Inclusion nickel oxide nanoparticles, method for producing same, light-emitting element, and display device
Clathrated nickel oxide nanoparticles, produced by encapsulating nickel oxide particles with a host like cyclodextrin, address the aggregation issue of conventional NiO particles, resulting in a more efficient and flat hole functional layer with improved light-emitting characteristics in display devices.
Patent Information
- Application Number
- PCT/JP2023/019966
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional nickel oxide (NiO) particles used in hole functional layers of light-emitting devices tend to aggregate in aqueous dispersions, leading to poor flatness and deteriorated light-emitting characteristics due to their larger size when doped with metal cations, which affects the luminous efficiency of OLEDs and QLEDs.
The production of clathrated nickel oxide nanoparticles, where nickel oxide nanoparticles are encapsulated by a host, such as cyclodextrin, to maintain a small particle size and prevent aggregation, achieved through a method involving the addition of a base to an aqueous solution containing a nickel salt and host, followed by separation and firing of nickel hydroxide fine particles to form stable nickel oxide nanoparticles.
This approach results in nickel oxide nanoparticles with a small, uniform particle size, enhancing the flatness and luminous efficiency of the hole functional layer in light-emitting devices and display devices by preventing aggregation and ensuring smooth dispersion for improved layer formation.
Smart Images

Figure JP2023019966_05122024_PF_FP_ABST
Abstract
Description
Clathrate nickel oxide nanoparticles, their production method, light-emitting element and display device
[0001] The present disclosure relates to clathrated nickel oxide nanoparticles, a method for producing the same, a light-emitting element, and a display device.
[0002] Various display devices equipped with light-emitting elements have been developed. Known examples of such light-emitting elements include OLEDs (organic light-emitting diodes) and QLEDs (quantum dot light-emitting diodes). The light-emitting elements have a laminated structure of a light-emitting layer and hole functional layers such as an electron transport layer, a hole injection layer, and a hole transport layer. Nickel oxide (NiO) is known as one suitable material for the hole functional layer.
[0003] A NiO hole functional layer is prepared by applying a dispersion of NiO particles, for example, an aqueous dispersion of NiO particles. NiO particles generally tend to aggregate in water. This can reduce the flatness of the prepared hole functional layer and the light-emitting characteristics of the light-emitting device. A known technique for improving the dispersibility of NiO particles in an aqueous dispersion involves precipitating nickel hydroxide from a nickel salt in the presence of a salt of a metal cation to produce nano-sized nickel hydroxide particles doped with the metal cation, and then heat-treating the nickel hydroxide particles. This method produces nano-sized NiO particles doped with the metal cation (see, for example, Patent Document 1).
[0004] Chinese Patent Application Publication No. 101570349
[0005] On the other hand, from the viewpoint of improving the flatness of the hole function layer, it is preferable that the size of the NiO particles is smaller.In the conventional techniques described above, the NiO particles are doped with metal cations, so the size of the NiO particles is larger than that of NiO particles that are not doped with metal cations.
[0006] A first object of one embodiment of the present disclosure is to provide nickel oxide nanoparticles having a small particle size, and a second object of one embodiment of the present disclosure is to realize a flat hole functional layer in a light-emitting element of a display device.
[0007] In order to solve the first problem, the encapsulated nickel oxide nanoparticles according to one embodiment of the present disclosure include nickel oxide nanoparticles and a host that encapsulates the nickel oxide nanoparticles.
[0008] In order to solve the first problem described above, a method for producing clathrate nickel oxide nanoparticles according to one embodiment of the present disclosure includes a first step of adding a base to an aqueous solution containing a nickel salt and a host to obtain an aqueous slurry of clathrate nickel hydroxide fine particles encapsulated by the host; a second step of separating the clathrate nickel hydroxide fine particles from the aqueous slurry; and a third step of calcining the separated clathrate nickel hydroxide fine particles to produce clathrate nickel oxide nanoparticles encapsulated by the host.
[0009] In order to achieve the second object, a light-emitting element according to an aspect of the present disclosure includes a light-emitting layer and a hole functional layer disposed on the light-emitting layer, and the hole functional layer contains the above-described clathrate nickel oxide nanoparticles.
[0010] In order to achieve the second object, a display device according to an aspect of the present disclosure includes the light-emitting element.
[0011] According to the present disclosure, nickel oxide nanoparticles having a small particle size can be provided, and a flat hole functional layer can be realized in a light-emitting element of a display device.
[0012] FIG. 1 is a diagram schematically illustrating clathrate nickel oxide nanoparticles according to an embodiment of the present disclosure. FIG. 2 is a diagram schematically illustrating an example of a process in a method for producing clathrate nickel oxide nanoparticles according to an embodiment of the present disclosure. FIG. 3 is a flowchart illustrating an example of a flow of processes in a method for producing clathrate nickel oxide nanoparticles according to an embodiment of the present disclosure. FIG. 4 is a diagram schematically illustrating a display device according to an embodiment of the present disclosure. FIG. 5 is a diagram schematically illustrating the layer structure of a light-emitting device according to an embodiment of the present disclosure. FIG. 6 is a diagram illustrating an X-ray diffraction chart of the clathrate nickel oxide nanoparticles of Example 1. FIG. 7 is a diagram illustrating an example of ultraviolet-visible spectral absorption spectra of particles and cyclodextrin of each of the examples and comparative examples.
[0013] [Encapsulated Nickel Oxide Nanoparticles] The encapsulated nickel oxide nanoparticles of the present disclosure have nickel oxide nanoparticles and a host that encapsulates the nickel oxide nanoparticles.
[0014] [Nickel oxide nanoparticles] Nickel oxide nanoparticles are nickel oxide particles with a nanometer-order particle size. The particle size is, for example, the particle size cumulative distribution median diameter D50, which can be measured, for example, by dynamic light scattering. Thus, nickel oxide nanoparticles may be substantially composed of particles with a nanometer-order particle size. "Substantially" may mean "within a range in which the effects of the present disclosure can be obtained," and within such a range, the nickel oxide nanoparticles of the present disclosure may include some particles with a micron-order or millimeter-order particle size.
[0015] The particle size of the nickel oxide nanoparticles is preferably as small as possible, for example, D50 of 30 nm or less, more preferably 20 nm or less, and even more preferably 15 nm or less, from the viewpoint of increasing the luminous efficiency of the light-emitting device when the particles are used as a material for the hole functional layer. From the above viewpoint, the particle size of the nickel oxide nanoparticles may be 10 nm or more.
[0016] The nickel oxide nanoparticles may be primary particles or aggregated particles, and the particle size of the nickel oxide nanoparticles is substantially the same as the particle size of the clathrate nickel oxide nanoparticles of the present disclosure.
[0017] [Host] The host is a component that encapsulates nickel oxide nanoparticles. The nickel oxide nanoparticles encapsulated in the host correspond to the guest.
[0018] The host is a component that encases (encapsulates) nickel oxide nanoparticles. The host is preferably a component that encapsulates nickel hydroxide fine particles in an aqueous slurry. One or more hosts may be encapsulated in one nickel oxide nanoparticle. The host is, for example, a compound that has a cavity of a size that matches the size of the guest particle and that has an interaction with the guest. Examples of such interactions include van der Waals forces, hydrogen bonds, hydrophobic bonds, and dipole-dipole interactions.
[0019] The host can be appropriately determined by identifying a compound having a size and molecular structure (skeleton and substituents) suitable for encapsulating a single or multiple nickel oxide nanoparticles through structural analysis of the molecular structure or by searching for such analytical data.
[0020] Furthermore, the host is preferably water-soluble from the viewpoint of encapsulating nickel hydroxide microparticles or nickel oxide nanoparticles in the aqueous slurry. The water solubility of the host can be expressed by hydrophilic structures in the molecular structure and can be adjusted by the number of such hydrophilic structures. Examples of such hydrophilic structures include hydrophilic substituents such as hydroxyl groups. Preferred examples of hosts in the present disclosure include cyclodextrin. The water-soluble host can be present in the system during the production of nickel hydroxide microparticles from nickel salt in the production method described below. Therefore, it is expected that the particle size of the nickel hydroxide microparticles can be controlled by the host by encapsulating nickel hydroxide microparticles of an appropriate size during the production process.
[0021] FIG. 1 is a schematic diagram showing encapsulated nickel oxide nanoparticles according to one embodiment of the present disclosure. As shown in FIG. 1, the encapsulated nickel oxide nanoparticles 5 have nickel oxide nanoparticles 51 and multiple cyclodextrins 52 that encapsulate the nickel oxide nanoparticles 51. The nickel oxide nanoparticles 51 are the guest, and the cyclodextrins 52 are the host. The cyclodextrins 52 are compounds with a cage-like molecular structure. As shown in FIG. 1, the encapsulated nickel oxide nanoparticles of the present disclosure are considered to be such that the multiple cyclodextrins 52 are independently arranged around the nickel oxide nanoparticles 51 in accordance with their structural correlation with the nickel oxide nanoparticles 51.
[0022] Note that FIG. 1 shows that cyclodextrin 52 encapsulates nickel oxide nanoparticles 51, but in the present disclosure, the number of cyclodextrins 52 encapsulating one nickel oxide nanoparticle 51 and the orientation of the cyclodextrins 52 are not limited by FIG. 1 .
[0023] [Method for Producing Clathrate Nickel Oxide Nanoparticles] The clathrate nickel oxide nanoparticles of the present disclosure can be suitably produced by a method including the first to third steps described below.
[0024] [First Step] The first step is a step of adding a base to an aqueous solution containing a nickel salt and a host to obtain an aqueous slurry of clathrated nickel hydroxide fine particles that are clathrated by the host.
[0025] The nickel salt is suitably selected from nickel salts that are water-soluble and produce nickel hydroxide upon addition of a base. The nickel salt may be a hydrate, and may consist of one or more types. For example, the nickel salt may be one or more salts selected from the group consisting of nickel nitrate, nickel chloride, nickel sulfate, and nickel carboxylate.
[0026] As described above, the host is preferably a water-soluble compound. The water-soluble host dissolves in water together with the nickel salt. The water-soluble host is expected to be included in the nickel hydroxide particles when the particles precipitated by the addition of a base grow to an appropriate size. From this perspective, the host is preferably water-soluble so that it dissolves in a sufficient amount in an aqueous solution of the nickel salt, and the cyclodextrin described above is an example of such a preferred host.
[0027] The base can be appropriately selected from known bases within a range that allows adjustment of the pH of the aqueous slurry described below. For example, the base is preferably one or more compounds selected from the group consisting of sodium hydroxide, potassium hydroxide, and ammonium hydroxide.
[0028] The amount of host added to the aqueous solution of nickel salt should be sufficient to encapsulate the resulting nickel hydroxide particles. If the amount of host added is too small, the encapsulation of the nickel hydroxide particles by the host may be insufficient. The amount of host added may be determined appropriately from the above viewpoints, and depending on the molecular structure of the host or the encapsulation amount of the host corresponding to the nickel hydroxide particles. For example, if the host is cyclodextrin, the ratio of the nickel hydroxide particles to the cyclodextrin (nickel hydroxide particles:cyclodextrin) may be about 5:1 by mass (2:0.1 by molar ratio).
[0029] The amount of base added to the aqueous solution of nickel salt may be any amount sufficient to produce nickel hydroxide microparticles. From the viewpoint of obtaining small and uniform clathrate nickel oxide nanoparticles, the base is preferably added so as to adjust the pH of the aqueous solution of nickel salt to preferably 8 or higher, more preferably 9 or higher, and even more preferably 10 or higher. From the above viewpoint, the pH of the aqueous solution of nickel salt at the time of addition of the base is preferably adjusted to 13 or lower, more preferably 12 or lower, and even more preferably 11 or lower.
[0030] The addition of the base to the aqueous solution of the nickel salt may be carried out under room temperature conditions. The temperature of the aqueous solution of the nickel salt when the base is added can be appropriately determined within the range in which nickel hydroxide fine particles are produced, and may be, for example, 20 to 80°C.
[0031] The addition of the base to the aqueous nickel salt solution and the production of the aqueous slurry of nickel hydroxide fine particles in the first step can be carried out under ordinary stirring conditions, and such stirring can be carried out using a known stirring device.
[0032] Incidentally, "aqueous slurry" refers to a dispersion liquid in which the dispersion medium is an aqueous medium. An aqueous medium refers to a medium whose main component is water. The aqueous medium may be water itself, or may further contain other components that are mixed with water. The proportion of water in the aqueous medium may be 50% by mass or more, 70% by mass or more, 80% by mass or more, or 100% by mass. Examples of other components include organic solvents that can be mixed with water in any ratio, such as lower alcohols, pH adjusters such as phosphoric acid or carboxylic acid, and ligands for increasing the dispersibility of nickel hydroxide microparticles in the aqueous slurry. From the viewpoint of achieving the above-mentioned pH adjustment in the first step, it is preferable that the aqueous medium be water itself and contain no other components.
[0033] It is believed that in the first step, one or more hosts are coordinated to the nickel hydroxide microparticles so as to cover or encase a portion of the nickel hydroxide microparticles. Because the host is present in the nickel salt aqueous solution in a sufficient amount relative to the nickel salt, it is believed that when the nickel hydroxide particles precipitated as microparticles grow to an appropriate size, the host is appropriately and sufficiently coordinated to the nickel hydroxide microparticles.
[0034] The nickel hydroxide "fine particles" produced in the first step are sufficiently small particles, having a particle size of less than millimeter order (less than 1 mm), for example, micro-order or nano-order particles. The particle size of the nickel hydroxide fine particles is, for example, the cumulative particle size distribution median diameter D50, as described for the nickel oxide nanoparticles, and can be measured, for example, by dynamic light scattering.
[0035] The aqueous slurry produced in the first step has a light blue appearance compared to an aqueous slurry produced without adding a host, but is less white and more transparent. This is thought to be because the production of nickel hydroxide fine particles and the coordination (inclusion) of the host proceed simultaneously, preventing the nickel hydroxide fine particles from aggregating in water and making it easier for the produced particles to remain small.
[0036] [Second Step] The second step is a step of separating the clathrate nickel hydroxide fine particles from the aqueous slurry. The separation of the clathrate nickel hydroxide fine particles from the aqueous slurry can be carried out by a known solid-liquid separation method capable of separating nano-order fine particles from an aqueous medium. For example, the separation can be carried out by filtration, decantation, or centrifugation. It is believed that the inclusion state of the host that encapsulates the clathrate nickel hydroxide fine particles remains unchanged before and after the separation.
[0037] [Third Step] The third step is a step of calcining the separated clathrate nickel hydroxide microparticles to produce clathrate nickel oxide nanoparticles in which the host is encapsulated. The calcination temperature may be any temperature at which water molecules are desorbed from nickel hydroxide, for example, 230 to 270°C. If the calcination temperature is too high, the host encapsulating the nickel oxide nanoparticles may be desorbed from the nickel oxide nanoparticles or may undergo thermal decomposition. From the viewpoint of enhancing the stability of the production of clathrate nickel oxide nanoparticles, it is preferable that the host in the present disclosure has a melting point or boiling point higher than the temperature at which water molecules are desorbed from nickel hydroxide. From this viewpoint as well, a preferred embodiment of the present disclosure is that the host is cyclodextrin.
[0038] The firing may be carried out in an air atmosphere or in an atmosphere of a gas that is inert to the firing, such as nitrogen gas.
[0039] The nickel oxide nanoparticles obtained by calcination in the third step are the clathrate nickel oxide nanoparticles of the present disclosure. It is believed that the inclusion state of the host that encapsulates the clathrate nickel oxide fine particles does not change before and after calcination.
[0040] The clathrate nickel oxide nanoparticles obtained in the third step have a black appearance, but compared to nickel oxide nanoparticles produced without adding a host in the preparation of the aqueous slurry, they have a stronger black appearance, a smaller overall particle bulk, and better fluidity. This is thought to be because the fine particle state at the time of aqueous slurry production is maintained even after calcination.
[0041] [Other Steps] The manufacturing method of the present disclosure may further include other steps in addition to the above-described first to third steps, as long as the effects of the present disclosure can be obtained. The other steps may be included as part of the above-described first to third steps, or may be performed as separate steps.
[0042] For example, in the manufacturing method of the present disclosure, the aqueous slurry may further be subjected to a dispersion treatment in the first step. Such a dispersion step can be carried out, for example, by irradiation with ultrasonic waves. The dispersion treatment of the aqueous slurry in the first step is preferable from the viewpoint of promoting the mixing of the components in the aqueous slurry and suppressing the coarsening (aggregation) of the nickel hydroxide fine particles produced. The dispersion step may be carried out alone or simultaneously with other operations such as stirring the aqueous slurry. The temperature in the dispersion step may be adjusted to a specific temperature, or may be a temperature elevated from that before irradiation due to ultrasonic irradiation. The treatment time in the dispersion step (or irradiation time in the case of ultrasonic irradiation) may be, for example, about 1 hour, as long as the effect of the dispersion step is sufficiently exhibited.
[0043] Furthermore, the production method of the present disclosure may further include a water-washing step of washing the clathrate nickel hydroxide fine particles separated from the aqueous slurry in the second step. The clathrate nickel hydroxide fine particles separated from the aqueous slurry may contain other water-soluble nickel salts produced as by-products. The inclusion of this water-washing step in the production method of the present disclosure is advantageous from the viewpoint of increasing the purity of the clathrate nickel hydroxide fine particles separated in the second step.
[0044] The production method of the present disclosure may further include a drying step of drying the clathrate nickel hydroxide fine particles separated in step 2. Including the drying step in the production method of the present disclosure is advantageous from the viewpoint of uniforming the state of the clathrate nickel hydroxide fine particles to be subjected to step 3 and stably carrying out step 3.
[0045] Furthermore, the manufacturing method of the present disclosure may further include a crushing step of crushing agglomerates of the clathrate nickel hydroxide fine particles to be subjected to the third step. Nickel hydroxide is crystalline, and this crystallinity can cause the nickel hydroxide fine particles to strongly aggregate together. The manufacturing method of the present disclosure further includes the crushing step, which is advantageous from the viewpoint of uniformly calcining the clathrate nickel hydroxide fine particles in the third step, improving the calcination quality, and shortening the calcination time.
[0046] [Specific Example of Manufacturing Method] The manufacturing method of the present disclosure will be further described with reference to the drawings. Fig. 2 is a diagram for schematically illustrating an example of steps in a manufacturing method of clathrate nickel oxide nanoparticles according to an embodiment of the present disclosure. Fig. 3 is a flowchart illustrating an example of the flow of steps in a manufacturing method of clathrate nickel oxide nanoparticles according to an embodiment of the present disclosure.
[0047] In step S1, nickel nitrate hexahydrate (NiNO 3 ・6H 2 O) and cyclodextrin (CD) were dissolved in pure water, and a cyclodextrin-nickel nitrate aqueous solution (NiNO 3 ・6H 2 O-CD aqueous solution) 1. 3 ・6H 2 The ratio of CD to O (NiNO 3 ・6H 2 O / CD) is, for example, 5 in mass ratio.
[0048] In step S2, NiNO 3 ・6H 2 Add 2 aqueous sodium hydroxide solution to 1 aqueous O-CD solution to obtain NiNO 3 ・6H 2 The pH of the O-CD aqueous solution 1 is adjusted to 12. Then, in step S3, Ni(OH)2 Ni(OH) was added to the water slurry while irradiating it with ultrasound. 2 The aqueous slurry is stirred. The stirring time of the aqueous slurry and the ultrasonic irradiation time are, for example, about 1 hour. 3 ・6H 2 O is nickel hydroxide (Ni(OH) 2 ), and as a result, nickel hydroxide fine particles 3 are dispersed in water, forming Ni(OH) 2 A water slurry of fine particles 3 is produced. The particles in the water slurry are Ni(OH) 2 Nickel hydroxide nanoparticles in which nanoparticles are encapsulated by CD (CD / Ni(OH) 2 Nanoparticles) 4. Steps 1 to 3 correspond to the first process described above.
[0049] In step S4, the aqueous slurry is centrifuged to separate the CD / Ni(OH) 2 The nanoparticles 4 are separated. Step 4 corresponds to the second step described above. If necessary, the separated CD / Ni(OH) 2 The nanoparticles 4 are washed with water. Then, in step S5, the separated CD / Ni(OH) 2 The nanoparticles 4 are dried. 2 In nanoparticle 4, the white circle in the center represents a nickel hydroxide fine particle, and the trapezoid surrounding it represents the CD that encapsulates the fine particle.
[0050] In step S6, the dried CD / Ni(OH) 2 The nanoparticles 4 are deagglomerated. For separation from the water slurry, the CD / Ni(OH) 2 The nanoparticles 4 are wet and therefore tend to form agglomerates, and it is preferable to crush the agglomerates after drying in order to heat the particles uniformly in the subsequent firing step and to shorten the firing time.
[0051] In step S7, the dried and crushed CD / Ni(OH) 2 The nanoparticles 4 are calcined at 230-270°C. The calcination results in CD / Ni(OH) 2Water is released from the nanoparticles 4, and the nickel hydroxide particles become nickel oxide particles. Thus, nickel oxide nanoparticles (NiO nanoparticles) are encapsulated with CD to form clathrated nickel oxide nanoparticles (CD / NiO nanoparticles) 5. In the CD / NiO nanoparticles 5 in FIG. 2, the black circle in the center represents the nickel oxide nanoparticle, and the trapezoids around it represent the CDs encapsulating the nanoparticles. In this way, powder of CD / NiO nanoparticles 5 is obtained. Step 7 corresponds to the third step described above.
[0052] The clathrate nickel oxide nanoparticles of the present disclosure have a nano-order particle size, and the particle size is small and uniform. The clathrate nickel oxide nanoparticles of the present disclosure are suitable for use as a material for a hole functional layer in a light-emitting device, and can realize a flat hole functional layer in a display device.
[0053] [Light-emitting element and display element] [Light-emitting element] The light-emitting element of the present disclosure includes a light-emitting layer and a hole functional layer disposed so as to overlap the light-emitting layer, and the hole functional layer contains the encapsulated nickel oxide nanoparticles of the present disclosure.
[0054] The light-emitting layer is a layer that emits light by the combination of holes (positive holes) and charges (electrons). The hole functional layer is a layer that has the function of supplying holes to the light-emitting layer. Examples of hole functional layers include a hole injection layer for stabilizing the injection of holes into the light-emitting layer and a hole transport layer for stabilizing the transport of holes to the light-emitting layer.
[0055] The light-emitting element of the present disclosure can be configured in the same manner as known light-emitting elements including a light-emitting layer and a hole functional layer, except that the hole functional material constituting the hole functional layer is the encapsulated nickel oxide nanoparticles of the present disclosure.
[0056] [Display Device] The display device of the present disclosure includes the light-emitting element of the present disclosure. The display device of the present disclosure is, for example, a full-color display device having light-emitting elements that emit light of each color of RGB, and at least one of the light-emitting elements of each color includes the light-emitting element of the present disclosure. The display device of the present disclosure can be configured in the same manner as known display devices that include light-emitting elements, except that it includes the light-emitting element of the present disclosure.
[0057] [Specific Embodiments] The display device and light-emitting device of the present disclosure will be further described below with reference to the drawings. In the following description, when a symbol R, G, or B representing each emitted color is added to a symbol, it means a configuration of a specific emitted color, and when a symbol representing each emitted color is not added, it means a configuration common to all colors regardless of the emitted color.
[0058] FIG. 4 is a schematic diagram illustrating a display device according to an embodiment of the present disclosure. As shown in FIG. 4 , the display device 100 includes a frame region NDA and a display region DA. The display region DA of the display device 100 includes a plurality of pixels PIX, each of which includes a red subpixel RSP, a green subpixel GSP, and a blue subpixel BSP. The red subpixel RSP includes a red light-emitting element 10R, the green subpixel GSP includes a green light-emitting element 10G, and the blue subpixel BSP includes a blue light-emitting element 10B. The light-emitting elements of each color are light-emitting elements according to the present disclosure. In the stacking direction, the display device 100 has a configuration in which, for example, a substrate, a barrier layer, a thin-film transistor, a bank and light-emitting element, a sealing layer, and a functional film are stacked in this order.
[0059] Fig. 5 is a diagram schematically illustrating the layer configuration of a light-emitting element according to an embodiment of the present disclosure. As shown in Fig. 5, a light-emitting element 10 is disposed on a barrier layer 12 disposed on a substrate 11. The barrier layer 12 is formed of, for example, an insulator. Banks 13 are formed on the barrier layer 12 to separate the subpixels SP in the planar direction. The light-emitting element 10 is configured by stacking a first electrode 21, a hole injection layer 22, a hole transport layer 23, a light-emitting layer 24, an electron transport layer 25, and a second electrode 26 in this order. Examples of the light-emitting element 10 include an OLED and a QLED.
[0060] The first electrode 21 is also referred to as an anode. The first electrode 21 is conductive and has optical properties such as reflecting part of visible light and transmitting the rest. The first electrode 21 includes both an electrode material that reflects visible light and an electrode material that transmits visible light.
[0061] Examples of electrode materials that reflect visible light include metal materials such as Al, Mg, Li, and Ag, alloys of these metal materials, and stacks (e.g., ITO / Ag / ITO) of these metal materials or their alloys with transparent metal oxides (e.g., indium tin oxide (ITO), indium zinc oxide, indium gallium zinc oxide, etc.). Examples of electrode materials that transmit visible light include thin films made of transparent metal oxides, metal materials such as Al and Ag, and nanowires made of these metal materials.
[0062] The first electrode 21 can be formed by a known method for forming an electrode layer in a light-emitting device. For example, the first electrode 21 can be formed by a physical vapor deposition (PVD) method or a chemical vapor deposition (CVD) method. Examples of physical vapor deposition methods include vacuum deposition, sputtering, electron beam (EB) deposition, and ion plating. Examples of methods for patterning the first electrode 21 include photolithography and inkjet printing.
[0063] The hole injection layer 22 is composed of a hole injection material capable of stabilizing the injection of holes into the light emitting layer 24. The hole injection material may be one or more types. Examples of hole injection materials include the encapsulated nickel oxide nanoparticles of the present disclosure, as well as poly(3,4-ethylenedioxythiophene):polystyrenesulfonic acid (PEDOT:PSS), Ni(OH) 2 , and CuSCN.
[0064] The hole transport layer 23 is composed of a hole transport material that can stabilize the transport of holes into the light-emitting layer 24. The hole transport material may be one or more types. Examples of hole transport materials include the encapsulated nickel oxide nanoparticles of the present disclosure, as well as poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl))diphenylamine)] (TFB), Ni(OH) 2 and poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine] (poly-TPD).
[0065] In the present disclosure, the encapsulated nickel oxide nanoparticles of the present disclosure may be contained in only one of the hole injection layer 22 and the hole transport layer 23, or may be contained in both.
[0066] The hole injection layer 22 or hole transport layer 23 containing the encapsulated nickel oxide nanoparticles of the present disclosure can be prepared by applying an ink containing the encapsulated nickel oxide nanoparticles. The hole injection layer 22 or hole transport layer 23 can be prepared by any known method for preparing a layer of a light-emitting device by applying an ink, except that an ink containing the encapsulated nickel oxide nanoparticles is used. For example, the hole injection layer 22 or hole transport layer 23 can be prepared using a slit coater or inkjet printing.
[0067] The encapsulated nickel oxide nanoparticles of the present disclosure are small, uniform nanoparticles that are encapsulated by a host. Therefore, they are uniformly dispersed in the ink solvent. A solvent with appropriate wettability for the application area is selected as the ink solvent. By applying ink containing uniformly dispersed encapsulated nickel oxide nanoparticles, the encapsulated nickel oxide nanoparticles are uniformly applied to the application area, forming a flat layer. Therefore, in the present disclosure, a flat hole injection layer 22 or hole transport layer 23 can be formed using the encapsulated nickel oxide nanoparticles.
[0068] The light-emitting layer 24 may be composed of quantum dots (QDs). QDs refer to dots with a maximum width of 100 nm or less. The shape of the QDs may be spherical (circular cross-sectional shape), or may be, for example, polygonal cross-sectional shape, rod-like shape, branch-like shape, or a three-dimensional shape with an uneven surface, or a combination thereof.
[0069] The QDs may have a core structure, a core / shell structure, a core / shell / shell structure, or a core / shell structure with a continuously varying core / shell ratio. The QDs may have a ligand, and if the QD has a core structure, the ligand may be provided on the surface of the core structure, or if the QD has a shell structure, the ligand may be provided on the surface of the shell structure.
[0070] Materials that make up the core structure of QDs include, if they are unicomponent, Si and C. If they are binary, they include CdSe, CdS, CdTe, InP, GaP, InN, ZnSe, ZnS, and ZnTe. If they are ternary, they include CdSeTe, GaInP, and ZnSeTe. If they are quaternary, they include AIGS.
[0071] Binary materials that make up the shell structure of QDs include CdS, CdTe, CdSe, ZnS, ZnSe, and ZnTe, and ternary materials include CdSSe, CdTeSe, CdSTe, ZnSSe, ZnSTe, ZnTeSe, and AIP.
[0072] The electron transport layer 25 is made of an electron transporting material that can stabilize the transport of electrons into the light-emitting layer 24. Examples of the electron transporting material include fine particles containing one or more elements selected from the group consisting of Zn, Mg, Ti, Si, Sn, W, Ta, Ba, Zr, Al, Y, and Hf.
[0073] The second electrode 26 is also referred to as a cathode. The second electrode 26 is conductive, for example, conductive and transparent to visible light. Examples of electrode materials constituting the second electrode 26 include the above-mentioned electrode materials that are transparent to visible light, such as ITO and Ag nanowires (NW). The second electrode 26 can be fabricated by the method described above for the first electrode 21 using a method appropriate for the electrode material. From the viewpoint of simplifying the manufacturing process, the second electrode 26 is integrally formed on both the electron transport layer 25 and the bank 13. The second electrode 26 is formed on the electron transport layer 25, but does not necessarily have to be formed on the bank 13.
[0074] [Major Actions and Effects] In the synthesis of nickel oxide particles by the sol-gel method, an inorganic base such as sodium hydroxide or potassium hydroxide is generally reacted with a nickel salt to produce intermediate nickel hydroxide particles. In this method, the distance between the particles produced is not maintained, and they tend to become hard crystalline. Therefore, when producing nickel oxide particles by calcination, calcination as is tends to produce agglomerated nickel oxide particles, and the nickel oxide particles themselves tend to become large.
[0075] When the hole function layer is prepared by coating ink, the ink is generally filtered before coating. A filter with a sufficiently small pore size, such as a membrane filter, is usually used for this filtration. When nickel oxide nanoparticles are prepared without adding a guest, the ink contains coarse nickel oxide particles due to the above-mentioned aggregation. Therefore, when the ink is filtered before coating, the coarse particles are filtered out, which can clog the filter and affect the smooth preparation of the hole function layer.
[0076] If the technology described in Patent Document 1 is adopted to suppress aggregation during the production of nickel hydroxide fine particles, the size of the nickel oxide particles will increase due to the doping of metal cations, as described above. For example, the particle size of the nickel oxide particles measured using a scanning electron microscope (SEM) is 150 nm. Thus, the nickel oxide particles described in Patent Document 1 are nano-order particles, and although the occurrence of the clogging described above can be suppressed, they have a large particle size.
[0077] In the present disclosure, a guest such as CD is used in the inclusion compound during the synthesis process, which produces guest-encapsulated nickel hydroxide particles as an intermediate, followed by a calcination process to obtain guest-encapsulated nickel oxide nanoparticles.
[0078] The clathrate nickel oxide nanoparticles are surrounded by the host as guests. This prevents the clathrate nickel oxide nanoparticles from aggregating. Furthermore, the clathrate nickel oxide nanoparticles are less likely to aggregate and are easily dispersed in water. Therefore, when ink for producing the hole function layer is prepared, aggregation in the ink is also prevented.
[0079] Furthermore, the clathrate nickel oxide nanoparticles have a particle size that can be surrounded by the host, and the particle size and crystallite size of the clathrate nickel oxide nanoparticles are smaller than those of nickel oxide nanoparticles produced without the addition of a host. For example, the size of the clathrate nickel oxide nanoparticles of the present disclosure can be about 5 nm, as calculated using the Scherrer formula from the peaks specific to nickel oxide in an X-ray diffraction chart. The crystallite size of nickel oxide nanoparticles is smaller than the particle size of primary particles, but in crystalline particles, the smaller the crystallite size, the smaller the primary particle size tends to be. The clathrate nickel oxide nanoparticles of the present disclosure are non-agglomerated particles, as described above. Therefore, a crystallite size of about 5 nm in the clathrate nickel oxide nanoparticles of the present disclosure suggests that the particle size of the clathrate nickel oxide nanoparticles is about 10 nanometers, as measured by the dynamic light scattering method described above. Therefore, the ink for the hole function layer containing the clathrated nickel oxide nanoparticles of the present disclosure can smoothly pass through a filter for filtration before application, for example, a filter with a pore size of 0.45 μm, and the hole function layer produced has excellent flatness and does not produce the above-mentioned white spots in the light-emitting element.
[0080] Thus, the present disclosure provides clathrate nickel oxide nanoparticles having nickel oxide nanoparticles and a host encapsulating the nickel oxide nanoparticles, and the clathrate nickel oxide nanoparticles can be produced by a method including the above-described steps 1 to 3. Thus, the present disclosure provides nickel oxide nanoparticles with small particle size and high size uniformity.
[0081] Furthermore, such clathrate nickel oxide nanoparticles can be used as a material for a hole functional layer of a light-emitting element including a light-emitting layer and a hole functional layer disposed over the light-emitting layer, and the light-emitting element can be applied to a display device. The use of such clathrate nickel oxide nanoparticles allows a flat hole functional layer to be realized in the light-emitting element of a display device. Furthermore, a flat hole functional layer formed from such uniform and small-sized clathrate nickel oxide nanoparticles is expected to contribute to improving the light-emitting characteristics of a QLED having such a hole functional layer.
[0082] From the viewpoint of producing nickel hydroxide as an intermediate in the production of such clathrate nickel oxide nanoparticles, known nickel salts such as one or more salts selected from the group consisting of nickel nitrate, nickel chloride, nickel sulfate, and nickel carboxylate can be suitably used as the nickel salt.
[0083] Furthermore, it is possible to use a compound having a molecular structure capable of encapsulating nickel oxide nanoparticles as the host, and more preferably, cyclodextrin is preferably used from the viewpoint of producing nickel hydroxide fine particles as an intermediate and encapsulated nickel oxide nanoparticles as the final product.
[0084] In addition, in the present disclosure, the host added in the production of nickel hydroxide microparticles is preferably water-soluble, which is advantageous for obtaining clathrate nickel oxide nanoparticles with small crystallite size and good particle size distribution.
[0085] [Summary] The configuration of the present disclosure can improve the flatness of the light-emitting element of a display device, particularly the flatness of the hole functional layer, and is expected to enable the light-emitting element and the display device to exhibit desired light-emitting characteristics or further improve the light-emitting characteristics. Therefore, the present disclosure is expected to contribute to achieving the goals of the United Nations' Sustainable Development Goals (SDGs), such as expanding technological innovation and ensuring sustainable consumption and production patterns.
[0086] The present disclosure is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present disclosure. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment.
[0087] An embodiment of the present disclosure is described below.
[0088] Example 1 The following components were mixed in the following amounts to obtain an aqueous solution containing cyclodextrin and nickel nitrate: Nickel nitrate hexahydrate 5.81 g, Cyclodextrin 1.0 g, Water 100 ml
[0089] While stirring the resulting aqueous solution, 10 M aqueous sodium hydroxide solution was added to the aqueous solution to adjust the pH of the resulting mixture to 12. The mixture was further stirred for 1 hour while being irradiated with ultrasound. In this way, an aqueous slurry of nickel hydroxide nanoparticles was obtained. The aqueous slurry was pale blue in color.
[0090] The resulting aqueous slurry was centrifuged and washed several times to remove the water-soluble nitrate by-product in the aqueous slurry. The dispersion medium (water) of the aqueous slurry from which the by-product salt had been removed was then distilled off, and the resulting cake of nickel hydroxide nanoparticles was dried at 80°C. The cake was baked at 275°C for 2 hours, and the baked cake was crushed in a mortar. Nickel oxide nanoparticles 51 were thus obtained by baking the light blue nickel hydroxide nanoparticles. The resulting nickel oxide nanoparticles 51 were black in color.
[0091] One part by mass of nickel oxide nanoparticles 51 was dispersed in an alcohol-based solvent to prepare ink 61 for fabricating a hole functional layer. The concentration of nickel oxide nanoparticles 51 in ink 61 was 0.1 to 10 mass %. Ink 61 was filtered through a membrane filter (pore size: 0.45 μm), and a hole transport layer having a thickness of 10 to 150 nm was fabricated using the filtered ink 61, thereby fabricating a light-emitting device having the layer structure shown in FIG.
[0092] When the membrane filter after filtration was visually inspected, no particulate matter was found remaining on the filter. Furthermore, when the fabricated light-emitting device was visually inspected from the second electrode side, no granular protrusions (white dots) were found.
[0093] Comparative Example 1 A nickel nitrate aqueous solution was prepared without adding cyclodextrin, and black nickel oxide nanoparticles C1 were obtained in the same manner as in Example 1, except that the nickel nitrate aqueous solution was used. Ink C1 was prepared in the same manner as in Example 1, except that the black nickel oxide nanoparticles C1 were used, and a light-emitting device was fabricated that included a hole transport layer prepared using ink C1.
[0094] Visual inspection of the membrane filter after filtration confirmed that black particles remained on almost the entire upper surface of the filter. Visual inspection of the fabricated light-emitting device from the second electrode side confirmed that white dots caused by granular protrusions were scattered on the filter.
[0095] [Evaluation] (1) X-ray Diffraction Method The nickel oxide nanoparticles 51 of Example 1 and the black nickel oxide nanoparticles C1 of Comparative Example 1 were each measured by X-ray diffraction (XRD). The XRD chart of the nickel oxide nanoparticles 51 of Example 1 is shown in Figure 6. From this XRD chart, it was confirmed that the nickel oxide nanoparticles 51 were nickel oxide particles. The XRD chart of the black nickel oxide nanoparticles C1 also showed peaks similar to those in the XRD chart of Figure 6, and it was confirmed from XRD that the black nickel oxide nanoparticles C1 were also nickel oxide particles.
[0096] (2) Crystallite Size For each of the nickel oxide nanoparticles 51 of Example 1 and the black nickel oxide nanoparticles C1 of Comparative Example 1, the crystallite sizes of the crystals at peaks where 2θ was around 37°, 43°, and 62.5° in the XRD chart were determined using Scherrer's formula. As a result, the crystallite size of the nickel oxide nanoparticles 51 of Example 1 was approximately 5 nm. The crystallite size of the black nickel oxide nanoparticles C1 was approximately 5 to 15 nm, which was larger than the crystallite size of the nickel oxide nanoparticles 51.
[0097] (3) Ultraviolet-visible (UV-VIS) Spectroscopic Analysis A 0.4 mass % aqueous dispersion of the nickel oxide nanoparticles 51 of Example 1 was prepared, and the aqueous dispersion was diluted two-fold with pure water to prepare a two-fold diluted solution (CD / NiO-2-fold diluted solution, particle concentration: 0.2 mass %), a three-fold diluted solution was diluted three-fold with pure water to prepare a three-fold diluted solution (CD / NiO-3-fold diluted solution, particle concentration: approximately 0.07 mass %), and a six-fold diluted solution was diluted six-fold with pure water to prepare a six-fold diluted solution (CD / NiO-6-fold diluted solution, particle concentration: approximately 0.01 mass %).
[0098] Next, a 0.4 mass% aqueous dispersion of the black nickel oxide nanoparticles C1 of Comparative Example 1 was prepared, and this was diluted two-fold with pure water to prepare a two-fold diluted solution (NiO-2-fold diluted solution, particle concentration 0.2 mass%). Furthermore, a 0.4 mass% aqueous dispersion of cyclodextrin was prepared, and this was diluted two-fold with pure water to prepare a two-fold diluted solution (CD-2-fold diluted solution, concentration 0.2 mass%). The UV-VIS spectroscopic absorption spectrum of the above diluted solution was measured. The results are shown in FIG. 7.
[0099] As is clear from Figure 7, although the CD / NiO-2-fold diluted solution and the NiO-2-fold diluted solution have the same concentration, the absorption peak of the CD / NiO-2-fold diluted solution is clearly smaller than that of the NiO-2-fold diluted solution. Furthermore, the CD-2-fold diluted solution has substantially no absorption peak at a wavelength of approximately 250 nm. From these results, it is believed that the absorption peak of the CD / NiO-2-fold diluted solution is weakened in intensity by the influence of the CD-2-fold diluted solution compared to the absorption peak of the NiO-2-fold diluted solution. Therefore, nickel oxide nanoparticles 51 are considered to be particles in which cyclodextrin covers nickel oxide nanoparticles, i.e., particles that are encapsulated by cyclodextrin.
[0100] Furthermore, the absorption peaks of the CD / NiO-2-fold diluted solution, the CD / NiO-3-fold diluted solution, and the CD / NiO-6-fold diluted solution decrease as the concentration decreases, but the peak wavelengths of these absorption peaks are substantially the same. Therefore, in nickel oxide nanoparticles 51, the optical effect of cyclodextrin on nickel oxide nanoparticles is considered to be the same regardless of the concentration of the dilution. Therefore, in nickel oxide nanoparticles 51, the number of cyclodextrins encapsulating one nickel oxide nanoparticle is considered to be substantially constant regardless of the concentration of the dilution. From the above, nickel oxide nanoparticles 51 are considered to be particles formed by encapsulating one nickel oxide nanoparticle with a specific number of cyclodextrins, as shown in FIG. 1 above.
[0101] The present disclosure is expected to be utilized in the production of fine, uniform, nano-order inorganic particles having strong crystallinity, and in a technology for improving the flatness of a functional layer in a light-emitting device having such a functional layer made of the inorganic particles.
[0102] REFERENCE SIGNS LIST 1 Cyclodextrin-nickel nitrate aqueous solution 2 Sodium hydroxide aqueous solution 3 Nickel hydroxide microparticles 4 Clathrated nickel hydroxide microparticles 5 Clathrated nickel oxide nanoparticles 10 Light-emitting element 11 Substrate 12 Barrier layer 13 Bank 21 First electrode 22 Hole injection layer 23 Hole transport layer 24 Light-emitting layer 25 Electron transport layer 26 Second electrode 51 Nickel oxide nanoparticles 52 Cyclodextrin 100 Display device DA Display area NDA Frame area PIX Pixel SP Subpixel
Claims
1. Encapsulated nickel oxide nanoparticles comprising nickel oxide nanoparticles and a host in which the nickel oxide nanoparticles are encapsulated.
2. The encapsulated nickel oxide nanoparticles of claim 1, wherein the host is a cyclodextrin.
3. A method for producing clathrate nickel oxide nanoparticles, comprising: a first step of adding a base to an aqueous solution containing a nickel salt and a host to obtain an aqueous slurry of clathrate nickel hydroxide fine particles that are encapsulated by the host; a second step of separating the clathrate nickel hydroxide fine particles from the aqueous slurry; and a third step of calcining the separated clathrate nickel hydroxide fine particles to produce clathrate nickel oxide nanoparticles that are encapsulated by the host.
4. The method for producing clathrate nickel oxide nanoparticles according to claim 3, wherein the nickel salt is one or more salts selected from the group consisting of nickel nitrate, nickel chloride, nickel sulfate and nickel carboxylate.
5. A light-emitting device comprising: a light-emitting layer; and a hole functional layer disposed so as to overlap the light-emitting layer, the hole functional layer including the encapsulated nickel oxide nanoparticles according to claim 1 or 2.
6. A display device comprising the light-emitting element according to claim 5.
Citation Information
Patent Citations
Composite material, preparation method thereof and quantum dot light-emitting diode
CN112397670A
Preparation method and application of nickel oxide nanoparticles
CN115043445A
Self-assembled nanostructured particles and method for preparing the same
JP2015501197A