Composite bulk block for manufacturing prosthesis, manufacturing method therefor, and prosthesis manufactured therefrom
The composite bulk block, featuring an amorphous glass matrix with crystalline phases and a polymer, addresses the limitations of existing dental prosthetic materials by providing immediate processing and natural tooth-like aesthetics and mechanical properties, suitable for CAD/CAM systems.
Patent Information
- Application Number
- PCT/KR2024/006835
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
AI Technical Summary
Current dental prosthetic materials, such as porcelain and metal, face challenges in aesthetics and physical properties, while zirconia and crystallized glass materials require heat treatment, making them unsuitable for immediate use as one-day prosthetics due to low processability and cracking issues at the margin area.
A composite bulk block combining an amorphous glass matrix with a crystalline phase, including leucite or lithium disilicate, and a polymer, which allows for immediate processing and has a gradient of light transmittance and color, mimicking natural teeth, with a biaxial bending strength of 180 to 260 MPa and a light transmittance gradient of 30 to 40%.
The composite bulk block enables quick and easy processing of aesthetic and functional restorations, replicating natural teeth with improved structural stability and aesthetics, suitable for CAD/CAM systems, and can be manufactured into a prosthesis with excellent color reproducibility and mechanical properties.
Smart Images

Figure PCTKR2024006835-APPB-IMG-000001 
Figure PCTKR2024006835-APPB-IMG-000002 
Figure PCTKR2024006835-APPB-IMG-000003
Abstract
Description
Composite bulk block for manufacturing prosthetics, method for manufacturing the same, and prosthetics manufactured therefrom
[0001] The present invention relates to a composite bulk block for manufacturing a dental prosthesis that can quickly and easily process an aesthetic and functional restoration that imitates a natural tooth, a method for manufacturing the same, and a prosthesis manufactured therefrom.
[0002] As the dental industry has developed, problems with the physical properties and aesthetics of teeth have emerged, leading to a gradual decline in market share for existing prosthetic materials such as porcelain and metal. To replace these, materials such as crystallized glass and zirconia are increasing their market share. Furthermore, the previously used hot pressing method for prosthetic manufacturing has the problem of long production times, making it difficult to produce the one-day prosthetics currently promoted in the dental market. Consequently, a shift towards CAD / CAM systems is underway. To support this shift, the utility of 1:1 processing materials, which can be processed and implanted immediately without additional heat treatment of crystallized glass, is being highlighted.
[0003] Of course, with the development of zirconia and crystallized glass, many materials with good aesthetics and high physical properties are being used, but most ceramic materials undergo a crystallization heat treatment process after processing, making them difficult to use as one-day prosthetics.
[0004] In addition, in the case of ceramic materials currently being processed in a 1:1 ratio, there is a problem in that the processability is low due to the use of ceramic materials that have already undergone crystallization, and there is a problem in that breakage occurs in the margin area (the boundary area between the prosthesis and the tooth).
[0005] To address these issues and meet the demands of the current dental market, composites, which combine organic and inorganic materials, have been developed. Composites are complementary materials, with the organic material suppressing brittleness, a drawback of inorganic materials, and the inorganic material enhancing the organic material's properties, such as low strength. Furthermore, composites offer the advantage of 1:1 machining, allowing immediate implantation into the oral cavity. This is why new products are being released as the technology continues to develop. Currently, commercially available composites have a strength of approximately 150 to 200 MPa, and their machinability is superior to that of conventional 1:1 machinable glass ceramics.
[0006] The present inventors have disclosed, in relation to such a composite, in Korean Patent Registration No. 10-1682542, a method for manufacturing a dental block, which comprises the steps of: preparing a glass ceramic; forming a porous ceramic body by porousing the glass ceramic; a first infiltration step of first infiltrating a polymer into the ceramic porous body in a vacuum chamber under vacuum; and a second infiltration step of secondly infiltrating a polymer into the ceramic porous body before the first infiltrated polymer is completely cured, and is characterized in that it realizes a biaxial flexural strength of 100 to 150 MPa.
[0007] The glass ceramic here is a feldspathic glass ceramic, and specifically, it contains 2.0 to 6.0 wt% of N2O, 60.0 to 65.0 wt% of SiO2, 8.0 to 15.0 wt% of K2O, 0.5 to 3.0 wt% of CaO, 0.5 to 2.0 wt% of BaO, 0.2 to 1.0 wt% of CeO2, 0 to 0.5 wt% of TiO2, 16.0 to 19.0 wt% of Al2O3 to increase the glass transition temperature and softening point and to enhance the chemical durability of the crystallized glass, and 0 to 1.0 wt% of a coloring component that affects the coloring such as brightness and saturation and exhibits fluorescence.
[0008] In addition, Korean Patent Registration No. 10-1609291 discloses a method for producing a glass, comprising: a step of crushing glass and then melting it at a temperature of 1,400 to 1,800°C; a step of cooling the melted glass, then crushing it, and performing a crystallization heat treatment on the crushed glass at a temperature of 875 to 970°C; a step of re-crushing the crystallized glass that has undergone the crystallization heat treatment, and then performing a porous heat treatment at a temperature of 700 to 840°C; A method for manufacturing a dental block is disclosed, comprising a step of infiltrating a polymer into a porous body formed in crystallized glass that has undergone the above porous heat treatment, wherein the glass melted at a temperature of 1,400 to 1,800°C comprises 2.0 to 6.0 wt% of N2O, 60 to 65.0 wt% of SiO2, 8.0 to 15 wt% of K2O, 0.5 to 3.0 wt% of CaO, 0.5 to 2.0 wt% of BaO, 0.2 to 1.0 wt% of CeO2, more than 0.5 wt% of TiO2O, and 16.0 to 19.0 wt% of Al2O3.
[0009] Specifically, the glass here was also feldspathic glass, and the resulting block was disclosed to have a biaxial flexural strength of approximately 100 to 150 MPa.
[0010] On the other hand, Korean Patent Registration No. 10-212202 discloses a method for manufacturing a composite using a chemical bond between an inorganic substance and an organic substance using a silane coupling agent. Specifically, the method comprises the steps of: adding a thermal initiator to a first mixture in which at least two or more organic substances having different viscosities are mixed at 20 to 70°C; surface-treating an inorganic substance using a second mixture in which 10 to 14 wt% of an acrylic silane coupling agent is mixed in ethanol; mixing the first mixture to which the thermal initiator has been added and the inorganic substance surface-treated by the second mixture; and curing using thermal polymerization at 100 to 150°C.
[0011] In addition, in Korean Patent Registration No. 10-2228118, a dental composite composition including crystallized glass and a curable organic material is proposed, wherein the crystallized glass has an average crystal size of 50 to 400 nm, and a biaxial flexural strength of 200 to 300 MPa and a Vickers hardness of 270 to 300 Hv, which can provide a dental composite composition.
[0012] As another example, U.S. Patent No. 7,807,227 discloses a composite material comprising a porous inorganic-nonmetallic matrix and a second material, and a method for producing the same, comprising the steps of: sintering an inorganic-nonmetallic starting material to obtain a porous inorganic-nonmetallic matrix sintered body; coating a coupling agent on the surface of the porous inorganic-nonmetallic matrix to obtain a surface-modified product; and infiltrating an organic material into the surface-modified porous inorganic-nonmetallic matrix. And a method for producing a composite material including a step of solidifying the organic material, which is for obtaining an isotropic composite material, the isotropic composite material comprising a porous inorganic-nonmetallic matrix having a flexural strength of at least 40 MPa measured according to ISO 6 872 and an organic material at least partially filling the pores of the porous inorganic-nonmetallic matrix, and the isotropic composite material is disclosed to have an elastic modulus of at least 25 GPa measured according to ISO 10 477 and a bending strength of at least 100 MPa measured according to ISO 6 872.
[0013] Japanese Patent Registration No. 4636514 discloses a dental material and a manufacturing method thereof that can maintain mechanical strength such as wear resistance and flexural strength, discoloration resistance, staining resistance, and aesthetics over a long period of time, and is excellent in modulus of bending elasticity and impact strength, and is also suitable for processing using an inexpensive CAD / CAM system, which is a manufacturing method of a dental material formed by impregnating a porous ceramic with a resin, comprising: (a) molding a mixture containing a ceramic powder containing a network-forming oxide, an intermediate oxide, and a network-modifying oxide and having an average particle size of 3.0 to 50 μm, and a binder, into a predetermined shape; (b) firing the molded mixture, and obtaining a porous ceramic block having interconnecting holes; (c) a coupling agent selected from a silane coupling agent, a titanate coupling agent, and a zircoaluminato coupling agent is permeated into the communicating hole of the porous ceramic block under ultrasonic waves and / or reduced pressure, thereby performing a coupling treatment on the surface of the communicating hole; and (d) a monomer and / or oligomer containing at least an ethylenic double bond is permeated into the communicating hole of the coupled-treated porous ceramic block under ultrasonic waves and / or reduced pressure, and then polymerized. As a specific example, the ceramic powder herein is an aluminosilicate ceramic powder in which the network-forming oxides are SiO2 and B2O3, the intermediate oxide is Al2O3, and the network-modifying oxide is Na2O, and by impregnating resin into the communicating pores of such porous ceramics, the filling ratio of the inorganic material can be increased, so that mechanical strength such as wear resistance and flexural strength, discoloration resistance, staining resistance, and aesthetics can be maintained over a long period of time, and also, since the stress within the ceramic is relaxed, a dental material excellent in flexural modulus, impact strength, etc. can be provided, and this is described as being suitable for a CAD / CAM system.
[0014] Meanwhile, natural teeth are divided into transparent and light-colored enamel, opaque and dark-colored dentin, and opaque and yellowish pulp. As for structural characteristics, the crown of a natural tooth is most transparent at the incisal part, and the color saturation and opacity gradually increase as it goes toward the cervical part.
[0015] Reflecting this point, a method of manufacturing artificial teeth that can imitate the deep color of natural teeth using the so-called build-up method has recently become known.
[0016] The build-up method is a method that forms artificial teeth by layering powders such as porcelain or zirconia and applying color, and then heat-treating them to create a color similar to natural teeth layer by layer. Although it can imitate the color of natural teeth quite closely, this method has low reproducibility as the aesthetics of the artificial teeth are determined entirely by the skilled skills of the dental technician, and it is not advantageous to the patient because it cannot be manufactured in an immediate manner, and it is difficult to implement with cutting processing methods such as CAD / CAM.
[0017] Meanwhile, when manufacturing artificial teeth using cutting processing methods such as CAD / CAM using existing bulk blocks, the resulting artificial teeth inevitably have a single color tone, unlike natural teeth, because the bulk blocks themselves are composed of materials exhibiting uniform physical properties. In particular, artificial teeth produced using this method inevitably have the problem of providing an aesthetically incongruous feel when applied to areas such as the front teeth, resulting in a lack of naturalness.
[0018] Although the method for manufacturing crystallized glass described in Korean Patent No. 10-1975548 by the applicant of the present invention allows for the control of transparency and processability through a secondary heat treatment process, the obtained crystallized glass is a single block with the same physical properties, and thus, in order to realize a deep color like natural teeth, it is necessary to apply a method of combining multiple results. In other words, it was not easy to immediately realize natural-colored teeth by directly applying cutting processing such as CAD / CAM using the bulk block itself.
[0019] Meanwhile, the present applicant has applied for and received registration for a bulk block that is useful for manufacturing artificial tooth prostheses similar to natural teeth, thereby shortening the time and process for manufacturing artificial tooth prostheses, and can also increase structural stability in terms of force distribution through gradient functionalization of mechanical properties (Korean Patent Registration No. 10-2246195). However, the bulk block herein is a glass-ceramic body and not a composite bulk block, and it was not easy to apply the manufacturing process of the glass-ceramic body bulk block to a natural tooth-simulating method of a composite bulk block containing a polymer.
[0020]
[0021] The present invention seeks to provide a composite bulk block for manufacturing a dental prosthesis that can be quickly and easily processed into an aesthetic and functional restoration that mimics a natural tooth.
[0022] The present invention also seeks to provide a method for reproducibly manufacturing a composite bulk block that can be quickly and easily processed into an aesthetic and functional restoration that mimics a natural tooth.
[0023] The present invention comprises a glass ceramic matrix and a polymer,
[0024] The glass ceramic matrix is composed of an amorphous glass matrix and a crystalline phase dispersed in the glass matrix, and the crystalline phase includes at least one selected from a leucite crystalline phase and a lithium disilicate crystalline phase as the main crystalline phase.
[0025] The polymer is included in an amount of 20 to 40 wt% based on the weight of the entire bulk block,
[0026] A composite bulk block for manufacturing a dental prosthesis is provided, which has a gradient of light transmittance according to the depth direction and an interface exists at a point of change in the gradient of light transmittance.
[0027] According to a preferred embodiment of the present invention, a composite bulk block for manufacturing a dental prosthesis may have a multilayer structure in which a plurality of layers having different average particle sizes of a glass ceramic matrix are laminated.
[0028] According to a preferred embodiment of the present invention, a composite bulk block for manufacturing a dental prosthesis may have a multilayer structure in which a plurality of layers having different contents of a coloring agent included in a glass ceramic matrix are laminated.
[0029] According to a preferred embodiment of the present invention, a composite bulk block for manufacturing a dental prosthesis may have a multilayer structure in which the average particle size of the glass ceramic matrix increases in one direction and the colorant content of the glass ceramic matrix decreases in response to that direction.
[0030] According to a preferred embodiment of the present invention, the composite bulk block for manufacturing a dental prosthesis may have a gradient of biaxial flexural strength, and more preferably, the gradient of biaxial flexural strength may be within a range of 180 to 260 MPa.
[0031] According to another embodiment of the present invention, when the composite bulk block for manufacturing a dental prosthesis is separated into specimens based on the change point of the light transmittance gradient value and the interlayer color difference is compared, △E * The value can be up to 4.
[0032] According to a preferred embodiment, the composite bulk block for manufacturing a dental prosthesis of the present invention may have a gradient of light transmittance within a range of 30 to 40% at a wavelength of 550 nm.
[0033] In a composite bulk block for manufacturing a dental prosthesis according to a preferred embodiment of the present invention, the polymer may be bonded to a glass ceramic matrix by a silane bond, and preferably, the polymer may be a cured product of a curable organic material selected from among (meth)acrylate monomers and oligomers containing an unsaturated double bond, and as a specific example, the curable organic material is selected from among hydroxy ethyl methacrylate (HEMA), 2,2-bis [4-(2-hydroxy-3-methacryloyloxy propoxy) phenyl] propane (Bis-GMA), triethylene glycol dimethacrylate (TEGDMA), diurethane dimethacrylate (UDMA), and urethane dimethacrylate (UDMA). The polymer may be at least one selected from the group consisting of propylene glycol dimethacrylate (PD-DMA), biphenyl dimethacrylate (BPDM), n-tolyglycine-glycidylmethacrylate (NTGE), polyethylene glycol dimethacrylate (PEG-DMA), and oligocarbonate dimethacrylic esters.
[0034] In a composite bulk block for manufacturing a dental prosthesis according to a preferred embodiment, the glass matrix may include 69.0 to 75.0 wt% of SiO2, 12.0 to 14.0 wt% of Li2O, 2.5 to 3.5 wt% of Al2O3, 0.12 to 0.22 wt% of ZnO, 1.1 to 2.7 wt% of K2O, 0.1 to 0.3 wt% of Na2O, 2.0 to 6.0 wt% of P2O5, and a coloring agent.
[0035] In a composite bulk block for manufacturing a dental prosthesis according to a specific embodiment, a glass ceramic matrix is a step of melting a glass composition including SiO2 69.0 to 75.0 wt%, Li2O 12.0 to 14.0 wt%, Al2O3 2.5 to 3.5 wt%, ZnO 0.12 to 0.22 wt%, K2O 1.1 to 2.7 wt%, Na2O 0.1 to 0.3 wt%, P2O 5 2.0 to 6.0 wt% and a coloring agent, water quenching the glass melt to obtain a glass molded body of an assembly size, and first crushing the same to prepare a glass powder having a maximum average particle size of 300 ㎛ or less; and a step of crystallizing the glass powder at a furnace temperature starting from room temperature to a maximum temperature of 755 to 810°C for 30 minutes to 6 hours. A method for producing a glass ceramic powder having a maximum average particle size of 100 ㎛ or less by crushing a crystallized heat-treated powder; and a method for forming the glass ceramic powder into a predetermined shape, wherein the glass ceramic powder may be formed into a multilayer structure by laminating different glass ceramic powders in which at least one factor selected from the average particle size of the glass ceramic powder and the content of a coloring agent in the glass ceramic powder is combined.
[0036] Another embodiment of the present invention comprises the steps of: melting a glass composition comprising SiO2 69.0 to 75.0 wt%, Li2O 12.0 to 14.0 wt%, Al2O3 2.5 to 3.5 wt%, ZnO 0.12 to 0.22 wt%, K2O 1.1 to 2.7 wt%, Na2O 0.1 to 0.3 wt%, and P2O5 2.0 to 6.0 wt% and a coloring agent, water quenching the glass melt to obtain a glass molded body of a granular size, and first crushing the glass to prepare a glass powder having a maximum average particle diameter of 300 ㎛ or less;
[0037] A step of crystallizing the glass powder by heat-treating the furnace temperature from room temperature to a maximum temperature of 755 to 810°C for 30 minutes to 6 hours;
[0038] A step of producing a glass ceramic powder having an average particle size of 100 ㎛ or less by crushing a crystallized heat-treated powder; and
[0039] It includes a step of forming a glass ceramic matrix by forming a glass ceramic powder into a predetermined shape,
[0040] A method for manufacturing a composite bulk block for manufacturing a dental prosthesis is provided, which comprises forming a multilayer structure by laminating different glass ceramic powders in which at least one factor selected from the average particle size of the glass ceramic powder and the content of a coloring agent in the glass ceramic powder is combined.
[0041] In terms of color reproducibility of the composite bulk block, it is desirable to separate the specimens based on the change point of the light transmittance gradient value for two bulk blocks that have undergone the same process, measure the color indices L, a, and b for each layer, and calculate the interlayer color difference between the two bulk blocks according to the following equation 1, △E * It may be done so that the value is at most 4.
[0042] <Formula 1>
[0043]
[0044] In the above formula, L1, a1, and b1 represent color index values obtained for the first block, and L2, a2, and b2 represent color index values obtained for the second block.
[0045] In another embodiment of the present invention, a prosthesis is provided, which comprises a glass ceramic matrix and a polymer, wherein the glass ceramic matrix is composed of an amorphous glass matrix and a crystal phase dispersed in the glass matrix, wherein the crystal phase includes at least one selected from a leucite crystal phase and a lithium disilicate crystal phase as a main crystal phase, and wherein the polymer is included in an amount of 20 to 40 wt% based on the weight of the entire bulk block, and has a gradient of light transmittance along a depth direction, and an interface exists at a point where the gradient value of light transmittance changes.
[0046] The composite bulk block according to the present invention can provide a composite bulk block for manufacturing a dental prosthesis that can quickly and easily process an aesthetic and functional restoration that mimics a natural tooth.
[0047] The aforementioned and additional aspects of the present invention will become more apparent through preferred embodiments described with reference to the accompanying drawings. Below, these embodiments of the present invention will be described in detail so that those skilled in the art can easily understand and reproduce them.
[0048]
[0049] The present invention comprises a glass ceramic matrix and a polymer,
[0050] A composite bulk block for manufacturing a dental prosthesis is provided, wherein the glass ceramic matrix is composed of an amorphous glass matrix and a crystal phase dispersed in the glass matrix, the crystal phase includes at least one selected from a leucite crystal phase and a lithium disilicate crystal phase as a main crystal phase, and a polymer is included in an amount of 20 to 40 wt% based on the weight of the entire bulk block, and has a gradient of light transmittance along the depth direction, and an interface exists at a point where the gradient of light transmittance value changes.
[0051] In the description above and below, the term “main crystal phase” is defined as a crystal phase that accounts for at least 50 wt% of the entire crystal phase, and the term “additional crystal phase” may be defined as the remaining crystal phase(s) other than the main crystal phase among the entire crystal phase.
[0052] The content of the crystal phase can be calculated through X-ray diffraction analysis, for example, the ratio F of crystal phase a in a specimen with two polymorphs a and b. a is quantitatively expressed by the following mathematical formula 1.
[0053]
[0054] This value can be obtained by measuring the intensity ratio of the two crystal phases and obtaining the integer K. K is the absolute intensity ratio I of the two pure polymorphs. oa / I ob , and is obtained by measuring standard substances.
[0055] In the descriptions above and below, the term "main crystal phase" may be defined as being established based on the content produced by this method.
[0056] In the description above and below, the bulk block has no limitation in shape, and may include various shapes of bulk bodies such as a block shape, a disk shape, an ingot shape, a cylinder shape, etc.
[0057] The composite bulk block according to the present invention includes a glass ceramic as a ceramic in consideration of the difference in refractive index between the monomer material forming the polymer and the ceramic, and in particular, a leucite-based glass ceramic or a lithium disilicate-based glass ceramic may be preferable in terms of aesthetics, and most preferably, a lithium disilicate-based glass ceramic may be preferable.
[0058] Meanwhile, it may be preferable that the polymer present in the composite bulk block be included in an amount of 20 to 40 wt% based on the weight of the entire bulk block. However, if the polymer is included in an amount of less than 20 wt% based on the weight of the entire bulk block, it may be disadvantageous in use due to low processability caused by the brittleness of ceramics, and if it is included in an amount exceeding 40 wt%, problems such as fracture and wear may occur due to excessively low physical properties.
[0059] The composite bulk block according to the present invention has a structure in which a gradient of optical transmittance is present along the depth direction, and an interface exists at a point where the gradient of optical transmittance is changed. Here, 'having a gradient of optical transmittance' means that when a graph of optical transmittance according to depth is drawn, the graph of optical transmittance changes to have a gradient, and the 'point of change in the gradient of optical transmittance' will be understood as a point where the gradient of optical transmittance is changed, and the meaning of 'existence of an interface' will be understood as the existence of an interface interpreted as a layer at a point where the gradient of optical transmittance is changed within the composite bulk block. In other words, it will be understood that the composite bulk block has a multilayer structure.
[0060] Composite bulk blocks satisfying this structure can exhibit appearances and physical properties similar to natural teeth, which are composed of transparent and light-colored enamel, opaque and dark-colored dentin, and opaque and more yellow-colored cementum.
[0061] Such composite bulk blocks for manufacturing dental prostheses may be implemented from a multilayer structure in which a plurality of layers having different average particle sizes of a glass ceramic matrix are laminated, or from a multilayer structure formed by laminating a plurality of layers having different contents of a coloring agent included in a glass ceramic matrix, or from a combination thereof.
[0062] For example, the results of confirming the effect of the average particle size of the glass ceramic matrix on the transmittance in a composite bulk block are as shown in Table 1 below. The particles here are the particle sizes of the glass ceramic powder forming the glass ceramic matrix, and each was manufactured into a composite bulk block through the same heat treatment temperature.
[0063] Sample average particle size (㎛) Transmittance (%) 130 44.8 47 2 15 42.1 24 36 40.7 5 6 44 41.33 2
[0064] From the description in Table 1 above, it was confirmed that the transmittance of the composite bulk block can be controlled depending on the size of the particles constituting the glass ceramic matrix in the composite bulk block. That is, it was confirmed that under the same conditions, the smaller the size of the particles constituting the glass ceramic matrix, the lower the transmittance of the composite bulk block.
[0065] Additionally, it was confirmed that the size of the particles constituting the glass ceramic matrix in the composite bulk block also affects physical properties such as flexural strength and surface hardness.
[0066] Sample average particle size (㎛) Biaxial flexural strength (MPa) Surface hardness (MPa) 130 130 550 215 170 600 36 210 680 44 215 685
[0067] Meanwhile, it was confirmed that the light transmittance of the composite bulk block varied depending on the content of the coloring agent included in the glass ceramic matrix. The specimens herein were manufactured into composite bulk blocks by maintaining the same sintering conditions under the same average particle size and heat treatment conditions constituting the glass ceramic matrix, but varying only the coloring agent content.
[0068] Sample average particle size (μm) Colorant (wt%) Transmittance (%) 140.336736.047240.394032.342340.422029.289441.018526.175
[0069]
[0070] As described in Table 3 above, it was confirmed that the transmittance decreased as the colorant content increased.
[0071] Typically, glass ceramics may contain various coloring agents in the glass composition, which may of course include various metal oxides that can be interpreted as colorants or fluorescent agents.
[0072] From the results shown in Tables 1 to 3 above, it can be seen that a composite bulk block for manufacturing a dental prosthesis can be provided in which the incisal portion, which has excellent aesthetics and relatively low physical properties, is composed of a glass ceramic matrix having a low colorant content and a large average particle size, the cervical portion is composed of a glass ceramic matrix having a high colorant content and a relatively small average particle size, and the middle portion is composed of a glass ceramic matrix by appropriately mixing the particle sizes applied in the incisal and cervical portions, thereby having a gradient of light transmittance along the depth direction and an interface exists at the point of change in the gradient of light transmittance. That is, the composite bulk block for manufacturing a dental prosthesis of the present invention according to a preferred embodiment has a multilayer structure in which the average particle size of the glass ceramic matrix increases in one direction and the colorant content of the glass ceramic matrix decreases corresponding to the direction, which may be preferable for simulating a natural tooth.
[0073] The composite bulk block according to one embodiment of the present invention has a gradient of biaxial flexural strength, and the gradient may be within a range of 180 to 260 MPa.
[0074] According to a preferred embodiment of the present invention, a composite bulk block for manufacturing a dental prosthesis may have a gradient of light transmittance within a range of 30 to 40% at a wavelength of 550 nm. In a specific example of an experiment, it was confirmed that the light transmittance varied in the depth direction as shown in Table 4 below.
[0075] Layer-by-layer optical transmittance of the composite bulk block of the present invention (%, at a wavelength of 550 nm) 1st layer 37.41 2nd layer 32.91 3rd layer 32.05
[0076] Normally, the enamel layer of a natural tooth exhibits a light transmittance of 35% or more, and the dentine layer exhibits a light transmittance of about 25%. Therefore, it was confirmed that the composite bulk block according to the present invention sufficiently mimics a natural tooth in terms of aesthetics.
[0077] Meanwhile, in the dental bulk block of the present invention, the polymer may be bonded to the glass ceramic matrix through a silane bond.
[0078] Such silane bonding is possible through surface treatment of the glass ceramic matrix, specifically, by treating the surface of the glass ceramic with an organic functional silane compound having an ethylenically unsaturated double bond and bonding a polymer thereto.
[0079] More specifically, the organofunctional silane may be at least one selected from the group consisting of, but not limited to, methacryloxyalkylene trialkoxysilane, 3-methacryloxypropyl trimethoxysilane, and 3-methacryloxypropyl triethoxysilane.
[0080] Examples of such processing methods include the method described in Korean Patent No. 10-1609291, the method described in Korean Patent No. 10-1682542, the method described in Korean Patent No. 10-2122202, or the method described in Korean Patent No. 10-2228118.
[0081] The polymer included in the composite bulk block according to the present invention may be a cured product of a curable organic material selected from among (meth)acrylate monomers and oligomers containing an unsaturated double bond. As a specific example, the curable organic material may be hydroxy ethyl methacrylate (HEMA), 2,2-bis [4-(2-hydroxy-3-methacryloyloxy propoxy) phenyl] propane (Bis-GMA), triethylene glycol dimethacrylate (TEGDMA), diurethane dimethacrylate (UDMA), urethane dimethacrylate (UDM), biphenyl dimethacrylate (BDM), It may be at least one selected from the group consisting of BPDM), n-tolyglycine-glycidylmethacrylate (NTGE), polyethylene glycol dimethacrylate (PEG-DMA), and oligocarbonate dimethacrylic esters.
[0082] Among these monomers and / or oligomers, for example, UDMA or Bis-GMA have high viscosity, so they can be mixed with TEGDMA, which has low viscosity, in a mass ratio of 5:5 to 6:4, but this is not limited thereto.
[0083] In the case of curable organic materials, shrinkage hardening occurs during polymerization, but the effect of minimizing changes in physical properties through shrinkage hardening can also be obtained through the organic functional silane described above.
[0084] It goes without saying that surface treatment of crystallized glass using such organic functional silanes can be performed using a solution of the organic functional silane diluted in ethanol, taking into account the specificity of dental composites.
[0085] In this way, by treating the surface of a glass ceramic with an organic functional silane and combining it with a polymer to manufacture a composite bulk block, the volume % of inorganic matter in the composite as a whole is increased, thereby improving biaxial flexural strength and hardness.
[0086] Meanwhile, an initiator may be included to cure the curable organic material by cross-linking it into a polymer form. Types of initiators include photoinitiators and thermal initiators. In the present invention, a preferred initiator is a thermal initiator, and a composite having superior physical properties can be obtained when thermally polymerized by including a thermal initiator compared to when photopolymerization is performed by including a photoinitiator.
[0087] The thermal initiator may be a variety of compounds known in the art, including, but not limited to, known peroxides such as dibenzoyl peroxide, dilauroyl peroxide, tert-butyl peroctoate, or tert-butyl perbenzoate.
[0088] In obtaining the dental composite bulk block according to the present invention as described above, it is preferable that the glass matrix include SiO2 69.0 to 75.0 wt%, Li2O 12.0 to 14.0 wt%, Al2O3 2.5 to 3.5 wt%, ZnO 0.12 to 0.22 wt%, K2O 1.1 to 2.7 wt%, Na2O 0.1 to 0.3 wt%, P2O5 2.0 to 6.0 wt% and a coloring agent.
[0089] This glass composition undergoes crystal nucleation and crystal growth heat treatment to precipitate a crystal phase within an amorphous glass matrix for crystallization. The temperature at which crystal nuclei and crystal growth occur in the above-mentioned glass matrix corresponds to 500°C to 880°C. That is, crystal nuclei begin to form from a minimum of 500°C and crystal growth occurs with increasing temperature, and this crystal growth exhibits the lowest light transmittance for use as an artificial tooth at a maximum of 880°C. That is, the light transmittance gradually decreases from the temperature at which crystals grow to a maximum of 880°C. When focusing on this crystal growth, crystal growth is performed to a degree that satisfies high strength while also satisfying machinability, and this can be useful as a glass ceramic matrix of a composite bulk block according to the present invention.
[0090] From this point of view, the glass ceramic constituting the dental composite block according to the present invention comprises the steps of: melting a glass composition including SiO2 69.0 to 75.0 wt%, Li2O 12.0 to 14.0 wt%, Al2O3 2.5 to 3.5 wt%, ZnO 0.12 to 0.22 wt%, K2O 1.1 to 2.7 wt%, Na2O 0.1 to 0.3 wt%, and P2O5 2.0 to 6.0 wt%, water quenching the glass melt to obtain a glass molded body of a granular size, and first crushing the same to prepare glass powder having a maximum average particle size of 300 ㎛ or less; performing a crystallization heat treatment on the glass powder at a furnace temperature starting from room temperature to a maximum temperature of 755 to 810°C for 30 minutes to 6 hours; It is preferable that the obtained product be a step of producing a glass ceramic powder having a maximum average particle size of 100 ㎛ or less by crushing a crystallized heat-treated powder; and a step of forming the glass ceramic powder into a predetermined shape.
[0091] A specific example for obtaining a glass ceramic constituting the composite blank of the present invention is as follows: First, a glass composition including 69.0 to 75.0 wt% of SiO2, 12.0 to 14.0 wt% of Li2O, 2.5 to 3.5 wt% of Al2O3, 0.12 to 0.22 wt% of ZnO, 1.1 to 2.7 wt% of K2O, 0.1 to 0.3 wt% of Na2O, and 2.0 to 6.0 wt% of P2O5 is weighed and mixed.
[0092] Instead of Li2O, Li2CO3 can be added as a glass composition, and carbon dioxide (CO2), which is the carbon (C) component of Li2CO3, is emitted as a gas during the melting process of the glass and escapes. In addition, instead of K2O and Na2O in the alkali oxide, K2CO3 and Na2CO3 can be added, respectively, and carbon dioxide (CO2), which is the carbon (C) component of K2CO3 and Na2CO3, is emitted as a gas during the melting process of the glass and escapes.
[0093] Mixing is done using a dry mixing process, and a ball milling process can be used as a dry mixing process. Specifically, the ball milling process involves loading the starting raw materials into a ball mill, and rotating the ball mill at a constant speed to mechanically pulverize and uniformly mix the starting raw materials. The balls used in the ball milling machine can be made of ceramic materials such as zirconia or alumina, and the balls can be all the same size or have at least two different sizes. The ball size, milling time, and the rotation speed of the ball milling machine are adjusted in consideration of the target particle size. For example, the ball size can be set to a range of about 1 mm to 30 mm in consideration of the particle size, and the rotation speed of the ball milling machine can be set to a range of about 50 to 500 rpm. It is preferable to perform ball milling for 1 to 48 hours in consideration of the target particle size, etc. By ball milling, the starting materials are ground into fine particles, which have a uniform particle size and are uniformly mixed at the same time.
[0094] The mixed starting materials are placed in a melting furnace, and the melting furnace containing the starting materials is heated to melt the starting materials. Here, melting means that the starting materials change into a viscous liquid state rather than a solid state. It is preferable that the melting furnace be made of a material with a high melting point, high strength, and a low contact angle to suppress the phenomenon of the melt material sticking together. For this purpose, it is preferable that the melting furnace be made of a material such as platinum (Pt), diamond-like carbon (DLC), or chamotte, or a material whose surface is coated with a material such as platinum (Pt) or diamond-like carbon (DLC).
[0095] Melting is preferably performed at 1,400 to 2,000°C under normal pressure for 1 to 12 hours. If the melting temperature is lower than 1,400°C, the starting material may not fully melt, and if the melting temperature exceeds 2,000°C, excessive energy consumption is required, which is not economical. Therefore, it is preferable to melt at a temperature within the above-mentioned range. In addition, if the melting time is too short, the starting material may not sufficiently melt, and if the melting time is too long, excessive energy consumption is required, which is not economical. The heating rate of the melting furnace is preferably 5 to 50°C / min. If the heating rate of the melting furnace is too slow, it takes a long time, which reduces productivity, and if the heating rate of the melting furnace is too fast, the rapid temperature increase may cause a large amount of volatilization of the starting material, which may deteriorate the physical properties of the crystallized glass. Therefore, it is preferable to increase the temperature of the melting furnace at a heating rate within the above-mentioned range. Melting is preferably performed in an oxidizing atmosphere such as oxygen (O2) or air.
[0096] To crush the glass melt into a desired shape and size, the glass melt is water quenched to obtain a glass molded body of an assembly size, and this is first crushed to prepare glass powder having a maximum average particle size of 300 ㎛ or less.
[0097] The glass powder obtained in this manner is transferred to a crystallization heat treatment furnace to manufacture the desired crystallization heat treatment powder.
[0098] At this time, the crystallization heat treatment is performed by starting the temperature inside the furnace from room temperature and increasing it to a maximum temperature of 755 to 810°C for 30 minutes to 6 hours, thereby obtaining a crystallization heat treatment powder having only pure lithium disilicate as a crystal phase and including a crystal phase having a crystal size of 0.01 to 1.0 μm.
[0099] Next, the crystallized heat-treated powder is pulverized to produce a glass ceramic powder having a maximum average particle size of 100 ㎛ or less.
[0100] Finally, a glass ceramic matrix can be obtained by shaping the glass ceramic powder into a predetermined shape.
[0101] By forming a multilayer structure by laminating different glass ceramic powders having at least one selected factor among the average particle size of the glass ceramic powder and the content of the colorant in the glass ceramic powder, a glass ceramic matrix multilayer structure molded product that aesthetically and physically resembles a natural tooth and exhibits different transmittance and mechanical properties can be manufactured.
[0102] By using the molded product obtained in this way as a glass ceramic matrix, a method described in Korean Patent No. 10-1609291, a method described in Korean Patent No. 10-1682542, a method described in Korean Patent No. 10-2122202, a method described in Korean Patent No. 10-2228118, etc., a dental bulk block comprising a glass ceramic matrix and a polymer according to the present invention can be manufactured, wherein the glass ceramic matrix is composed of an amorphous glass matrix and a crystal phase dispersed in the glass matrix, the crystal phase includes at least one selected from a leucite crystal phase and a lithium disilicate crystal phase as a main crystal phase, and the polymer is included in an amount of 20 to 40 wt% based on the weight of the entire bulk block, has a gradient of light transmittance in the depth direction, and an interface exists at a point of change in the gradient value of light transmittance.
[0103]
[0104] As a fair indicator, for two bulk blocks that performed the same process, the specimens were separated based on the change point of the light transmittance gradient value, and the color indices L, a, and b values were measured layer by layer, and the interlayer color difference between the two bulk blocks was calculated according to the following equation 1, and △E* It may be desirable to perform this so that the value is at most 4.
[0105] <Formula 1>
[0106]
[0107] In the above formula, L1, a1, and b1 represent color index values obtained for the first block, and L2, a2, and b2 represent color index values obtained for the second block.
[0108] Generally △E * A value of 0 means there is no color difference, and if the two specimens are from the same lot, it means that the color reproducibility is very good, a value of 0 to 2 means that there is a very slight difference in color, and a value of 2 to 4 means that the color difference is noticeable.△E * If the value is 4 to 6, the color difference is easily (appreciable) distinguished, and if two products are from the same lot, it corresponds to the clinically usable limit (poor aesthetics), and if the product has a value of 6 or more, it may mean that the color difference is too great to be used clinically. The manufacturing method of the composite bulk block according to the present invention is △E * It was confirmed that a process with excellent color reproducibility can be realized with a value of up to 4.
[0109] In the above description, “two bulk blocks that have undergone the same process” should be understood as being based on the process identity as well as the raw material identity between the two bulk blocks.
[0110]
[0111] The obtained composite bulk block can be machined into a desired shape and manufactured into a prosthesis by processing using CAD-CAM, etc. as described above.
[0112] A machined prosthesis comprises a glass ceramic matrix and a polymer, wherein the glass ceramic matrix is composed of an amorphous glass matrix and a crystal phase dispersed in the glass matrix, wherein the crystal phase comprises at least one selected from a leucite crystal phase and a lithium disilicate crystal phase as a main crystal phase, and the polymer is included in an amount of 20 to 40 wt% based on the weight of the entire bulk block, and has a gradient of light transmittance along a depth direction, and an interface exists at a point where the gradient of light transmittance value changes, thereby providing a prosthesis simulating a natural tooth.
[0113]
[0114] Although the present invention has been described with reference to an embodiment, this is merely exemplary, and those skilled in the art will understand that various modifications and equivalent other embodiments are possible therefrom.
[0115]
[0116] The present invention discloses a composite bulk block for manufacturing a dental prosthesis, which is a composite bulk block for manufacturing a dental prosthesis that can be quickly and easily processed into an aesthetic and functional restoration that mimics a natural tooth, and can be useful for manufacturing a dental prosthesis.
Claims
1. Contains a glass ceramic matrix and a polymer, The glass ceramic matrix is composed of an amorphous glass matrix and a crystalline phase dispersed in the glass matrix, and the crystalline phase includes at least one selected from a leucite crystalline phase and a lithium disilicate crystalline phase as the main crystalline phase. The polymer is included in an amount of 20 to 40 wt% based on the weight of the entire bulk block, It has a gradient of light transmittance along the depth direction, and an interface exists at the point of change in the gradient of light transmittance. Composite bulk blocks for the manufacture of dental prosthetics.
2. In the first paragraph, characterized in that the glass ceramic matrix has a multilayer structure in which a plurality of layers having different average particle sizes are laminated. Composite bulk blocks for the manufacture of dental prosthetics.
3. In the first paragraph, it is characterized in that it is a multilayer structure in which a plurality of layers having different contents of coloring agents included in the glass ceramic matrix are laminated. Composite bulk blocks for the manufacture of dental prosthetics.
4. In the first paragraph, it is characterized in that it is a multilayer structure in which the average particle size of the glass ceramic matrix increases in one direction and the content of the colorant of the glass ceramic matrix decreases corresponding to that direction. Composite bulk blocks for the manufacture of dental prosthetics.
5. In the first paragraph, characterized in that it has a gradient of biaxial flexural strength, Composite bulk blocks for the manufacture of dental prosthetics.
6. In the first paragraph, the slope of the biaxial flexural strength is characterized in that it is within the range of 180 to 260 MPa. Composite bulk blocks for the manufacture of dental prosthetics.
7. In the first paragraph, the gradient of the light transmittance is characterized in that it is within the range of 30 to 40% at a wavelength of 550 nm. Composite bulk blocks for the manufacture of dental prosthetics.
8. In the first paragraph, the polymer is characterized in that it is bonded to the glass ceramic matrix by a silane bond. Composite bulk blocks for the manufacture of dental prosthetics.
9. In the first paragraph, the polymer is characterized in that it is a cured product of a curable organic material selected from among (meth)acrylate monomers and oligomers containing unsaturated double bonds. Composite bulk blocks for the manufacture of dental prosthetics.
10. In the 9th paragraph, the curable organic material is hydroxy ethyl methacrylate (HEMA), 2,2-bis [4-(2-hydroxy-3-methacryloyloxy propoxy) phenyl] propane (Bis-GMA), triethylene glycol dimethacrylate (TEGDMA), diurethanedimethacrylate (UDMA), urethane dimethacrylate (UDM), biphenyldimethacrylate (BPDM), n-tolyglycine-glycidylmethacrylate (NTGE), polyethylene glycol characterized by at least one selected from the group consisting of polyethylene glycol dimethacrylate (PEG-DMA) and oligocarbonate dimethacrylic esters. Composite bulk blocks for the manufacture of dental prosthetics.
11. In the first paragraph, the glass matrix is characterized in that it contains 69.0 to 75.0 wt% of SiO2, 12.0 to 14.0 wt% of Li2O, 2.5 to 3.5 wt% of Al2O3, 0.12 to 0.22 wt% of ZnO, 1.1 to 2.7 wt% of K2O, 0.1 to 0.3 wt% of Na2O, 2.0 to 6.0 wt% of P2O5 and a coloring agent. Composite bulk blocks for the manufacture of dental prosthetics.
12. In the first paragraph, the glass ceramic matrix comprises a step of melting a glass composition including SiO2 69.0 to 75.0 wt%, Li2O 12.0 to 14.0 wt%, Al2O3 2.5 to 3.5 wt%, ZnO 0.12 to 0.22 wt%, K2O 1.1 to 2.7 wt%, Na2O 0.1 to 0.3 wt%, P2O5 2.0 to 6.0 wt% and a coloring agent, water quenching the glass melt to obtain a glass molded body of a granulated size, and first crushing the glass powder to prepare a glass powder having a maximum average particle size of 300 ㎛ or less; and a step of crystallization heat-treating the glass powder at a furnace temperature starting from room temperature to a maximum temperature of 755 to 810°C for 30 minutes to 6 hours. A method for producing a glass ceramic powder having a maximum average particle size of 100 ㎛ or less by crushing a crystallized heat-treated powder; and a method for forming the glass ceramic powder into a predetermined shape, characterized in that the glass ceramic powder is formed into a multilayer structure by laminating different glass ceramic powders in which at least one factor selected from the average particle size of the glass ceramic powder and the content of a coloring agent in the glass ceramic powder is combined. Composite bulk blocks for the manufacture of dental prosthetics.
13. A step of melting a glass composition containing 69.0 to 75.0 wt% of SiO2, 12.0 to 14.0 wt% of Li2O, 2.5 to 3.5 wt% of Al2O3, 0.12 to 0.22 wt% of ZnO, 1.1 to 2.7 wt% of K2O, 0.1 to 0.3 wt% of Na2O, and 2.0 to 6.0 wt% of P2O5 and a coloring agent, water quenching the glass melt to obtain a glass molded body of a granular size, and first crushing the glass to prepare a glass powder having a maximum average particle size of 300 ㎛ or less; A step of crystallizing the glass powder by heat-treating the furnace temperature from room temperature to a maximum temperature of 755 to 810°C for 30 minutes to 6 hours; A step of producing a glass ceramic powder having an average particle size of 100 ㎛ or less by crushing a crystallized heat-treated powder; and It includes a step of forming a glass ceramic matrix by forming a glass ceramic powder into a predetermined shape, A multilayer structure is formed by laminating different glass ceramic powders in which at least one selected factor among the average particle size of the glass ceramic powder and the content of the colorant in the glass ceramic powder is combined. Method for manufacturing composite bulk blocks for manufacturing dental prostheses.
14. In paragraph 13, for two bulk blocks that performed the same process, the specimens were separated based on the change point of the light transmittance gradient value, and the color indices L, a, and b values were measured layer by layer, and the interlayer color difference between the two bulk blocks was calculated according to the following equation 1, when △E * characterized in that it is performed so that the value is at most 4, Method for manufacturing composite bulk blocks for manufacturing dental prostheses. <Formula 1> In the above formula, L1, a1, and b1 represent color index values obtained for the first block, and L2, a2, and b2 represent color index values obtained for the second block.
15. In the 13th paragraph, characterized in that it is performed by a method of forming a multilayer structure by stacking a plurality of layers having different average particle sizes of a glass ceramic matrix. Method for manufacturing composite bulk blocks for manufacturing dental prostheses.
16. In the 13th paragraph, characterized in that it is performed by a method of forming a multilayer structure by laminating a plurality of layers having different contents of coloring agents included in a glass ceramic matrix. Method for manufacturing composite bulk blocks for manufacturing dental prostheses.
17. In the 13th paragraph, it is characterized in that it is performed by a method of forming a multilayer structure in which the average particle size of the glass ceramic matrix increases in one direction and the content of the colorant of the glass ceramic matrix decreases corresponding to the direction. Method for manufacturing composite bulk blocks for manufacturing dental prostheses.
18. Processed from the composite bulk block of Article 1, Containing a glass ceramic matrix and a polymer, The glass ceramic matrix is composed of an amorphous glass matrix and a crystalline phase dispersed in the glass matrix, and the crystalline phase includes at least one selected from a leucite crystalline phase and a lithium disilicate crystalline phase as the main crystalline phase. The polymer is included in an amount of 20 to 40 wt% based on the weight of the entire bulk block, It has a gradient of light transmittance along the depth direction, and an interface exists at the point of change in the gradient of light transmittance. Prosthesis.
Citation Information
Patent Citations
Manufacturing methods for dental materials
JP4636514B2
Polymer infiltrated glass or glass-ceramic composites for dental blanks and preparation method thereof
KR101609291B1
Method for manufacturing dental block
KR101682542B1
Method for preparing glass-ceramics, capable of adjusting machinability or translucency through change in temperature of heat treatment
KR101975548B1
Method for manufacturing composite using chemical bonding between inorganic and organic materials using silane coupling agent
KR102122202B1