Sea wave splash zone corrosion-resistant 460 mpa grade hot-rolled strip for building structure

Through the design and process optimization of low-carbon microalloy composition, hot-rolled strip steel with high yield strength and low yield strength ratio is formed, which solves the problem of insufficient corrosion resistance and mechanical properties of steel structures in the environment of wave splash zones, and realizes the High corrosion resistance and good mechanical properties in the sea wave splash zone.

WO2024244624A1PCT designated stage expired Publication Date: 2024-12-05BAOSHAN IRON & STEEL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082492
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-03-19
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The prior art is difficult to meet the corrosion resistance and mechanical properties requirements of steel for building structures in the environment of sea wave splash zones, especially in terms of low-temperature impact toughness and yield strength ratio.

Method used

Hot-rolled strip steel designed with low-carbon microalloy compositions is formed through smelting, casting, billet forming, heating and rolling processes, and a composite structure with industrial pure titanium corrosion-resistant layer and carbon steel base layer is formed to control the thickness of the interface transition layer. and refine the structure to achieve high yield strength and low yield strength ratio of the base layer, and ensure low temperature impact toughness through two-stage cooling.

Benefits of technology

Without reducing the corrosion resistance of the corrosion resistance layer, the mechanical properties of the base layer are improved, meeting the high corrosion resistance and good mechanical properties requirements of the wave splash zone, and are suitable for facilities such as harbor terminals and marine oil production platforms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082492_05122024_PF_FP_ABST
    Figure CN2024082492_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to a hot-rolled strip for a building structure and a manufacturing method therefor. The hot-rolled strip comprises a base layer, a corrosion resistant layer, and an interfacial transition layer located between the base layer and the corrosion resistant layer. The base layer comprises the following chemical elements in percentage by mass: C: 0.03-0.13%, Si: 0.15-0.35%, Mn: 1.00-1.50%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.10-0.65%, Ni: 0.2-1.0%, Cu : 0.10-0.25%, Al: 0.020-0.050%, Ti: 0.0090-0.0160%, Nb: 0.060-0.100%, N: 0.0005-0.0050%, and V: 0.08-0.25%, with the balance being Fe and other inevitable impurities. The corrosion resistant layer is made of commercially pure titanium. According to the hot-rolled strip for a building structure of the present disclosure, the base layer has a yield strength of ≥460 MPa, a tensile strength of ≥580 MPa, a yield-tensile ratio of ≤0.81, and -40°C impact energy of ≥190 J; the corrosion resistant layer has a sea wave splash corrosion resistance rate of ≤0.006 mm / year; and the interfacial transition layer has a thickness of ≤8 μm, and an interfacial shear strength of ≥268 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

460MPa grade hot-rolled steel strip for building structures resistant to sea wave splash zone corrosion and its manufacturing method Technical Field

[0001] The present disclosure relates to steel for building structures and a manufacturing method thereof, and in particular to a hot-rolled steel strip for building structures that is resistant to corrosion in a wave splash zone and a manufacturing method thereof. Background Art

[0002] The ocean is a harsh and complex corrosive environment. Seawater is a strong electrolyte solution containing high concentrations of chloride ions. Steel structures, the main structural components of marine engineering facilities, are highly susceptible to electrochemical reactions with the surrounding medium, leading to severe corrosion and significantly reducing the service life of these facilities. This is particularly true in the splash zone, the most demanding marine corrosion zone. Various facilities are subject to a range of external factors, including alternating wet and dry conditions, ocean spray, sunlight, corrosive components in the atmosphere, and oxygen, leading to particularly severe material corrosion.

[0003] Investigations show that the wave splash zone of steel piles in facilities such as harbor terminals and offshore oil platforms is subject to severe corrosion, typically 3 to 10 times the depth of the fully immersed seawater zone. Once severe localized corrosion damage occurs, the bearing capacity of the entire facility is significantly reduced, shortening its service life, impacting production safety, and even leading to premature decommissioning.

[0004] In the splash zone, due to its alternating dry and wet atmosphere and ample oxygen supply, the corrosion products produced offer no protective effect. Splashing seawater can directly strike metal surfaces, causing severe corrosion. Corrosion tests and surveys have shown that, under normal circumstances, the average corrosion rate of ordinary carbon steel and low-alloy steel in marine atmosphere is approximately 0.03 to 0.08 mm / year, while in the splash zone, it is 0.3 to 0.5 mm / year. In the splash zone, steel piles are susceptible to severe corrosion damage, significantly reducing the bearing capacity of the entire steel structure, impacting safe production, shortening its service life, and leading to premature scrapping.

[0005] Based on the aforementioned operating conditions, industrially pure titanium was selected as the corrosion-resistant layer. Titanium is highly chemically active and readily reacts with oxygen in air to form oxides. The oxides on the titanium metal surface are dense, stable, and possess a strong self-healing ability. This self-healing ability primarily refers to the ability of titanium oxide to rapidly form a new film after damage to a specific area on the titanium surface, preventing further contact with corrosive media.

[0006] For steel used in marine building structures, in addition to meeting the requirements of corrosion resistance, it must also have good mechanical properties. Among them, the yield ratio and low-temperature impact toughness are increasingly becoming the key indicators of construction steel. The yield ratio is the ratio of the yield strength of steel to the tensile strength. Its size reflects the ability of steel to not produce strain concentration during plastic deformation. The lower the yield ratio, the more evenly the plastic deformation of the steel can be distributed over a wider range. Under the action of seismic forces, the plastic deformation of steel structure systems made of steel with low yield ratio can be evenly distributed over a wider range; while materials with high yield ratio may experience strain concentration, reducing the overall plastic deformation ability of the steel, resulting in brittle failure of the structure, causing structural instability and sudden collapse.

[0007] Steel undergoes a brittle transition at low temperatures, shifting its fracture pattern from ductile to brittle. This engineering significance lies in the fact that components will not experience brittle fracture when exposed to temperatures above this threshold. Therefore, structural steel typically requires specific low-temperature impact resistance based on the material's service environment. Ocean temperatures vary significantly at different latitudes. For example, near China's Bohai Bay, winter seaside temperatures can reach below -20°C, requiring building materials to possess excellent impact resistance at -40°C to prevent brittle fracture.

[0008] However, when the plastic toughness of steel is improved, if the increase in tensile strength is small, the yield ratio will increase significantly, making it difficult to control the low yield ratio.

[0009] Chinese patent application CN 201210260231.7 discloses a method for preparing a titanium-steel-titanium double-sided composite plate. The method comprises stacking four titanium plates and three steel plates in a certain order in a closed frame welded with two outermost steel plates, adding an isolation agent made of a mixture of 1 part by weight of active α-Al2O3 and 1.5 parts by weight of a 4% polyvinyl alcohol aqueous solution between the titanium plates, and using a nickel-based alloy as a transition layer between the titanium plates. The plate is heated to 500°C to 630°C and vacuumed, kept warm for 1 to 2 hours, and the vacuum degree reaches 20 to 200 Pa. The method is characterized in that welding is first performed after assembly, and then vacuuming is performed. Only ordinary welding is required during welding. Conventional arc welding and submerged arc welding can meet the conditions. Compared with welding under vacuum conditions, the welding conditions are less demanding, the cost is low, and there is no need to set up a separate vacuum chamber. The combined billets are then rolled and composited in a conventional heating furnace at a rolling temperature of 700°C to 900°C. The C in the coal gas can be blocked by sealing the outermost steel plate and vacuuming. At the same time, a nickel-based alloy isolation layer is added to prevent the formation of TiC at the interface, resulting in a titanium-steel composite plate with a shear strength of 230 to 260 MPa and an interface bonding rate of 99.6% to 100%.

[0010] Chinese patent application CN201710769999.X discloses a method for preparing a titanium-steel composite plate, which comprises selecting the surfaces of titanium-steel composite billets in contact with each other, applying a high-temperature resistant anti-carburizing and anti-nitriding isolation coating on the contacting titanium surfaces, and drying them at room temperature; after the drying process, the titanium billets are aligned and stacked in pairs, and a steel billet is placed in the middle to complete the assembly to obtain a composite billet, wherein the thickness of the titanium plate used is greater than 2 mm, and the thickness of the steel plate is greater than 5 mm, and then the composite billet is sealed and welded around and a certain size of unwelded area is left, and the billet is vacuumed to 10 -2 ~10 -3 Pa and then welded; the slab is heated to 500-700°C and rolled, with a first-pass reduction exceeding 25%, a final-pass reduction not exceeding 15%, a total reduction of 60-70%, and a rolling speed of 0.1-1.0 mm / s. This patent application utilizes a high-temperature impermeability protection coating to protect against the diffusion and oxidation of other impurity elements at high temperatures, blocking the diffusion of elements such as C and N. The embodiment utilizes a combination of Q235 and TA1, producing steel plates with shear strengths of 176 MPa, 181 MPa, and 182 MPa, respectively.

[0011] The above two patent applications mainly avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy isolation layer between titanium and carbon steel.

[0012] Chinese patent application CN201811327623.4 discloses a titanium-steel-titanium composite plate and its preparation method, which is a process of fixing a carbon steel between two titanium plates of the same size, and performing warm composite rolling through an irreversible large rolling force warm rolling mill to composite the three layers of strips into one. After rolling, the rolled composite plate is subjected to heat treatment, including an initial annealing at 500-600°C for 20-60 minutes and a recrystallization annealing at 680-700°C for 30-120 minutes. Finally, the product is obtained by straightening, flattening, shearing and shaping. This patent application mainly describes a method for preparing a non-hot-rolled composite titanium steel plate. However, due to the use of an irreversible rolling mill, only single-pass rolling production can be carried out, and heat treatment is also required. The embodiment mainly involves the steel strip production method, and the performance after composite is not mentioned.

[0013] Chinese patent application CN201510543767.3 discloses a method for preparing a titanium-steel composite plate. The titanium-steel composite plate obtained by this method has high bonding strength. The patent application fixes a titanium plate between two ordinary carbon steel plates or billets, welds the billets around the edges in a vacuum environment, heats the combined billets to 850-900°C for 120-360 minutes, controls the start rolling temperature to above 800°C and the final rolling temperature to below 700°C, and controls the single-pass deformation to be between 20-30%, with the total rolling deformation ≥90%. A large reduction is performed to break up the brittle phase compounds generated at the interface and reduce their impact on the bonding surface, thereby rolling to obtain a titanium-steel composite plate with a bonding strength greater than 240 MPa. However, the pass reduction rate and total deformation required by the patent application are both very high, which can easily cause edge weld cracking during the rolling process, destroying the vacuum degree and making it unsuitable for interface bonding.

[0014] Chinese patent application CN201610994234.1 discloses a method for producing titanium-steel composite plates, which involves an annealing technology production method for titanium-steel plates. First, the titanium plate and the steel plate are assembled to form a symmetrical multi-layer composite billet of steel plate-titanium plate-isolator-titanium plate-steel plate, which is then compounded by rolling compounding or explosive compounding. The compounded billet is annealed and pickled in a continuous annealing and pickling line, first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. The purpose of this patent application is to simultaneously obtain the properties of the composite material and the substrate through a two-stage heat treatment. However, the two-stage heat treatment will lead to excessive diffusion of titanium, iron, and carbon elements, resulting in brittle substances such as iron-titanium intermetallic compounds and titanium carbide, which deteriorate the interface shear strength.

[0015] Chinese patent application CN201710996925.X discloses a thin-layer double-sided titanium-steel composite plate and its preparation method. Through large-thickness billet assembly and large-reduction rolling technology, a good composite between titanium and steel is achieved. This patent application is a double-sided titanium composite plate composed of a titanium composite layer, a base layer and a titanium composite layer. The titanium composite layer is made of TA2, and the thickness of the titanium composite layer is 0.2 to 1 mm. The billets are stacked in the order of cover plate, titanium composite material, carbon steel substrate, titanium composite material, and cover plate from top to bottom. After vacuum is drawn in a vacuum chamber, the gaps around them are vacuum electron beam sealed and welded. The vacuum degree is 1.0×10 -2 ~4.5×10 -2Pa. The composite billet after the sealing welding process is heated to 900-920℃ and kept warm. The holding time is calculated according to 1min / mm×total thickness of the composite billet. The starting rolling temperature is 880-900℃, the final rolling temperature is above 800℃, and it is air-cooled to room temperature. The single-pass reduction rate is ≥15%, and the first three-pass reduction rate is ≥20%, and the total reduction rate is ≥80%. The composite plate obtained after rolling is trimmed, split, and surface-grinded to obtain a double-sided titanium-steel composite plate. This patent application uses surface cleaning treatment of the composite slab, the air isolation effect of the cover plate, the control of the rolling temperature, and the use of large reduction to break and refine the titanium iron and titanium carbon compounds generated at the composite interface, disperse them at the composite interface, improve the distribution state of the compounds, further ensure the composite quality and performance stability, and achieve a shear strength of 241MPa.

[0016] Chinese patent application CN201710983322.6 discloses a thin-layer titanium-steel composite plate and its preparation method, which adopts a double-layer structure of titanium and carbon steel. Its assembly method and heating process are similar to those of Chinese patent application CN201710996925.X. The starting rolling temperature is 880-900℃, the single-pass reduction rate is 25-30%, and the total reduction rate is ≥85%. While controlling the single-pass reduction rate and the total reduction rate, the thickness of the titanium-steel composite plate is limited to 3-16mm, the final rolling temperature is above 800℃, and it is air-cooled to room temperature. The titanium-steel composite plate is obtained by surface treatment, and the titanium composite layer thickness is ≤1mm. This patent application improves the composite quality by symmetrical assembly and welding titanium seals into carbon steel plates. After rolling, the shear strength of the steel plate reaches more than 238MPa, and the composite interface bonding rate is 100%. Its carbon steel layer meets the national standard requirements for Q345 grade carbon steel.

[0017] However, the above two patent applications did not mention the detailed design of the composite layer and the base layer, and only described the tensile properties and shear strength. The required pass reduction rate and total reduction rate of the composite layer were both relatively high, and there was no control over the corrosion resistance of the material, the low-temperature impact performance of the base material, the yield strength ratio and other performance indicators, which did not meet the requirements for steel used in building structures.

[0018] In summary, the above patent applications mainly describe the preparation method of composite steel plates, and the specific embodiments briefly describe the interface shear strength and tensile properties in terms of performance. In addition to being resistant to corrosion in the wave splash zone, steel used for steel structures in the wave splash zone must also ensure that they meet the necessary structural steel performance requirements, as well as the aforementioned low yield ratio and corresponding low-temperature impact performance to ensure structural safety. However, the above patent applications do not carry out relevant component and process design for the corrosion rate, yield ratio, low-temperature impact, etc. of the corrosion-resistant layer, and cannot guarantee that the use requirements of high-corrosion-resistant steel plates for steel structures in the wave splash zone environment can be met.

[0019] Summary of the Invention

[0020] In view of the above-mentioned shortcomings of the prior art, the present invention aims to provide a hot-rolled steel strip for building steel structures and a method for manufacturing the same. The hot-rolled steel strip for building steel structures disclosed herein can ensure that the mechanical properties of the base layer (carbon steel) meet the corresponding strength level requirements without compromising the corrosion resistance of the corrosion-resistant layer itself, and the base layer also has excellent yield strength ratio and low-temperature impact toughness.

[0021] Therefore, in one aspect, the present disclosure provides a hot-rolled steel strip for building structures, wherein the hot-rolled steel strip comprises a base layer, a corrosion-resistant layer, and an interface transition layer between the base layer and the corrosion-resistant layer;

[0022] In addition to Fe and other inevitable impurities, the base layer also contains the following chemical elements in the following mass percentages: C: 0.03-0.13%, Si: 0.15-0.35%, Mn: 1.00-1.50%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.10-0.65%, Ni: 0.2-1.0%, Cu: 0.10-0.25%, Al: 0.020-0.050%, Ti: 0.0090-0.0160%, Nb: 0.060-0.100%, N: 0.0005-0.0050%, and V: 0.08-0.25%;

[0023] The corrosion-resistant layer is made of industrial pure titanium, preferably TA1, TA2, TA3 or TA4.

[0024] Preferably, the chemical composition of the base layer also satisfies the following relationship:

[0025] 0.32%≤Cu+Ni≤1.15%;

[0026] 2(C+N)≤Ti+Nb+Cr+V≤0.90%.

[0027] Preferably, the mass percentage of each chemical element in the base layer is: C: 0.03-0.13%, Si: 0.15-0.35%, Mn: 1.00-1.50%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.10-0.65%, Ni: 0.2-1.0%, Cu: 0.10-0.25%, Al: 0.020-0.050%, Ti: 0.0090-0.0160%, Nb: 0.060-0.100%, N: 0.0005-0.0050%, V: 0.08-0.25%, and the remainder is Fe and other inevitable impurities.

[0028] Preferably, the microstructure of the base layer is ferrite + bainite + martensite, the content of bainite + martensite is 5% to 15%, and the average grain size of ferrite is ≥8.5.

[0029] Preferably, the yield strength of the base layer is ≥460 MPa, the tensile strength is ≥580 MPa, the yield strength ratio is ≤0.81, preferably the yield strength ratio is ≤0.75, and the impact energy at -40°C is ≥190 J.

[0030] Preferably, the microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.

[0031] Preferably, the wave splash corrosion resistance rate of the corrosion-resistant layer is ≤0.006 mm / year.

[0032] Preferably, the thickness of the interface transition layer is ≤8 μm, the average grain size is 15-40 μm, and it contains precipitated (Ti, Nb)C particles with a diameter less than 120 nm, and the interface shear strength is ≥268 MPa.

[0033] The interface transition layer of the hot-rolled steel strip disclosed herein has 100% metallurgical bonding, highly coherent atoms, and fine grains in the interface transition layer (average grain size is 15-40 μm).

[0034] Preferably, the thickness of the hot-rolled steel strip for building structures is 1 to 16 mm. The hot-rolled steel strip for building structures disclosed herein has a base yield strength of ≥460 MPa, a tensile strength of ≥580 MPa, a yield strength ratio of ≤0.81 (preferably ≤0.75), an impact energy of ≥190 J at -40°C, a corrosion rate of the corrosion-resistant layer against seawater splashing of ≤0.006 mm / year, an interface transition layer thickness of ≤8 μm, and an interface shear strength of ≥268 MPa. The hot-rolled steel strip disclosed herein can meet the corrosion resistance requirements for use in seawater splash zones, possessing both good mechanical properties for seawater splash zone corrosion resistance and high economic efficiency, and is suitable for use in steel structures such as steel piles for facilities such as seaport terminals and offshore oil platforms.

[0035] The present invention adopts a low-carbon microalloying composition design to achieve an excellent combination of titanium and carbon steel without adding a metal isolation layer, and effectively controls the thickness of the interface transition layer, so that the mechanical properties of the base layer (carbon steel) can meet the corresponding strength level requirements without reducing the corrosion resistance of the corrosion-resistant layer itself.

[0036] In another aspect, the present disclosure provides a method for manufacturing the above-mentioned hot-rolled steel strip for building structures, comprising the following steps performed in sequence:

[0037] 1) Smelting and casting

[0038] According to the above compositions of the base layer and the corrosion-resistant layer, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively;

[0039] 2) Assembly

[0040] The base blank and the corrosion-resistant layer blank are ground and polished, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are vacuumed;

[0041] 3) heating and rolling the composite billet to form a steel strip, wherein

[0042] The composite blank is heated to 900-1000° C.;

[0043] Rough rolling temperature ≥ 860°C; finishing rolling temperature is 760-850°C, preferably 780-850°C; pass reduction rate is 5-20%, preferably 10-15%; cumulative reduction rate ≥ 88%;

[0044] 4) Cooling

[0045] The steel strip is cooled to 300-450°C and then coiled at this temperature to produce hot-rolled strip steel.

[0046] Preferably, in step 2), the thickness of the corrosion-resistant layer is 1 to 10% of the thickness of the composite blank.

[0047] Preferably, in step 3), the thickness of the interface transition layer formed between the base layer and the corrosion-resistant layer is ≤8 μm. Preferably, in step 4), the cooling comprises two stages, wherein in the first stage, the steel strip is cooled to 700-750°C at a cooling rate of 2-10°C / s after exiting the rolling mill stand; in the second stage, the steel strip is cooled to 300-450°C at a cooling rate of 30-50°C / s.

[0048] Through the preparation method disclosed in the present invention, especially the control of the heating, rolling and cooling processes, the base layer in the strip steel exhibits a low yield ratio and good low-temperature impact toughness, while the corrosion-resistant layer has excellent corrosion resistance and high bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] FIG1 is a schematic diagram of the interlayer structure of a hot-rolled steel strip for building structures according to one embodiment of the present disclosure.

[0050] FIG2 is a schematic diagram of the interlayer structure of a hot-rolled steel strip for building structures according to another embodiment of the present disclosure.

[0051] FIG3 is a microstructure photograph of the corrosion-resistant layer of Example 3.

[0052] FIG4 is a scanning image of the interface transition layer between the base layer and the corrosion-resistant layer of Example 3. FIG.

[0053] FIG5 is a microstructure photograph of the base layer of Example 3. DETAILED DESCRIPTION

[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. The terms used in the description of the present disclosure are for the purpose of describing particular embodiments only and are not intended to limit the present disclosure.

[0055] In this article, “the content of bainite + martensite” refers to the area ratio of the “bainite + martensite” structure in the photo observed by metallographic observation.

[0056] In this article, "industrially pure titanium" refers to dense metallic titanium with a titanium content of not less than 99% and a small amount of impurities such as iron, carbon, oxygen, nitrogen and hydrogen. "TA1, TA2, TA3, TA4" represent the grades of industrially pure titanium. This grading standard is based on GB / T3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Composition", and grades pure titanium according to purity (i.e. impurity content).

[0057] In this article, "yield strength ratio" refers to the ratio of the yield strength of steel to its tensile strength. Its size reflects the ability of steel to avoid strain concentration during plastic deformation.

[0058] In this paper, the yield strength and tensile strength are measured with reference to GB / T 6396-2008 “Mechanical and process properties of composite steel plates” and GB / T 228-2010 “Methods of tensile test at room temperature for metallic materials”.

[0059] In this article, the -40℃ impact energy KV2 / J (longitudinal) is measured with reference to GB / T 6396-2008 "Mechanical and process properties of composite steel plates" and GB / T 229-2020 "Charpy pendulum impact test method for metallic materials".

[0060] In this paper, grain size rating is performed as follows: According to GB / T 6394-2017 “Method for determination of average grain size of metals”, the intercept method is used to grade the grain size of ferrite in stainless steel and carbon steel respectively.

[0061] In this paper, the wave splash corrosion rate is measured as follows: the composite steel plate coupons are placed in the wave splash zone of the South China Sea for 6 months and then the corrosion conditions are observed and recorded. First, the coupons are cleaned and weighed, and the loss volume is obtained by dividing the loss weight by the density. Then, the loss volume is divided by the exposed area of ​​the coupon to obtain the loss thickness.

[0062] In this paper, the interface shear strength was measured with reference to GB / T 6396-2008 “Mechanical and process properties of composite steel plates”.

[0063] In this paper, the metals of the base layer and corrosion-resistant layer undergo recrystallization and grain growth under high temperature and high pressure. During this process, some grains pass through the interface. At the same time, due to the difference in element content on both sides of the interface, the metal elements diffuse from areas of high concentration to areas of low concentration at high temperatures. These two factors work together to form the interface transition layer. In the base layer composition design of the hot-rolled strip steel for building steel structures disclosed in this disclosure:

[0064] C: It plays a role of solid solution strengthening in steel and can significantly improve the strength of steel. However, too high a C content is detrimental to welding performance and toughness. More importantly, when the C content is too high, C will diffuse to the composite interface, forming a large number of large-granular TiC hard phases in the interface transition layer, reducing the composite interface strength. Therefore, in order to ensure the shear strength of the interface, a low C content must be adopted. The change in C content has less effect on the yield strength of steel than on the tensile strength. Therefore, under the premise of ensuring the formability and welding performance of the product, appropriately increasing the C content is beneficial to reducing the yield strength ratio of steel. Based on this, in the base component disclosed in the present invention, the C content is controlled at 0.03~0.13%.

[0065] Si: Adding Si to steel effectively deoxidizes and improves its purity. Furthermore, Si acts as a solid solution strengthener in steel, increasing its strength and hardness. However, excessive Si content can negatively impact the material's weldability. Therefore, in the base composition disclosed herein, the Si content is controlled to 0.15-0.35%.

[0066] Mn: Mn is the cheapest matrix-strengthening element. It can lower the austenite transformation temperature, delay pearlite transformation, refine ferrite grains, and increase steel strength. Mn also counteracts the effects of sulfur on steel. However, excessive Mn content can easily lead to segregation bands and martensitic structures, which negatively impact the toughness of the steel. Therefore, in the base composition disclosed herein, the Mn content is controlled within a range of 1.00% to 1.50%.

[0067] Al: Al is mainly added to the steel in excess as a de-O element to ensure that the O content in the steel is as low as possible. After de-O, the excess Al combines with the N element in the steel to form AlN precipitates. During the heating process, AlN hinders the growth of austenite grains, refines the austenite grains, and improves the strength and toughness of the matrix. At the same time, the formation of AlN fixes part of the N in the matrix, reduces the diffusion of interstitial atomic N in the carbon steel base layer to the composite interface, and forms hard TiN in the interface transition layer (which deteriorates the interface shear strength of the composite plate); at the same time, the amount of Ti and Nb added can be reduced, reducing the total cost. Based on this, in the base layer components disclosed in the present invention, the Al content is controlled at 0.020-0.050%, preferably 0.020-0.030%.

[0068] Ti: Ti forms stable TiN or Ti(N, C) at high temperatures, which plays a role in fixing C and N, preventing the interstitial C and N atoms in the carbon steel base from diffusing to the interface, and forming hard TiN or Ti(N, C) precipitation in the interface transition layer to obtain a composite plate with high interface shear strength. At the same time, TiN hinders the growth of austenite during the heating process, can refine the austenite grains, and can improve the strength and toughness of the matrix. In subsequent welding, TiN inhibits the growth of austenite grains, especially in the heat-affected zone (HAZ) close to the molten boundary of the weld, thereby improving the toughness of the welding HAZ, thereby being able to adapt to the needs of large welding heat input processes. Reducing the diffusion of C and N to the interface can increase the strength of the low-carbon matrix and obtain a composite plate with high interface shear strength. Based on this, in the base composition disclosed in the present invention, the Ti content is controlled at 0.0090~0.0160%.

[0069] Nb: Nb exists in the steel in the form of solid solution Nb and Nb(C, N), and plays the role of solid solution drag and precipitation pinning during the recrystallization process. The main purpose of adding a small amount of Nb to the base carbon steel is to increase the recrystallization temperature, so that the base carbon steel can be grain refined after rolling in the recrystallization and non-recrystallization zones, which is beneficial to improving the low-temperature impact toughness of the base carbon steel. Due to the action of the Nb(C, N) precipitation phase, the original austenite grains will be finer, thereby promoting the formation of finer recrystallized grains and obtaining an ideal combination of high strength and high toughness. At the same time, Nb can fix the interstitial C and N atoms in the matrix, reduce the diffusion of C and N to the interface, and obtain a composite plate with high interface shear strength. Based on this, in the base layer disclosed in the present invention, the Nb content is controlled at 0.060~0.100%.

[0070] Cu: Cu plays a role in solid solution strengthening, and as the Cu content increases, the room temperature impact toughness of the steel slightly increases. Therefore, in the base composition of the present disclosure, the Cu content is controlled to be 0.10-0.25%.

[0071] N: Elemental N can react with Ti and Al to form second-phase particles, refining austenite grains and improving matrix strength and toughness. However, excessive N content can produce excessive amounts of TiN and overly coarse particles, which can affect the plasticity and toughness of carbon steel. Therefore, in the base layer of this disclosure, the N content is controlled to 0.0005% to 0.0050%.

[0072] Nickel: Nickel stabilizes austenite and contributes to improved toughness and strength. Adding nickel to steel significantly improves its low-temperature impact toughness. However, nickel is expensive, and adding too much increases the cost of the composite plate. Therefore, an appropriate amount of nickel is added to the base layer of the present invention, with the nickel content controlled to 0.2-1.0%.

[0073] Cr: Cr is a strong carbide-forming element with a slow diffusion rate in austenite, while hindering the diffusion of C. During low-temperature processes, Cr forms fine carbides with C, which play a role in precipitation strengthening. At the same time, Cr can fix the interstitial C and N atoms in the matrix, reducing the diffusion of C and N to the interface, and obtaining a composite plate with high interfacial shear strength. However, while Cr increases the matrix strength in steel, it also reduces toughness. Therefore, in order to achieve the best match between strength and toughness, the Cr content in the base component of the present disclosure is controlled to 0.10-0.65%.

[0074] V: V is a strong carbonitride-forming element. When added to steel in combination with Ti and Nb, it can form fine composite carbonitrides, and the precipitation temperature range is widened, which can effectively prevent the growth of austenite grains, inhibit the recrystallization process, and improve the strength and toughness of the base carbon steel. At the same time, the precipitation temperature of V carbonitride is relatively low, and precipitation during the phase transformation process can effectively prevent the growth of ferrite grains and strengthen the ferrite matrix strength. Based on this, an appropriate amount of V is added to the base component of the present disclosure, and the V content is controlled to 0.08-0.25%.

[0075] In the hot-rolled steel strip for building structures disclosed herein, S and P are both unavoidable impurity elements, and the lower their content, the better. However, considering the actual steelmaking level of the steel mill, the S and P contents in the base composition disclosed herein are controlled to be: S ≤ 0.010%; P ≤ 0.003%;

[0076] In addition, in the base chemical composition design of the hot-rolled steel strip for building steel structure disclosed in the present invention:

[0077] Both Cu and Ni can improve the toughness of the base layer, and the combined addition effect is particularly significant. Furthermore, the addition of Ni can reduce the diffusion rate of carbon in steel, reducing its diffusion to the interface. Therefore, to achieve better performance, the base layer composition of the present disclosure preferably satisfies the following requirements: 0.32% ≤ Cu + Ni ≤ 1.15%. This helps to control the interface transition layer to within 8 μm.

[0078] Ti, Nb, Cr and V are all strong carbonitride-forming elements, which can form corresponding carbonitrides in the base carbon steel. This can fix the interstitial atoms in the base, hinder the diffusion of C and N interstitial atoms to the interface, and form large-grained, aggregated carbonitrides in the interface transition layer, which helps to control the interface transition layer within 8μm, thereby improving the interface shear strength. At the same time, Ti, Nb and Cr can play a role in refining the base carbon steel grains and improving toughness at different stages of hot rolling. Therefore, in order to obtain better performance, in the base composition disclosed in the present invention, it is preferred that the contents of Ti, Nb, Cr and V further satisfy the following requirements: 2(C+N)≤Ti+Nb+Cr+V≤0.90%.

[0079] The corrosion-resistant layer disclosed herein uses industrial pure titanium, preferably TA1, TA2, TA3 and TA4, whose composition meets the standard of GB / T3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Composition".

[0080] The method for manufacturing hot-rolled steel strip for building structures disclosed herein comprises the following steps:

[0081] 1) Smelting and casting

[0082] According to the compositions of the base layer and the corrosion-resistant layer, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively;

[0083] 2) Assembly

[0084] The base blank and the corrosion-resistant layer blank are ground and polished, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are vacuumed;

[0085] 3) heating and rolling the composite billet to form a steel strip, wherein

[0086] The composite blank is heated to 900-1000° C.;

[0087] The rough rolling temperature is above 860℃, the finishing rolling temperature is 760~850℃, the pass reduction rate is 5~20%, and the cumulative reduction rate is ≥88%;

[0088] 4) Cooling: The steel strip is cooled to 300-450°C and coiled at this temperature to produce hot-rolled strip steel.

[0089] Preferably, in step 4), the cooling comprises two-stage cooling, wherein in the first stage, the steel strip is cooled to 700-750°C at a cooling rate of 2-10°C / s after leaving the rolling mill stand, and then in the second stage, it is cooled to 300-450°C at a cooling rate of 30-50°C / s.

[0090] Preferably, in step 2), the thickness of the corrosion-resistant layer is 1 to 10% of the total thickness of the composite blank.

[0091] Preferably, in step 3), the reduction ratio during rolling is 10-15%.

[0092] In the manufacturing method of the present disclosure:

[0093] 1) Metallurgy: P and S elements degrade the fracture toughness of steel, so low P and S levels are crucial during the smelting process to improve billet quality. Ideally, clean steel production technology should be employed to reduce the gas and inclusion content in the steel, thereby improving the overall performance of the steel, particularly its lamellar tearing resistance.

[0094] 2) Assembly: Preferably, the thickness of the corrosion-resistant layer is 1-10% of the total thickness of the composite billet. The corrosion-resistant layer and base carbon steel billet are pre-treated, and the billet bonding surfaces are welded and sealed on all sides. The sealed bonding surfaces are then vacuumed. The vacuum treatment protects the corrosion-resistant layer from oxidation and is an important factor in ensuring the corrosion-resistant layer's resistance to seawater splash zone corrosion. It also prevents edge cracking and corrosion-resistant layer breakage during subsequent deformation at high cumulative reduction rates.

[0095] 3) Heating: For single carbon steel, the slab heating temperature is generally controlled between 1000°C and 1250°C. This facilitates the dissolution and full diffusion of precipitates in the steel, promotes element homogenization in the slab, and maximizes the strengthening effect of microalloying elements in the steel. For single commercially pure titanium plates, the heating temperature is generally controlled between 850°C and 1000°C. Excessively high heating temperatures can produce a β phase transformation, which can rapidly grow and degrade the properties of commercially pure titanium. High heating temperatures allow for full element diffusion, promoting subsequent 100% metallurgical bonding at the interface. However, excessively high heating temperatures increase the tendency for austenite grains to coarsen, making subsequent controlled rolling more difficult. More importantly, they accelerate the diffusion of C, N, Ti, and Fe into the interface, forming thick brittle precipitates and intermetallic compounds at the interface, resulting in a thick interfacial transition layer and degrading interfacial shear strength. Taking these factors into consideration, the method disclosed herein utilizes a lower heating temperature than conventional carbon steel production, controlling the heating temperature between 900°C and 1000°C.

[0096] 4) Rolling: The rough rolling temperature is controlled at above 860°C. A high reduction rate is applied in the high-temperature rough rolling zone to fully recrystallize the structure, refine the grains, and improve the material's strength and toughness. Controlled rolling is performed in the non-recrystallized zone of the finishing rolling process, and no austenite recrystallization occurs at this stage. Reasonable reduction rates and finishing temperatures are used to accumulate deformation energy and deformation dislocations, forming high-density deformation bands within the austenite grains. This increases the number of ferrite phase deformation nuclei, further refines the matrix's post-phase transformation grain size, and improves the material's strength and toughness. Simultaneously, deformation induces the precipitation of carbonitrides of Nb, Ti, Cr, and V at this stage, increasing the strength of the matrix and inhibiting the diffusion of C to the interface, thus preventing the formation of excessively thick TiC at the interface that degrades the interfacial shear strength. The pass reduction is controlled between 5% and 20%, with a cumulative reduction of ≥88%. Preferably, the finishing rolling temperature is controlled between 780°C and 850°C. This ensures the corrosion resistance of titanium while preventing the base layer from rolling in the two-phase region. This results in a base layer with a microstructure of ferrite, bainite, and martensite, with an average ferrite grain size of ≥8.5 and a bainite + martensite content of 5% to 15%. During the rolling process, the corrosion-resistant layer and the base layer undergo only metallurgical bonding and necessary dimensional changes, without any compositional changes between the corrosion-resistant layer and the base layer.

[0097] 5) Cooling: By controlling the initial cooling, final cooling and cooling rate, the post-rolling microstructure type, microstructure size and various contents can be controlled. Too fast a cooling rate will form a large amount of bainite and martensite microstructures, among which the martensite phase is a low-toughness and high-yield ratio microstructure, which is detrimental to the performance of the steel plate; too slow a cooling rate will lead to the generation of a large amount of coarse ferrite microstructures, among which the coarse ferrite microstructures are beneficial to the expansion of cracks, resulting in a decrease in impact performance. Therefore, the cooling rate should be reasonably controlled. Controlling the final rolling temperature of finishing rolling can avoid the occurrence of abnormally coarse microstructures caused by rolling in the two-phase region; at the same time, after rolling, it can be quickly cooled to the phase transformation temperature, further inhibiting the growth of the microstructure, improving the material strength and low-temperature impact toughness by refining the grains, and forming more than 5% of hard phase microstructure to ensure strength. Preferably, a staged cooling method is adopted. After the steel strip leaves the rolling mill stand, it is first cooled to the ferrite phase transformation temperature at a cooling rate of ≤10°C / s, and then rapidly cooled to 350-450°C at a cooling rate of 30-50°C / s, and then coiled, thereby obtaining a small amount of bainite and martensite structure, and achieving structure recovery during the coiling process, and promoting the precipitation of V carbonitride, ensuring that the base layer has a low yield ratio and high low-temperature impact toughness.

[0098] If the corrosion-resistant layer is too thick, it will affect the mechanical properties of the material and the production cost. If the corrosion-resistant layer is too thin, it will reduce the corrosion resistance and service life of the material. Preferably, the thickness of the corrosion-resistant layer is controlled to be 1-10% of the total thickness of the composite blank during the blank assembly process.

[0099] By combining the corrosion-resistant layer with the base layer, combining the design of their composition and thickness ratio, and rolling the base layer, a corrosion-resistant layer resistant to splash zone corrosion is formed on the surface of the carbon steel strip. The result is the disclosed hot-rolled steel strip for building structures that combines splash zone corrosion resistance with excellent mechanical properties and high economic efficiency. This steel strip can then be processed into structural components for use in splash zone environments.

[0100] Compared with the prior art, the hot-rolled steel strip for building structures disclosed in the present invention has the following beneficial effects:

[0101] The hot-rolled steel strip for building structures disclosed herein is designed with a low-carbon microalloying composition, achieving an excellent combination of titanium and carbon steel without adding a metal isolation layer, and effectively controlling the thickness of the interface transition layer, so that the mechanical properties of the base layer (carbon steel) can meet the corresponding strength level requirements without reducing the corrosion resistance of the corrosion-resistant layer itself.

[0102] The hot-rolled steel strip for building structures disclosed herein reduces the carbon content to minimize the formation of TiC compounds in the interface transition layer and carbonitrides in the base layer, hindering grain growth and improving the base layer's low-temperature impact toughness. Furthermore, the addition of microalloying elements and a rational rolling and cooling process address the issue of low material strength in low-carbon conditions, achieving a base layer yield strength of 460 MPa or higher and a tensile strength of 580 MPa or higher. Furthermore, it maintains a yield strength ratio of 0.81 or lower and an impact energy of 190 J or higher at -40°C, both exceeding the performance requirements of the Chinese national standard GB / T 19879-2015, "Steel Plate for Building Structures."

[0103] Chinese patent application CN201210260231.7 adds a nickel plate as an isolation layer between the cladding layer and the base layer to prevent the formation of TiC at the interface, resulting in a titanium-steel composite plate with an interface bonding ratio of 99.6-100%. In contrast, the hot-rolled steel strip for building structures disclosed herein utilizes a low-carbon and microalloyed design, reducing nickel addition and production costs. Furthermore, through optimized heating and rolling processes, it forms a transition layer with a defined thickness and reduces the formation of brittle TiC in the interface transition layer, achieving a complete metallurgical bond with a 100% interface bonding ratio.

[0104] Chinese patent application CN201710769999.X uses a slab heating temperature of 500-700°C and a total reduction rate of 60-70%. The resulting strip has a maximum interfacial shear strength of 182 MPa. In contrast, the inventors fully considered the impact of the high-temperature phase transformation of the industrial pure titanium in the corrosion-resistant layer on corrosion resistance and the strength and toughness control of the base carbon steel. Incorporating low-carbon microalloy design and through comprehensive processing technology design, they set the heating temperature of the composite billet to 900-1000°C. At this temperature, the corrosion-resistant layer does not undergo phase transformation, ensuring that the precipitates in the base carbon steel are fully dissolved, refining the base grains during controlled rolling and improving the strength and toughness of the base. At the same time, the cumulative reduction rate is controlled to ≥85%, which breaks up the brittle phases in the interface transition layer and improves the interfacial shear strength.

[0105] Chinese patent applications CN201210260231.7 and CN201710769999.X primarily avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy barrier layer between titanium and carbon steel. In contrast, the present invention achieves a complete metallurgical bond with a 100% interfacial bonding ratio through composition and process design without adding a barrier layer. Furthermore, the hot-rolled steel strip for building structures disclosed in the present invention differs from the above two patent applications in its assembly method and the base carbon steel material is also significantly different.

[0106] Through the process conditions disclosed in the present invention, the original corrosion resistance of the industrial pure titanium of the corrosion-resistant layer can be guaranteed, and the mechanical properties of the base layer can be guaranteed, solving the problem that the processing windows of traditional titanium and carbon steel are too different to be taken into account; at the same time, the elements of the base layer and the corrosion-resistant layer are fully diffused to form an interface transition layer no larger than 8μm. The grains of this layer are fine, with an average grain size of 15 to 40μm, and contain (Ti, Nb)C precipitated particles smaller than 120nm, which enhances the interface bonding performance and ensures that the interface shear strength is ≥268MPa, which is much higher than the interface shear strength of 182MPa of Chinese patent application CN201710769999.X.

[0107] The process of Chinese patent application CN201811327623.4 achieves compounding through warm rolling, which is followed by a two-stage heat treatment operation, including a primary annealing at 500-600°C for 20-60 minutes and a recrystallization annealing at 680-700°C for 30-120 minutes. It involves a method for preparing non-hot-rolled composite titanium strip steel, which is completely different from the manufacturing method disclosed herein.

[0108] The heating temperature used in the process of Chinese patent application CN201510543767.3 is 850-900℃, the final rolling temperature is below 700℃, and the single-pass reduction rate is 20-30%, the total rolling reduction rate is ≥90%, and the shear strength of the titanium-steel composite plate is greater than 240MPa. The pass reduction rate and total reduction rate required by this patent application are both very high, which can easily cause edge weld cracking during the rolling process, destroy the vacuum degree, make it difficult to composite, and have poor rolling stability. In contrast, the single-pass reduction rate of the present invention is controlled at 5-20%, which can effectively control the weld from cracking during the rolling process, ensure the vacuum degree inside the slab, and improve the interface shear strength and the stability and success rate of rolling.

[0109] Chinese patent application CN201610994234.1 relates to a method for producing titanium-steel composite plates. First, titanium plates and steel plates are assembled to form a symmetrical multi-layer composite billet of steel plate-titanium plate-isolator-titanium plate-steel plate. The billet is then compounded by rolling or explosive compounding. The compounded billet is annealed and pickled in a continuous annealing and pickling line. It is first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. However, the patent application does not specifically clarify the rolling process and the corrosion and structural properties of the obtained steel plate. The process of the patent application is significantly different from the method disclosed in the present invention in terms of manufacturing process. The method disclosed in the present invention does not require a two-stage heat treatment, which avoids the excessive diffusion of titanium, iron and carbon elements, the production of brittle intermetallic compounds of iron and titanium carbide, and the degradation of interface shear strength.

[0110] The titanium-steel composite plate disclosed in Chinese patent application CN201710996925.X features a corrosion-resistant layer made of TA2, with the titanium cladding layer having a thickness of 0.2 to 1 mm. The manufacturing process is as follows: the sealed welded composite billet is heated to 900-920°C for insulation, then rolled at an initial rolling temperature of 880-900°C, finished at a temperature above 800°C, and air-cooled to room temperature. The resulting composite plate has a shear strength of 241 MPa. In comparison, the method disclosed herein employs a heating temperature of 900-1000°C and a finish rolling temperature of 750-850°C. The method disclosed herein employs a two-stage cooling process. The disclosed method can produce hot-rolled plates with TA1, TA2, TA3, and TA4 as corrosion-resistant layers, with the corrosion-resistant layers comprising 1-10% of the total thickness of the composite billet, and an interfacial shear strength of 268 MPa or greater.

[0111] The process disclosed in Chinese patent application CN201710983322.6 uses a similar assembly and heating process to that of Chinese patent application CN201710996925.X. The reduction rate per pass is 25-30%, and the total reduction rate is ≥85%. While controlling the reduction rate per pass and the total reduction rate, the thickness of the titanium-steel composite plate is limited to 3-16 mm. The final rolling temperature is above 800°C, and the plate is air-cooled to room temperature. The titanium-steel composite plate is surface treated to produce a titanium cladding layer thickness of ≤1 mm. In contrast, the process disclosed herein uses a single-pass reduction rate of 5-20% to control rolling stability. A two-stage cooling method is used to ensure the material's microstructure, thereby controlling the yield strength ratio and toughness. Furthermore, the process disclosed herein differs significantly from the process disclosed in Chinese patent application CN201710983322.6 in terms of corrosion-resistant layer thickness and total composite strip thickness.

[0112] The hot-rolled steel strip for building structures disclosed herein can address the challenges faced when using stainless steel or carbon steel in wave splash zones. It can be effectively applied to the manufacture of steel structures used in wave splash zones, such as those found in harbors, docks, offshore oil platforms, and other facilities. This hot-rolled steel strip for building structures can meet the corrosion resistance and mechanical performance requirements of these components in wave splash zones, significantly improving their applicability, safety, and durability, and offering significant economic and social benefits.

[0113] Example

[0114] The technical solutions of the present disclosure are further described in detail below with reference to the examples and accompanying drawings. It should be understood that the following examples are merely illustrative of specific embodiments of the present disclosure and do not constitute any limitation on the scope of protection of the present disclosure. All reagents used in the examples are commercially available. Experimental methods in the examples where specific conditions are not specified were performed according to conventional conditions known in the art or according to the conditions recommended by the manufacturer.

[0115] 1 , 2 and 4 , which show schematic diagrams of two interlayer structures of the hot-rolled steel strip for building structures disclosed herein, wherein 1 is a base layer, 2 is a corrosion-resistant layer, and 3 is an interface transition layer.

[0116] The compositions of the base layer and the corrosion-resistant layer of Examples 1-8 and Comparative Examples 1-5 are shown in Table 1. Examples 1-8 and Comparative Examples 1-5 were prepared by the following steps:

[0117] 1) Smelting and casting

[0118] According to the compositions of the base layer and the corrosion-resistant layer shown in Table 1, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively;

[0119] 2) Assembly

[0120] The base blank and the corrosion-resistant layer blank are ground and polished, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are vacuumed;

[0121] 3) heating and rolling the composite billet to form a steel strip, wherein:

[0122] heating the composite blank to 900-1000° C.;

[0123] Rough rolling temperature ≥860℃; finishing rolling temperature 760~850℃; pass reduction rate 5~20%; cumulative reduction rate ≥88%;

[0124] 5) Cooling

[0125] The steel strip is cooled in two stages to 300-450°C and then coiled at this temperature.

[0126] The specific parameters of the manufacturing process of Examples 1-8 and Comparative Examples 1-5 are shown in Table 2.

[0127] Then, performance tests were performed on the base layer, corrosion-resistant layer, and composite steel plate of Examples 1-8 and Comparative Examples 1-5. Yield strength and tensile strength were measured in accordance with GB / T 6396-2008, "Mechanical and Processing Properties of Composite Steel Plates," and GB / T 228-2010, "Metallic Materials Room Temperature Tensile Test Methods." -40°C impact energy (KV2 / J) (longitudinal) was measured in accordance with GB / T 6396-2008, "Mechanical and Processing Properties of Composite Steel Plates," and GB / T 229-2020, "Metallic Materials Charpy Pendulum Impact Test Method." Grain size rating was performed as follows: Ferrite structures in stainless steel and carbon steel were graded using the intercept method according to GB / T 6394-2017, "Method for Determination of Average Grain Size of Metals."

[0128] The metallographic structures and mechanical properties of the base layer and the corrosion-resistant layer, and the thickness and mechanical properties of the interface transition layer in the composite steel plates of Examples 1-8 and Comparative Examples 1-5 are shown in Table 3.

[0129] Figure 3 shows the metallographic structure of the corrosion-resistant layer of Example 3. As shown in Figure 3 , the metallographic structure of the corrosion-resistant layer of Example 3 is single, equiaxed α-Ti with an average grain size of 103.4 μm.

[0130] Figure 4 shows the interface transition layer of Example 3. As shown in Figure 4 , the thickness of the interface transition layer is 7.6 μm, and the discontinuous fine particles therein are TiC with a size of less than 120 nm.

[0131] Figure 5 shows the metallographic structure of the base layer of Example 3. As shown in Figure 5 , the metallographic structure of the base carbon steel of Example 3 is ferrite + bainite + martensite, the volume fraction of bainite + martensite is 7.8%, and the ferrite grain size is ≥8.5.

[0132] Furthermore, the corrosion resistance of the composite steel plates of Examples 1-8 and Comparative Examples 1-5 was tested, and the results are shown in Table 4. The corrosion resistance was specifically tested as follows: Coupon specimens of the composite steel plates of Examples 1-8 and Comparative Examples 1-5 were placed in the wave splash zone of the South China Sea (selected at different placement locations, namely, Scenes 1 to 8) for 6 months, and the corrosion conditions were observed and recorded.

[0133] Comparative Examples 1-5 use unqualified composition design and thermal processing conditions, resulting in certain properties of the composite steel plates failing to meet the use requirements (performance parameters are not within the scope of the invention).

[0134] The pass reduction rate and cumulative reduction rate of Comparative Example 1 do not meet the process requirements of the present disclosure, its grains are coarse, the yield strength and impact energy of the base layer cannot meet the requirements, and the corrosion resistance is poor.

[0135] The Ti content of Comparative Example 2 is too high, its impact performance cannot meet the requirements, and its corrosion resistance is poor.

[0136] The coiling temperature of Comparative Example 3 does not meet the process requirements of the present disclosure, and the yield ratio cannot meet the requirements.

[0137] In Comparative Example 4, no V element was added, and the cooling speed after leaving the rack and the speed in the second stage cold zone did not meet the process requirements of the present disclosure, lacking the necessary precipitation strengthening effect.

[0138] The heating temperature and finishing rolling temperature of Comparative Example 5 do not meet the process requirements of the present disclosure, the thickness of the transition layer is too high, the shear strength cannot meet the requirements, and the corrosion resistance is poor.

[0139] In comparison, the base layer of Examples 1-8 has a yield strength of ≥460 MPa, a tensile strength of ≥580 MPa, a yield strength ratio of ≤0.81, an impact energy at -40°C of ≥190 J, and a wave splash corrosion rate of the corrosion-resistant layer of ≤0.006 mm / year.

[0140] It should be noted that the combination of the various technical features in the present disclosure is not limited to the combination described in the claims or the combination in the embodiments. All technical features described in the present disclosure can be freely combined or combined in any way unless there is a contradiction between them.

[0141] It should be noted that the embodiments listed above are only specific examples of the present disclosure. Obviously, the present disclosure is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily associated with the contents of the present disclosure by those skilled in the art should fall within the scope of protection of the present disclosure.

Claims

1. A hot-rolled steel strip for building structure, characterized in that: The hot-rolled steel strip comprises a base layer, a corrosion-resistant layer, and an interface transition layer between the base layer and the corrosion-resistant layer; In addition to Fe and other inevitable impurities, the base layer also contains the following chemical elements in the following mass percentages: C: 0.03-0.13%, Si: 0.15-0.35%, Mn: 1.00-1.50%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.10-0.65%, Ni: 0.2-1.0%, Cu: 0.10-0.25%, Al: 0.020-0.050%, Ti: 0.0090-0.0160%, Nb: 0.060-0.100%, N: 0.0005-0.0050%, V: 0.08-0.25%; The corrosion-resistant layer is made of industrial pure titanium, preferably TA1, TA2, TA3 or TA4.

2. The hot-rolled steel strip for building structure according to claim 1, characterized in that: The chemical composition of the base layer also satisfies the following relationship: 0.32%≤Cu+Ni≤1.15%; 2(C+N)≤Ti+Nb+Cr+V≤0.90%.

3. The hot rolled steel strip for building structure according to claim 1 or 2, characterized in that: The mass percentage of each chemical element of the base layer is: C: 0.03-0.13%, Si: 0.15-0.35%, Mn: 1.00-1.50%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.10-0.65%, Ni: 0.2-1.0%, Cu: 0.10-0.25%, Al: 0.020-0.050%, Ti: 0.0090-0.0160%, Nb: 0.060-0.100%, N: 0.0005-0.0050%, V: 0.08-0.25%, and the balance is Fe and other inevitable impurities.

4. The hot rolled steel strip for building structure according to any one of claims 1 to 3, characterized in that: The microstructure of the base layer is ferrite+bainite+martensite structure, the content of bainite+martensite is 5% to 15%, and the average grain size of ferrite is ≥8.

5.

5. The hot rolled steel strip for building structure according to any one of claims 1 to 4, characterized in that: The yield strength of the base layer is ≥460MPa, the tensile strength is ≥580MPa, the yield strength ratio is ≤0.81, and the impact energy at -40°C is ≥190J.

6. The hot rolled steel strip for building structure according to any one of claims 1 to 5, characterized in that: The microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.

7. The hot rolled steel strip for building structure according to any one of claims 1 to 6, characterized in that: The sea wave splash corrosion resistance rate of the corrosion resistant layer is ≤0.006mm / year.

8. The hot rolled steel strip for building structure according to any one of claims 1 to 7, characterized in that: The thickness of the interface transition layer is ≤8 μm, the average grain size is 15-40 μm, and it contains precipitated particles of (Ti, Nb)C less than 120 nm, and the interface shear strength is ≥268 MPa.

9. The hot rolled steel strip for building structure according to any one of claims 1 to 8, characterized in that: The thickness of the hot-rolled steel strip is 1 to 16 mm.

10. The hot rolled steel strip for building structure according to any one of claims 1 to 9, characterized in that: The hot-rolled strip has a base yield strength of ≥460MPa, a tensile strength of ≥580MPa, a yield strength ratio of ≤0.81, an impact energy of -40°C ≥190J, a sea wave splash corrosion rate of the corrosion-resistant layer of ≤0.006mm / year, and an interface shear strength of ≥268MPa.

11. A method for manufacturing the hot rolled steel strip for building structure according to any one of claims 1 to 10, characterized in that: The method comprises the following steps performed in sequence: 1) Smelting and casting According to the composition of the base layer and the corrosion-resistant layer as described in any one of claims 1 to 3, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively; 2) Assembly The base blank and the corrosion-resistant layer blank are subjected to surface grinding and polishing, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are subjected to vacuum treatment; 3) heating and rolling the composite billet to form a steel strip, wherein: The composite blank is heated to 900-1000° C.; The rough rolling temperature is ≥860°C; the finishing rolling temperature is 760-850°C, preferably 780-850°C; the pass reduction rate is 5-20%, preferably 10-15%; the cumulative reduction rate is ≥88%; 4) Cooling The steel strip is cooled to 300-450°C and then coiled at this temperature to obtain hot-rolled strip steel.

12. The method according to claim 11, characterized in that In step 2), the thickness of the corrosion-resistant layer is 1-10% of the thickness of the composite blank; and / or in step 3), the thickness of the interface transition layer formed between the base layer and the corrosion-resistant layer is ≤8 μm.

13. The method according to claim 11 or 12, characterized in that In step 4), the cooling includes two stages of cooling, wherein in the first stage, the steel strip is cooled to 700-750°C at a cooling rate of 2-10°C / s after leaving the rolling mill stand; in the second stage, the steel strip is cooled to 300-450°C at a cooling rate of 30-50°C / s.

Citation Information

Patent Citations

  • Manufacturing method of titanium-steel-titanium two-sided composite plate

    CN102773670A

  • Preparation method of titanium-steel clad plate

    CN105107841A

  • Production method of titanium-steel composite plate

    CN106269963A

  • A method for preparing titanium-steel composite plates

    CN107626764B

  • A titanium-steel-titanium composite plate and its preparation method

    CN109304367B