Negative electrode particle and preparation method therefor, and negative electrode plate and energy storage apparatus
By preparing negative electrode particles with specific pore structures, the problems of negative electrode material's capacity and circulation performance are solved, high capacity and high first-time efficiency are achieved, and the circulation performance of the battery is maintained, thereby improving the energy density of the battery.
Patent Information
- Application Number
- PCT/CN2024/072970
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-01-18
- Publication Date
- 2024-11-28
AI Technical Summary
The gram capacity of the negative electrode material and the first-time Coulomb efficiency are low, resulting in the inability to improve the energy density of the battery, and the increase in nanopores will lead to poor cell circulation performance.
By preparing negative electrode particles with specific closed-pore and open-pore structures, the pore volume ratio between closed-pore and open-pore is controlled to be between 6 and 11, not only to build an ion conduction channel, but also to avoid side reactions, and to improve the capacity and first-time efficiency. At the same time, maintain battery circulation performance.
The high capacity and high first-time efficiency of the negative electrode particles are achieved without affecting the circulation performance of the energy storage device, and the energy density and circulation performance of the battery are improved.
Smart Images

Figure CN2024072970_28112024_PF_FP_ABST
Abstract
Description
Negative electrode particles, preparation method thereof, negative electrode sheet and energy storage device Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a negative electrode particle and a preparation method thereof, a negative electrode plate and an energy storage device. Background Art
[0002] With the continuous development of battery technology, batteries are required to have higher energy density and better cycle performance. As a key material in batteries, anode materials face a series of challenges. The low gram capacity and initial coulombic efficiency of anode materials have prevented further improvement in battery energy density. Nanopores in anode materials can increase the storage sites of active ions, thereby increasing the gram capacity of anode materials. However, the increase in nanopores can easily lead to increased side reactions between the anode material and the electrolyte, resulting in poor battery cycle performance.
[0003] Summary of the Invention
[0004] In response to the above problems, an embodiment of the present application provides a negative electrode particle, which has a higher gram capacity and a higher initial efficiency, and does not affect the cycle performance of the energy storage device.
[0005] The first embodiment of the present application provides a negative electrode particle, comprising: closed pores located inside the negative electrode particle and open pores located on the surface of the negative electrode particle, wherein the ratio of the pore volume of the closed pores to the pore volume of the open pores is in the range of 6≤C1 / C2≤11; the pore volume of the closed pores is in the range of 0.03cm 3 / g≤C1≤0.12cm 3 / g.
[0006] A second embodiment of the present application provides a method for preparing negative electrode particles, which includes:
[0007] Providing precursors and soluble salts;
[0008] Placing the precursor in the soluble salt system and pre-carbonizing the precursor at a first temperature to obtain first particles, wherein the first particles include the precursor and the soluble salt dispersed in the precursor, and the first temperature is higher than the melting temperature of the soluble salt;
[0009] removing soluble salts in the first particles to obtain second particles; and
[0010] The second particles are carbonized at a second temperature to obtain the negative electrode particles, wherein the second temperature is greater than the first temperature, the negative electrode particles have closed pores located inside the negative electrode particles and open pores located on the surface of the negative electrode particles, the ratio of the pore volume of the closed pores to the pore volume of the open pores is in the range of 6≤C1 / C2≤11, and the pore volume of the closed pores is in the range of 0.03cm 3 / g≤C1≤0.12cm 3 / g.
[0011] A third embodiment of the present application provides a negative electrode plate, which includes: a current collector and an active material layer, wherein the active material layer is arranged on the surface of the current collector, and the active material layer includes the negative electrode particles described in the embodiment of the present application.
[0012] The fourth aspect of the present application provides an energy storage device, comprising: an electrolyte, a positive electrode plate, a diaphragm, and the negative electrode plate described in the embodiment of the present application, wherein the positive electrode plate is at least partially immersed in the electrolyte, the diaphragm is located on one side of the positive electrode plate and is at least partially immersed in the electrolyte, and the negative electrode plate is arranged on the side of the diaphragm away from the positive electrode plate and is at least partially immersed in the electrolyte.
[0013] The negative electrode particles of the present application have closed pores located inside the negative electrode particles and open pores located on the surface of the negative electrode particles. The open pores on the surface of the negative electrode particles not only provide storage sites for active ions and facilitate the electrolyte to infiltrate the negative electrode particles, thereby constructing ion conduction channels. However, the open pores on the surface of the negative electrode particles will also lead to an increase in side reactions between the negative electrode particles and the electrolyte, thereby reducing the initial efficiency of the negative electrode particles. The closed pores inside the negative electrode particles increase the storage sites for active ions, thereby improving the gram capacity and initial efficiency of the negative electrode particles to a certain extent. However, too many closed pores inside the negative electrode particles will affect the electrolyte infiltration of the negative electrode particles, resulting in limited ion conduction channels, thereby reducing the gram capacity of the negative electrode particles. By controlling the ratio of the pore volume of the closed pores to the pore volume of the open pores to be between 6 and 11, the pore volume of the closed pores is in the range of 0.03cm 3 / g to 0.12cm 3 / g, which can not only construct a certain ion conduction channel, but also avoid serious side reactions between the negative electrode particles and the electrolyte. At the same time, the negative electrode particles have more active ion storage sites, so that the negative electrode particles have higher gram capacity and first efficiency. When the negative electrode particles are used in energy storage devices, they will not affect the cycle performance of the energy storage device. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0015] FIG1 is a schematic structural diagram of negative electrode particles according to an embodiment of the present application.
[0016] FIG2 is a flow chart of a method for preparing negative electrode particles according to an embodiment of the present application.
[0017] FIG3 is a schematic structural diagram of a negative electrode sheet according to an embodiment of the present application.
[0018] FIG4 is a schematic cross-sectional view of the negative electrode sheet according to an embodiment of the present application along the AA direction in FIG3 .
[0019] FIG5 is a schematic structural diagram of an energy storage device according to an embodiment of the present application.
[0020] FIG6 is a schematic cross-sectional view of the energy storage device according to an embodiment of the present application along the BB direction in FIG5 .
[0021] Explanation of reference numerals: 100 - negative electrode particles, 101 - closed pores, 102 - open pores, 200 - negative electrode sheet, 210 - current collector, 220 - active material layer, 300 - energy storage device, 310 - separator, 320 - positive electrode sheet. DETAILED DESCRIPTION
[0022] In order to enable those skilled in the art to better understand the present invention, the following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0023] The terms "first," "second," and the like in the specification and claims of this application and the accompanying drawings are used to distinguish between different objects, not to describe a particular order. Furthermore, the terms "including," "having," and any variations thereof, are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or apparatus comprising a series of steps or elements is not limited to the listed steps or elements but may optionally include steps or elements not listed, or may optionally include other steps or elements inherent to the process, method, product, or apparatus.
[0024] The technical solutions in the embodiments of the present application will be described below with reference to the accompanying drawings.
[0025] It should be noted that, for the convenience of explanation, in the embodiments of the present application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments.
[0026] With the continuous development of battery technology, batteries are required to have higher energy density and better cycle performance. As a key material in batteries, anode materials face a series of challenges. The low gram capacity and initial coulombic efficiency of anode materials have prevented further improvement in battery energy density. Nanopores in anode materials can increase the storage sites of active ions, thereby improving the gram capacity of anode materials. However, as the number of nanopores increases, the side reactions between the anode material and the electrolyte increase, resulting in poor battery cycle performance.
[0027] Referring to FIG1 , the first embodiment of the present application provides a negative electrode particle 100, which includes: closed pores 101 located inside the negative electrode particle 100 and open pores 102 located on the surface of the negative electrode particle 100, wherein the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is in the range of 6≤C1 / C2≤11; the pore volume of the closed pores 101 is in the range of 0.03cm 3 / g≤C1≤0.12cm 3 / g.
[0028] Specifically, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 can be 6, 7, 8, 9, 10, 11, or any value in between. Specifically, the pore volume of the closed pores 101 can be 0.03 cm 3 / g, 0.04cm 3 / g, 0.05cm 3 / g, 0.06cm 3 / g, 0.07cm 3 / g, 0.08cm 3 / g, 0.09cm 3 / g, 0.10cm 3 / g, 0.11cm 3 / g, 0.12cm 3 / g, and any values between the above values.
[0029] It can be understood that the closed pores 101 refer to cavities and pores inside the particles that are not connected to the outside world; and the open pores 102 refer to cavities and pores inside the particles that are connected to the outside world.
[0030] It is understandable that the actual open pores 102 and the actual closed pores 101 in the negative electrode particles 100 are irregular, and the regular shapes in FIG. 1 are only for convenience of illustration.
[0031] It is understood that the negative electrode particles 100 may be, but are not limited to, hard carbon, graphite, soft carbon, etc.
[0032] When the negative electrode particles 100 have closed pores 101 located within the negative electrode particles 100 and open pores 102 located on the surface of the negative electrode particles 100, the open pores 102 on the surface of the negative electrode particles 100 not only provide storage sites for active ions and facilitate the electrolyte's infiltration of the negative electrode particles 100, thus forming ion conduction channels, but the open pores 102 on the surface of the negative electrode particles 100 also increase side reactions between the negative electrode particles 100 and the electrolyte, thereby reducing the initial efficiency of the negative electrode particles 100. The closed pores 101 within the negative electrode particles 100 increase the storage sites for active ions, thereby improving the specific capacity and initial efficiency of the negative electrode particles 100 to a certain extent. However, excessive closed pores 101 within the negative electrode particles 100 impede the electrolyte's infiltration of the negative electrode particles 100, resulting in restricted ion conduction channels and thus reducing the specific capacity of the negative electrode particles 100. By controlling the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 to be between 6 and 11, the pore volume of the closed pores 101 is in the range of 0.03 cm 3 / g to 0.12cm 3 / g, a certain ion conduction channel can be constructed, and serious side reactions between the negative electrode particles 100 and the electrolyte can be avoided. At the same time, the negative electrode particles 100 have more active ion storage sites, so that the negative electrode particles 100 have higher gram capacity and first efficiency. When the negative electrode particles 100 are used in the energy storage device 300, the cycle performance of the energy storage device 300 will not be affected.
[0033] In some embodiments, the pore volume C2 of the opening 102 is in the range of: 0.005 cm 3 / g≤C2≤0.01cm 3 Specifically, the pore volume C2 of the opening 102 may be 0.005 cm 3 / g, 0.006cm 3 / g, 0.007cm 3 / g, 0.008cm 3 / g, 0.009cm 3 / g, 0.01cm 3 / g, and any values between the above values.
[0034] When the pore volume of the opening 102 is less than 0.005 cm 3 / g, the electrolyte is difficult to penetrate the negative electrode particles 100, and the rate performance of the negative electrode particles 100 is poor. When the pore volume of the opening 102 is greater than 0.01cm 3 / g, the side reaction between the negative electrode particles 100 and the electrolyte increases, which reduces the initial efficiency of the negative electrode particles 100. When the pore volume of the opening 102 is 0.005cm 3 / g to 0.01cm 3 / g, the negative electrode particles 100 have both good rate performance and high initial efficiency.
[0035] In some embodiments, the average pore size D1 of the closed pores 101 of the negative electrode particles 100 is in the range of 0.8 nm ≤ D1 ≤ 2.0 nm. Specifically, the average pore size D1 of the closed pores 101 of the negative electrode particles 100 can be 0.8 nm, 1.0 nm, 1.2 nm, 1.4 nm, 1.6 nm, 1.8 nm, 2.0 nm, or any value in between.
[0036] When the average pore size of the closed pores 101 is less than 0.8 nm, the active ions are difficult to embed, affecting the gram capacity of the negative electrode particles 100. When the average pore size of the closed pores 101 is greater than 2.0 nm, the binding energy of the active ions increases, hindering the embedding and de-embedding of the active ions. When the average pore size of the closed pores 101 is between 0.8 nm and 2.0 nm, the active ions are more easily embedded and de-embedding, which helps to increase the gram capacity of the negative electrode particles 100.
[0037] In some embodiments, the ratio of the specific surface area S1 of the closed pores 101 of the negative electrode particles 100 to the specific surface area S of the negative electrode particles 100 is in the range of 40≤S1 / S≤200. Specifically, the ratio of the specific surface area S1 of the closed pores 101 of the negative electrode particles 100 to the specific surface area S of the negative electrode particles 100 can be 40, 50, 70, 90, 110, 130, 150, 170, 190, 200, and any value in between.
[0038] It can be understood that the specific surface area of the closed pores 101 of the negative electrode particles 100 refers to the total area of the inner walls of the closed pores 101 of the negative electrode particles 100 per unit weight.
[0039] It can be understood that the specific surface area of the negative electrode particles 100 is the specific surface area of the negative electrode particles 100 per unit weight and the specific surface area of the pores 102 in the negative electrode particles 100 .
[0040] When the ratio of the specific surface area S1 of the closed pores 101 to the specific surface area S of the negative electrode particles 100 is less than 40, the specific surface area S of the negative electrode particles 100 is large, and the contact area between the negative electrode particles 100 and the electrolyte increases, which reduces the initial efficiency of the negative electrode particles 100. When the ratio of the specific surface area S1 of the closed pores 101 to the specific surface area S of the negative electrode particles 100 is greater than 200, the specific surface area of the open pores 102 is too small, the contact area between the negative electrode particles 100 and the electrolyte is small, and the electrolyte has difficulty in wetting the negative electrode particles 100, resulting in poor rate performance of the negative electrode particles 100. When the ratio of the specific surface area S1 of the closed pores 101 to the specific surface area S of the negative electrode particles 100 is between 40 and 200, the negative electrode particles 100 have good initial efficiency and rate performance.
[0041] In some embodiments, the specific surface area S1 of the closed pores 101 is in the range of: 40 m 2 / g≤S1≤400m 2 / g. Specifically, the specific surface area of the closed pores 101 can be 40m 2 / g, 60m 2 / g、80m 2 / g、100m 2 / g, 120m 2 / g, 140m 2 / g, 160m 2 / g, 180m 2 / g, 200m 2 / g, 220m 2 / g, 240m 2 / g, 260m 2 / g, 280m 2 / g、300m 2 / g、320m 2 / g、340m 2 / g、360m 2 / g、380m 2 / g, 400m 2 / g, and any values between the above values.
[0042] When the specific surface area of the closed pores 101 is less than 40 m 2 / g, the negative electrode particles 100 have fewer storage sites for active ions and the gram capacity of the negative electrode particles 100 is lower. When the specific surface area of the closed pores 101 is greater than 400m 2 / g, the structure of the negative electrode particles 100 is not stable enough, which reduces the compaction density of the negative electrode particles 100. When the specific surface area of the closed pores 101 is 40m 2 / g to 400m 2 / g, the negative electrode particles 100 have a higher gram capacity and a higher compaction density.
[0043] In some embodiments, the specific surface area S of the negative electrode particles 100 is in the range of: 1 m 2 / g≤S≤5m 2 / g. Specifically, the specific surface area S of the negative electrode particles 100 can be 1m 2 / g, 2m 2 / g、3m 2 / g、4m 2 / g、5m 2 / g, and any values between the above values.
[0044] When the specific surface area S of the negative electrode particles 100 is less than 1 m 2 / g, the contact area between the negative electrode particles 100 and the electrolyte is small, the electrolyte is difficult to penetrate the negative electrode particles 100, and the rate performance of the negative electrode particles 100 is poor. When the specific surface area S of the negative electrode particles 100 is greater than 5m 2 / g, the contact area between the negative electrode particles 100 and the electrolyte increases, which will reduce the initial efficiency of the negative electrode particles 100. When the specific surface area S of the negative electrode particles 100 is 1m 2 / g to 5m 2 / g, the negative electrode particles 100 have good initial efficiency and rate performance.
[0045] In some embodiments, when the negative electrode particles 100 are layered structures, the ratio of the true density ρ1 of the negative electrode particles 100 to the theoretical true density ρ2 of the negative electrode particles 100 is in the range of: 0.75≤ρ 1 / ρ2≤0.95. Specifically, the ratio of the true density ρ1 of the negative electrode particles 100 to the theoretical true density ρ2 of the negative electrode particles 100 can be 0.75, 0.8, 0.85, 0.9, 0.95, or any value in between.
[0046] It is understood that the true density refers to the actual mass of a solid substance per unit volume in an absolutely dense state, that is, the density after removing internal pores or gaps between particles.
[0047] It is understandable that, since the true density test uses nitrogen adsorption, the internal pores removed here are only the pores of the openings 102 .
[0048] It is understood that the theoretical true density refers to the highest true density of the material under ideal conditions, that is, there are no pores inside the material or no gaps between particles. The theoretical true density of the layered negative electrode particles 100 is 2.26 g / cm 3 .
[0049] When the ratio of the true density ρ1 of the negative electrode particles 100 to the theoretical density ρ2 of the negative electrode particles 100 is less than 0.75, the compacted density of the negative electrode particles 100 is low. When the negative electrode particles 100 are used in the energy storage device 300, the energy density of the energy storage device 300 is reduced. When the ratio of the true density ρ1 of the negative electrode particles 100 to the theoretical density ρ2 of the negative electrode particles 100 is greater than 0.95, the negative electrode particles 100 have fewer storage sites for active ions and the gram capacity of the negative electrode particles 100 is low. When the ratio of the true density ρ1 of the negative electrode particles 100 to the theoretical density ρ2 of the negative electrode particles 100 is between 0.75 and 0.95, the compacted density of the negative electrode particles 100 is high and also has a high gram capacity.
[0050] In some embodiments, the true density ρ1 of the negative electrode particles 100 is in the range of 1.8 g / cm 3 ≤ρ1≤2.1g / cm 3 Specifically, the true density of the negative electrode particles 100 may be 1.8 g / cm 3 , 1.9g / cm 3 , 2.0g / cm 3 , 2.1g / cm 3 , and any values between the above values.
[0051] When the true density of the negative electrode particles 100 is less than 1.8 g / cm 3 When the negative electrode particles 100 have a low compaction density, when the negative electrode particles 100 are used in the energy storage device 300, the energy density of the energy storage device 300 will be reduced. When the true density of the negative electrode particles 100 is greater than 2.1 g / cm 3 When the negative electrode particles 100 have fewer active ion storage sites, the gram capacity of the negative electrode particles 100 is lower. When the true density of the negative electrode particles 100 is 1.8 g / cm 3 to 2.1g / cm 3 When the negative electrode particles 100 have a higher compaction density and a higher gram capacity, the negative electrode particles 100 have a higher compaction density and a higher gram capacity.
[0052] Referring to FIG. 2 , a second embodiment of the present application provides a method for preparing negative electrode particles 100 , which includes:
[0053] S201, providing a precursor and a soluble salt;
[0054] S202, placing the precursor in the soluble salt system, and pre-carbonizing the precursor at a first temperature to obtain first particles, wherein the first particles include the precursor and the soluble salt dispersed in the precursor, and the first temperature is higher than the melting temperature of the soluble salt;
[0055] S203, removing soluble salts in the first particles to obtain second particles; and
[0056] S204, carbonizing the second particles at a second temperature to obtain the negative electrode particles 100, wherein the second temperature is greater than the first temperature, and the negative electrode particles 100 have closed pores 101 located inside the negative electrode particles 100 and open pores 102 located on the surface of the negative electrode particles 100, and the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is in the range of 6≤C1 / C2≤11, and the pore volume of the closed pores 101 is in the range of 0.03cm 3 / g≤C1≤0.12cm 3 / g.
[0057] The precursor is placed in the soluble salt system and pre-carbonized at the first temperature. The fusible salt is in a molten state. The volatile matter in the precursor gradually evaporates at the first temperature and leaves pores. The molten fusible salt occupies the pores. After removing the fusible salt, carbonization is performed to obtain negative electrode particles 100. The pores in the negative electrode particles 100 are small, and the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is between 6 and 11. The pore volume of the closed pores 101 is in the range of 0.03 cm 3 / g to 0.12cm 3 / g, a certain ion conduction channel can be constructed, and serious side reactions between the negative electrode particles 100 and the electrolyte can be avoided. At the same time, the negative electrode particles 100 have more active ion storage sites. The negative electrode particles 100 have a higher gram capacity and first efficiency. When the negative electrode particles 100 are used in the energy storage device 300, the cycle performance of the energy storage device 300 will not be affected.
[0058] It is understandable that the precursor may be, but is not limited to, at least one of asphalt, petroleum coke, sub-bituminous coal, bituminous coal, biomass resin, coconut shell, walnut shell, etc.
[0059] Furthermore, the carbon content of the precursor ranges from 20% to 70%.
[0060] In the embodiments of the present application, when a numerical value range from a to b is involved, unless otherwise specified, it means that the numerical value can be any numerical value between a and b, including the endpoint numerical value a and the endpoint numerical value b.
[0061] Specifically, the carbon content of the precursor may be in the range of 20%, 40%, 60%, 70%, and any value in between.
[0062] When the carbon content of the precursor is less than 20%, the carbon yield of the negative electrode particles 100 is low, that is, the conversion rate of the negative electrode particles 100 obtained from the precursor is low. When the carbon content of the precursor is greater than 70%, the precursor has low volatile matter, and the resulting negative electrode particles 100 have few pores. When the carbon content of the precursor is between 20% and 70%, the carbon yield of the precursor is high, and the resulting negative electrode particles 100 have more pores, which provides the negative electrode particles 100 with more active ion storage sites.
[0063] It is understood that the soluble salt refers to a salt that can be dissolved in a liquid (eg, a salt that is soluble in water, a salt that is soluble in an organic solvent, etc.).
[0064] It is understandable that the soluble salt may be, but is not limited to, at least one of sodium chloride, potassium chloride, calcium chloride, sodium fluoride, potassium fluoride, sodium hydroxide, potassium hydroxide, and the like.
[0065] In some embodiments, the mass ratio of the soluble salt to the precursor ranges from 10% to 200%.
[0066] Specifically, the mass ratio of the soluble salt to the precursor can be 10%, 20%, 40%, 60%, 80%, 100%, 120%, 140%, 160%, 180%, 200%, and any value in between.
[0067] When the mass ratio of the soluble salt to the precursor is less than 10%, the volatile matter in the precursor gradually evaporates, leaving pores. The molten fusible salt cannot completely occupy these pores, causing the pores to easily close at high temperatures, reducing the active ion storage sites in the negative electrode particles 100 and lowering the specific capacity. When the mass ratio of the soluble salt to the precursor is greater than 200%, the production cost of the negative electrode particles 100 increases. When the mass ratio of the soluble salt to the precursor is between 10% and 200%, the negative electrode particles 100 have more active ion storage sites, higher specific capacity, and lower production costs.
[0068] In some embodiments, the density of the precursor is greater than or equal to the density of the soluble salt in a molten state. In other words, the density of the precursor is greater than or equal to the density of the soluble salt melt.
[0069] When the density of the precursor is greater than or equal to the density of the soluble salt in the molten state, when the soluble salt is in the molten state, the precursor can fully contact the soluble salt, and the molten soluble salt can better occupy the pores in the precursor, preventing the pores from shrinking rapidly or even closing under the action of high temperature.
[0070] In some embodiments, the precursor is placed in the soluble salt system and pre-carbonized at a first temperature, including placing the precursor in the soluble salt system and heating it to a first temperature at a first heating rate R1 in the range of 0.5°C / min≤R1≤3°C / min to pre-carbonize the precursor, wherein the range of the first temperature T1 is: 400°C≤T1≤1000°C.
[0071] Specifically, the first heating rate R1 can be 0.5°C / min, 1°C / min, 2°C / min, 3°C / min, or any value therebetween. Specifically, the first temperature T1 can be 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, or any value therebetween.
[0072] When the first heating rate R1 is less than 0.5°C / min, the heating process takes too long, increasing manufacturing costs. When the first heating rate R1 is greater than 3°C / min, the volatiles escape quickly, resulting in larger pores, which increases the binding energy of the active ions and hinders the insertion and extraction of active ions. When the first heating rate R1 is between 0.5°C / min and 3°C / min, it helps form smaller pores without significantly increasing manufacturing costs.
[0073] When the first temperature T1 is less than 400°C, the fusible salt cannot become molten, or the volatile matter cannot be completely volatilized. When the first temperature T1 is greater than 1000°C, the pores obtained after the volatile matter escapes will shrink or even partially close, resulting in the fusible salt being unable to be removed in the subsequent process, affecting the gram capacity of the negative electrode particles 100 and increasing the manufacturing cost. When the first temperature T1 is between 400°C and 1000°C, the fusible salt is in a molten state, and the volatile matter in the precursor gradually volatilizes at the first temperature and leaves pores. The molten fusible salt occupies the pores and can be easily removed in the subsequent process. After removing the fusible salt, carbonization is performed to obtain the negative electrode particles 100, and the pores in the negative electrode particles 100 are relatively small.
[0074] In some embodiments, carbonizing the second particles at a second temperature to obtain the negative electrode particles 100 includes heating the second particles to a second temperature at a second heating rate R2 in the range of 1°C / min≤R2≤10°C / min to carbonize the second particles, wherein the second temperature T2 is in the range of 1000°C≤T2≤1700°C.
[0075] Specifically, the second heating rate R2 can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, or any value therebetween. Specifically, the second temperature T2 can be 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, or any value therebetween.
[0076] When the second heating rate R2 is less than 1°C / min, the heating process takes too long, increasing manufacturing costs. Furthermore, the content of closed pores 101 within the negative electrode particles 100 is low, hindering the improvement of the specific capacity of the negative electrode particles 100. When the second heating rate R2 is greater than 10°C / min, the heating equipment suffers significant wear and tear, shortening its service life. When the second heating rate R2 is between 1°C / min and 10°C / min, the degree of disorder within the negative electrode particles 100 increases, increasing the internal closed pores 101 and thereby increasing the specific capacity of the negative electrode particles 100.
[0077] When the second temperature T2 is less than 1000°C, the negative electrode particles 100 have many defects, resulting in a low initial efficiency. When the second temperature T2 is greater than 1700°C, the interlayer spacing of the negative electrode particles 100 becomes smaller, which is not conducive to the storage of active ions and increases the manufacturing cost of the negative electrode particles 100. When the second temperature T2 is between 1000°C and 1700°C, the negative electrode particles 100 have a high initial efficiency, are easy to store active ions, and do not significantly increase the manufacturing cost.
[0078] In some embodiments, the second heating rate R2 is greater than the first heating rate R1.
[0079] When the second heating rate R2 is greater than the first heating rate R1, it is helpful to form smaller pores and can also aggravate the disorder inside the negative electrode particles 100, increase the internal micropores, and increase the gram capacity of the negative electrode particles 100.
[0080] In some embodiments, after removing the soluble salt in the first particle to obtain the second particle, and before carbonizing the second particle at a second temperature, the method further includes: depositing a carbon layer on the surface of the second particle to close some of the open pores 102 located on the surface of the second particle to form closed pores 101, so that the obtained negative electrode particles 100 have more closed pores 101 and less open pores 102.
[0081] It will be appreciated that the carbon layer may be deposited on the surface of the particles by chemical vapor deposition.
[0082] By depositing a carbon layer on the surface of the second particles, part of the open pores 102 on the surface of the second particles are closed to form closed pores 101 , which can prevent the increase of side reactions between the negative electrode particles 100 and the electrolyte and prevent the initial efficiency of the negative electrode particles 100 from decreasing.
[0083] In some embodiments, after carbonizing the second particles at the second temperature, the method further includes: depositing a carbon layer on the surface of the carbonized second particles to close some of the open pores 102 on the surface of the carbonized second particles to form closed pores 101.
[0084] By depositing a carbon layer on the surface of the carbonized second particles, some of the open pores 102 on the surface of the carbonized second particles are closed to form closed pores 101, thereby preventing an increase in side reactions between the negative electrode particles 100 and the electrolyte and preventing a decrease in the initial efficiency of the negative electrode particles 100.
[0085] In some embodiments, the carbon layer is deposited at a third temperature T3 for a deposition time of 1 hour to 4 hours, wherein the third temperature T3 is in the range of 800° C. ≤ T3 ≤ 1200° C.
[0086] Specifically, the third temperature T3 may be 800° C., 850° C., 900° C., 950° C., 1000° C., 1100° C., 1200° C., or any value therebetween. The deposition time may be 1 hour, 2 hours, 3 hours, 4 hours, or any value therebetween.
[0087] When the third temperature T3 is less than 800°C, the deposited carbon layer has poor electrical conductivity. When the third temperature T3 is greater than 1200°C, the interlayer spacing between the negative electrode particles 100 is small, affecting the dynamic performance. When the third temperature T3 is between 800°C and 1200°C, the deposited carbon layer has both good electrical conductivity and good dynamic performance.
[0088] Please refer to Figures 3 and 4. The third embodiment of the present application provides a negative electrode plate 200, which includes: a current collector 210 and an active material layer 220. The active material layer 220 is arranged on the surface of the current collector 210, and the active material layer 220 includes the negative electrode particles 100 described in the embodiment of the present application.
[0089] It is understood that the current collector 210 may be, but is not limited to, copper foil, aluminum foil, etc.
[0090] Please refer to Figures 5 and 6. The fourth embodiment of the present application provides an energy storage device 300, which includes: an electrolyte, a positive electrode plate 320, a diaphragm 310 and the negative electrode plate 200 described in the embodiment of the present application, the positive electrode plate 320 is at least partially immersed in the electrolyte, the diaphragm 310 is located on one side of the positive electrode plate 320 and is at least partially immersed in the electrolyte, and the negative electrode plate 200 is arranged on the side of the diaphragm 310 away from the positive electrode plate 320 and is at least partially immersed in the electrolyte.
[0091] The energy storage device 300 of the embodiment of the present application may be, but is not limited to, a lithium-ion secondary energy storage device 300 , a lithium-ion primary energy storage device 300 , a sodium-ion energy storage device 300 , a lithium-sulfur energy storage device 300 , or the like.
[0092] It is understandable that the energy storage device 300 may be, but is not limited to, a battery cell, a battery module, a battery pack, etc.
[0093] Optionally, the diaphragm 310 may be, but is not limited to, at least one of a polypropylene film (PP) and a polyethylene film (PE).
[0094] The present application is further described below with reference to the following examples. It should be understood that the examples provided herein are merely to aid understanding of the present application and should not be considered as specific limitations of the present application.
[0095] For ease of understanding, the present application lists the following examples. Those skilled in the art should understand that if no specific conditions are specified in the examples, the conventional conditions should be followed.
[0096] Example 1
[0097] 1) Preparation of negative electrode particles 100:
[0098] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0099] In the second step, the crushed precursor coconut shell is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0100] In the third step, the precursor coconut shell powder after ash removal and potassium hydroxide were mixed in a ratio of 1:1 and loaded into a crucible; the mixture was placed in a tube furnace, heated to 650°C at a rate of 0.5°C / min under a protective atmosphere and kept at this temperature for 2 hours; after the holding period, the mixture was cooled and set aside;
[0101] In the fourth step, the cooled precursor coconut shell powder and potassium hydroxide mixture is poured into pure water, washed and filtered multiple times to obtain pre-carbonized coconut shell powder, which is then dried for later use;
[0102] In the fifth step, a protective gas was introduced into the tubular furnace, and the pre-carbonized precursor coconut shell powder was heated to 1400°C at a rate of 2°C / min and kept at this temperature for 6 hours. After the heat preservation was completed, it was cooled to room temperature to obtain the negative electrode particles 100 hard carbon. The parameters such as the closed pore volume and true density of the hard carbon are shown in Table 2.
[0103] 2) Preparation of negative electrode sheet 200: Disperse negative electrode particles 100 hard carbon, conductive carbon SP and binder CMC in deionized water at a mass ratio of 90:5:5 and mix them evenly to obtain negative electrode slurry. Apply the negative electrode slurry on the negative electrode current collector 210 copper foil and dry it. The coating weight of the negative electrode active material layer 220 is 3 mg / cm 2 After rolling and punching, the negative electrode sheet 200 is obtained.
[0104] 3) Preparation of diaphragm 310:
[0105] A 16 μm polyethylene film is used as the separator 310 .
[0106] 4) Preparation of electrolyte:
[0107] Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1 to obtain a mixed solvent, and then dry sodium salt NaPF6 was added thereto to prepare an electrolyte with a concentration of 1 mol / L.
[0108] 5) Preparation of the energy storage device 300: Provide a sodium sheet, and place the sodium sheet, the above-mentioned separator 310, and the negative electrode plate 200 in the negative electrode side housing of a button battery in that order, so that the separator 310 is located between the sodium sheet and the negative electrode plate 200 to act as an insulator, drip two drops of electrolyte, and then place the button battery into the positive electrode side housing to obtain the energy storage device 300 described in Example 1.
[0109] Example 2 and Example 3
[0110] 1) Preparation of negative electrode particles 100:
[0111] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0112] In the second step, the crushed precursor coconut shell is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0113] In the third step, the precursor coconut shell powder after ash removal and potassium hydroxide were mixed in a ratio of 1:1 and loaded into a crucible; the mixture was placed in a tube furnace, heated to 650° C. at a certain first heating rate R1 under a protective atmosphere and kept at this temperature for 2 hours; after the holding period, the mixture was cooled for standby use; the first heating rate R1 is specifically shown in Table 1;
[0114] In the fourth step, the cooled precursor coconut shell powder and potassium hydroxide mixture is poured into pure water, washed and filtered multiple times to obtain pre-carbonized coconut shell powder, which is then dried for later use;
[0115] In the fifth step, a protective gas was introduced into the tubular furnace, and the pre-carbonized precursor coconut shell powder was heated to 1400°C at a rate of 2°C / min and kept at this temperature for 6 hours. After the heat preservation was completed, it was cooled to room temperature to obtain the negative electrode particles 100 hard carbon. The parameters such as the closed pore volume and true density of the hard carbon are shown in Table 2.
[0116] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0117] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0118] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0119] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0120] Example 4 and Example 5
[0121] 1) Preparation of negative electrode particles 100:
[0122] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0123] In the second step, the crushed precursor coconut shell is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0124] In the third step, the precursor coconut shell powder after ash removal and potassium hydroxide were mixed in a ratio of 1:1 and loaded into a crucible; the mixture was placed in a tube furnace, heated to 650°C at a rate of 0.5°C / min under a protective atmosphere and kept at this temperature for 2 hours; after the holding period, the mixture was cooled and set aside;
[0125] In the fourth step, the cooled precursor coconut shell powder and potassium hydroxide mixture is poured into pure water, washed and filtered multiple times to obtain pre-carbonized coconut shell powder, which is then dried for later use;
[0126] In the fifth step, a protective gas is introduced into the tubular furnace, and the pre-carbonized precursor coconut shell powder is heated to 1400°C at a certain second heating rate R2 and kept warm for 6 hours; after the insulation is completed, it is cooled to room temperature to obtain the negative electrode particles 100 hard carbon; the second heating rate R2 is specifically shown in Table 1, and the parameters such as the closed pore volume 101 and true density of the hard carbon are shown in Table 2.
[0127] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0128] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0129] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0130] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0131] Example 6 and Example 7
[0132] 1) Preparation of negative electrode particles 100:
[0133] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0134] In the second step, the crushed precursor coconut shell is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0135] In the third step, the precursor coconut shell powder after ash removal and potassium hydroxide were mixed in a ratio of 1:1 and loaded into a crucible; the mixture was placed in a tube furnace, heated to 650°C at a rate of 0.5°C / min under a protective atmosphere and kept at this temperature for 2 hours; after the holding period, the mixture was cooled and set aside;
[0136] In the fourth step, the cooled precursor coconut shell powder and potassium hydroxide mixture is poured into pure water, washed and filtered multiple times to obtain pre-carbonized coconut shell powder, which is then dried for later use;
[0137] In the fifth step, a protective gas is introduced into the tubular furnace, and the pre-carbonized precursor coconut shell powder is heated to a second temperature T2 at a rate of 2°C / min and kept warm for 6 hours. After the insulation is completed, it is cooled to room temperature to obtain the negative electrode particles 100 hard carbon. The second temperature T2 is specifically shown in Table 1, and the parameters such as the closed pore volume 101 and true density of the hard carbon are shown in Table 2.
[0138] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0139] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0140] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0141] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0142] Example 8
[0143] 1) Preparation of negative electrode particles 100:
[0144] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0145] In the second step, the crushed precursor coconut shell is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0146] In the third step, the precursor coconut shell powder after ash removal and potassium hydroxide were mixed in a ratio of 1:1 and loaded into a crucible; the mixture was placed in a tube furnace, heated to 650°C at a rate of 0.5°C / min under a protective atmosphere and kept at this temperature for 2 hours; after the holding period, the mixture was cooled and set aside;
[0147] In the fourth step, the cooled precursor coconut shell powder and potassium hydroxide mixture is poured into pure water, washed and filtered multiple times to obtain pre-carbonized coconut shell powder, which is then dried for later use;
[0148] In the fifth step, a protective gas is introduced into the tubular furnace, and the pre-carbonized precursor coconut shell powder is heated to 1000°C at a rate of 2°C / min. A certain proportion of acetylene is introduced and the mixture is kept warm for 2 hours. After the insulation is completed, the acetylene is stopped and the mixture is cooled to room temperature under a protective atmosphere to obtain the negative electrode particles 100 hard carbon. The parameters such as the closed pore volume and true density of the hard carbon are shown in Table 2.
[0149] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0150] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0151] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0152] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0153] Comparative Example 1
[0154] 1) Preparation of negative electrode particles 100:
[0155] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0156] In the second step, the crushed precursor coconut shell powder is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0157] In the third step, the precursor coconut shell powder after ash removal is loaded into a crucible, placed in a tubular furnace, and heated to 650°C at 6°C / min under a protective atmosphere and kept warm for 2 hours; after the insulation is completed, the temperature is increased to 1400°C at 2°C / min and kept warm for 6 hours; after the insulation is completed, it is cooled to room temperature to obtain the negative electrode particles 100 hard carbon; the parameters such as the closed pore volume, true density, etc. of the hard carbon are shown in Table 2.
[0158] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0159] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0160] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0161] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0162] Comparative Example 2
[0163] 1) Preparation of negative electrode particles 100:
[0164] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0165] In the second step, the crushed precursor coconut shell powder is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0166] In the third step, the precursor coconut shell powder after ash removal is loaded into a crucible, placed in a tube furnace, and heated to 1400°C at 5°C / min and kept warm for 6 hours; after the insulation is completed, it is cooled to room temperature to obtain the negative electrode particles 100 hard carbon; the parameters such as the closed pore volume and true density of the hard carbon are shown in Table 2.
[0167] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0168] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0169] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0170] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0171] Comparative Example 3
[0172] 1) Preparation of negative electrode particles 100:
[0173] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0174] In the second step, the crushed precursor coconut shell is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0175] In the third step, the precursor coconut shell powder after ash removal and potassium hydroxide were mixed in a ratio of 1:1 and loaded into a crucible; the mixture was placed in a tube furnace, heated to 300°C at a rate of 0.5°C / min under a protective atmosphere and kept at this temperature for 2 hours; after the holding period, the mixture was cooled and set aside;
[0176] In the fourth step, the cooled precursor coconut shell powder and potassium hydroxide mixture is poured into pure water, washed and filtered multiple times to obtain pre-carbonized coconut shell powder, which is then dried for later use;
[0177] In the fifth step, a protective gas was introduced into the tubular furnace, and the pre-carbonized precursor coconut shell powder was heated to 1400°C at a rate of 5°C / min and kept at this temperature for 6 hours. After the insulation was completed, it was cooled to room temperature to obtain the negative electrode particles 100 hard carbon. The parameters of the closed pore 101 pore volume, true density, etc. of the hard carbon are shown in Table 2.
[0178] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0179] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0180] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0181] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0182] Comparative Example 4
[0183] 1) Preparation of negative electrode particles 100:
[0184] In the first step, the precursor coconut shell was crushed to 8 μm and collected for later use;
[0185] In the second step, the crushed precursor coconut shell powder is chemically deashed using a mixture of 5M / L hydrochloric acid and 20% hydrofluoric acid, washed with water, and dried for later use;
[0186] In the third step, the precursor coconut shell powder after ash removal is loaded into a crucible, placed in a tubular furnace, and heated to 650°C at 0.5°C / min under a protective atmosphere and kept warm for 2 hours; after the insulation is completed, the temperature is increased to 1100°C at 2°C / min and kept warm for 6 hours; after the insulation is completed, it is cooled to room temperature to obtain the negative electrode particles 100 hard carbon; the closed pore 101 pore volume, true density and other parameters of the hard carbon are shown in Table 2.
[0187] 2) Preparation of the negative electrode sheet 200: the same as the preparation of the negative electrode sheet 200 in Example 1.
[0188] 3) Preparation of the diaphragm 310: The preparation of the diaphragm 310 is the same as that in Example 1.
[0189] 4) Preparation of electrolyte: the same as the preparation of electrolyte in Example 1.
[0190] 5) Preparation of the energy storage device 300: The preparation of the energy storage device 300 is the same as that described in Example 1.
[0191] Performance Testing
[0192] 1) Pore volume of the closed pores 101 of the negative electrode particles 100
[0193] The pore volume of the closed pores 101 of the negative electrode particles 100 = 1 / ρ1 - 1 / ρ2.
[0194] 2) The pore size of the closed pores 101 of the negative electrode particles 100
[0195] The following parameters were obtained by using small angle X-ray scattering (SAXS) testing:
[0196] The closed cell 101 Wherein, Δρ is the contrast, F(Q,r) is the scattering shape factor, V(r) is the volume of the negative electrode particle 100, N is the total number of negative electrode particles 100, and P(r) is the probability of the negative electrode particle 100 of size r appearing.
[0197] 3) Specific surface area of the closed pores 101 of the negative electrode particles 100
[0198] Using small angle X-ray scattering (SAXS), the scattering vector q and scattering intensity I(q) are obtained, where 2θ is the scattering angle, λ is the wavelength of X-rays, where K = lim q→∞ q 4 I(q), K is the Porod constant, the specific surface area of the closed pore 101 Wherein, A is the porosity of the negative electrode particle 100 .
[0199] 4) Pore volume of the opening 102 of the negative electrode particle 100
[0200] Using an ASAP2460 physical adsorption analyzer, the dried and degassed sample was placed in liquid nitrogen. The nitrogen adsorption was measured at different test pressures, and adsorption and desorption isotherms were plotted. The pore shape was determined based on the shape of the hysteresis loop, yielding the pore volume of the opening 102.
[0201] 5) Specific surface area of the openings 102 of the negative electrode particles 100
[0202] The ASAP2460 physical adsorption analyzer is used to place the dried and degassed sample in liquid nitrogen. Different test pressures are adjusted to measure the adsorption amount of nitrogen and obtain the specific surface area of the opening 102.
[0203] 6) Negative electrode particles 100% true density
[0204] The true density was tested using the American Quantachrome UltraPYC 1200e fully automatic true density analyzer using the true density liquid analysis method.
[0205] 7) Energy storage device 300 times rate performance
[0206] The energy storage device 300 obtained in the above embodiment was subjected to a rate test on a charge-discharge instrument. The test temperature was 25°C, and the device was cycled three times at a rate of 0.5C (i.e., both the charge rate and the discharge rate were 0.5C). The third charge capacity was recorded as C1. The device was then discharged at a rate of 0.1C, and then fully charged at a rate of 0.1C. The charge capacity was recorded as C2. The 0.5C / 0.1C rate capacity retention ratio was C2 / C1.
[0207] 8) 300-cycle performance of energy storage device
[0208] The energy storage device 300 obtained in the above embodiment was subjected to a charge-discharge cycle test on a charge-discharge instrument at a test temperature of 25°C, a cycle rate of 0.2C (i.e., both the charge rate and the discharge rate were 0.2C), and a charge voltage of 5mV to 2V. The capacity retention rate after the cycles was calculated. The capacity retention rate calculation formula is: Capacity retention rate after the nth cycle = (charge capacity after the nth cycle / maximum cycle charge capacity) × 100%.
[0209] It should be understood that the term "cycles" in this application refers to the number of times the energy storage device 300 is charged at a preset rate and discharged at a preset rate. One cycle is the number of times the energy storage device 300 completes a charge and discharge cycle. The 0.2C / 0.2C 50-cycle capacity retention rate refers to the capacity retention rate after the energy storage device 300 undergoes 50 charge and discharge cycles at a 0.2C charge rate and a 0.2C discharge rate at a test temperature of 25°C.
[0210] The first heating rates and first temperatures of Examples 1 to 8 and Comparative Examples 1 to 4 are shown in Table 1:
[0211] Table 1
[0212] Table 2
[0213] The test data of the energy storage device 300 is shown in Table 3:
[0214] Table 3
[0215] From the data in Table 2, the closed pore volume 101 of the negative electrode particles 100 of Comparative Example 1 is 0.139 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 12.99, the pore diameter of the closed pores 101 is 2.6nm, the gram capacity of the negative electrode particles 100 is only 262mAh / g, and the first efficiency is 86.5%, which is much lower than the gram capacity and first efficiency of Example 1. This is because there is no soluble salt during pre-carbonization in Comparative Example 1, and the first heating rate is faster, the volatile matter escapes faster, and the resulting pore diameter is larger. The pore volume of the closed pores 101 in Comparative Example 1 is too large, the pore diameter of the closed pores 101 is larger, the binding energy of the active ions becomes larger, which is not conducive to the embedding and extraction of active ions. The ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is large, which affects the electrolyte infiltration of the negative electrode particles 100, resulting in limited ion conduction channels, thereby reducing the gram capacity of the negative electrode particles 100.
[0216] The closed pore volume 101 of the negative electrode particles 100 of Comparative Example 2 is 0.135 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 12.86, the pore diameter of the closed pores 101 is 2.4nm, the gram capacity of the negative electrode particles 100 is only 267mAh / g, and the first efficiency is 86.1%, which is much lower than the gram capacity and first efficiency of Example 1. This is because Comparative Example 2 does not have a pre-carbonization process, and directly adopts a larger second heating rate for carbonization, which causes the volatiles in the precursor to escape too quickly, resulting in an increase in the pore diameter. The pore volume of the closed pores 101 in Comparative Example 2 is too large, and the pore diameter of the closed pores 101 is large. The binding energy of the active ions becomes larger, which is not conducive to the embedding and extraction of the active ions. The ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is large, which affects the electrolyte infiltration of the negative electrode particles 100, resulting in limited ion conduction channels, thereby reducing the gram capacity of the negative electrode particles 100.
[0217] The closed pore volume 101 of the negative electrode particles 100 of Comparative Example 3 is 0.132 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 12.69, the pore diameter of the closed pores 101 is 2.2nm, and the gram capacity of the negative electrode particles 100 is only 274mAh / g, with an initial efficiency of 86.7%, which are far lower than the gram capacity and initial efficiency of Example 1. This is because in Comparative Example 3, the first temperature is low, the soluble salt does not melt, and only some volatiles escape during the pre-carbonization process, forming some pores. However, the soluble salt is not melted and cannot occupy these pores. The second heating rate is fast, resulting in faster escape of volatiles during the carbonization process, resulting in a larger pore diameter of the closed pores 101. The binding energy of the active ions becomes larger, which is not conducive to the embedding and extraction of active ions, thereby reducing the gram capacity of the negative electrode particles 100.
[0218] The closed pores 101 of the negative electrode particles 100 of Example 2 have a pore size of 1.6 nm, a ratio of the specific surface area of the closed pores 101 to the specific surface area of the negative electrode particles 100 of 45.5, a gram capacity of the negative electrode particles 100 of 288 mAh / g, and an initial efficiency of 88.4%, which are lower than the gram capacity and initial efficiency of Example 1. The closed pores 101 of the negative electrode particles 100 of Example 3 have a pore size of 1.8 nm, a ratio of the specific surface area of the closed pores 101 to the specific surface area of the negative electrode particles 100 of 47.7, a gram capacity of the negative electrode particles 100 of 281 mAh / g, and an initial efficiency of 87.7%, which are slightly lower than the gram capacity and initial efficiency of Example 2. This is because as the first heating rate increases, the pore size of the closed pores 101 becomes larger, the binding energy of the active ions becomes larger, which is not conducive to the insertion and extraction of active ions, resulting in a decrease in the gram capacity and initial efficiency of the negative electrode particles 100.
[0219] The closed pore volume 101 of the negative electrode particles 100 of Example 4 is 0.0651 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 8.14, the gram capacity of the negative electrode particles 100 is 305 mAh / g, and the capacity retention rate of 50 cycles of 0.2C / 0.2C is 90%, which is slightly higher than the gram capacity of Example 1. This is because the second heating rate of Example 4 is relatively large, which will increase the degree of disorder inside the negative electrode particles 100, increase the tendency of the microcrystals to form pores, increase the internal micropores, and increase the gram capacity of the negative electrode particles 100. The pore volume of the closed pores 101 of the negative electrode particles 100 of Example 5 is 0.0677 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 8.36, the gram capacity of the negative electrode particles 100 is 309 mAh / g, and the capacity retention rate after 50 cycles of 0.2C / 0.2C is 90%, which is slightly lower than the cycle capacity retention rate of Example 4. This is because as the second heating rate continues to increase, the degree of disorder of the negative electrode particles 100 continues to increase, resulting in an increase in the gram capacity of the negative electrode particles 100.
[0220] The closed pore volume 101 of the negative electrode particles 100 of Example 6 is 0.0625 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 7.35, the gram capacity of the negative electrode particles 100 is 283 mAh / g, and the first efficiency is 88%, which is slightly lower than the gram capacity and first efficiency of Example 1. This is because the second temperature of Example 6 is slightly lower, which makes the negative electrode particles 100 have more defects, and the first efficiency and gram capacity are reduced. The pore volume of the closed pores 101 of the negative electrode particles 100 of Example 7 is 0.0501 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 6.51, and the gram capacity of the negative electrode particles 100 is 276 mAh / g, which is slightly lower than the gram capacity of Example 6. This is because the second temperature of Example 7 is higher. As the second temperature continues to increase, the interlayer spacing of the negative electrode particles 100 becomes smaller, which is not conducive to the storage of active ions, resulting in a decrease in the gram capacity of the negative electrode particles 100.
[0221] The pore volume of the closed pores 101 of the negative electrode particles 100 of Example 8 is 0.0783 cm 3 / g, the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102 is 10.3, the gram capacity of the negative electrode particles 100 is 316 mAh / g, and the first efficiency is 90.3%, all of which are significantly higher than the gram capacity and first efficiency of Example 1. This is because Example 5 adds chemical vapor deposition to close the pores 101, which increases the number of closed pores 101 in the negative electrode particles 100 and increases the ratio of the pore volume of the closed pores 101 to the pore volume of the open pores 102, thereby preventing serious side reactions between the negative electrode particles 100 and the electrolyte. At the same time, the negative electrode particles 100 have more active ion storage sites, resulting in higher gram capacity and first efficiency. In addition, because the chemical vapor deposition closes the pores 101 and a carbon layer is deposited on the surface, the specific surface area of the negative electrode particles 100 is small, but there are more closed pores 101 inside, resulting in better rate performance.
[0222] Mentioning "embodiments" and "implementation methods" in this application means that the specific features, structures or characteristics described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrases in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, unless there is a contradiction between them.
[0223] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solutions of the present application and are not limiting. Although the present application has been described in detail with reference to the above preferred implementation modes, ordinary technicians in this field should understand that the technical solutions of the present application can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A negative electrode particle, wherein: The negative electrode particles have closed pores located inside the negative electrode particles and open pores located on the surface of the negative electrode particles. The ratio of the pore volume of the closed pores to the pore volume of the open pores is in the range of 6≤C1 / C2≤11. The pore volume of the closed pores is in the range of 0.03cm 3 / g≤C1≤0.12cm 3 / g.
2. The negative electrode particle according to claim 1, wherein The average pore diameter D1 of the closed pores of the negative electrode particles is in the range of 0.8 nm ≤ D1 ≤ 2.0 nm.
3. The negative electrode particle according to claim 1, wherein The ratio of the specific surface area S1 of the closed pores of the negative electrode particles to the specific surface area S of the negative electrode particles is in the range of 40≤S1 / S≤200.
4. The negative electrode particle according to claim 3, wherein: The specific surface area S1 of the closed pores is in the range of: 40m 2 / g≤S1≤400m 2 / g; the specific surface area S of the negative electrode particles is in the range of: 1m 2 / g≤S≤5m 2 / g.
5. The negative electrode particle according to claim 1, wherein When the negative electrode particles have a layered structure, the ratio of the true density ρ1 of the negative electrode particles to the theoretical true density ρ2 of the negative electrode particles is in the range of 0.75≤ρ1 / ρ2≤0.
95.
6. A method for preparing negative electrode particles, wherein: include: Providing precursors and soluble salts; Placing the precursor in the soluble salt system, and pre-carbonizing the precursor at a first temperature to obtain first particles, wherein the first particles include the precursor and the soluble salt dispersed in the precursor, and the first temperature is higher than the melting temperature of the soluble salt; removing soluble salts in the first particles to obtain second particles; and The second particles are carbonized at a second temperature to obtain the negative electrode particles, wherein the second temperature is greater than the first temperature, the negative electrode particles have closed pores located inside the negative electrode particles and open pores located on the surface of the negative electrode particles, the ratio of the pore volume of the closed pores to the pore volume of the open pores is in the range of 6≤C1 / C2≤11, and the pore volume of the closed pores is in the range of 0.03cm 3 / g≤C1≤0.12cm 3 / g.
7. The method for preparing negative electrode particles according to claim 6, wherein: Placing the precursor in the soluble salt system and pre-carbonizing at a first temperature comprises: The precursor is placed in the soluble salt system, and the temperature is increased to a first temperature at a first heating rate R1 in the range of 0.5°C / min≤R1≤3°C / min to pre-carbonize the precursor, wherein the first temperature range is: 400°C≤T1≤1000°C.
8. The method for preparing negative electrode particles according to claim 7, wherein: The step of carbonizing the second particles at the second temperature to obtain the negative electrode particles comprises: The second temperature T2 is increased to a second temperature at a second heating rate R2 in the range of 1°C / min≤R2≤10°C / min to carbonize the second particles, wherein the second heating rate R2 is greater than the first heating rate R1, and the range of the second temperature T2 is: 1000°C≤T2≤1700°C.
9. The method for preparing negative electrode particles according to claim 6, wherein: The density of the precursor is greater than or equal to the density of the soluble salt in a molten state.
10. The method for preparing negative electrode particles according to claim 6, wherein: After removing the soluble salt in the first particles to obtain the second particles, and before carbonizing the second particles at the second temperature; or after carbonizing the second particles at the second temperature, the method further comprises: A carbon layer is deposited on the surface of the second particle or the second particle after carbonization, so that part of the open pores on the surface of the second particle or the second particle after carbonization are closed to form closed pores.
11. A negative electrode sheet, wherein: include: current collector; as well as An active material layer, wherein the active material layer is disposed on the surface of the current collector, and the active material layer comprises the negative electrode particles according to any one of claims 1 to 10.
12. An energy storage device, wherein: include: Electrolyte, A positive electrode sheet, wherein the positive electrode sheet is at least partially immersed in the electrolyte; a diaphragm, located on one side of the positive electrode plate and at least partially immersed in the electrolyte, and The negative electrode plate according to claim 11 is arranged on a side of the diaphragm away from the positive electrode plate and is at least partially immersed in the electrolyte.
Citation Information
Patent Citations
Negative-electrode active material for sodium-ion secondary battery, method for manufacturing said negative-electrode active material, and sodium-ion secondary battery
CN105247713A
Cathode active material for lithium secondary battery and prepattion method thereof
CN106450321A
Low-expansion silicon negative electrode material
CN114792782A
Composite negative electrode material, preparation method thereof and lithium ion battery
CN115172746A
High-rate hard carbon negative electrode material and preparation method and application thereof
CN115849332A