Capacity recovery method for vanadium redox flow battery
By using liquid reducing agent for self-circulation reduction in all vanadium liquid flow batteries, the capacity attenuation problem caused by the increase in the price state of the electrolyte is solved, and capacity recovery and stack performance protection is achieved, which simplifies operation and reduces risks.
Patent Information
- Application Number
- PCT/CN2024/096212
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-06
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-12
AI Technical Summary
During the long-term charging and discharging process of all vanadium liquid flow batteries, due to the influence of hydrogen evolution reaction or oxygen, the comprehensive valence state of the electrolyte increases, resulting in damage to the discharge capacity. There are reducing agent selection and long reaction time in existing chemical or electrochemical reduction methods. , high risks and other problems make it difficult to effectively restore battery capacity.
Using liquid reducing agent, by adding pentavalent vanadium-rich electrolyte to the positive electrode reservoir of the battery, reacting with the reducing agent, and using self-cycling to complete chemical reduction, strictly monitor the reaction measurement, ensure that the reaction is only carried out in the electrolyte, and avoiding electricity. Contact with stack materials to reduce residual risk.
The injection design is simplified, the capacity recovery time is shortened, the impact on stack performance is reduced, the reduction agent is fully reacted, the stack performance damage is avoided, and the battery capacity and efficiency is significantly improved.
Smart Images

Figure CN2024096212_12122024_PF_FP_ABST
Abstract
Description
A method for recovering capacity of all-vanadium redox flow battery Technical Field
[0001] This article relates to electrochemical energy storage technology, and in particular to a battery capacity recovery method for an all-vanadium redox flow battery based on chemical reduction. Background Art
[0002] All-vanadium redox flow batteries (AVFBs) are a medium- to long-term energy storage technology that is reaching commercial maturity. They fall within the category of electrochemical energy storage. Compared to other electrochemical energy storage technologies, they are inherently safe, capable of deep charge and discharge cycles, and pose no risk of fire or explosion. While the initial cost of the electrolyte, the most expensive component of an AVFB system, is significantly affected by vanadium prices, existing electrolyte regeneration technology ensures the long-term recycling of vanadium ions.
[0003] The active electrolyte in an all-vanadium flow battery is vanadium ions dissolved in an aqueous solution of sulfuric acid. The positive electrode of an all-vanadium flow battery contains tetravalent vanadium V(IV) and pentavalent vanadium V(V), while the negative electrode contains divalent vanadium V(II) and trivalent vanadium V(III). During charging, electrical energy is stored as chemical energy in the vanadium ions of varying valences. During discharge, the vanadium ions undergo their corresponding reversible electrochemical reactions, releasing the chemical energy as electrical energy.
[0004] Typically, when not charging, the positive electrode electrolyte contains tetravalent vanadium V(IV), and the negative electrode contains trivalent vanadium V(III), resulting in an average overall electrolyte valence of 3.5. However, during long-term charge and discharge in all-vanadium flow batteries, the overall electrolyte valence tends to increase due to small amounts of hydrogen evolution or the influence of small amounts of oxygen. When the overall valence of a vanadium battery exceeds 3.5, its discharge capacity is affected, and electrolyte utilization is compromised. In principle, this problem can be solved by correcting the electrolyte valence.
[0005] Currently, the methods reported domestically and internationally for restoring battery capacity by reducing the electrolyte valence state mainly include chemical and electrochemical methods. All of these methods are based on the mechanism of reduction. Existing chemical reduction schemes have one or more of the following drawbacks:
[0006] 1. The selection of reducing agents includes certain solid compounds, which poses challenges to the sampling requirements of the battery system pipelines;
[0007] 2. The reaction of the reducing agent occurs after the battery is discharged. At this time, the content of pentavalent vanadium (V) in the positive electrode electrolyte is relatively low. As the main reactant of the reduction reaction, it will result in a longer reduction time.
[0008] 3. The reaction of the reducing agent occurs during the battery charging and discharging reaction, which means that the reducing agent will come into contact with the surface of the vanadium battery stack material, posing a risk of affecting the performance of the stack;
[0009] 4. The residual amount of reducing agent after the reaction is not monitored, which poses a risk of affecting the performance of the fuel cell stack.
[0010] Summary of the Invention
[0011] The present application provides a method for recovering the capacity of an all-vanadium liquid flow battery. By using a liquid reducing agent, the sampling is simplified, and the reducing agent reacts quickly with an electrolyte containing a large amount of pentavalent vanadium (V). At the same time, the degree of reaction of the reducing agent in the reduced valence state and the residual amount are strictly monitored, thereby reducing the risk of affecting the performance of the battery stack due to the residual reducing agent.
[0012] Compared with the related art, the present application relates to a method for recovering the capacity of an all-vanadium redox flow battery, comprising the following steps:
[0013] S100: calibrating the comprehensive valence state of vanadium ions in the battery storage tank after the discharge capacity has decayed, and charging the battery;
[0014] S200: adding a reducing agent to the positive electrode storage tank of the battery;
[0015] S300: The battery positive electrode storage tank performs self-circulation to complete the chemical reduction reaction;
[0016] S400: calibrating the comprehensive valence of vanadium ions in the battery storage tank and determining the residual reducing agent; and / or
[0017] S500: Add reducing agent to the positive electrode storage tank of the battery, and repeat steps S300-S400 until the comprehensive valence average value of vanadium ions in the battery storage tank is restored to 3.5 and no reducing agent residue is present in the electrolyte.
[0018] In an exemplary embodiment, step S100 includes:
[0019] S101: Sampling the electrolytes in the positive and negative electrode storage tanks of the battery respectively, and performing electrochemical titration analysis and cyclic voltammetry analysis to obtain the valence and concentration of vanadium ions in the positive and negative electrode electrolytes, wherein a disk platinum electrode or a glassy carbon electrode is used as a working electrode in the cyclic voltammetry analysis;
[0020] S102: Calculate the comprehensive valence A of the vanadium ions in the current battery liquid storage tank based on the measurement results in step S101. The calculation formula is as follows:
[0021] Among them, a p and a n Represent the valence states of vanadium ions in the positive and negative electrolytes, respectively, c p and c n Represent the concentration of vanadium ions in the positive and negative electrolytes, V p and Vn Represent the volume of the positive and negative electrolytes respectively.
[0022] In an exemplary embodiment, optionally, step S100 further includes:
[0023] S103: Charge the battery to SOC 50%-70%, preferably 65%.
[0024] In an exemplary embodiment, step S200 includes calculating the theoretical amount of the reducing agent based on the comprehensive valence state in step S100 and the reaction formula of pentavalent vanadium ion V(V) and the reducing agent, wherein the reaction formula is as follows: qV(V)+C x H y O z →qV(IV)+xCO2+zH2O,
[0025] That is, when the valence of vanadium ions in the electrolyte is reduced by 1 mol, the theoretical amount of the reducing agent is 1 / qmol.
[0026] In an exemplary embodiment, in step S200, optionally, 70% to 90% of the theoretical amount of reducing agent is added to the positive electrode liquid storage tank of the battery.
[0027] In an exemplary embodiment, in step S200, optionally, the reducing agent is an organic reducing agent, preferably one or more of pyridine, ascorbic acid, oxalic acid, formic acid, and ethylene glycol, more preferably ethylene glycol.
[0028] In an exemplary embodiment, in step S300, optionally, the self-circulation time of the battery positive electrode liquid storage tank is 2-24 hours, preferably, 5 hours.
[0029] In an exemplary embodiment, step S400 includes repeating steps S101 and S102, determining the comprehensive valence state of vanadium ions in the battery storage tank, and determining the residual reducing agent according to cyclic voltammetry, wherein a disk platinum electrode or a glassy carbon electrode is used as a working electrode in the electrochemical cyclic voltammetry analysis.
[0030] In an exemplary embodiment, step S500 includes: according to the measurement result in step S400, adding the reducing agent to the positive electrode storage tank of the battery and repeating steps S300-S400 multiple times until the comprehensive valence average value of vanadium ions in the battery storage tank is restored to 3.5, and no obvious reducing agent residue appears in the electrochemical cyclic voltammetry analysis.
[0031] In an exemplary embodiment, optionally, in step S500 , the amount of reducing agent added each time is 5% of the theoretical amount, and the self-circulation time each time is 2 hours.
[0032] In an exemplary embodiment, the method further includes completely discharging the all-vanadium redox flow battery after capacity recovery.
[0033] Compared with the related art, the method described in this application has the following beneficial effects:
[0034] 1. This application method uses liquid chemical reagents entirely, has low requirements for the sample injection design of the battery system, and is easy to operate.
[0035] 2. In the method of the present application, the reducing agent is added to the positive electrode electrolyte in a certain state of charge, which contains a large amount of pentavalent vanadium V (V). The reaction between the reducing agent and pentavalent vanadium can be completed in a short time to reduce the valence state, thereby reducing the time requirement for capacity recovery.
[0036] 3. In the method of the present application, the reaction between the reducing agent and the electrolyte after addition only occurs in the electrolyte and does not come into contact with the electrode material and membrane material of the battery stack, thus avoiding the risk of affecting the performance of the battery stack material.
[0037] 4. In the method of the present application, the amount of reducing agent added is strictly controlled, and the residual amount of the reducing agent after the reaction is completed is promptly monitored by electrochemical cyclic voltammetry, thereby preventing excessive reducing agent from entering the fuel cell stack and affecting the performance of the fuel cell stack.
[0038] Other features and advantages of the present application will be described in the following description, and in part will become apparent from the description, or will be understood by practicing the present application. Other advantages of the present application can be realized and obtained through the solutions described in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings are used to provide an understanding of the technical solution of the present application and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present application and do not constitute a limitation on the technical solution of the present application.
[0040] FIG1 is a capacity attenuation diagram of the all-vanadium redox flow battery after long-term operation in Example 1 of the present application before the method of the present application is used;
[0041] FIG2 is an electrochemical cyclic voltammetry curve in Example 1 of the present application: Curve 1 is an electrochemical cyclic voltammetry curve of the electrolyte sample before adding the reducing agent ethylene glycol, Curve 2 is an electrochemical cyclic voltammetry curve of the electrolyte sample fifteen minutes after adding the reducing agent ethylene glycol, and Curve 3 is an electrochemical cyclic voltammetry curve of the electrolyte sample five hours after adding the reducing agent ethylene glycol;
[0042] FIG3 is a schematic diagram of the electrochemical cyclic voltammetry method for detecting the residual amount of reducing agent in the present invention;
[0043] FIG4 shows the charge and discharge capacity of the all-vanadium redox flow battery after capacity recovery in Example 1 of the present application;
[0044] FIG5 shows the battery efficiency of the all-vanadium redox flow battery after capacity recovery in Example 1 of the present application;
[0045] FIG6 shows the effects of different reducing agents on the valence state of the electrolyte in Experimental Example 1 of the present application. DETAILED DESCRIPTION
[0046] The embodiments described below are used to understand the technical solutions of the present invention. The scope of patent protection of the present invention is not limited by them. Non-creative variations and improvements based on the present invention all fall within the scope of protection of the present invention.
[0047] Example 1.
[0048] Reducing agent: ethylene glycol (molar mass: 62 g / mol, density: 1.11 g / mL)
[0049] 1) A vanadium redox flow battery system with a discharge capacity of 1kW / 4kWh (containing 240L of 1.7M electrolyte with an initial valence of 3.51) was subjected to 1000 charge-discharge cycles. The discharge capacity showed significant degradation. The battery's initial discharge capacity was approximately 310Ah, but the capacity decayed rapidly over time. As shown in Figure 1, the capacity decay exceeded 50Ah between the 900th and 950th charge-discharge cycles.
[0050] 2) The positive and negative electrolytes were sampled, respectively, and electrochemical titration analysis and cyclic voltammetry analysis were performed to obtain the valence state of vanadium ions in the positive and negative electrodes and the concentration of vanadium ions in the positive and negative electrodes, as shown in Table 1 below; wherein, the electrochemical titration analysis steps were carried out with reference to the test method of electrolyte for all-vanadium redox flow batteries in NB / T 42006-2013, and the cyclic voltammetry analysis steps were carried out with reference to: Li L, Kim S, Wang W, et al. A stable vanadium redox-flow battery with high energy density for large-scale energy storage [J]. Advanced Energy Materials, 2011, 1(3): 394-400.
[0051] Table 1
[0052] Based on the measurement results, the comprehensive valence state A of the vanadium ions in the current battery reservoir is calculated, and the battery is then charged to 55% SOC:
[0053] 3) Based on the comprehensive valence state A of the vanadium ions in the current battery storage tank and the reaction formula between pentavalent vanadium ions V(V) and the reducing agent, calculate the theoretical value of the reducing agent ethylene glycol that needs to be added: 10V(V)+C2H6O2→10V(IV)+2CO2+2H2O,
[0054] According to the measurement results, theoretically, to reduce 408 mol of 0.12 valence electrolyte, 4.9 mol of ethylene glycol, or 274 mL of ethylene glycol, is required.
[0055] 4) Based on this, 220 mL of ethylene glycol was added to the positive electrode storage tank of the battery for the first time, and the positive electrode electrolyte storage tank was turned on for self-circulation. After 15 minutes of self-circulation, 10 mL of the electrolyte in the positive and negative electrode storage tanks of the battery was sampled for electrochemical cyclic voltammetry analysis. The results were compared with the electrolyte sample measured at the initial valence state before adding ethylene glycol in step 2). The results are shown in Figure 2.
[0056] As shown in Figure 2, the voltammogram curve 2 for the sample after a short period of addition of the reducing agent, ethylene glycol, exhibits a larger oxidation current (-0.11 mA) compared to Curve 1 without the addition of the reducing agent, while the corresponding reduction current is smaller. This phenomenon is due to the amount of current at the electrode converted from V(IV) to V(V). This is because, within a short period of time after the addition of the reducing agent, the ethylene glycol in the electrolyte sample has not yet completely reacted. When measuring the oxidation current using a circular glassy carbon electrode, the presence of the reducing agent, ethylene glycol, converts V(V) to V(IV), which then contributes to the current at the electrode surface. This results in an amplified oxidation current compared to Curve 1 without the reducing agent (as shown in Figure 3). After five hours of self-circulation in the positive electrode reservoir, step 2 was repeated. The resulting voltammogram curve (Curve 3) is essentially identical to Curve 1 before the addition of the reducing agent, indicating that the reducing agent, ethylene glycol, has completely reacted. However, because the overall valence state had not yet dropped to 3.5, 14 mL of ethylene glycol was added, and the reservoir was self-circulated for another two hours.
[0057] 5) After repeating step 2) three times, the electrolyte valence was found to have dropped to 3.52, and no ethylene glycol residue remained in the electrolyte. The electrolyte was then circulated to the stack for a single discharge.
[0058] 6) Finally, this 1kW / 4kWh all-vanadium redox flow battery was subjected to 180 charge-discharge cycles. Its charge-discharge capacity is shown in Figure 4. Compared to the capacity before adding the reducing agent (Figure 1), the battery capacity has significantly increased and has essentially recovered to its initial capacity of 310Ah. The battery efficiency after capacity recovery also remained stable, as shown in Figure 5, with a coulombic efficiency of approximately 98% and an energy efficiency of approximately 83%.
[0059] Experimental Example 1. Comparison of the effects of different reducing agents
[0060] Different reducing agents were used to investigate a 1.7M vanadium electrolyte with an initial valence of approximately 4.8, with the goal of reducing the valence of 500 mL of electrolyte by 0.5. The specific steps are as follows:
[0061] Based on the redox reaction formula of the present application, the usage of different reducing agents was calculated and the reducing agents were added; 10 mL of the electrolyte was sampled before and 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 10 h, 14 h, 18 h, 22 h and 26 h after the addition of the reducing agent, and the valence state of the electrolyte was measured and recorded using the electrochemical titration method.
[0062] Inspection items: 1. Whether the reaction mechanism is consistent with the redox reaction formula of this application; 2. Whether the reaction time meets the requirements.
[0063] The changes in the electrolyte valence state after adding different reducing agents are shown in Figure 6.
[0064] Conclusion: When ethylene glycol in Example 1 of the present invention is used as a reducing agent, after the theoretically calculated amount is added to the electrolyte, the valence state of the electrolyte can be reduced to the expected value (4.8 to 4.3), and the reaction time is short (about 5 hours), which can achieve the technical effect of the present application; when other reducing agents, such as glucose, are used, although they themselves have reducing properties, due to the high activation energy required for their reaction, their reaction is weak and basically cannot reduce the valence state; when other reducing agents, such as glycerol, are used, it is found from the results of valence state monitoring that their reaction rate with vanadium ions is slow, and even at the end of the reaction, the valence state cannot be reduced to the expected value. It is speculated that the reaction mechanism of glycerol and vanadium ions may be more complicated, the reaction ratio is difficult to determine, and other side reactants are easily produced.
[0065] The embodiments of the present application are illustrative rather than restrictive, and it is obvious to a person skilled in the art that there may be more embodiments and implementations within the scope of the embodiments described in the present application.
Claims
1. A method for recovering the capacity of an all-vanadium liquid flow battery, characterized in that: The following steps are involved: S100: calibrating the comprehensive valence state of vanadium ions in the battery storage tank after the discharge capacity decays, and charging the battery; S200: adding a reducing agent to the positive electrode storage tank of the battery; S300: The positive electrode storage tank of the battery performs self-circulation to complete the chemical reduction reaction; S400: recalibrating the comprehensive valence state of vanadium ions in the battery storage tank and determining the residual reducing agent; and / or S500: Add reducing agent to the positive electrode storage tank of the battery, and repeat steps S300-S400 until the comprehensive valence average value of vanadium ions in the battery storage tank is restored to 3.5, and there is no reducing agent residue in the electrolyte.
2. The method according to claim 1, characterized in that: Step S100 includes: S101: sampling the positive and negative electrolytes in the battery storage tank, respectively, and performing electrochemical titration analysis and cyclic voltammetry analysis to obtain the valence and concentration of vanadium ions in the positive and negative electrolytes; S102: According to the measurement result in step S101, the comprehensive valence state A of the vanadium ions in the current battery storage tank is calculated, and the calculation formula is as follows: Among them, a p and a n Represent the valence states of vanadium ions in the positive and negative electrolytes, respectively, c p and c n Represent the concentration of vanadium ions in the positive and negative electrolytes, V p and V n Represent the volume of the positive and negative electrolytes respectively.
3. The method according to claim 2, characterized in that: Step S100 also includes: S103: Charge the battery to SOC 50%-70%.
4. According to the method of claim 3, step S100 further comprises: S103: Charge the battery to SOC 65%.
5. The method according to claim 1, characterized in that: Step S200 includes: calculating the theoretical amount of the reducing agent according to the comprehensive valence state in step S100 and the reaction formula of pentavalent vanadium ion V (V) and the reducing agent, and the reaction formula is as follows: qV(V)+C x H y O z →qV(IV)+xCO2+zH2O, The theoretical amount of the reducing agent is 1 / qmol for each 1mol reduction of one valence state of vanadium ions in the electrolyte; Add 70% to 90% of the theoretical amount of reducing agent into the positive electrode storage tank of the battery.
6. The method according to claim 5, characterized in that: The reducing agent is selected from one or more of pyridine, ascorbic acid, oxalic acid, formic acid and ethylene glycol.
7. The method according to claim 6, characterized in that: The reducing agent is ethylene glycol.
8. The method according to claim 1, characterized in that: In step S300, the self-circulation time of the battery positive electrode liquid storage tank is 2-24 hours.
9. The method according to claim 8, characterized in that: In step S300, the self-circulation time of the battery positive electrode liquid storage tank is 5 hours.
10. The method according to claim 2, characterized in that: Step S400 includes: repeating steps S101 and S102, determining the comprehensive valence state of vanadium ions in the battery storage tank, and determining the residual reducing agent according to cyclic voltammetry.
11. The method according to claim 1, characterized in that: Step S500 includes: according to the measurement result in step S400, adding the reducing agent to the positive electrode storage tank of the battery and repeating steps S300-S400 multiple times until the comprehensive valence average value of vanadium ions in the battery storage tank is restored to 3.5, and no obvious reducing agent residue appears in the electrochemical cyclic voltammetry analysis.
Citation Information
Patent Citations
Regeneration method for waste liquor of all-vanadium flow battery
CN102468499A
Method for restoring battery capacity in situ
CN103035963A
Method for controlling valence state equilibrium of electrolyte in energy storage module of all-vanadium liquid flow battery
CN109841875A
All-vanadium redox flow battery on-line capacity recovery method
CN114094148A
Preparation method of 3.5-valent sulfate acid system vanadium electrolyte
CN115882021A
Cited By
Method for repairing valence imbalance of all-vanadium electrolyte
CN120970737A