Exterior material for power storage device and power storage device
The exterior material for power storage devices, featuring a hydrophobic insulating inorganic filler-based adhesive layer and high-melting-point sealant layer, addresses the insulation issues under heated and pressurized conditions, preventing short circuits and ensuring reliable performance.
Patent Information
- Application Number
- PCT/JP2024/018873
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
Existing exterior materials for power storage devices, such as lithium secondary batteries, fail to maintain adequate insulation when heated and pressurized, leading to potential short circuits due to sealant flow and adhesive layer deformation.
An exterior material comprising a base material layer, a barrier layer, an adhesive layer with hydrophobic insulating inorganic fillers, and a sealant layer, where the adhesive layer is viscous and less likely to flow, enhancing insulation properties even under heated and pressurized conditions.
The proposed exterior material ensures superior insulation and prevents short circuits by maintaining adhesive layer integrity and sealant layer thickness, even when subjected to high temperatures and pressures.
Smart Images

Figure JP2024018873_28112024_PF_FP_ABST
Abstract
Description
Exterior material for power storage device and power storage device
[0001] The present disclosure relates to an exterior material for an electricity storage device and an electricity storage device.
[0002] Secondary batteries such as lithium ion batteries are widely used in portable electronic devices, electric vehicles, hybrid electric vehicles, and other devices powered by electricity. Lithium ion batteries generally include a battery cell containing a positive electrode and a negative electrode, and an outer bag containing the battery cell. The outer bag is obtained using an outer packaging material. Because such lithium secondary batteries can have large battery capacities and current draws, the outer packaging material is required to have better insulating properties to ensure higher safety. For example, Patent Document 1 below proposes a battery outer packaging material with excellent insulating properties, which is composed of an outer layer including a heat-resistant resin film, a metal foil layer, an adhesive layer, and an inner layer including a thermoplastic resin film. The adhesive layer contains insulating particles, and the insulating particles are either inorganic particles having an average particle size of 0.1 μm to 4 μm, organic particles having an average particle size of 0.1 μm to 4 μm, or a mixture of these. The amount of insulating particles added to the adhesive layer is 1 to 30% by mass.
[0003] JP 2014-127258 A
[0004] Lithium secondary batteries include all-solid-state batteries that use a solid electrolyte. Energy storage devices such as these all-solid-state batteries are sometimes constrained under pressure via an exterior material in a direction perpendicular to the surface of a battery cell containing a positive electrode, a solid electrolyte, and a negative electrode. This is intended to reduce the resistance between the positive electrode or negative electrode and the solid electrolyte by increasing the adhesion between the positive electrode or negative electrode and the solid electrolyte, thereby achieving and maintaining sufficient battery performance of the energy storage device. However, when the exterior material described in Patent Document 1 is used as an exterior bag for a battery cell, the battery cell may heat up. When the exterior material is pressurized under prolonged heating, the sealant layer may be crushed and further flow, potentially resulting in a short circuit between the metal layer of the exterior material and the positive electrode or negative electrode of the battery cell. Therefore, the exterior material described in Patent Document 1 leaves room for improvement in terms of insulation properties when used as an exterior bag for an energy storage device under heated and pressurized conditions.
[0005] The present disclosure has been made in consideration of the above-mentioned problems, and aims to provide an exterior material for an energy storage device and an energy storage device that have excellent insulating properties even when used under heated and pressurized conditions as an outer bag for the energy storage device.
[0006] In order to solve the above problems, the present disclosure provides an exterior packaging material for an electricity storage device, which comprises, in this order, at least a substrate layer, a barrier layer including a metal layer, an adhesive layer, and a sealant layer, wherein the adhesive layer contains a hydrophobic insulating inorganic filler.
[0007] The above-described packaging material exhibits excellent insulating properties even when used as an outer bag for an energy storage device under heated and pressurized conditions. The inventors of the present disclosure speculate that the reason for this effect is as follows. Specifically, in the packaging material of the present disclosure, the adhesive layer generally becomes a viscous fluid under prolonged heated and pressurized conditions. However, because the adhesive layer is adjacent to a barrier layer containing a metal layer, friction with the barrier layer makes the adhesive layer less likely to flow than the sealant layer. Furthermore, the hydrophobic insulating inorganic filler has hydrophobic properties, which increases affinity with other components in the adhesive layer and improves the cohesive strength of the adhesive layer. Therefore, the adhesive layer is less likely to flow even when heated and pressurized. Furthermore, the inclusion of the hydrophobic insulating inorganic filler in the adhesive layer makes it more likely for unevenness to form on the surface of the adhesive layer facing the sealant layer, increasing the contact area between the adhesive layer and the sealant layer and improving adhesion between the adhesive layer and the sealant layer, thereby making the sealant layer less likely to flow even when heated and pressurized. As a result, the adhesive layer and sealant layer are less likely to flow even when the packaging material is heated and pressurized. Furthermore, the hydrophobic insulating inorganic filler is less likely to deform under prolonged heating and pressure conditions than an insulating organic filler, and even if the adhesive layer is compressed by heating and pressure, the adhesive layer and sealant layer (hereinafter collectively referred to as the "insulating layer") can ensure a thickness at least equal to the size of the hydrophobic insulating inorganic filler. Furthermore, since electrically conductive moisture is less likely to adhere to the hydrophobic insulating inorganic filler, a decrease in the electrical resistance of the adhesive layer can be suppressed, and a decrease in the insulating properties of the adhesive layer can be suppressed. Based on the above, the inventors of the present disclosure speculate that the packaging material will have excellent insulating properties even when used under heated and pressurized conditions as an outer bag for battery cells of an energy storage device.
[0008] In the above-described packaging material for a storage battery device, the adhesive layer is preferably obtained using a composition containing the hydrophobic insulating inorganic filler, the composition containing the hydrophobic insulating inorganic filler, a resin, and a polyfunctional isocyanate compound, and the resin is a modified polyolefin resin. In this case, the reaction between the modified polyolefin resin and the polyfunctional isocyanate compound contained in the composition makes the adhesive layer obtained using the composition less likely to flow even under prolonged heating and pressure conditions, thereby more effectively preventing the insulating layer including the adhesive layer from collapsing. Therefore, the packaging material can have superior insulating properties even when used under heating and pressure conditions as an outer bag for a battery cell of a storage battery device. Furthermore, the adhesive layer is obtained using a composition containing a modified polyolefin resin, which further improves the adhesion of the adhesive layer to the barrier layer and the sealant layer. Furthermore, the composition further contains a polyfunctional isocyanate compound, which further improves the moisture barrier property while further improving the seal strength.
[0009] In the packaging material for a power storage device, the sealant layer preferably has an MFR of 20 g / 10 min or less. By making the sealant layer less likely to flow even under heated and pressurized conditions by setting the MFR of the sealant layer to 20 g / 10 min or less, the sealant layer is less likely to collapse even when the packaging material is used as an outer bag under heated and pressurized conditions, and the thickness of the insulating layer including the sealant layer can be sufficiently ensured, resulting in better insulating properties.
[0010] In the above-described packaging material for a power storage device, the melting point of the sealant layer is preferably 160°C or higher. By setting the melting point of the sealant layer to 160°C or higher, the flow of the sealant layer can be sufficiently suppressed even under heated and pressurized conditions. This makes it possible to more sufficiently suppress the crushing of the insulating layer including the adhesive layer. Therefore, the packaging material can have better insulating properties even when used under heated and pressurized conditions as an outer bag for a battery cell of a power storage device.
[0011] In the above-mentioned packaging material for a storage battery device, the hydrophobic insulating inorganic filler preferably has an average particle size of 1 to 20 μm. In this case, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm, the packaging material can have better insulating properties even when used under heated and pressurized conditions as an outer bag for a battery cell of a storage battery device. Furthermore, the hydrophobic insulating inorganic filler can be maintained in a well-dispersed state in the composition, which makes it difficult for the cohesive force of the adhesive layer to decrease, and makes it difficult for the adhesion strength of the adhesive layer to the barrier layer and sealant layer and the sealing strength of the sealant layer to decrease.
[0012] The packaging material for an electricity storage device preferably has a breakdown voltage of at least 100 V when heated and pressurized for 24 hours under conditions of 150° C. and 3 MPa. In this case, even under severe heating and pressurizing conditions, the packaging material can have better insulating properties when used under heated and pressurized conditions as an outer bag for a battery cell of an electricity storage device.
[0013] In the packaging material for a power storage device, the modified polyolefin resin is preferably an acid-modified polyolefin resin. This packaging material improves the adhesion of the adhesive layer to the barrier layer, making the adhesive layer less likely to flow even when the packaging material is heated and pressurized. Furthermore, the improved adhesion of the adhesive layer to the barrier layer also improves heat resistance.
[0014] In the packaging material for a power storage device, the polyfunctional isocyanate compound preferably contains an isocyanurate-type polyfunctional isocyanate compound. According to this packaging material, the polyfunctional isocyanate compound contains an isocyanurate-type polyfunctional isocyanate compound, which allows the adhesive layer to have excellent adhesion and heat resistance, and allows the adhesive layer to have high seal strength, heat resistance, and excellent barrier properties.
[0015] In the electrical storage device packaging material, the content of the hydrophobic insulating inorganic filler in the adhesive layer is preferably 0.5 to 20% by mass. In this case, compared to when the content of the hydrophobic insulating inorganic filler in the composition is less than 0.5% by mass, the packaging material is more likely to maintain a uniform thickness of the insulating layer, including the adhesive layer, even when used under heated and pressurized conditions as an outer bag for a battery cell of an electrical storage device. Furthermore, compared to when the content of the filler in the composition exceeds 20% by mass, the decrease in cohesive strength of the adhesive layer is suppressed, and the decrease in seal strength and adhesion is further suppressed. Furthermore, the decrease in brittleness of the adhesive layer can also be further suppressed.
[0016] In the energy storage device packaging material, the barrier layer may further include a corrosion prevention treatment layer on one or both surfaces of the metal layer. This packaging material improves adhesion of the adhesive layer to the corrosion prevention treatment layer and suppresses flow of the adhesive layer, allowing the packaging material to have better insulating properties even when used under heated and pressurized conditions as an outer packaging bag for battery cells of an energy storage device. The energy storage device packaging material may further include a first adhesive layer between the base material layer and the barrier layer, the adhesive layer being a second adhesive layer, and the second adhesive layer having a thickness greater than that of the first adhesive layer. In this case, the second adhesive layer may contain a hydrophobic insulating inorganic filler, thereby preventing the adhesive strength of the second adhesive layer from decreasing below the adhesive strength of the first adhesive layer. Furthermore, the hydrophobic insulating inorganic filler is less likely to be exposed from the surface of the second adhesive layer, making it easier to prevent a decrease in adhesion between the second adhesive layer and the sealant layer or barrier layer.
[0017] In the packaging material for an electricity storage device, the electricity storage device may be an all-solid-state battery.
[0018] The present disclosure also provides an energy storage device including a battery cell having a positive electrode, an electrolyte, and a negative electrode in this order, and an outer bag containing the battery cell, the outer bag having the above-described outer bag packaging material for an energy storage device. According to the energy storage device of the present disclosure, the outer bag has excellent insulating properties even when used as an outer bag in a heated and pressurized state, and therefore, even when the energy storage device is heated in a state where it is pressurized in a direction perpendicular to the interface between the battery cell and the outer bag packaging material, short-circuiting between the positive electrode or negative electrode in the battery cell and the metal layer of the outer bag packaging material can be suppressed.
[0019] The power storage device may be an all-solid-state battery.
[0020] According to the present disclosure, it is possible to provide an exterior packaging material for an electricity storage device and an electricity storage device that have excellent insulating properties even when used as an exterior bag for the electricity storage device in a heated and pressurized state.
[0021] Fig. 1 is a cross-sectional view showing a first embodiment of an exterior packaging material for an energy storage device according to the present disclosure. Fig. 2 is a cross-sectional view showing a second embodiment of an exterior packaging material for an energy storage device according to the present disclosure. Fig. 3 is a perspective view showing an embodiment of an energy storage device according to the present disclosure. Fig. 4 is a cross-sectional view showing the battery cell of Fig. 3. Fig. 5 is a plan view showing a folded cut piece before cutting out a test piece for measuring seal strength used in Examples and Comparative Examples.
[0022] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In the drawings, the same or corresponding parts are designated by the same reference numerals, and redundant explanations will be omitted.
[0023] [First embodiment of exterior packaging material for an energy storage device] First, a first embodiment of an exterior packaging material for an energy storage device according to the present disclosure will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view showing the first embodiment of the exterior packaging material for an energy storage device according to the present disclosure. An exterior packaging material for an energy storage device (hereinafter also simply referred to as "exterior packaging material") 10 shown in Fig. 1 is an exterior packaging material used for an energy storage device, and includes, in this order, a base layer 11, a first adhesive layer 12a, a barrier layer 13, a second adhesive layer 12b as an adhesive layer, and a sealant layer 16.
[0024] The second adhesive layer 12b contains a hydrophobic insulating inorganic filler. The second adhesive layer 12b is obtained using an adhesive as a composition containing the hydrophobic insulating inorganic filler.
[0025] The barrier layer 13 has a first corrosion prevention treatment layer 14a and a second corrosion prevention treatment layer 14b on both sides of the metal layer 14c. The first corrosion prevention treatment layer 14a is disposed between the substrate layer 11 and the metal layer 14c, and the second corrosion prevention treatment layer 14b is disposed between the metal layer 14c and the second adhesive layer 12b. Although Fig. 1 shows the case where the corrosion prevention treatment layers 14a and 14b are provided on both sides of the metal layer 14c, only one of the corrosion prevention treatment layers 14a and 14b may be provided.
[0026] In the exterior packaging material 10, the base material layer 11 is the outermost layer and the sealant layer 16 is the innermost layer. That is, the exterior packaging material 10 is used with the base material layer 11 facing the exterior side of the electricity storage device and the sealant layer 16 facing the interior side of the electricity storage device.
[0027] The exterior material 10 has excellent insulating properties even when used under heat and pressure as an exterior bag for an electricity storage device.
[0028] Each layer constituting the exterior packaging material 10 will be specifically described below.
[0029] <Substrate Layer> The substrate layer 11 imparts heat resistance to the packaging material 10 in the sealing step of the exterior bag when manufacturing the electricity storage device, and plays a role in suppressing the occurrence of pinholes that may occur during molding, processing, or distribution of the packaging material 10. In particular, in the case of packaging materials for large-scale electricity storage devices, the substrate layer 11 can also impart scratch resistance, chemical resistance, insulating properties, and the like.
[0030] The base layer 11 is preferably a layer formed of an insulating resin, such as polyester resin, polyamide resin, polyimide resin, polyamideimide resin, polyetherketone resin, polyphenylene sulfide resin, polyetherimide resin, polysulfone resin, fluororesin, phenol resin, melamine resin, urethane resin, allyl resin, silicone resin, epoxy resin, furan resin, or acetyl cellulose resin.
[0031] Among these resins, polyester resins and polyamide resins are preferred for the base layer 11 because of their excellent moldability. Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyamide resins include nylon 6, nylon 6,6, a copolymer of nylon 6 and nylon 6,6, nylon 6, nylon 9T, nylon 10, polymetaxylylene adipamide (MXD6), nylon 11, and nylon 12.
[0032] The substrate layer 11 may contain additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a dehydrating agent, a crystal nucleating agent, and a tackifier, as needed.
[0033] The substrate layer 11 may be in the form of a stretched or unstretched film, or in the form of a coating film. The substrate layer 11 may be a single layer or a multilayer, and in the case of a multilayer, different resins may be used in combination. When the substrate layer 11 is a film, a laminate obtained by co-extruding multiple layers, or a laminate obtained by laminating multiple layers via an adhesive, may be used as the substrate layer 11. When the substrate layer 11 is a coating film, a substrate obtained by coating a coating liquid the number of times the coating liquid is applied may be used as the substrate layer 11, or a multilayer formed by combining a film and a coating film may be used.
[0034] When these resins are used in the form of a film, the base layer 11 is preferably a biaxially stretched film. Examples of the stretching method when the base layer 11 is a biaxially stretched film include sequential biaxial stretching, tubular biaxial stretching, and simultaneous biaxial stretching. From the viewpoint of obtaining better deep drawability, the biaxially stretched film is preferably a film stretched by tubular biaxial stretching.
[0035] The thickness of the substrate layer 11 is preferably 6 to 40 μm, and more preferably 10 to 30 μm. When the thickness of the substrate layer 11 is 6 μm or more, the pinhole resistance and insulating properties of the packaging material 10 tend to be improved. When the thickness of the substrate layer 11 is 40 μm or less, the total thickness of the packaging material 10 can be reduced.
[0036] The melting point of the base layer 11 is higher than the melting point of the sealant layer 16, preferably 30° C. or more higher than the melting point of the sealant layer 16, in order to suppress deformation of the base layer 11 during sealing.
[0037] <First Adhesive Layer> The first adhesive layer 12a is a layer that bonds the base layer 11 and the metal layer 14c. The first adhesive layer 12a is obtained using a first adhesive layer-forming composition (adhesive). The first adhesive layer-forming composition includes, for example, a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol, and a bifunctional or higher isocyanate compound (polyfunctional isocyanate compound). The various polyols described above can be used alone or in combination of two or more types depending on the functions and performance required of the exterior material 10. In addition to the above-mentioned first adhesive layer-forming composition, the first adhesive layer-forming composition that forms the first adhesive layer 12a can also be a first adhesive layer-forming composition containing a base material such as an epoxy resin and a curing agent, but the first adhesive layer-forming composition is not limited thereto.
[0038] The composition for forming the first adhesive layer may contain various additives such as flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, dehydrating agents, nucleating agents, and tackifiers, depending on the performance required of the first adhesive layer 12a.
[0039] The thickness of the first adhesive layer 12a is not particularly limited, but from the viewpoint of obtaining the desired adhesive strength, conformability, processability, etc., it is preferably, for example, 1 to 10 μm, and more preferably 2 to 7 μm.
[0040] <Barrier Layer> (Metal Layer) The metal layer 14c has water vapor barrier properties that prevent moisture from penetrating into the interior of the power storage device. The metal layer 14c may also have extensibility for deep drawing. Examples of the metal layer 14c that can be used include various metal foils such as aluminum, stainless steel, and copper, as well as metal vapor deposition films and films with such vapor deposition films. Examples of films with vapor deposition films include aluminum vapor deposition films. In terms of mass (specific gravity), moisture resistance, processability, and cost, metal foils are preferred for the metal layer 14c, and aluminum foil is more preferred.
[0041] As the aluminum foil, soft aluminum foil that has been annealed can be preferably used because it can impart the desired ductility during molding. However, it is more preferable to use aluminum foil containing iron for the purpose of imparting further pinhole resistance and ductility during molding. The iron content in the aluminum foil is preferably 0.1 to 9.0 mass%, more preferably 0.5 to 2.0 mass%, based on 100 mass% of the aluminum foil. By having an iron content of 0.1 mass% or more, an exterior packaging material 10 having better pinhole resistance and ductility can be obtained. By having an iron content of 9.0 mass% or less, an exterior packaging material 10 having better flexibility can be obtained. As the aluminum foil, untreated aluminum foil may be used, but it is preferable to use aluminum foil that has been degreased in order to impart corrosion resistance. When degreasing the aluminum foil, the degreasing treatment may be performed on only one side of the aluminum foil, or on both sides.
[0042] The thickness of the metal layer 14c is not particularly limited, but is preferably 9 to 200 μm, more preferably 15 to 100 μm, in consideration of barrier properties, pinhole resistance, and processability.
[0043] (First Anti-Corrosion Treatment Layer and Second Anti-Corrosion Treatment Layer) The first anti-corrosion treatment layer 14a and the second anti-corrosion treatment layer 14b are layers provided to prevent corrosion of the metal layer 14c. The first anti-corrosion treatment layer 14a prevents corrosion of the metal layer 14c due to corrosive gases contained in the atmosphere and also serves to increase the adhesion between the metal layer 14c and the first adhesive layer 12a. The second anti-corrosion treatment layer 14b prevents corrosion of the metal layer 14c due to the electrolyte and gases generated inside the battery (e.g., hydrogen sulfide gas), thereby further improving resistance to the electrolyte and gases generated inside the battery and increasing the adhesion between the metal layer 14c and the second adhesive layer 12b. The first and second anti-corrosion treatment layers 14a and 14b can maintain the reliability of the exterior material 10 for a longer period of time. The first anti-corrosion treatment layer 14a and the second anti-corrosion treatment layer 14b may be layers of the same configuration or layers of different configurations. The first and second corrosion prevention treatment layers 14a, 14b (hereinafter simply referred to as "corrosion prevention treatment layers 14a, 14b") are formed, for example, by subjecting the metal foil constituting the metal layer 14c to degreasing treatment, hydrothermal treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.
[0044] Degreasing treatments include acid degreasing and alkaline degreasing. Acid degreasing treatments include methods using inorganic acids such as sulfuric acid, nitric acid, hydrochloric acid, and hydrofluoric acid alone, or methods using a mixture of these. Furthermore, acid degreasing is preferably performed using an acid degreasing agent prepared by dissolving a fluorine-containing compound such as monosodium ammonium difluoride in the inorganic acid. This treatment, particularly when aluminum foil is used for the metal layer 14c, not only achieves aluminum degreasing effects but also allows the formation of aluminum fluoride, which is passive. Therefore, this treatment is effective in terms of corrosion resistance. Alkaline degreasing treatments include methods using sodium hydroxide, etc.
[0045] An example of the hydrothermal modification treatment is boehmite treatment, in which aluminum foil is immersed in boiling water containing triethanolamine. An example of the anodization treatment is alumite treatment.
[0046] Examples of chemical conversion treatments include immersion-type chemical conversion treatments and coating-type chemical conversion treatments. Examples of immersion-type chemical conversion treatments include chromate treatment, ceria sol treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment, and various chemical conversion treatments consisting of mixed phases of these. On the other hand, examples of coating-type chemical conversion treatments include a method in which a coating agent having corrosion prevention properties is applied to the metal layer 14c.
[0047] When forming at least a part of the corrosion prevention treatment layer by any of these corrosion prevention treatments, i.e., hydrothermal conversion treatment, anodizing treatment, or chemical conversion treatment, it is preferable to perform the degreasing treatment described above in advance. Note that when a degreased metal foil, such as a metal foil that has been subjected to an annealing process, is used as the metal layer 14c, there is no need to perform a degreasing treatment again when forming the corrosion prevention treatment layers 14a and 14b.
[0048] The coating agent used in the spray-type chemical conversion treatment preferably contains trivalent chromium. The coating agent may also contain at least one polymer selected from the group consisting of cationic polymers and anionic polymers, which will be described later.
[0049] Furthermore, among the above treatments, particularly hydrothermal conversion treatment and anodizing treatment, the aluminum foil surface is dissolved by a treatment agent to form aluminum compounds (boehmite, alumite) with excellent corrosion resistance. Therefore, a bicontinuous structure is formed from the metal layer 14c using aluminum foil to the corrosion prevention treatment layers 14a, 14b, and therefore the above treatments are included in the definition of chemical conversion treatment. On the other hand, as described below, it is also possible to form the corrosion prevention treatment layers 14a, 14b using a pure coating method, which is not included in the definition of chemical conversion treatment. One example of this method is a method using a sol of a rare earth element oxide, such as cerium oxide, with an average particle size of 100 nm or less, which has an aluminum corrosion prevention effect (inhibitor effect) and is environmentally friendly. By using this method, it is possible to impart corrosion prevention effects to metal foils such as aluminum foil using a common coating method.
[0050] Examples of the rare earth element oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, and ether-based solvents. Of these, water-based sols (sols using water-based solvents) are preferred.
[0051] In order to stabilize the dispersion of the rare earth element oxide sol, inorganic acids such as nitric acid, hydrochloric acid, phosphoric acid, or their salts, or organic acids such as acetic acid, malic acid, ascorbic acid, and lactic acid are usually used as dispersion stabilizers. Of these dispersion stabilizers, phosphoric acid in particular is expected to have the following effects (1) to (4) in the packaging material 10: (1) stabilization of the sol dispersion; (2) improvement of adhesion to the metal layer 14c by utilizing the aluminum chelating ability of phosphoric acid; (3) imparting corrosion resistance by capturing aluminum ions (passivation); and (4) improvement of the cohesion of the corrosion prevention treatment layers (oxide layers) 14a, 14b due to the tendency of phosphoric acid to undergo dehydration condensation even at low temperatures.
[0052] Since the corrosion prevention treatment layers 14a, 14b formed from the rare earth element oxide sol are aggregates of inorganic particles, the cohesive strength of the layers themselves may be reduced even after the dry-cure process. Therefore, in this case, the corrosion prevention treatment layers 14a, 14b are preferably compounded with an anionic polymer or a cationic polymer to compensate for the cohesive strength.
[0053] The corrosion prevention treatment layers 14a, 14b are not limited to the layers described above. For example, they may be formed using a treatment agent containing a resin binder (such as aminophenol) mixed with phosphoric acid and a chromium compound, as in the case of a known paint-type chromate. Using this treatment agent can provide a layer that combines both corrosion prevention functionality and adhesion. Furthermore, although the stability of the coating liquid must be considered, the corrosion prevention treatment layers 14a, 14b can be provided as layers that combine both corrosion prevention functionality and adhesion by using a coating agent in which a rare earth element oxide sol and a polycationic polymer or a polyanionic polymer are preliminarily mixed into a single liquid.
[0054] The mass per unit area of the corrosion prevention treatment layers 14a and 14b is 0.005 to 0.200 g / m2, whether the layer has a multi-layer structure or a single-layer structure. 2 is preferred, and 0.010 to 0.100 g / m 2 It is more preferable that the mass per unit area is 0.005 g / m 2 If the mass per unit area is 0.200 g / m or more, it is easy to impart a corrosion prevention function to the metal layer 14c. 2 Even if the thickness exceeds 100 μm, the corrosion prevention function does not change significantly. On the other hand, when a rare earth element oxide sol is used, if the coating is thick, the heat curing during drying may be insufficient, which may result in a decrease in cohesive force. The thickness of the corrosion prevention treatment layers 14 a and 14 b can be calculated from their specific gravity.
[0055] From the viewpoint of making it easier to maintain adhesion between the sealant layer 16 and the barrier layer 13, the corrosion prevention treatment layers 14a, 14b may be in an embodiment containing, for example, cerium oxide, 1 to 100 parts by mass of phosphoric acid or a phosphate salt per 100 parts by mass of the cerium oxide, and a cationic polymer, or may be in an embodiment formed by subjecting the metal layer 14c to a chemical conversion treatment, or may be in an embodiment formed by subjecting the metal layer 14c to a chemical conversion treatment and containing a cationic polymer.
[0056] <Second Adhesive Layer> The second adhesive layer 12b is a layer that bonds the metal layer 14c and the sealant layer 16. The second adhesive layer 12b is obtained using a composition (adhesive) containing a hydrophobic insulating inorganic filler. The composition may also contain a resin.
[0057] (Hydrophobic insulating inorganic filler) The hydrophobic insulating inorganic filler is an insulating inorganic filler having hydrophobic properties, and is a filler obtained by surface-treating an insulating inorganic filler with an organosilicon compound. By surface-treating the insulating inorganic filler with an organosilicon compound, the surface of the insulating inorganic filler is hydrophobized, thereby imparting hydrophobicity to the insulating inorganic filler. The filler is an inorganic filler because it is less likely to deform even when heated and pressurized for a long time compared to organic fillers. Note that the insulating inorganic filler is, for example, non-hydrophobic.
[0058] Examples of non-hydrophobic insulating inorganic fillers include silica and talc, with silica being preferred from the viewpoints of insulating properties and particle size control.
[0059] The organosilicon compound may be, for example, an alkoxysilane. The alkoxysilane may have an alkyl group such as a methyl group. In this case, the non-hydrophobic insulating inorganic filler and the alkoxysilane are more likely to react with each other.
[0060] The average particle size of the hydrophobic insulating inorganic filler is not particularly limited, but is preferably 1 μm or more. In this case, the exterior material 10 can have better insulating properties even when used under heat and pressure as an exterior bag for a battery cell of an electricity storage device, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm. The average particle size of the hydrophobic insulating inorganic filler is more preferably 3 μm or more, and even more preferably 5 μm or more.
[0061] The average particle size of the hydrophobic insulating inorganic filler is preferably 20 μm or less. In this case, the hydrophobic insulating inorganic filler can be maintained in a well-dispersed state in the composition, the cohesive force of the second adhesive layer 1b is less likely to decrease, and the adhesion strength of the second adhesive layer 12b to the barrier layer 13 and the sealant layer 16 and the sealing strength of the sealant layer 16 are less likely to decrease. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less.
[0062] The average particle size of the hydrophobic insulating inorganic filler can be determined by taking an enlarged photograph of a plurality of hydrophobic insulating inorganic fillers using an electron microscope, then determining the particle size of each hydrophobic insulating inorganic filler by image analysis, and calculating the average of these particle sizes. Specifically, the particle size of each hydrophobic insulating inorganic filler can be determined by taking the area S of each hydrophobic insulating inorganic filler determined by image analysis as the area of a circle, and then calculating the radius r (r = (S / π) 1/2 ) is doubled.
[0063] In the second adhesive layer-forming composition, the content of the hydrophobic insulating inorganic filler in the total solid content, i.e., the content of the hydrophobic insulating inorganic filler in the second adhesive layer 12b, is not particularly limited, but is preferably 0.5% by mass or more. In this case, compared to when the content of the hydrophobic insulating inorganic filler in the total solid content is less than 0.5% by mass, the thickness of the insulating layer including the second adhesive layer 12b is more likely to be maintained uniform even when the exterior material 10 is used under heated and pressurized conditions as an exterior bag for a battery cell of an energy storage device. The content of the hydrophobic insulating inorganic filler in the total solid content is more preferably 1% by mass or more, even more preferably 2% by mass or more, and particularly preferably 4% by mass or more.
[0064] The content of the hydrophobic insulating inorganic filler in the total solid content is preferably 20% by mass or less. In this case, the decrease in cohesive force of the second adhesive layer 12b is suppressed, and the decrease in seal strength and adhesion is further suppressed, compared to when the content of the hydrophobic insulating inorganic filler in the total solid content exceeds 20% by mass. In addition, the decrease in brittleness of the second adhesive layer 12b can be further suppressed. The content of the hydrophobic insulating inorganic filler in the total solid content is more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 8% by mass or less.
[0065] (Resin) The resin is not particularly limited, but preferably contains a modified polyolefin resin. The modified polyolefin resin allows the hydrophobic insulating inorganic filler to be dispersed more effectively in the resin. Furthermore, by including the modified polyolefin resin in the resin, the second adhesive layer 12b can have high adhesion to the barrier layer 13 and the sealant layer 16, thereby improving the laminate strength of the packaging material 10. Examples of modified polyolefin resins include hydroxyl-modified polyolefin resins, glycidyl-modified polyolefin resins, and acid-modified polyolefin resins. Among these, acid-modified polyolefin resins are preferred in terms of adhesion to the barrier layer 13 and the sealant layer 16. The acid-modified polyolefin resin is a polyolefin resin graft-modified with an unsaturated carboxylic acid derivative derived from an unsaturated carboxylic acid, an unsaturated sulfonic acid, an acid anhydride of an unsaturated carboxylic acid, an ester of an unsaturated carboxylic acid, or the like.
[0066] Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid.
[0067] Examples of the acid anhydrides of unsaturated carboxylic acids include acid anhydrides of unsaturated carboxylic acids such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride.
[0068] Examples of the esters of unsaturated carboxylic acids include esters of unsaturated carboxylic acids such as methyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, dimethyl maleate, monomethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconate, dimethyl tetrahydrophthalate, and dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate.
[0069] Examples of polyolefin resins include polyethylene-based resins such as low-density polyethylene (LDPE or LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and ethylene-α-olefin copolymers; and polypropylene-based resins such as homopolypropylene, block polypropylene, random polypropylene, and propylene-α-olefin copolymers. Among these, polypropylene-based resins are preferred from the viewpoint of heat resistance.
[0070] The acid-modified polyolefin resin is preferably a polyolefin resin modified with maleic anhydride, from the viewpoint of obtaining excellent adhesion between the barrier layer 13 and the second adhesive layer 12b. Suitable modified polyolefin resins include, for example, "ADMER" manufactured by Mitsui Chemicals, Inc., "MODIC" manufactured by Mitsubishi Chemical Corporation, "TOYOTAC" manufactured by Toyobo Co., Ltd., and "SUNTACK" manufactured by Sanyo Chemical Industries, Ltd. Such modified polyolefin resins have excellent reactivity with various metals and polymers having various functional groups, and this reactivity can be used to impart adhesion to the second adhesive layer 12b.
[0071] When the resin composition for forming the sealant layer 16 contains a polyolefin resin as a resin, it is preferable to use a polyolefin resin similar to that polyolefin resin. For example, when the resin composition for forming the sealant layer contains a polypropylene-based resin as a resin, it is preferable that the acid-modified polyolefin resin of the composition for forming the second adhesive layer is an acid-modified polypropylene-based resin. In this case, the second adhesive layer 12b can have high adhesion to the sealant layer 16 and can also improve the heat resistance of the exterior material 10.
[0072] When the resin contains a modified polyolefin resin, the composition for forming the second adhesive layer preferably further contains a polyfunctional isocyanate compound as a curing agent. In this case, the second adhesive layer 12b further contains a polyfunctional isocyanate compound, which allows the second adhesive layer 12b to have excellent adhesion and heat resistance, high seal strength, heat resistance, and excellent barrier properties. Examples of polyfunctional isocyanate compounds include diisocyanates such as tolylene diisocyanate, xylylene diisocyanate or hydrogenated products thereof, hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate or hydrogenated products thereof, and isophorone diisocyanate; or polyisocyanates such as adducts obtained by reacting these isocyanates with polyhydric alcohols such as trimethylolpropane, biuret compounds obtained by reacting these isocyanates with water, or trimer isocyanurates (isocyanurate-type polyfunctional isocyanate compounds); or blocked polyisocyanates obtained by blocking these polyisocyanates with alcohols, lactams, oximes, etc. Among these, the polyfunctional isocyanate compound preferably includes an isocyanurate (isocyanurate-type polyfunctional isocyanate compound). When the polyfunctional isocyanate compound contains an isocyanurate, the second adhesive layer 12b can have excellent adhesion and heat resistance, and the exterior material 10 can have high sealing strength and heat resistance.
[0073] The amount of the polyfunctional isocyanate compound may be, for example, 3 parts by mass or less, 2 parts by mass or less, or 1 part by mass or less per 100 parts by mass of the modified polyolefin resin (solid content). The amount of the polyfunctional isocyanate compound may be more than 0 parts by mass or 0.5 parts by mass or more per 100 parts by mass of the modified polyolefin resin (solid content).
[0074] When the resin contains an acid-modified polyolefin resin as the modified polyolefin resin, it is preferable that the resin further contains a carbodiimide compound as a curing agent. When the second adhesive layer-forming composition further contains a carbodiimide compound, the heat resistance of the packaging material 10 can be further improved compared to when the second adhesive layer-forming composition does not contain a carbodiimide compound. This is because the crosslink density increases due to the reaction between the carbodiimide compound and the acid-modified polyolefin resin. Examples of carbodiimide compounds include N,N'-di-o-toluylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-di-2,6-dimethylphenylcarbodiimide, N,N'-bis(2,6-diisopropylphenyl)carbodiimide, N,N'-dioctyldecylcarbodiimide, N-triyl-N'-cyclohexylcarbodiimide, N,N'-di-2,2-di-t-butylphenylcarbodiimide, N-triyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-cyclohexylcarbodiimide, and N,N'-di-p-toluylcarbodiimide. These may be used alone or in combination of two or more.
[0075] The amount of the carbodiimide compound may be, for example, 3 parts by mass or less per 100 parts by mass of the modified polyolefin resin (solid content).
[0076] The composition for forming the second adhesive layer may further contain various additives such as flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, tackifiers, dehydrating agents, and nucleating agents, as needed.
[0077] In addition, as the second adhesive layer forming composition for forming the second adhesive layer 12b, for example, a polyurethane adhesive containing a polyester polyol consisting of a hydrogenated dimer fatty acid and a diol, a polyisocyanate, and a hydrophobic insulating inorganic filler can be used. Examples of the second adhesive layer forming composition include polyurethane resins in which a bifunctional or higher isocyanate compound is reacted with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol, and epoxy resins in which an amine compound or the like is reacted with a base material having an epoxy group, and these are preferred from the viewpoint of heat resistance.
[0078] The second adhesive layer 12b may be composed of a single layer or multiple layers. When the second adhesive layer 12b is composed of multiple layers, all of the layers may contain the hydrophobic insulating inorganic filler, or only some of the layers may contain the hydrophobic insulating inorganic filler.
[0079] The thickness of the second adhesive layer 12b is not particularly limited, but is preferably 0.2 to 30 μm. In this case, sufficient adhesion can be obtained compared to when the thickness of the second adhesive layer 12b is less than 0.2 μm. Furthermore, the volumetric energy density of the power storage device can be further increased compared to when the thickness of the second adhesive layer 12b is greater than 30 μm. The thickness of the second adhesive layer 12b is more preferably 0.2 to 25 μm, even more preferably 0.2 to 20 μm, and particularly preferably 0.2 to 10 μm. The thickness of the second adhesive layer 12b may be less than or greater than the thickness of the first adhesive layer 12a, but is preferably greater than the thickness of the first adhesive layer 12a. In this case, the inclusion of a hydrophobic insulating inorganic filler in the second adhesive layer 12b can prevent the adhesive strength of the second adhesive layer 12b from decreasing below the adhesive strength of the first adhesive layer 12a. Furthermore, the hydrophobic insulating inorganic filler is less likely to be exposed from the surface of the second adhesive layer 12b, which makes it easier to prevent a decrease in adhesion between the second adhesive layer 12b and the sealant layer 16 or the barrier layer 13. In this case, the ratio R of the thickness of the second adhesive layer 12b to the thickness of the first adhesive layer 12a may be greater than 1, but is preferably 2 or greater, and more preferably 3 or greater. R may be 10 or less, 8 or less, 6 or less, or 5 or less.
[0080] <Sealant Layer> The sealant layer 16 is a layer that imparts heat-sealing sealability to the packaging material 10, and is a layer that is disposed on the inner side and heat-sealed (thermally fused) when assembling the electricity storage device. The sealant layer 16 is obtained using a resin composition for forming a sealant layer that contains a resin.
[0081] (Resin composition for forming sealant layer) (Resin) Examples of the resin contained in the resin composition for forming the sealant layer include polyolefin resins and polyester resins. These resins (hereinafter also referred to as "base resins") constituting the sealant layer 16 may be used alone or in combination of two or more.
[0082] Examples of polyolefin resins include polyethylene resins such as low-density polyethylene (LDPE or LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and ethylene-α-olefin copolymers; polypropylene resins such as homopolypropylene, block polypropylene, and propylene-α-olefin copolymers; and polybutene. From the viewpoints of heat resistance and flexibility, polypropylene resins are preferred as polyolefin resins, and homopolypropylene and block polypropylene, which have high melting points, are particularly preferred.
[0083] Examples of polyester resins include polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polyethylene naphthalate (PEN) resin, polybutylene naphthalate (PBN) resin, and copolymers thereof.
[0084] (Hydrophobic insulating inorganic filler) The resin composition for forming a sealant layer may or may not contain a hydrophobic insulating inorganic filler, but preferably contains one.
[0085] The average particle size of the hydrophobic insulating inorganic filler is not particularly limited, but is preferably 1 μm or more. In this case, the exterior material 10 can have better insulating properties even when used under heat and pressure as an exterior bag for a battery cell of an electricity storage device, compared to when the average particle size of the hydrophobic insulating inorganic filler is less than 1 μm. The average particle size of the hydrophobic insulating inorganic filler is more preferably 3 μm or more, and even more preferably 5 μm or more.
[0086] The average particle size of the hydrophobic insulating inorganic filler is preferably 20 μm or less. In this case, the hydrophobic insulating inorganic filler can be maintained in a well-dispersed state in the composition, the cohesive force of the sealant layer 16 is less likely to decrease, and the adhesion strength of the sealant layer 16 to the second adhesive layer 12b and the sealing strength of the sealant layer 16 are less likely to decrease. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less.
[0087] The content of the hydrophobic insulating inorganic filler in the sealant layer-forming resin composition is not particularly limited, but is preferably 0.5% by mass or more. In this case, compared to when the content of the hydrophobic insulating inorganic filler in the sealant layer-forming resin composition is less than 0.5% by mass, the thickness of the insulating layer including the sealant layer 16 is more easily maintained uniformly even when the packaging material 10 is used under heat and pressure as an outer bag for a battery cell of an electrical storage device. The content of the hydrophobic insulating inorganic filler in the sealant layer-forming resin composition is more preferably 1% by mass or more, even more preferably 2% by mass or more, and particularly preferably 4% by mass or more. The content of the hydrophobic insulating inorganic filler in the sealant layer-forming resin composition is preferably 20% by mass or less. In this case, compared to when the content of the hydrophobic insulating inorganic filler in the sealant layer-forming resin composition exceeds 20% by mass, the decrease in cohesive strength of the sealant layer 16 is more suppressed, and the decrease in sealing strength and adhesion is more suppressed. Furthermore, the decrease in brittleness of the sealant layer 16 can be more suppressed. The content of the hydrophobic insulating inorganic filler in the resin composition for forming a sealant layer is more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 8% by mass or less.
[0088] The sealant layer 16 may be either a single-layer film or a multilayer film. When the sealant layer 16 is a multilayer film, all layers may contain the hydrophobic insulating inorganic filler, or only some layers may contain the hydrophobic insulating inorganic filler. For example, when the sealant layer 16 is a two-layer film, all layers may contain the hydrophobic insulating inorganic filler, or only the layer of the two-layer film on the second adhesive layer 12b side may contain the hydrophobic insulating inorganic filler, or only the layer of the two-layer film on the opposite side of the second adhesive layer 12b may contain the hydrophobic insulating inorganic filler.
[0089] The sealant layer 16 may also contain additives such as slip agents, antiblocking agents, antioxidants, light stabilizers, flame retardants, dehydrating agents, tackifiers, and crystal nucleating agents. The content of these additives is preferably 5 parts by mass or less, assuming that the total mass of the sealant layer 16 is 100 parts by mass.
[0090] The MFR of the sealant layer 16 is not particularly limited, but is preferably 20 g / 10 min or less. By making the sealant layer 16 less likely to flow even under heated and pressurized conditions by setting the MFR of the sealant layer 16 to 20 g / 10 min or less, the sealant layer 16 is less likely to collapse even when the packaging material 10 is used as an outer bag under heated and pressurized conditions. This ensures a sufficient thickness of the insulating layer including the sealant layer 16, resulting in better insulating properties. The MFR of the sealant layer 16 is preferably 18 g / 10 min or less, and more preferably 15 g / 10 min or less. The MFR of the sealant layer 16 may be 0.1 g / 10 min or more, 0.3 g / 10 min or more, 1 g / 10 min or more, 2 g / 10 min or more, 4 g / 10 min or more, 6 g / 10 min or more, 8 g / 10 min or more, or 10 g / 10 min or more. The MFR of the sealant layer 16 can be obtained by measuring it using a melt flow rate measuring device (manufactured by Toyo Seiki Seisakusho, measuring temperature: 230° C.) in accordance with JIS K7210.
[0091] The melting point of the sealant layer 16 is not particularly limited, but is preferably 160°C or higher. By setting the melting point of the sealant layer 16 to 160°C or higher, the flow of the sealant layer 16 can be minimized even under heated and pressurized conditions. This more effectively prevents the insulating layer, including the second adhesive layer 12b, from being crushed. Therefore, the packaging material 10 can have superior insulating properties even when used under heated and pressurized conditions as an outer bag for a battery cell of an energy storage device. When differential scanning calorimetry (DSC) is performed on the sealant layer 16, if a single peak corresponding to the melting point of the sealant layer 16 appears, the melting point refers to the temperature at the apex of that peak. If multiple peaks corresponding to the melting point of the sealant layer 16 appear, the melting point refers to the temperature at the apex of the peak with the greatest intensity (main peak) among the multiple peaks. The melting point of the sealant layer 16 is more preferably 161°C or higher, and particularly preferably 162°C or higher. The melting point of the sealant layer 16 is more preferably 270° C. or less, and particularly preferably 260° C. or less.
[0092] The thickness of the sealant layer 16 is not particularly limited, but is preferably in the range of 20 to 150 μm, more preferably in the range of 30 to 150 μm, and even more preferably in the range of 40 to 100 μm. When the thickness of the sealant layer 16 is 20 μm or more, the sealing strength of the packaging material 10 is further improved. When the thickness of the sealant layer 16 is 150 μm or less, the volumetric energy density of the electricity storage device can be further increased.
[0093] <Exterior Material> The exterior material 10 preferably has a breakdown voltage of 100 V or more, more preferably 0.5 kV or more, and particularly preferably 1 kV or more, when heated and pressurized for 24 hours under conditions of 150°C and 3 MPa. In this case, even under harsh heating and pressurizing conditions, the exterior material 10 can have better insulating properties when used under heating and pressurization as an exterior bag for battery cells of an energy storage device. The breakdown voltage may be 5 kV or less when heated and pressurized for 24 hours under conditions of 150°C and 3 MPa.
[0094] [Second Embodiment of Sheathing Material for Energy Storage Device] Next, a second embodiment of the sheathing material for an energy storage device according to the present disclosure will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing the second embodiment of the sheathing material for an energy storage device according to the present disclosure. As shown in Fig. 2, the sheathing material 20 of this embodiment differs from the sheathing material 10 of the first embodiment, which includes a second adhesive layer 12b obtained using an adhesive, in that it includes an adhesive resin layer 15 obtained using a resin composition for forming an adhesive resin layer containing a resin and a hydrophobic insulating inorganic filler, as an adhesive layer between the barrier layer 13 and the sealant layer 16. Note that the sheathing material 20 shown in Fig. 2 may further include a second adhesive layer 12b between the barrier layer 13 and the adhesive resin layer 15.
[0095] The adhesive resin layer 15 may be either a single-layer film or a multilayer film. When the adhesive resin layer 15 is a multilayer film, all layers may contain the hydrophobic insulating inorganic filler, or only some layers may contain the hydrophobic insulating inorganic filler.
[0096] The thickness of the adhesive resin layer 15 is not particularly limited, but is preferably 5 to 30 μm. When the thickness of the adhesive resin layer 15 is 5 μm or more, sufficient adhesion is obtained. When the thickness of the adhesive resin layer 15 is 30 μm or less, the total thickness of the exterior packaging material 10 is reduced, thereby suppressing a decrease in the volumetric energy density of the battery when the exterior packaging material 10 is used to fabricate the battery. The thickness of the adhesive resin layer 15 may be the same as or less than that of the sealant layer 16 from the viewpoints of stress relaxation and moisture permeation. The thickness of the adhesive resin layer 15 may be less than or greater than the thickness of the first adhesive layer 12a, but is preferably greater than the thickness of the first adhesive layer 12a. In this case, the adhesive resin layer 15 contains a hydrophobic insulating inorganic filler, thereby suppressing a decrease in the adhesive strength of the adhesive resin layer 15 compared to the adhesive strength of the first adhesive layer 12a. Furthermore, the hydrophobic insulating inorganic filler is less likely to be exposed from the surface of the adhesive resin layer 15, which makes it easier to prevent a decrease in adhesion between the adhesive resin layer 15 and the sealant layer 16 or the barrier layer 13. In this case, the ratio R of the thickness of the adhesive resin layer 15 to the thickness of the first adhesive layer 12a may be greater than 1, but is preferably 2 or more, and more preferably 3 or more. R may be 10 or less, 8 or less, 6 or less, or 5 or less.
[0097] [Method of Manufacturing the Sheathing Material] Next, an example of a method of manufacturing the sheathing material 10 shown in Fig. 1 will be described. Note that the method of manufacturing the sheathing material 10 is not limited to the following method.
[0098] The manufacturing method of the exterior material 10 includes the steps of forming a barrier layer 13 by laminating corrosion prevention treatment layers 14a, 14b on both sides of a metal layer 14c, respectively; bonding the base material layer 11 and the barrier layer 13 together using a first adhesive layer 12a to obtain a first laminate; further laminating a sealant layer 16 onto the barrier layer 13 of the first laminate via a second adhesive layer 12b to produce a second laminate; and, if necessary, aging the obtained second laminate.
[0099] (Step of Laminating Anti-Corrosion Treatment Layer on Metal Layer) This step is a step of forming the anti-corrosion treatment layers 14a and 14b on both sides of the metal layer 14c, respectively, to form the barrier layer 13. As described above, examples of the method for this include subjecting the metal layer 14c to degreasing treatment, hydrothermal treatment, anodizing treatment, or chemical conversion treatment, or applying a coating agent having anti-corrosion properties.
[0100] Furthermore, when the corrosion prevention treatment layers 14a, 14b are multi-layered, the corrosion prevention treatment layers 14a, 14b can be formed, for example, by applying a coating liquid (coating agent) constituting the lower corrosion prevention treatment layer (metal layer 14c side) to the metal layer 14c and baking it to form a first layer, and then applying a coating liquid (coating agent) constituting the upper corrosion prevention treatment layer to the first layer and baking it to form a second layer, and repeating the process of forming the first and second layers as necessary.
[0101] The degreasing treatment can be carried out by a spray method or an immersion method. The hydrothermal conversion treatment and anodizing treatment can be carried out by an immersion method. The chemical conversion treatment can be carried out by an immersion method, a spray method, a coating method, or the like, appropriately selected depending on the type of chemical conversion treatment.
[0102] The coating agent having corrosion prevention properties can be applied by gravure coating, reverse coating, roll coating, bar coating, or the like.
[0103] As described above, the various treatments may be performed on either one or both sides of the metal foil constituting the metal layer 14c, but in the case of one-side treatment, the treated side is preferably the side on which the sealant layer 16 is laminated. Note that the above treatments may also be performed on the surface of the base layer 11, if required.
[0104] The coating amount of the coating agent for forming the first layer and the second layer is 0.005 to 0.200 g / m 2 , or 0.010 to 0.100 g / m 2 may be.
[0105] Furthermore, if dry curing is required, the drying can be performed at a base material temperature in the range of 60 to 300° C. depending on the drying conditions of the corrosion prevention treatment layers 14 a and 14 b used. Here, the base material temperature refers to the temperature of the barrier layer 13 (e.g., metal foil).
[0106] (Step of bonding substrate layer and barrier layer) This step is a step of bonding the barrier layer 13 and the substrate layer 11 via the first adhesive layer 12a to obtain a first laminate. Examples of the bonding method include a method of bonding both (the barrier layer 13 and the substrate layer 11) using the above-mentioned first adhesive layer-forming composition that constitutes the first adhesive layer 12a, using techniques such as dry lamination, non-solvent lamination, and wet lamination. The first adhesive layer 12a is applied in a dry coating amount of 1 to 10 g / m 2 or 2 to 7 g / m 2 It may be set in the range.
[0107] (Laminating Step of Second Adhesive Layer and Sealant Layer) This step is a step of laminating the sealant layer 16 to the second corrosion prevention treatment layer 14b side of the first laminate via the second adhesive layer 12b to obtain a second laminate. Examples of lamination methods include wet lamination and dry lamination.
[0108] For example, when the sealant layer 16 is attached by dry lamination, a second adhesive layer-forming composition for forming the second adhesive layer 12b is applied to the second corrosion prevention treatment layer 14b, and the composition is dried at a predetermined temperature to remove the solvent, and then the sealant layer 16 is laminated. Examples of methods for applying the second adhesive layer-forming composition include gravure coating, reverse coating, roll coating, and bar coating. The preferred dry application amount of the second adhesive layer-forming composition may be appropriately determined depending on the thickness of the second adhesive layer 12b.
[0109] The composition for forming the second adhesive layer can be obtained by dissolving or dispersing a resin, a hydrophobic insulating inorganic filler, etc. in a solvent. Preferably, the composition for forming the second adhesive layer is prepared by first dispersing the hydrophobic insulating inorganic filler in a solvent, and then blending the resin and curing agent therein.
[0110] It is preferable that the composition for forming the second adhesive layer further contains a dispersant. In this case, the dispersant can improve the dispersibility of the hydrophobic insulating inorganic filler and make it easier to suppress a decrease in the functionality (e.g., adhesion strength) of the second adhesive layer 12b. As the dispersant, for example, a surfactant such as metal soap (e.g., zinc stearate) is used. When the resin contains a modified polyolefin resin, the modified polyolefin resin can also function as a dispersant. From the viewpoint of improving the dispersibility of the hydrophobic insulating inorganic filler, it is preferable to disperse the hydrophobic insulating inorganic filler using a dispersing device such as a bead mill.
[0111] The average particle size of the hydrophobic insulating inorganic filler in the composition for forming the second adhesive layer is not particularly limited, but is preferably 20 μm or less. By ensuring that the average particle size of the hydrophobic insulating inorganic filler is 20 μm or less, the dispersion state of the hydrophobic insulating inorganic filler can be maintained well, and a decrease in the cohesive strength of the second adhesive layer 12b as a coating film after film formation can be suppressed. Furthermore, the hydrophobic insulating inorganic filler is less likely to fall off from the second adhesive layer 12b. Furthermore, the height of the convex portions from the surface of the second adhesive layer 12b is not too large, making it less likely for air bubbles to be trapped between the sealant layer 16 and the second adhesive layer 12b when the sealant layer 16 is bonded. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less. The average particle size of the hydrophobic insulating inorganic filler is preferably 1 μm or more. In this case, compared to when the average particle size of the hydrophobic insulating inorganic filler is less likely to cause aggregation between particles and form aggregates during dispersion, resulting in a more stable average particle size.
[0112] In the second adhesive layer-forming composition, the content of the hydrophobic insulating inorganic filler in the total solid content is preferably 20% by mass or less. In this case, the viscosity (thixotropy) of the second adhesive layer-forming composition does not increase too much, compared to when the content of the hydrophobic insulating inorganic filler in the total solid content exceeds 20% by mass, and the second adhesive layer-forming composition becomes more suitable for coating.
[0113] The sealant layer 16 can be produced, for example, by a melt extrusion molding machine with a T-die using the above-described resin composition for forming the sealant layer 16. From the viewpoint of productivity, the melt extrusion molding machine can have a processing speed of 80 m / min or more.
[0114] When forming a sealant layer 16 containing a hydrophobic insulating inorganic filler, a masterbatch may be prepared by mixing a resin and the hydrophobic insulating inorganic filler in advance, and then this masterbatch may be mixed with the base resin described above during extrusion lamination or the like to obtain a sealant layer-forming resin composition. In this case, the base resin may be a resin having similar properties, such as MFR, to the resin contained in the masterbatch. The resin mixed with the hydrophobic insulating inorganic filler when preparing the masterbatch may be a modified polyolefin resin. Acid-modified polyolefin resins are particularly preferred as modified polyolefin resins from the viewpoint of improving dispersibility in the base resin. Furthermore, the concentration of the masterbatch in the sealant layer-forming resin composition may be, for example, 5 to 50% by mass. A masterbatch concentration of 5% by mass or more in the sealant layer-forming resin composition allows the masterbatch to be sufficiently dispersed in the sealant layer 16. Furthermore, a masterbatch concentration of 50% by mass or less in the sealant layer-forming resin composition allows for sufficient dispersion during kneading during extrusion, reducing the likelihood of problems such as film breakage.
[0115] Furthermore, when forming the sealant layer 16, the resin composition for forming the sealant layer preferably further contains a dispersant. In this case, the dispersant can enhance the dispersibility of the hydrophobic insulating inorganic filler and also facilitates suppressing a decrease in the functionality of the sealant layer 16 (e.g., adhesion strength, sealing strength, etc.). As the dispersant, for example, a surfactant such as metal soap (e.g., zinc stearate) is used. When the resin contains a modified polyolefin resin, the modified polyolefin resin can also function as a dispersant.
[0116] The average particle size of the hydrophobic insulating inorganic filler in the resin composition for forming the sealant layer is not particularly limited, but is preferably 20 μm or less. By having the average particle size of the hydrophobic insulating inorganic filler be 20 μm or less, the dispersed state of the hydrophobic insulating inorganic filler can be maintained well. The average particle size of the hydrophobic insulating inorganic filler is more preferably 15 μm or less, and particularly preferably 10 μm or less. The average particle size of the hydrophobic insulating inorganic filler is preferably 1 μm or more. In this case, compared to when the average particle size of the hydrophobic insulating inorganic filler is less likely to cause aggregation between particles, and less likely to form aggregates during dispersion, resulting in a stable average particle size.
[0117] (Aging Treatment Step) This step is a step of aging (curing) the second laminate. By aging the second laminate, it is possible to promote adhesion between the metal layer 14c, the second corrosion prevention treatment layer 14b, the second adhesive layer 12b, and the sealant layer 16. The aging treatment can be performed at a temperature ranging from room temperature to 100°C. The aging time is, for example, 1 to 10 days.
[0118] In this manner, the exterior packaging material 10 shown in FIG. 1 can be manufactured.
[0119] Next, a description will be given of an example of a method for manufacturing the exterior packaging material 20 shown in Fig. 2. Note that the method for manufacturing the exterior packaging material 20 is not limited to the following method.
[0120] The manufacturing method of the exterior material 20 includes the steps of forming the barrier layer 13 by forming the corrosion prevention treatment layers 14a, 14b on both sides of the metal layer 14c, respectively, the step of bonding the base material layer 11 and the barrier layer 13 together using the first adhesive layer 12a to obtain a first laminate, the step of further laminating the adhesive resin layer 15 and the sealant layer 16 on the barrier layer 13 of the first laminate to obtain a second laminate, and the step of heat-treating the obtained second laminate, as necessary. Note that the steps up to the step of bonding the base material layer 11 and the barrier layer 13 to obtain the first laminate can be carried out in the same manner as the manufacturing method of the exterior material 10 described above.
[0121] (Laminating Process of Adhesive Resin Layer and Sealant Layer) This process is a process of forming an adhesive resin layer 15 and a sealant layer 16 on the second corrosion prevention treatment layer 14b of the first laminate formed in the previous process to obtain a second laminate. Examples of the method include a method of sand laminating the adhesive resin layer 15 together with the sealant layer 16 using an extrusion laminator, and a thermal lamination method such as co-extrusion in which the adhesive resin layer 15 and the sealant layer 16 are extruded. In forming the adhesive resin layer 15 and the sealant layer 16, for example, the above-mentioned resin composition for forming the adhesive resin layer and resin composition for forming the sealant layer are used.
[0122] When forming the adhesive resin layer 15, a masterbatch may be prepared by mixing a resin and a hydrophobic insulating inorganic filler in advance, and then this masterbatch may be mixed with the base resin described above to obtain a resin composition for forming an adhesive resin layer. In this case, the base resin may be a resin having similar properties, such as MFR, to the resin contained in the masterbatch. The resin mixed with the hydrophobic insulating inorganic filler when preparing the masterbatch may be a modified polyolefin resin. Acid-modified polyolefin resins are particularly preferred as modified polyolefin resins because they are easily mixed with the base resin and improve adhesion between the barrier layer 13 and the adhesive resin layer 15. Furthermore, the concentration of the masterbatch in the resin composition for forming the adhesive resin layer may be, for example, 5 to 50% by mass. When the concentration of the masterbatch in the resin composition for forming the adhesive resin layer is 5% by mass or more, the masterbatch can be sufficiently dispersed in the adhesive resin layer 15. Furthermore, when the concentration of the masterbatch in the resin composition for forming the adhesive resin layer is 50% by mass or less, sufficient dispersion is achieved during kneading during extrusion, reducing the likelihood of defects such as film breakage.
[0123] Furthermore, when forming the adhesive resin layer 15, the resin composition for forming the adhesive resin layer preferably further contains a dispersant. In this case, the dispersant can enhance the dispersibility of the hydrophobic insulating inorganic filler and also facilitates suppressing a decrease in the functionality (e.g., adhesion strength) of the adhesive resin layer 15. As the dispersant, for example, a surfactant such as metal soap (e.g., zinc stearate) is used. When the resin contains a modified polyolefin resin, the modified polyolefin resin can also function as a dispersant.
[0124] The method for forming the sealant layer 16 is the same as the method for forming the sealant layer 16 in the method for manufacturing the exterior packaging material 10.
[0125] This process produces a second laminate in which the layers are laminated in the following order: base layer 11 / first adhesive layer 12a / first corrosion prevention treatment layer 14a / metal layer 14c / second corrosion prevention treatment layer 14b / adhesive resin layer 15 / sealant layer 16, as shown in Figure 2.
[0126] (Heat Treatment Step) This step is a step of heat treating the second laminate. Heat treating the second laminate can improve adhesion between the metal layer 14c, the second corrosion prevention treatment layer 14b, the adhesive resin layer 15, and the sealant layer 16. As a heat treatment method, it is preferable to treat at a temperature at least equal to or higher than the melting point of the adhesive resin layer 15.
[0127] In this manner, the exterior packaging material 20 shown in FIG. 2 can be manufactured.
[0128] [Electricity Storage Device] Next, an embodiment of the electricity storage device of the present disclosure will be described with reference to Figures 3 and 4. Figure 3 is a perspective view of the embodiment of the electricity storage device of the present disclosure, and Figure 4 is a cross-sectional view showing the battery cell of Figure 3. As shown in Figure 3, the electricity storage device 50 includes a battery cell 52 and an outer bag 54 that houses the battery cell 52. The electricity storage device 50 may further include two metal terminals (current extraction terminals) 53 that extend from the battery cell 52 and are used to extract current to the outside. The two metal terminals 53 are sandwiched by the outer bag 54.
[0129] As shown in FIG. 4, the battery cell 52 has a positive electrode 52a, an electrolyte 52c, and a negative electrode 52b in this order.
[0130] The exterior bag 54 has an exterior material 10. In the exterior material 10, the base material layer 11 is the outermost layer and the sealant layer 16 is the innermost layer. The exterior bag 54 is formed by folding one exterior material 10 in half and heat-sealing the peripheral edges, or by stacking two exterior materials 10 and heat-sealing the peripheral edges, so that the base material layer 11 is on the outer side of the electricity storage device 50 and the sealant layer 16 is on the inner side of the electricity storage device 50. The metal terminal 53 is sandwiched by the peripheral edges of the exterior bag 54. The metal terminal 53 may be sandwiched by the exterior material 10 via a tab sealant.
[0131] According to the energy storage device 50, even when the exterior material 10 is used in a heated and pressurized state as the exterior bag 54, the energy storage device 50 has excellent insulating properties, and therefore, even when the energy storage device 50 is heated in a state where it is pressurized in a direction perpendicular to the interface between the battery cell 52 and the exterior material 10, it is possible to prevent a short circuit between the positive electrode 52a or negative electrode 52b in the battery cell 52 and the metal layer 14c of the exterior material 10.
[0132] The electrolyte 52c may be, for example, a solid electrolyte. In this case, the power storage device 50 is an all-solid-state battery. Examples of the solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.
[0133] Metal terminal 53 is a part of the current collector that is taken out to the outside of exterior packaging material 10, and is made of a metal foil such as copper foil or aluminum foil. Note that in electricity storage device 50, exterior packaging material 20 may be used instead of exterior packaging material 10.
[0134] Hereinafter, the present disclosure will be described more specifically based on examples, but the present disclosure is not limited to the following examples.
[0135] [Materials Used] The materials used in the Examples and Comparative Examples are as follows: <Base Layer> A nylon (Ny) film (manufactured by Toyobo Co., Ltd.) having a thickness of 15 μm was used.
[0136] <First adhesive layer-forming composition> As the first adhesive layer-forming composition, a polyurethane adhesive (manufactured by Toyo Ink Co., Ltd.) containing a polyester polyol-based base agent and a tolylene diisocyanate adduct-based curing agent was used.
[0137] <Materials for Forming the First Corrosion Prevention Treatment Layer (Substrate Layer Side) and the Second Corrosion Prevention Treatment Layer (Sealant Layer Side)> The following (CL-1) and (CL-2) were used as materials for forming the first corrosion prevention treatment layer (substrate layer side) and the second corrosion prevention treatment layer (sealant layer side). (CL-1): "Sodium polyphosphate-stabilized cerium oxide sol" obtained by using distilled water as a solvent and adjusting the solids concentration to 10% by mass. The sodium polyphosphate-stabilized cerium oxide sol was obtained by blending 10 parts by mass of sodium salt of phosphoric acid with 100 parts by mass of cerium oxide. (CL-2): A composition consisting of 90% by mass of "polyallylamine (manufactured by Nitto Boseki Co., Ltd.)" and 10% by mass of "polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation)" obtained by using distilled water as a solvent and adjusting the solids concentration to 5% by mass.
[0138] <Metal Layer> A soft aluminum foil (manufactured by Toyo Aluminum K.K., "8079 material") having a thickness of 40 μm that had been annealed and degreased was used.
[0139] <Composition for forming adhesive layer> As compositions for forming an adhesive layer, a composition for forming a second adhesive layer (adhesive) and a resin composition for forming an adhesive resin layer (adhesive resin) were prepared as follows: (Composition for forming second adhesive layer) The composition for forming a second adhesive layer was prepared by dispersing the hydrophobic insulating inorganic filler described below in a solvent consisting of methylcyclohexane and methyl ethyl ketone as needed, and then adding the acid-modified polyolefin resin-containing liquid, polyfunctional isocyanate compound-containing liquid, and carbodiimide compound-containing liquid described below.
[0140] (Resin composition for forming adhesive resin layer) Using a twin-screw extruder, the following hydrophobic insulating inorganic filler was dispersed as needed in an adhesive resin (random polypropylene (PP)-based acid-modified polypropylene resin composition, manufactured by Mitsui Chemicals, Inc.) to prepare a resin composition for forming an adhesive resin layer.
[0141] (1) Acid-modified polyolefin resin-containing liquid Nippon Paper Industries Co., Ltd., product name: 150S, acid-modified polyolefin resin: maleic anhydride-modified polypropylene (2) Polyfunctional isocyanate compound-containing liquid Tosoh Corporation, product name: Coronate HXR, polyfunctional isocyanate compound: hexamethylene diisocyanate (HDI)-based polyisocyanurate resin (3) Carbodiimide compound-containing liquid Nisshinbo Chemical Inc., product name: V-03 (4) Hydrophobic insulating inorganic filler A: Hydrophobic silica filler (product name "Sylophorbic 100", Fuji Silysia Chemical Ltd., average particle size: 2.7 μm, surface-treated with an organosilicon compound) B: Hydrophobic silica filler (product name "Sylophorbic 704", Fuji Silysia Chemical Ltd., average particle size: 6.2 μm, surface-treated with an organosilicon compound) C: Hydrophobic silica filler (product name "Silohobic 4004", manufactured by Fuji Silysia Chemical Ltd., average particle size: 8.0 μm, surface treated with an organosilicon compound)
[0142] <Resin Composition for Forming Sealant Layer> A resin composition for forming a sealant layer containing a polypropylene-polyethylene random copolymer (manufactured by Prime Polymer Co., Ltd., trade name: F744NP) was prepared using a twin-screw extruder.
[0143] [Production of Exterior Material] (Example 1) First, a first and a second corrosion prevention treatment layer were formed on both sides of a metal layer by the following procedure. That is, the above (CL-1) was applied to both sides of the metal layer in a dry coating amount of 70 mg / m 2 The coated layer was then subjected to a baking treatment at 200°C in a drying unit to obtain a first layer. Next, (CL-2) was applied to the obtained first layer in a dry coating amount of 20 mg / m 2 The coating was applied by microgravure coating so that the second layer was obtained. In this way, composite layers composed of the first and second layers were formed on both sides of the metal layer as a first corrosion prevention treatment layer and a second corrosion prevention treatment layer, respectively, to obtain barrier layers. This composite layer exhibits corrosion prevention performance by combining the two types of compounds (CL-1) and (CL-2).
[0144] Next, the first corrosion prevention treatment layer of the barrier layer obtained as described above was attached to the substrate layer by dry lamination using a composition for forming a first adhesive layer (a polyurethane adhesive). Specifically, the lamination of the barrier layer and the substrate layer was performed by applying a polyurethane adhesive to the surface of the first corrosion prevention treatment layer opposite the metal layer so that the thickness after curing would be 5 μm, drying at 80° C. for 1 minute, laminating the substrate layer thereon, and aging at 60° C. for 72 hours. In this way, a first laminate including the barrier layer and the substrate layer was obtained.
[0145] Next, the first laminate obtained as described above was set on the unwinding section of an extrusion laminator, and the second adhesive layer-forming composition, in which the type, content and average particle size of the hydrophobic insulating inorganic filler in the total solids of the second adhesive layer-forming composition (adhesive layer (second adhesive layer)) were as shown in Table 1, was applied to the second corrosion prevention treatment layer so that the thickness after curing was 20 μm, dried at 100 ° C. for 1 minute, laminated with a sealant layer, and aged at 40 ° C. for 72 hours. This sealant layer was produced by extruding the sealant layer-forming resin composition under processing conditions of 270 ° C. and 100 m / min.
[0146] In this way, an exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) was produced.
[0147] Example 2 In the same manner as in Example 1, a first laminate including a barrier layer and a substrate layer was obtained.
[0148] Next, the first laminate obtained as described above was set on the unwinding section of an extrusion laminator, and an adhesive resin composition having the type, content and average particle size of the hydrophobic insulating inorganic filler as shown in Table 1 and a resin composition for forming a sealant layer were co-extruded onto the second corrosion prevention treatment layer under processing conditions of 270°C and 100 m / min, thereby laminating an adhesive resin layer (thickness 20 μm) and a sealant layer (thickness 60 μm) in this order, thereby obtaining a second laminate.
[0149] The second laminate thus obtained was subjected to a heat treatment so that the maximum temperature of the second laminate reached was 190° C. In this manner, an exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / adhesive resin layer / sealant layer) was produced.
[0150] (Examples 3 to 4) In the composition for forming the second adhesive layer, the type, content and average particle size of the hydrophobic insulating inorganic filler in the total solid content were as shown in Table 1, and in the composition for forming the second adhesive layer, the amount of the polyfunctional isocyanate compound blended was 1 part by mass per 100 parts by mass of the acid-modified polyolefin as shown in Table 1. Except for this, an exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) was produced in the same manner as in Example 1.
[0151] Comparative Example 1 In the composition for forming the second adhesive layer, the content of the hydrophobic insulating inorganic filler in the total solid content was 0 mass % as shown in Table 1, in the composition for forming the second adhesive layer, the amount of the polyfunctional isocyanate compound per 100 mass parts of acid-modified polyolefin was 0 mass parts as shown in Table 1, and the MFR of the sealant layer was 30 g / 10 min as shown in Table 1. An exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) was produced in the same manner as in Example 1, except that
[0152] (Comparative Example 2) The content of the hydrophobic insulating inorganic filler in the adhesive resin composition was 0 mass% as shown in Table 1, the amount of the polyfunctional isocyanate compound in the composition for forming the second adhesive layer was 0 mass parts per 100 mass parts of acid-modified polyolefin as shown in Table 1, and the MFR of the sealant layer was 30 g / 10 min as shown in Table 1. An exterior material (substrate layer / first adhesive layer / first corrosion prevention treatment layer / metal layer / second corrosion prevention treatment layer / adhesive resin layer / sealant layer) was produced in the same manner as in Example 2, except that the content of the hydrophobic insulating inorganic filler in the adhesive resin composition was 0 mass% as shown in Table 1, the amount of the polyfunctional isocyanate compound in the composition for forming the second adhesive layer was 0 mass parts per 100 mass parts of acid-modified polyolefin as shown in Table 1, and the MFR of the sealant layer was 30 g / 10 min as shown in Table 1.
[0153] <Evaluation> (1) Heat sealability (1-1) Preparation of test pieces The packaging materials obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were cut to a size of 50 mm (TD direction) x 100 mm (MD direction) to obtain cut pieces. This cut piece was folded in two so as to sandwich a chemical conversion treated aluminum foil cut to a size of 50 mm x 50 mm, and the end opposite the folded part (crease) was heat sealed over a width of 10 mm at 180 ° C. / 0.6 MPa / 10 seconds. Then, a 15 mm wide piece was cut out along the MD direction so as to include the center part in the longitudinal direction (TD direction) of the heat sealed part (see FIG. 5), and a test piece was prepared. (1-2) Seal Strength (Room Temperature) A T-peel test was performed on the test pieces prepared as described above at a room temperature (25°C) environment and a tensile speed of 50 mm / min using a tensile tester (manufactured by Shimadzu Corporation) to peel the exterior material from the chemically treated aluminum foil, and the seal strength (burst strength) was measured. (1-3) Evaluation The heat sealability was evaluated based on the seal strength (burst strength) obtained in (1-2) above, based on the following criteria. The seal strength and evaluation results are shown in Table 2. (Criteria) A: Seal strength is 20 N / 15 mm or more B: Seal strength is 15 N / 15 mm or more, but less than 20 N / 15 mm C: Seal strength is less than 15 N / 15 mm
[0154] (2) Adhesion The exterior packaging materials obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were cut to a width of 15 mm and a length of 120 mm to prepare test specimens. A T-peel test, in which the metal layer and the sealant layer were peeled off, was then performed on these test specimens using a tensile tester (manufactured by Shimadzu Corporation) at room temperature and a tensile speed of 50 mm / min to measure the laminate strength. The adhesion between the metal layer and the sealant layer was then evaluated based on the obtained laminate strength, according to the following criteria. The laminate strength and evaluation results are shown in Table 2. (Criteria) A: Laminate strength of 10 N / 15 mm or more, or peeling not possible B: Laminate strength of 3 N / 15 mm or more but less than 10 N / 15 mm C: Laminate strength of less than 3 N / 15 mm
[0155] (3) Insulation after Heat and Pressure The packaging materials obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were cut into 100 mm x 100 mm pieces to prepare test pieces. These test pieces were sandwiched between two electrodes measuring 20 mm x 20 mm, and heated and pressed at 150°C and 3 MPa for 24 hours, after which the breakdown voltage in the direction perpendicular to the surface of the test piece was measured. The insulation of the packaging material after heating and pressure was judged from the measured breakdown voltage based on the following criteria. The results are shown in Table 2. (Criteria) ◯: Breakdown voltage is 50 V or more ×: Breakdown voltage is less than 50 V
[0156]
[0157] The results shown in Table 2 show that in Examples 1 to 4, the insulation voltage after heating and pressurization was higher than 100 V, whereas in Comparative Examples 1 and 2, the insulation voltage after heating and pressurization was lower than 10 V.
[0158] From the above, it was confirmed that the packaging material for an electricity storage device according to the present disclosure has excellent insulating properties even when used as an outer bag for an electricity storage device in a heated and pressurized state.
[0159] The present disclosure is outlined as follows. [1] An electrical storage device packaging material including at least a substrate layer, a barrier layer including a metal layer, an adhesive layer, and a sealant layer, in this order, wherein the adhesive layer contains a hydrophobic insulating inorganic filler. [2] The electrical storage device packaging material according to [1], wherein the adhesive layer is obtained using a composition including the hydrophobic insulating inorganic filler, the composition including the hydrophobic insulating inorganic filler, a resin, and a polyfunctional isocyanate compound, and the resin is a modified polyolefin resin. [3] The electrical storage device packaging material according to [1] or [2], wherein the sealant layer has an MFR of 20 g / 10 min or less. [4] The electrical storage device packaging material according to any one of [1] to [3], wherein the sealant layer has a melting point of 160°C or higher. [5] The electrical storage device packaging material according to any one of [1] to [4], wherein the hydrophobic insulating inorganic filler has an average particle size of 1 to 20 μm. [6] The packaging material for a storage battery device according to any one of [1] to [5], which has a breakdown voltage of 100 V or more when heated and pressed for 24 hours under conditions of 150°C and 3 MPa. [7] The packaging material for a storage battery device according to [2], wherein the modified polyolefin resin is an acid-modified polyolefin resin. [8] The packaging material for a storage battery device according to [2], wherein the polyfunctional isocyanate compound contains an isocyanurate-type polyfunctional isocyanate compound. [9] The packaging material for a storage battery device according to any one of [1] to [8], wherein the content of the hydrophobic insulating inorganic filler in the adhesive layer is 0.5 to 20 mass %.
[10] The packaging material for a storage battery device according to any one of [1] to [9], wherein the barrier layer further comprises a corrosion prevention treatment layer on one or both surfaces of the metal layer.
[11] The packaging material for an electricity storage device according to any one of [1] to
[10] , further comprising a first adhesive layer between the base material layer and the barrier layer, the adhesive layer being a second adhesive layer, and the thickness of the second adhesive layer being greater than the thickness of the first adhesive layer.
[12] The packaging material for an electricity storage device according to any one of [1] to
[11] , wherein the electricity storage device is an all-solid-state battery.
[13] An electricity storage device comprising: a battery cell having a positive electrode, an electrolyte, and a negative electrode in this order; and an outer packaging bag that houses the battery cell, the outer packaging bag comprising the packaging material for an electricity storage device according to any one of [1] to
[11] .
[14] The electricity storage device according to
[13] , wherein the electricity storage device is an all-solid-state battery.
[0160] 10, 20...outer packaging material (outer packaging material for electricity storage device), 11...substrate layer, 12b...second adhesive layer (adhesive layer), 13...barrier layer, 14a...first corrosion prevention treatment layer (corrosion prevention treatment layer), 14b...second corrosion prevention treatment layer (corrosion prevention treatment layer), 14c...metal layer, 15...adhesive resin layer (adhesive layer, second adhesive layer), 16...sealant layer, 50...electricity storage device, 52...battery cell, 52a...positive electrode, 52b...negative electrode, 52c...electrolyte, 54...outer packaging bag.
Claims
1. An exterior material for an electricity storage device comprising, in this order, at least a base material layer, a barrier layer including a metal layer, an adhesive layer, and a sealant layer, wherein the adhesive layer contains a hydrophobic insulating inorganic filler.
2. The exterior material for a storage battery device according to claim 1, wherein the adhesive layer is obtained using a composition containing a hydrophobic insulating inorganic filler, the composition containing the hydrophobic insulating inorganic filler, a resin and a polyfunctional isocyanate compound, and the resin is a modified polyolefin resin.
3. The packaging material for a storage battery device according to claim 1, wherein the MFR of the sealant layer is 20 g / 10 min or less.
4. The packaging material for a storage battery device according to claim 1, wherein the melting point of the sealant layer is 160°C or higher.
5. The packaging material for a storage battery device according to claim 1, wherein the hydrophobic insulating inorganic filler has an average particle size of 1 to 20 μm.
6. The packaging material for a storage battery device according to claim 1, which has a dielectric breakdown voltage of 100 V or more when heated and pressed at 150° C. and 3 MPa for 24 hours.
7. The exterior packaging material for a storage battery device according to claim 2, wherein the modified polyolefin resin is an acid-modified polyolefin resin.
8. The packaging material for a storage battery device according to claim 2, wherein the polyfunctional isocyanate compound includes an isocyanurate-type polyfunctional isocyanate compound.
9. The exterior packaging material for a storage battery device according to claim 1, wherein the content of the hydrophobic insulating inorganic filler in the adhesive layer is 0.5 to 20 mass %.
10. The packaging material for an electricity storage device according to claim 1, wherein the barrier layer further comprises a corrosion prevention treatment layer on one or both surfaces of the metal layer.
11. The exterior material for a storage battery device according to claim 1, further comprising a first adhesive layer between the base material layer and the barrier layer, the adhesive layer being a second adhesive layer, and the thickness of the second adhesive layer being greater than the thickness of the first adhesive layer.
12. The exterior packaging material for an electricity storage device according to claim 1, wherein the electricity storage device is an all-solid-state battery.
13. An electricity storage device comprising: a battery cell having a positive electrode, an electrolyte, and a negative electrode in this order; and an outer bag that houses the battery cell, the outer bag having the outer casing material for electricity storage devices according to any one of claims 1 to 11.
14. The power storage device according to claim 13, which is an all-solid-state battery.
Citation Information
Patent Citations
Battery packaging film and manufacturing method thereof
CN116254069A
Barrier laminate, packaging material using the same, and package using packaging material
JP2000006304A
Laminated material for secondary cell
JP2003217529A
Exterior material for battery and lithium secondary battery
JP2014127258A
Exterior material for power storage device
JP2017050168A