Secondary battery and electric device

By using sulfate ester compounds and fluorobase compounds in secondary batteries to form SEI films and control the composition of electrolytes, the shell deformation and energy density reduction caused by gas generation in the electrical cycle of the secondary battery are solved, and the problem of achieving the Longer service life and higher energy density.

WO2024239342A1PCT designated stage expired Publication Date: 2024-11-28CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/096401
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The secondary battery produces gas by-products during the electrical cycle, causing deformation and shortening of the battery housing. Increasing the housing space to accommodate gas will reduce the energy density, making it difficult to take into account both service life and energy density.

Method used

Using a battery case with a housing cavity, a secondary battery containing an electrolyte solution of sulfate compounds is built into. By controlling the mass content and residual space ratio of the sulfate compounds, an inorganic SEI film is formed to reduce gas generation, and fluorocarbonic acid is used. Ester compounds and sulfonate compounds further reduce side reactions and optimize the composition of the electrolyte to improve service life and energy density.

Benefits of technology

It effectively reduces the internal pressure of the battery case, extends the service life, and improves the energy density, taking into account the safety and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023096401_28112024_PF_FP_ABST
    Figure CN2023096401_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present application are a secondary battery and an electric device. The secondary battery comprises a battery shell having an accommodating cavity, a battery cell assembly located in the accommodating cavity and an electrolyte comprising a first additive, the first additive comprising a sulfate compound, wherein based on the total mass of the electrolyte, a ratio W / R of the mass content W of the sulfate compound to the residual space R within the range of 0.03% to 40% can make the obtained secondary battery take both the service life and the energy density into consideration.
Need to check novelty before this filing date? Find Prior Art

Description

Secondary batteries and electrical devices Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a secondary battery and an electrical device. Background Art

[0002] In recent years, secondary batteries have been widely used in energy storage systems such as portable electronic devices, hydropower, thermal, wind, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. With the goals of achieving peak carbon emissions and achieving carbon neutrality, as well as increasing environmental protection requirements, the development of secondary batteries is driving them towards higher energy density, power performance, and cycle life.

[0003] During the electrical cycle, secondary batteries undergo various chemical reactions that produce gaseous byproducts. This can lead to internal gassing defects within the battery, shortening the battery's lifespan. Increasing the space inside the battery casing for these gaseous byproducts can reduce risks such as casing deformation caused by gassing, extending the battery's lifespan but reducing its energy density. There is a need for a secondary battery that can reduce gassing defects while maintaining both longevity and energy density.

[0004] Summary of the Invention

[0005] In view of the problems existing in the background technology, the present application provides a secondary battery, aiming to take into account both the service life and energy density of the secondary battery.

[0006] In a first aspect of the present application, a secondary battery is provided, comprising a battery housing having a receiving cavity, a battery cell assembly located in the receiving cavity, and an electrolyte comprising a first additive, wherein the first additive is selected from sulfate compounds;

[0007] Wherein, based on the total mass of the electrolyte, the mass content W of the first additive and the residual space R satisfy: 0.03%≤W / R≤40%, optionally 0.03%≤W / R≤20%, and the residual space R is expressed as: Among them, V1 represents the internal volume of the secondary battery housing; V2 represents the volume of the battery cell assembly; V3 represents the volume of the electrolyte; and C represents the discharge capacity of the secondary battery.

[0008] In the secondary battery provided by the present application, the sulfate compound can form an inorganic SEI film (solid electrolyte interphase) at the interface between the electrolyte and the negative electrode plate, effectively reducing the side reactions caused by the contact between the electrolyte and the negative electrode plate, reducing gas generation, and improving the service life of the secondary battery; an appropriate residual space R can provide a certain amount of space for the battery shell to accommodate the gases generated by the battery side reactions, but an increased residual space R can reduce the energy density of the secondary battery. When the mass content W of the sulfate compound and the residual space R meet the above relationship, the battery shell can not only accommodate the gases generated by the side reactions of the electrode plate reduced by the addition of the sulfate compound, but also achieve an increase in energy density, taking into account both the service life and energy density of the secondary battery.

[0009] In any embodiment, the sulfate ester compound includes one or more of 4,4'-vinyl sulfate, vinyl sulfate, diethyl sulfate, dimethyl sulfate, and 4,4-bis(1,3,2-dioxathiolane)-2,2,2,2-tetraoxide, and optionally includes one or more of 4,4'-vinyl sulfate and vinyl sulfate.

[0010] The above-mentioned sulfate compounds can form an inorganic SEI film at the interface between the electrolyte and the negative electrode, effectively reducing the side reactions occurring during the contact between the electrolyte and the negative electrode, reducing gas generation, and improving the service life of the secondary battery.

[0011] In any embodiment, based on the total mass of the electrolyte, the mass content W of the first additive is 0.045% to 2%, and can be optionally 0.1% to 2%.

[0012] Controlling the mass content of the first additive within an appropriate range can not only reduce interfacial side reactions, but also reduce the impact of the introduction of the first additive on the electrolyte, for example, affecting the fast charging and power performance of the secondary battery, while taking into account the service life and electrical performance of the secondary battery.

[0013] In any embodiment, the residual space R is 0.05 mL / Ah to 3 mL / Ah, and can be optionally 0.1 mL / Ah to 1.5 mL / Ah.

[0014] Controlling the residual space R within an appropriate range can not only provide sufficient space for the battery cell components to improve the energy density of the secondary battery, but also provide sufficient space to accommodate the gas generated by the side reactions of the battery cell components, reduce the internal pressure of the battery shell or maintain the internal pressure basically stable, and improve the safety of the secondary battery.

[0015] In any embodiment, the electrolyte includes a second additive, and the second additive is selected from one or more of fluorinated carbonate compounds and sulfonate compounds.

[0016] The second additive comprising one or more fluorocarbonate compounds and sulfonate compounds is beneficial to the formation of an inorganic SEI film rich in LiF and Li2SO3 on the negative electrode side, which is beneficial to further reduce the side reactions occurring due to the contact between the electrolyte and the negative electrode, reduce gas generation, and improve the service life of the secondary battery.

[0017] In any embodiment, the fluorinated carbonate compound includes one or more of fluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate, optionally including fluoroethylene carbonate and 1,2-difluoroethylene carbonate; and / or

[0018] The sulfonate compound includes one or more of 1,3-propane sultone, propene sultone, and 3-fluoro-1,3-propane sultone, and optionally includes 1,3-propane sultone.

[0019] In any embodiment, the second additive includes fluoroethylene carbonate and 1,3-propane sultone. In any embodiment, the second additive includes 1,2-difluoroethylene carbonate and 1,3-propane sultone. The mass ratio of the fluoroethylene carbonate or 1,2-difluoroethylene carbonate to 1,3-propane sultone is (0.1-50):1, and can optionally be (0.1-30):1.

[0020] The above-mentioned fluorinated carbonate compounds and sulfonate compounds can form an inorganic SEI film at the interface between the electrolyte and the negative electrode, effectively reducing the side reactions caused by further contact between the electrolyte and the negative electrode, reducing gas generation, and improving the service life of the secondary battery.

[0021] In any embodiment, based on the total mass of the electrolyte, the mass content W of the first additive and the mass content A of the second additive satisfy: 0.045%≤W+A≤15%, optionally 0.1%≤W+A≤11%.

[0022] W+A satisfies the above relationship, which can not only form a sufficient amount of inorganic SEI film at the interface between the electrolyte and the negative electrode plate to reduce gas generation and increase the service life of the battery; it can also reduce the impact of the introduction of the first additive and the second additive on the fast charging and power performance of the secondary battery, while taking into account the service life and electrical performance of the secondary battery.

[0023] In any embodiment, based on the total mass of the electrolyte, the mass content A of the second additive is 0.05% to 10%, and can be optionally 0.5% to 7%.

[0024] Controlling the mass content of the second additive within an appropriate range can not only reduce interfacial side reactions, but also reduce the impact of the introduction of the second additive on secondary battery performance, such as fast charging and power performance, and can take into account both the service life and electrical performance of the secondary battery.

[0025] In any embodiment, the battery cell assembly includes a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector and including at least a positive electrode active material. The thickness of the positive electrode current collector is 4 μm to 14 μm, and can be optionally 5 μm to 13 μm.

[0026] In any embodiment, the secondary battery includes a negative electrode current collector, and the thickness of the negative electrode current collector is 3 μm to 10 μm, and optionally 4 μm to 8 μm.

[0027] Controlling the thickness of the positive electrode current collector and / or the negative electrode current collector within an appropriate range can not only meet the requirements of mechanical strength and the requirements of electron conduction during charging and discharging; but also release a certain amount of space to accommodate more positive electrode active materials / negative electrode active materials, thereby improving the energy density of the secondary battery, or release a certain amount of space to accommodate the gas in the battery, thereby reducing the internal pressure of the battery case or maintaining the internal pressure basically stable, thereby improving the service life of the secondary battery and reducing the safety hazards of the secondary battery.

[0028] In any embodiment, the filling coefficient of the secondary battery is 1 g / Ah to 3 g / Ah, and can be optionally 1.5 g / Ah to 2.5 g / Ah.

[0029] Controlling the filling coefficient of the secondary battery within an appropriate range can not only provide enough electrolyte to meet the needs of the secondary battery, but also release a certain amount of space to accommodate more positive electrode active materials / negative electrode active materials, thereby improving the energy density of the secondary battery, or release a certain amount of space to accommodate the gas in the battery, thereby reducing the internal pressure of the battery shell or maintaining the internal pressure basically stable, thereby improving the service life of the secondary battery and reducing safety hazards of the shell.

[0030] In any embodiment, the electrolyte includes a solvent, and the solvent includes at least one of a carboxylate solvent, a cyclic carbonate solvent, and a linear carbonate solvent.

[0031] The carboxylate solvent, the cyclic carbonate solvent or the linear carbonate solvent may be used in combination with the first additive and / or the second additive to enable the secondary battery to have an excellent service life and energy density.

[0032] In any embodiment, the solvent includes at least two of the carboxylate solvent, the cyclic carbonate solvent, and the linear carbonate solvent.

[0033] In any embodiment, the mass content X of the cyclic carbonate solvent is 2% to 35% based on the total mass of the solvent.

[0034] In any embodiment, based on the total mass of the solvent, the mass content X of the cyclic carbonate solvent is 20% to 35%, the mass content Y of the linear carbonate solvent is 0% to 75%, and the mass content of the carboxylate solvent is (100%-XY).

[0035] The combination of carboxylate solvents, cyclic carbonate solvents and linear carbonate solvents and controlling the mass content of carboxylate solvents, cyclic carbonate solvents and linear carbonate solvents within an appropriate range helps to reduce the viscosity of the electrolyte, improve the dynamics and wettability of the electrolyte, and provide the battery with an excellent service life.

[0036] In any embodiment, the carboxylate solvent comprises a structure shown in Formula I,

[0037] Wherein, R1 and R2 each independently include C 1-10 Alkyl, optionally, the carboxylate solvent includes one or more of methyl formate, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, isopropyl acetate, and isoamyl acetate; and / or

[0038] The cyclic carbonate solvent includes one or more of ethylene carbonate and propylene carbonate; and / or

[0039] The linear carbonate solvent includes at least one of dimethyl carbonate, diethyl carbonate, methyl propyl carbonate and methyl ethyl carbonate.

[0040] The above substances can be used in combination with the first additive and / or the second additive to ensure that the secondary battery has excellent service life and energy density.

[0041] In any embodiment, the linear carbonate solvent includes two of dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, and methyl ethyl carbonate.

[0042] In any embodiment, the linear carbonate solvent includes dimethyl carbonate and ethyl methyl carbonate, and the mass ratio of dimethyl carbonate to ethyl methyl carbonate is 5:90 to 70:10, and can be optionally 10:80 to 60:10.

[0043] The solvent further includes two linear carbonate solvents and / or controls the two linear carbonate solvents, which can reduce the viscosity of the electrolyte, improve the wettability and dynamics of the electrolyte, and take into account the service life and gas production performance of the battery.

[0044] In any embodiment, the secondary battery includes one or more of a lithium secondary battery, a sodium secondary battery, and a potassium secondary battery.

[0045] A second aspect of the present application provides an electrical device comprising the secondary battery of the first aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0047] FIG2 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG1 ;

[0048] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application;

[0049] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0050] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;

[0051] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0052] Description of reference numerals:

[0053] 1. Battery pack; 2. Upper case; 3. Lower case; 4. Battery module; 5. Secondary battery; 5. Casing; 5. Cell assembly; 5. Cover. DETAILED DESCRIPTION

[0054] Below, the embodiments of the electrolyte, secondary battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0055] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0056] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0057] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0058] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0059] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0060] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0061] Side reactions between the electrolyte and the electrode generate gases that increase the internal pressure of the battery casing, which can easily cause deformation and even shorten the battery's lifespan. This is often achieved by increasing the space in the battery casing not occupied by the cell components and electrolyte to provide sufficient space for gas, thereby reducing internal pressure and improving battery safety and lifespan. However, this also results in a decrease in battery energy density, which cannot meet market demand. Therefore, a new battery design is needed that balances longevity and energy density.

[0062] [Secondary battery]

[0063] Based on this, the present application proposes a secondary battery, comprising a battery housing having a receiving cavity, a battery cell assembly located in the receiving cavity, and an electrolyte comprising a first additive, wherein the first additive is selected from sulfate compounds;

[0064] Wherein, based on the total mass of the electrolyte, the mass content W of the first additive and the residual space R satisfy: 0.03%≤W / R≤40%, and optionally 0.03%≤W / R≤20%. The residual space R is expressed as: Among them, V1 represents the internal volume of the secondary battery housing (ml); V2 represents the volume of the battery cell assembly (ml); V3 represents the volume of the electrolyte (ml); and C represents the discharge capacity of the secondary battery (Ah).

[0065] Herein, “W / R” refers to the ratio of the mass content W to the residual space R (mL / Ah).

[0066] The accommodating cavity generally refers to the internal space of the battery housing. In some embodiments, as shown in FIG2 , the housing 51 may include a bottom plate and side plates connected to the bottom plate, and the bottom plate and the side plates together form the accommodating cavity.

[0067] In this application, the capacity of the secondary battery represented by C is the discharge capacity of the secondary battery. Generally speaking, the capacity of the secondary battery needs to be pre-set during the preparation process to meet different usage scenarios. This pre-set battery capacity is the design capacity. After the secondary battery is prepared, the discharge capacity can be obtained through testing. In some cases, such as during the battery preparation process, the design capacity is used instead of the discharge capacity for material calculation and preparation. In other cases, such as after the battery is freshly prepared, the slight difference between the two is acceptable in this field and the two can be used instead. It is understood that during the battery preparation process, the design capacity can be used as the discharge capacity to adjust the residual space in order to obtain the desired secondary battery. For a secondary battery that has been prepared, the discharge capacity is used to calculate and adjust the residual space of the secondary battery. The test method of the discharge capacity of a secondary battery, or the calculation method of the design capacity of a secondary battery, are both public and known to those skilled in the art.

[0068] In some embodiments, a method for testing the discharge capacity of a single cell in a secondary battery may include: placing the secondary battery in a 25°C environment and allowing it to rest until the battery temperature reaches a constant 25°C; charging the battery at a current of 1 / 3C1 to the charge end voltage; allowing it to rest for 10 minutes; charging the battery at a current of 0.05C1 to the charge end voltage; allowing it to rest for 10 minutes; and discharging the battery at a current of 1 / 3C1 to the discharge end voltage. The discharge capacity at this step is recorded as the battery discharge capacity C at 25°C @ 0.33C1, where C1 is the rated capacity indicated on the battery cell. The rated capacity indicated on the battery cell is also referred to as the rated capacity.

[0069] In the present application, the residual space R can be adjusted by adjusting one or more parameters including V1, V2, V3 and C to obtain the expected residual space R value. In some embodiments, the shell of the secondary battery does not change, and the residual space R can be adjusted by adjusting one or more parameters including V2, V3 and C to obtain the expected residual space R value. In some embodiments, the shell of the secondary battery and the capacity of the battery do not change, and the residual space R can be adjusted by adjusting one or more parameters including V2 and V3 to obtain the expected residual space R value. The value of the residual space R can be adjusted in ways including but not limited to the above-mentioned methods. Based on the common technical knowledge in this field mastered by those skilled in the art, the expected residual space R value can be obtained by adjusting one or more parameters including V1, V2, V3 and C.

[0070] In some embodiments, based on the total mass of the electrolyte, the ratio W of the mass content W of the sulfate compound to the residual space R W / R can be selected to be 0.03%, 0.05%, 0.1%, 0.5%, 1%, 2%, 4%, 5%, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, 22%, 25%, 28%, 30%, 34%, 35%, 36%, 40%, or a value in the range consisting of any two of the above points.

[0071] In some embodiments, based on the total mass of the electrolyte, the mass content W of the first additive and the residual space R satisfy: 0.1%≤W / R≤40%, 0.2%≤W / R≤40%, 0.5%≤W / R≤40%, 1%≤W / R≤40%, 4%≤W / R≤40%, 10%≤W / R≤40%, 0.1%≤W / R≤20%, 0.2%≤W / R≤20%, 0.5%≤W / R≤20%, 1%≤W / R≤20%, and 4%≤W / R≤20%.

[0072] In the secondary battery provided in the present application, the sulfate ester compound can form an inorganic SEI film at the interface between the electrolyte and the negative electrode plate, effectively reducing the side reactions occurring due to the contact between the electrolyte and the negative electrode plate, reducing the pulverization of the negative electrode plate and the generation of gas, reducing the risk of deformation of the battery shell and improving the service life of the secondary battery.

[0073] In a secondary battery, when the residual space R decreases, the space occupied by the battery cell components increases, increasing the secondary battery's energy density. However, this reduces the space available for gas storage within the battery casing, increasing the internal pressure of the battery casing, increasing the risk of casing deformation and shortening the battery cell's lifespan. When the W / R ratio is within the above range, the battery casing not only accommodates the gas generated by the electrode side reactions, which is reduced by the addition of sulfate compounds, but also provides space to accommodate more or larger battery cell components, thereby improving the secondary battery's lifespan and energy density.

[0074] In some embodiments, the sulfate ester compound includes one or more of 4,4'-vinyl sulfate, vinyl sulfate, diethyl sulfate, dimethyl sulfate, and 4,4-bis(1,3,2-dioxathiolane)-2,2,2,2-tetraoxide, and optionally includes one or more of 4,4'-vinyl sulfate and vinyl sulfate.

[0075] In some embodiments, the sulfate ester compound comprises 4,4'-vinyl sulfate. In some embodiments, the sulfate ester compound comprises vinyl sulfate. In some embodiments, the sulfate ester compound comprises dimethyl sulfate. In some embodiments, the sulfate ester compound comprises 4,4-bis(1,3,2-dioxathiolane)-2,2,2,2-tetraoxide. In some embodiments, the sulfate ester compound comprises 4,4'-vinyl sulfate and dimethyl sulfate. In some embodiments, the sulfate ester compound comprises 4,4'-vinyl sulfate.

[0076] The above-mentioned sulfate compounds can form an inorganic SEI film at the interface between the electrolyte and the negative electrode, effectively reducing the side reactions occurring during the contact between the electrolyte and the negative electrode, reducing gas generation, and improving the service life of the secondary battery.

[0077] In some embodiments, based on the total mass of the electrolyte, the mass content W of the first additive is 0.045% to 2%, optionally 0.1% to 2%, 0.05 to 2%, 0.15 to 1.5%, 0.1% to 2%, or 0.5% to 1.5%.

[0078] In some embodiments, based on the total mass of the electrolyte, the mass content W of the first additive can be selected to be 0.05%, 0.1%, 0.15%, 0.2%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, or a value in the range consisting of any two of the above points.

[0079] When the mass content of the first additive is too low, it is insufficient to form a SEI film of sufficient thickness at the interface, failing to effectively suppress interfacial side reactions. When the mass content of the first additive is too high, it can affect the power performance and fast charging performance of the secondary battery. Controlling the mass content of the first additive within an appropriate range can both reduce interfacial side reactions and minimize the impact of the first additive on the fast charging and power performance of the secondary battery, thus balancing the service life and electrical performance of the secondary battery.

[0080] In some embodiments, the residual space R is 0.05 mL / Ah to 3 mL / Ah, optionally 0.1 mL / Ah to 1.5 mL / Ah, 0.5 mL / Ah to 3 mL / Ah, 1 mL / Ah to 3 mL / Ah, 1.5 mL / Ah to 3 mL / Ah, 0.05 mL / Ah to 1.5 mL / Ah.

[0081] In some embodiments, the residual space R can be selected as 0.05 mL / Ah, 0.1 mL / Ah, 0.2 mL / Ah, 0.4 mL / Ah, 0.5 mL / Ah, 0.6 mL / Ah, 0.8 mL / Ah, 1 mL / Ah, 1.2 mL / Ah, 1.4 mL / Ah, 1.5 mL / Ah, or a value in the range consisting of any two of the above points.

[0082] When the residual space R is above the above range, while the space for gas storage increases, the secondary battery's energy density decreases. When the residual space R is below the above range, the reduced space for gas storage increases the risk of casing deformation. Controlling the residual space R within an appropriate range can both increase the secondary battery's energy density and provide sufficient space to accommodate gases generated by side reactions in the battery cell assembly, thereby reducing or maintaining a relatively stable internal pressure in the battery casing. This helps improve the safety of the secondary battery, allowing the battery to achieve both energy density and safety.

[0083] In some embodiments, the electrolyte includes a second additive, and the second additive is selected from one or more of fluorocarbonate compounds and sulfonate compounds.

[0084] In some embodiments, the second additive comprises a fluorinated carbonate compound. In some embodiments, the second additive comprises a sulfonate compound. In some embodiments, the second additive comprises a fluorinated carbonate compound and a sulfonate compound.

[0085] The second additive, which includes at least one of a fluorocarbonate compound and a sulfonate compound, is beneficial to the formation of an inorganic SEI film rich in LiF and Li2SO3 on the negative electrode side, which is beneficial to further reduce the side reactions occurring due to the contact between the electrolyte and the negative electrode, reduce gas generation, and improve the service life of the secondary battery.

[0086] In some embodiments, the fluorinated carbonate compound includes one or more of fluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate, and optionally includes fluoroethylene carbonate and 1,2-difluoroethylene carbonate.

[0087] In some embodiments, the sulfonate compound includes one or more of 1,3-propane sultone, propene sultone, and 3-fluoro-1,3-propane sultone, and optionally includes 1,3-propane sultone.

[0088] In some embodiments, the second additive comprises fluoroethylene carbonate and 1,3-propane sultone. In some embodiments, the second additive comprises 1,2-difluoroethylene carbonate and 1,3-propane sultone.

[0089] In some embodiments, the mass ratio of fluoroethylene carbonate or 1,2-difluoroethylene carbonate to 1,3-propane sultone is (0.1-50):1, which can be optionally (0.1-30):1, (0.1-20):1, (0.1-10):1, (0.1-5):1, (0.1-3):1, (0.1-1):1 or (0.1-0.5):1.

[0090] The above-mentioned fluorinated carbonate compounds and sulfonate compounds can form an inorganic SEI film at the interface between the electrolyte and the negative electrode. The use of the second additive alone or the coordinated use of the second additive containing two different substances can effectively reduce the side reactions occurring in the contact between the electrolyte and the positive and negative electrode plates, reduce gas generation, and improve the service life of the secondary battery.

[0091] In some embodiments, based on the total mass of the electrolyte, the mass content W of the first additive and the mass content A of the second additive satisfy the following: 0.045% ≤ W + A ≤ 15%, optionally 0.1% ≤ W + A ≤ 11%, 0.1% ≤ W + A ≤ 10%, 0.1% ≤ W + A ≤ 8%, 0.1% ≤ W + A ≤ 5%, 0.1% ≤ W + A ≤ 1.5%, 0.5% ≤ W + A ≤ 11%, 0.5% ≤ W + A ≤ 5%, 0.5% ≤ W + A ≤ 2%, 0.05% ≤ W + A ≤ 1% or 0.05% ≤ W + A ≤ 2%.

[0092] Herein, "W+A" refers to the sum of the mass content W (%) and the mass content A (%).

[0093] In some embodiments, W+A can be selected as 0.05%, 0.15%, 0.6%, 1.3%, 1.5%, 2%, 4%, 5%, 6%, 7%, 8%, 10%, 13%, 15% or a value in the range consisting of any two of the above points.

[0094] Introducing too much of the first and second additives into the electrolyte can affect the thickness of the SEI film and the viscosity of the electrolyte, thereby reducing the battery's fast-charging and power performance. Controlling the mass content W of the first additive and the mass content A of the second additive to satisfy the above relationship can not only form a sufficient amount of inorganic SEI film at the interface between the electrolyte and the negative electrode, reducing gas generation and extending the battery's service life, but also reduce the impact of the introduction of the first and second additives on the electrolyte, such as affecting the fast-charging and power performance of the secondary battery, while taking into account both the service life and electrical performance of the secondary battery.

[0095] In some embodiments, based on the total mass of the electrolyte, the mass content A of the second additive is 0.05% to 10%, optionally 0.5% to 7%, 0.1% to 10%, 0.2% to 10%, 0.5% to 10%, 0.1% to 7%, 0.1% to 6.5%, 0.5% to 6.5%, 0.2% to 6.5%.

[0096] In some embodiments, based on the total mass of the electrolyte, the mass content A of the second additive may be selected to be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, or a value in the range consisting of any two of the above points.

[0097] Controlling the mass content of the second additive within an appropriate range can not only reduce the interface side reactions between the positive and negative electrodes and further improve the service life of the secondary battery; it can also reduce the impact of the introduction of the second additive on the fast charging and power performance of the secondary battery, so that the secondary battery can have both service life and electrical performance.

[0098] In some embodiments, the battery cell assembly includes a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector and including at least a positive electrode active material. The thickness of the positive electrode current collector is 4 μm to 14 μm, and can be optionally 5 μm to 13 μm.

[0099] In some embodiments, the thickness of the positive electrode current collector may be 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, or a value in a range consisting of any two of the above points.

[0100] In some embodiments, the secondary battery includes a negative electrode current collector, and the thickness of the negative electrode current collector is 3 μm to 10 μm, and optionally 4 μm to 8 μm.

[0101] In some embodiments, the thickness of the negative electrode current collector may be 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or a value in a range consisting of any two of the above values.

[0102] When the thickness of the positive electrode current collector and / or the negative electrode current collector exceeds the above range, the gas space within the battery case is reduced, affecting the service life of the secondary battery. When the thickness is below the above range, the mechanical strength of the current collector and the conduction of electrons are affected. Controlling the thickness of the positive electrode current collector and / or the negative electrode current collector within an appropriate range can not only meet the requirements of mechanical strength and the requirements of electron conduction during charging and discharging, but also free up a certain amount of space to accommodate more positive electrode active material / negative electrode active material, thereby improving the energy density of the secondary battery, or free up a certain amount of space to accommodate gas, thereby reducing the internal pressure of the battery case or maintaining the internal pressure basically stable, which helps to improve the service life and safety of the secondary battery.

[0103] In some embodiments, the filling coefficient of the secondary battery is 1 g / Ah to 3 g / Ah, and can be optionally 1.5 g / Ah to 3 g / Ah, or 1.5 g / Ah to 2.5 g / Ah.

[0104] In some embodiments, the filling coefficient of the secondary battery can be selected as 1g / Ah, 1.2g / Ah, 1.4g / Ah, 1.5g / Ah, 1.6g / Ah, 1.8g / Ah, 2g / Ah, 2.2g / Ah, 2.4g / Ah, 2.5g / Ah, 2.6g / Ah, 2.8g / Ah, 3g / Ah, or a value in the range formed by any two of the above points.

[0105] In this application, the term "filling coefficient" refers to the ratio of the mass (g) of the electrolyte injected into the secondary battery to the capacity (Ah) of the secondary battery. The capacity may be the designed capacity of the secondary battery.

[0106] Controlling the filling coefficient of the secondary battery within an appropriate range can not only provide enough electrolyte to meet the needs of the secondary battery, but also release a certain amount of space to accommodate more positive electrode active materials / negative electrode active materials, thereby improving the energy density of the secondary battery; or release a certain amount of space to accommodate the gas generated by side reactions, thereby reducing the internal pressure of the battery shell and improving the service life and safety of the secondary battery.

[0107] In some embodiments, the electrolyte includes a solvent, and the solvent includes one or more of a carboxylate solvent, a cyclic carbonate solvent, and a linear carbonate solvent.

[0108] In some embodiments, the solvent comprises a carboxylate solvent, in some embodiments, the solvent comprises a cyclic carbonate solvent, in some embodiments, the solvent comprises a linear carbonate solvent.

[0109] The carboxylate solvent, the cyclic carbonate solvent or the linear carbonate solvent may be used in combination with the first additive and / or the second additive to enable the secondary battery to have an excellent service life and energy density.

[0110] In some embodiments, the solvent includes at least two of a carboxylate solvent, a cyclic carbonate solvent, and a linear carbonate solvent.

[0111] In some embodiments, based on the total mass of the solvent, the mass content X of the cyclic carbonate solvent in the solvent is 2% to 35% / 10% to 35%, 15% to 35%, or 20% to 35%.

[0112] In some embodiments, based on the total mass of the solvent, the mass content Y of the linear carbonate solvent in the solvent is 0% to 80%, 20% to 80%, or 40% to 80%.

[0113] In some embodiments, based on the total mass of the solvent, the mass content Y of the carboxylate solvent in the solvent is 0% to 80%, 20% to 80%, or 20% to 70%.

[0114] In some embodiments, based on the total mass of the solvent, the mass content X of the cyclic carbonate solvent in the solvent is 2% to 35%, the mass content Y of the linear carbonate solvent is 0% to 80%, and the mass content of the carboxylate solvent is (100%-XY).

[0115] In some embodiments, based on the total mass of the solvent, the mass content X of the cyclic carbonate solvent is 20% to 35%, the mass content Y of the linear carbonate solvent is 0% to 75%, and the mass content of the carboxylate solvent is (100%-XY).

[0116] In some embodiments, the solvent includes a carboxylate solvent and a cyclic carbonate solvent. Based on the total mass of the solvent, the mass ratio of the carboxylate solvent and the cyclic carbonate solvent is 5:95 to 80:20, optionally 10:90 to 70:30. In some embodiments, the mass ratio of the carboxylate solvent and the cyclic carbonate solvent can be optionally 5:95, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55, 50:50, 55:45, 60:40, 65:35, 70:30, 75:25 or 80:20.

[0117] In some embodiments, the solvent includes a cyclic carbonate solvent and a linear carbonate solvent. Based on the total mass of the solvent, the mass ratio of the cyclic carbonate solvent to the linear carbonate solvent is 5:95 to 65:35, optionally 10:90 to 70:30. In some embodiments, the mass ratio of the cyclic carbonate solvent to the linear carbonate solvent can be 5:95, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55, 50:50, 55:45, 60:40 or 65:35.

[0118] Controlling the mass ratio of different solvents within an appropriate range is beneficial to reducing the viscosity of the electrolyte and improving the dynamics of the electrolyte, further enhancing the electrical performance of the secondary battery.

[0119] In some embodiments, the solvent includes a carboxylate solvent, a cyclic carbonate solvent, and a linear carbonate solvent. Based on the total mass of the solvent, the mass content X of the cyclic carbonate solvent is 2% to 35%, the mass content Y of the linear carbonate solvent is 8% to 60%, and the mass content of the carboxylate solvent is (100% - XY). In some embodiments, based on the total mass of the solvent, the mass content X of the cyclic carbonate solvent is 20% to 30%, the mass content Y of the linear carbonate solvent is 50% to 60%, and the mass content of the carboxylate solvent is (100% - XY).

[0120] In some embodiments, the mass ratio of the carboxylate solvent, the cyclic carbonate solvent, and the linear carbonate solvent is 5:35:60 to 90:2:8, 30:20:50 to 10:30:60, 5:35:60, 10:30:60, 15:25:60, 15:35:50, 20:35:45, 20:25:55, 25:15:60, 25:25:50 , 25:20:55, 35:15:50, 40:5:55, 45:25:30, 50:35:15, 50:25:25, 55:20:25, 55:35:10, 60:20:20, 60:25:15, 65:25:10, 65:15:20, 70:15:15, 80:10:10, 85:5:10 or 90:2:8.

[0121] The electrical performance of the secondary battery is improved as much as possible by using a combination of carboxylate solvents, cyclic carbonate solvents, and linear carbonate solvents and controlling the mass ratio of the carboxylate solvents, cyclic carbonate solvents, and linear carbonate solvents.

[0122] In some embodiments, the carboxylate solvent comprises a structure shown in Formula I,

[0123] Wherein, R1 and R2 each independently include C 1-10 The alkyl group,

[0124] In some embodiments, R1 and R2 each independently include C 1-4 In some embodiments, R1 and R2 each independently include C 1-3 In some embodiments, R1 and R2 each independently include methyl and ethyl.

[0125] In some embodiments, the carboxylate solvent includes one or more of methyl formate, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, isopropyl acetate, and isoamyl acetate.

[0126] In some embodiments, the cyclic carbonate solvent includes one or more of ethylene carbonate and propylene carbonate.

[0127] In some embodiments, the linear carbonate solvent includes at least one of dimethyl carbonate, diethyl carbonate, methylpropyl carbonate, and methylethyl carbonate.

[0128] The above substances can be used in combination with the first additive and / or the second additive to ensure that the secondary battery has excellent service life and energy density.

[0129] In some embodiments, the linear carbonate solvent includes two of dimethyl carbonate, diethyl carbonate, methylpropyl carbonate, and methylethyl carbonate.

[0130] In some embodiments, linear carbonate solvents include dimethyl carbonate and diethyl carbonate. In some embodiments, linear carbonate solvents include dimethyl carbonate and methyl propyl carbonate. In some embodiments, linear carbonate solvents include dimethyl carbonate and methyl ethyl carbonate. In some embodiments, linear carbonate solvents include diethyl carbonate and methyl propyl carbonate. In some embodiments, linear carbonate solvents include diethyl carbonate and methyl ethyl carbonate. In some embodiments, linear carbonate solvents include methyl propyl carbonate and methyl ethyl carbonate.

[0131] In some embodiments, the linear carbonate solvent comprises dimethyl carbonate and ethyl methyl carbonate, and the mass ratio of the two linear carbonate solvents is 5:90 to 70:10, and can be 10:80 to 60:10. In some embodiments, the mass ratio of the two linear carbonate solvents can be 5:90, 10:80, 15:80, 10:80, 25:65, 30:60, 35:60, 40:50, 45:45, 50:30, 55:20, 60:10 or 70:10.

[0132] The solvent further includes two linear carbonate solvents and / or controls the two linear carbonate solvents, which is beneficial to further improve the properties of the electrolyte, thereby improving the properties of the secondary battery.

[0133] In some embodiments, the electrolyte further includes a lithium salt, and the lithium salt includes one or more of LiFSI, LiPF6, LiBF4, LiTFSI, LiClO4, LiAsF6, LiBOB, LiDFOB, and LiDFOP.

[0134] In some embodiments, the electrolyte further includes a sodium salt, and the sodium salt includes one or more of NaFSI, NaPF6, NaBF4, NaTFSI, NaClO4, and NaAsF6.

[0135] [Positive electrode]

[0136] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.

[0137] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0138] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0139] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0140] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0141] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0142] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0143] [Negative electrode]

[0144] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector.

[0145] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0146] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0147] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0148] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0149] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0150] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0151] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0152] [Isolation film]

[0153] In some embodiments, the secondary battery further includes a separator, which can be any known porous separator with good chemical and mechanical stability.

[0154] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different.

[0155] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be made into a battery cell assembly through a winding process or a lamination process.

[0156] In some embodiments, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte in some embodiments.

[0157] In some embodiments, the secondary battery includes one or more of a lithium secondary battery, a sodium secondary battery, and a potassium secondary battery.

[0158] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the battery cell components and the electrolyte.

[0159] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0160] The shape of the secondary battery in this application can be cylindrical, square or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.

[0161] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation film can be formed into a battery cell assembly 52 through a winding process or a lamination process. The battery cell assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the battery cell assembly 52. ​​The number of battery cell assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0162] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0163] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0164] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0165] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0166] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0167] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0168] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0169] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0170] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0171] Example

[0172] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0173] 1. Preparation method

[0174] Example 1

[0175] 1) Electrolyte

[0176] In an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm), ethylene carbonate and ethyl methyl carbonate (mass ratio of 3:7) were mixed, lithium hexafluorophosphate was added to the mixed solvent so that the mass content of the lithium salt in the electrolyte was 12%, and after stirring evenly, 1% of the total mass of the electrolyte was added with 4,4'-ethylene disulfate, and mixed to prepare an electrolyte.

[0177] 2) Preparation of positive electrode sheet

[0178] 1wt% polyvinylidene fluoride binder was fully dissolved in N-methylpyrrolidone. 1wt% carbon black conductive agent and 98wt% Li(NiCoMn)O2, the ternary positive electrode active material, were added and mixed thoroughly to form a positive electrode slurry. The slurry was evenly coated on the surface of the current collector aluminum foil to form a positive electrode film, which was then transferred to a vacuum drying oven for complete drying. The dried electrode sheets were then roll-pressed and punched to form positive electrode sheets.

[0179] 3) Preparation of negative electrode sheet

[0180] The negative electrode active material, artificial graphite, the conductive agent, carbon black, the thickener, carboxymethyl cellulose (CMC-Na), and the binder, styrene-butadiene rubber (SBR), were mixed and dissolved in deionized water at a weight ratio of 96:2:1:1. The negative electrode slurry was prepared using a vacuum mixer and then coated on the surface of copper foil. Finally, the slurry was transferred to a vacuum drying oven for complete drying before being slit and die-cut to produce negative electrode sheets.

[0181] 4) Isolation film

[0182] Polypropylene film is used as the isolation film.

[0183] 5) Preparation of batteries

[0184] The positive electrode sheet, the separator, and the negative electrode sheet are wound or stacked in order. The separator is placed between the positive and negative electrode sheets to act as an isolater. The bare battery cell is welded with the pole ear and placed in an aluminum shell. The bare battery cell is baked at 80°C to remove water, and then the above-mentioned electrolyte is injected and sealed to obtain an uncharged battery. The uncharged battery then undergoes the processes of standing, hot and cold pressing, formation, shaping, and capacity testing in sequence. Among them, the internal volume of the secondary battery accommodating cavity is 1011.3ml, the volume of the battery cell assembly is 751ml, the volume of the electrolyte is 195.2ml, and the capacity of the secondary battery is 130.1Ah, thereby obtaining the lithium secondary battery product of Example 1. The injection coefficient of the electrolyte is 1.8g / Ah, and the residual space R of the lithium secondary battery is 0.5mL / Ah.

[0185] Examples 2 to 38

[0186] The battery preparation methods in Examples 2 to 38 are basically similar to those in Example 1, but the preparation parameters of the electrolyte are adjusted. The specific parameters are shown in Table 1.

[0187] Among them, in Example 6, the internal volume of the secondary battery accommodating cavity is kept unchanged, the volume of the battery cell assembly is adjusted to 792.6 ml, the volume of the electrolyte is adjusted to 211.7 ml, the capacity of the secondary battery is 141.1 Ah, and a secondary battery with a residual space R of 0.05 mL / Ah is obtained.

[0188] In Example 7, the internal volume of the secondary battery accommodating cavity is kept unchanged, the volume of the battery cell assembly is adjusted to 680.6 ml, the volume of the electrolyte is adjusted to 165.3 ml, the capacity of the secondary battery is adjusted to 110.2 Ah, and a secondary battery with a residual space R of 1.5 mL / Ah is obtained.

[0189] In Example 9, the internal volume of the secondary battery accommodating cavity is kept unchanged, the volume of the battery cell assembly is adjusted to 787 ml, the volume of the electrolyte is adjusted to 210.3 ml, the capacity of the secondary battery is adjusted to 140.2 Ah, and a secondary battery with a residual space R of 0.1 mL / Ah is obtained.

[0190] In Example 10, the internal volume of the secondary battery accommodating cavity is kept unchanged, the volume of the battery cell assembly is adjusted to 691.2 ml, the volume of the electrolyte is adjusted to 171.5 ml, the capacity of the secondary battery is 114.3 Ah, and a secondary battery with a residual space R of 1.3 mL / Ah is obtained.

[0191] In Example 11, the internal volume of the secondary battery accommodating cavity is kept unchanged, the volume of the battery cell assembly is adjusted to 680.6 ml, the volume of the electrolyte is adjusted to 165.3 ml, the capacity of the secondary battery is 110.2 Ah, and a secondary battery with a residual space R of 1.5 mL / Ah is obtained.

[0192] In Example 12, the internal volume of the secondary battery accommodating cavity is kept unchanged, the volume of the battery cell assembly is adjusted to 614 ml, the volume of the electrolyte is adjusted to 132.3 ml, the capacity of the secondary battery is 88.2 Ah, and a secondary battery with a residual space R of 3 mL / Ah is obtained.

[0193] In Example 29, the internal volume and residual space of the secondary battery accommodating cavity are kept unchanged, the volume of the battery cell assembly is adjusted to 835.2 ml, the volume of the electrolyte is adjusted to 110 ml, the capacity of the secondary battery is adjusted to 132 Ah, and a secondary battery with an injection coefficient of 1 g / Ah is obtained.

[0194] In Example 30, the internal volume and residual space of the secondary battery accommodating cavity are kept unchanged, the volume of the battery cell assembly is adjusted to 774.8 ml, the volume of the electrolyte is adjusted to 169 ml, the capacity of the secondary battery is adjusted to 135.2 Ah, and a secondary battery with a filling coefficient of 1.5 g / Ah is obtained.

[0195] In Example 31, the internal volume and residual space of the secondary battery accommodating cavity are kept unchanged, the volume of the battery cell assembly is adjusted to 762 ml, the volume of the electrolyte is adjusted to 181.3 ml, the capacity of the secondary battery is adjusted to 136 Ah, and a secondary battery with an injection coefficient of 1.6 g / Ah is obtained.

[0196] In Example 32, the internal volume and residual space of the secondary battery accommodating cavity are kept unchanged, the volume of the battery cell assembly is adjusted to 658.6 ml, the volume of the electrolyte is adjusted to 279.8 ml, the capacity of the secondary battery is adjusted to 146 Ah, and a secondary battery with a filling coefficient of 2.3 g / Ah is obtained.

[0197] In Example 33, the internal volume and residual space of the secondary battery accommodating cavity were kept unchanged, the volume of the battery cell assembly was adjusted to 628.9 ml, the volume of the electrolyte was adjusted to 308.8 ml, the capacity of the secondary battery was adjusted to 148.2 Ah, and a secondary battery with a liquid injection coefficient of 2.5 g / Ah was obtained.

[0198] In Example 34, the internal volume and residual space of the secondary battery accommodating cavity are kept unchanged, the volume of the battery cell assembly is adjusted to 551 ml, the volume of the electrolyte is adjusted to 383.5 ml, the capacity of the secondary battery is adjusted to 153.4 Ah, and a secondary battery with a filling coefficient of 3 g / Ah is obtained.

[0199] Comparative Example 1

[0200] The battery preparation method in Comparative Example 1 is basically similar to that in Example 1, but the first additive and the second additive are not contained in the electrolyte. The specific parameters are shown in Table 1.

[0201] Comparative Example 2

[0202] The battery preparation method in Comparative Example 2 was essentially similar to that in Example 1. The internal volume of the secondary battery chamber remained unchanged, the volume of the battery cell assembly was adjusted to 795 ml, the volume of the electrolyte was adjusted to 213.5 ml, the capacity of the secondary battery was adjusted to 142.3 Ah, and the R value of the secondary battery was adjusted to 0.02 mL / Ah to achieve a W / R ratio of 50. Specific parameters are shown in Table 1.

[0203] Comparative Example 3

[0204] The battery preparation method in Comparative Example 3 is basically similar to that in Example 1, but the W content of the first additive in the secondary battery is adjusted to 0.01% to make W / R 0.02. The adjustment method is similar to that in Examples 7 to 12. The specific parameters are shown in Table 1.

[0205] Comparative Example 4

[0206] The battery preparation method in Comparative Example 4 is basically similar to that in Comparative Example 1, but a second additive is introduced into the electrolyte. The specific parameters are shown in Table 1.

[0207] Comparative Example 5

[0208] The battery preparation method in Comparative Example 5 is basically similar to that in Comparative Example 2, but a second additive is introduced into the electrolyte. The specific parameters are shown in Table 1.

[0209] Comparative Example 6

[0210] The battery preparation method in Comparative Example 6 is basically similar to that in Comparative Example 3, but a second additive is introduced into the electrolyte. The specific parameters are shown in Table 1.

[0211] 2. Performance Testing

[0212] 1. Battery performance test

[0213] 1) DC resistance (DCR) test

[0214] At -25°C, adjust the single cell state of charge to 50% SOC and let it rest for 30 minutes. Record the battery voltage at this point as U1 (V). Discharge it at 0.36C for 10 seconds and record the battery voltage at this point as U2 (V). The corresponding discharge current I (mA) is 0.36 × the battery's design capacity (mAh). DC resistance DCR (mΩ) = (U1 - U2) / I.

[0215] 2) Energy density test

[0216] At 25°C, charge the battery at a constant current and constant voltage of 0.33C to the designed upper limit voltage, with a cut-off current of 0.05C. After standing for 30 minutes, discharge it at 0.33C to the designed lower limit voltage. Record the discharge energy P (Wh) and the cell weight m (kg). The energy density (Wh / kg) = P / m.

[0217] 3) High temperature gas production test

[0218] The high-temperature gas production test process is as follows: the prepared battery is charged to 100% SOC at a rate of 0.1C, stored at 60°C, and the internal pressure of the battery is monitored online using a barometer. When the cut-off pressure is 0.35MPa, the number of days stored at 60°C is recorded.

[0219] 4) Cyclic performance test

[0220] The cycle performance test process is as follows: at 45°C, the prepared battery is charged to 4.25V at a constant current of 1C, then charged at a constant voltage of 4.25V until the current drops to 0.05C. After standing for 5 minutes, it is discharged to 2.5V at a constant current of 1C. This is the first charge / discharge cycle of the battery, and the discharge capacity at this time is recorded as the discharge capacity of the battery in the first cycle (C1); the above steps are repeated for the same battery, and the process capacity of the battery after the nth cycle (Cn) is the capacity retention rate after n cycles = Cn / C1×100%. The number of cycles at which the cycle capacity retention rate is 80% is recorded. The test process of the comparative example and other embodiments is the same as above.

[0221] 3. Analysis of test results of various embodiments and comparative examples

[0222] Batteries of various examples and comparative examples were prepared according to the above methods, and various performance parameters were measured. The results are shown in Tables 1 and 2 below.

[0223] Table 1

[0224] Table 2

[0225] According to the above results of Examples 1 to 38, when the ratio W / R of the mass content W of the sulfate compound to the residual space R is in the range of 0.03% to 40%, the prepared secondary battery has both good energy density and high-temperature storage days.

[0226] From the comparison of Examples 1 to 12 with Comparative Example 1, and Examples 13 to 28 with Comparative Example 4, it can be seen that the electrolyte including the sulfate ester compound is beneficial to improving the high-temperature storage performance and cycle performance of the battery. From the comparison of Examples 1 to 12 with Comparative Examples 2 to 3, and Examples 13 to 28 with Comparative Examples 5 to 6, it can be seen that when the ratio W / R of the mass content W of the sulfate ester compound to the residual space R is in the range of 0.03% to 40%, the battery has improved energy density while further improving the high-temperature storage performance and cycle performance of the battery. From the comparison of Examples 1 to 5, 7 to 12 with Example 6, it can be seen that when the ratio W / R of the mass content W of the sulfate ester compound to the residual space R is in the range of 0.03% to 20%, it is beneficial to significantly improve the high-temperature storage performance of the battery.

[0227] As can be seen from Examples 1 to 5, controlling the mass content W of the first additive to 0.05% to 2% based on the total mass of the electrolyte results in a battery with low DC resistance, high energy density, and excellent high-temperature storage and cycling performance. A comparison of Examples 1, 3 to 5 with Example 2 shows that a mass content W of the first additive of 0.1% to 2% further improves the battery's high-temperature storage and cycling performance.

[0228] From the comparison between Examples 8 to 11 and Example 12, it can be seen that controlling R to 0.05 mL / Ah to 1.5 mL / Ah is beneficial to improving the energy density of the battery.

[0229] From the comparison of Examples 8 and 11, it can be seen that controlling R to 0.1 mL / Ah to 1.3 mL / Ah takes into account the energy density, high-temperature storage performance and cycle performance of the battery.

[0230] As can be seen from Examples 1 to 21, based on the total mass of the electrolyte, when the sum of the mass content W of the first additive and the mass content A of the second additive is controlled within the range of 0.045% to 11%, the battery has a low DC resistance, high energy density, excellent high-temperature storage performance and cycle performance. From the comparison of Examples 1 to 5 and Comparative Example 3, it can be seen that the addition of 4,4'-disulfate vinyl ester to the electrolyte in the range of 0.045% to 2% helps to improve the high-temperature storage days of the secondary battery. From the comparison of Examples 13 to 19, Examples 21 to 23 and Example 22, it can be seen that when the sum of the mass content W of the first additive and the mass content A of the second additive is within the range of 0.7% to 11%, the high-temperature storage performance and cycle performance of the battery are further improved.

[0231] Comparison of Examples 13-17 with Examples 18-19 shows that controlling the mass content of the second additive A to 0.1% to 7% based on the total mass of the electrolyte further improves the cycle performance. Comparison of Examples 13, 15-16 with Examples 14 and 17 shows that further controlling the mass content of the second additive A to 0.5% to 6.5% balances the DC resistance, high-temperature storage performance, and cycle performance of the battery.

[0232] It can be seen from Examples 22 to 23 that the second additive includes at least two of fluoroethylene carbonate, 1,3-propane sultone, and 1,2-difluoroethylene carbonate, which can make the battery have lower DC resistance, high energy density, excellent high-temperature storage performance and cycle performance.

[0233] In Examples 24 to 26, a composite solvent comprising at least two of ethylene carbonate, dimethyl carbonate, ethyl acetate, and methyl acetate was used. In Examples 27 to 28, a composite solvent comprising a carboxylate solvent, a cyclic carbonate solvent, and a linear carbonate solvent was used, which helps to reduce the DC impedance of the battery and further improve the cycle performance of the battery.

[0234] As can be seen from Examples 29 to 34, the battery exhibits excellent energy density, high-temperature storage performance, and cycling performance when the injection coefficient is controlled within the range of 1 g / Ah to 3 g / Ah. A comparison of Examples 20 to 33 with Examples 29 and 34 shows that further controlling the injection coefficient to 1.5 g / Ah to 2.5 g / Ah can achieve a balance between energy density, high-temperature storage performance, and cycling performance.

[0235] It can be seen from Examples 35 to 36 and Examples 37 to 38 that when the thickness of the positive electrode current collector is 4 μm to 14 μm or the thickness of the negative electrode current collector is 3 μm to 10 μm, it helps to improve the electronic conductivity of the current collector and thus improve the cycle performance of the battery; the thickness helps to provide suitable space in the battery to improve the gas generated by the side reactions of the electrode, thereby enabling the battery to have excellent energy density, high temperature storage performance and cycle performance.

[0236] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A secondary battery, characterized in that: The invention comprises a battery housing having a receiving cavity, a battery core assembly located in the receiving cavity, and an electrolyte comprising a first additive, wherein the first additive is selected from sulfate compounds; Wherein, based on the total mass of the electrolyte, the mass content W of the first additive and the residual space R satisfy: 0.03%≤W / R≤40%, which can be 0.03%≤W / R≤20%; in, Among them, V1 represents the internal volume of the secondary battery housing cavity; V2 represents the volume of the battery cell assembly; V3 represents the volume of the electrolyte; and C represents the discharge capacity of the secondary battery.

2. The secondary battery according to claim 1, characterized in that: The sulfate ester compound includes one or more of 4,4'-vinyl sulfate, vinyl sulfate, diethyl sulfate, dimethyl sulfate, and 4,4-bis(1,3,2-dioxathiolane)-2,2,2,2-tetraoxide, and optionally includes one or more of 4,4'-vinyl sulfate and vinyl sulfate.

3. The secondary battery according to claim 1 or 2, characterized in that: Based on the total mass of the electrolyte, the mass content W of the first additive is 0.045% to 2%, and can be optionally 0.1% to 2%.

4. The secondary battery according to any one of claims 1 to 3, characterized in that: R is 0.05mL / Ah to 3mL / Ah, and can be optionally 0.1mL / Ah to 1.5mL / Ah.

5. The secondary battery according to any one of claims 1 to 4, characterized in that: The electrolyte includes a second additive, and the second additive is selected from one or more of fluorocarbonate compounds and sulfonate compounds.

6. The secondary battery according to claim 5, characterized in that: The fluorinated carbonate compound includes one or more of fluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate, and optionally includes fluoroethylene carbonate and 1,2-difluoroethylene carbonate; and / or The sulfonate compound includes one or more of 1,3-propane sultone, propene sultone, and 3-fluoro-1,3-propane sultone, and optionally includes 1,3-propane sultone.

7. The secondary battery according to claim 5 or 6, characterized in that: The second additive includes fluoroethylene carbonate and 1,3-propane sultone; or, the second additive includes 1,2-difluoroethylene carbonate and 1,3-propane sultone; Wherein, the mass ratio of the fluoroethylene carbonate or 1,2-difluoroethylene carbonate to 1,3-propane sultone is (0.1-50):1, and can be optionally (0.1-30):

1.

8. The secondary battery according to any one of claims 5 to 7, characterized in that: Based on the total mass of the electrolyte, the mass content W of the first additive and the mass content A of the second additive satisfy: 0.045%≤W+A≤15%, optionally 0.1%≤W+A≤11%.

9. The secondary battery according to any one of claims 5 to 8, characterized in that: Based on the total mass of the electrolyte, the mass content A of the second additive is 0.05% to 10%, and can be optionally 0.5% to 7%.

10. The secondary battery according to any one of claims 1 to 9, characterized in that: The battery core assembly comprises a positive electrode current collector and a positive electrode film layer located on at least one side of the positive electrode current collector and comprising at least a positive electrode active material. The thickness of the positive electrode current collector is 4 μm to 14 μm, and can be optionally 5 μm to 13 μm.

11. The secondary battery according to any one of claims 1 to 10, characterized in that: The secondary battery comprises a negative electrode current collector, and the thickness of the negative electrode current collector is 3 μm to 10 μm, and can be 4 μm to 8 μm.

12. The secondary battery according to any one of claims 1 to 11, characterized in that: The liquid filling coefficient of the secondary battery is 1 g / Ah to 3 g / Ah, and can be optionally 1.5 g / Ah to 2.5 g / Ah.

13. The secondary battery according to any one of claims 1 to 12, characterized in that: The electrolyte includes a solvent, and the solvent includes at least two of a carboxylate solvent, a cyclic carbonate solvent, and a linear carbonate solvent.

14. The secondary battery according to claim 13, characterized in that: The mass content X of the cyclic carbonate solvent is 2% to 35% based on the total mass of the solvent.

15. The secondary battery according to claim 13 or 14, characterized in that: Based on the total mass of the solvent, the mass content X of the cyclic carbonate solvent is 20% to 35%, the mass content Y of the linear carbonate solvent is 0% to 75%, and the mass content of the carboxylate solvent is (100%-XY).

16. The secondary battery according to any one of claims 12 to 15, characterized in that: The carboxylate solvent includes a structure shown in Formula I, Wherein, R1 and R2 each independently include C 1-10 alkyl, optionally, the carboxylate solvent includes one or more of methyl formate, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, isopropyl acetate, and isoamyl acetate; and / or The cyclic carbonate solvent includes one or more of ethylene carbonate and propylene carbonate; and / or The linear carbonate solvent includes at least one of dimethyl carbonate, diethyl carbonate, methyl propyl carbonate and methyl ethyl carbonate.

17. The secondary battery according to claim 13 or 16, characterized in that: The linear carbonate solvent includes two of dimethyl carbonate, diethyl carbonate, methyl propyl carbonate and methyl ethyl carbonate.

18. The secondary battery according to claim 17, characterized in that: The linear carbonate solvent includes dimethyl carbonate and ethyl methyl carbonate, and the mass ratio of dimethyl carbonate to ethyl methyl carbonate is 5:90 to 70:10, and can be optionally 10:80 to 60:

10.

19. The secondary battery according to any one of claims 1 to 18, characterized in that: The secondary battery includes one or more of a lithium secondary battery, a sodium secondary battery, and a potassium secondary battery.

20. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to any one of claims 1 to 19.

Citation Information

Patent Citations

  • Ternary positive electrode material, positive electrode plate, preparation method and application

    CN113594447A

  • Negative active material, negative pole piece, preparation method and application

    CN113594451A

  • Cobalt-free lithium ion battery electrolyte and cobalt-free lithium ion battery containing same

    CN115377497A

  • Secondary battery, battery module, battery pack, and electric device

    CN115692842A

  • Negative electrode slurry, negative electrode pole piece, lithium ion battery, battery module, battery pack and electric device

    CN115832235A