Lithium ion secondary battery

By dispersing surface-treated boron nitride nanotubes in the electrolyte, the ionic conductivity and stability of lithium ion secondary batteries are improved, addressing the conductivity limitations and enhancing performance and safety.

WO2024242237A1PCT designated stage expired Publication Date: 2024-11-28NAIEEL TECHNOLOGY INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/012578
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-03
Filing Date
2023-08-24
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face limitations in ionic conductivity, affecting their efficiency and performance, particularly due to the low dispersibility of boron nitride nanotubes in organic and aqueous solvents, which hampers their charging and discharging capabilities.

Method used

Dispersing boron nitride nanotubes in the electrolyte of lithium ion secondary batteries, with surface treatment to enhance hydrophilicity or hydrophobicity, improves their ionic conductivity and stability, thereby enhancing the battery's performance and safety.

Benefits of technology

The dispersion of boron nitride nanotubes in the electrolyte increases lithium ion conductivity, maintains performance over time, and improves thermal stability, leading to enhanced charge/discharge capacity and long-term stability of lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023012578_28112024_PF_FP_ABST
    Figure KR2023012578_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a lithium ion secondary battery, the lithium ion secondary battery according to an embodiment of the present invention comprising: an electrode assembly comprising a negative electrode, a positive electrode, and a separator disposed therebetween; a case accommodating the electrode assembly; and an electrolyte filling the case, wherein boron-nitride nanotubes are dispersed in the electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

lithium ion secondary battery

[0001] The present invention relates to a lithium ion secondary battery.

[0002] Secondary batteries, unlike disposable batteries that are discarded after use, are reusable through repeated charging and discharging. They are used in various fields such as mobile phones, laptops, and electric vehicles, and their use as energy storage devices is also increasing recently.

[0003] There are various types of secondary batteries, but the most representative one is the lithium-ion secondary battery. Lithium-ion secondary batteries have high energy density, no memory effect, relatively short charging times, and easy charging and discharging. Meanwhile, the charge / discharge efficiency and charging time of lithium-ion secondary batteries are affected by the ionic conductivity of lithium ions. Therefore, to improve the efficiency of lithium-ion secondary batteries, the ionic conductivity of lithium ions needs to be improved.

[0004] Embodiments of the present invention provide a lithium ion secondary battery having improved ionic conductivity.

[0005] One embodiment of the present invention discloses a lithium ion secondary battery comprising: an electrode assembly including a cathode, an anode, and a separator disposed between the cathode and the anode; a case accommodating the electrode assembly; and an electrolyte filled within the case; wherein boron nitride nanotubes are dispersed within the electrolyte.

[0006] According to embodiments of the present invention, boron nitride nanotubes are dispersed in an electrolyte, thereby increasing the ionic conductivity of a lithium ion secondary battery, and thus improving the performance of the lithium ion secondary battery.

[0007] In addition, the thermal stability of the separator is improved by the boron nitride nanotubes attached to the surface of the separator, so that the safety of the secondary battery can be improved.

[0008] FIG. 1 is a cross-sectional view schematically illustrating an example of a lithium ion secondary battery according to one embodiment of the present invention.

[0009] FIG. 2 is a perspective view schematically illustrating an example of boron nitride nanotubes dispersed in the electrolyte of FIG. 1.

[0010] Figure 3 is a TEM image of boron nitride nanotubes dispersed in the electrolyte of Figure 1.

[0011] FIG. 4 is a perspective view schematically illustrating an example of surface-treated boron nitride nanotubes dispersed in the electrolyte of FIG. 1.

[0012] Figure 5 is a flowchart schematically illustrating a method for surface treatment of boron nitride nanotubes of Figure 4.

[0013] FIG. 6 is a perspective view schematically illustrating another example of surface-treated boron nitride nanotubes dispersed in the electrolyte of FIG. 1.

[0014] Figure 7 is a flowchart schematically illustrating a method for surface treatment of boron nitride nanotubes of Figure 6.

[0015] Figure 8 is a graph showing lithium ion conductivity when boron nitride nanotubes are dispersed in an electrolyte.

[0016] Figure 9 is a graph showing lithium ion conductivity according to temperature change when boron nitride nanotubes are dispersed in an electrolyte.

[0017] Figure 10 is a graph showing lithium ion conductivity when various additives are dispersed in the electrolyte.

[0018] Figures 11 and 12 are graphs showing the results of CV (cyclic vloltammetry) tests of lithium ion secondary batteries.

[0019] Figure 13 is a graph showing the results of measuring the charge / discharge capacity of the lithium ion secondary battery of Figure 1.

[0020] Figures 14 to 16 are diagrams showing the characteristics (rate performance) of a lithium ion secondary battery according to temperature and charge / discharge rate.

[0021] Figure 17 is a graph showing the results of a long-term stability test of a lithium ion secondary battery.

[0022] Figure 18 is an SEM image showing a cross-section of a separator.

[0023] Figure 19 shows the results of measuring the shrinkage of the separator of Figure 18.

[0024] Figure 20 is a graph showing the results of a CV (cyclic vloltammetry) test of a lithium ion secondary battery when surface-treated with boron nitride nanotubes.

[0025] One embodiment of the present invention discloses a lithium ion secondary battery comprising: an electrode assembly including a cathode, an anode, and a separator disposed between the cathode and the anode; a case accommodating the electrode assembly; and an electrolyte filled within the case; wherein boron nitride nanotubes are dispersed within the electrolyte.

[0026] In the present embodiment, the boron nitride nanotubes may be included in the electrolyte in an amount of 0.1 wt% to 3.0 wt% with respect to 100 wt% of the electrolyte.

[0027] In this embodiment, the aspect ratio of the boron nitride nanotube may be 20 to 6000.

[0028] In this embodiment, the boron nitride nanotubes may be surface-treated to have hydrophilicity or hydrophobicity.

[0029] In the present embodiment, the surface-treated boron nitride nanotube further includes a first layer positioned on at least a portion of the boron nitride nanotube, wherein the first layer includes a hydroxyphenyl group and is capable of forming a π bond with the boron nitride nanotube.

[0030] In this embodiment, the surface-treated boron nitride nanotubes may have the hydrophilicity.

[0031] In the present embodiment, the first layer may include at least one of a polyphenol group, tannic acid, gallic acid, catechol, epigallocatechin, pyrogallol, hexahydroxydiphenic acid, ellagic acid, and chlorogenic acid.

[0032] In the present embodiment, the surface-treated boron nitride nanotube further includes a second layer on the first layer, the second layer is surface-treated to include an amine group or a thiol group as a hydrocarbon group, and the surface-treated boron nitride nanotube may have hydrophobicity.

[0033] In the present embodiment, the second layer may include at least one of an alkyl amine, an alkyl thiol, an aryl amine, an aryl thiol, a benzyl amine, and a benzyl thiol.

[0034] In this embodiment, the boron nitride nanotubes can be attached to the surface of the separator.

[0035] The present invention is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. The effects and features of the present invention, as well as the methods for achieving them, will become clearer with reference to the embodiments described in detail below, along with the drawings. However, the present invention is not limited to the embodiments disclosed below and can be implemented in various forms.

[0036] In the examples below, the terms first, second, etc. are not used in a limiting sense, but are used for the purpose of distinguishing one component from another.

[0037] In the examples below, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0038] In the examples below, terms such as “include” or “have” mean that a feature or component described in the specification is present, and do not preclude the possibility that one or more other features or components may be added.

[0039] In the following examples, when a part such as a film, region, component, etc. is said to be on or above another part, it includes not only a case where it is directly on top of the other part, but also a case where another film, region, component, etc. is interposed in between.

[0040] For convenience of explanation, the sizes of components in the drawings may be exaggerated or reduced. For example, the sizes and thicknesses of each component shown in the drawings are arbitrarily indicated for convenience of explanation, and thus the present invention is not necessarily limited to what is shown.

[0041] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings, and when describing with reference to the drawings, identical or corresponding components will be given the same drawing reference numerals.

[0042] FIG. 1 is a cross-sectional view schematically illustrating an example of a lithium ion secondary battery according to an embodiment of the present invention, FIG. 2 is a perspective view schematically illustrating an example of boron nitride nanotubes dispersed in the electrolyte of FIG. 1, and FIG. 3 is a TEM image of boron nitride nanotubes dispersed in the electrolyte of FIG. 1.

[0043] First, referring to FIG. 1, a lithium ion secondary battery (10) according to one embodiment of the present invention may include an electrode assembly (100), a case (200) that accommodates the electrode assembly, and an electrolyte (300) filled within the case (200).

[0044] The electrode assembly may include an anode (110), a cathode (120), and a separator (130) therebetween to prevent short circuiting of the anode (110) and the cathode (120).

[0045] The positive electrode (110) may include a positive electrode film (112) and a positive electrode active material layer (114) applied on the positive electrode film (112). In FIG. 1, the positive electrode active material layer (114) is illustrated as being applied to one side of the positive electrode film (112), but this is not limited thereto, and the positive electrode active material layer (114) may be applied to both sides of the positive electrode film (112).

[0046] The anode film (112) may be a metal formed of aluminum, stainless steel, titanium, silver, or a combination of materials selected from these.

[0047] The positive electrode active material layer (114) may include a positive electrode active material, a binder, and a conductive agent.

[0048] The cathode active material may be formed of a material capable of reversibly absorbing and releasing lithium ions. For example, the cathode active material may include at least one material selected from the group consisting of lithium transition metal oxides such as lithium cobaltate, lithium nickelate, lithium nickel cobaltate, lithium nickel cobalt alumina, lithium nickel cobalt manganese, lithium manganate, and lithium iron phosphate, nickel sulfide, copper sulfide, sulfur, iron oxide, and vanadium oxide.

[0049] The binder may include at least one material selected from the group consisting of polyvinylidene fluoride-based binders such as polyvinylidene fluoride, vinylidene fluoride / hexafluoropropylene copolymer, vinylidene fluoride / tetrafluoroethylene copolymer, carboxymethylcellulose-based binders such as sodium-carboxymethylcellulose, lithium-carboxymethylcellulose, acrylate-based binders such as polyacrylic acid, lithium-polyacrylic acid, acrylic, polyacrylonitrile, polymethyl methacrylate, polybutylacrylate, polyamideimide, polytetrafluoroethylene, polyethylene oxide, polypyrrole, lithium-Nafion, and styrene butadiene rubber-based polymers.

[0050] The conductive agent may include at least one material selected from the group consisting of carbon-based conductive agents such as carbon black, carbon fibers, carbon nanotubes, and graphite, conductive fibers such as metal fibers, metal powders such as fluorocarbon powder, aluminum powder, and nickel powder, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and conductive polymers such as polyphenylene derivatives.

[0051] The negative electrode (120) may include a negative electrode film (122) and a negative electrode active material layer (124) applied on the negative electrode film (122). The negative electrode active material layer (124) may be applied on one or both sides of the negative electrode film (122).

[0052] The negative electrode film (122) may include at least one metal selected from the group consisting of copper, stainless steel, nickel, titanium, etc. The negative electrode active material layer (124) may include a negative electrode active material, a binder, and a conductive agent.

[0053] The negative electrode active material may be formed of a material capable of alloying with lithium or reversibly absorbing and releasing lithium. For example, the negative electrode active material may include at least one material selected from the group consisting of metals, carbon-based materials, metal oxides, and lithium metal nitrides.

[0054] The metal may include at least one material selected from the group consisting of lithium, silicon, magnesium, calcium, aluminum, germanium, tin, lead, arsenic, antimony, bismuth, silver, gold, zinc, cadmium, mercury, copper, iron, nickel, cobalt and indium.

[0055] The carbon-based material may include at least one material selected from the group consisting of graphite, graphite carbon fibers, carbon nanotubes, coke, mesocarbon microbeads (MCMB), polyacene, pitch-based carbon fibers, and hard carbon.

[0056] The metal oxide may include at least one selected from the group consisting of lithium titanium oxide, titanium oxide, molybdenum oxide, niobium oxide, iron oxide, tungsten oxide, tin oxide, amorphous tin composite oxide, silicon monoxide, cobalt oxide, and nickel oxide.

[0057] The binder and the conductive agent may be the same as those included in the positive electrode active material layer, respectively.

[0058] The separator (130) separates the positive electrode (110) and the negative electrode (120) to prevent a short circuit between the positive electrode (110) and the negative electrode (120). The separator (130) may be manufactured by coating a polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP co-polymer) on any one substrate selected from the group consisting of, for example, polyethylene (PE), polystyrene (PS), polypropylene (PP), and a copolymer of polyethylene (PE) and polypropylene (PP), but is not limited thereto.

[0059] The case (200) may be made of various shapes and materials depending on the type of lithium ion secondary battery (10). The lithium ion secondary battery (10) may be coin-shaped, square-shaped, pouch-shaped, or cylindrical, and accordingly, the case (200) may be rigid coin-shaped, square-shaped, or cylindrical, or flexible pouch-shaped.

[0060] An electrolyte (300) is filled inside the case (200), and the electrode assembly (100) can be immersed in the electrolyte (300).

[0061] The electrolyte (300) may be a non-aqueous electrolyte including a lithium salt, an organic solvent, etc. However, the present invention is not limited thereto, and the electrolyte (300) may be an aqueous electrolyte, a gel polymer electrolyte, etc. In addition, the electrolyte (300) may have hydrophilicity or hydrophobicity.

[0062] Boron nitride nanotubes (BNNT) can be dispersed within the electrolyte (300) to improve the conductivity of lithium ions. As illustrated in FIG. 2, boron nitride nanotubes (BNNT) are one-dimensional hexagonal nanotubes in which nitrogen (N) and boron (B) are alternately arranged, and can have an aspect ratio of 20 to 6000, and the outer surface and inner space of the one-dimensional boron nitride material (BNNT) can be utilized as a migration path for lithium ions.

[0063] More specifically, the electron deficiency (Lewis acid) at the boron center of boron nitride nanotubes (BNNTs) can interact with oxygen-rich electrolyte molecules to induce the desolvation of lithium ions, thereby improving lithium ion transport across the surface and within the BNNTs. That is, the Lewis acid interaction between the anion / solvent and the BNNTs can promote the dissociation of lithium ions and accelerate the transport of lithium ions, leading to high lithium ion transport rates.

[0064] Such boron nitride nanotubes (BNNTs) can be included in an amount of 0.1 wt% to 3.0 wt% relative to 100 wt% of the electrolyte (300) containing boron nitride nanotubes (BNNTs).

[0065] When the content of boron nitride nanotubes (BNNT) is 0.1 wt% or more with respect to the total 100 wt% of the electrolyte (300), lithium ion conductivity increases, and thus the performance of the lithium ion secondary battery (10) may be improved. On the other hand, when the content of boron nitride nanotubes (BNNT) is greater than 3 wt% with respect to the total 100 wt% of the electrolyte (300), the amount of the electrolyte (300) in the lithium ion secondary battery (10) decreases, and aggregation of the boron nitride nanotubes (BNNT) occurs, thereby decreasing lithium ion conductivity and reducing the charging performance and capacity of the lithium ion secondary battery.

[0066] Meanwhile, to improve lithium ion conductivity, boron nitride nanotubes (BNNTs) need to be uniformly dispersed within the electrolyte (300). However, since boron nitride nanotubes (BNNTs) generally have low dispersibility in organic and aqueous solvents, the dispersibility of boron nitride nanotubes (BNNTs) can be improved by surface-treating the surface of the boron nitride nanotubes (BNNTs) to be hydrophilic or hydrophobic. This will be described with reference to FIGS. 4 to 7.

[0067] FIG. 4 is a perspective view schematically illustrating an example of surface-treated boron nitride nanotubes dispersed in the electrolyte of FIG. 1, and FIG. 5 is a flowchart schematically illustrating a method for surface-treating the boron nitride nanotubes of FIG. 4.

[0068] FIG. 4 illustrates an example of a surface-treated boron nitride nanotube (BNNT'). Referring to FIG. 4, the surface-treated boron nitride nanotube (BNNT') may include a first layer (410) on at least a portion of the boron nitride nanotube (BNNT) surface.

[0069] The first layer (410) can, for example, include a hydroxyphenyl group to make the boron nitride nanotube (BNNT) hydrophilic, thereby allowing the surface-treated boron nitride nanotube (BNNT') to be well dispersed in a polar electrolyte.

[0070] For example, the first layer (410) may include a hydroxyphenyl group and may form a bond with boron nitride nanotubes (BNNTs). As an example, the first layer (410) may include a polyphenol group, such as at least one of tannic acid, gallic acid, catechol, epigallocatechin, pyrogallol, hexahydroxydiphenic acid, ellagic acid, and chlorogenic acid.

[0071] The polyphenol group of the first layer (410) can be oxidized into a highly reactive quinone oligomer and attached to the surface of a boron nitride nanotube (BNNT), and the first layer (410) can be formed on the boron nitride nanotube (BNNT) by a strong interaction between the catechol molecules of the polyphenol group and the boron nitride nanotube (BNNT) through van der Waals bonding and π-π stacking.

[0072] In this way, since the first layer (410) is formed on at least a portion of the surface of the boron nitride nanotube (BNNT), thereby allowing hydroxyl groups to exist on the surface of the boron nitride nanotube (BNNT), the surface-treated boron nitride nanotube (BNNT') can have hydrophilicity, and thus, the dispersibility in a hydrophilic electrolyte can be improved.

[0073] The method for forming the first layer (410) may include, as illustrated in FIG. 5, a step (S110) of forming a mixture by mixing a first surface treatment agent in water, a step (S120) of dispersing boron nitride nanotubes (BNNTs) in the mixture to form a dispersion, and a step (S130) of washing and drying boron nitride nanotubes (BNNTs) from the dispersion.

[0074] The first surface treatment agent is a material capable of forming the first layer (410) and may include a hydroxyphenyl group. For example, the first surface treatment agent may include a polyphenol group and at least one of tannic acid, gallic acid, catechol, epigallocatechin, pyrogallol, hexahydroxydiphenic acid, ellagic acid, and chlorogenic acid.

[0075] The first surface treatment agent may be included in an amount of 0.1 wt% to 0.2 wt% based on the entire mixture. If the content of the first surface treatment agent in the mixture is less than 0.1 wt%, it is difficult to form a first layer (410) capable of imparting hydrophilicity to boron nitride nanotubes (BNNTs). On the other hand, even if the content of the first surface treatment agent is greater than 0.2 wt%, the surface treatment effect of the boron nitride nanotubes (BNNTs) does not continuously increase. Therefore, the content of the first surface treatment agent is preferably 0.1 wt% to 0.2 wt% based on the entire mixture.

[0076] Next, boron nitride nanotubes (BNNTs) are dispersed in the mixture. Dispersion can be achieved by ultrasonic dispersion, stirring, etc.

[0077] At this time, the dispersion may have a weak alkaline property. Since the dispersion has a weak alkaline property, the polyphenol group can be oxidized into a highly reactive quinone oligomer by the dissolved oxygen in the dispersion, and as a result, it can be attached to the surface of boron nitride nanotubes (BNNTs), thereby forming a first layer (410).

[0078] The pH of the dispersion can be adjusted using a base such as sodium hydroxide. For example, the pH of the dispersion can be 8 to 9. If the pH of the dispersion is lower than 8 or higher than 9, it is difficult to form quinone oligomers, so the pH of the dispersion is preferably 8 to 9.

[0079] The mixing ratio of boron nitride nanotubes (BNNTs) dispersed in the dispersion and the first surface treatment agent may be 1:1 to 1:0.1 in wt%. If the content of boron nitride nanotubes (BNNTs) dispersed in the dispersion exceeds 10 times that of the first surface treatment agent, it may be difficult to effectively form the first layer (410) on the surface of the boron nitride nanotubes (BNNTs). On the other hand, if the content of boron nitride nanotubes (BNNTs) dispersed in the dispersion is less than 1 time that of the first surface treatment agent, the amount of the first surface treatment agent discarded in the subsequent washing process increases rapidly.

[0080] After dispersing boron nitride nanotubes (BNNT) in a mixture to form a dispersion, the boron nitride nanotubes (BNNT) in which the first layer (410) is formed are washed and dried.

[0081] In the washing step, the surface-treated boron nitride nanotubes (BNNTs) are washed with water to remove any remaining polyphenol groups. Subsequently, only the surface-treated boron nitride nanotubes (BNNTs) are collected through centrifugation or filtering, and then dried to obtain a powder of surface-treated boron nitride nanotubes (BNNTs) that have been imparted with hydrophilicity.

[0082] The above method can be performed at room temperature and in an air atmosphere. Therefore, according to the present invention, boron nitride nanotubes can be made hydrophilic by a simple method of dispersing the boron nitride nanotubes in a mixture of the first surface treatment agent and water, without creating a specific environment. Furthermore, tannic acid and the like contained in the first layer are environmentally friendly substances derived from nature, so the surface-treated boron nitride nanotubes may not cause environmental pollution.

[0083] FIG. 6 is a perspective view schematically illustrating another example of surface-treated boron nitride nanotubes dispersed in the electrolyte of FIG. 1, and FIG. 7 is a flowchart schematically illustrating a method for surface-treating the boron nitride nanotubes of FIG. 6.

[0084] Fig. 6 illustrates another example of a surface-treated boron nitride nanotube (BNNT''). Referring to Fig. 6, the surface-treated boron nitride nanotube (BNNT'') may include a first layer (410) formed on at least a portion of the surface of the boron nitride nanotube (BNNT) and a second layer (420) on the first layer (410). That is, compared to the surface-treated boron nitride nanotube (BNNT') of Fig. 4, by further including the second layer (420), the boron nitride nanotube (BNNT) may be made hydrophobic.

[0085] The second layer (420) can be formed on the first layer (410). The first layer (410) is the same as that illustrated and described in FIG. 4, and thus will not be described again.

[0086] The second layer (420) is a layer for imparting hydrophobicity to boron nitride nanotubes (BNNTs) and may include an amine group or a thiol group as a hydrocarbon group. For example, the second layer (420) may include at least one of an alkyl amine, an alkyl thiol, an aryl amine, an aryl thiol, a benzyl amine, and a benzyl thiol.

[0087] Meanwhile, the polyphenol group of the first layer (410) can be oxidized into a highly reactive quinone oligomer and attached to the surface of a boron nitride nanotube (BNNT), and the quinone structure attached in this way can anchor the primary amine group of the second layer (420) by a Michael addition mechanism. More specifically, the reaction of the amine or thiol of the second layer (420) and the hydroxyl group of the first layer (410) is a reaction in which the amine or thiol of the second layer (420) undergoes a Michael addition to the hydroxyl group of the first layer (410), thereby allowing the second layer (420) to be formed on the first layer (410).

[0088] By including a second layer (420) like this, the surface-treated boron nitride nanotube (BNNT'') becomes hydrophobic, and thus can have excellent dispersibility for an electrolyte having hydrophobicity.

[0089] Meanwhile, the first layer (410) is omitted and the second layer (420) is not formed directly on the surface of the boron nitride nanotube (BNNT). Therefore, in order to form the second layer (420) to impart hydrophobicity to the boron nitride nanotube (BNNT), the first layer (410) must be formed first.

[0090] A method for forming a second layer (420) may include, as illustrated in FIG. 6, a step of forming a first mixture by mixing a first surface treatment agent in water (S210), a step of dispersing boron nitride nanotubes (BNNTs) in the first mixture to form a dispersion (S220), a step of forming a second mixture by mixing a second surface treatment agent in the dispersion (S230), and a step of washing and drying boron nitride nanotubes (BNNTs) from the second mixture (S240).

[0091] The step of forming the first mixture (S210) and the step of forming the dispersion (S220) are the same as the step of forming the mixture (S110 of FIG. 5) and the step of forming the dispersion (S120 of FIG. 5) of FIG. 5, so they will not be described repeatedly, and only the differences from FIG. 5 will be described.

[0092] Referring to Fig. 7, after forming a dispersion, a second surface treatment agent is additionally mixed into the dispersion to form a second mixture (S230). The second surface treatment agent is a substance for imparting hydrophobicity to boron nitride nanotubes (BNNTs) and may include an amine group or a thiol group as a hydrocarbon group capable of undergoing a Michael addition to the hydroxyl group of the first layer (410).

[0093] For example, the second surface treatment agent may include at least one of an alkyl amine, an alkyl thiol, an aryl amine, an aryl thiol, a benzyl amine, and a benzyl thiol.

[0094] The amount of the second surface treatment agent mixed may be 0.5 to 2 times the amount of the boron nitride nanotubes (BNNTs). If the amount of the second surface treatment agent mixed is less than 0.5 times the amount of the boron nitride nanotubes (BNNTs), it is difficult for the second layer to be effectively formed, making it difficult for the boron nitride nanotubes (BNNTs) to become hydrophobic. On the other hand, if the amount of the second surface treatment agent mixed is greater than 2 times the amount of the boron nitride nanotubes (BNNTs), the amount of the second surface treatment agent discarded during the subsequent washing process increases rapidly.

[0095] After dispersing boron nitride nanotubes (BNNTs) in the second mixture to form a dispersion, the boron nitride nanotubes on which the second layer is formed are washed and dried (S240).

[0096] In the washing step, the surface-treated boron nitride nanotubes (BNNTs) are sequentially washed with water and ethanol to remove any remaining polyphenol and hydrocarbon groups. Subsequently, only the boron nitride nanotubes (BNNTs) are collected through centrifugation or filtering, and then dried to obtain a powder of boron nitride nanotubes (BNNTs) that have been surface-treated to impart hydrophobicity.

[0097] Meanwhile, unlike the above method, when a second surface treatment agent was mixed in an organic solvent such as toluene and boron nitride nanotubes (BNNTs) were dispersed, a second layer (420) was not formed on the surface of the boron nitride nanotubes (BNNTs), and thus hydrophobicity could not be imparted to the boron nitride nanotubes (BNNTs). That is, in order to form the second layer (420), a first layer (410) must be formed in advance on the surface of the boron nitride nanotubes (BNNTs) by the first surface treatment agent.

[0098] The above method can be performed at room temperature and in an air atmosphere. Therefore, according to the present invention, boron nitride nanotubes (BNNTs) can be made hydrophobic by a simple method of dispersing BNNTs in a mixture of a first surface treatment agent and water, and then further mixing a second surface treatment agent, without creating a specific environment. In addition, according to the present method, since water is used as a dispersion medium in the process of surface-treating boron nitride nanotubes (BNNTs) to make them hydrophobic, the problem of environmental pollution caused by the use of organic solvents does not arise.

[0099] Figure 8 is a graph showing lithium ion conductivity when boron nitride nanotubes are dispersed in an electrolyte, and Figure 9 is a graph showing lithium ion conductivity according to temperature change when boron nitride nanotubes are dispersed in an electrolyte.

[0100] In Figs. 8 and 9, the electrolyte used was a 1:1 mixture of EC and DMC, in which 1 M LiPF6 was dispersed, and boron nitride nanotubes were dispersed within the electrolyte by ultrasonic dispersion. In addition, the ionic conductivity of the electrolyte was measured by electrochemical impedance spectroscopy (EIS) using a stainless steel disk as a blocking electrode.

[0101] Meanwhile, in Fig. 8, Neat represents the lithium ion conductivity when boron nitride nanotubes are not dispersed in the electrolyte. In addition, the content of boron nitride nanotubes is 1.5 g / cm when the density of the electrolyte is 1.5 g / cm. 3 The content was increased from 0.5 wt% to 1.1 wt% in increments of 0.2 wt%. Lithium ion conductivity was measured at room temperature (25°C), and the lithium ion conductivity was measured four times on the 1st, 3rd, 15th, and 30th days.

[0102] As can be seen in Fig. 8, in the case of Neat, the lithium ion conductivity on the first day was approximately 0.75 mS / cm, whereas in all cases where boron nitride nanotubes were dispersed in the electrolyte, the lithium ion conductivity increased compared to Neat. In this case, it was found that when the content of boron nitride nanotubes was 0.1 wt% or more, the lithium ion conductivity of the electrolyte increased.

[0103] Meanwhile, if the electrolyte contains more than 3.0 wt% of boron nitride nanotubes, the ionic conductivity decreases again. This is because, as the boron nitride nanotubes are applied in excess, the electrolyte content decreases and aggregation of the boron nitride nanotubes partially occurs. Therefore, it is preferable that the boron nitride nanotubes be contained in an amount of 0.1 wt% to 3.0 wt% based on 100 wt% of the total electrolyte including the boron nitride nanotubes.

[0104] Meanwhile, according to Fig. 8, the lithium ion conductivity of the electrolyte decreases over time, and it can be seen that the rate of decrease in lithium ion conductivity is relatively smaller in the case where boron nitride nanotubes are dispersed in the electrolyte compared to the case where boron nitride nanotubes are neat. From this, it can be seen that dispersing boron nitride nanotubes in the electrolyte improves lithium ion conductivity and maintains lithium ion conductivity over time.

[0105] Figure 9 shows the lithium ion conductivity according to the change in temperature when Neat and 0.9 wt% boron nitride nanotubes are dispersed in the electrolyte. Referring to Figure 9, it can be seen that when boron nitride nanotubes are dispersed in the electrolyte, the lithium ion conductivity increases compared to Neat not only at room temperature (25°C) and high temperature (60°C), but also at low temperature (-10°C).

[0106] In particular, in the case of Neat at low temperature (-10℃), the ionic conductivity was 0.22 mS / cm, whereas when 0.9 wt% of boron nitride nanotubes were dispersed in the electrolyte, the ionic conductivity was 0.27 mS / cm, indicating an increase of approximately 23%. Therefore, by dispersing boron nitride nanotubes in the electrolyte, rapid performance degradation of lithium ion secondary batteries at low temperatures can be prevented or minimized.

[0107] Table 1 below shows the results of measuring the lithium ion transference number when boron nitride nanotubes were dispersed in the electrolyte. The lithium ion transference number in Table 1 below was measured using the potentiostatic polarization method by fabricating a lithium symmetric cell using the electrolyte of Figure 8.

[0108] I ss (μA)I0(μA)R0(Ω)R ss (Ω)t + Neat19.3021.90380.44362.590.490.5wt%30.1032.40254.62250.240.660.7wt%37.7039.302 21.35218.100.700.9wt%34.0035.60224.22216.230.731.1wt%23.4026.16259.70251.860.70

[0109] As can be seen in Table 1 above, the ion transport number (t) is increased as a result of dispersing boron nitride nanotubes in the electrolyte. + ) can be seen to have increased. This is because boron nitride nanotubes function as a passage for lithium ions and can selectively improve the movement of lithium ions by accelerating the movement speed of lithium ions while suppressing the movement of anions. Figure 10 is a graph showing the lithium ion conductivity when various additives are dispersed in the electrolyte.

[0110] In Fig. 10, lithium ion conductivity was measured using the same method as in Fig. 8. However, in addition to boron nitride nanotubes (BNNT), various additives were used in the electrolyte, such as SiO2, h-BN, TiO2, and Al2O3, and the content of each additive was 0.9 wt%.

[0111] Figure 10 shows the lithium ion conductivity immediately after dispersion of the additive and 30 days after dispersion of the additive.

[0112] First, looking at the lithium ion conductivity immediately after dispersion of the additive, when boron nitride nanotubes (BNNT) are included in the electrolyte, the ion conductivity is improved compared to Neat, whereas when SiO2, h-BN, TiO2, and Al2O3 are included in the electrolyte, the ion conductivity is similar to or even lower than Neat.

[0113] In addition, the lithium ion conductivity measured 30 days after additive dispersion shows a significant decrease in the ion conductivity in the case of Neat. On the other hand, in the case of including SiO2, h-BN, TiO2, and Al2O3, the rate of decrease in lithium ion conductivity over time is smaller than that of Neat, but it is still greater than that of the case of including boron nitride nanotubes (BNNT).

[0114] In particular, when h-BN is included in the electrolyte, the ionic conductivity is lower than when boron nitride nanotubes (BNNTs) are included in the electrolyte. This is presumed to be because the plate-like shape of h-BN blocks the pores of the separator, preventing the ionic conductivity from improving.

[0115] In contrast, when boron nitride nanotubes (BNNTs) are included in the electrolyte, not only is the initial ionic conductivity improved by the boron nitride nanotubes (BNNTs), but the phenomenon of ionic conductivity decrease over time is reduced, so that excellent ionic conductivity characteristics can be maintained for a long period of time.

[0116] Figures 11 and 12 are graphs showing the results of CV (cyclic vloltammetry) tests of lithium ion secondary batteries.

[0117] Figures 11 and 12 are tests to confirm the possibility of a chemical reaction between an electrode and an electrolyte that occurs during charging and discharging of a lithium ion secondary battery. These are the results of confirming whether a chemical reaction occurred between a lithium metal electrode and a stainless steel electrode in a configuration having a separator between the lithium metal electrode and the stainless steel electrode.

[0118] Figure 11 shows the results of Neat, where boron nitride nanotubes were not dispersed in the electrolyte, and Figure 12 shows the results when 0.9 wt% of boron nitride nanotubes were dispersed in the electrolyte. In Figures 11 and 12, the scan rate was set to 0.1 mV and -0.2 to 5 V.

[0119] Referring to FIGS. 11 and 12, as can be seen in FIG. 12, even when boron nitride nanotubes are dispersed in the electrolyte, no significant peaks are generated in the CV (cyclic vloltammetry) test when the reduction voltage is less than 0 V or when the oxidation voltage is greater than 0 V. In particular, the irreversible oxidation peak when the voltage exceeds 4.8 V demonstrates the electrochemical stability of boron nitride nanotubes dispersed in the electrolyte and their feasibility for practical battery applications.

[0120] Figure 13 is a graph showing the results of measuring the charge / discharge capacity of a lithium ion secondary battery.

[0121] Figure 13 shows the results of precycling a lithium ion secondary battery including an NCM622 positive electrode and a graphite negative electrode from 2.7 V to 4.2 V at a charge / discharge rate of 0.1 C.

[0122] As can be seen in Fig. 13, the charge / discharge capacity of Neat, which does not contain boron nitride nanotubes in the electrolyte, is 152 mAh / g, whereas the charge / discharge capacity increases to 160.3 mAh / g when 0.9 wt% of boron nitride nanotubes are dispersed in the electrolyte. In other words, it can be seen that the charge capacity of a lithium ion secondary battery is improved as a result of dispersing boron nitride nanotubes in the electrolyte.

[0123] Figures 14 to 16 are diagrams showing the characteristics (rate performance) of a lithium ion secondary battery according to temperature and charge / discharge rate, respectively.

[0124] Figures 14 to 16 illustrate the specific capacity measured at different charge / discharge rates of the lithium ion secondary battery of Figure 13. Here, Figure 14 illustrates the results of measuring the specific capacity at 25°C, Figure 15 illustrates the results at 60°C, and Figure 16 illustrates the results at -10°C.

[0125] First, referring to FIG. 14, when 0.9 wt% of boron nitride nanotubes were dispersed in the electrolyte at 0.5 C, 1.0 C, 5.0 C, 10 C, and 15 C, the specific capacities were 157.9 mAh / g, 153.2 mAh / g, 137.2 mAh / g, 81.2 mAh / g, and 39.5 mAh / g, and in the case of Neat, the specific capacities were 129.4 mAh / g, 125.3 mAh / g, 91.0 mAh / g, 23.13 mAh / g, and 9.7 mAh / g.

[0126] Also, referring to FIG. 15, when 0.9 wt% of boron nitride nanotubes were dispersed in the electrolyte at 0.5 C, 1.0 C, 5.0 C, 10 C, and 15 C, the specific capacities were 116.4 mAh / g, 108.4 mAh / g, 87.99 mAh / g, 65.91 mAh / g, and 40.82 mAh / g, and in the case of Neat, the specific capacities were 83.9 mAh / g, 71.69 mAh / g, 50.25 mAh / g, 31.13 mAh / g, and 15.5 mAh / g.

[0127] Also, referring to FIG. 16, when 0.9 wt% of boron nitride nanotubes were dispersed in the electrolyte at 0.5 C, 1.0 C, 5.0 C, and 10 C, the specific capacities were 88.6 mAh / g, 38.7 mAh / g, 4.9 mAh / g, and 0.95 mAh / g, respectively, and in the case of Neat, the specific capacities were 63.3 mAh / g, 27.1 mAh / g, 4.7 mAh / g, and 0.04 mAh / g, respectively.

[0128] As can be seen from the above results, when boron nitride nanotubes are dispersed in the electrolyte, the charge / discharge and specific capacity characteristics are improved at low, room, and high temperatures compared to when they are not dispersed.

[0129] Figure 17 is a graph showing the results of a long-term stability test of a lithium ion secondary battery.

[0130] In Fig. 17, the lithium ion secondary battery used in Fig. 13 was used, and the charge / discharge test was measured under the conditions of 25°C, voltage 3.0 to 4.2 V, and C-rate 10C.

[0131] As can be seen in Fig. 17, the case of Neat, which does not contain boron nitride nanotubes in the electrolyte, has a charge / discharge capacity of 40 mAh / g and a coulombic efficiency of 97.5%, whereas the case where 0.9 wt% of boron nitride nanotubes are dispersed in the electrolyte maintains a charge / discharge capacity of 71.5 mAh / g and a coulombic efficiency of 99.6% even at a fast charge / discharge rate of 10C and stable charge / discharge even after more than 500 cycles. In other words, it can be seen that dispersing boron nitride nanotubes in the electrolyte not only improves the performance of lithium ion secondary batteries but also enhances their long-term stability.

[0132] Fig. 18 is an SEM image showing a cross-section of a separator, and Fig. 19 is a result of measuring the shrinkage result of the separator of Fig. 18.

[0133] In addition, Table 2 below shows the results of a heat shrinkage test of the separator. The heat shrinkage results measured in Table 2 represent the results of separating the separator from the lithium ion secondary battery of Fig. 13, drying it, and heat-treating it at 120°C for 1 hour.

[0134] Shrinkage (%)Neat10.530.5wt%5.260.7wt%5.260.9wt%4.741.1wt%4.211.8wt%2.63

[0135] As can be seen in Table 2 and FIG. 19, as the content of boron nitride nanotubes included in the electrolyte increases, the thermal shrinkage tendency of the separator decreases. This is because, as shown in FIG. 18, the boron nitride nanotubes are coated and attached to the surface of the separator as the separator is impregnated with the electrolyte. In addition, as shown in FIG. 18, it can be confirmed that the boron nitride nanotubes are attached in a direction that forms an angle with the surface of the separator rather than being completely laid down and attached to the surface of the separator, so that they can act as a passage for lithium ions to move directionally between the negative electrode and the positive electrode. Therefore, it can be seen that when boron nitride nanotubes are dispersed in the electrolyte, not only the ionic conductivity of the lithium ion secondary battery but also the thermal stability are improved.

[0136] Meanwhile, as the content of boron nitride nanotubes included in the electrolyte increases, the thermal stability of the separator improves. However, as explained above, when the content of boron nitride nanotubes exceeds 3.0 wt%, the amount of electrolyte decreases, which actually reduces lithium ion conductivity. Therefore, the content of boron nitride nanotubes should be less than 3.0 wt% in the electrolyte.

[0137] Figure 20 is a graph showing the results of a CV (cyclic vloltammetry) test when a lithium ion secondary battery includes surface-treated boron nitride nanotubes.

[0138] In Fig. 20, a lithium ion secondary battery was formed using the same method as in Fig. 11. However, in Fig. 20, boron nitride nanotubes dispersed in the electrolyte were surface-treated to have hydrophilic properties.

[0139] More specifically, 0.1 g of tannic acid was mixed in 100 mL of water and bath sonicated for 10 minutes to form a mixture, then 1 g of boron nitride nanotube powder was added to the mixture and tip sonicated for 60 minutes to form a dispersion. At this time, sodium hydroxide was mixed into the mixture so that the pH became 8. The surface-treated boron nitride nanotubes in the dispersion were washed with water, collected by filtering or centrifugation, and then dried at 80°C for 8 hours to surface-treat the boron nitride nanotubes.

[0140] As a result of dispersing 1.0 wt% of the surface-treated boron nitride nanotubes as described above in the electrolyte, the ionic conductivity was improved by 7 to 10% compared to when the same amount of non-surface-treated boron nitride nanotubes was dispersed in the electrolyte. This is because, as the boron nitride nanotubes are surface-treated, they are more uniformly dispersed in the electrolyte and their characteristics of maintaining the dispersed state are also improved.

[0141] In addition, the results of a CV (cyclic vloltammetry) test of a lithium ion secondary battery using an electrolyte in which surface-treated boron nitride nanotubes are dispersed in this manner using the same method as in FIG. 11 are shown in FIG. 20.

[0142] In Fig. 20, (E) is a case where an electrolyte is formed in which 1.0 wt% of boron nitride nanotubes are dispersed on both sides of the separator, and (F) is a case where an electrolyte is formed in which 1.5 wt% of boron nitride nanotubes are dispersed on both sides of the separator.

[0143] Referring to Fig. 20, the CV (cyclic vloltammetry) test results show that no significant peaks were generated, and from this, it can be confirmed that even when the boron nitride nanotubes are surface-treated using tannic acid, no chemical reaction occurs between the electrode and the electrolyte when reducing below 0 voltage or when oxidizing above 0 voltage. In other words, it can be confirmed that not only the dispersion characteristics but also the chemical stability are maintained by the surface treatment of the boron nitride nanotubes.

[0144] While the present invention has been described with reference to the embodiments illustrated in the drawings, these are merely exemplary, and those skilled in the art will appreciate that various modifications and variations of the embodiments are possible. Therefore, the true scope of technical protection of the present invention should be determined by the technical spirit of the appended claims.

Claims

1. An electrode assembly comprising a cathode, an anode, and a separator disposed between the cathode and the anode; a case accommodating the electrode assembly; and An electrolyte filled within the case; A lithium ion secondary battery having boron nitride nanotubes dispersed within the electrolyte.

2. In paragraph 1, A lithium ion secondary battery, wherein the boron nitride nanotubes are contained in the electrolyte in an amount of 0.1 wt% to 3.0 wt% with respect to 100 wt% of the electrolyte.

3. In paragraph 1, A lithium ion secondary battery wherein the aspect ratio of the above boron nitride nanotubes is 20 to 6000.

4. In paragraph 1, The above boron nitride nanotubes are surface-treated to have hydrophilic or hydrophobic properties, and are lithium ion secondary batteries.

5. In paragraph 1, In paragraph 4, The surface-treated boron nitride nanotube further comprises a first layer positioned on at least a portion of the boron nitride nanotube, A lithium ion secondary battery wherein the first layer contains a hydroxyphenyl group and forms a π bond with the boron nitride nanotube.

6. In paragraph 5, The surface-treated boron nitride nanotubes are a lithium ion secondary battery having the hydrophilic properties.

7. In paragraph 5, A lithium ion secondary battery wherein the first layer comprises at least one of a polyphenol group, tannic acid, gallic acid, catechol, epigallocatechin, pyrogallol, hexahydroxydiphenic acid, ellagic acid, and chlorogenic acid.

8. In paragraph 4, The surface-treated boron nitride nanotube further comprises a second layer on the first layer, The second layer is surface-treated to include an amine group or a thiol group as a hydrocarbon group, and the surface-treated boron nitride nanotube has hydrophobicity. A lithium ion secondary battery.

9. In paragraph 8, A lithium ion secondary battery, wherein the second layer comprises at least one of alkyl amine, alkyl thiol, aryl amine, aryl thiol, benzyl amine, and benzyl thiol.

10. In paragraph 1, The above boron nitride nanotubes are attached to the surface of the separator in a lithium ion secondary battery.

Citation Information

Patent Citations

  • Antioxidant, anti-inflammatory and skin soothing composition containing mung bean extract as an active ingredient

    KR1020240048978A

  • Drone Goods Discharge Device

    KR102594395B1

  • High temperature li-ion battery cells utilizing boron nitride aerogels and boron nitride nanotubes

    US20180159180A1