Light-emitting element, method producing light-emitting element, and display device
The introduction of a light-emitting element with a quantum dot-containing layer divided by gaps addresses the light extraction efficiency issue in QLEDs, enhancing brightness by scattering light at the interface, thus overcoming the refractive index-related challenges in QLEDs.
Patent Information
- Application Number
- PCT/JP2023/018995
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
QLED display devices face a reduction in light extraction efficiency due to total reflection at the interface between the light emitting layer and the transport layer, caused by the increased refractive index of inorganic materials used in QLEDs.
A light-emitting element with a stacked anode and cathode structure, including a functional layer with a light-emitting layer containing quantum dots, where the light-emitting layer is divided by gaps extending from the front to the back side, improving light extraction efficiency by scattering light at the interface.
Enhances light extraction efficiency and external quantum efficiency, leading to improved brightness in QLED display devices.
Smart Images

Figure JP2023018995_28112024_PF_FP_ABST
Abstract
Description
Light-emitting element, method for manufacturing the same, and display device
[0001] The present disclosure relates to a light-emitting element, a method for manufacturing a light-emitting element, and a display device.
[0002] In recent years, various display devices equipped with light-emitting elements have been developed, and in particular, display devices equipped with QLEDs (Quantum dot Light Emitting Diodes) or OLEDs (Organic Light Emitting Diodes) have attracted much attention because of their ability to achieve low power consumption, thinness, high image quality, etc. Patent Document 1 discloses an OLED with improved light output.
[0003] International Publication No. 2008 / 140644
[0004] On the other hand, because QLEDs use inorganic materials as light-emitting materials, the refractive index becomes high, which causes total reflection at the interface between the light-emitting layer and the transport layer, resulting in a problem of reduced light extraction efficiency.
[0005] In order to solve the above problems, a light-emitting element according to one aspect of the present disclosure includes a laminate of an anode, a cathode, and a functional layer located between the anode and the cathode, the functional layer having a light-emitting layer, the light-emitting layer including quantum dots, the light-emitting layer having a light-emitting region where the anode and the cathode face each other, and the light-emitting layer being divided by a gap extending from the front side to the back side of the light-emitting region.
[0006] A display device according to an aspect of the present disclosure includes a plurality of light-emitting elements according to an aspect.
[0007] A method for manufacturing a light-emitting element according to one aspect of the present disclosure is a method for manufacturing a light-emitting element according to one aspect, and includes the steps of: applying a dispersion liquid in which the quantum dots are dispersed in a solvent to either the anode, the cathode, or the functional layer; and evaporating the solvent by at least one of heating and reducing pressure to form a coating layer containing the quantum dots; and, after the step of forming the coating layer, further heating the coating layer to form the light-emitting layer having the gaps.
[0008] According to one aspect of the present disclosure, it is possible to improve the light extraction efficiency of a light-emitting element using quantum dots.
[0009] 1 is a plan view showing a schematic configuration of a display device 100 according to an embodiment of the present disclosure. FIG. 2 is a plan view showing a schematic configuration of light-emitting elements 1R, 1G, and 1B included in a plurality of light-emitting elements 1 provided in a display device 100 according to an embodiment of the present disclosure. FIG. 3 is a cross-sectional view showing a schematic configuration of light-emitting elements 1R, 1G, and 1B included in a light-emitting element 1 according to an embodiment of the present disclosure. FIG. 4 is a schematic flow diagram showing an example of a first manufacturing method for a light-emitting element 1, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a step of applying a quantum dot dispersion liquid containing quantum dots 30L1 and a precursor 31P, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a state of a layer obtained by applying a quantum dot dispersion liquid containing quantum dots 30L1 and a precursor 31P before heating, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a step of forming a light-emitting layer 24, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a step of forming an electron transport layer 22, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a step of forming an electron transport layer 22, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a step of forming an electron transport layer 22, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a step of applying a quantum dot dispersion liquid containing quantum dots 30L1 and a precursor 31P, the manufacturing method according to an embodiment of the present disclosure including: a diagram outlining a step of forming an electron transport layer 2 ... 1 is a diagram illustrating an outline of a light-emitting element 1 including a light-emitting layer 24 formed by a manufacturing method according to one aspect (first aspect) of the present disclosure. FIG. 2 is a diagram illustrating an outline of a step of applying quantum dot dispersion liquid containing quantum dots 30L1 and quantum dots 30L1, which is included in a manufacturing method according to one aspect (second aspect) of the present disclosure. FIG. 3 is a diagram illustrating an outline of a state of a light-emitting layer 24A obtained by applying a quantum dot dispersion liquid containing quantum dots 30L1 and quantum dots 30L2, before heating, which is included in a manufacturing method according to one aspect (second aspect) of the present disclosure. FIG. 4 is a diagram illustrating an outline of a light-emitting element 1A including a light-emitting layer 24A formed by a manufacturing method according to one aspect (second aspect) of the present disclosure. FIG. 5 is a fluorescent microscope image of the surface of the light-emitting layer in a light-emitting element according to Example 1 of the present disclosure. FIG. 6 is a fluorescent microscope image according to Example 1 of the present disclosure. FIG. 7 is a graph comparing the correlation between current density and EQE between light-emitting elements having cracks on the surface of the light-emitting layer and light-emitting elements not having cracks on the surface of the light-emitting layer, according to examples of the present disclosure.
[0010] <Overview of Display Device> Fig. 1 is a plan view showing an example of a schematic configuration of a display device 100 according to one embodiment of the present disclosure. As shown in Fig. 1, the display device 100 according to the present disclosure includes a display area DA that performs display by extracting light from light-emitting elements (described later) and a frame area NA that surrounds the periphery of the display area DA. Although not shown, terminals are formed in the frame area NA to which signals for driving the light-emitting elements of the display device 100 are input.
[0011] Fig. 2 is a plan view showing an example of a schematic configuration of the display area DA shown in Fig. 1. Fig. 2 corresponds to a plan view showing an enlarged view of one pixel PIX shown in Fig. 1. As shown in Fig. 2, the light-emitting element 1 includes light-emitting elements 1R, 1G, and 1B, and each of the light-emitting elements 1R, 1G, and 1B includes a light-emitting area 1R-LEA (Light Emitting Area), 1G-LEA, or 1B-LEA surrounded by a bank 12, which is a partition wall described below. Each of these light-emitting areas 1R-LEA, 1G-LEA, and 1B-LEA can constitute a sub-pixel within one pixel PIX shown in Fig. 1.
[0012] <Outline of Light-Emitting Element> The configuration of the first aspect of the light-emitting element 1 of the present disclosure will be described with reference to appropriate drawings. Fig. 3 is a cross-sectional view showing a schematic configuration of the light-emitting element 1 in one aspect, and corresponds to the cross-sectional view taken along line B-B in Fig. 2 .
[0013] 3 , the light-emitting elements 1R, 1G, and 1B in one embodiment include a substrate 4, anodes 10R, 10G, and 10B formed on the substrate 4, a cathode 16, and functional layers 14R, 14G, and 14B provided between the anodes 10R, 10G, and 10B and the cathode 16. Here, the functional layers 14R, 14G, and 14B provided on the anodes 10R, 10G, and 10B include a hole injection layer (HIL) 20, a hole transport layer (HTL) 22, one of emission layers (EML) 24R, 24G, and 24B, and an electron transport layer (ETL) 26. In the light-emitting elements 1R, 1G, and 1B, the hole injection layer 20 and the hole transport layer 22 are provided between the anode 10 and the light-emitting layer 24R, 24G, or 24B, and the electron transport layer 26 can also be expressed as being provided between the cathode 16 and the light-emitting layer 24R, 24G, or 24B. Note that, although Fig. 3 shows the light-emitting elements as having a conventional structure (forward stack structure) in which the anode is formed on the substrate, they may also be formed as having an inverted structure (inverted stack structure) in which the cathode, functional layer, and anode are formed in this order on the substrate.
[0014] 1 and 2, in the light-emitting elements 1R, 1G, and 1B, at least the anodes 10R, 10G, and 10B and the light-emitting layers 24R, 24G, and 24B are separated by the banks 12. As a result, the light-emitting elements 1R, 1G, and 1B have light-emitting regions 1R-LEA, 1G-LEA, and 1G-LEA surrounded by the banks 12.
[0015] As shown in Fig. 3, a light-emitting element 1G that emits green light is formed inside an opening of a bank 12 provided on a substrate 4. The substrate 4 may be an active matrix substrate, for example, on which a barrier layer (not shown), a thin-film transistor layer including a transistor TR, and an anode 10G are provided in this order from the substrate 4 side. Fig. 3 is a cross-sectional view mainly showing the light-emitting element 1G, but the light-emitting elements 1R and 1B may also have a configuration similar to that of the light-emitting element 1G.
[0016] The substrate 4 may be, for example, a resin substrate made of a resin material such as polyimide, or a glass substrate. When the display device 100 is a non-flexible display device, the substrate 4 may be a glass substrate.
[0017] The banks 12 that separate the light emitting regions 1R-LEA, 1G-LEA, and 1G-LEA can be made of a resin material such as polyimide or acrylic.
[0018] Each of the anodes 10R, 10G, and 10B is provided in an island shape for each sub-pixel included in one pixel PIX shown in Fig. 1, and is also called a "pixel electrode." The cathode 16 is also called a "common electrode."
[0019] Each of the anodes 10R, 10G, and 10B may be formed, for example, from an electrode material that reflects visible light, and the cathode 16 may be formed, for example, from an electrode material that transmits visible light.
[0020] The electrode material that reflects visible light is not particularly limited as long as it can reflect visible light and has conductivity, and examples thereof include metal materials such as Al, Cu, Au, Mg, Li, and Ag, alloys of the above metal materials, laminates of the above metal materials and transparent metal oxides (e.g., indium tin oxide, indium zinc oxide, indium gallium zinc oxide, etc.), and laminates of the above alloys and the above transparent metal oxides.
[0021] On the other hand, the electrode material that transmits visible light is not particularly limited as long as it can transmit visible light and has conductivity, and examples thereof include transparent metal oxides (e.g., indium tin oxide, indium zinc oxide, indium gallium zinc oxide, etc.), thin films made of metal materials such as Al and Ag, and nanowires made of metal materials such as Al and Ag.
[0022] The hole injection layer 20 may be a layer for injecting holes into the light-emitting layers 24R, 24G, and 24B. The hole injection layer 20 is a layer that transports holes from the anodes 10R, 10G, and 10B, respectively, toward the light-emitting layers 24R, 24G, and 24B, and may be one embodiment of a hole transport layer. Examples of hole-injecting materials contained in the hole injection layer include NiO, CuI, and Cu. 2 O, CoO, Cr 2 O 3 , CuAlS 2 The nanoparticles that are hole-injecting materials may have thiol, amine, or the like as ligands.
[0023] The hole transport layer 22 is a layer that transports holes from each of the anodes 10R, 10G, and 10B toward the light-emitting layer 24R, 24G, or 24B. The hole transport layer can be formed on the anode or the hole injection layer.
[0024] The material used in the hole transport layer is not particularly limited as long as it is a hole transport material that can stabilize the transport of holes to the light-emitting layers 24R, 24G, and 24B. The hole transport material in the hole transport layer preferably has high hole mobility. Furthermore, the hole transport material is preferably a material (electron-blocking material) that can prevent electrons transferred from the cathode 16 from penetrating through the hole transport layer. This is because the recombination efficiency of holes and electrons in the light-emitting layers 24R, 24G, and 24B can be increased. Examples of hole transport materials include poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine] (poly-TPD), polyvinylcarbazole (PVK), and poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl))diphenylamine)] (TFB). These hole transport materials may be used alone or in a suitable mixture of two or more types. A hole injection layer (not shown) may also be formed. Examples include a composite of poly(3,4-ethylenedioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS) (abbreviated as "PEDOT:PSS"), NiO (nickel oxide), and CuSCN (copper thiocyanate). These materials may be used alone or in a suitable mixture of two or more types.
[0025] The light-emitting layers 24R, 24G, and 24B are layers in which recombination of holes from the anode 10 and electrons from the cathode 16 occurs, exciting the light-emitting body, and emitting light when the excited light-emitting body returns to the ground state. The light-emitting layer 24 has a light-emitting region 1-LEA in the portion where the anode 10 and the cathode 16 face each other, and application of a voltage or current to the light-emitting region 1-LEA causes recombination in the light-emitting layer 24, resulting in light emission.
[0026] The light-emitting layers 24R, 24G, and 24B can emit any of red light, green light, and blue light in the light-emitting regions 1R-LEA, 1G-LEA, and 1B-LEA, respectively. Here, red light refers to light having a central emission wavelength in a wavelength band of more than 600 nm and not more than 780 nm. Furthermore, green light refers to light having a central emission wavelength in a wavelength band of more than 500 nm and not more than 600 nm. Furthermore, blue light refers to light having a central emission wavelength in a wavelength band of 400 nm or more and not more than 500 nm. In one embodiment, the multiple types of quantum dots are a combination of red quantum dots, green quantum dots, and blue quantum dots, but this combination is not necessarily required.
[0027] In the light-emitting regions 1R-LEA, 1G-LEA, and 1B-LEA, the light-emitting layer 24R, the light-emitting layer 24G, and the light-emitting layer 24B contain quantum dots with organic ligands as light emitters, respectively. Here, "quantum dots" means dots with a maximum width of 100 nm or less.
[0028] In the light-emitting device 1 according to one embodiment (first embodiment), the light-emitting layer 24, such as the light-emitting layer 24R, 24G, or 24B, preferably contains an aggregate of quantum dots 30 in a metal sulfide matrix 31, as described below ( FIG. 9 ). The metal sulfide matrix 31 may be formed from a metal sulfide precursor 31P, as described below.
[0029] In addition, in the light-emitting element according to one embodiment (second embodiment), the light-emitting layer 24 may include quantum dots 30L2 having a ligand L2 or quantum dots 30L3 having a ligand L3, as described below (FIG. 12).
[0030] The light-emitting layers 24R, 24G, and 24B may be continuous layers of a metal sulfide film containing quantum dots, as described below, and are divided by a plurality of gaps 32 extending from the front surface side to the back surface side. The manner in which the gaps 32 divide the light-emitting layer 24 is not particularly limited, but they may be formed as cracks that randomly divide each of the light-emitting layers 24R, 24G, and 24B in a top view of the light-emitting region of each of these light-emitting layers. Note that, for example, when the gaps 32 in the light-emitting layers 24R, 24G, and 24B are formed as random cracks, it is sufficient that at least a portion of the random cracks penetrate from the front surface side to the back surface side of the light-emitting layer. In other words, it is sufficient that at least a portion of the random cracks have a depth corresponding to the thickness of the light-emitting layers 24R, 24G, and 24B.
[0031] The light extraction efficiency of the light-emitting layers 24R, 24G, and 24B is improved by light scattering at the interfaces between the surfaces of these light-emitting layers and the surfaces of the gaps 32 and the electron transport layer 26. This increases the external quantum efficiency (EQE) of the light-emitting layers 24R, 24G, and 24B. The occupancy rate of the gaps 32 that provides an optimal light scattering effect can be expressed as follows. That is, the ratio of the area occupied by the gaps 32 on the surfaces of the light-emitting layers 24R, 24G, and 24B is preferably 5% to 10% of the surface area. The occupancy rate of the gaps 32 in each of the light-emitting layers 24R, 24G, and 24B can be determined by image analysis. More specifically, the occupancy rate of the gaps 32 can be determined by grayscale conversion and binarization of image data obtained from a photograph of the light-emitting element captured with a fluorescence microscope, and then evaluating the occupancy rate.
[0032] The width of the gap 32 is preferably greater than the wavelength of light emitted by the quantum dots and is preferably 2 μm or less. Here, the "width" of the gap 32 can be determined, for example, by photographing cracks extending randomly on the surface of the light-emitting layer, converting the photograph into grayscale, and using the binarized image data to identify the largest crack that satisfies the condition of being at least 5 μm in length, and then measuring the maximum width of the crack.
[0033] In the light-emitting layers 24R, 24G, and 24B, the degree of light scattering varies depending on the occupancy rate of the gaps 32, which can change the light extraction efficiency of the light-emitting layers. The light extraction efficiency can vary depending on the difference between the average refractive index of the gap-provided light-emitting layer and the material constituting the light-emitting layer, i.e., the refractive index of the light-emitting layer in the non-gap region. The greater the difference between the average refractive index of the gap-provided light-emitting layer and the refractive index of the material constituting the light-emitting layer, within the range of 0.1 to 1.0, the higher the light extraction efficiency of the light-emitting layer. The smaller the difference between the average refractive index of the gap-provided light-emitting layer and the refractive index of the material constituting the light-emitting layer, within the range of 0.1 to 1.0, the greater the proportion of the gaps in the light-emitting layer, which can prevent a deterioration in the electrical properties of the light-emitting layer itself. Here, the average refractive index of the gap-provided light-emitting layer and the refractive index of the material constituting the light-emitting layer can be measured using ellipsometry or the like.
[0034] 3, the end of the light-emitting layer 24R overlaps with the end of the light-emitting layer 24G, and the end of the light-emitting layer 24G overlaps with the end of the light-emitting layer 24B on the bank 12. Although not shown, the end of the light-emitting layer 24B may also overlap with the end of the light-emitting layer 24R. The overlapping of the ends of the light-emitting layers 24R, 24G, and 24B allows the thickness of the light-emitting layers on the bank 12 to be increased, making it difficult for current to flow through the light-emitting layers on the bank 12. This makes it possible to suppress unintended light emission on the bank 12.
[0035] In the light-emitting element 1, it is preferable to reduce the current that flows directly to the anode and cathode via only the hole injection layer 20 and the hole transport layer 22 in the functional layers 14R, 14G, and 14B, or via only the electron transport layer 26, that is, the so-called leakage current. Therefore, it is preferable that the gap 32 is filled with at least a layer that contacts the upper surface of the light-emitting region in which it is present, i.e., a portion of the electron transport layer 26. This structure can prevent leakage current from occurring in the gap 32 between the cathode 16 and the hole transport layer 22. Furthermore, because the hole transport layer 22 and the electron transport layer 26 are in direct contact with each other in the gap 32, it is preferable that the gap 32 have physical properties that prevent leakage current from occurring between the two layers. Specifically, it is preferable that the difference between the HOMO level of the material of the hole transport layer 22 and the HOMO level of the material of the electron transport layer 26 is 1.0 eV or more, preferably 1.5 eV or more, and more preferably 2.0 eV or more, and the difference between the LUMO level of the material of the hole transport layer 22 and the LUMO level of the material of the electron transport layer 26 is 1.0 eV or more, preferably 1.5 eV or more, and more preferably 2.0 eV or more.
[0036] The electron transport layer 26 transports electrons from the cathode 16 side toward the light-emitting layers 24R, 24G, and 24B. Although not shown, the charge transport layer may be composed of a plurality of layers.
[0037] The material used for the electron transport layer 26 is not particularly limited as long as it is an electron transport material that can stabilize the transport of electrons to the light emitting layers 24R, 24G, and 24B. Examples of the electron transport material include ZnO, ZnS, ZrO, MgZnO, AlZnO, and TiO. 2 These nanoparticles may have ligands, such as organic ligands and inorganic ligands, on their surfaces.
[0038] [Method for manufacturing light-emitting element according to first embodiment] The light-emitting element 1 according to the first embodiment can be provided by a first manufacturing method described below. Fig. 4 is a schematic flow diagram showing the first manufacturing method for the light-emitting element 1 according to one embodiment.
[0039] In the method for manufacturing a light-emitting element according to one embodiment, first, a substrate 4 is formed (step S2). The substrate 4 may be formed by, for example, forming a TFT directly on a rigid glass substrate.
[0040] Anodes are formed on the substrate 4 (step S4). The anodes may be formed, for example, by forming a thin film of a metal material by a sputtering method, a vacuum deposition method, or the like, and then patterning the thin film by dry etching or wet etching using a photoresist. As a result, island-shaped anodes 10 (i.e., anodes 10R, anode 10G, and anode 10B) are formed on the substrate 4 for each sub-pixel that constitutes one pixel PIX.
[0041] Next, an insulating bank 12 is formed (step S6) to cover the edge of the anode 10. The bank 12 is made of a resin material such as polyimide or acrylic, and can be formed into a desired pattern by photolithography.
[0042] Next, the hole injection layer 20 is formed (step S8). For example, the hole injection layer 20 may be formed by dispersing a hole injection material in a solvent to obtain a dispersion of a hole transport material, applying the dispersion of the hole injection material onto the bank 12 and the anode 10, and then volatilizing and removing the solvent from the hole injection material by heating or the like to form the hole injection layer 20.
[0043] Next, the hole transport layer 22 is formed (step S10). For example, the hole transport layer 22 may be formed by dissolving a hole transport material in a solvent to prepare a solution of the hole transport material, applying the solution of the hole transport material onto the hole injection layer 20, and then volatilizing and removing the solvent from the hole transport material by heating or the like to form the hole transport layer 22.
[0044] The hole injection layer 20 and the hole transport layer 22 may be formed without the patterning process after the solvent has been removed by evaporation. In this case, the manufacturing process is simplified and the layers can be manufactured easily. Alternatively, the hole injection layer and the hole transport layer on the banks between pixels may be formed as multiple discontinuous layers by patterning a thin film of a hole transport material by dry etching or wet etching using a photoresist.
[0045] Next, the light-emitting layer 24 is formed (step S12). As shown in FIGS. 4 to 7, the light-emitting layer 24 is formed by 1 and a metal sulfide precursor 31P is dissolved in the quantum dots 30L. 1 A step (S120) of applying the dispersion liquid onto the hole transport layer 22 and evaporating the solvent by at least one of heating and reducing pressure to form quantum dots 30L. 1 and forming a layer containing quantum dots 30L (S122). 1 and further heating the layer containing the compound (S124) to form the light-emitting layer 24 having the gap 32.
[0046] As mentioned above, the term "quantum dot" refers to a dot having a maximum width of 100 nm or less. 1 In the step (S120) of applying the dispersion liquid onto the hole transport layer 22, 1 The shape of the quantum dot 30 in which the coordinated atoms are located may be any shape as long as it satisfies the above-mentioned maximum width, and may be, for example, a spherical three-dimensional shape (circular cross-sectional shape), a polygonal cross-sectional shape, a rod-like three-dimensional shape, a branch-like three-dimensional shape, a three-dimensional shape having an uneven surface, or a combination thereof, but in one embodiment, a cubic shape is preferable.
[0047] The quantum dots 30 may have, for example, a core structure, a core / shell structure, a core / shell / shell structure, or a shell structure with a continuously varying core / shell ratio. The shell may completely cover the core or may only partially cover the core. The core may be composed of, for example, Si or C in the case of a unicomponent system; CdSe, CdS, CdTe, InP, GaP, InN, ZnSe, ZnS, or ZnTe in the case of a binary system; CdSeTe, GaInP, or ZnSeTe in the case of a ternary system; or AgInGaS (AIGS) in the case of a quaternary system. In the case of a binary system, the shell portion can be composed of, for example, CdS, CdTe, CdSe, ZnS, ZnSe, ZnTe, etc., and in the case of a ternary system, the shell portion can be composed of, for example, CdSSe, CdTeSe, CdSTe, ZnSSe, ZnSTe, ZnTeSe, AgInP (AIP), etc.
[0048] Quantum Dot 30L 1 In the dispersion, the organic ligand L coordinated to the quantum dots 30 1 has a coordinating group selected from the group consisting of an amino group, a mercapto group, a carboxylic acid group, and a phosphonic acid group, or a coordinating group selected from a dithiocarboxylic acid group, a xanthic acid group, and a thiourea group, and may have a hydrocarbon group having 1 to 5 carbon atoms, or may have a hydrocarbon group having 6 to 24 carbon atoms. 1 As a coordinating group of the ligand L, it is preferable that the ligand L has a coordinating group selected from a dithiocarboxylic acid group, a xanthogen acid group, and a thiourea group. 1 The quantum dots 30 can be encapsulated in a matrix 31 derived from the precursor 31P. 1 However, since it is not a halogen (halogen ion) such as chlorine, quantum dot 30L 1 This is preferable from the viewpoint that the repulsion between the precursor 31P and the precursor 31P can be suppressed and the gap 32 can be successfully formed as described later.
[0049] Quantum Dot 30L 1 30L of quantum dots contained in dispersion 1 The concentration of the quantum dots is not limited, but for example, 30 L 1 The content of the solvent may be in the range of 1.4 to 12.5 parts by mass, where the total of the solvent and the sol- vent is 100 parts by mass. This allows the light-emitting layer 24 containing the quantum dots 30 to be formed, and the light-emitting layer 24 to be heated, thereby generating cracks.
[0050] Quantum Dot 30L 1 The precursor 31P contained in the dispersion liquid is a metal complex, and the metal (metal ion) in the metal complex preferably contains, for example, zinc (Zn), magnesium (Mg), or gallium (Ga), and may further contain tellurium (Te), and more preferably the metal is zinc (Zn). In addition, the ligand of the metal complex that is the precursor 31P is the ligand L 1 The ligand may be a ligand having a coordinating group selected from a dithiocarboxylic acid group, a xanthogen acid group, and a thiourea group, and a hydrocarbon group having 1 to 24 carbon atoms.
[0051] The ligand of the metal complex precursor 31P is the ligand L 1 The ligand L has a coordinating group selected from a dithiocarboxylic acid group, a xanthogen acid group, and a thiourea group. 1 Then, the metal sulfide matrix 31 can be formed from the precursor 31P. 1 The larger the number of carbon atoms in the hydrocarbon group within the range of 1 to 24, the more the contraction of the metal sulfide can be enhanced, and the more successfully the gaps 32, which are cracks, can be formed. 1 The fewer the carbon atoms in the hydrocarbon group contained in the ligand L within the range of 1 to 24, the lower the thermal decomposition temperature can be. 1 The number of carbon atoms in the hydrocarbon group of the ligand L is preferably 6 to 24 from the viewpoint of facilitating crack formation, and is preferably in the range of 1 to 5 from the viewpoint of lowering the thermal decomposition temperature. 1is sometimes called a thermally decomposable ligand because it decomposes thermally upon heating.
[0052] Quantum Dot 30L 1 The concentration of the precursor 31P contained in the dispersion is not limited, but for example, 100 parts by mass of the quantum dots 30L 1 The content of the luminescent layer 24 may be in the range of 40 to 100 parts by mass relative to the total mass of the luminescent layer 24. This allows cracks to be generated while the luminescent layer 24 is being formed.
[0053] Quantum Dot 30L 1 In the dispersion liquid, quantum dots 30L 1 The solvent for dispersing the quantum dots 30L and dissolving the precursor 31P is preferably a non-polar solvent or a low-polarity solvent. Examples of the non-polar solvent include aromatic hydrocarbon solvents such as toluene and xylene, and examples of the low-polarity solvent include halogenated aromatic hydrocarbon solvents such as chlorotoluene, chlorobenzene, bromobenzene, and iodobenzene; halogenated aliphatic hydrocarbon solvents such as chloroform and tetrachloromethane; and ether solvents such as cyclopentyl methyl ether and dimethyl ether. By using a low-polarity solvent as the solvent, the quantum dots 30L can be easily dispersed. 1 In the dispersion liquid, quantum dots 30L 1 can be stably dispersed and the precursor 31P can be dissolved.
[0054] Quantum Dot 30L 1 The dispersion liquid can be applied to the hole transport layer 22 by a known coating method such as spin coating, slit coating, or ink jetting.
[0055] Quantum dots 30L shown in FIGS. 1 In the step (S122) of forming a layer containing the quantum dots 30L coated on the hole transport layer 22, the quantum dots 30L are formed by heating or reducing the pressure, or both. 1 The solvent can be removed from the dispersion. 1 A coating layer containing the quantum dots 30 is formed, and some of the quantum dots 30 aggregate in the coating layer, thereby forming quantum dot aggregates 30A. 1Quantum dots 30L can be formed. 1 The drying conditions (pre-drying conditions) for the coating layer formed by applying the dispersion liquid are not limited. However, the heating conditions are 1 The temperature may be in the range of 50°C to 200°C, for example, when isopropyl xanthate is used in combination with the ligand L 1 When using the quantum dot 30L as the ion source, the temperature is preferably 130°C or less. 1 This can also be referred to as a coating layer pre-drying step including the steps of:
[0056] In the step (S124) of forming the light-emitting layer 24 shown in FIGS. 4 and 7, the quantum dots 30L 1 By heating the coating layer containing the ligand L, the light-emitting layer 24 having the gap 32 is formed from the coating layer. In the process of forming the light-emitting layer 24, the coating layer is heated to form the ligand L 1 The reaction is carried out at a temperature equal to or higher than the decomposition temperature of the ligand L 1 The temperature may be designed depending on the type of the material, and is not limited thereto, but is preferably 200° C. or less. By heating at this temperature, a matrix 31 of metal sulfide derived from the precursor 31P, which is a metal complex contained in the coating layer, is generated. At this time, the quantum dots 30 and the quantum dot aggregates 30A 1 The gaps 32 are formed as cracks that are randomly formed in the top view of the light-emitting layer 24, starting from at least one of the above. Here, the precursor 31P can form a matrix 31 of metal sulfide as a result of thermal decomposition. The gaps 32 can be formed in the light-emitting layer 24 by the self-aggregation force between the quantum dots 30 and the metal sulfide contained in the matrix 31. Examples of the metal sulfide include ZnS (zinc sulfide), ZnTeS, and ZnMgS. 2 , MgS, Ga 2 S 3 , ZnGa 2 S 4 , MgGa 2 S 4These crystals may be contained in the matrix 31. The coating layer for forming the light-emitting layer 24 preferably contains aggregates of the quantum dots in a volume ratio of 4 to 100 times the volume of the primary particles of the quantum dots. This allows the occupancy rate of the gaps to be increased.
[0057] In the light-emitting device 1 according to one embodiment, the matrix 31 fills at least a portion of the gaps between the quantum dots in the light-emitting layer 24. The matrix refers to a material that contains and holds other substances, and can be referred to as a base material, a host material, or a filler. The matrix may be a material that contains and holds multiple quantum dots. The matrix may be filled into the light-emitting layer. The matrix may fill the region (space) between two adjacent quantum dots. The matrix may fill the region (space) in the light-emitting layer other than the multiple quantum dots. The term "a matrix being filled between multiple quantum dots" means that the region between two adjacent quantum dots is filled with the matrix, and it is sufficient to know this. Since the desired effect of the matrix is exerted at least in the region between two adjacent quantum dots, it is not necessarily necessary to know that the matrix is filled between all (more than two) quantum dots within a certain range. The outer edges (top and bottom surfaces) of the light-emitting layer may be covered with the matrix. Alternatively, the light-emitting layer may be configured such that a matrix portion extends from the outer edge, and the quantum dots are positioned away from the outer edge. The outer edge of the light-emitting layer may not be formed solely by the matrix, and a portion of the quantum dots may be exposed from the matrix. The matrix may refer to the portion of the light-emitting layer excluding the quantum dots. The matrix may contain multiple quantum dots. The matrix may be formed so as to partially or completely fill the space formed between two adjacent quantum dots. The light-emitting layer may have voids. The light-emitting layer may have multiple quantum dots, and the matrix may partially or completely fill the area other than the multiple quantum dots. Each of two adjacent quantum dots included in the multiple quantum dots may be embedded in the matrix with a gap therebetween. The matrix may be made of the same material as the shell of the quantum dots. In this case, the average distance between adjacent cores (core-to-core distance) of two adjacent quantum dots may be 3 nm or more, or may be 5 nm or more. Alternatively, the average distance between adjacent cores may be 0.5 times or more the average core diameter.The inter-core distance is, for example, the average distance between 20 adjacent cores in a space containing 20 cores. The inter-core distance should be kept wider than the distance when shells are in contact with each other. The average core diameter is, for example, the average core diameter of 20 cores in a cross-sectional observation of a space containing 20 cores. The core diameter can be the diameter of a circle having the same area as the core area in cross-sectional observation. The matrix may contain a substance different from the main material (e.g., an inorganic substance such as an inorganic semiconductor) as, for example, an additive. The observation results of a portion of the light-emitting layer may be applied to the entire light-emitting layer.
[0058] The continuous film means a film that is not divided by materials other than the material that constitutes the continuous film. The continuous film may be an integrated film that is connected without interruption by chemical bonds of the materials contained in the matrix. The continuous film of the light-emitting layer 24 has a thickness of 1000 nm or more in a plane perpendicular to the thickness direction at any position in the thickness direction. 2 The light-emitting layer 24 may have an area of 10 nm or more and have gaps, such as cracks, in the continuous film. The matrix may be, for example, an inorganic matrix composed mainly of an inorganic compound. The inorganic compound may be, for example, a metal sulfide such as ZnS. The average film thickness of the light-emitting layer 24 may be 10 nm or more and 100 nm or less.
[0059] 4 and 8, the electron transport layer 26 is formed (step S14). The electron transport layer 26 is preferably formed so as to cover the entire light-emitting layer 24, including the gap 32 above the light-emitting layer 24. The electron transport layer 26 can be formed, for example, by a method in which an electron transport material is dissolved in a solvent to obtain a solution, the solution of the electron transport material is applied onto the light-emitting layer 24 and the hole transport layer 22, and the solvent is volatilized and removed by heating or the like.
[0060] 4 and 9, the cathode 16 is formed (step S16). The cathode 16 may be formed by, for example, forming a thin film of a metal material by vacuum deposition, sputtering, or the like, in common with each sub-pixel. In this way, the light-emitting element 1 having the light-emitting region 1-LEA is formed.
[0061] Although not shown, the light-emitting element may include forming a sealing layer (step S18). The sealing layer covers the light-emitting layer 24 and the bank 12 and seals the light-emitting element 1. The sealing layer reduces the penetration of foreign matter, including moisture, into the light-emitting layer, electron transport layer, etc. from the outside of the sealing layer side of the light-emitting element. The sealing layer may have a laminated structure of, for example, an inorganic sealing film made of an inorganic material and an organic sealing film made of an organic material.
[0062] [Light-emitting device according to a second aspect and a manufacturing method according to the second aspect] The light-emitting device according to one aspect of the present disclosure and the manufacturing method of the light-emitting device are not limited to the first aspect. For example, a light-emitting device 1A according to a second aspect of the present disclosure includes a light-emitting layer 24A including a low-polarity ligand L 2 and highly polar ligand L 3 Quantum dots 30 (L 2 , L 3 ) and quantum dots 30 (L 2 , L 3 ) Aggregate 30A 2 For convenience of explanation, since steps S2 to S10 and steps S14 to S18 are the same as those in the first manufacturing method, their explanation will be omitted and only step S12 relating to the formation of the light-emitting layer 24 will be explained.
[0063] As shown in FIGS. 10 and 11, the method for forming the light-emitting layer 24A by the manufacturing method according to the second embodiment is as follows: 2 , and ligand L 3 Quantum dot 30 (L 2 , L 3 Quantum dots 30 (L 2 , L 3 ) to form a coating layer containing the above-mentioned components.
[0064] Quantum dot 30 (L 2 , L 3 ) is the ligand L 2 and the ligand L 2 is the above-mentioned L 1Among these, it is preferable that the ligand L has a coordinating group selected from the group consisting of an amino group, a mercapto group, a carboxylic acid group, and a phosphonic acid group, a coordinating group selected from the group consisting of an amino group, a mercapto group, a carboxylic acid group, and a phosphonic acid group, or a coordinating group selected from the group consisting of a dithiocarboxylic acid group, a xanthic acid group, and a thiourea group. 3 Preferably, the ligand L has a hydrocarbon group having 6 to 24 carbon atoms. 2 is the above-mentioned L 1 Among these, a ligand having a relatively low polarity is selected.
[0065] Quantum dot 30 (L 2 , L 3 ) is the ligand L 3 and the ligand L 3 may have a coordinating group selected from the group consisting of an amino group, a mercapto group, a carboxylic acid group, and a phosphonic acid group, or a coordinating group selected from a dithiocarboxylic acid group, a xanthic acid group, and a thiourea group. 3 preferably has a hydrocarbon group having 1 to 5 carbon atoms, and wherein the ligand L 3 In the hydrocarbon group having 1 to 5 carbon atoms, at least one hydrogen atom may be substituted with a hydroxyl group. 3 is the ligand L 1 Among these, the above-mentioned ligand L 2 The highly polar ligand is selected from those having a high polarity compared to the
[0066] Ligand L 2 and L 3 The difference in the number of carbon atoms in the hydrocarbon group between the quantum dots 30 (L 2 , L 3 ) When removing the solvent from the dispersion, aggregates 30A 2 and the aggregate 30A 2 This is more preferable because the gap 32 can be formed starting from this point.
[0067] Quantum dot 30 (L 2 , L 3) in which a ligand L selected from organic ligands with low polarity 2、 and highly polar ligand L 3 The ratio of quantum dots 30 (L 2 , L 3 The polarity of the solvent for dispersing the quantum dots 30 (L 2 , L 3 When a non-polar solvent or a low polarity solvent is used as a solvent for dispersing the ligand L 2 and highly polar ligand L 3 The mass ratio is L 2 : L 3 is preferably in the range of 1:1 to 4:1, and within this range, the highly polar ligand L 2 The larger the mass ratio of the quantum dots 30 (L 2 , L 3 ) After the dispersion liquid is applied, aggregate 30A 2 can be suitably formed.
[0068] Furthermore, for example, when a highly polar solvent is used as the solvent, a ligand L selected from low polar ligands is used. 2 and highly polar ligand L 3 The mass ratio is L 2 : L 3 is preferably in the range of 1:1 to 4:1, and within this range, the highly polar ligand L 3 The larger the mass ratio of the quantum dots 30 (L 2 , L 3 ) After the dispersion liquid is applied, aggregate 30A 2 can be suitably formed.
[0069] Quantum dot 30 (L 2 , L 3 Quantum dots 30 (L 2 , L 3 The concentration of the quantum dots 30 (L 2 , L 3 The total amount of the solvent and the ionic liquid may be in the range of 1.4 to 12.5 parts by mass, where 100 parts by mass is the total amount of the ionic liquid and the solvent. 2As a result, the light-emitting layer 24A having the gaps 32 formed therein can be formed.
[0070] Quantum dot 30 (L 2 , L 3 The solvent contained in the quantum dot dispersion liquid containing the hydroxybenzoates may be at least one solvent selected from non-polar solvents and low-polarity solvents. Non-polar solvents may be selected from aliphatic hydrocarbon solvents such as hexane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as toluene and xylene. In addition, low-polarity solvents may include the above-mentioned halogenated aromatic hydrocarbon solvents, halogenated aliphatic hydrocarbon solvents, and ether solvents.
[0071] Quantum dot 30 (L 2 , L 3 The solvent contained in the quantum dot dispersion liquid containing the dimethylformamide (DMF), N-methylformamide (NMF), N-methyl-2-pyrrolidone (NMP), and other amide-based solvents, ester-based solvents such as ethyl acetate and butyl acetate, ketone-based solvents such as acetone and methyl ethyl ketone, sulfoxide-based solvents such as dimethyl sulfoxide (DMSO), ether-based solvents known as highly polar solvents such as tetrahydrofuran (THF), thioether-based solvents such as diethyl sulfide (DES), and nitrile-based solvents such as acetonitrile and propionitrile.
[0072] Quantum dot 30 (L 2 , L 3 ) The dispersion liquids are made of ligands L having different polarities. 2 , L 3 As a result, as shown in FIG. 11, the quantum dots 30 (L 2 , L 3 ) aggregated aggregate 30A 2 At this time, quantum dots 30 (L 2 , L 3 ) Aggregates 30A of dispersion 212, an electron transport layer and a cathode are formed in the same manner as in the first embodiment, thereby manufacturing a light-emitting element 1A.
[0073] In addition, quantum dots 30 (L 2 , L 3 The dispersion may contain the precursor described above. For example, but not limited to, 100 parts by mass of quantum dots (L 2 , L 3 The precursor may be contained in a range of 0 to 100 parts by mass relative to the total amount of the metal sulfide. This may form a continuous film of metal sulfide in the light-emitting layer 24A.
[0074] 1 to 12, the light-emitting element 1 including a top-emission type light-emitting element and the manufacturing method thereof have been described, but the light-emitting element according to one embodiment is not limited to a top-emission type light-emitting element and may be a bottom-emission type light-emitting element. In this case, the light-emitting element may have a cathode disposed above the anode, the anode formed from an electrode material that transmits visible light, and the cathode formed from an electrode material that reflects visible light.
[0075] In one embodiment, the light-emitting element may have a forward stack structure, but is not limited thereto and may have an inverted stack structure. Although not shown, a light-emitting element having an inverted stack structure can be constructed by stacking an electron transport layer, an emitting layer, a hole transport layer, a hole injection layer, and an anode in this order from a cathode provided on a substrate. When the light-emitting element has an inverted stack structure, a hole transport layer may be filled in the gap provided in the emitting layer.
[0076] [Effects] According to the configuration and manufacturing method of the above-described embodiment, by using a quantum dot light-emitting layer having gaps, light is scattered at the interface of the light-emitting layer, including the gaps, and a light-emitting device is provided in which the light-extraction efficiency of the light-emitting layer is improved, thereby providing a light-emitting device with improved external quantum efficiency.
[0077] Furthermore, one aspect of the present disclosure includes a display device including a plurality of the light-emitting elements, thereby providing a QLED display device with improved brightness.
[0078] The present disclosure is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. An embodiment obtained by appropriately combining the technical means disclosed in each of the different embodiments is also included in the technical scope of the present disclosure. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment.
[0079] An embodiment of the present disclosure is described below.
[0080] A light-emitting element of Example 1 in which cracks were formed in the light-emitting layer and a light-emitting element of Comparative Example 1 in which cracks were not formed in the light-emitting layer were fabricated, and the voltage-current density characteristics, luminance-current density characteristics, and external quantum efficiency (EQE)-current density characteristics were evaluated.
[0081] (Preparation of composition for light-emitting layer) Example 1: 4 mg of quantum dots InP / ZnS (core / shell) and 150 mg of zinc isopropyl xanthate were stirred in DMF, and then the mixture was centrifuged to precipitate the quantum dots InP / ZnS, and the DMF was removed. The quantum dots InP / ZnS from which the DMF had been removed were redispersed in 0.2 ml of chlorobenzene to prepare a quantum dot dispersion (Sample 1) for forming the light-emitting device of Example 1.
[0082] It was confirmed by DLS that the quantum dot dispersion of Sample 1 contained aggregates of InP / ZnS (core / shell) quantum dots. It was confirmed by DLS that the volume-based median particle diameter (D50) of the primary particles was 8.4 nm, and the size of the aggregates was approximately 20 times larger. Comparative Example 1: A quantum dot dispersion (Comparative Sample 1) for forming the light-emitting device of Comparative Example 1 was prepared by dissolving 4 mg of InP / ZnS (core / shell) quantum dots in 0.2 ml of chlorobenzene.
[0083] (Fabrication of Light-Emitting Device) Using each of the compositions of Example 1, a light-emitting device was formed having a cathode, an electron transport layer (ETL), an emitting layer (EML), a hole transport layer (HTL), a hole injection layer (HIL), and an anode.
[0084] The materials used to form each layer are as follows: Cathode: Ag Electron transport layer: MgZnO Emitting layer: Sample 1 or Comparative Sample 1 Hole transport layer: TFB (American Dye Source) Hole injection layer: PEDOT and PSS composite Bank: Polyimide Anode: ITO / Ag Substrate: Glass An Ag / ITO anode and bank were patterned on a 5 cm x 5 cm substrate, and a hole injection layer and a hole transport layer were formed in this order on the formed anode. Next, the quantum dot dispersion of Sample 1 was spin-coated on the hole transport layer and heated and dried at 130 ° C. for 5 minutes (pre-drying). The substrate coated with Sample 1 was further heated at 150 ° C. for 30 minutes to form an emitting layer with cracks on the surface. Subsequently, a solution prepared by dissolving 20 mg of MgZnO, a material for the electron transport layer, in 1 ml of a solvent was spin-coated on the formed light-emitting layer, and the solution was dried by heating to form an electron transport layer. Furthermore, a cathode was formed, thereby forming the light-emitting element of Example 1.
[0085] Similarly, a light-emitting device of Comparative Example 1 was fabricated in accordance with the same procedure as that for the light-emitting device of Example 1, except that Comparative Sample 1 was used instead of Sample 1.
[0086] The HOMO and LUMO of TFB in the hole transport layer and the HOMO and LUMO of MgZnO in the electron transport layer, evaluated by electron yield spectroscopy (PYS) and ultraviolet-visible spectroscopy (UV-vis), are shown in Table 1 below.
[0087] [Evaluation of Refractive Index] For each of the light-emitting layers of Example 1 and Comparative Example 1, the difference between the average refractive index and the refractive index of the material constituting the light-emitting layer was measured using an ellipsometer M-2000 (manufactured by JA Woollam Japan).
[0088] The quantum dot dispersion of Sample 1 was spin-coated onto a hole transport layer prepared according to the procedure described above (Preparation of Light-Emitting Device), and the refractive index of the resulting layer was measured as the refractive index of the material of the light-emitting layer. The light-emitting layer of Sample 1, whose refractive index had been measured, was then further heated at 150°C for 30 minutes to form a light-emitting layer having cracks on the surface. The average refractive index of the light-emitting layer was measured, and the difference between the average refractive index of the light-emitting layer formed from Sample 1 and the refractive index of the material of the light-emitting layer was determined. The refractive index of the light-emitting layer was measured under the same conditions as Sample 1, except that Comparative Sample 1 was used, and the refractive index of the light-emitting layer heated at 130°C for 5 minutes was measured as the refractive index of the material of the light-emitting layer. The average refractive index of the light-emitting layer heated at 150°C for 30 minutes was then measured, and the difference between the average refractive index of the light-emitting layer formed from Comparative Sample 1 and the refractive index of the material of the light-emitting layer was determined.
[0089] The evaluation results of the difference between the average refractive index of the light-emitting layer and the refractive index of the material of the light-emitting layer are shown in Table 2 below.
[0090]
[0091] [Photographing Fluorescent Microscope Images and Evaluation of Crack Occupancy on the Surface of the Light-Emitting Layer] Fluorescent microscope images of the surface of the light-emitting layer were taken for the light-emitting element of Example 1. Fig. 13 shows a fluorescent microscope image of the surface of the light-emitting element of Example 1, and Fig. 14 shows an enlarged image of the fluorescent microscope image of the surface of the light-emitting element of Example 1. As shown in Figs. 13 and 14, it was confirmed that minute cracks were randomly formed on the surface of the light-emitting element of Example 1.
[0092] Next, the crack occupancy rate on the surface of the light-emitting layer was evaluated. Image data obtained from a photograph of the light-emitting element taken with a fluorescence microscope was converted to grayscale, and the crack occupancy rate on the surface of the light-emitting layer was calculated from the binarized data. The crack occupancy rate calculated from the photograph of the light-emitting element was 5.2%.
[0093] [Evaluation of crack width on the surface of the light-emitting layer] For the light-emitting element of Example 1, image data obtained from a photograph of the light-emitting element taken with a fluorescence microscope was converted to grayscale, and the width of the cracks on the surface of the light-emitting layer was determined from the binarized data. The largest crack satisfying the condition of a length of 62.5 μm was identified, and the maximum width of the crack was measured. The maximum crack width determined for the light-emitting element of Example 1 was 2 μm, which was confirmed to be larger than the wavelength of light emitted by the light-emitting element of Example 1, 634 nm.
[0094] [Evaluation of Current Density-External Quantum Efficiency] The current density-external quantum efficiency (EQE) characteristics were evaluated for each of the light-emitting devices of Example 1 and Comparative Example 1. The current density-external quantum efficiency evaluation was performed using an IVL characteristic evaluation device.
[0095] 15 is a graph showing the current density-external quantum efficiency (EQE) characteristics of the light-emitting elements of Example 1 and Comparative Example 1. As shown in Fig. 15, in the current density-external quantum efficiency characteristics, the external quantum efficiency of the light-emitting element of Example 1, in which cracks that are gaps are formed in the light-emitting layer, was higher than the external quantum efficiency characteristics of the light-emitting element of Comparative Example 1.
[0096] 1, 1A, 1R, 1G, 1B Light-emitting element 1-LEA, 1R-LEA, 1G-LEA, 1B-LEA, light-emitting region 4 Substrate 10, 10R, 10B, 10G Anode 12 Bank (partition) 14, 14R, 14G, 14B Functional layer 16 Cathode 20 Hole injection layer 22 Hole transport layer 24, 24A, 24R, 24G, 24B Light-emitting layer 26 Electron transport layer 30 Quantum dot 30A 1 , 30A 2 Aggregate 31P Precursor (metal complex) 31 Matrix (metal sulfide) L 1 , L 2 , L 3 Ligand (organic ligand) 32 Gap 100 Display device
Claims
1. A light-emitting element comprising: an anode, a cathode; and a functional layer located between the anode and the cathode, the functional layer having a light-emitting layer, the light-emitting layer including quantum dots, the light-emitting layer having a light-emitting region at a portion where the anode and the cathode face each other, the light-emitting layer being divided by a gap extending from the front side to the back side of the light-emitting region.
2. The light-emitting device of claim 1, wherein the light-emitting layer comprises a matrix of a metal sulfide.
3. The light-emitting device according to claim 2, wherein the matrix includes a continuous film of a metal sulfide encapsulating the quantum dots.
4. The light-emitting element according to claim 2 or 3, wherein the metal sulfide is derived from a metal complex, and the metal complex has a coordinating group selected from a dithiocarboxylic acid group, a xanthic acid group, and a thiourea group, and a hydrocarbon group having 1 to 24 carbon atoms.
5. The light-emitting device according to claim 4, wherein the hydrocarbon group is selected from hydrocarbon groups having 1 to 5 carbon atoms.
6. The light-emitting device according to claim 4, wherein the hydrocarbon group is selected from hydrocarbon groups having 6 to 24 carbon atoms.
7. The light-emitting device according to any one of claims 1 to 3, wherein the quantum dot comprises both a low-polarity organic ligand and a high-polarity organic ligand, each of the low-polarity organic ligand and the high-polarity organic ligand having a coordinating group selected from the group consisting of an amino group, a mercapto group, a carboxylic acid group, and a phosphonic acid group, a dithiocarboxylic acid group, a xanthic acid group, and a thiourea group, the high-polarity organic ligand having a hydrocarbon group selected from hydrocarbon groups having 1 to 5 carbon atoms, some of the hydrogen atoms of the hydrocarbon group having 1 to 5 carbon atoms being substituted with hydroxyl groups or not being substituted, and the low-polarity organic ligand having a hydrocarbon group selected from hydrocarbon groups having 6 to 24 carbon atoms.
8. The light-emitting device of claim 7, wherein the organic ligand has a coordinating group selected from the group consisting of an amino group, a mercapto group, a carboxylic acid group, and a phosphonic acid group.
9. The light-emitting element according to any one of claims 1 to 8, further comprising a partition wall surrounding either the anode or the cathode, and the light-emitting region.
10. The light-emitting element according to any one of claims 1 to 9, wherein the ratio of the area of the gap to the surface area of the light-emitting region is 5% or more and 10% or less.
11. The light-emitting device according to any one of claims 1 to 10, wherein the width of the gap is greater than the wavelength of light emitted by the quantum dot.
12. The light-emitting element according to any one of claims 1 to 11, wherein the width of the gap is 2 μm or less.
13. The light-emitting element according to any one of claims 1 to 12, wherein the gaps are cracks that randomly divide the light-emitting region.
14. The light-emitting device according to any one of claims 1 to 13, wherein the light-emitting layer contains aggregates of the quantum dots.
15. The light-emitting element according to any one of claims 1 to 14, comprising a hole transport layer and an electron transport layer as the functional layers, the hole transport layer being provided between the anode and the light-emitting layer, and the electron transport layer being provided between the cathode and the light-emitting layer.
16. The light-emitting element according to claim 15, wherein either the electron transport layer or the hole transport layer fills the gap in the light-emitting region.
17. The light-emitting device according to any one of claims 1 to 16, wherein the difference between the refractive index of the material of said light-emitting layer and the average refractive index of said light-emitting layer is within the range of 0.1 to 1.
0.
18. The light-emitting element according to claim 15 or 16, wherein the difference between the HOMO of the material of the hole transport layer and the HOMO of the material of the electron transport layer is 1.0 eV or more, and the difference between the LUMO of the material of the hole transport layer and the LUMO of the material of the electron transport layer is 1.0 eV or more.
19. A display device comprising a plurality of light-emitting elements according to any one of claims 1 to 18.
20. A method for manufacturing a light-emitting device according to any one of claims 1 to 6 and 8 to 18, comprising the steps of: applying a dispersion liquid in which the quantum dots are dispersed in a solvent onto any one of the anode, the cathode, or the functional layer, and evaporating the solvent by at least one of heating and reducing pressure to form a coating layer containing the quantum dots; and after the step of forming the coating layer, further heating the coating layer to form the light-emitting layer having the gaps, wherein the dispersion liquid contains at least one solvent selected from a non-polar solvent and a low-polarity solvent, the non-polar solvent being selected from an aromatic hydrocarbon solvent, and the low-polarity solvent being selected from at least one solvent selected from a halogenated aromatic hydrocarbon solvent, a halogenated aliphatic hydrocarbon solvent, and an ether solvent.
21. A method for manufacturing a light-emitting device according to any one of claims 1 and 7 to 18, comprising the steps of applying a dispersion liquid in which the quantum dots are dispersed in a solvent onto any one of the anode, the cathode, or the functional layer, and evaporating the solvent by at least one of heating and reducing pressure, thereby forming a light-emitting layer having the gaps, wherein the dispersion liquid is at least one solvent selected from a non-polar solvent, a low polarity solvent, and a high polarity solvent.
22. The manufacturing method described in claim 20 or 21, wherein the dispersion in which the quantum dots are dispersed in a solvent contains aggregates of the quantum dots in a volume ratio of 4 to 100 times the volume of the primary particles of the quantum dots.
Citation Information
Patent Citations
Light emitting diode and preparation method thereof
CN110364634A
Light-emitting device including semiconductor nanocrystal layer free of void and its manufacturing method
JP2007095685A
Light-emitting device and apparatus including the same
US20210296605A1
Light-emitting device, display apparatus and manufacturing method
US20220173344A1
Light-emitting device
WO2012161179A1