Method for producing lithium-metal composition oxide

The method of continuously fluidizing and collecting scattered powder in a rotary kiln with scraping blades and decarbonizing cooling ensures better lithium-metal composite oxide production, addressing yield and compositional issues, and enhancing battery performance.

WO2024245785A1PCT designated stage expired Publication Date: 2024-12-05BASF SE

Patent Information

Application Number
PCT/EP2024/063684
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-17
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The production of lithium-metal composite oxides in rotary kilns faces challenges due to gas flow causing scattered powder loss and compositional variations, leading to reduced yield and quality, and the use of refrigerant gases can result in carbonation of lithium compounds, affecting the lithiation reaction and battery performance.

Method used

A method involving a firing step with a continuously fluidized mixture of precursor and lithium compounds, collection of scattered powder from exhaust gas, and controlled mixing to maintain the Li/(Ni+M) ratio, using a rotary kiln with scraping blades and decarbonizing cooling to prevent corrosion and ensure efficient thermal conduction.

Benefits of technology

This method enhances the yield and quality of lithium-metal composite oxides, maintaining the desired composition and preventing lithium carbonate formation, thus improving battery characteristics without loss of quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024063684_05122024_PF_FP_ABST
    Figure EP2024063684_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a lithium-metal composite oxide of the present disclosure comprises: a firing step, in which a powdered mixture, comprising a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised; a collecting step, in which collected powder is obtained by cooling an exhaust gas that contains scattered powder that has been produced by the fluidisation of the powdered mixture in the firing step, and collecting the scattered powder contained in the exhaust gas; and a mixing step, in which a powdered mixture is obtained in the form of a mixture of at least the precursor compound, the lithium compound, and the collected powder.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR PRODUCING LITHIUM-METAL COMPOSITION OXIDE

[0002] TECHNICAL FIELD

[0003] The present disclosure relates to a method for producing a lithium-metal composite oxide.

[0004] BACKGROUND

[0005] Nonaqueous electrolyte secondary batteries, which are compact and lightweight, and have a high energy density, are used as power sources for operating cellular telephones and notebook personal computers, for example. These include widely used lithium ion secondary batteries that have a large charging / discharging capacity and that utilize materials such as lithium nickel oxide in the positive electrode.

[0006] Lithium-metal composite oxides of the general formula Li(NiM)C>2 (where M is an element including, for example, a transition metal) are used, for example, as the positive electrode active material for lithium ion secondary batteries. Raw material powders of transition metal-containing precursor compounds and lithium compounds can commonly be fired to produce these sorts of lithium-metal composite oxides.

[0007] A firing vessel such as a sagger or crucible can be filled with the raw material powders, and conditions such as temperature and time can be adjusted, as appropriate, to fire the raw material powders, more than once, as needed, in a furnace such as an electric furnace or roller hearth kiln. However, rather than these types of furnaces, attempts have been made to use equipment in which, for example, the raw material powders are fired while fluidised, such as externally heated rotary kilns, because of the higher and more efficient thermal conduction to the powder mixture that is being treated.

[0008] When raw material powder is fired using a rotary kiln, the powder mixture gradually being fed into the furnace is usually fluidised while being scraped and stirred, and is heated by a heater through the furnace wall.

[0009] At that time, a gas stream may be introduced from outside the rotary kiln in order to allow gas containing carbon dioxide or steam that results in impurities inside the furnace to be discharged out of the furnace, and to maintain the desired oxidizing atmosphere inside the furnace. However, the flow of gas into the rotary kiln ends up causing the raw material powder to float inside the rotary kiln, and some is furthermore swept away by the flow of gas inside the furnace and ends up being discharged out of the rotary kiln system. Because of this phenomenon, there is concern that the yield and quality of the final fired product (lithium-metal composite oxide) may be compromised.

[0010] The scattered powder that is thus discharged from the rotary kiln can be collected using a collector. In the method for producing a lithium-metal composite oxide that is disclose in Patent Document 1 , for example, a rotary kiln is used to fire the raw material powder. In the rotary kiln, a dust collector is placed between a raw material powder feed port and a rotating cylinder that serves as the firing furnace. The scattered powder that has been scattered as noted above is collected by the dust collector as a result of the flow of the gas introduced from the discharge end of the rotary kiln as well as the airflow generated by the dust collector, and is then discharged to the feed port, for example, and then reintroduced into the rotary cylinder.

[0011] SUMMARY OF THE INVENTION

[0012] The present invention provides a method for producing a lithium-metal composite oxide, comprising: a firing step, in which a powdered mixture, comprising a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised; a collecting step, in which collected powder is obtained by cooling an exhaust gas that contains scattered powder that has been produced by the fluidisation of the powdered mixture in the firing step, and collecting the scattered powder contained in the exhaust gas; and a mixing step, in which the powdered mixture is obtained in the form of a mixture of at least the precursor compound, the lithium compound, and the collected powder.

[0013] The present disclosure provides a method for producing a lithium-metal composite oxide that can serve as the positive electrode active material for a nonaqueous electrolyte secondary battery to provide better battery characteristics without any loss of quality.

[0014] DETAILED DESCRIPTION OF THE INVENTION

[0015] As disclosed in Patent Document 1 , when the scattered powder is collected by the dust collector and is then reintroduced into the rotary cylinder to be fired together with the raw material powder in the rotary cylinder, the decrease in the yield of the lithium-metal composite oxide that is obtained can be controlled to a certain extent.

[0016] However, the composition of the scattered powder is different from the composition of the target lithium-metal composite oxide, that is, the composition of the raw material. Specifically, in cases where the lithium metal composite oxide is represented by the above general formula Li(NiM)C>2 (where M is an element including, for example, a transition metal), the amount of Li relative to the total amount of Ni and M (Li / (Ni+M) ratio) tends to be smaller than in the raw material powder. Accordingly, when the scattered powder is reintroduced as such into the furnace, components with a greater Li / (Ni+M) ratio and components with a smaller Li / (N i+M) ratio will occur, resulting in a positive electrode active material that has an irregular composition. The temperature inside the furnace also needs to be increased in order to achieve more efficient firing in the rotary kiln and to ensure that the positive electrode active material is of good quality. However, this also results in a higher exhaust gas temperature, which can sometimes be as high as around 400°C. Thus, when the scattered powder is collected, it can be difficult to collect the scattered powder using a dust collector unless the length of the piping is extended using a high temperature- resistant material as the exhaust piping, or unless the exhaust piping is cooled by heat exchange with cooling water, for example, or unless the exhaust gas is cooled by being sprayed with a refrigerant gas. Depending on the type of raw material, the scattered powder may also become strongly alkaline, leading to the degradation, i.e. , corrosion, of the equipment.

[0017] The cooling method using the refrigerant gas noted above is economical, easy to control, and more productive, and is thus more suitable than other cooling methods. However, in cases where the refrigerant gas contains carbon dioxide and the lithium compound used in the powder mixture is lithium hydroxide, the Li component will become carbonated during the cooling process, resulting in the formation of a less reactive lithium carbonate and in less reaction of lithium. This results in changes in the raw material composition that are not suitable for the intended lithium-metal composite oxide. The lithiation reaction also will not progress enough during firing, leading to increases in the amount of lithium carbonate remaining in the resulting lithium-metal composite oxide as well as to poor battery performance in lithium ion secondary batteries in which the material is used as the positive electrode active material.

[0018] Simply continuing the firing process while reintroducing the scattered powder that has been collected in the dust collector into the rotary cylinder results in problems such as a loss of quality in the lithium-metal composite oxide that is obtained as well as deterioration of the collector.

[0019] In light of the circumstances noted above, the present disclosure is intended to provide a method for producing a lithium-metal composite oxide that, when used as a positive electrode active material for a nonaqueous electrolyte secondary battery, can ensure better battery characteristics, without any loss of quality.

[0020] The inventors engaged in extensive research to solve the problems noted above. As a result, the inventors discovered it was possible to provide a method for producing a lithium-metal composite oxide that, when used as a positive electrode active material for a nonaqueous electrolyte secondary battery, can ensure better battery characteristics, without any loss of quality, wherein said method for producing a lithium- metal composite oxide, comprises: a firing step, in which a powdered mixture, comprising a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised; a collecting step, in which collected powder is obtained by cooling an exhaust gas that contains scattered powder that has been produced by the fluidisation of the powdered mixture in the firing step, and collecting the scattered powder contained in the exhaust gas; and a mixing step, in which a powdered mixture is obtained in the form of a mixture of at least the precursor compound, the lithium compound, and the collected powder. Specifically, the present disclosure provides the following.

[0021] (1) A method for producing a lithium-metal composite oxide, comprising: a firing step, in which a powdered mixture, comprising a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised; a collecting step, in which collected powder is obtained by cooling an exhaust gas that contains scattered powder that has been produced by the fluidisation of the powdered mixture in the firing step, and collecting the scattered powder contained in the exhaust gas; and a mixing step, in which the powdered mixture is obtained in the form of a mixture of at least the precursor compound, the lithium compound, and the collected powder.

[0022] (2) The method for producing a lithium-metal composite oxide according to (1), wherein the powdered mixture is furthermore a mixture with a doping source compound and / or a coating source compound.

[0023] (3) The method for producing a lithium-metal composite oxide according according to (1) or (2), wherein the powdered mixture is prepared by controlling the mass ratio represented in either (a) or (b) below to 2:98 to 40:60:

[0024] (a) mass ratio of the amount of the collected powder to the total amount of the precursor compound and the lithium compound

[0025] (b) mass ratio of the amount of the collected powder to the amount of the powdered mixture.

[0026] (4) The method for producing a lithium-metal composite oxide according to (1) or (2), wherein a rotary kiln equipped with scraping blades on the surface inside the furnace core tube is used in the firing step to carry out scraped stirring, where the material being fired in the furnace core tube is stirred while scraped.

[0027] (5) The method for producing a lithium-metal composite oxide according to (4), wherein the powdered mixture that has been prepared in advance is introduced into the rotary kiln to carry out the scraped stirring.

[0028] (6) The method for producing a lithium-metal composite oxide according to (4), wherein the exhaust gas is cooled in a decarbonising atmosphere as a temperature over the dew point temperature of the system containing the exhaust gas is maintained. (7) The method for producing a lithium-metal composite oxide according to (1) or (2), wherein the lithium compound is lithium carbonate, the precursor compounds is a hydroxide, and the exhaust gas is cooled as a temperature over the dew point temperature of the system containing the exhaust gas is maintained.

[0029] (8) The method for producing a lithium-metal composite oxide according to (1) or (2), wherein the firing temperature in the firing step is 400°C to under 700°C, and the method further comprises a second firing step after the above firing step, wherein the fired material obtained in the above firing step is further fired at a temperature of 700°C to 1000°C.

[0030] The present disclosure can provide a method for producing a lithium-metal composite oxide that can serve as the positive electrode active material for a nonaqueous electrolyte secondary battery to provide better battery characteristics without any loss of quality.

[0031] BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Fig. 1 is a schematic radial cross-sectional view of the furnace core tube of a rotary kiln which can be used in the method for producing a lithium-metal composite oxide.

[0033] Fig. 2 is a schematic radial cross-sectional view of the furnace core tube of the rotary kiln used in the examples, comparative examples, and reference examples.

[0034] Fig. 3 is a flowchart (flow a) of the method for producing the positive electrode active material of Example 1-1.

[0035] Fig. 4 is a flowchart (flow P) of the method for producing the positive electrode active material of Example 1-2.

[0036] Fig. 5 is a flowchart (flow y) of the method for producing the positive electrode active material of Reference Example 1-1.

[0037] Fig. 6 is a flowchart (flow 5) of the method for producing the positive electrode active material of Comparative Example 1-1.

[0038] Fig. 7 is a flowchart (flow E) of the method for producing the positive electrode active material of Comparative Example 1-2.

[0039] Fig. 8 is a flowchart (flow Q of the method for producing the positive electrode active material of Example 2-1.

[0040] Fig. 9 is a flowchart (flow q) of the method for producing the positive electrode active material of Comparative Example 2-1.

[0041] Fig. 10 is a flowchart (flow i) of the method for producing the positive electrode active material of Comparative Example 2-2.

[0042] EMBODIMENTS

[0043] Embodiments of the present disclosure are described below, but the present disclosure is not limited in any way by the description of the embodiments and can be worked with additional modifications, as appropriate. <Method for Producing Lithium-Metal Composite Oxide>

[0044] The method for producing a lithium-metal composite oxide in an embodiment of the present disclosure comprises: a firing step, in which a powdered mixture, comprising a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised; a collecting step, in which collected powder is obtained by cooling an exhaust gas that contains scattered powder that has been produced by the fluidisation of the powdered mixture in the firing step, and collecting the scattered powder contained in the exhaust gas; and a mixing step, in which a powdered mixture is obtained in the form of a mixture of at least the precursor compound, the lithium compound, and the collected powder.

[0045] In order to efficiently produce a lithium-metal composite oxide as a positive electrode active material for nonaqueous electrolyte secondary batteries, at least the precursor compound and lithium compound raw material powders are preferably fired while continuously fluidised, rather than being allowed to stand, so as to ensure greater thermal conductivity from the firing equipment. However, when the raw material powder is fluidised, the flow of externally introduced gas tends to cause the raw material powder to float, and some of the raw material powder is swept away in the form of scattered powder by the flow of gas inside the furnace and ends up being discharged out of the system. This compromises the yield and quality of the resulting lithium-metal composite oxide.

[0046] The loss of lithium-metal composite oxide yield can be curbed to some extent by firing the raw materials as the scattered powder that is discharged out of the system is collected and is re-introduced to be fluidised again. However, as noted above, the amount of lithium in the composition of the scattered powder tends to be lower than in the composition of the fluidised powder mixture. Compositional variation in the system therefore cannot be curbed when the scattered powder that has been collected is fluidised as such along with the starting material powder. The temperature of the exhaust gas containing the scattered powder is also elevated, and attempts to collect the scattered powder at that temperature will therefore result in the corrosion of the collector. It is thus important to prevent compositional variation between the collected scattered powder and the fluidised powder mixture in order to preserve the quality of the intended lithium-metal composite oxide and to protect the recycling equipment against corrosion.

[0047] Each of the steps in the method for producing a lithium-metal composite oxide in the present disclosure are discussed below.

[0048] In the firing step, a powdered mixture, comprising a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised. The powdered mixture that is fired in the firing step is prepared by mixing at least a precursor compound of a lithium metal composite oxide, a lithium compound, and collected powder.

[0049] Among these, the precursor compound is, for example, a compound composed of at least one element (M) and oxygen (O). Specific examples of compounds that can be used include hydroxides containing the element M, oxides obtained by firing the hydroxides, and carbonate compounds (metal hydroxides, metal oxides, and carbonates, for example, when the element M is a metal). As two or more elements M can be selected, in such cases, the hydroxides, oxides, and carbonate compounds of each element M can be used while mixed, and composite hydroxides and composite oxides (metal composite hydroxides, metal composite oxides, and composite carbonates when the elements M are metals) can also be used.

[0050] The element M is not particularly limited, provided that it is an element other than Li and allows a lithium-metal composite compound to be formed. Specifically, the element M can be selected as befits the composition of the target lithium-metal composite oxide, where examples that can be used include nickel (Ni), cobalt (Co), manganese (Mn), magnesium (Mg), aluminum (Al), titanium (Ti), zinc (Zn), niobium (Nb), tungsten (W), molybdenum (Mo), vanadium (V), chromium (Cr), calcium (Ca), iron (Fe), gallium (Ga), strontium (Sr), yttrium (Y), ruthenium (Ru), indium (In), tin (Sn), tantalum (Ta), bismuth (Bi), zirconium (Zr), boron (B), and phosphorus (P). A composite hydroxide, composite oxide, or composite carbonate, for example, that contains at least Ni, is preferably used as the precursor compound, and the use of a composite hydroxide, composite oxide, or composite carbonate, for example, that contains at least Ni, Co, and Al and / or Mn, for example, is even more preferred.

[0051] Examples of methods that can be used to synthesize the precursor compound include, but are not particularly limited to, methods of synthesis such as the following: methods in which at least one aqueous solution of at least one element M or compound thereof is first prepared as befits the intended lithium-metal composite oxide composition, and the blending ratio is adjusted, as needed; the solution is then added drop-wise into a reaction tank in which, for example, one or more alkali aqueous solutions, such as a sodium hydroxide aqueous solution or ammonia solution, are being stirred as the mother liquor, the pH is adjusted to within the range of 10.5 to 13, for example, and coprecipitation is brought about by means of a crystallization reaction to obtain a hydroxide, oxide, or carbonate, for example. The configuration of the hydroxide, oxide, or carbonate, for example, is not particularly limited, but is preferably in the form of secondary particles that have been formed via the aggregation of a plurality of primary particles.

[0052] Examples of element M compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of nickel compounds, cobalt compounds, manganese compounds, magnesium compounds, aluminum compounds, titanium compounds, zinc compounds, niobium compounds, and tungsten compounds.

[0053] Examples of nickel compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of nickel sulphate, nickel oxide, nickel hydroxide, nickel nitrate, nickel carbonate, nickel chloride, nickel iodide, and metallic nickel.

[0054] Examples of cobalt compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of cobalt sulphate, cobalt oxide, cobalt hydroxide, cobalt nitrate, cobalt carbonate, cobalt chloride, cobalt iodide, and metallic cobalt.

[0055] Examples of manganese compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of manganese sulphate, manganese oxide, manganese hydroxide, manganese nitrate, manganese carbonate, manganese chloride, manganese iodide, and metallic manganese.

[0056] Examples of magnesium compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of magnesium sulphate, magnesium oxide, magnesium hydroxide, magnesium nitrate, magnesium carbonate, magnesium chloride, magnesium iodide, and metallic magnesium.

[0057] Examples of aluminum compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of aluminum sulphate, aluminum oxide, aluminum hydroxide, aluminum nitrate, aluminum carbonate, aluminum chloride, aluminum iodide, sodium aluminate, and metallic aluminum.

[0058] Examples of titanium compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of titanyl sulphate, titanium oxide, titanium hydroxide, titanium nitrate, titanium carbonate, titanium chloride, titanium iodide, and metallic titanium.

[0059] Examples of zinc compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of zinc sulphate, zinc oxide, zinc hydroxide, zinc nitrate, zinc carbonate, zinc chloride, zinc iodide, and metallic zinc.

[0060] Examples of niobium compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of niobium oxide, niobium chloride, lithium niobate, and niobium iodide. Examples of tungsten compounds that can be used include, but are not particularly limited to, one or more selected from the group consisting of tungsten oxide, sodium tungstate, ammonium para-tungstate, tungsten hexacarbonyl, and tungsten sulphide.

[0061] The type of element M compounds and the amounts in which they are blended can be adjusted, in view of the composition of the target lithium-metal composite oxide, to ensure that the various elements are evenly dispersed in the secondary particles.

[0062] The precursor composite compound obtained by means of a wet reaction can also be subjected to a washing treatment and then a drying treatment after de-watering. A washing treatment will make it possible to wash out impurities such as sulphate radicals or carbonate radicals and Na fractions that have been incorporated into agglomerated particles or that have become stuck on the surface layer during the reaction. The drying treatment can also be carried out in an oxidizing atmosphere at a temperature of 50°C to 250°C, for example.

[0063] The precursor compound can also be subjected to an oxidation treatment in an oxidizing atmosphere at a temperature of 300°C to 800°C, for example. The oxidation treatment will allow the precursor compound to be oxidized and will allow impurities such as sulphate radicals or carbonate radicals and sodium fractions to be removed from the precursor compound to increase the purity of the precursor compound. The bulk density of the lithium-metal composite oxide that is obtained can also be increased, and production efficiency can be improved.

[0064] The precursor compound synthesized in this way and a lithium compound are then mixed in a predetermined ratio to prepare a powdered mixture. Examples of methods that can be used to mix the precursor compound and lithium compound include, but are not particularly limited to, methods in which, for example, the precursor compound powder and lithium compound powder are weighed out in prescribed proportions, and are mixed by a dry method using a mixer, for example. The proportions in which the precursor compound and lithium compound are blended can be adjusted to ensure the desired proportions of the total amounts of the Li and element M in the composition of the intended composite lithium-metal composite oxide.

[0065] The lithium compound is not particularly limited, and a variety of lithium salts, for example, can be used. Specific examples of lithium compounds that can be used include one or more selected from the group consisting of lithium hydroxides, such as lithium carbonate, lithium hydroxide hydrate, and anhydrous lithium hydroxide, as well as lithium nitrate, lithium acetate, lithium bromide, lithium chloride, lithium citrate, lithium fluoride, lithium iodide, lithium lactate, lithium oxalate, lithium phosphate, lithium pyruvate, lithium sulphate, and lithium oxide. Preferred examples of lithium compounds that can be used include one or more selected from the group consisting of lithium hydroxides such as lithium carbonate, lithium hydroxide hydrate, and anhydrous lithium hydroxide.

[0066] A doping source compound or coating source compound can also be added, as needed. These compounds can be added when the precursor compound and the lithium compound are mixed. Examples of methods that can be used to add these compounds include, but are not particularly limited to, adding them in the form of a powder or spraying them in the form of a solution. Examples of compounds that can be selected as compounds of elements serving as such additives include, but are not particularly limited to, compounds of elements M.

[0067] In the firing step, a powdered mixture, that comprises a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised.

[0068] When the powdered mixture obtained by the method noted above is fired to produce a fired product in the firing step, the powder mixture is fired while continuously fluidised to ensure that heat is uniformly conducted throughout the powder mixture as a whole.

[0069] Examples of methods for firing the powder mixture in the firing step include, but are not particularly limited to, methods in which the powder mixture may be simply swirled, but a method in which the powder mixture is stirred while scraped is preferably used. A rotary kiln equipped with scraping blades on the surface inside the furnace core tube is preferably used to effect scraped stirring. The use of this type of rotary kiln will allow a fired product to be produced continuously and easily.

[0070] The significance of scraped stirring is discussed below. When the powder mixture is fired while simply fluidised, it is more difficult for the powdered mixture to flow near the furnace wall, resulting in areas that are more readily heated by the furnace wall and areas that are less readily heated, thus leading to the danger of lower quality. However, when the powder mixture is fired while being scraped and stirred, it will be easier for the powder mixture to flow even near the furnace wall, ensuring that firing will progress uniformly.

[0071] Although it will depend on whether or not the powder mixture tends to separate upon falling, when the powder mixture is fluidised by being scraped and stirred, the material should not be scraped up too high relative to the maximum height of the fired material that is not being scraped and stirred, so as to ensure that the material is more efficiently fired while in a highly thermal conductive state and to curb variation in the composition of the fired product.

[0072] The maximum height to which the powder mixture is scraped and stirred is considered to be related to, for example, the particle sizes of the precursor compound and the lithium compound, the ratio of the particle sizes of the two components, the particle size of any added compounds, and the angle of repose of the powder mixture; the height to which the material is scraped can be determined in view of these factors.

[0073] When increasing thermal conduction to the powder mixture via scraping and stirring, consideration should be given to how much heat can be provided to the powder mixture as a whole. For example, when using a rotary kiln equipped with scraping blades on the surface inside the furnace core tube, consideration should be given to how much of the powder mixture can be brought into contact with the surface inside the furnace core tube (also referred to below as the furnace wall). For example, thermal conduction to the powder mixture can be increased by appropriately adjusting the rotary kiln rotating speed and the rate at which the powder mixture is loaded into the rotary kiln.

[0074] However, caution should be exercised to ensure that the powder mixture does not separate when the powder mixture is fluidizing via scraping and stirring. When, for example, a rotary kiln equipped with scraping blades on the surface inside the furnace core tube is used, the angle at which the scraping blades are installed should be appropriately adjusted and the angle of repose of the powder mixture should be appropriately adjusted in view of the relationship between the extent to which the powder mixture is scraped in the furnace and the dead space between the scraping blades and wall.

[0075] When the material is scraped and stirred using a rotary kiln equipped with scraping blades on the surface inside the furnace core tube, the scraping blades should be set up in a direction parallel to the axial direction of the furnace core tube. This will allow the scraping blades to be brought into contact with the furnace wall more efficiently. However, given that thermal conduction to the fired material is to be increased while preventing the powder mixture from separating, as noted above, the angle at which the scraping blades are installed should not be determined by focusing only on efficiently bringing the firing material into contact with the furnace wall.

[0076] If the installation angle of the scraping blades is too great, the scraping blades will be more parallel to the axial direction of the furnace core tube. In that case, more powder will be scattered when the powder mixture is scraped up and falls back. A resulting danger is that the amount of the lithium-metal composite oxide that is obtained will be lower relative to the amount of powder mixture that is introduced, leading to lower productivity and to greater variation in the Li / M ratio of the lithium-metal composite oxide that is obtained On the other hand, if the installation angle of the scraping blades is too low, the scraping blades will be more perpendicular to the axial direction of the furnace core tube. This might result in dead space between the scraping blades and furnace wall and thus a lower contact frequency between the powder mixture and the furnace wall as well as less efficient thermal conduction. Furthermore, when the angle of repose of the powder mixture is taken into consideration, it may not be possible to scrape off much material or to achieve more effective thermal conduction via scraping and stirring.

[0077] Thus, when the powder mixture is scraped and stirred using a rotary kiln equipped with scraping blades on the surface inside the furnace core tube, the installation angle (0 in Fig. 1) of the scraping blades should be, for example, 15 degrees or more, and preferably 20 degrees or more, in the direction perpendicular to the axial direction of the furnace core tube. On the other hand, the installation angle of the scraping blades should be no more than 85 degrees, and preferably no more than 80 degrees.

[0078] Fig. 1 is a schematic radial cross-sectional view of the furnace core tube of a rotary kiln which can be used in the method for producing a lithium-metal composite oxide. The furnace core tube 1 of the rotary kiln in Fig. 1 has a plurality of scraping blades 3 on the surface portion 2, and rotates in the direction of arrow A. The installation angle 0 of the scraping blades 3 is an angle is in the direction perpendicular to the direction of the axis 4 of the furnace core tube 1.

[0079] The number of scraping blades installed on the surface of the furnace core tube is not particularly limited, and should ensure that the contents are sufficiently scraped and stirred according to the retort diameter, for example. For example, three to six scraping blades are preferably installed when the retort diameter is 200 to 700 mm. On the other hand, four to ten scraping blades are preferably installed, for example, when the retort diameter is 1000 to 2000 mm.

[0080] The angle of repose of the powder mixture is preferably enough to allow the mixture to be scraped up to the expected height by the scraping blades, and preferably enough to ensure that the powder mixture does not separate when it is scraped up and falls back.

[0081] An angle of repose that is too great may result in poor powder mixture fluidity when the powder mixture is scraped up and falls back, as well as in less efficient thermal conduction to the powder mixture being scraped and stirred. When the angle of repose of the powder mixture or mixture is too low, a resulting danger is that the scraping and stirring will be less effective in allowing the powder mixture to flow and fall back while being scraped. The angle of repose of the powder mixture is therefore preferably 20° to 80°. The angle of repose of the powder mixture is determined by the injection method.

[0082] The angle of repose of the powder mixture can be determined on the basis of at least the particle sizes of the precursor compound, lithium compound, and collected powder contained therein. The scraping and stirring conditions are not particularly limited, but the following conditions, for example, should preferably be taken into consideration.

[0083] The rotating speed of the retort may be increased as the residence time in the furnace core tube of the rotary kiln is maintained in order to improve the thermal conduction of the powder mixture. However, a retort rotating speed that is too high may result in rapid discharge from the rotary kiln and thus the risk of inadequate progression of firing- induced lithiation and a lithium-metal composite oxide of poor quality. On the other hand, if the retort rotating speed is too low, lithium may adhere to the furnace wall, potentially resulting in compositional variation in the powder mixture that is obtained. The retort rotating speed is therefore preferably adjusted appropriately depending on, for example, the diameter of the furnace (retort diameter). For example, when the retort diameter is 200 to 1500 mm, the retort rotating speed is preferably adjusted to 0.3 to 6.0 rpm.

[0084] The rate at which the powder mixture is loaded into the rotary kiln furnace (percentage expressed as the volume of firing material / inner volume of rotary kiln) can be adjust by varying the gas input rate and residence time of the powder mixture depending on the type of rotary kiln. Of these, the residence time can be adjusted by varying the retort tilt angle and the retort rotating speed. However, a loading rate that is too high will result in a lower retort cross-sectional area and greater air speed, and thus in a greater amount of scattered powder, thereby leading to the risk of lower productivity and a lithium-metal composite oxide of poor quality. On the other hand, a loading rate that is too low may not allow adequate productivity to be achieved. The powdery mixture loading rate should therefore preferably be 2 to 30%, and more preferably 3 to 20%.

[0085] Both furnace air speed and dew point can be adjusted by varying the gas input velocity. A gas input velocity that is too low and a dew point that is too high will result in condensation around the retort feed port through which the powder mixture is introduced. A resulting danger is that the lithium from the lithium compound in the powder mixture will be dissolved in the water from the condensation, leading to irregular aggregation / fusing, etc., of primary and secondary particles, as well as a lithium-metal composite oxide of poor quality. Conversely, a gas input velocity that is too high and a furnace air speed that is too high will result in the danger of selective powder mixture scattering (separation). A separate exhaust port at a location that is different from the furnace inlet can also be used to introduce the gas into the furnace.

[0086] The rate at which the temperature is increased can be adjusted via the temperature setting of the rotary kiln. A rate of increase that is too low may not allow adequate productivity to be achieved. On the other hand, a rate of increase that is too high will result in the danger of local lithiation reactions as well as a lithium-metal composite oxide of lower homogeneity and poor quality. If the maximum temperature of the powder mixture is too low when the powder mixture is fired while being scraped and stirred, the fired product may be of poor quality. On the other hand, if the maximum temperature of the powder mixture is too high, a resulting danger is that crystal growth will progress concurrently with the lithiation reaction, resulting in a lithium-metal composite oxide of poor quality. In this case, the melting point will vary, depending on the type of lithium compound constituting the powder mixture, and the surface temperature of the furnace core tube should therefore be determined accordingly.

[0087] Specifically, the firing temperature is preferably 400°C or higher, 410°C or higher, 420°C or higher, 430°C or higher, 440°C or higher, 450°C or higher, 460°C or higher, 470°C or higher, 480°C or higher, 490°C or higher, or 500°C or higher. On the other hand, the firing temperature may be less than 700°C, 690°C or lower, 680°C or lower, 670°C or lower, 660°C or lower, 650°C or lower, 640°C or lower, 630°C or lower, 620°C or lower, 610°C or lower, or 600°C or lower. When, for example, lithium hydroxide is used as the lithium compound, the maximum temperature of the powder mixture is preferably 500°C to 650°C, or 530°C to 630°C. When the lithium compound is lithium carbonate, the maximum temperature of the powder mixture is preferably 600°C to 770°C, 630°C to 770°C, or 690°C to 760°C. During the firing process, the temperature setting of the rotary kiln is preferably adjusted in consideration of the rate at which the powder mixture is loaded into the kiln.

[0088] Specifically, the powder mixture is preferably fired, with the surface temperature of the furnace core tube (heated by a heater) set to 400°C or higher, 450°C or higher, or 500°C or higher, and to 1000°C or lower, 950°C or lower, 900°C or lower, or 850°C or lower.

[0089] The firing atmosphere in the firing step is not particularly limited, and should be an atmosphere that ensures the reliable and homogeneous progress of the lithiation reaction and crystal growth. For example, an oxidative decarbonising gas atmosphere having a carbon dioxide gas concentration of 30 ppm or less, or an oxygen atmosphere having an oxygen concentration of 80 vol% or more, and preferably 90 vol% or more, is preferably used.

[0090] The firing time is not particularly limited, provided that it is a time ensuring the reliable and homogeneous progress of the lithiation reaction and crystal growth, and is preferably, for example, 1 or 12 hours or 2 to 10 hours.

[0091] The firing step noted above (also referred to below as "first firing step") will make it possible to produce a lithium-metal composite oxide having the intended composition, but a second firing step can also be established to further fire the lithium-metal composite oxide obtained in the first firing step. Including such a second firing step to allow the material to be fired more than once will result in more reliable and homogeneous crystal growth as well as in a lithium-metal composite oxide of greater quality.

[0092] During the second firing, for example, the lithium-metal composite oxide that has been obtained can be loaded into a firing vessel such as a sagger or a crucible and fired using equipment such as a static furnace, i.e. , and electric furnace, or a roller hearth kiln. A rotary kiln can also be used in the same manner as in the firing step. Equipment that allows conditions suitable for crystallization to be fine-tuned should be selected for use in further firing.

[0093] The firing atmosphere in the second firing step is not particularly limited, and should be an atmosphere that ensures more reliable and homogeneous progress of crystal growth. Specifically, an oxidative decarbonising gas atmosphere having a carbon dioxide gas concentration of 30 ppm or less, or an oxygen atmosphere having an oxygen concentration of 80 vol% or more, and preferably 90 vol% or more, is preferably used, for example, as the atmosphere.

[0094] The heating temperature in the second firing step may be adjusted in consideration of the maximum temperature of the powder mixture in the first firing step or the composition of the intended lithium-metal composite oxide, but the heating is preferably adjusted to between 700°C and 1050°C.

[0095] The firing time is not particularly limited, provided that it is enough time to obtain a lithium-metal composite oxide having the desired crystal structure, and should be 1 to 12 hours, and preferably 2 to 10 hours, for example.

[0096] The second firing step can also be performed by adding a doping source compound and / or a coating source compound to the lithium-metal composite oxide obtained in the first firing step. Thus adding a doping source compound and / or coating source compound to the lithium-metal composite oxide obtained in the firing step will allow the inherent functions of the compound itself or of the elements included in the compound to be brought out. When a doping source compound and / or coating source compound are thus added, they can be added in the form of powder or added by being sprayed in the form of a solution.

[0097] Specific examples of doping source compounds that can be used include one or more selected from the group consisting of cobalt oxide, cobalt hydroxide, manganese oxide, manganese hydroxide, manganese carbonate, magnesium oxide, magnesium hydroxide, aluminum oxide, aluminum hydroxide, aluminum chloride, aluminum fluoride, titanium oxide, titanium hydroxide, titanium chloride, zinc oxide, niobium oxide, niobium hydroxide, niobium chloride, tungsten oxide, tungsten chloride, molybdenum oxide, vanadium oxide, chromium oxide, iron oxide, iron hydroxide, and zirconium oxide.

[0098] Specific examples of coating source compounds that can be used include one or more selected from the group consisting of gallium oxide, potassium oxide, potassium hydroxide, barium oxide, barium hydroxide, barium chloride, calcium oxide, calcium hydroxide, gallium oxide hydroxide, strontium oxide, strontium hydroxide, yttrium oxide, ruthenium oxide, indium oxide, tin oxide , tantalum oxide, bismuth oxide, boric acid, boron oxide, boron carbide, phosphoric acid, and ammonium hydrogen phosphate.

[0099] Nickel-rich lithium-metal composite oxides (lithium-metal composite oxides that contain nickel as element M and have a nickel content of, for example, 80 mol% or more) that have been obtained via the first firing step or the second firing step may sometimes have a higher unreacted lithium compound content or a higher content of lithium compounds that have moved from the crystal structure to the particle surface layer over the course of the firing step (also referred to below as "residual lithium compounds") compared with nickel-poor lithium-metal composite oxides. The residual lithium compound content can be lowered, for example, by washing the lithium-metal composite oxide with water, or by surface treating the surfaces of the primary particles and / or secondary particles of the lithium-metal composite oxide.

[0100] Even when the lithium-metal composite oxide obtained via the first firing step or second firing step is a nickel-poor lithium-metal composite oxide, if it is in the form of secondary particles composed of generally small primary particles, it will have a large specific surface area, resulting in the danger of metal elution induced by hydrogen fluoride, which can come into contact in the form of nonaqueous electrolyte, when the composite oxide is used as positive electrode active material. This sort of lithium-metal composite oxide should therefore be surface treated.

[0101] Examples of methods that can be used as the surface treatment method include, but are not particularly limited to, methods in which fine aluminum oxide particles are deposited by a dry method on the surface layer of the lithium-metal composite oxide particles as shearing force is applied, followed by heat treatment at about 300°C to 700°C. Another method can be used as the surface treatment method, wherein a prescribed amount of the lithium-metal composite oxide is mixed and stirred for about 5 to 10 minutes into an aqueous solution in which a prescribed amount of aluminum sulphate has been dissolved, and the resulting mixture is de-watered, dried, and then heat treated at about 250°C to 700°C, thereby coating the particle surface layer with the aluminum compound. In addition to aluminum compounds, one or more compounds such as boron compounds and tungsten compounds can also be used.

[0102] Even when the lithium-metal composite oxide is in the form of secondary particles consisting of large primary particles, a sintering accelerator such as potassium hydroxide may be used prior to firing in order to obtain the primary particle configuration. The lithium-metal composite oxide may be washed with water in order to wash out such a sintering accelerator.

[0103] The collecting step is a step in which collected powder is obtained by cooling an exhaust gas that contains scattered powder that has been produced by the fluidisation of the powdered mixture in the firing step, and collecting the scattered powder contained in the exhaust gas.

[0104] As noted above, when the powder mixture is fired while continuously fluidised, the flow of the gas introduced into the system ends up causing the powder material to float, some of which is entrained in the form of scattered powder in the gas flow and ends up being discharged out of the system while contained in the exhaust gas. In the collection step, collected powder is obtained by collecting the scattered powder that is thus discharged out of the system while contained in the exhaust gas.

[0105] However, the exhaust gas containing the scattered powder becomes alkaline as a result of at least the lithium in the lithium compound. Exhaust gas containing scattered powder is also produced when the powder mixture is fired, and is thus heated to an elevated temperature of 200°C to 400°C at a firing temperature is 400°C to 600°C. A resulting danger that the metal material, for example, of the equipment involved in collection may be damaged due to corrosion. The exhaust gas containing the scattered powder is therefore cooled to prevent corrosion of the equipment involved in collection.

[0106] The temperature of the cooled exhaust gas is not particularly limited, and should be set according to, for example, the type of the metal material of the equipment involved in collection; the temperature is preferably, for example, 200°C or lower, 195°C or lower, 190°C or lower, 185°C or lower, 180°C or lower, 175°C or lower, 170°C or lower, 165°C or lower, 160°C or lower, 155°C or lower, 150°C or lower, 145°C or lower, 140°C or lower, 135°C or lower, 130°C or lower, 125°C or lower, 120°C or lower, 115°C or v, or 110°C or lower.

[0107] An example of a method that can be considered for cooling exhaust gas is to use a material capable of withstanding elevated temperatures for the exhaust piping through which the exhaust gas passes, and to extend the length of the piping, but a risk associated with increasing the length of the piping is that scattered powder will accumulate in the exhaust piping, resulting in lower yields. Another method that can be considered is to use a heat exchanger to cool the exhaust piping through heat exchange with cooling water, for example, but a resulting danger is that the heat exchanger may cause local condensation and lead to blockage through the accumulation of scattered powder. The use of a method in which a refrigerant gas such as air is brought into contact via spraying, for example, with the exhaust gas containing the scattered powder is therefore preferred. This sort of method allows the exhaust gas to be cooled relatively quickly, and is thus more economical and productive. This method is also easy to control.

[0108] The exhaust gas may also be cooled via natural cooling. The exhaust gas or refrigerant gas may also be heated if the temperature of the exhaust gas drops too much.

[0109] Here, when a hydroxide is used as the precursor compound and / or lithium hydroxide is used as the lithium compound, the exhaust gas will contain water vapour because of the water that is produced via firing. In cases such as this, the exhaust gas is preferably cooled as a temperature over the dew point temperature of the system containing the exhaust gas is maintained.

[0110] At atmospheric pressure, the exhaust gas is preferably cooled while the exhaust gas temperature is maintained at over 100°C, 102°C or higher, 105°C or higher, 107°C or higher, or 110°C or higher.

[0111] In cases where lithium hydroxide is used as the lithium compound or a hydroxide is used as the precursor compound, the further inclusion of carbon dioxide in the refrigerant gas (atmosphere of the cooling mechanism) tends to result in the carbonation of the lithium hydroxide and the production of lithium carbonate. Here, lithium carbonate is less reactive than other lithium compounds, such as lithium hydroxide, and the portion of the lithium that is converted to lithium carbonate therefore will not react very well with the precursor compound even when the scattered powder contained in the lithium carbonate is fired. Depending on the heating temperature, the lithiation reaction of the precursor compound therefore may not progress sufficiently, and lithium carbonate may end up being left over in the resulting fired product. In cases such as this, then, the exhaust gas is preferably cooled in a decarbonising atmosphere. Curbing the production of lithium carbonate in this manner will allow the amount of lithium carbonate remaining in the target lithium-metal composite oxide to be reduced and the quality of the lithium-metal composite oxide to be preserved.

[0112] In cases where lithium carbonate is used as the lithium compound and a hydroxide is used as a precursor compound, or where lithium carbonate and lithium hydroxide are used as the lithium compounds, lithium carbonate will already be present, making it unnecessary to for the atmosphere in the system to be a decarbonising atmosphere, and the exhaust gas should be cooled as the temperature is maintained over the dew point temperature of the system containing the exhaust gas. The lithium carbonate should be removed after the lithium-metal composite oxide has been prepared.

[0113] The exhaust gas can be cooled by bringing a decarbonising refrigerant gas into contact with the exhaust gas. The carbon dioxide concentration of the decarbonising refrigerant gas is preferably 200 ppm or less, 170 ppm or less, 150 ppm or less, 120 ppm or less, 100 ppm or less, 70 ppm or less, 50 ppm or less, 30 ppm or less, 20 ppm or less, 15 ppm or less, or 10 ppm or less. For example, one or more refrigerant gases selected from the group consisting of low dew point-decarbonising air, gas having an oxygen concentration of 90 vol% or more, nitrogen gas, and argon gas, for example, can be used.

[0114] In cases where lithium hydroxide is used as the lithium compound, cooling the exhaust gas in a decarbonising atmosphere while maintaining the temperature over the dew point temperature in this manner can curb the production of lithium carbonate. The condensation of water vapour can also be suppressed in the piping while in contact with the decarbonising gas. The lithium portion of the scattered powder can also be prevented from precipitating and sticking to the inner wall of the piping. The inner wall of the piping can thus be prevented from becoming corroded by the lithium in addition to preserving the fluidity of the scattered powder to ensure that it is more efficiently collected.

[0115] In cases where lithium carbonate is used as the lithium compound, cooling the exhaust gas while maintaining the temperature over the dew point temperature can prevent the lithium carbonate from partially dissolving in condensed water vapour and sticking to the piping.

[0116] Controlling the lithium carbonate while the exhaust gas is cooled as noted above can also reduce the residual amount of lithium carbonate in the lithium-metal composite oxide that is obtained, but the residual amount of lithium carbonate can also be reduced by other methods as well. Specifically, the material can be fired at a temperature that is approximately 100°C higher than the melting point of lithium carbonate when the material is fired in the firing step or is fired thereafter. This will allow the residual amount of lithium carbonate in the manufactured lithium-metal composite oxide to be reduced.

[0117] The residual amount of lithium carbonate is, for example, 0.60% by weight or less, and preferably 0.55% by weight or less.

[0118] The residual amount of lithium carbonate is determined using the Walder method. Specifically, the amount is determined by adding 20 g of a lithium metal composite oxide sample to 100 mL of water, stirred the contents for 20 minutes at room temperature, filtering off the solids, and titrating the resulting supernatant using 0.2 N hydrochloric acid. The two points with the greatest slopes on a pH curve (drawn by plotting the titration amount (mL) on the horizontal axis and the supernatant pH on the vertical axis) are used as the first titration point and second titration point, beginning with the lower titration amount. Based on the titration amounts at these points, the following formula is used to calculate each amount, defined as the residual amount of lithium carbonate. The abbreviations used in the calculation formula are given below. T Titration amount up to first titration point (mL) T2: Titration amount up to second titration point (mL) CHCI: Concentration of hydrochloric acid used for titration (mol / L) FHCI: Factor of hydrochloric acid used for titration M: Molecular weight of lithium carbonate W: Weight of lithium-metal composite oxide sample (g) Residual amount of lithium carbonate (wt%) = (T2-T1) x CHCIXFHCIxM x 2 x 100 / ( Wx 1000)

[0119] After the exhaust gas is cooled as noted above, the scattered powder contained in the exhaust gas is collected using a collector, for example.

[0120] Specific examples of collectors that can be used to collect scattered powder include, but are not particularly limited to, bag filters and cyclones.

[0121] In the mixing step, the collected powder obtained by collecting the scattered powder is again exposed to the firing step to thus obtain a powder mixture in the form of a mixture of at least the precursor compound, the lithium compound, and the collected powder.

[0122] The composition of the scattered powder produced by the fluidisation of the powder mixture and the composition of the collected powder may sometimes be different from the metal composition of the precursor compound and the lithium compound. Specifically, the ratio of the amount of Li to the total amount of element M in the scattered powder and collected powder (referred to below as the Li / M ratio) may sometimes be smaller than the Li / M ratio of the powder mixture (equivalent to that of the intended lithium-metal composite oxide). Accordingly, in order to produce a lithium- metal composite oxide using collected powder, compositional variation should be prevented by taking into consideration the balance between the Li / M ratio of the collected powder and the Li / M ratio of the powder mixture in the system. In cases where the scattered powder is discharged at a constant hourly rate and the amount of scattered powder discharged out of the system is about the same as the amount of collected powder that is added and mixed, no substantial variation will occur during the steady operation of the system.

[0123] No particular limitations are imposed on, for example, the order or location in which the precursor compound, lithium compound, and collected powder are added and mixed, or the equipment that is used when the ingredients are added and mixed. For example, any of the following mixing methods 1 through 4 can be used when the various ingredients are added in a single location. However, the addition of the precursor compound, lithium compound, and collected powder is not limited to a single location. Mixing method 1: A powder mixture is prepared by mixing collected powder with a precursor compound and a lithium compound.

[0124] Mixing method 2: A powder mixture is prepared by mixing collected powder with a previously prepared mixture of a precursor compound and a lithium compound.

[0125] Mixing method 3: A powder mixture is prepared by mixing collected scattered powder with a precursor compound, which are then further mixed with a lithium compound.

[0126] Mixing method 4: A powder mixture is prepared by mixing collected scattered powder with a lithium compound, which are then further mixed with a precursor compound.

[0127] Mixing method 1-1 and mixing method 1-2 are given below as more specific examples of mixing method 1.

[0128] Mixing method 1-1 : A precursor compound, lithium compound, and collected powder are precision mixed in, for example, a mixer that allows the ingredients to be mixed evenly and homogeneously (referred to below as precision mixing).

[0129] Mixing method 1-2: The precursor compound and lithium compound are precision mixed, then collected powder is mixed by being added to a conveyance path through which the resulting precision mixture is conveyed, while rotated by rotating means such as a screw, to a mixture storage tank, for example, that is equipped with rotating means such as a screw or ribbon blender, and / or the collected powder is added to, and mixed with, the fed precision mixture in the mixture storage tank, for example.

[0130] Mixing method 2-1 and mixing method 2-2 are given below as more specific examples of mixing method 2.

[0131] Mixing method 2-1 : A powder mixture and scattered powder are precision mixed in, for example, a mixer that allows the ingredients to be precision mixed.

[0132] Mixing method 2-2: Collected powder is mixed by being added to a conveyance path through which the powder mixture is conveyed, while rotated by rotating means such as a screw, to a mixture storage tank, for example, that is equipped with rotating means such as a screw or ribbon blender, and / or the collected powder is added to, and mixed with, the fed powder mixture in the mixture storage tank, for example.

[0133] In mixing methods 3 and 4, the various mixing operations should be performed in a mixer capable of precision mixing, a conveyance path through which the mixture is conveyed to a mixture storage tank, for example, and a mixture storage tank, for example, in the same manner as in mixing methods 1 and 2.

[0134] As noted above, the precursor compound, the lithium compound, and the collected powder are mixed, before being exposed to the firing step, to produce the homogeneous mixture that will be exposed to the firing step, thereby facilitating the progress of the lithiation of unreacted element M in the collected powder. As a result, the Li / M ratio in the collected powder will be closer to the Li / M ratio of the intended lithium-metal composite oxide, thereby ensuring a more consistent Li / M ratio in the mixture exposed to the firing step and allowing more homogeneous crystal growth and particle growth to be achieved.

[0135] The powder mixture may also be prepared by mixing a doping source compound and / or a coating source compound in addition to the precursor compound, lithium compound, and collected scattered powder. In that case, the powdered mixture is furthermore a mixture with a doping source compound and / or a coating source compound. No particular limitations are imposed on the order or location in which the doping source compound and / or coating source compound is or are added and mixed, or the equipment in which they are added and mixed.

[0136] The same doping source compounds and coating source compounds noted above can be used.

[0137] As exemplified in mixing methods 1 through 4, the powder mixture should be prepared in advance from collected powder along with the precursor compound and lithium compound being fired. For example, in cases where the mixture is fired while fluidised by being scraped and stirred using the rotary kiln noted above, the powder mixture is prepared in advance before being fired in the rotary kiln, and is introduced into the rotary kiln, where it is scraped and stirred. No particular limitations are imposed on the time at which the mixture is prepared.

[0138] The entire amount of collected powder is preferably mixed into the powder mixture in the mixing step. In this case, the proportions in which the precursor compound, lithium compound, and collected powder are mixed should be determined so as to be constant based on, for example, the particle size of the precursor compound, the particle size of the lithium compound, the difference between the two, and the ingredients should be mixed based upon a consideration of the Li / M ratio of the powder mixture.

[0139] Specifically, the powder mixture is preferably prepared by controlling the mass ratio represented by either (a) or (b) below to 2:98 to 40:60, 5:95 to 40:60, or 7:93 to 37:63:

[0140] (a) mass ratio of the amount of collected powder to the total amount of precursor compound and lithium compound,

[0141] (b) mass ratio of the amount of collected powder to the amount of powdered mixture. The amount of scattered powder that is scattered per hour and the amount of collected powder that is again added and mixed in the mixing step should be equalized within this range. The collected powder must be controlled so as to be continuously added in cases where it is mixed and fired after being added in the absence of any mixture storage tank or batch type mixer downstream from where it is added. The addition of the powder mixture is preferably controlled to within the same range even when it also contains the above-mentioned doping source compound and / or coating source compound.

[0142] As the quality of the lithium-metal composite oxide that is obtained may be compromised if the mass ratio represented by (a) or (b) varies over time, the fluidisation conditions must be reset.

[0143] Preparing the powder mixture by controlling the amount in which the collected powder is added in this way will ensure that the lithium-metal composite oxide that is obtained by firing the powder mixture will have the intended Li / M ratio.

[0144] The composition of the lithium-metal composite oxide produced by the method of production according to the present disclosure is not particularly limited, provided that it is composed of a lithium-metal composite oxide that contains Li and at least one element M, but the composition is preferably represented, for example, by formula (I): LiaMO2(I)

[0145] (in the formula, M is an element other than Li or O, and 0.95<a<1.40).

[0146] In the lithium-metal composite compound having a composition represented by formula (I), the Li stoichiometric ratio a, specifically, the ratio of the number of mols of Li to the total number of mols of element M (Li / M), is preferably 0.95<a<1.40, 0.95<a<1.25, or 0.96<a<1.15.

[0147] In the lithium-metal composite oxide having the composition represented by formula (I), the element M is preferably at least Ni, and is more preferably at least Ni, Co, Al and / or Mn. When M is at least Ni, the stoichiometric ratio b of Ni, specifically, the ratio of the number of mols of Ni to the total number of mols of element M (Ni / M), is preferably 0.3<b<1, 0.5<b<1, or 0.8<b<1. When lithium carbonate is used as the lithium compound, the Ni / M ratio is more preferably 0.3<b<0.8.

[0148] In the lithium-metal composite oxide produced by the method of production according to the present disclosure, the average particle size of the secondary particles (average secondary particle size) and crystallite size should preferably fall with the ranges given below. The average secondary particle diameter is preferably, for example, 1 m to 30pm, and more preferably 2pm to 25pm.

[0149] The average secondary particle size is the D50, as determined on a volume basis by a wet laser method using a laser type particle size distribution analyser (Microtrac HRA, manufactured by Nikkiso Co., Ltd.).

[0150] The crystallite size is preferably, for example, 50 nm to 600 nm, and more preferably 60 nm to 500 nm.

[0151] The crystallite size is determined by Rietveld analysis of the XRD diffraction data of the lithium-metal composite oxide, which is obtained by the following method.

[0152] XRD diffraction data of lithium-metal composite oxides is obtained under the following X-ray diffraction conditions using an X-ray diffraction apparatus (SmartLab, produced by Rigaku Corp.), and the XRD diffraction data is then subjected to Rietveld analysis, with reference to R. A. Young, Ed., “The Rietveld Method,” Oxford University Press (1992).

[0153] X-ray source: Cu-Ka

[0154] Acceleration voltage and current: 45 kV and 200 mA

[0155] Sampling width: 0.02 deg.

[0156] Scan width: 15 deg. to 122 deg.

[0157] Scan speed: 1.0 steps / sec

[0158] Divergence slit: 2 / 3 deg.

[0159] Receiving slit width: 0.15 mm

[0160] Scattering slit: 2 / 3 deg.

[0161] In the method of production in the present disclosure, as noted above, the scattered powder that is generated (when the powder mixture is fired while continuously fluidised) is collected, and the collected powder, rather than be fired as such, is mixed with at least a precursor compound and a lithium compound before being fired. This makes it possible to curb compositional variation in the lithium-metal composite oxide that is obtained, and allows a lithium-metal composite oxide having the intended composition to be obtained.

[0162] An example that can be used as an indicator of variation in the Li / M ratio is the coefficient of variation of the Li / M ratio (also referred to below as the "coefficient of Li / M variation") of a plurality of fired samples (sampled from different parts) of a fired product that has been obtained after a prescribed period of time following the starting firing. A fired product that has a low coefficient of Li / M variation at any given time point indicates low variation in the Li / M ratio. The more similar the composition of N number (such as N>10) of fired samples taken from different parts of a fired product that has been obtained after a prescribed period of time, the coefficient of Li / M variation tends to be closer to 0%. Specifically, the lower the Li / M variation coefficient, the better. A coefficient of Li / M variation that is too great indicates that compositional variation has occurred in the fired samples that have been obtained after a predetermined period of time has elapsed. The method of production according can adequately curb compositional variation in fired product samples obtained after any given period of time, such as 1 hour, 2 hours, 3 hours, and 4 hours. The coefficient of Li / M variation is determined every hour for 10 consecutive hours (total of 10 times). The coefficient of Li / M variation is not particularly limited, but is preferably 0.7% or less, 0.6% or less, or 0.5% or less, at any time.

[0163] The coefficient of Li / M variation is determined, based on the following formula, using the average and standard deviation based on the Li / M ratio of N (N=10) fired samples obtained after the prescribed period of time. The coefficient is determined on the basis of the Li / M ratio of the various fired product samples, and the ratio is determined by quantifying each element, using an ICP-AES (Optima 8300, by PerkinElmer), in a solution that is prepared by heating and dissolving a 0.2 g sample of the fired product in 25 mL of 20% hydrochloric acid solution, cooling the solution, transferring the solution to a 100 mL measuring flask, and adding purified water.

[0164] Coefficient of Li / M variation (%) = (standard deviation / mean value)* 100%

[0165] The lithium-metal composite oxide produced by the method of production according to the present disclosure can be used as a positive electrode active material for a nonaqueous electrolyte secondary battery. Nonaqueous electrolyte secondary batteries are composed of a positive electrode, a negative electrode, and an electrolytic solution containing an electrolyte, and the positive electrode active material for the nonaqueous electrolyte secondary battery can be included in the positive electrode therein.

[0166] When the positive electrode is produced, a conductive agent and a binder are admixed with the positive electrode active material. Acetylene black, carbon black, and graphite, etc. are preferred as conductive agents, for example. Polytetrafluoroethylene and polyvinylidene fluoride, etc. are preferred as binders, for example.

[0167] Examples of active materials that can be used for the negative electrode include negative electrode active materials such as lithium metal, graphite, and low-crystallinity carbon materials, as well as one or more non-metal or metal elements selected from the group consisting of Si, Al, Sn, Pb, Zn, Bi and Cd, or alloys comprising the same, or chalcogen compounds comprising the same.

[0168] Examples of solvents that can be used for the electrolytic solution include organic solvents including one or more selected from the group consisting of carbonates, such as ethylene carbonate, propylene carbonate, dimethyl carbonate, and diethyl carbonate, or ethers such as dimethoxyethane.

[0169] In addition to, in particular, lithium hexafluorophosphate (LiPFe), one or more selected from the group consisting of lithium salts such as lithium perchlorate or lithium tetrafluoroborate can be used as the electrolyte. The electrolyte can be used while dissolved in the solvents noted above.

[0170] The production method of present disclosure makes it possible to produce a lithium- metal composite oxide that, when used as the positive electrode active material for a nonaqueous electrolyte secondary battery, can ensure better battery characteristics, without any loss of quality.

[0171] EXAMPLES

[0172] The present disclosure is illustrated in detail below using examples of the present disclosure, but is not limited in any way by these examples.

[0173] Samples of the examples and comparative examples were analysed by the following methods.

[0174] XRD diffraction data of lithium-metal composite oxide samples was obtained under the following X-ray diffraction conditions using an X-ray diffraction apparatus (SmartLab, produced by Rigaku Corp.), and the XRD diffraction data was then subjected to Rietveld analysis, with reference to R. A. Young, Ed., “The Rietveld Method,” Oxford University Press (1992).

[0175] X-ray source: Cu-Ka

[0176] Acceleration voltage and current: 45 kV and 200 mA Sampling width: 0.02 deg.

[0177] Scan width: 15 deg. to 122 deg.

[0178] Scan speed: 1.0 steps / sec Divergence slit: 2 / 3 deg. Receiving slit width: 0.15 mm Scattering slit: 2 / 3 deg.

[0179] <Composition of Precursor Compounds and Lithium-Metal Composite Oxide Samples> A precursor compound or lithium-metal composite oxide sample (0.2 g) is heated and dissolved in 25 mL of 20% hydrochloric acid solution, the solution is cooled and then transferred to a 100 mL measuring flask, and purified water is added, where the resulting solution is used to quantify each element using an ICP-AES (Optima 8300, by PerkinElmer).

[0180] <Coin Cell Utilizing Lithium-Metal Composite Oxide> 2032 type coin cells in which lithium-metal composite oxide samples were used as positive electrode active material were produced using positive electrodes, negative electrodes, and electrolytic solutions prepared by the following methods.

[0181] < Positive electrode>

[0182] Using acetylene black and graphite as the conductive agent at a weight ratio of acetylene black:graphite=1 :1 , and using polyvinylidene fluoride as the binder, the positive electrode active material, conductive agent and binder were blended to achieve a weight ratio of positive electrode active materiakconductive agent:binder=90:6:4, and a slurry obtained by mixing these materials with N- methylpyrrolidone was coated on an aluminum foil. The coated aluminum foil was dried at 110°C to prepare a sheet which was punched to a diameter of 15 mm and then rolled to a composite material density of 3.0 g / cm3, and this was used as the positive electrode.

[0183] <Negative electrode>

[0184] A lithium foil having a thickness of 500 pm punched to a diameter of 16 mm was used as the negative electrode.

[0185] <Electrolytic solution>

[0186] A mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) was prepared at a volume ratio of EC:DMC=1 :2, and a solution obtained by mixing a 1 M LiPFe electrolyte therewith was used as the electrolytic solution.

[0187] <Nonaqueous Electrolyte Secondary Battery Characteristics>

[0188] (Initial Charging Capacity and Initial Charging / Discharging Efficiency)

[0189] Coin cells produced by the method in section [Coin Cell Utilizing Lithium-Metal Composite Oxide] were charged at a constant current at a current density of 18 mA / g to 4.30 V (upper limit voltage) at 25°C, and were then charged at a constant voltage to a current density of 2 mA / g. The capacity at this time was used as the initial charging capacity (mAh / g).

[0190] After a 5-minute break, constant current discharging was then performed at a current density of 18 mA / g to 3.00 V under the same conditions, and the initial discharging capacity (mAh / g) was measured after a 5-minute break.

[0191] The initial charging / discharging efficiency was calculated on the basis of the following equation using the initial measured initial charging capacity and the initial measured discharging capacity.

[0192] Initial charging / discharging efficiency (%) = (initial discharging capacity / initial charging capacity) x 100% <Sample Preparation

[0193] The lithium-metal composite oxide materials of the examples and comparative examples were prepared by the following methods.

[0194] Synthesis of Precursor Compound 1 : A nickel sulphate aqueous solution, cobalt sulphate aqueous solution, and aluminum sulphate aqueous solution were mixed to an Ni, Co, Al ratio (molar ratio) of Ni:Co:AI= 89:7:4 to obtain a mixed aqueous solution. 10 L of pure water to which 300 g of a sodium hydroxide aqueous solution and 500 g of aqueous ammonia had been added was prepared in advance as the mother liquor in a reactor, the interior of the reactor was purged with nitrogen gas at a flow rate of 0.7 L / min to create a nitrogen atmosphere, and the reaction was also carried out under a nitrogen atmosphere.

[0195] The aqueous solution mixture, the sodium hydroxide aqueous solution, and the aqueous ammonia were then simultaneously added drop-wise at a predetermined rate as a stirring blade was rotated at 1000 rpm, and the Ni, Co and Al were co-precipitated by being crystallized into particle aggregates through a crystallization reaction in which the amount of the alkaline solution drops was adjusted to a pH of 11.8, thus giving a co-precipitate.

[0196] The slurry inside the reactor was then separated into liquid and solids, which were washed with pure water to lower residual impurities, and the co-precipitate in the form of caked was then dried for 12 hours at 110°C in the atmosphere to obtain Precursor Compound 1. The D50 of the volume-based particle size distribution of Precursor Compound 1 at this time was 11.2pm. The angle of repose of Precursor Compound 1 , as determined by the injection method, was 34.2°.

[0197] Example 1-1 : Production of Lithium-Metal Composite Oxide Sample

[0198] Fig. 3 is a flowchart (flow a) of the method for producing the positive electrode active material of Example 1-1. The lithium-metal composite oxide sample of Example 1-1 was produced according to flow a.

[0199] Precursor Compound 1 and anhydrous lithium hydroxide (angle of repose, as determined by injection method: 52.2°) were weighed out such that the ratio (molar ratio) of Li versus the total amount of Ni, Co, and Al was Li / (Ni+Co+AI)=1 .02, the ingredients were introduced into a mixer, in such a way as to control the mass ratio of collected powder versus the total amount of Precursor Compound 1 and anhydrous lithium hydroxide (scattered powdertotal amount), as described below, and the contents were precision mixed to prepare Mixture 1. The resulting Mixture 1 was further mixed continuously while conveyed by a screw, and was further mixed continuously in a mixture storage tank equipped with a mixing function based on a screw (rotating speed: 104 rpm) and stored in the tank. The angle of repose of Mixture 1 , as determined by the injection method, was 43.7°.

[0200] Mixture 1 was then introduced from the mixture storage tank into a rotary kiln and fired. Mixture 1 was fired, while being scraped and stirred as well as continuously fluidised (Mixture 1 flow shown by arrow B), for 13 hours under the rotary kiln conditions detailed below in an oxygen atmosphere (oxygen concentration: 97 vol%) using a rotary kiln that had a retort diameter of 300 mm and that was circumferentially equipped with four scraping blades at an angle of 30 degrees on the surface portion inside the furnace core tube illustrated in Fig. 2.

[0201] Exhaust gas (approximately 280°C) containing the scattered powder that was generated during the firing process was discharged out of the system on the inlet side of the rotary kiln, and a decarbonising refrigerant gas (ultra-low dew point-dry air, carbon dioxide concentration: 10 ppm or less) was introduced and brought into contact with the exhaust gas, thus cooling the exhaust gas containing the scattered powder in the decarbonising atmosphere. The temperature of the exhaust gas at this time was about 180°C at a slightly negative pressure of approximately 101.2 kPa.

[0202] Then, as the temperature of the exhaust gas was maintained at approximately 180°C at a slightly negative pressure of approximately 101.2 kPa in the same manner as during cooling, the scattered powder contained in the exhaust gas was collected, as the collected powder, using a filter fabric type of bag filter.

[0203] The collected powder was introduced into the mixer in which Precursor Compound 1 and the anhydrous lithium hydroxide were being mixed to prepare Mixture 1 , and Precursor Compound 1, the anhydrous lithium hydroxide, and the scattered powder were precision mixed to prepare a powder mixture. The amount of collected powder introduced at this time was controlled such that the mass ratio of the amount of collected powder to the total amount of Precursor Compound 1 and the anhydrous lithium hydroxide (scattered powder: Precursor Compound 1 and anhydrous lithium hydroxide) was approximately 13:87. The resulting powder mixture was continuously mixed while conveyed by the screw, and was further mixed continuously in the mixture storage tank and stored in the tank.

[0204] The powder mixture was then introduced from the mixture storage tank into the rotary kiln, and was fired continuously to continuously obtain a lithium-metal composite oxide. The yield of the resulting lithium-metal composite oxide was about 82% relative to the total amount (mass) of Precursor Compound 1 and the anhydrous lithium hydroxide that had been introduced.

[0205] When the powder mixture was introduced into the rotary kiln and discharged stably and continuously during the firing process, the powder mixture firing time was set to 3 hours, and the powder mixture was fired at the maximum temperature (approximately 600°C) for approximately 1.5 hours.

[0206] The powder mixture was scraped and stirred by the scraping blades to a maximum height that was approximately 1.0 times the maximum height when not being scraped and stirred. The size of the scraping blades was sufficient to allow 50% of the total amount of a mixture loaded at a 20% rate to be stirred per rotation.

[0207] Rotary Kiln Conditions:

[0208] Retort rotating speed: 0.9 rpm

[0209] Loading rate: 20%

[0210] Furnace air speed and dew point: Gas input rate adjusted to 47 L / min

[0211] Heating rate: Surface temperature of furnace core tube set as shown below

[0212] Maximum surface temperature of furnace core tube: 640°C

[0213] Maximum temperature of mixture: approximately 600°C

[0214] As the powder mixture was fired over a 13-hour period, 10 samples of fired product were obtained from different parts of the fired product, where the first was obtained at the point in time when discharge had stabilized (4 hours after the start of firing), and the rest were obtained every hour thereafter; the Li / M ratio of each sample was determined, and the coefficient of Li / M variation at each time point was calculated based on the standard deviation and average per the method noted above.

[0215] The resulting lithium-metal composite oxide was randomly sampled, and the samples were loaded into a 300 mm wide and 100 mm deep sagger and then fired for 5 hours at 750°C in an oxygen atmosphere (oxygen concentration: 98 vol%) in a static furnace to obtain lithium-metal composite oxide samples.

[0216] The residual amount of lithium carbonate in the resulting lithium-metal composite oxide samples was 0.49% by weight, as determined according to the method noted above.

[0217] Example 1-2: Production of Lithium-Metal Composite Oxide Sample

[0218] Fig. 4 is a flowchart (flow P) of the method for producing the positive electrode active material of Example 1-2. The lithium-metal composite oxide sample of Example 1-2 was produced according to flow p.

[0219] A lithium-metal composite oxide sample was produced in the same manner as in Example 1-1 , except that no collected powder was introduced into the mixer in which Precursor Compound 1 and the anhydrous lithium hydroxide were being mixed to prepare Mixture 1 , the prepared Mixture 1 and scattered powder were continuously mixed while conveyed by the screw to prepare the powder mixture, which was further mixed continuously in the mixture storage tank and stored in the tank, and the mixture was then introduced from the mixture storage tank into a rotary kiln and continuously fired to continuously obtain a fired product. The yield of the resulting lithium-metal composite oxide sample was 82% relative to the total amount (mass) of Precursor Compound 1 and the anhydrous lithium hydroxide that had been introduced. The residual amount of lithium carbonate was 0.51% by mass.

[0220] Reference Example 1-1 : Production of Lithium-Metal Composite Oxide Sample

[0221] Fig. 5 is a flowchart (flow y) of the method for producing the positive electrode active material of Reference Example 1-1. The lithium-metal composite oxide sample of Reference Example 1-1 was produced according to flow y.

[0222] A lithium-metal composite oxide sample was produced in the same manner as in Example 1-1 , except that the scattered powder contained in the exhaust gas was collected without cooling the exhaust gas that contained the scattered powder in a decarbonising atmosphere (a refrigerant gas that was not a decarbonising gas (dry air, carbon dioxide concentration: approximately 400 ppm) was introduced into contact with the exhaust gas). The yield of the resulting lithium-metal composite oxide was 81% relative to the total amount (mass) of Precursor Compound 1 and the anhydrous lithium hydroxide that had been introduced. The residual amount of lithium carbonate was 0.69% by mass.

[0223] Comparative Example 1-1 : Production of Lithium-Metal Composite Oxide Sample Fig. 6 is a flowchart (flow 5) of the method for producing the positive electrode active material of Comparative Example 1-1. The lithium-metal composite oxide sample of Comparative Example 1-1 was produced according to flow 5.

[0224] A lithium-metal composite oxide sample was produced in the same manner as in Example 1-1 , except that the exhaust gas containing the scattered powder was cooled by piping that had been extended in length to the outside in order to protect the equipment, and the scattered powder was treated with a scrubber, so that only the Powder Mixture 1 was fired, without the scattered powder contained in the exhaust gas being collected. The yield of the resulting lithium-metal composite oxide sample was 72% relative to the total amount (mass) of Precursor Compound 1 and the anhydrous lithium hydroxide that had been introduced. The residual amount of lithium carbonate was 0.53% by weight.

[0225] Comparative Example 1-2: Production of Lithium-Metal Composite Oxide Sample Fig. 7 is a flowchart (flow E) of the method for producing the positive electrode active material of Comparative Example 1-2. The lithium-metal composite oxide sample of Comparative Example 1-2 was produced according to flow E.

[0226] A lithium-metal composite oxide sample was produced in the same manner as in Example 1-1 , except that Mixture 1 and the collected powder were introduced separately into the rotary kiln. The yield of the resulting lithium-metal composite oxide sample was 82% relative to the total amount (mass) of Precursor Compound 1 and the anhydrous lithium hydroxide that had been introduced. The residual amount of lithium carbonate was 0.53% by mass.

[0227] Table 1 shows the coefficient of Li / M variation at each time point in the lithium metal composite oxide samples of Examples 1-1 and 1-2, Reference Example 1-1 , and Comparative Examples 1-1 and 1-2. Table 2 shows the yields, as well as the residual amounts of lithium carbonate, of the lithium-metal composite oxide samples of Examples 1-1 and 1-2, Reference Examples 1-1 and Comparative Examples 1-1 and 1-2, and also the initial charge capacity and initial charge / discharge efficiency of nonaqueous electrolyte secondary batteries in which the samples were used as positive electrode active material.

[0228] Table 1

[0229] Table 2

[0230] Synthesis of Precursor Compound 2: A nickel sulphate aqueous solution, cobalt sulphate aqueous solution, and manganese sulphate aqueous solution were mixed to an Ni and Co and Mn ratio (molar ratio) of Ni:Co:Mn=4:3:3, giving an aqueous solution mixture. 10 L of pure water to which 300 g of a sodium hydroxide aqueous solution and 500 g of aqueous ammonia had been added was prepared in advance as the mother liquor in a reactor, the interior of the reactor was purged with nitrogen gas at a flow rate of 0.7 L / min to create a nitrogen atmosphere, and the reaction was also carried out under a nitrogen atmosphere.

[0231] The aqueous solution mixture, the sodium hydroxide aqueous solution, and the aqueous ammonia were then simultaneously added drop-wise at a predetermined rate as a stirring blade was rotated at 1100 rpm, and the Ni, Co and Mn were coprecipitated by being crystallized into particle aggregates through a crystallization reaction in which the amount of the alkaline solution drops was adjusted to a pH of 12.2, thus giving a co-precipitate.

[0232] The slurry inside the reactor was then separated into liquid and solids, which were washed with pure water to lower residual impurities, and the co-precipitate in the form of caked was then dried for 12 hours at 110°C in the atmosphere to obtain Precursor Compound 2. The D50 of the volume-based particle size distribution of Precursor Compound 2 at this time was 5.8pm. The angle of repose of Precursor Compound 2, as determined by the injection method, was 46.1°.

[0233] Example 2-1: Production of Lithium-Metal Composite Oxide Sample

[0234] Fig. 8 is a flowchart (flow Q of the method for producing the positive electrode active material of Example 2-1. The lithium-metal composite oxide sample of Example 2-1 was produced according to flow ■

[0235] Precursor Compound 2 and lithium carbonate (angle of repose, as determined by injection method: 60.1°) were weighed out such that the ratio (molar ratio) of Li versus the total amount of Ni, Co, and Mn was Li / (Ni+Co+Mn)=1.10, the ingredients were introduced into a mixer, in such a way as to control the weight ratio of collected powder versus the total amount of Precursor Compound 2 and lithium carbonate (amount of scattered powder: total amount), as described below, and the contents were precision mixed to prepare Mixture 2. The resulting Mixture 2 was further mixed continuously while conveyed by a screw, and was further mixed continuously in a mixture storage tank equipped with a screw (rotating speed: 104 rpm) and stored in the tank. The angle of repose of Powder Mixture 2, as determined by the injection method, was 51.2°.

[0236] Mixture 2 was then introduced from the mixture storage tank into a rotary kiln and fired. Mixture 2 was fired, while being scraped and stirred as well as continuously fluidised (Mixture 2 flow shown by arrow B), for 13 hours under the rotary kiln conditions detailed below in an oxidizing atmosphere (oxygen concentration: 21 vol%) with low dew pointdry air using a rotary kiln that had a retort diameter of 300 mm and that was circumferentially equipped with four scraping blades at an angle of 30 degrees on the surface portion inside the furnace core tube illustrated in Fig. 2. Exhaust gas (approximately 270°C) containing the scattered powder that was generated during the firing process was discharged out of the system on the inlet side of the rotary kiln, and a refrigerant gas (low dew point-dry air) was introduced and brought into contact with the exhaust gas, thus cooling the exhaust gas containing the scattered powder. The temperature of the exhaust gas at this time was about 160°C at a slightly negative pressure of approximately 101.2 kPa.

[0237] Then, as the temperature of the exhaust gas was maintained at approximately 160°C at a slightly negative pressure of approximately 101.2 kPa in the same manner as during cooling, the scattered powder contained in the exhaust gas was collected as the collected powder.

[0238] The collected powder was introduced into the mixer in which Precursor Compound 2 and the lithium carbonate were being mixed to prepare Mixture 2, and Precursor Compound 2, the lithium carbonate, and the scattered powder were precision mixed to prepare a powder mixture. The amount of collected powder introduced at this time was controlled such that the mass ratio of the amount of collected powder to the total amount of Precursor Compound 2 and the lithium carbonate (scattered powder: Precursor Compound 2 and lithium carbonate) was approximately 12:88. The resulting powder mixture was continuously mixed while conveyed by the screw, and was further mixed in the mixture storage tank and stored in the tank.

[0239] The powder mixture was then introduced from the mixture storage tank into the rotary kiln, and was fired continuously to continuously obtain a lithium-metal composite oxide. The yield of the resulting lithium-metal composite oxide was 80% relative to the total amount (mass) of Precursor Compound 2 and the lithium carbonate that had been introduced.

[0240] When the powder mixture was introduced into the rotary kiln and discharged stably and continuously during the firing process, the powder mixture firing time was set to 3 hours, and the powder mixture was fired at the maximum temperature (approximately 600°C.) for approximately 1.5 hours.

[0241] The powder mixture was scraped and stirred by the scraping blades to a maximum height that was approximately 1.0 times the maximum height when not being scraped and stirred. The size of the scraping blades was sufficient to allow 50% of the total amount of a mixture loaded at a 20% rate to be stirred per rotation.

[0242] Rotary Kiln Conditions:

[0243] Retort rotating speed: 1.25 rpm

[0244] Loading rate: 20%

[0245] Furnace air speed and dew point: Gas input rate adjusted to 52 L / min

[0246] Heating rate: Surface temperature of furnace core tube set as shown below Maximum surface temperature of furnace core tube: 640°C

[0247] Maximum temperature of mixture: approximately 600°C

[0248] As the powder mixture was fired over a 13-hour period, 10 samples of fired product were randomly obtained from different parts of the fired product, where the first was obtained at the point in time when discharge had stabilized (4 hours after the start of firing), and the rest were obtained every hour thereafter; the Li / M ratio of each sample was determined, and the coefficient of Li / M variation at each time point was calculated based on the standard deviation and average per the method noted above.

[0249] The resulting lithium-metal composite oxide was randomly sampled, and the samples were loaded into a 300 mm wide and 100 mm deep sagger and then fired for 5 hours at 980°C in an oxidizing atmosphere (oxygen concentration: 21 vol%) with low dew pointdry air in a static furnace to obtain lithium-metal composite oxide samples.

[0250] Comparative Example 2-1: Production of Lithium-Metal Composite Oxide Sample Fig. 9 is a flowchart (flow q) of the method for producing the positive electrode active material of Comparative Example 2-1. The lithium-metal composite oxide sample of Comparative Example 2-1 was produced according to flow q.

[0251] A lithium-metal composite oxide sample was produced in the same manner as in Example 2-1 , except that the exhaust gas containing the scattered powder was cooled by piping that had been extended in length to the outside in order to protect the equipment, and the scattered powder was treated with a scrubber, so that only the Powder Mixture 2 was fired, without the scattered powder contained in the exhaust gas being collected. The yield of the resulting lithium-metal composite oxide sample was 69% relative to the total amount (mass) of Precursor Compound 2 and the lithium carbonate that had been introduced.

[0252] Comparative Example 2-2: Production of Lithium-Metal Composite Oxide Sample Fig. 10 is a flowchart (flow i) of the method for producing the positive electrode active material of Comparative Example 2-2. The lithium-metal composite oxide sample of Comparative Example 2-2 was produced according to flow i.

[0253] A lithium-metal composite oxide sample was produced in the same manner as in Example 2-1, except that Mixture 2 and the collected powder were introduced separately into the rotary kiln. The yield of the resulting lithium-metal composite oxide sample was 79% relative to the total amount (mass) of Precursor Compound 2 and the lithium carbonate that had been introduced.

[0254] Table 3 shows the coefficient of Li / M variation at each time point in the lithium metal composite oxide samples of Example 2-1, and Comparative Examples 2-1 and 2-2. Table 4 shows the yields, as well as the residual amounts of lithium carbonate, of the lithium-metal composite oxide samples of the fired products of Examples 2-1 , and Comparative Examples 2-1 and 2-2, and also the initial charge capacity and initial charge / discharge efficiency of nonaqueous electrolyte secondary batteries in which the samples were used as positive electrode active material.

[0255] Table 3 Table 4

[0256] Key to Symbols:

[0257] 1 Furnace core tube 2 Surface portion

[0258] 3 Scraping blades

[0259] 4 Axis

[0260] 0 Installation angle

Claims

CLAIMS1. A method for producing a lithium-metal composite oxide, comprising: a firing step, in which a powdered mixture, comprising a mixture of at least a precursor compound, a lithium compound, and collected powder, is fired while continuously fluidised; a collecting step, in which collected powder is obtained by cooling an exhaust gas that contains scattered powder that has been produced by the fluidisation of the powdered mixture in the firing step, and collecting the scattered powder contained in the exhaust gas; and a mixing step, in which the powdered mixture is obtained in the form of a mixture of at least the precursor compound, the lithium compound, and the collected powder.

2. The method of production according to Claim 1 , wherein the powdered mixture is furthermore a mixture with a dope source compound and / or a coating source compound.

3. The method of production according to Claim 1 or 2, wherein the powdered mixture is prepared by controlling the mass ratio represented in either (a) or (b) below to 2:98 to 40:60:(a) mass ratio of the amount of the collected powder to the total amount of the precursor compound and the lithium compound,(b) the mass ratio of the amount of the collected powder to the amount of the powdered mixture.

4. The method of production according to Claim 1 or 2, wherein a rotary kiln equipped with a scraping blade on the surface inside the furnace core tube is used in the firing step to carry out scraped stirring, where the material being fired in the furnace core tube is stirred while scraped.

5. The method according to Claim 4 for producing a lithium-metal composite oxide, wherein the powdered mixture that has been prepared in advance is introduced into the rotary kiln to carry out the scraped stirring.

6. The method of production according to Claim 1 or 2, wherein the lithium compound is lithium hydroxide, and the exhaust gas is cooled in a decarbonising atmosphere as a temperature over the dew point temperature of the system containing the exhaust gas is maintained.

7. The method according to Claim 1 or 2 for producing a lithium-metal composite oxide, wherein the lithium compound is lithium carbonate, the precursor compounds is a hydroxide, and the exhaust gas is cooled as a temperature overthe dew point temperature of the system containing the exhaust gas is maintained.

8. The method for producing a lithium-metal composite oxide according to Claim 1 or 2, wherein the firing temperature in the firing step is 400°C to under 700°C, and the method further comprises a second firing step after the above firing step, wherein the fired material obtained in the above firing step is further fired at a temperature of 700°C to 1000°C.

Citation Information

Patent Citations

  • Fluidized bed reaction furnace for sintering anode material of lithium ion battery

    CN111023813A

  • Lithium ion battery ternary material dynamic synthesis device and method

    CN112747590A

  • Lithium battery positive electrode material roasting and cooling system and method

    CN113834321A

  • System for collecting raw material powder

    JP2013036717A

Cited By

  • Single-phase nickel-based high-temperature alloy powder for additive manufacturing, preparation method of single-phase nickel-based high-temperature alloy powder and alloy part manufacturing process

    CN121360819A