (3-10): (0.01-0.05).
21. The preparation method according to claim 20, characterized in that: In step S3, the second binder is at least one of polyfurfuryl alcohol or polyethylene glycol.
22. The preparation method according to claim 20, characterized in that: In step S3, the third binder is at least one of sodium alginate, lithium alginate, sodium carboxymethyl cellulose, carboxymethyl cellulose, polyacrylic acid, sodium polyacrylate or lithium polyacrylate.
23. The preparation method according to claim 9, characterized in that: In step S3, the coating amount of the coating C accounts for 0.5%-2.0% of the mass of the modified inoculation substrate.
24. A negative electrode plate, characterized in that: It comprises a current collector and the zinc germanate / carbon composite negative electrode material according to any one of claims 1 to 8 arranged on the surface of the current collector.
25. A method for preparing the negative electrode sheet according to claim 24, characterized in that: The zinc germanate / carbon composite negative electrode material is flattened on a current collector with a binder, and dried and cold pressed to obtain the negative electrode sheet.
26. The method according to claim 25, characterized in that The binder is at least one of sodium carboxymethyl cellulose, guar gum, styrene-butadiene rubber, polyacrylic acid, polytetrafluoroethylene, polyimide, polyvinyl alcohol or polyacrylonitrile.
27. The method according to claim 25, characterized in that The amount of the binder used is 0.8%-5% of the mass of the zinc germanate / carbon composite negative electrode material.
Citation Information
Patent Citations
Lithium ion battery flexible anode material and preparation method thereof
CN107634206A
Silicon-based composite negative electrode plate, preparation method, and lithium ion secondary battery
CN107799723A
Silicon-based composite negative electrode material for lithium ion battery and preparation method thereof
CN109411730A
Energy storage devices
US20180219222A1