Flow guide tube and crystal pulling furnace used in process of pulling crystal rod by czochralski method

By using a deflector with a notch during the straight-pull faucet crystal making rod, the gas flow rate on the melt liquid surface is adjusted, and the interference between oxygen concentration control and production efficiency is solved, and oxygen on single crystal silicon rods is achieved The fine adjustment and uniformity of concentration improve the performance of the silicon wafer.

WO2024244346A1PCT designated stage expired Publication Date: 2024-12-05XIAN ESWIN MATERIAL TECHNOLOGY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/135270
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2023-11-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

During the straight-pull faucet crystal making process, there is interference between controlling the oxygen concentration and production efficiency in the single crystal silicon rod. The existing methods mainly rely on controlling the heating temperature of the quartz crucible, and it is difficult to independently adjust the oxygen content and distribution.

Method used

Design a flow guide cylinder with a notch at the bottom, adjusting the oxygen concentration by changing the flow rate of protective gas flowing through the melt liquid surface in the reference radial direction, and controlling the oxygen by adjusting the relative position between the flow guide cylinder and the horizontal magnetic field. Volatilize to achieve fine adjustment of the oxygen concentration of the crystal rod.

Benefits of technology

Effectively reduce or increase the oxygen concentration in single crystal silicon rods, reduce the unevenness of oxygen concentration, meet the strict requirements for oxygen content of electronic devices for different purposes, and improve the stability of silicon wafer performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023135270_05122024_PF_FP_ABST
    Figure CN2023135270_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A flow guide tube and a crystal pulling furnace used in a process of pulling a crystal rod by the Czochralski method, a bottom part of the flow guide tube has a notch, and the notch is used to change the flow rate of a protective gas flowing through the liquid surface of a melt in a reference radial direction by rotating the flow guide tube around the longitudinal axis thereof.
Need to check novelty before this filing date? Find Prior Art

Description

A guide tube and a crystal pulling furnace used in the process of pulling a crystal rod by the Czochralski method

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310611770.9 filed in China on May 26, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the field of semiconductor silicon wafer production, and in particular to a guide tube and a crystal pulling furnace used in the process of pulling a crystal rod by the Czochralski method. Background Art

[0004] Silicon wafers used in the production of semiconductor electronic components such as integrated circuits are primarily manufactured by slicing single-crystal silicon ingots pulled using the Czochralski method. The Czochralski method involves melting polycrystalline silicon in a quartz crucible to produce a silicon melt, immersing a single crystal seed crystal in the silicon melt, and continuously lifting the seed crystal away from the surface of the silicon melt, thereby growing a single crystal silicon ingot at the phase interface during this process.

[0005] The oxygen concentration in the pulled single crystal silicon rod is an important factor affecting the performance of the silicon wafer. The oxygen in the single crystal silicon rod can enhance the strength of the silicon wafer or form bulk micro defects (BMD) in the silicon wafer. The function of BMD is to absorb metal impurities generated during the processing. However, oxygen precipitation may also damage the performance of electronic devices, such as easily causing leakage current and device breakdown. Therefore, for electronic devices with different uses, there are different requirements for the size and distribution of their oxygen content, and these requirements are relatively stringent, which makes it necessary to better control the oxygen content in the crystal during crystal growth.

[0006] Oxygen in single-crystal silicon rods primarily originates from the melting of quartz crucibles, and its melting rate is related to the temperature and convection of the melt. Currently, the oxygen concentration in the drawn single-crystal silicon rod is typically controlled by controlling the heating temperature of the quartz crucible. However, the heating temperature of the quartz crucible must also meet requirements such as production efficiency, which leads to interference between the oxygen concentration requirements in the single-crystal silicon rod and production efficiency requirements. Therefore, providing a method for controlling the oxygen concentration in the drawn single-crystal silicon rod that is different from controlling the heating temperature of the quartz crucible has become an urgent problem in the field.

[0007] Summary of the Invention

[0008] In order to solve the above technical problems, the embodiments of the present application hope to provide a guide tube and a crystal pulling furnace used in the process of pulling crystal rods by the Czochralski method, which can control the oxygen concentration in the pulled single crystal silicon rod in a way different from controlling the heating temperature of the quartz crucible.

[0009] The technical solution of this application is achieved as follows:

[0010] In a first aspect, an embodiment of the present application provides a guide tube used in the process of pulling a crystal rod by the Czochralski method, wherein the bottom of the guide tube has a recess, and the recess is used to change the flow rate of the protective gas flowing through the liquid surface of the melt in a reference radial direction by rotating the guide tube around its own longitudinal axis.

[0011] When the direction of the horizontal magnetic field applied to the melt is the above-mentioned reference radial direction, when the guide tube is in a position where the recess is vertically opposite to the liquid surface of the melt and parallel to the horizontal magnetic field, the protective gas will flow through the recess at the bottom of the guide tube in the direction of the horizontal magnetic field, so the flow rate will be relatively large, thereby promoting the volatilization of oxygen in the melt, resulting in less oxygen reaching the solid-liquid interface between the crystal rod and the melt, and reducing the oxygen concentration in the crystal rod. When the guide tube is in a position where the recess is not vertically opposite to the liquid surface of the melt and parallel to the horizontal magnetic field, the protective gas cannot flow through the recess at the bottom of the guide tube in the direction of the horizontal magnetic field, and can only flow through the gap between the part of the bottom of the guide tube where the recess is not formed and the liquid surface of the melt, so the flow rate will be relatively small, thereby suppressing the volatilization of oxygen in the melt, resulting in more oxygen reaching the solid-liquid interface between the crystal rod and the melt, and increasing the oxygen concentration in the crystal rod.

[0012] Optionally, there are two recesses, which are opposite to each other in the radial direction of the guide sleeve.

[0013] Since the area that can be affected by the flow rate of the protective gas flowing through the liquid surface of the melt for the volatilization of oxygen in the melt exists in the entire radial direction, the two radially opposite notches can make full use of such an area. For example, when it is necessary to lower the oxygen concentration in the pulled crystal rod, compared with a guide tube with only a single notch, the guide tube with two radially opposite notches can better promote the volatilization of oxygen from the melt and thus reduce the oxygen concentration.

[0014] Optionally, the guide sleeve is arranged so that a connecting line between two of the recesses is parallel to a horizontal magnetic field applied to the melt.

[0015] In this case, for the protective gas flowing through the liquid surface of the melt, the flow rate is the largest in the direction parallel to the horizontal magnetic field, because the protective gas can flow through the recess at the bottom of the guide tube. In other words, over the entire circumference of the guide tube, the gap between the portion of the bottom where the recess is formed and the liquid surface of the melt is the largest, thereby obtaining a crystal rod with the lowest possible oxygen concentration.

[0016] In this case, the non-uniformity of the oxygen concentration in the circumferential direction of the crystal rod is minimized.

[0017] Optionally, the guide sleeve is arranged so that a connecting line between two notches is perpendicular to a horizontal magnetic field applied to the melt.

[0018] In this case, for the protective gas flowing through the liquid surface of the melt, the flow rate is the smallest in the direction parallel to the horizontal magnetic field, because the protective gas can only flow through the gap between the portion of the bottom of the guide tube where no notch is formed and the liquid surface of the melt, or in other words, it can only flow through the gap between the portion of the bottom of the guide tube that is raised relative to the notch and the liquid surface of the melt, and this gap is the smallest in the entire circumference of the guide tube, thereby obtaining a crystal rod with an oxygen concentration as high as possible.

[0019] Optionally, the notch is rectangular. In this way, for the protective gas flowing through the liquid surface of the melt, when, for example, it is necessary to accurately calculate the flow rate values ​​at different positions on the circumference of the guide tube, the calculation process can be simplified.

[0020] Optionally, the recess gradually expands toward the bottom of the guide tube. In this way, when the recess is obtained by removing material, the guide tube with the recess can be more easily manufactured.

[0021] In a second aspect, an embodiment of the present application further provides a crystal pulling furnace used in a process of pulling a crystal rod by the Czochralski method, wherein the crystal pulling furnace includes the guide tube according to the first aspect.

[0022] Optionally, the crystal pulling furnace further includes:

[0023] a furnace body, wherein the furnace body defines a furnace cavity;

[0024] A crucible is provided in the furnace cavity, and the melt is contained in the crucible.

[0025] Optionally, the crystal pulling furnace further comprises a heater, which is disposed in the furnace cavity and at the periphery of the crucible to heat the crucible, thereby melting the solid raw material contained in the crucible into the melt.

[0026] Optionally, the crystal pulling furnace further includes a heat-insulating element, which is disposed on an inner wall of the furnace body to suppress heat generated by the crucible heater from being dissipated through the furnace body. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] FIG1 is a schematic structural diagram of a conventional crystal pulling furnace for pulling crystal rods;

[0028] FIG2 is a schematic diagram of the trajectory of melt flow under the combined action of the heater and the horizontal magnetic field shown in FIG1 ;

[0029] FIG3 is a perspective schematic diagram of a guide tube used in a process of pulling a crystal ingot by the Czochralski method according to an embodiment of the present application;

[0030] FIG4 is a cross-sectional schematic diagram of a flow guide tube in a first position relative to a horizontal magnetic field according to an embodiment of the present application;

[0031] FIG5 is a cross-sectional schematic diagram of a flow guide tube in a second position relative to a horizontal magnetic field according to an embodiment of the present application;

[0032] FIG6 is a schematic diagram of the temperature distribution of the melt in a plane parallel to the liquid surface under the action of the heater shown in FIG1 ;

[0033] FIG7 is a front view schematic diagram of a guide tube used in a process of pulling a crystal ingot by the Czochralski method according to another embodiment of the present application;

[0034] FIG8 is a schematic structural diagram of a crystal pulling furnace used in a process of pulling a crystal rod by the Czochralski method according to an embodiment of the present application. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application.

[0036] First, referring to FIG1 , a conventional crystal pulling furnace 1A for pulling a crystal ingot R is shown. The crystal pulling furnace may include: a furnace body 20A; a crucible 30A disposed within the furnace body 20A and configured to contain a melt M; a heater 40A configured to heat the crucible 30A to melt a solid raw material, such as solid polysilicon, into the melt M and to maintain the melt M at a desired temperature; and a draft tube 10A configured to guide a protective gas, such as argon (not shown in detail in FIG1 ), to the liquid surface of the melt M to prevent undesirable chemical reactions in the melt M.

[0037] The oxygen contained in the pulled crystal ingot R primarily comes from the crucible 30A. Specifically, the crucible 30A melts under the high temperature of the melt M, and the oxygen contained in the crucible 30A enters the melt M. If the oxygen in the melt M reaches the solid-liquid interface between the crystal ingot R and the melt M, it will enter the crystal ingot R.

[0038] On the other hand, in the crystal pulling furnace 1A, under the heating action of the heater 40A, the melt M contained in the crucible 30A will generate thermal convection, and the instability of the melt M caused by the thermal convection will affect crystal pulling. In order to reduce the intensity of the convection in the melt M, a magnetic field is applied to the melt M to slow down the convection in the melt M through the Lorentz force. The types of applied magnetic fields can be divided into vertical magnetic fields, horizontal magnetic fields, and hook-shaped magnetic fields. These magnetic fields have their own advantages and disadvantages, and the horizontal magnetic field HM shown in Figure 1 can provide the highest intensity magnetic field (up to 0.4T) because its required coil diameter is smaller than that of the other two magnetic fields. However, the problem with the horizontal magnetic field HM is that it provides a non-center-symmetric magnetic field compared to the other two magnetic fields, which leads to complex asymmetry in the convection in the melt M.

[0039] Oxygen generated by the melting of crucible 30A under the high temperature of the melt M primarily exists on the inner wall of crucible 30A and flows along with the convection of the melt M formed under the action of the horizontal magnetic field HM, thereby reaching the solid-liquid interface between the crystal ingot R and the melt M. The following describes in detail how oxygen existing on the inner wall of crucible 30A reaches the solid-liquid interface between the crystal ingot R and the melt M, in conjunction with the convection of the melt M formed under the action of the horizontal magnetic field HM.

[0040] Referring to FIG2 , which schematically illustrates the flow trajectory of the melt M under the combined action of the heater 40A and the horizontal magnetic field HM shown in FIG1 , the crystal pulling furnace 1A shown in FIG1 and the flow trajectory shown in FIG2 are in the same coordinate system XYZ. Combining FIG1 and FIG2 , it can be seen that, in the XZ plane perpendicular to the horizontal magnetic field HM, due to the presence of a large, stable eddy current, oxygen dissolved at the inner wall of the crucible 30A quickly reaches the free surface of the melt M as the eddy current flows and rapidly volatilizes. However, in the XY plane, a vertical plane parallel to the horizontal magnetic field HM, namely the vertical plane, the melt M at the inner wall of the crucible 30A tends to flow toward the center of the entire melt M. In other words, within this plane, oxygen dissolved from the crucible 30A is unlikely to flow to the free surface of the melt M in a timely manner and volatilize. Instead, it is more likely to flow to the solid-liquid interface, causing an increase in the oxygen concentration in the crystal ingot R.

[0041] In this case, it is easy to understand that if one wants to influence the volatilization of oxygen in the melt M by the flow rate of protective gas flowing through the liquid surface of the melt M: assuming that the protective gas flows in the direction of the Z axis, or in other words, flows in a direction perpendicular to the horizontal magnetic field HM, then no matter what the flow rate of the protective gas is, it will not affect the volatilization of oxygen, because in this direction, the oxygen in the melt M has mainly reached the free surface of the melt M and volatilized; however, assuming that the protective gas flows in the direction of the Y axis, or in other words, flows in a direction parallel to the horizontal magnetic field HM, then when the flow rate of the protective gas is large, the volatilization of oxygen in the melt M will be promoted, thereby resulting in less oxygen reaching the solid-liquid interface between the crystal rod R and the melt M, thereby reducing the oxygen concentration in the crystal rod R; when the flow rate of the protective gas is small, the volatilization of oxygen in the melt M will be suppressed, thereby resulting in more oxygen reaching the solid-liquid interface between the crystal rod R and the melt M, thereby increasing the oxygen concentration in the crystal rod R.

[0042] On this basis, referring to Figures 3 to 5, an embodiment of the present application provides a guide tube 10 used in the process of pulling a crystal rod R as shown in Figure 1 by the Czochralski method. As shown in the stereoscopic view of Figure 3 and the cross-sectional view of Figure 4, the bottom 10B of the guide tube 10 may have a recess 10N, and the recess 10N is used to change the flow rate of the protective gas PG flowing through the liquid surface L of the melt M in the reference radial direction by rotating the guide tube 10 around its own longitudinal axis 10X. Specifically, assuming that the direction of the horizontal magnetic field HM is the above-mentioned reference radial direction, when the guide tube 10 is in the position shown in FIG4 relative to the horizontal magnetic field HM, in the direction of the horizontal magnetic field HM, or in the direction of the Y axis shown in FIG1 and FIG2 , the protective gas PG will flow through the notch 10N of the bottom 10B of the guide tube 10, so the flow rate will be relatively large, thereby promoting the volatilization of oxygen in the melt M as mentioned above, resulting in less oxygen reaching the solid-liquid interface between the crystal rod R and the melt M, reducing the oxygen concentration in the crystal rod R, and when the guide tube 10 is relative to the water When the flat magnetic field HM is in the position shown in FIG5 , in the direction of the horizontal magnetic field HM, or in the direction of the Y-axis shown in FIG1 and FIG2 , the protective gas PG cannot flow through the notch 10N of the bottom 10B of the guide tube 10, and can only flow through the gap between the portion of the bottom 10B of the guide tube 10 where the notch 10N is not formed and the liquid surface L of the melt M. Therefore, the flow rate will be relatively small. As mentioned above, the volatilization of oxygen in the melt M will be suppressed, resulting in more oxygen reaching the solid-liquid interface between the crystal rod R and the melt M, thereby increasing the oxygen concentration in the crystal rod R.

[0043] That is, the embodiment of the present application provides a guide tube 10 having a notch 10N at its bottom 10B, and the oxygen concentration in the pulled crystal ingot R can be controlled by rotating the guide tube 10 around its longitudinal axis 10X.

[0044] In an optional embodiment of the present application, referring to Figures 3 and 4 , the number of the notches 10N can be two, and they are radially opposed to each other in the guide tube 10. As previously mentioned, with respect to the volatilization of oxygen in the melt M, the area that can be affected by the flow rate of the protective gas PG flowing through the liquid surface L of the melt M exists throughout the entire radial direction. Therefore, the two radially opposed notches 10N can fully utilize such an area. For example, when it is desired to lower the oxygen concentration in the pulled crystal ingot R, compared to a guide tube 10 having only a single notch 10N, the two radially opposed notches 10N in the guide tube 10 can better promote the volatilization of oxygen from the melt M, thereby reducing the oxygen concentration.

[0045] A higher oxygen concentration may be required for the pulled ingot R. To this end, in an optional embodiment of the present application, referring to FIG5 , the guide tube 10 may be configured such that the connecting line between the two notches 10N is perpendicular to the horizontal magnetic field HM applied to the melt M. FIG5 is a cross-sectional view, so the notches 10N are not shown. However, it is understood that the connecting line between the two notches 10N of the guide tube 10 is perpendicular to the page showing FIG5 . In this case, the protective gas PG flowing through the liquid surface L of the melt M has a minimum flow rate in a direction parallel to the horizontal magnetic field HM, because the protective gas PG can only flow through the gap between the portion of the bottom 10B of the guide tube 10 without the notches 10N and the liquid surface L of the melt M, or in other words, can only flow through the gap between the portion of the bottom 10B of the guide tube 10 that is raised relative to the notches 10N and the liquid surface L of the melt M. This gap is the smallest along the entire circumference of the guide tube 10.

[0046] The pulled crystal rod R may need to have a low oxygen concentration. In addition, in addition to the requirement for the oxygen concentration of the entire crystal rod R, the oxygen concentration may also need to be uniform in the circumferential direction of the crystal rod R.

[0047] In this regard, in an optional embodiment of the present application, referring to Figure 4, the guide tube 10 can be configured so that the connecting line between the two recesses 10N is parallel to the horizontal magnetic field HM applied to the melt M, wherein Figure 4 is a cross-sectional schematic diagram after the guide tube 10 is rotated 90° around its own longitudinal axis 10X based on Figure 5, or in other words, Figure 5 is a cross-sectional schematic diagram after the guide tube 10 is rotated 90° around its own longitudinal axis 10X based on Figure 4, so in Figure 4, the connecting line between the two recesses 10N of the guide tube 10 is in the cross section.

[0048] In this case, for the protective gas PG flowing through the liquid surface L of the melt M, the flow rate is the largest in the direction parallel to the horizontal magnetic field HM, because the protective gas PG can flow through the recess 10N of the bottom 10B of the guide tube 10, or in other words, in the entire circumference of the guide tube 10, the gap between the portion of the bottom 10B where the recess 10N is formed and the liquid surface L of the melt M is the largest.

[0049] Regarding the uniformity of oxygen concentration around the circumference of the crystal ingot R, as previously described, the oxygen in the crystal ingot R primarily comes from oxygen that enters the melt M due to melting of the crucible 30A at high temperature. However, under the influence of the horizontal magnetic field HM, the temperature of the melt M is non-uniform around its circumference. Specifically, see FIG6 , which shows a schematic diagram of the temperature distribution of the melt M in a plane parallel to the liquid surface under the influence of the heater 40A shown in FIG1 . As can be seen from FIG6 , in a direction parallel to the horizontal magnetic field HM, the temperature of the melt M near the crucible 30A is higher, resulting in more melting of the crucible 30A and more oxygen entering the melt M. In a direction perpendicular to the horizontal magnetic field HM, the temperature of the melt M near the crucible 30A is lower, resulting in less melting of the crucible 30A and less oxygen entering the melt M. Without considering the convection caused by the horizontal magnetic field HM, as shown in FIG2 , or assuming that the probability of oxygen entering the melt M reaching the solid-liquid interface between the ingot R and the melt M is uniform, then, in the direction parallel to the horizontal magnetic field HM, more oxygen enters the melt M, and therefore more oxygen enters the ingot R, while in the direction perpendicular to the horizontal magnetic field HM, less oxygen enters the melt M, and therefore less oxygen enters the ingot R. This results in a non-uniform oxygen concentration in the circumferential direction of the ingot R, and more specifically, the oxygen concentration in the direction parallel to the horizontal magnetic field HM is greater than that in the direction perpendicular to the horizontal magnetic field HM. On the other hand, under the influence of convection as shown in FIG2 , as previously described, the oxygen in the melt M is difficult to volatilize in the direction parallel to the horizontal magnetic field HM, resulting in an increase in the oxygen concentration in the ingot R, while the oxygen in the melt M is easy to volatilize in the direction perpendicular to the horizontal magnetic field HM, which suppresses the increase in the oxygen concentration in the ingot R. In other words, the circumferential oxygen concentration nonuniformity of the crystal ingot R is further exacerbated or worsened. In this embodiment, as described above, the flow rate of the protective gas PG flowing through the liquid surface L of the melt M in a direction parallel to the horizontal magnetic field HM is maximized, thereby maximizing the volatilization of oxygen in the melt M. Minimum oxygen reaches the solid-liquid interface between the crystal ingot R and the melt M, minimizing the oxygen concentration in the crystal ingot R in a radial direction parallel to the horizontal magnetic field HM. Thus, the circumferential oxygen concentration nonuniformity of the crystal ingot R is minimized.

[0050] In an optional embodiment of the present application, as shown in FIG3 , the notch 10N may be rectangular. This simplifies the calculation process for the protective gas PG flowing through the liquid surface L of the melt M, for example, when it is necessary to accurately calculate the flow rate at different circumferential positions of the draft tube 10 .

[0051] In an optional embodiment of the present application, referring to Figure 7 , the recess 10N may gradually expand toward the bottom 10B of the guide tube 10. In this way, when the recess 10N is obtained by removing material, the guide tube 10 having the recess 10N can be more easily manufactured.

[0052] 8 , an embodiment of the present application further provides a crystal pulling furnace 1 used in the process of pulling a crystal rod R by the Czochralski method. The crystal pulling furnace 1 may include the guide tube 10 described in the above embodiments of the present application.

[0053] In an optional embodiment of the present application, the crystal pulling furnace 1 may further include:

[0054] A furnace body 20, wherein the furnace body 20 defines a furnace cavity 20C;

[0055] The crucible 30 is disposed in the furnace cavity 20C, and the melt M is contained in the crucible 30 .

[0056] In an optional embodiment of the present application, referring to FIG8 , the crystal pulling furnace 1 may further include a heater 40, which is disposed in the furnace body cavity 20C and on the periphery of the crucible 30 to heat the crucible 30, thereby melting the solid raw material contained in the crucible 30 into the melt M.

[0057] In an optional embodiment of the present application, referring to FIG. 8 , the crystal pulling furnace 1 may further include a heat preservation element 50 , which is disposed on the inner wall of the furnace body 20 to suppress the heat generated by the heater 40 from being dissipated through the furnace body 20 .

[0058] Unless otherwise defined, the technical or scientific terms used in this application should have the usual meanings understood by people with ordinary skills in the field to which the utility model belongs. The "first", "second" and similar words used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0059] It should be noted that the technical solutions described in the embodiments of this application can be combined arbitrarily without conflict.

[0060] The above description is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in this application should be included in the scope of protection of this application. Therefore, the scope of protection of this application should be based on the scope of protection of the claims.

Claims

1. A guide tube used in a process of pulling a crystal rod by a Czochralski method, wherein the bottom of the guide tube has a notch, and the notch is used to change the flow rate of a protective gas flowing through the liquid surface of a melt in a reference radial direction by rotating the guide tube around its own longitudinal axis.

2. The guide tube according to claim 1, in, The number of the recesses is two and the recesses are opposite to each other in the radial direction of the guide sleeve.

3. The guide tube according to claim 2, in, The guide sleeve is arranged so that a connecting line between two notches is parallel to a horizontal magnetic field applied to the melt.

4. The guide tube according to claim 2, in, The guide sleeve is arranged so that a connecting line between two of the notches is perpendicular to a horizontal magnetic field applied to the melt.

5. The guide tube according to any one of claims 1 to 4, in, The notch is rectangular.

6. The guide tube according to any one of claims 1 to 4, in, The notch gradually expands toward the bottom of the guide tube.

7. A crystal pulling furnace used in a process of pulling a crystal rod by the Czochralski method, the crystal pulling furnace comprising the guide tube according to any one of claims 1 to 6.

8. The crystal pulling furnace according to claim 7, in, The crystal pulling furnace also includes: A furnace body, wherein the furnace body defines a furnace body cavity; A crucible is disposed in the furnace cavity, and the melt is contained in the crucible.

9. The crystal pulling furnace according to claim 8, in, The crystal pulling furnace further includes a heater disposed in the furnace body cavity and at an outer periphery of the crucible to heat the crucible, thereby melting the solid raw material contained in the crucible into the melt.

10. The crystal pulling furnace according to claim 9, in, The crystal pulling furnace further includes a heat preservation element, which is disposed on an inner wall of the furnace body to suppress the heat generated by the heater from being dissipated through the furnace body.

Citation Information

Patent Citations

  • Semiconductor crystal growth device

    CN112095143A

  • Semiconductor crystal growth device

    CN112680788A

  • Semiconductor crystal growth device

    CN112680793A

  • Adjustable guide cylinder and semiconductor crystal growth device

    CN113337880A

  • Heater and working method thereof

    CN115044966A