Water-based ceramic slurry, preparation method therefor and use thereof
By preparing an aqueous ceramic slurry and coating it onto a base membrane, the interfacial compatibility and resistance issues of ceramic composite separators were resolved, resulting in a high-performance lithium-ion battery separator that improves battery safety and electrochemical performance.
Patent Information
- Application Number
- PCT/CN2023/137213
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2023-12-07
- Publication Date
- 2024-11-28
AI Technical Summary
Existing ceramic composite separators suffer from poor interfacial compatibility, high interfacial resistance, and insufficient thermal stability, which affect the electrochemical and safety performance of lithium-ion batteries.
A water-based ceramic slurry, comprising ceramic particles, bentonite, sodium carboxymethyl cellulose, dispersant, and activator, is prepared by mixing and coating onto a base membrane to form a water-based ceramic diaphragm. This improves the affinity with the base membrane and the wetting performance of the electrolyte, and reduces the interfacial resistance.
The prepared aqueous ceramic separator has good thermal stability and low interfacial resistance, which improves the cycle stability and rate performance of lithium-ion batteries and enhances battery safety.
Smart Images

Figure PCTCN2023137213-FTAPPB-I100001 
Figure PCTCN2023137213-FTAPPB-I100002 
Figure PCTCN2023137213-FTAPPB-I100003
Abstract
Description
A water-based ceramic slurry and its preparation method and application
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 24, 2023, with application number 202310589769.0. The entire contents of the above application are incorporated by reference into this application. Technical Field
[0002] The present application belongs to the technical field of diaphragm materials, and for example relates to a water-based ceramic slurry and a preparation method and application thereof. Background Art
[0003] As a key component of lithium-ion batteries, the performance of the separator directly impacts the internal resistance, capacity, cycling performance, and safety of the assembled battery. On the one hand, the poor affinity between non-polar polyolefin separators and polar electrolytes results in high interfacial resistance in lithium-ion batteries. On the other hand, traditional polyolefin separators suffer from low melting points, strong thermal shrinkage, and easy deformation. They are prone to melting and shrinking near their melting point, causing battery short circuits and explosions, significantly impacting battery safety.
[0004] Related technologies disclose ceramic composite diaphragms, which can improve the thermal stability and mechanical strength of polyolefin diaphragms and prevent diaphragm puncture from causing battery short circuits. However, the following problems exist during their application: on the one hand, the interface compatibility between organic and inorganic materials in ceramic composite diaphragms is poor, which often leads to powder loss problems in ceramic composite diaphragms; on the other hand, the ceramic coating in the ceramic composite diaphragm increases the interface resistance between the diaphragm and the electrode material to a certain extent, affecting the electrochemical performance of the battery.
[0005] Therefore, in this field, there is an urgent need to develop a ceramic composite diaphragm with good interface compatibility, low resistance and thermal stability to solve the above problems. Technical issues
[0006] The present application provides a water-based ceramic slurry, a preparation method, and applications thereof. The water-based ceramic slurry provided in the present application has good affinity with the base membrane, and the resulting separator not only has good electrolyte wettability and high liquid absorption rate, but also has good thermal stability and low interfacial resistance. Technical Solutions
[0007] In a first aspect, an embodiment of the present application provides an aqueous ceramic slurry. Taking the total mass of the aqueous ceramic slurry as 100%, the aqueous ceramic slurry includes the following raw materials:
[0008] In a second aspect, an embodiment of the present application provides a method for preparing the aqueous ceramic slurry according to the first aspect, the method comprising the following steps:
[0009] Ceramic particles, bentonite, sodium carboxymethyl cellulose, a dispersant, an active agent and water are mixed according to the formula to obtain the water-based ceramic slurry.
[0010] In a third aspect, an embodiment of the present application provides a water-based ceramic diaphragm, which includes a base membrane and a water-based ceramic layer arranged on at least one side of the base membrane, and the water-based ceramic layer is prepared from the water-based ceramic slurry described in the first aspect.
[0011] In a fourth aspect, an embodiment of the present application provides a method for preparing the water-based ceramic diaphragm according to the third aspect, the method comprising the following steps:
[0012] The base film is immersed in the aqueous ceramic slurry described in the first aspect, and the aqueous ceramic diaphragm is obtained after drying.
[0013] In a fifth aspect, an embodiment of the present application provides a secondary battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the separator is the aqueous ceramic separator according to the third aspect. Beneficial effects
[0014] Beneficial effects of the present application: The present application provides an aqueous ceramic slurry, which has good affinity with the base membrane, and the prepared diaphragm not only has good wettability and high liquid absorption rate to the electrolyte, but also has good thermal stability and low interface resistance. Among them, the ceramic particles can not only improve the thermal stability of the prepared diaphragm, but also have a high specific surface energy, which can greatly improve the affinity of the aqueous ceramic slurry with the base membrane, so that the diaphragm has stronger wettability and liquid absorption rate, reduces the battery interface impedance, and the assembled secondary battery can also show better cycle stability and rate performance. In addition, bentonite can play an anti-settling role to avoid the sedimentation of the slurry; the active agent can activate the active ingredients in the ceramic particles, and the dispersant and the active agent have a synergistic effect, which is conducive to ensuring the uniform dispersion of ceramic particles in the aqueous slurry system. Modes for Carrying Out the Invention
[0015] The present application provides a water-based ceramic slurry. Taking the total mass of the water-based ceramic slurry as 100%, the water-based ceramic slurry comprises the following raw materials:
[0016] The present application provides a water-based ceramic slurry with a specific composition, so that the water-based ceramic slurry and the base film have good affinity, and the prepared diaphragm not only has good wettability and high liquid absorption rate to the electrolyte, but also has good thermal stability and low interface resistance. Among them, the ceramic particles can not only improve the thermal stability of the prepared diaphragm, but also have a high specific surface energy, which can greatly improve the affinity of the water-based ceramic slurry and the base film, so that the diaphragm has stronger wettability and liquid absorption rate, reduces the battery interface impedance, and the assembled secondary battery can also show better cycle stability and rate performance. In addition, bentonite can play an anti-settling role to avoid the sedimentation of the slurry; the active agent can activate the active ingredients in the ceramic particles, and the dispersant and the active agent have a synergistic effect, which is conducive to ensuring the uniform dispersion of ceramic particles in the aqueous slurry system.
[0017] Compared with traditional ceramic composite diaphragms, the diaphragms prepared by the aqueous ceramic slurry provided in this application have lower charge transfer resistance and excellent interfacial compatibility, so that the assembled lithium-ion batteries exhibit good rate performance and cycle performance, especially at high current density, so that the lithium-ion batteries with the prepared ceramic composite diaphragms have the advantage of higher discharge specific capacity.
[0018] In the present application, the content of the ceramic particles is 25-35%, for example, it can be 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, etc.
[0019] In this application, by adjusting the content of ceramic particles, the diaphragm can store more electrolyte to facilitate the transmission of lithium ions. If the content is too low, the spacing between the ceramic particles will be too large, making it difficult to support the diaphragm coating to resist thermal shrinkage. Conversely, tiny bubbles will be generated in the slurry during the coating process, and the bubbles will absorb heat and burst during the subsequent drying process.
[0020] In the present application, the content of bentonite is 0.2-2%, for example, it can be 0.2%, 0.3%, 0.5%, 0.8%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, etc.
[0021] In the present application, the content of sodium carboxymethyl cellulose is 1-10%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.
[0022] In the present application, the content of the dispersant is 1-5%, for example, 1%, 2%, 3%, 4%, 5%, etc.
[0023] In this application, by adjusting the content of the dispersant, the dispersibility of the powder is improved and the medium surface is reduced. If the content is too low, the slurry will have a very high viscosity, resulting in extremely poor fluidity, which will seriously affect the quality of the ceramic slurry. Conversely, the slurry will flocculate and the stability will deteriorate, resulting in the slurry viscosity becoming higher and higher, becoming thicker and thicker, and reducing the various performance properties of the original slurry.
[0024] In the present application, the content of the active agent is 1-5%, for example, it can be 1%, 2%, 3%, 4%, 5%, etc.
[0025] In this application, by adjusting the content of the surfactant, the surface tension of the rubber is reduced, the interfacial activity is increased, and the penetration and diffusion of the slurry into the diaphragm are promoted and improved. If the content is too low, the slurry will cause agglomeration, and vice versa, it will cause excessive slurry foam that is difficult to eliminate.
[0026] In the present application, the water content is 45-60%, for example, it can be 45%, 48%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, etc.
[0027] Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the aqueous ceramic slurry comprises the following raw materials:
[0028] Preferably, the ceramic particles include any one of silicon nitride, aluminum oxide, zirconium oxide or titanium dioxide, or a combination of at least two thereof.
[0029] Preferably, the crystal structure of the silicon nitride is β phase.
[0030] Preferably, the average particle size of the ceramic particles is 30-100 nm, for example, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc.
[0031] In the present application, by regulating the average particle size of the ceramic particles, the diaphragm has a uniform porosity, which is beneficial for the diaphragm to store more electrolyte, provide more channels for lithium ion transport, and facilitate the rapid migration of lithium ions during the charging and discharging process.
[0032] Preferably, the aqueous ceramic slurry further comprises a binder.
[0033] In this application, the addition of a binder has a thickening effect.
[0034] Preferably, the binder includes any one of polytetrafluoroethylene (PTFE), styrene-butadiene emulsion (SBR) or water-based polyacrylate (PAA) or a combination of at least two thereof.
[0035] Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the binder is 3-7%, for example, 3%, 4%, 5%, 6%, 7%, etc.
[0036] Preferably, the dispersant includes any one of ammonium acrylate, ethylene-vinyl acetate copolymer or polystyrene, or a combination of at least two thereof.
[0037] Preferably, the active agent includes any one of isomeric decanol polyoxyethylene ether, alkylphenol polyoxyethylene ether or polyoxyethylene ester, or a combination of at least two thereof.
[0038] Preferably, the aqueous ceramic slurry further comprises a defoaming agent.
[0039] In the present application, the addition of a defoaming agent has the effect of preventing the generation of tiny bubbles when the membrane is painted.
[0040] Preferably, the defoaming agent includes any one or a combination of at least two of GPES defoaming agent, higher alcohol, tributyl phosphate or dimethyl silicone oil.
[0041] Preferably, based on the total mass of the aqueous ceramic slurry as 100%, the mass percentage of the defoaming agent is 2-4%, for example, it can be 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, etc.
[0042] Preferably, the viscosity of the aqueous ceramic slurry is 0.1-0.5 Pa·s, for example, it can be 0.1 Pa·s, 0.2 Pa·s, 0.3 Pa·s, 0.4 Pa·s, 0.5 Pa·s, etc.
[0043] Preferably, the solid content of the aqueous ceramic slurry is 60-80%, for example, 60%, 65%, 70%, 75%, 80%, etc.
[0044] The present application provides a method for preparing the aqueous ceramic slurry according to the first aspect, the method comprising the following steps:
[0045] Ceramic particles, bentonite, sodium carboxymethyl cellulose, a dispersant, an active agent and water are mixed according to the formula to obtain the water-based ceramic slurry.
[0046] Preferably, a binder and a defoamer may be added before mixing.
[0047] Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the binder is 3-7%, for example, 3%, 4%, 5%, 6%, 7%, etc.
[0048] Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the defoaming agent is 2-4%, for example, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, etc.
[0049] Preferably, the specific process of mixing ceramic particles, bentonite, sodium carboxymethyl cellulose, a binder, a dispersant, an active agent, a defoaming agent and water according to the formula comprises the following steps:
[0050] Mixing sodium carboxymethyl cellulose and water once to obtain a sodium carboxymethyl cellulose solution, and then mixing the sodium carboxymethyl cellulose solution with bentonite, water, a dispersant, an active agent, and a defoamer twice to obtain a mixed slurry;
[0051] The obtained mixed slurry is mixed with ceramic particles and a binder to obtain the water-based ceramic slurry.
[0052] The present application provides a water-based ceramic diaphragm, which includes a base membrane and a water-based ceramic layer arranged on at least one side of the base membrane, and the water-based ceramic layer is prepared by the water-based ceramic slurry according to the first aspect.
[0053] Preferably, the thickness of the aqueous ceramic layer is 8-12 μm, for example, 8 μm, 8.2 μm, 8.5 μm, 8.8 μm, 9 μm, 9.2 μm, 9.5 μm, 9.8 μm, 10 μm, 10.2 μm, 10.5 μm, 10.8 μm, 11 μm, 11.2 μm, 11.5 μm, 11.8 μm, or 12 μm.
[0054] In this application, by regulating the thickness of the water-based ceramic layer, the silicon nitride particles are dispersed and densely arranged on the surface of the base membrane under the action of the binder. The interfacial bonding force between the silicon nitride coating and the base membrane is strong, which reduces the spacing between the silicon nitride particles. The coating acts as a skeleton to support the diaphragm and resists thermal shrinkage.
[0055] Preferably, the base film comprises a polyethylene base film and / or a polypropylene base film.
[0056] Preferably, the base film has a thickness of 16 μm-20 μm, for example, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc.
[0057] The present application provides a method for preparing the water-based ceramic diaphragm according to the third aspect, the method comprising the following steps:
[0058] The base film is immersed in the aqueous ceramic slurry described in the first aspect, and the aqueous ceramic diaphragm is obtained after drying.
[0059] As a preferred technical solution of this application, the method includes the following steps:
[0060] First, the base film is pre-dried to remove moisture. The specific pre-drying conditions are drying at 80-110°C for 1 hour. Then, the pre-dried base film is immersed in the slurry for 2-15 minutes until there is basically no bubble escape. After drying, the water-based ceramic diaphragm is obtained.
[0061] In a fifth aspect, the present application provides a secondary battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the separator is the aqueous ceramic separator according to the third aspect.
[0062] Example 1
[0063] This embodiment provides a water-based ceramic slurry. Taking the total mass of the water-based ceramic slurry as 100%, the water-based ceramic slurry includes the following raw materials:
[0064] The average particle size of the β-phase silicon nitride is 65 nm, the viscosity of the water-based ceramic slurry is 0.3 Pa·s, and the solid content is 70%.
[0065] This embodiment provides a method for preparing the above-mentioned water-based ceramic slurry, which comprises the following steps:
[0066] (1) mixing sodium carboxymethyl cellulose and water to obtain a sodium carboxymethyl cellulose solution, and then mixing the sodium carboxymethyl cellulose solution with bentonite, water, an ammonium acrylate dispersant, an isomeric decanol polyoxyethylene ether active agent, and a GPES defoamer to obtain a mixed slurry;
[0067] (2) The mixed slurry obtained in step (1) was stirred with β-phase silicon nitride at a speed of 500 r / min for 2 h, and then stirred with a polytetrafluoroethylene binder at a speed of 600 r / min for 5 h to obtain the water-based ceramic slurry.
[0068] Example 2
[0069] This embodiment provides a water-based ceramic slurry. Taking the total mass of the water-based ceramic slurry as 100%, the water-based ceramic slurry includes the following raw materials:
[0070] The average particle size of the β-phase silicon nitride is 65 nm, the viscosity of the water-based ceramic slurry is 0.3 Pa·s, and the solid content is 70%.
[0071] This embodiment provides a method for preparing the above-mentioned water-based ceramic slurry, which comprises the following steps:
[0072] (1) mixing sodium carboxymethyl cellulose and water to obtain a sodium carboxymethyl cellulose solution, and then mixing the sodium carboxymethyl cellulose solution with bentonite, water, an ammonium acrylate dispersant, an alkylphenol polyoxyethylene ether active agent, and a higher alcohol defoamer to obtain a mixed slurry;
[0073] (2) The mixed slurry obtained in step (1) is stirred with β-phase silicon nitride at a speed of 500 r / min for 2 hours, and then stirred with a styrene-butadiene emulsion binder at a speed of 600 r / min for 5 hours to obtain the water-based ceramic slurry.
[0074] Example 3
[0075] This embodiment provides a water-based ceramic slurry. Taking the total mass of the water-based ceramic slurry as 100%, the water-based ceramic slurry includes the following raw materials:
[0076] The average particle size of the β-phase silicon nitride is 65 nm, the viscosity of the water-based ceramic slurry is 0.3 Pa·s, and the solid content is 70%.
[0077] This embodiment provides a method for preparing the above-mentioned water-based ceramic slurry, which comprises the following steps:
[0078] (1) mixing sodium carboxymethyl cellulose and water to obtain a sodium carboxymethyl cellulose solution, and then mixing the sodium carboxymethyl cellulose solution with bentonite, water, an ammonium acrylate dispersant, a polyoxyethylene ester active agent, and a tributyl phosphate defoamer to obtain a mixed slurry;
[0079] (2) The mixed slurry obtained in step (1) was stirred with β-phase silicon nitride at a speed of 500 r / min for 2 h, and then stirred with a water-based polyacrylate binder at a speed of 600 r / min for 5 h to obtain the water-based ceramic slurry.
[0080] Example 4
[0081] The difference between this embodiment and embodiment 1 is that the viscosity of the aqueous ceramic slurry is 0.05 Pa·s, and the other aspects are the same as those of embodiment 1.
[0082] Example 5
[0083] The difference between this embodiment and embodiment 1 is that the viscosity of the aqueous ceramic slurry is 1 Pa·s, and the other aspects are the same as those of embodiment 1.
[0084] Example 6
[0085] The difference between this embodiment and embodiment 1 is that the solid content of the aqueous ceramic slurry is 50%, and the other aspects are the same as those of embodiment 1.
[0086] Example 7
[0087] The difference between this embodiment and embodiment 1 is that the solid content of the aqueous ceramic slurry is 90%, and the other aspects are the same as those of embodiment 1.
[0088] Comparative Example 1
[0089] The difference between this comparative example and Example 1 is that, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of β-phase silicon nitride is 10%, and the water content is adaptively adjusted so that the content of the aqueous ceramic slurry system is 100%. The rest is the same as Example 1.
[0090] Comparative Example 2
[0091] The difference between this comparative example and Example 1 is that, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of β-phase silicon nitride is 40%, and the water content is adaptively adjusted so that the content of the aqueous ceramic slurry system is 100%. The rest is the same as Example 1.
[0092] Comparative Example 3
[0093] The difference between this comparative example and Example 1 is that the acrylic acid ammonium salt dispersant is replaced by an equal amount of isomeric decanol polyoxyethylene ether active agent, and the rest is the same as Example 1.
[0094] Comparative Example 4
[0095] The difference between this comparative example and Example 1 is that the isomeric decanol polyoxyethylene ether active agent is replaced by an equal amount of acrylic acid ammonium salt dispersant, and the rest is the same as Example 1.
[0096] Comparative Example 5
[0097] The difference between this comparative example and Example 1 is that, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the ammonium acrylate dispersant is 0.1%, and the mass percentage of the isomeric decanol polyoxyethylene ether active agent is 5.9%. The rest are the same as Example 1.
[0098] Comparative Example 6
[0099] The difference between this comparative example and Example 1 is that, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the ammonium acrylate dispersant is 5.9%, and the mass percentage of the isomeric decanol polyoxyethylene ether active agent is 0.1%. The rest are the same as Example 1.
[0100] Application Examples 1 to 7 and Comparative Application Examples 1 to 6
[0101] The aqueous ceramic slurries provided in Examples 1 to 7 and Comparative Examples 1 to 6 were used to prepare aqueous ceramic diaphragms. The preparation method is as follows:
[0102] First, the base membrane is dried at 100°C for 1 hour, and the pre-dried base membrane is cooled to below 60°C. Then, the pre-dried base membrane is immersed in a water-based ceramic slurry for 15 minutes until basically no bubbles escape. The immersed membrane is hung in an electric blast drying oven at 50°C to dry the surface moisture, and then placed in a vacuum drying oven at 80°C for 24 hours to dry out the moisture in the pores to obtain the water-based ceramic membrane.
[0103] The prepared waterborne ceramic diaphragm is assembled into a lithium ion half-cell, and the preparation method is as follows:
[0104] Manganese iron lithium, Super P conductive agent and polyvinylidene fluoride binder are mixed with an appropriate amount of N-methylpyrrolidone in a mass ratio of 95:3:2, and then evenly applied on aluminum foil. The mixture is placed in a vacuum oven and dried at 180°C for 8 hours. A pole piece with a diameter of 10 mm is prepared using a slicer and assembled with the above-mentioned diaphragm and lithium metal sheet to form a manganese iron lithium half-cell.
[0105] Test conditions
[0106] The water-based ceramic diaphragms provided in Application Examples 1 to 7 and Comparative Application Examples 1 to 6 were tested using the following method:
[0107] (1) Thermal shrinkage: Stack the diaphragm into 3 layers, flatten them, expel the air between the films, take out the cutting plate (20×20), cut out the diaphragm sample, measure the diameter A1 of the cut sample, set the oven temperature to 150℃, and keep it warm for 1 hour after the temperature is reached. Place the sample in the oven and keep it warm for 2 hours. Use a stopwatch or the timer of the oven to time it. After 2 hours, take out the diaphragm, cool it for 10 minutes, and measure the diameter A2 of the sample. Diaphragm thermal shrinkage = (A1-A2) / A1×100%;
[0108] (2) Porosity: First, put the sample under weight, record it as M0. Put it in a clean beaker, and pour water into it until it is submerged. Then put the beaker directly into the drying oven and heat it until it boils. The boiling state needs to be maintained for two hours. When the water completely penetrates into the air in the electrode, stop heating and lower the temperature in the room. Take out the sample and put it in a small hanging basket, and put it on the hook. The sample must be submerged in water. At this time, weigh it again and record it as M1. Take out the sample, wipe off all the moisture on the surface, and weigh it again. The weight at this time is recorded as M2. Membrane porosity = (M2-M0) / (M2-M1)×100%;
[0109] (3) Liquid absorption rate: First, place the sample under a load, recorded as M0, in a beaker with electrolyte, let it stand for 30 minutes, take out the sample, weigh it, recorded as M1, the membrane liquid absorption rate = (M1-M0) / M0×100%;
[0110] (4) Impedance: The ordinary diaphragm and the ceramic modified diaphragm were assembled into button cells and EIS tests were performed.
[0111] The lithium ion half-cells provided in Application Examples 1 to 7 and Comparative Application Examples 1 to 6 were subjected to cycle performance tests, and the test method was as follows:
[0112] At 45°C, the lithium-ion battery is charged at a constant current of 0.5C (nominal capacity) to a voltage of 4.2V, then charged at a constant voltage of 4.2V to a current of ≤0.05C. After standing for 10 minutes, it is discharged at a constant current of 3C to a cut-off voltage of 2.5V. The above is one charge and discharge cycle. The lithium-ion battery is subjected to 1000 charge and discharge cycles at 45°C according to the above conditions. Among them, the capacity retention rate is calculated according to the following formula.
[0113] The test results are shown in Table 1:
[0114] Table 1
[0115] It can be seen from Table 1 that the water-based ceramic diaphragms prepared in Application Examples 1-3 provided in this application can maintain a good state, among which the ceramic diaphragm provided in Application Example 1 has the best performance, and the corresponding half-cell also has relatively good cycle performance.
[0116] Compared with Application Example 1, Application Example 4 reduces the viscosity of the aqueous ceramic slurry. The resulting modified ceramic diaphragm has excessively high thermal shrinkage and porosity, and its impedance is relatively large, thereby affecting the service life of the battery.
[0117] Compared with Application Example 1, Application Example 5 increases the viscosity of the aqueous ceramic slurry too much, making the slurry increasingly thicker and causing flocculation. At the same time, the stability of the slurry deteriorates, thereby affecting the performance of the modified ceramic diaphragm and reducing the service life of the battery.
[0118] Compared with Application Example 1, Application Example 6 has an excessively low solid content, which results in a significant decrease in the thermal stability of the modified ceramic diaphragm, thereby reducing the safety performance of the battery, and further causing the impedance of the resulting battery to be relatively high, affecting the cycle performance of the battery.
[0119] Compared with Application Example 1, Application Example 7 has a higher solid content, which makes the over-curing phenomenon more obvious, resulting in edge scattering effect of the ceramic slurry, affecting its liquid absorption rate and impedance, and reducing the battery cycle performance.
[0120] The difference between Comparative Application Example 1 and Application Example 1 is that, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of β-phase silicon nitride is 10%. There are too few ceramic particles, resulting in excessive spacing between the ceramic particles, making it difficult to support the coating of the diaphragm to resist thermal shrinkage. Therefore, the thermal shrinkage rate is extremely large, affecting the high-temperature cycle characteristics of the battery.
[0121] The difference between Comparative Application Example 2 and Application Example 1 is that, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of β-phase silicon nitride is 40%. There are too many ceramic particles, which causes tiny bubbles to be generated in the slurry during the coating process. The bubbles absorb heat and burst during the subsequent drying process, so the porosity is too large, resulting in excessive impedance, which affects the battery life and is difficult to apply in actual production.
[0122] Comparative Application Examples 3 and 5 show that the content of the dispersant exceeds the preferred range of this application, resulting in flocculation of the slurry, poor stability, and increasing viscosity of the slurry, which in turn affects the service life of the battery.
[0123] Comparative Application Examples 4 and 6 show that when the content of the active agent is too low, the slurry will clump together, and when the content is too high, the slurry will have excessive foam that is difficult to eliminate, making it difficult for the slurry to diffuse and penetrate into the diaphragm, resulting in low interfacial activity of the diaphragm and excessively high surface tension, which affects the impedance and cycle performance of the battery.
[0124] Comparative Application Examples 3 and 4 show that there is a synergistic effect between the acrylic acid ammonium salt dispersant and the isomeric decanol polyoxyethylene ether active agent.
Claims
1. A water-based ceramic slurry, based on the total mass of the water-based ceramic slurry being 100%, the water-based ceramic slurry comprises the following raw materials:
2. The aqueous ceramic slurry according to claim 1, wherein Taking the total mass of the aqueous ceramic slurry as 100%, the aqueous ceramic slurry includes the following raw materials:
3. The aqueous ceramic slurry according to claim 1 or 2, wherein: The ceramic particles include any one of silicon nitride, aluminum oxide, zirconium oxide or titanium dioxide, or a combination of at least two thereof; Preferably, the crystal structure of the silicon nitride is β phase; Preferably, the average particle size of the ceramic particles is 30-100 nm.
4. The aqueous ceramic slurry according to any one of claims 1 to 3, further comprising a binder; Preferably, the binder comprises any one of polytetrafluoroethylene, styrene-butadiene emulsion or water-based polyacrylate or a combination of at least two thereof; Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the binder is 3-7%; Preferably, the dispersant comprises any one or a combination of at least two of ammonium acrylate, ethylene-vinyl acetate copolymer or polystyrene; Preferably, the active agent includes isomeric decyl alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether or polyoxyethylene ether. Any one or a combination of at least two of oxyethylene esters; Preferably, the aqueous ceramic slurry further comprises a defoaming agent; Preferably, the defoamer comprises any one or a combination of at least two of GPES defoamer, higher alcohol, tributyl phosphate or dimethyl silicone oil; Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the defoaming agent is 2-4%; Preferably, the viscosity of the aqueous ceramic slurry is 0.1-0.5 Pa·s; Preferably, the solid content of the aqueous ceramic slurry is 60-80%.
5. A method for preparing the aqueous ceramic slurry according to any one of claims 1 to 4, the method comprising the following steps: Ceramic particles, bentonite, sodium carboxymethyl cellulose, a dispersant, an active agent and water are mixed according to the formula amount to obtain the water-based ceramic slurry.
6. The method according to claim 5, wherein a binder and a defoamer may be added before the mixing; Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the binder is 3-7%; Preferably, based on the total mass of the aqueous ceramic slurry being 100%, the mass percentage of the defoaming agent is 2-4%; Preferably, the specific process of mixing ceramic particles, bentonite, sodium carboxymethyl cellulose, a binder, a dispersant, an active agent, a defoamer and water according to the formula comprises the following steps: The sodium carboxymethyl cellulose and water are mixed once to obtain a sodium carboxymethyl cellulose solution, and then the sodium carboxymethyl cellulose solution is mixed twice with bentonite, water, a dispersant, an active agent and a defoamer to obtain a mixed slurry; The obtained mixed slurry is mixed with ceramic particles and a binder to obtain the aqueous ceramic slurry.
7. A water-based ceramic diaphragm, comprising a base membrane and a water-based ceramic layer arranged on at least one side of the base membrane, wherein the water-based ceramic layer is prepared from the water-based ceramic slurry according to any one of claims 1 to 4.
8. The water-based ceramic diaphragm according to claim 7, wherein: The thickness of the water-based ceramic layer is 8 μm-12 μm; Preferably, the base film comprises a polyethylene base film and / or a polypropylene base film; Preferably, the base film has a thickness of 16 μm-20 μm.
9. A method for preparing the water-based ceramic diaphragm according to claim 7 or 8, the method comprising the following steps: The base film is immersed in the aqueous ceramic slurry according to any one of claims 1 to 4, and the aqueous ceramic diaphragm is obtained after drying. 10 . A secondary battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the separator is the aqueous ceramic separator according to claim 7 or 8 .
Citation Information
Patent Citations
Ceramic slurry, ceramic composite diaphragm and lithium ion battery
CN109449354A
Diaphragm, preparation method thereof and battery
CN109950461A
Composite diaphragm slurry, preparation method thereof and battery diaphragm
CN113611983A
Coating slurry, preparation method thereof, composite diaphragm and lithium ion battery
CN114243215A
Water-based ceramic slurry as well as preparation method and application thereof
CN116606147A