500 mpa-grade hot-rolled strip steel for building structure resistant to sea wave splashing area corrosion and manufacturing method for hot-rolled strip steel

Through the design of low-carbon microalloy composition and specific process processing, the formed hot-rolled strip steel provides high corrosion resistance and excellent mechanical properties in the wave splash zone, solving the corrosion and low-temperature impact of steel structures in the marine environment in the prior art. Problem, meet the needs of high-strength level building structures.

WO2024244625A1PCT designated stage expired Publication Date: 2024-12-05BAOSHAN IRON & STEEL CO LTD

Patent Information

Application Number
PCT/CN2024/082496
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-03-19
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The prior art cannot provide high corrosion resistance and excellent mechanical properties in the wave splash zone, especially in the corrosion and low-temperature impact toughness of steel structures in marine environments, and cannot meet the requirements of high-strength grade use.

Method used

Hot-rolled strip designed with low carbon microalloy composition, through industrial pure titanium as corrosion-resistant layer and carbon steel as the base layer, and through specific heating and rolling processes without adding metal isolation layer The layer achieves an excellent combination of titanium and carbon steel, ensures the yield and strength ratio of the base layer and the low-temperature impact toughness, while maintaining the corrosion resistance of the corrosion-resistant layer.

Benefits of technology

Without reducing the corrosion resistance of the corrosion resistance layer, the mechanical properties of the base layer are improved, meeting the requirements of 500MPa yield strength and 640MPa tensile strength, and significantly improving the impact work and interface shear strength of -40℃, suitable for Steel structural parts in the splashing area of ​​sea waves.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082496_05122024_PF_FP_ABST
    Figure CN2024082496_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to a hot-rolled strip steel for a building structure and a manufacturing method for the hot-rolled strip steel. The hot-rolled strip steel comprises a base layer, a corrosion-resistant layer, and an interface transition layer located between the base layer and the corrosion-resistant layer; the mass percentages of chemical elements of the base layer are: C: 0.050-0.100%, Si: 0.15-0.30%, Mn: 1.0-1.8%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.80-1.60%, Ni: 0.50-1.20%, Cu: 0.20-0.40%, Al: 0.020-0.050%, Ti: 0.010-0.018%, Nb: 0.020-0.100%, N: 0.0005-0.0050%, Mo: 0.20-0.50%, and the balance of Fe and other inevitable impurities; and the corrosion-resistant layer is prepared from industrial pure titanium. The yield strength of the base layer of the hot-rolled strip steel for a building structure in the present disclosure is greater than or equal to 500 MPa, the tensile strength is greater than or equal to 640 MPa, the yield strength ratio is 0.75-0.85, the impact energy at -40°C is greater than or equal to 190 J, the speed of the sea wave splashing corrosion resistance of the corrosion-resistant layer is lower than or equal to 0.006 mm / year, the thickness of the interface transition layer is smaller than or equal to 8 μm, and the interfacial shear strength is greater than or equal to 263 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

500MPa grade hot-rolled steel strip for building structures resistant to sea wave splash zone corrosion and its manufacturing method Technical Field

[0001] The present disclosure relates to steel for building structures and a manufacturing method thereof, and in particular to a hot-rolled steel strip for building structures that is resistant to corrosion in a wave splash zone and a manufacturing method thereof. Background Art

[0002] Traditional marine structures and equipment are primarily constructed from low-strength steel. However, as the development of marine resources gradually shifts from shallow water to deep water, the requirements for structural and equipment strength, toughness, and corrosion resistance are becoming increasingly stringent, necessitating the use of new materials. The ocean is a harsh and complex corrosive environment. Seawater is a strong electrolyte solution containing high concentrations of chloride ions. Steel facilities, which form the backbone of marine engineering facilities, are susceptible to electrochemical reactions with the surrounding medium, causing severe corrosion, significantly reducing their service life. This is especially true in the splash zone, the harshest marine corrosion zone. Facilities are subject to a range of external factors, including alternating dry and wet conditions, ocean spray, sunlight, corrosive components in the atmosphere, and oxygen, leading to particularly severe material corrosion.

[0003] Investigations show that steel piles in facilities such as harbors and offshore oil platforms are subject to severe corrosion, typically 3 to 10 times the strength of the fully immersed seawater area. Once severe localized corrosion damage occurs, the bearing capacity of the entire facility is significantly reduced, shortening its service life, impacting production safety, and even leading to premature decommissioning.

[0004] In the splash zone, due to its alternating dry and wet atmosphere and ample oxygen supply, the corrosion products produced offer no protective effect. Splashing seawater can directly strike metal surfaces, causing severe corrosion. Corrosion tests and surveys have shown that, under normal circumstances, the average corrosion rate of ordinary carbon steel and low-alloy steel in marine atmosphere is approximately 0.03 to 0.08 mm / year, while in the splash zone, it is 0.3 to 0.5 mm / year. In the splash zone, steel piles are susceptible to severe corrosion damage, significantly reducing the bearing capacity of the entire steel structure, impacting safe production, shortening its service life, and leading to premature scrapping.

[0005] Based on the aforementioned operating conditions, industrially pure titanium was selected as the corrosion-resistant layer. Titanium is highly chemically active and readily reacts with oxygen in air to form oxides. The oxides on the titanium metal surface are dense, stable, and possess a strong self-healing ability. This self-healing ability primarily refers to the ability of titanium oxide to rapidly form a new film after damage to a specific area on the titanium surface, preventing further contact with corrosive media.

[0006] For steel used in marine building structures, in addition to meeting the requirements of corrosion resistance, it must also have good mechanical properties. Among them, the yield ratio and low-temperature impact toughness are increasingly becoming the key indicators of construction steel. The yield ratio is the ratio of the yield strength of steel to the tensile strength. Its size reflects the ability of steel to not produce strain concentration during plastic deformation. The lower the yield ratio, the more evenly the plastic deformation of the steel can be distributed over a wider range. Under the action of seismic forces, the plastic deformation of steel structure systems made of steel with low yield ratio can be evenly distributed over a wider range; while materials with high yield ratio may experience strain concentration, reducing the overall plastic deformation ability of the steel, resulting in brittle failure of the structure, causing structural instability and sudden collapse.

[0007] Steel undergoes a brittle transition at low temperatures, shifting its fracture pattern from ductile to brittle. This engineering significance lies in the fact that components will not experience brittle fracture when exposed to temperatures above this threshold. Therefore, structural steel typically requires specific low-temperature impact resistance based on the material's service environment. Ocean temperatures vary significantly at different latitudes. For example, near China's Bohai Bay, winter seaside temperatures can reach below -20°C, requiring building materials to possess excellent impact resistance at -40°C to prevent brittle fracture.

[0008] However, when the plastic toughness of steel is improved, if the increase in tensile strength is small, the yield ratio will increase significantly, making it difficult to control the low yield ratio.

[0009] Japanese patent application JP 2011167002A discloses a steel marine structure with excellent corrosion resistance, which reduces painting costs. The solution is to use coated steel with a specified coating thickness in height zones where the amount of incoming sea salt particles exceeds a specified threshold, and uncoated steel in height zones where the amount of incoming sea salt particles falls below the threshold. The threshold is 0.1 mdd or less. The unpainted steel material contains, by mass%, less than 0.08% C, less than 0.75% Si, less than 2.0% Mn, less than 0.030% P, less than 0.030% S, 0.01-0.05% Al, less than 0.010% N, 0.50-1.0% W, 0.010-0.200% Nb, and less than 0.01-0.10% Cr. Furthermore, it preferably contains one or two selected from 0.05-0.50% Cu and 0.05-0.50% Ni. Marine structures are preferred, particularly offshore wind turbines. This significantly reduces the area to be painted, shortening the painting process, reducing re-painting time, and lowering painting costs. While this patent application provides a marine steel structure, the corrosion resistance of the steel structure is achieved through painting.

[0010] Chinese patent application CN 201210260231.7 discloses a method for preparing a titanium-steel-titanium double-sided composite plate. The method comprises stacking four titanium plates and three steel plates in a certain order in a closed frame welded with two outermost steel plates, adding an isolation agent made of a mixture of 1 part by weight of active α-Al2O3 and 1.5 parts by weight of a 4% polyvinyl alcohol aqueous solution between the titanium plates, and using a nickel-based alloy as a transition layer between the titanium plates. The plate is heated to 500°C to 630°C and vacuumed, kept warm for 1 to 2 hours, and the vacuum degree reaches 20 to 200 Pa. The method is characterized in that welding is first performed after assembly, and then vacuuming is performed. Only ordinary welding is required during welding. Conventional arc welding and submerged arc welding can meet the conditions. Compared with welding under vacuum conditions, the welding conditions are less demanding, the cost is low, and there is no need to set up a separate vacuum chamber. The combined billets are then rolled and composited in a conventional heating furnace at a rolling temperature of 700°C to 900°C. The C in the coal gas can be blocked by sealing the outermost steel plate and vacuuming. At the same time, a nickel-based alloy isolation layer is added to prevent the formation of TiC at the interface, resulting in a titanium-steel composite plate with a shear strength of 230 to 260 MPa and an interface bonding rate of 99.6% to 100%.

[0011] Chinese patent application CN201710769999.X discloses a method for preparing a titanium-steel composite plate, which comprises selecting the surfaces of titanium-steel composite billets in contact with each other, applying a high-temperature resistant anti-carburizing and anti-nitriding isolation coating on the contacting titanium surfaces, and drying them at room temperature; after the drying process, the titanium billets are aligned and stacked in pairs, and a steel billet is placed in the middle to complete the assembly to obtain a composite billet, wherein the thickness of the titanium plate used is greater than 2 mm, and the thickness of the steel plate is greater than 5 mm, and then the composite billet is sealed and welded around and a certain size of unwelded area is left, and the billet is vacuumed to 10 -2 ~10 -3 Pa and then welded; the slab is heated to 500-700°C and rolled, with a first-pass reduction exceeding 25%, a final-pass reduction not exceeding 15%, a total reduction of 60-70%, and a rolling speed of 0.1-1.0 mm / s. This patent application utilizes a high-temperature impermeability protection coating to protect against the diffusion and oxidation of other impurity elements at high temperatures, blocking the diffusion of elements such as C and N. The embodiment utilizes a combination of Q235 and TA1, producing steel plates with shear strengths of 176 MPa, 181 MPa, and 182 MPa, respectively.

[0012] The above two patent applications mainly avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy isolation layer between titanium and carbon steel.

[0013] Chinese patent application CN201811327623.4 discloses a titanium-steel-titanium composite plate and its preparation method, which is a process of fixing a carbon steel between two titanium plates of the same size, and performing warm composite rolling through an irreversible large rolling force warm rolling mill to composite the three layers of strips into one. After rolling, the rolled composite plate is subjected to heat treatment, including an initial annealing at 500-600°C for 20-60 minutes and a recrystallization annealing at 680-700°C for 30-120 minutes. Finally, the product is obtained by straightening, flattening, shearing and shaping. This patent application mainly describes a method for preparing a non-hot-rolled composite titanium steel plate. However, due to the use of an irreversible rolling mill, only single-pass rolling production can be carried out, and heat treatment is also required. The embodiment mainly involves the steel strip production method, and the performance after composite is not mentioned.

[0014] Chinese patent application CN201510543767.3 discloses a method for preparing a titanium-steel composite plate. The titanium-steel composite plate obtained by this method has high bonding strength. The patent application fixes a titanium plate between two ordinary carbon steel plates or billets, welds the billets around the edges in a vacuum environment, heats the combined billets to 850-900°C for 120-360 minutes, controls the start rolling temperature to above 800°C and the final rolling temperature to below 700°C, and controls the single-pass deformation to be between 20-30%, with the total rolling deformation ≥90%. A large reduction is performed to break up the brittle phase compounds generated at the interface and reduce their impact on the bonding surface, thereby rolling to obtain a titanium-steel composite plate with a bonding strength greater than 240 MPa. However, the pass reduction rate and total deformation required by the patent application are both very high, which can easily cause edge weld cracking during the rolling process, destroying the vacuum degree and making it unsuitable for interface bonding.

[0015] Chinese patent application CN201610994234.1 discloses a method for producing titanium-steel composite plates, which involves an annealing technology production method for titanium-steel plates. First, the titanium plate and the steel plate are assembled to form a symmetrical multi-layer composite billet of steel plate-titanium plate-isolator-titanium plate-steel plate, which is then compounded by rolling compounding or explosive compounding. The compounded billet is annealed and pickled in a continuous annealing and pickling line, first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. The purpose of this patent application is to simultaneously obtain the properties of the composite material and the substrate through a two-stage heat treatment. However, the two-stage heat treatment will lead to excessive diffusion of titanium, iron, and carbon elements, resulting in brittle substances such as iron-titanium intermetallic compounds and titanium carbide, which deteriorate the interface shear strength.

[0016] Chinese patent application CN201710996925.X discloses a thin-layer double-sided titanium-steel composite plate and its preparation method. Through large-thickness billet assembly and large-reduction rolling technology, a good composite between titanium and steel is achieved. This patent application is a double-sided titanium composite plate composed of a titanium composite layer, a base layer and a titanium composite layer. The titanium composite layer is made of TA2, and the thickness of the titanium composite layer is 0.2 to 1 mm. The billets are stacked in the order of cover plate, titanium composite material, carbon steel substrate, titanium composite material, and cover plate from top to bottom. After vacuum is drawn in a vacuum chamber, the gaps around them are vacuum electron beam sealed and welded. The vacuum degree is 1.0×10 -2 ~4.5×10 -2 Pa. The composite billet after the sealing welding process is heated to 900-920℃ and kept warm. The holding time is calculated according to 1min / mm×total thickness of the composite billet. The starting rolling temperature is 880-900℃, the final rolling temperature is above 800℃, and it is air-cooled to room temperature. The single-pass reduction rate is ≥15%, and the first three-pass reduction rate is ≥20%, and the total reduction rate is ≥80%. The composite plate obtained after rolling is trimmed, split, and surface-grinded to obtain a double-sided titanium-steel composite plate. This patent application uses surface cleaning treatment of the composite slab, the air isolation effect of the cover plate, the control of the rolling temperature, and the use of large reduction to break and refine the titanium iron and titanium carbon compounds generated at the composite interface, disperse them at the composite interface, improve the distribution state of the compounds, further ensure the composite quality and performance stability, and achieve a shear strength of 241MPa.

[0017] Chinese patent application CN201710983322.6 discloses a thin-layer titanium-steel composite plate and its preparation method, which adopts a double-layer structure of titanium and carbon steel. Its assembly method and heating process are similar to those of Chinese patent application CN201710996925.X. The starting rolling temperature is 880-900℃, the single-pass reduction rate is 25-30%, and the total reduction rate is ≥85%. While controlling the single-pass reduction rate and the total reduction rate, the thickness of the titanium-steel composite plate is limited to 3-16mm, the final rolling temperature is above 800℃, and it is air-cooled to room temperature. The titanium-steel composite plate is obtained by surface treatment, and the titanium composite layer thickness is ≤1mm. This patent application improves the composite quality by symmetrical assembly and welding titanium seals into carbon steel plates. After rolling, the shear strength of the steel plate reaches more than 238MPa, and the composite interface bonding rate is 100%. Its carbon steel layer meets the national standard requirements for Q345 grade carbon steel.

[0018] However, the above two patent applications did not mention the detailed design of the composite layer and the base layer, and only described the tensile properties and shear strength. The required pass reduction rate and total reduction rate of the composite layer were both relatively high, and there was no control over the corrosion resistance of the material, the low-temperature impact performance of the base material, the yield strength ratio and other performance indicators, which did not meet the requirements for steel used in building structures.

[0019] In summary, the above patent applications mainly describe the preparation method of composite steel plates, and the specific embodiments briefly describe the interface shear strength and tensile properties in terms of performance. In addition to being resistant to corrosion in the wave splash zone, steel used for steel structures in the wave splash zone must also ensure that they have the necessary structural steel performance requirements, as well as the aforementioned low yield ratio and corresponding low-temperature impact performance to ensure structural safety. However, the products involved in the above patent applications are all at a strength level of 345MPa, which cannot meet the use requirements of high-strength structural components, and the above patent applications have not carried out relevant component and process design for the corrosion rate, yield ratio, low-temperature impact, etc. of the corrosion-resistant layer, and cannot guarantee that the use requirements of high-corrosion-resistant and high-strength steel plates for steel structures in the wave splash zone environment can be met.

[0020] Summary of the Invention

[0021] In view of the above-mentioned shortcomings of the prior art, the present invention aims to provide a hot-rolled steel strip for building steel structures and a method for manufacturing the same. The hot-rolled steel strip for building steel structures disclosed herein can ensure that the mechanical properties of the base layer (carbon steel) meet the corresponding strength level requirements without compromising the corrosion resistance of the corrosion-resistant layer itself, and the base layer also has excellent yield strength ratio and low-temperature impact toughness.

[0022] Therefore, in one aspect, the present disclosure provides a hot-rolled steel strip for building structures, wherein the hot-rolled steel strip comprises a base layer, a corrosion-resistant layer, and an interface transition layer between the base layer and the corrosion-resistant layer;

[0023] In addition to Fe and other inevitable impurities, the base layer also contains the following chemical elements in the following mass percentages: C: 0.050-0.100%, Si: 0.15-0.30%, Mn: 1.0-1.8%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.80-1.60%, Ni: 0.50-1.20%, Cu: 0.20-0.40%, Al: 0.020-0.050%, Ti: 0.010-0.018%, Nb: 0.020-0.100%, N: 0.0005-0.0050%, Mo: 0.20-0.50%;

[0024] The corrosion-resistant layer is made of industrial pure titanium, preferably TA1, TA2, TA3 or TA4.

[0025] Preferably, the chemical composition of the base layer also satisfies the following relationship: 0.9%≤Cu+Ni≤1.45%; 2(C+N)≤Ti+Nb+Cr+Mo≤1.90%.

[0026] Preferably, the mass percentage of each chemical element in the base layer is: C: 0.050-0.100%, Si: 0.15-0.30%, Mn: 1.0-1.8%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.80-1.60%, Ni: 0.50-1.20%, Cu: 0.20-0.40%, Al: 0.020-0.050%, Ti: 0.010-0.018%, Nb: 0.020-0.100%, N: 0.0005-0.0050%, Mo: 0.20-0.50%, and the remainder is Fe and other inevitable impurities.

[0027] Preferably, the microstructure of the base layer is granular bainite and / or lath bainite, and the effective grain size is ≤10 μm.

[0028] Preferably, the yield strength of the base layer is ≥500 MPa, the tensile strength is ≥640 MPa, the yield strength ratio is 0.75-0.85, and the impact energy at -40°C is ≥190 J.

[0029] Preferably, the microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.

[0030] Preferably, the wave splash corrosion resistance rate of the corrosion-resistant layer is ≤0.006 mm / year.

[0031] Preferably, the thickness of the interface transition layer is ≤8 μm, the average grain size is 15-40 μm, and it contains precipitated (Ti, Nb)C particles with a size less than 120 nm, and the interface shear strength is ≥263 MPa.

[0032] The interface transition layer of the hot-rolled steel strip disclosed herein has 100% metallurgical bonding, highly coherent atoms, and fine grains in the interface transition layer (average grain size is 15-40 μm).

[0033] Preferably, the thickness of the hot-rolled steel strip for building structures is 3 to 16 mm.

[0034] The hot-rolled steel strip for building structures disclosed herein has a base yield strength of ≥500 MPa, a tensile strength of ≥640 MPa, a yield strength ratio of 0.75 to 0.85, an impact energy at -40°C of ≥190 J, a sea wave splash corrosion rate of the corrosion-resistant layer of ≤0.006 mm / year, an interface transition layer thickness of ≤8 μm, and an interface shear strength of ≥263 MPa. The hot-rolled steel strip disclosed herein can meet the corrosion resistance requirements for use in sea wave splash zone environments, and has both good mechanical properties for resistance to sea wave splash zone corrosion and high economic efficiency, and can be applied to steel structural parts such as steel piles of facilities such as seaport terminals and offshore oil platforms.

[0035] The present invention adopts a low-carbon microalloying component design, which achieves an excellent combination of titanium and carbon steel without adding a metal isolation layer, and effectively controls the thickness of the interface transition layer, so that the mechanical properties of the base layer (carbon steel) can meet the corresponding strength level requirements without reducing the corrosion resistance of the corrosion-resistant layer itself, and the base layer has an excellent yield strength ratio and low-temperature impact toughness.

[0036] In another aspect, the present disclosure provides a method for manufacturing the hot-rolled steel strip for building structures, comprising the following steps performed in sequence:

[0037] 1) Smelting and casting

[0038] According to the above compositions of the base layer and the corrosion-resistant layer, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively;

[0039] 2) Assembly

[0040] The base blank and the corrosion-resistant layer blank are ground and polished, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are vacuumed;

[0041] 3) heating and rolling the composite billet to form a steel strip, wherein:

[0042] The composite blank is heated to 900-1000° C.;

[0043] The rough rolling temperature is ≥880°C; the finishing rolling temperature is 760-850°C, preferably 780-850°C; the pass reduction rate is 5-20%, preferably 10-20%; the cumulative reduction rate is ≥88%;

[0044] 4) Cooling

[0045] After leaving the rolling mill stand, the steel strip is cooled to 300-450°C at a cooling rate of 10-25°C / s, and then coiled at this temperature to produce hot-rolled strip steel.

[0046] Preferably, in step 2), the thickness of the corrosion-resistant layer is 1 to 10% of the thickness of the composite blank.

[0047] Preferably, in step 3), the thickness of the interface transition layer formed between the base layer and the corrosion-resistant layer is ≤8 μm.

[0048] Through the preparation method disclosed in the present invention, especially the control of the heating, rolling and cooling processes, the base layer in the strip steel exhibits excellent yield strength ratio and low-temperature impact toughness, while the corrosion-resistant layer has excellent corrosion resistance and high bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] FIG1 is a schematic diagram of the interlayer structure of a hot-rolled steel strip for building structures according to one embodiment of the present disclosure.

[0050] FIG2 is a schematic diagram of the interlayer structure of a hot-rolled steel strip for building structures according to another embodiment of the present disclosure.

[0051] FIG3 is a microstructure photograph of the corrosion-resistant layer of Example 3.

[0052] FIG4 is a scanning image of the interface transition layer between the base layer and the corrosion-resistant layer of Example 3. FIG.

[0053] FIG5 is a microstructure photograph of the base layer of Example 3. DETAILED DESCRIPTION

[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. The terms used in the description of the present disclosure are for the purpose of describing particular embodiments only and are not intended to limit the present disclosure.

[0055] In this article, "industrially pure titanium" refers to dense metallic titanium with a titanium content of not less than 99% and a small amount of impurities such as iron, carbon, oxygen, nitrogen and hydrogen. "TA1, TA2, TA3, TA4" represent the grades of industrially pure titanium. This grading standard is based on GB / T3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Composition", and grades pure titanium according to purity (i.e. impurity content).

[0056] In this article, "yield ratio" refers to the ratio of the yield strength of steel to its tensile strength, and its size reflects the ability of steel to avoid strain concentration during plastic deformation.

[0057] In this paper, the yield strength and tensile strength were measured with reference to GB / T 6396-2008 “Mechanical and process properties of composite steel plates” and GB / T 228-2010 “Methods of tensile test at room temperature for metallic materials”.

[0058] In this article, the -40℃ impact energy KV2 / J (longitudinal) is measured with reference to GB / T 6396-2008 "Mechanical and process properties of composite steel plates" and GB / T 229-2020 "Charpy pendulum impact test method for metallic materials".

[0059] In this paper, grain size rating is performed as follows: According to GB / T 6394-2017 “Method for determination of average grain size of metals”, the intercept method is used to grade the grain size of ferrite in stainless steel and carbon steel respectively.

[0060] In this paper, the wave splash corrosion rate is measured as follows: the composite steel plate coupons are placed in the wave splash zone of the South China Sea for 6 months and then the corrosion conditions are observed and recorded. First, the coupons are cleaned and weighed, and the loss volume is obtained by dividing the loss weight by the density. Then, the loss volume is divided by the exposed area of ​​the coupon to obtain the loss thickness.

[0061] In this paper, the interface shear strength was measured with reference to GB / T 6396-2008 “Mechanical and process properties of composite steel plates”.

[0062] In this article, the metals of the base layer and the corrosion-resistant layer undergo recrystallization and grain growth under high temperature and high pressure. During this process, some grains will pass through the interface; at the same time, due to the difference in element content on both sides of the interface, the metal elements will diffuse from high concentration to low concentration at high temperature. The above two factors work together to form an interface transition layer.

[0063] In the base composition design of the hot-rolled steel strip for building steel structure disclosed in the present invention:

[0064] C: It plays a role of solid solution strengthening in steel and can significantly improve the strength of steel. However, too high a C content is detrimental to welding performance and toughness. More importantly, when the C content is too high, C will diffuse to the composite interface, forming a large number of large-granular TiC hard phases in the interface transition layer, reducing the composite interface strength. Therefore, in order to ensure the shear strength of the interface, a low C content must be adopted. The change in C content has less effect on the yield strength of steel than on the tensile strength. Therefore, under the premise of ensuring the formability and welding performance of the product, appropriately increasing the C content is beneficial to reducing the yield strength ratio of steel. Based on this, in the base component disclosed in the present invention, the C content is controlled at 0.050~0.100%.

[0065] Si: Adding Si to steel effectively deoxidizes and improves its purity. Furthermore, Si acts as a solid solution strengthener in steel, increasing its strength and hardness. However, excessive Si content can negatively impact the material's weldability. Therefore, in the base composition disclosed herein, the Si content is controlled within a range of 0.15-0.30%.

[0066] Mn: Mn is the cheapest matrix-strengthening element. It can lower the austenite transformation temperature, delay pearlite transformation, refine ferrite grains, and increase steel strength. Mn also counteracts the effects of sulfur on steel. However, excessive Mn content can easily lead to segregation bands and martensitic structures, which negatively impact the toughness of the steel. Therefore, in the base composition disclosed herein, the Mn content is controlled to 1.0-1.8%.

[0067] Al: Al is mainly added to the steel in excess as a de-O element to ensure that the O content in the steel is as low as possible. After de-O, the excess Al combines with the N element in the steel to form AlN precipitates. During the heating process, AlN hinders the growth of austenite grains, refines the austenite grains, and improves the strength and toughness of the matrix. At the same time, the formation of AlN fixes part of the N in the matrix, reduces the diffusion of interstitial atomic N in the carbon steel base layer to the composite interface, and forms hard TiN in the interface transition layer (which deteriorates the interface shear strength of the composite plate); at the same time, the amount of Ti and Nb added can be reduced, reducing the total cost. Based on this, in the base composition disclosed in the present invention, the Al content is controlled at 0.020~0.050%.

[0068] Ti: Ti forms stable TiN or Ti(N, C) at high temperatures, which plays a role in fixing C and N, preventing the interstitial C and N atoms in the carbon steel base from diffusing to the interface, and forming hard TiN or Ti(N, C) precipitation in the interface transition layer to obtain a composite plate with high interface shear strength. At the same time, TiN hinders the growth of austenite during the heating process, can refine the austenite grains, and can improve the strength and toughness of the matrix. In subsequent welding, TiN inhibits the growth of austenite grains, especially in the heat-affected zone (HAZ) close to the molten boundary of the weld, thereby improving the toughness of the welding HAZ, thereby being able to adapt to the needs of large welding heat input processes. Reducing the diffusion of C and N to the interface can increase the strength of the low-carbon matrix and obtain a composite plate with high interface shear strength. Based on this, in the base composition disclosed in the present invention, the Ti content is controlled at 0.010-0.018%.

[0069] Nb: Nb exists in the steel in the form of solid solution Nb and Nb(C, N), and plays the role of solid solution drag and precipitation pinning during the recrystallization process. The main purpose of adding a small amount of Nb to the base carbon steel is to increase the recrystallization temperature, so that the base carbon steel can be refined after rolling in the recrystallization and non-recrystallization zones, which is beneficial to improving the low-temperature impact toughness of the base carbon steel. Due to the action of the Nb(C, N) precipitation phase, the original austenite grains will be finer, thereby promoting the formation of finer recrystallized grains and obtaining an ideal combination of high strength and high toughness. At the same time, Nb can fix the interstitial C and N atoms in the matrix, reduce the diffusion of C and N to the interface, and obtain a composite plate with high interface shear strength. Based on this, in the base layer disclosed in the present invention, the Nb content is controlled at 0.020~0.100%.

[0070] Cu: Cu plays a role in solid solution strengthening, and as the Cu content increases, the room temperature impact toughness of the steel slightly increases. Therefore, in the base composition disclosed herein, the Cu content is controlled to be 0.20-0.40%.

[0071] N: Elemental N can react with Ti and Al to form second-phase particles, refining austenite grains and improving matrix strength and toughness. However, excessive N content can produce excessive amounts of TiN and overly coarse particles, which can affect the plasticity and toughness of carbon steel. Therefore, in the base layer of this disclosure, the N content is controlled to 0.0005% to 0.0050%.

[0072] Ni: Ni can improve the hardenability of the base carbon steel, thereby obtaining a full bainite structure, and is an element that stabilizes austenite. During the coiling process, it can promote the formation of stable Mahor islands in granular bainite, which can greatly improve the low-temperature impact toughness and plasticity of the steel. At the same time, Ni can effectively prevent the diffusion of Ti into the base carbon steel, which helps to control the thickness of the interface transition layer. In addition, the use of Ni in combination with Cr and Mo can improve the corrosion resistance of the base carbon steel. However, nickel is expensive, and adding too much will increase the cost of the composite plate. Based on this, an appropriate amount of Ni is added to the base component of the present invention, and the Ni content is controlled to be 0.50-1.20%.

[0073] Cr: Cr is a strong carbide-forming element with a slow diffusion rate in austenite, while hindering the diffusion of C. During low-temperature processes, Cr forms fine carbides with C, which play a role in precipitation strengthening. At the same time, Cr can fix the interstitial C and N atoms in the matrix, reducing the diffusion of C and N to the interface, and obtaining a composite plate with high interfacial shear strength. However, while Cr increases the matrix strength in steel, it also reduces toughness. Therefore, in order to achieve the best match between strength and toughness, the Cr content in the base composition disclosed herein is controlled to be between 0.80% and 1.60%.

[0074] Mo: In the base layer of the present disclosure, Mo significantly refines grains, improves the strength and toughness of the matrix, and forms stable carbides with carbon, increasing the strength of the base layer. Mo also improves the hardenability of the base carbon steel, facilitating the formation of bainite in the base layer. Therefore, an appropriate amount of Mo can be added to the base layer of the present disclosure, with the mass percentage of Mo controlled within 0.20-0.50%.

[0075] In the hot-rolled steel strip for building structures disclosed herein, S and P are both unavoidable impurity elements, and the lower their content, the better. However, considering the actual steelmaking level of the steel mill, the S and P contents in the base composition disclosed herein are controlled to be: P: 0.0005-0.003%, S: 0.0005-0.010%;

[0076] In addition, in the base chemical composition design of the hot-rolled steel strip for building steel structure disclosed in the present invention:

[0077] Both Cu and Ni can improve the toughness of the base layer, and the combined addition effect is particularly significant. Furthermore, the addition of Ni can reduce the diffusion rate of carbon in steel, reducing its diffusion to the interface. Therefore, to achieve better performance, the base layer composition of the present disclosure preferably satisfies the following conditions: 0.9% ≤ Cu + Ni ≤ 1.45%. This helps to control the interfacial transition layer to within 8 μm.

[0078] Ti, Nb, Cr and Mo are all strong carbonitride-forming elements, which can form corresponding carbonitrides in the base carbon steel. This can fix the interstitial atoms in the base, hinder the diffusion of C and N interstitial atoms to the interface, and form large-grained, aggregated carbonitrides in the interface transition layer, which helps to control the interface transition layer within 8μm, thereby improving the interface shear strength. At the same time, Ti, Nb and Cr can play a role in refining the base carbon steel grains and improving toughness at different stages of hot rolling. Therefore, in order to obtain better performance, in the base composition disclosed in the present invention, it is preferred that the content of Ti, Nb, Cr and Mo further satisfy the following requirements: 2(C+N)≤Ti+Nb+Cr+Mo≤1.90%.

[0079] The corrosion-resistant layer disclosed herein uses industrial pure titanium, preferably TA1, TA2, TA3 and TA4, whose composition meets the standard of GB / T3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Composition".

[0080] The method for manufacturing hot-rolled steel strip for building structures disclosed herein comprises the following steps performed in sequence:

[0081] 1) Smelting and casting

[0082] According to the compositions of the base layer and the corrosion-resistant layer, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively;

[0083] 2) Assembly

[0084] The base blank and the corrosion-resistant layer blank are ground and polished, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are vacuumed;

[0085] 3) heating and rolling the composite billet to form a steel strip, wherein:

[0086] The composite blank is heated to 900-1000° C.;

[0087] The rough rolling temperature is above 880℃, the finishing rolling temperature is 760~850℃, the pass reduction rate is 5~20%, the cumulative reduction rate is ≥88%, no descaling water is used, and a heat insulation cover is added;

[0088] 4) Cooling

[0089] After leaving the rolling mill stand, the steel strip is cooled to 300-450°C at a cooling rate of 10-25°C / s, and then coiled at this temperature to produce hot-rolled strip steel.

[0090] Preferably, in step 2), the thickness of the corrosion-resistant layer is 1 to 10% of the thickness of the composite blank.

[0091] Preferably, in step 3), the pass reduction rate used during rolling is 10-20%.

[0092] In the manufacturing method of the present disclosure:

[0093] 1) Metallurgy: P and S elements degrade the fracture toughness of steel, so low P and S levels are crucial during the smelting process to improve billet quality. Ideally, clean steel production technology should be employed to reduce the gas and inclusion content in the steel, thereby improving the overall performance of the steel, particularly its lamellar tearing resistance.

[0094] 2) Assembly: Preferably, the thickness of the corrosion-resistant layer is 1-10% of the total thickness of the composite billet. The corrosion-resistant layer and base carbon steel billet are pre-treated, and the bonding surfaces of the billet are welded and sealed on all sides. The sealed bonding surfaces are then vacuumed. Vacuuming protects the surface of the corrosion-resistant layer from oxidation and is an important factor in ensuring the corrosion-resistant layer's resistance to corrosion in the splash zone.

[0095] 3) Heating: For single carbon steel, the slab heating temperature is generally controlled between 1000 and 1250°C, which is conducive to the dissolution and full diffusion of precipitates in the steel, promotes the homogenization of slab elements, and exerts the strengthening effect of microalloying elements in the steel. For single industrial pure titanium plates, the heating temperature is generally controlled between 850 and 1000°C. Heating temperatures that are too high will produce β phase transformation, and the β phase will grow rapidly, degrading the performance of industrial pure titanium. High heating temperatures allow for full diffusion of elements, promoting the subsequent 100% metallurgical bonding of the interface. However, excessively high heating temperatures increase the tendency of austenite grains to coarsen, increasing the difficulty of subsequent controlled rolling. More importantly, they accelerate the diffusion of C, N, Ti, and Fe to the interface, forming thick brittle precipitates and intermetallic compounds at the interface, forming a thick interface transition layer, and degrading the interface shear strength. Taking all the above factors into consideration, the method disclosed herein controls the heating temperature between 900 and 1000°C.

[0096] 4) Rolling: The rough rolling temperature is controlled at above 880°C. High reduction rates are applied in the high-temperature zone to fully recrystallize the structure, refine the grains, and improve the material's strength and toughness. The pass reduction rate is maintained at 5-20%, with a cumulative reduction rate of ≥88%. Controlled rolling is performed in the non-recrystallized zone, where no austenite recrystallization occurs. Reasonable reduction rates and final rolling temperatures are used to accumulate deformation energy and deformation dislocations, forming high-density deformation bands within the austenite grains. This increases phase deformation nuclei, further refines the effective grain size after the matrix phase transformation, and improves the material's strength and toughness. Simultaneously, deformation-induced precipitation of Nb, Ti, and Cr carbonitrides at this stage enhances the matrix's strength, inhibits the diffusion of C to the interface, and prevents the formation of excessively thick TiC at the interface, which degrades the interfacial shear strength. Preferably, the finishing rolling temperature is controlled between 760°C and 850°C to achieve granular bainite and / or lath bainite with an effective grain size of less than 10 μm while maintaining the corrosion resistance of titanium. During the rolling process, the corrosion-resistant layer and the base layer undergo only metallurgical bonding and necessary dimensional changes, without any compositional changes between the corrosion-resistant layer and the base layer.

[0097] 5) Cooling: By controlling the initial cooling, final cooling, and cooling rate, the type and size of the post-rolling microstructure can be controlled. Excessively fast cooling rates will form martensite. Martensite has low toughness and a high yield ratio, which is detrimental to the performance of the steel plate. Excessively slow cooling rates will result in the formation of a large amount of coarse ferrite. Coarse ferrite promotes crack propagation, resulting in a decrease in impact properties. Therefore, the cooling rate should be reasonably controlled. Controlling the final rolling temperature during finishing can prevent the formation of ferrite and reduce the strength of the base layer. At the same time, rapid cooling to the phase transformation temperature after rolling further inhibits microstructure growth, thereby improving material strength and low-temperature impact toughness through grain refinement. Preferably, water cooling is used, with a cooling rate controlled between 10 and 25°C / s and a final cooling temperature between 300 and 450°C to ensure that the base layer has a low yield ratio and high low-temperature impact toughness.

[0098] If the corrosion-resistant layer is too thick, it will affect the mechanical properties of the material and the production cost. If the corrosion-resistant layer is too thin, it will reduce the corrosion resistance and service life of the material. Preferably, the thickness of the corrosion-resistant layer is controlled to be 1-10% of the total thickness of the composite blank during the blank assembly process.

[0099] By combining the corrosion-resistant layer with the base layer, combining the design of their composition and thickness ratio, and rolling the base layer, a corrosion-resistant layer resistant to splash zone corrosion is formed on the surface of the carbon steel plate. The result is the disclosed hot-rolled steel strip for building structures that combines splash zone corrosion resistance with excellent mechanical properties and high economic efficiency. This steel strip can then be processed into structural components for use in splash zone environments.

[0100] Compared with the prior art, the hot-rolled steel strip for building structures disclosed in the present invention has the following beneficial effects:

[0101] The hot-rolled steel strip for building structures disclosed herein is designed with a low-carbon microalloying composition, achieving an excellent combination of titanium and carbon steel without adding a metal isolation layer, and effectively controlling the thickness of the interface transition layer, so that the mechanical properties of the base layer (carbon steel) can meet the corresponding strength level requirements without reducing the corrosion resistance of the corrosion-resistant layer itself, and the base layer has an excellent yield strength ratio and low-temperature impact toughness.

[0102] The hot-rolled steel strip for building structures disclosed herein reduces the carbon content to minimize the formation of TiC compounds in the interfacial transition layer and carbonitrides in the base layer, hindering grain growth and improving the base layer's low-temperature impact toughness. Furthermore, the addition of microalloying elements addresses the issue of low material strength in low-carbon conditions, achieving a base layer yield strength ≥ 500 MPa, a tensile strength ≥ 640 MPa, a yield-to-strength ratio of 0.75 to 0.85, and a -40°C impact energy ≥ 190 J, all exceeding the performance requirements of the Chinese national standard GB / T 19879-2015, "Steel Plates for Building Structures."

[0103] Compared with the steel marine structure disclosed in Japanese patent application JP 2011167002A (which achieves corrosion resistance through painting), the present disclosure achieves 100% metallurgical bonding of the corrosion-resistant layer and the base layer through hot rolling, eliminating the need for painting and achieving a one-time solution.

[0104] Chinese patent application CN201210260231.7 adds a nickel plate as an isolation layer between the cladding layer and the base layer to prevent the formation of TiC at the interface, resulting in a titanium-steel composite plate with an interface bonding ratio of 99.6-100%. In contrast, the hot-rolled steel strip for building structures disclosed herein utilizes a low-carbon and microalloyed design, reducing nickel addition and production costs. Furthermore, through optimized heating and rolling processes, it forms a transition layer with a defined thickness and reduces the formation of brittle TiC in the interface transition layer, achieving a complete metallurgical bond with a 100% interface bonding ratio.

[0105] Chinese patent application CN201710769999.X uses a slab heating temperature of 500-700°C and a total reduction rate of 60-70%. The resulting steel plate has a maximum interfacial shear strength of 182 MPa. In contrast, the inventors fully considered the impact of the high-temperature phase transformation of industrial pure titanium in the corrosion-resistant layer on corrosion resistance and the strength and toughness control of the base carbon steel. Combining low-carbon microalloy design with a global design of the processing technology, they set the heating temperature of the composite slab to 900-1000°C. At this temperature, the corrosion-resistant layer does not undergo phase transformation, ensuring that the precipitates in the base carbon steel are fully dissolved, refining the base grains during controlled rolling and improving the strength and toughness of the base. At the same time, the cumulative reduction rate is controlled to ≥88%, which breaks up the brittle phases in the interface transition layer and improves the interfacial shear strength.

[0106] Chinese patent applications CN201210260231.7 and CN201710769999.X primarily avoid the formation of brittle Ti compounds by adding an additional nickel-based alloy barrier layer between titanium and carbon steel. In contrast, the present invention achieves a complete metallurgical bond with a 100% interfacial bonding ratio through composition and process design without adding a barrier layer. Furthermore, the hot-rolled steel strip for building structures disclosed in the present invention differs from the above two patent applications in its assembly method and the base carbon steel material is also significantly different.

[0107] Through the process conditions disclosed in the present invention, the original corrosion resistance of the industrial pure titanium of the corrosion-resistant layer can be guaranteed, and the mechanical properties of the base layer can be guaranteed, solving the problem that the processing windows of traditional titanium and carbon steel are too different to be taken into account; at the same time, the elements of the base layer and the corrosion-resistant layer are fully diffused to form an interface transition layer no larger than 8μm. The grains of this layer are fine, with an average grain size of 15 to 40μm, and contain (Ti, Nb)C precipitated particles smaller than 120nm, which enhances the interface bonding performance and ensures that the interface shear strength is ≥263MPa, which is much higher than the interface shear strength of 182MPa of Chinese patent application CN201710769999.X.

[0108] The process of Chinese patent application CN201811327623.4 achieves composite by warm rolling, which is followed by a two-stage heat treatment operation, including a primary annealing at 500-600°C for 20-60 minutes and a recrystallization annealing at 680-700°C for 30-120 minutes. It involves a method for preparing composite titanium steel plates that are not hot-rolled and composite, which is completely different from the manufacturing method disclosed herein.

[0109] The heating temperature used in the process of Chinese patent application CN201510543767.3 is 850-900℃, the final rolling temperature is below 700℃, and the deformation of each pass is between 20-30%, the total deformation of rolling is ≥90%, and the shear strength of the titanium steel composite plate is greater than 240MPa. The pass reduction and total deformation required by this patent application are both very high, which can easily cause edge weld cracking during the rolling process, destroy the vacuum degree, make it difficult to composite, and have poor rolling stability. In contrast, the single-pass reduction rate of the present invention is controlled at 5-20%, which can effectively control the weld from cracking during the rolling process, ensure the vacuum degree inside the slab, and improve the interface shear strength and the stability and success rate of rolling.

[0110] Chinese patent application CN201610994234.1 relates to a method for producing titanium-steel composite plates. First, titanium plates and steel plates are assembled to form a symmetrical multi-layer composite billet of steel plate-titanium plate-isolator-titanium plate-steel plate. The billet is then compounded by rolling or explosive compounding. The compounded billet is annealed and pickled in a continuous annealing and pickling line. It is first heated to 500-750°C to recrystallize the core titanium plate, and then heated to 950-1050°C to recrystallize the base steel plate. However, the patent application does not specifically clarify the rolling process and the corrosion and structural properties of the obtained steel plate. The process of the patent application is significantly different from the method disclosed in the present invention in terms of manufacturing process. The method disclosed in the present invention does not require a two-stage heat treatment, which avoids the excessive diffusion of titanium, iron and carbon elements, the production of brittle intermetallic compounds of iron and titanium carbide, and the degradation of interface shear strength.

[0111] The titanium-steel composite plate disclosed in Chinese patent application CN201710996925.X features a corrosion-resistant layer made of TA2, with the titanium cladding layer having a thickness of 0.2 to 1 mm. The manufacturing process is as follows: the sealed welded composite billet is heated to 900 to 920°C for insulation, then rolled at a starting temperature of 880 to 900°C, finished at a temperature above 800°C, and air-cooled to room temperature. The resulting composite plate has a shear strength of 241 MPa. In contrast, the method disclosed herein employs a heating temperature of 900 to 1000°C, a finishing temperature of 780 to 850°C, and water cooling with a controlled cooling rate of 10 to 25°C / s. The disclosed method can produce hot-rolled plates with TA1, TA2, TA3, and TA4 as corrosion-resistant layers, with the corrosion-resistant layer comprising 1 to 10% of the total thickness of the composite billet, and an interfacial shear strength of 263 MPa or greater.

[0112] The process disclosed in Chinese patent application CN201710983322.6 uses a similar assembly and heating process to that of Chinese patent application CN201710996925.X. The reduction rate per pass is 25-30%, and the total reduction rate is ≥85%. While controlling the reduction rate per pass and the total reduction rate, the thickness of the titanium-steel composite plate is limited to 3-16 mm. The final rolling temperature is above 800°C, followed by air cooling to room temperature. The titanium-steel composite plate is surface treated to produce a titanium cladding layer thickness of ≤1 mm, and the steel plate strength is approximately 345 MPa, which is insufficient for applications in higher-strength structural components. In contrast, the process disclosed herein uses a single-pass reduction rate of 5-20% to control rolling stability. Through composition and process design, the material yield strength can reach over 500 MPa. Furthermore, the process disclosed herein differs significantly from the process disclosed in Chinese patent application CN201710983322.6 in terms of corrosion-resistant layer thickness and total composite strip thickness.

[0113] The hot-rolled steel strip for building structures disclosed herein can address the challenges faced when using stainless steel or carbon steel in wave splash zones. It can be effectively applied to the manufacture of steel structures used in wave splash zones, such as those found in harbors, docks, offshore oil platforms, and other facilities. This hot-rolled steel strip for building structures can meet the corrosion resistance and mechanical performance requirements of these components in wave splash zones, significantly improving their applicability, safety, and durability, and offering significant economic and social benefits.

[0114] Example

[0115] The technical solutions of the present disclosure are further described in detail below with reference to the examples and accompanying drawings. It should be understood that the following examples are merely illustrative of specific embodiments of the present disclosure and do not constitute any limitation on the scope of protection of the present disclosure. All reagents used in the examples are commercially available. Experimental methods in the examples where specific conditions are not specified were performed according to conventional conditions known in the art or according to the conditions recommended by the manufacturer.

[0116] 1 , 2 and 4 , which show schematic diagrams of two interlayer structures of the hot-rolled steel strip for building structures disclosed herein, wherein 1 is a base layer, 2 is a corrosion-resistant layer, and 3 is an interface transition layer.

[0117] The compositions of the base layer and the corrosion-resistant layer of Examples 1-8 and Comparative Examples 1-5 are shown in Table 1. Examples 1-8 and Comparative Examples 1-5 were prepared by the following steps:

[0118] 1) Smelting and casting

[0119] According to the compositions of the base layer and the corrosion-resistant layer shown in Table 1, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively;

[0120] 2) Assembly

[0121] The base blank and the corrosion-resistant layer blank are ground and polished, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are vacuumed;

[0122] 3) heating and rolling the composite billet to form a steel strip, wherein:

[0123] heating the composite blank to 900-1000° C.;

[0124] The rough rolling temperature is ≥880°C; the finishing rolling temperature is 760-850°C, preferably 780-850°C; the pass reduction rate is 5-20%, preferably 10-20%; the cumulative reduction rate is ≥88%;

[0125] 4) Cooling

[0126] After leaving the rolling mill stand, the steel strip is cooled to 300-450°C at a cooling rate of 10-25°C / s, and then coiled at this temperature to produce hot-rolled strip steel.

[0127] The specific parameters of the manufacturing process of Examples 1-8 and Comparative Examples 1-5 are shown in Table 2.

[0128] Then, performance tests were performed on the base layer, base layer, and composite steel plates of Examples 1-8 and Comparative Examples 1-5. Yield strength and tensile strength were measured in accordance with GB / T 6396-2008, "Mechanical and Processing Properties of Composite Steel Plates," and GB / T 228-2010, "Metallic Materials Room Temperature Tensile Test Methods." -40°C impact energy (KV2 / J) (longitudinal) was measured in accordance with GB / T 6396-2008, "Mechanical and Processing Properties of Composite Steel Plates," and GB / T 229-2020, "Metallic Materials Charpy Pendulum Impact Test Methods." Grain size rating was performed as follows: Ferrite structures in stainless steel and carbon steel were graded using the intercept method according to GB / T 6394-2017, "Method for Determination of Average Grain Size of Metals."

[0129] The metallographic structures and mechanical properties of the base layer and the corrosion-resistant layer, and the thickness and mechanical properties of the interface transition layer in the composite steel plates of Examples 1-8 and Comparative Examples 1-5 are shown in Table 3.

[0130] Figure 3 shows the metallographic structure of the corrosion-resistant layer of Example 3. As shown in Figure 3 , the metallographic structure of the corrosion-resistant layer of Example 3 is a single, equiaxed α-Ti with an average grain size of 105.6 μm.

[0131] Figure 4 shows the interface transition layer of Example 3. As shown in Figure 4 , the thickness of the interface transition layer 3 is 6.9 μm, and the discontinuous fine particles therein are TiC with a size of less than 120 nm.

[0132] Figure 5 shows the metallographic structure of the base layer of Example 3. As shown in Figure 5 , the metallographic structure of the base layer carbon steel of Example 3 is granular bainite and lath martensite.

[0133] Furthermore, the corrosion resistance of the composite steel plates of Examples 1-8 and Comparative Examples 1-5 was tested, and the results are shown in Table 4. The corrosion resistance was specifically tested as follows: Coupon specimens of the composite steel plates of Examples 1-8 and Comparative Examples 1-5 were placed in the wave splash zone of the South China Sea (selected at different placement locations, namely, Scenes 1 to 8) for 6 months, and the corrosion conditions were observed and recorded.

[0134] Comparative Examples 1-5 use unqualified composition design and thermal processing conditions, resulting in certain properties of the composite steel plates failing to meet the use requirements (performance parameters are not within the scope of the invention).

[0135] The Cr content of Comparative Example 1 is too high and does not meet the composition formula (0.9%≤Cu+Ni≤1.45% and 2(C+N)≤Ti+Nb+Cr+Mo≤1.90%), which cannot effectively hinder the formation of carbides. The thickness of the interface transition layer is too thick, the bonding strength is insufficient, and the corrosion resistance is poor.

[0136] The Al content of Comparative Example 2 is not within the range defined by the present invention, and the finishing temperature and cooling rate are not within the range defined by the present invention. The grains are coarse, the impact properties thereof cannot meet the requirements, and the corrosion resistance is poor.

[0137] The Cr content of Comparative Example 3 is too high, and the coiling temperature is not within the range defined by the present invention, so its yield strength and tensile strength cannot meet the requirements.

[0138] The Al content and Cu content of Comparative Example 4 are not within the range defined by the present invention, and the cumulative reduction rate is not within the range defined by the present invention. Its tensile strength, yield strength ratio and impact properties cannot meet the requirements, and its corrosion resistance is poor.

[0139] The heating temperature, finishing rolling temperature and cooling rate of Comparative Example 5 are not within the range defined by the present invention. Since the heating temperature is too high, β-Ti cannot be completely eliminated during the subsequent processing and cooling process, and the corrosion rate is too high.

[0140] In comparison, the base yield strength of Examples 1-8 is ≥500 MPa, the tensile strength is ≥640 MPa, the yield strength ratio is 0.75-0.85, the impact energy at -40°C is ≥190 J, and the corrosion rate of the corrosion-resistant layer against sea wave splash is ≤0.006 mm / year.

[0141] It should be noted that the combination of the various technical features in the present disclosure is not limited to the combination described in the claims or the combination in the embodiments. All technical features described in the present disclosure can be freely combined or combined in any way unless there is a contradiction between them.

[0142] It should be noted that the embodiments listed above are only specific examples of the present disclosure. Obviously, the present disclosure is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily associated with the contents of the present disclosure by those skilled in the art should fall within the scope of protection of the present disclosure.

Claims

1. A hot-rolled steel strip for building structures, It is characterized in that The hot-rolled steel strip comprises a base layer, a corrosion-resistant layer, and an interface transition layer between the base layer and the corrosion-resistant layer; In addition to Fe and other inevitable impurities, the base layer also contains the following chemical elements in the following mass percentages: C: 0.050-0.100%, Si: 0.15-0.30%, Mn: 1.0-1.8%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.80-1.60%, Ni: 0.50-1.20%, Cu: 0.20-0.40%, Al: 0.020-0.050%, Ti: 0.010-0.018%, Nb: 0.020-0.100%, N: 0.0005-0.0050%, Mo: 0.20-0.50%; The corrosion-resistant layer is made of industrial pure titanium, preferably TA1, TA2, TA3 or TA4.

2. The hot-rolled steel strip for building structure according to claim 1, It is characterized in that The chemical composition of the base layer also satisfies the following relationship: 0.9%≤Cu+Ni≤1.45%; 2(C+N)≤Ti+Nb+Cr+Mo≤1.90%.

3. The hot-rolled steel strip for building structure according to claim 1 or 2, It is characterized in that The mass percentage of each chemical element of the base layer is: C: 0.050-0.100%, Si: 0.15-0.30%, Mn: 1.0-1.8%, P: 0.0005-0.003%, S: 0.0005-0.01%, Cr: 0.80-1.60%, Ni: 0.50-1.20%, Cu: 0.20-0.40%, Al: 0.020-0.050%, Ti: 0.010-0.018%, Nb: 0.020-0.100%, N: 0.0005-0.0050%, Mo: 0.20-0.50%, and the balance is Fe and other inevitable impurities.

4. The hot rolled steel strip for building structure according to any one of claims 1 to 3, It is characterized in that The microstructure of the base layer is granular bainite and / or lath bainite, and the effective grain size is ≤10 μm.

5. The hot rolled steel strip for building structure according to any one of claims 1 to 4, It is characterized in that The yield strength of the base layer is ≥500MPa, the tensile strength is ≥640MPa, the yield strength ratio is 0.75-0.85, and the impact energy at -40°C is ≥190J.

6. The hot rolled steel strip for building structure according to any one of claims 1 to 5, It is characterized in that The microstructure of the corrosion-resistant layer is single, equiaxed α-Ti.

7. The hot rolled steel strip for building structure according to any one of claims 1 to 6, It is characterized in that The sea wave splash corrosion resistance rate of the corrosion resistant layer is ≤0.006mm / year.

8. The hot rolled steel strip for building structure according to any one of claims 1 to 7, It is characterized in that The thickness of the interface transition layer is ≤8 μm, the average grain size is 15-40 μm, and it contains precipitated particles of (Ti, Nb)C less than 120 nm, and the interface shear strength is ≥263 MPa.

9. The hot rolled steel strip for building structure according to any one of claims 1 to 8, It is characterized in that The thickness of the hot-rolled steel strip is 3 to 16 mm.

10. The hot rolled steel strip for building structure according to any one of claims 1 to 9, It is characterized in that The hot-rolled strip has a base yield strength of ≥500MPa, a tensile strength of ≥640MPa, a yield strength ratio of 0.75-0.85, an impact energy of ≥190J at -40°C, a sea wave splash corrosion rate of the corrosion-resistant layer of ≤0.006mm / year, and an interface shear strength of ≥263MPa.

11. A method for manufacturing the hot rolled steel strip for building structures according to any one of claims 1 to 10, It is characterized in that The method comprises the following steps performed in sequence: 1) Smelting and casting According to the composition of the base layer and the corrosion-resistant layer as described in any one of claims 1 to 3, the base layer and the corrosion-resistant layer are smelted and cast into billets respectively; 2) Assembly The base blank and the corrosion-resistant layer blank are subjected to surface grinding and polishing, and the bonding surfaces of the blanks are welded and sealed on all sides to form a composite blank including the base and the corrosion-resistant layer; the bonding surfaces after welding and sealing are subjected to vacuum treatment; 3) heating and rolling the composite billet to form a steel strip, wherein: The composite blank is heated to 900-1000° C.; The rough rolling temperature is ≥880°C; the finishing rolling temperature is 760-850°C, preferably 780-850°C; the pass reduction rate is 5-20%, preferably 10-20%; the cumulative reduction rate is ≥88%; 4) Cooling After the steel strip leaves the rolling mill stand, it is cooled to 300-450°C at a cooling rate of 10-25°C / s, and then coiled at this temperature to produce hot-rolled strip steel.

12. The method according to claim 11, It is characterized in that In step 2), the thickness of the corrosion-resistant layer is 1-10% of the thickness of the composite blank; and / or in step 3), the thickness of the interface transition layer formed between the base layer and the corrosion-resistant layer is ≤8 μm.

Citation Information

Patent Citations

  • Manufacturing method of titanium-steel-titanium two-sided composite plate

    CN102773670A

  • Preparation method of titanium-steel clad plate

    CN105107841A

  • Production method of titanium-steel composite plate

    CN106269963A

  • A method for preparing titanium-steel composite plates

    CN107626764B

  • A titanium-steel-titanium composite plate and its preparation method

    CN109304367B

Cited By

  • Production method of low-residual-stress steel plate for ship and ocean engineering

    CN120945290A