Emulsifier type cold-mixed and cold-laid asphalt mixture and preparation method therefor

Through the combination of water-reactive resin deemulsifier and modified emulsified asphalt, the problems of low early strength and reduced crack resistance of traditional emulsified dosage-form cold-mixed and cold-paved asphalt mixture are solved, and the early strength of asphalt mixture is accelerated and road The performance improvement simplifies the preparation process and promotes pavement recycling.

WO2025007644A1PCT designated stage expired Publication Date: 2025-01-09SOUTH CHINA UNIV OF TECH +1

Patent Information

Application Number
PCT/CN2024/092151
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-04
Filing Date
2024-05-10
Publication Date
2025-01-09

AI Technical Summary

Technical Problem

The traditional emulsifier dosage form cold-mixed and cold-paved asphalt mixture has low strength in the early stage, which cannot meet the requirements for the maintenance of asphalt pavement at 110°C for 24 hours. The crack resistance after adding cement is reduced, making it difficult to recover the pavement.

Method used

Water-reactive resin-based deemulsifiers are used to form hydrogen bonds with the moisture in the modified emulsified bitumen to accelerate the deemulsification speed and early strength formation, avoid defects in cement addition, and ensure the early strength and road performance of the bitumen mixture.

Benefits of technology

Without cement, the early strength formation speed of the asphalt mixture is improved, road performance is ensured, and the preparation process is simplified, which is convenient for later recycling and avoids the problems of brittleness and cracks on the road surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024092151-FTAPPB-I100001
    Figure PCTCN2024092151-FTAPPB-I100001
Patent Text Reader

Abstract

Disclosed in the present invention are an emulsifier type cold-mixed and cold-laid asphalt mixture and a preparation method therefor. The emulsifier type cold-mixed and cold-laid asphalt mixture comprises the following components in parts by mass: 400-600 parts of coarse aggregate, 400-600 parts of fine aggregate, 90-160 parts of modified emulsified asphalt, 10-30 parts of a mineral filler, and 2-8 parts of a water reaction type resin demulsifier, wherein the molecular weight of the water reaction type resin demulsifier is 1 million-10 million. According to the emulsifier type cold-mixed and cold-laid asphalt mixture provided by the present scheme, without using cement, the forming speed of the early strength of the asphalt mixture is increased while ensuring the pavement performance of the asphalt mixture, and the technical problem in the prior art of the reclamation difficulty in a pavement laid by an asphalt mixture in which cement is added is solved, thereby overcoming defects in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Emulsifier-type cold-mix cold-paving asphalt mixture and preparation method thereof

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application with application number 202310812371.9 filed with the Patent Office of China on July 4, 2023, entitled "A kind of emulsifier-type cold-mix cold-laid asphalt mixture and its preparation method", the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present invention relates to the technical field of road engineering, and in particular to an emulsifier-type cold-mix cold-paving asphalt mixture and a preparation method thereof. Background Art

[0004] Cold-mix, cold-laid asphalt pavement technology is the most energy-efficient and environmentally friendly technology compared to hot-mix, hot-laid asphalt pavement technology. Due to the inherent properties of cold-mix asphalt raw materials, it can be produced and applied at room temperature. Compared to traditional hot-mix, hot-laid asphalt mixtures, this technology reduces energy consumption during the heating of aggregates and asphalt, thereby achieving low energy consumption, low emissions, and minimal pollution in road construction. These advantages are well-received by the public and road workers.

[0005] Currently, there are two main types of cold-mix, cold-paved asphalt mixtures used in road construction and maintenance. Solvent-based cold-mix, cold-paved asphalt mixtures utilize various solvents to dilute viscous asphalt, making it fluid and enabling mixing, paving, and compaction at room temperature. Emulsifier-based cold-mix, cold-paved asphalt mixtures utilize emulsified asphalt as a binder, enabling construction at room temperature.

[0006] Because the solvents used in solvent-based cold-mix asphalt mixtures are volatile and highly polluting, they are currently primarily used for emergency pothole repairs and are rarely used on a large scale in road construction. Traditional emulsified cold-mix, cold-laid asphalt mixtures, using emulsified asphalt as a binder, offer advantages such as ease of construction, low energy consumption, minimal pollution, and minimal construction requirements. However, due to the difficulty in timely drainage of residual water after emulsified asphalt demulsification, asphalt pavements paved with them have a water loss rate of only 87% to 93% after 24 hours of curing at 110°C. Excessive free water results in poor adhesion between the emulsified asphalt and aggregate, resulting in low early strength of the cold-mix, cold-laid asphalt mixture, which cannot meet the required water loss rate of at least 98% after 24 hours of curing at 110°C. Therefore, traditional emulsified cold-mix, cold-laid asphalt mixtures are limited to localized and surface repairs. In addition, in traditional emulsifier-type cold-mixed and cold-laid asphalt mixtures, the emulsified asphalt demulsifies slowly, resulting in a slow rate of early strength formation in the cold-mixed and cold-laid asphalt mixtures, and a longer time for the asphalt pavement to be opened.

[0007] In the prior art, in order to break through the limitations of the use of traditional emulsified cold-mixed cold-laid asphalt mixtures and shorten the time it takes for asphalt pavements to be opened, cement is usually added to the emulsified cold-mixed cold-laid asphalt mixture as a curing agent to consume the moisture in the emulsified asphalt, thereby increasing the early strength of the asphalt mixture and enabling it to meet the opening requirements of the asphalt pavement; at the same time, the addition of cement can also increase the rate of water consumption in the emulsified asphalt, thereby increasing the rate of early strength formation and enabling the asphalt pavement to be opened as soon as possible. However, after adding cement, the emulsified cold-mixed cold-laid asphalt mixture will become brittle during long-term use, and its crack resistance will decrease, resulting in cracks in the asphalt pavement, which will reduce its road performance and make it unable to meet the use requirements of existing asphalt pavements. In addition, adding cement to the asphalt mixture will also make the later recycling of the asphalt pavement more difficult, which is not conducive to the recycling of the asphalt mixture.

[0008] Summary of the Invention

[0009] One of the purposes of the present invention is to propose an emulsifier-type cold-mix cold-paved asphalt mixture, which accelerates the early strength formation of the asphalt mixture without using cement and ensuring its road performance, and solves the technical problem of the difficulty in recycling the road surface paved with asphalt mixture added with cement in the prior art, so as to overcome the shortcomings of the prior art.

[0010] The second purpose of the present invention is to propose a preparation method for the above-mentioned emulsifier-type cold-mix cold-laid asphalt mixture. The preparation method is simple and easy to operate, which is beneficial to avoid weakening the relevant properties of the asphalt mixture during the preparation process and is conducive to later recycling.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] An emulsifier-type cold-mix cold-paved asphalt mixture comprises, by weight, 400-600 parts of coarse aggregate, 400-600 parts of fine aggregate, 90-160 parts of modified emulsified asphalt, 10-30 parts of mineral filler, and 2-8 parts of a water-reactive resin demulsifier; wherein the molecular weight of the water-reactive resin demulsifier is 1 million to 10 million.

[0013] Furthermore, the crosslinking degree of the water-reactive resin demulsifier is 0.05 to 1.0%;

[0014] The molecular weight of the water-reactive resin demulsifier is 2 to 7 million.

[0015] Furthermore, the water absorption ratio of the water-reactive resin demulsifier is 30-100.

[0016] Furthermore, the water-reactive resin demulsifier includes a hydrophilic acrylic organic compound, sodium hydroxide, water, an initiator and a cross-linking agent.

[0017] Furthermore, the mass mixing ratio of the hydrophilic propylene organic compound to the sodium hydroxide is (1.5-2):1;

[0018] The mass mixing ratio of the initiator to the hydrophilic propylene organic compound is (2-3):2000;

[0019] The mass mixing ratio of the cross-linking agent to the hydrophilic acrylic organic compound is (3-5):4000.

[0020] Furthermore, the hydrophilic acrylic organic compound includes any one or a combination of two of acrylic acid and acrylamide;

[0021] The initiator includes any one of sodium persulfate and ammonium persulfate or a combination of the two;

[0022] The cross-linking agent is divinylbenzene.

[0023] Furthermore, the solid content of the modified emulsified asphalt is 62-65% by mass;

[0024] The modified emulsified asphalt includes an SBS modifier, and the amount of the SBS modifier added is ≥8% by mass;

[0025] The modified emulsified asphalt includes any one of star-shaped SBS modified asphalt and linear SBS modified asphalt.

[0026] Furthermore, the modified emulsified asphalt has an elastic recovery of ≥95% at 25°C and a composite shear modulus G at 60°C. * ≥10KPa, 60℃ dynamic viscosity ≥40,000Pa·s, G of evaporation residue * / sinδ≥2.2kPa, critical temperature≥88℃.

[0027] A method for preparing an emulsifier-type cold-mix cold-paved asphalt mixture, for preparing the above-mentioned emulsifier-type cold-mix cold-paved asphalt mixture, comprises the following steps:

[0028] A. mixing the coarse aggregate and the fine aggregate to obtain a first mixed aggregate;

[0029] B. adding modified emulsified asphalt and mineral filler to the first mixed aggregate and stirring to obtain a second mixed aggregate;

[0030] C. adding a water-reactive resin demulsifier to the second mixed aggregate and stirring the mixture to obtain an emulsifier-type cold-mix cold-paved asphalt mixture;

[0031] D. Compact the prepared emulsified cold-mixed cold-laid asphalt mixture at room temperature and cure it at 110°C for 11 to 13 hours.

[0032] Furthermore, the stirring time of step A is 20 to 40 s; the stirring time of step B is 50 to 70 s, the stirring time of step C is 20 to 60 s, and the total stirring time of steps A, B and C is ≥108 s.

[0033] The technical solutions provided by the embodiments of the present application may have the following beneficial effects:

[0034] 1. The water-reactive resin demulsifier uses the water in the modified emulsified asphalt as a reactant, forming a strong hydrogen bond with the water in the modified emulsified asphalt, causing the modified emulsified asphalt to demulsify and adhere to the surface of the aggregate to form an asphalt film to wrap and bond the aggregate, so that the asphalt mixture is bonded to form a whole, ensuring the early strength of the asphalt mixture, and avoiding the situation where the residual water after the modified emulsified asphalt is demulsified cannot be discharged in time, and excessive free water causes poor adhesion between the emulsified asphalt and the aggregate, affecting the early strength of the cold-mixed cold-laid asphalt mixture; at the same time, the water-reactive resin demulsifier will solidify and provide a certain strength during the demulsification process of the modified emulsified asphalt to ensure the early strength of the asphalt mixture. In addition, since the water-reactive resin demulsifier uses the water in the modified emulsified asphalt as a reactant, it consumes the water in the modified emulsified asphalt at a faster rate, which can accelerate the demulsification of the emulsified asphalt at room temperature, so that the asphalt mixture can increase the speed of forming early strength without adding cement; in addition, since no cement is used, on the one hand, it is conducive to later recycling and on the other hand, it also avoids the emulsifier-type cold-mixed cold-laid asphalt mixture becoming brittle during long-term use, and the anti-cracking performance will decrease, resulting in cracks in the asphalt pavement and a decrease in road performance.

[0035] 2. Since the early strength of asphalt mixture and the speed of early strength formation are greatly affected by water-reactive resin demulsifiers, when ordinary water-reactive resin demulsifiers are used, the modified emulsified asphalt will not be demulsified enough, making it impossible for the modified emulsified asphalt to wrap and bond the aggregate well, and the early strength cannot be guaranteed. At the same time, the demulsification speed is also slow, which makes the early strength formation speed slow. Therefore, this plan controls the molecular weight of the water-reactive resin demulsifier to reach 1 to 10 million to ensure the performance of the asphalt mixture. If the molecular weight of the water-reactive resin demulsifier is greater than 10 million, its reaction rate with the water in the modified emulsified asphalt is too fast, making it impossible for the modified emulsified asphalt to wrap and bond the aggregate well, resulting in poor bonding performance between the modified emulsified asphalt and the aggregate, greatly reducing the asphalt film thickness between the aggregates, and reducing the early strength of the asphalt mixture, making it impossible to guarantee road performance; if the molecular weight of the water-reactive resin demulsifier is less than 1 million, its reaction rate with the water in the emulsified asphalt is slow, and the expected early strength formation rate cannot be achieved.

[0036] 3. The technical solution proposes a method for preparing an emulsifier-type cold-mixed cold-laid asphalt mixture, which has simple steps and strong operability, is conducive to avoiding weakening the relevant properties of the asphalt mixture during the preparation process, and is conducive to later recycling and utilization. DETAILED DESCRIPTION

[0037] The present technical solution provides an emulsifier-type cold-mix cold-laid asphalt mixture, which includes, by weight, 400-600 parts of coarse aggregate, 400-600 parts of fine aggregate, 90-160 parts of modified emulsified asphalt, 10-30 parts of mineral filler and 2-8 parts of water-reactive resin demulsifier; wherein the molecular weight of the water-reactive resin demulsifier is 1 million to 10 million.

[0038] In order to accelerate the early strength formation of asphalt mixture without using cement and ensuring its road performance, and to solve the technical problem of difficulty in recycling pavement paved with asphalt mixture containing cement in the existing technology, this technical solution proposes an emulsifier-type cold-mix cold-paved asphalt mixture, the raw materials of which include coarse aggregate, fine aggregate, modified emulsified asphalt, mineral filler and water-reactive resin demulsifier.

[0039] First, the water-reactive resin demulsifier uses the water in the modified emulsified asphalt as a reactant, forming a strong hydrogen bond with the water in the modified emulsified asphalt, causing the modified emulsified asphalt to demulsify, adhere to the surface of the aggregate to form an asphalt film to wrap and bond the aggregate, so that the asphalt mixture is bonded to form a whole, ensuring the early strength of the asphalt mixture, and avoiding the situation where the residual water after the modified emulsified asphalt is demulsified cannot be discharged in time, and excessive free water causes poor adhesion between the emulsified asphalt and the aggregate, affecting the early strength of the cold-mixed cold-laid asphalt mixture; at the same time, the water-reactive resin demulsifier will solidify and provide a certain strength during the demulsification process of the modified emulsified asphalt to ensure the early strength of the asphalt mixture. In addition, since the water-reactive resin demulsifier uses the water in the modified emulsified asphalt as a reactant, it consumes the water in the modified emulsified asphalt at a faster rate, which can accelerate the demulsification of the emulsified asphalt at room temperature, so that the asphalt mixture can increase the speed of forming early strength without adding cement; in addition, since no cement is used, on the one hand, it is conducive to later recycling and on the other hand, it also avoids the emulsifier-type cold-mixed cold-laid asphalt mixture becoming brittle during long-term use, and the anti-cracking performance will decrease, resulting in cracks in the asphalt pavement and a decrease in road performance.

[0040] Since the early strength of asphalt mixture and the speed of early strength formation are greatly affected by water-reactive resin demulsifiers, when ordinary water-reactive resin demulsifiers are used, the modified emulsified asphalt will not be demulsified enough, making it impossible for the modified emulsified asphalt to wrap and bond the aggregate well, and the early strength cannot be guaranteed. At the same time, the demulsification speed is also slow, which makes the early strength formation speed slow. Therefore, this scheme controls the molecular weight of the water-reactive resin demulsifier to reach 1 to 10 million to ensure the performance of the asphalt mixture. If the molecular weight of the water-reactive resin demulsifier is greater than 10 million, its reaction rate with the water in the modified emulsified asphalt is too fast, making it impossible for the modified emulsified asphalt to wrap and bond the aggregate well, resulting in poor bonding performance between the modified emulsified asphalt and the aggregate, greatly reducing the asphalt film thickness between the aggregates, and reducing the early strength of the asphalt mixture, making it impossible to guarantee road performance; if the molecular weight of the water-reactive resin demulsifier is less than 1 million, its reaction rate with the water in the emulsified asphalt is slow, and the expected early strength formation rate cannot be achieved.

[0041] Furthermore, the asphalt mixture in the present technical solution also includes coarse aggregate and fine aggregate. The coarse aggregate and fine aggregate in the asphalt mixture constitute the key to the skeleton structure. The coarse aggregates are embedded in each other to form the skeleton of the asphalt mixture, providing support for the asphalt mixture. The fine aggregate can fill the skeleton to ensure the strength and stability of the skeleton structure. At the same time, the surface of the coarse aggregate is rough and dry, and has a low water absorption rate, which is conducive to increasing its adhesion with the modified emulsified asphalt, ensuring the strength of the asphalt mixture, and thus ensuring its road performance.

[0042] Furthermore, the modified emulsified asphalt in this technical solution not only breaks the emulsion under the action of the water-reactive resin demulsifier, but also adheres to the surface of the aggregate to form an asphalt film to wrap the aggregate, so that the asphalt mixture is bonded to form a whole, thereby ensuring the strength of the asphalt mixture. In addition, it can also deform in high and low temperature environments to prevent the asphalt mixture from being damaged, thereby further ensuring the road performance of the asphalt mixture.

[0043] In addition, adding mineral fillers to the asphalt mixture can effectively increase the thickness of the asphalt film, thereby improving its anti-aging ability. In addition, it combines with modified emulsified asphalt to form asphalt mortar, filling the remaining gaps in the mixture skeleton, playing the role of sealing the gaps and transferring loads, ensuring that the road surface has good shear resistance and bonding strength, and further ensuring the road performance of the asphalt mixture.

[0044] Preferably, the mineral filler in this technical solution is mineral powder. Mineral powder has a large surface area and a strong adsorption capacity for asphalt. Using mineral powder as a filler in this solution can effectively increase the thickness of the asphalt film, while improving the strength of the asphalt mixture, and further ensuring the road performance of the asphalt mixture.

[0045] It should be noted that the coarse aggregate used in this technical solution can be diabase crushed stone, and the fine aggregate can be limestone machine-made sand, which is not limited here.

[0046] In terms of mass, the asphalt mixture of this scheme includes 400-600 parts of coarse aggregate, 400-600 parts of fine aggregate, 90-160 parts of modified emulsified asphalt, 10-30 parts of mineral filler and 2-8 parts of water-reactive resin demulsifier.

[0047] Water-reactive resin demulsifier uses the water in modified emulsified asphalt as a reactant, and demulsifies the modified emulsified asphalt at room temperature through physical and chemical reactions, ensuring the early strength of the asphalt mixture and its road performance, while accelerating the formation speed of the early strength of the asphalt mixture. When the amount of water-reactive resin demulsifier added is less than 2 parts, the modified emulsified asphalt demulsifies too slowly, causing the asphalt mixture to form slowly at room temperature, affecting the speed of early strength formation of the asphalt mixture; at the same time, the modified emulsified asphalt demulsifies too slowly, and the modified emulsified asphalt has insufficient adhesion to the aggregate, resulting in the aggregate and the modified emulsified asphalt being unable to bond into a whole, affecting the early strength of the asphalt mixture, and thus resulting in its insufficient road performance; when the amount of water-reactive resin demulsifier added is greater than 8 parts, the modified emulsified asphalt demulsifies faster, causing the modified emulsified asphalt to demulsify between the aggregates before completely coating the aggregates, and failing to play a good role in bonding the aggregates, resulting in a large number of adhesive interfaces between the modified emulsified asphalt and the aggregate failing, which also affects the early strength of the asphalt mixture and resulting in its insufficient road performance.

[0048] Modified emulsified asphalt primarily wraps and bonds aggregates, forming the asphalt mixture into a cohesive whole and ensuring its early strength. It can also deform in high and low temperature environments to prevent damage to the asphalt mixture, thereby improving the performance of the asphalt mixture. When the amount of modified emulsified asphalt added exceeds 160 parts, the asphalt film between the aggregates becomes too thick due to the excessive amount of modified emulsified asphalt, making it difficult to extrude the aggregates together, affecting the early strength of the asphalt mixture. Furthermore, the excessive thickness of the asphalt film between the aggregates results in insufficient shear resistance, which can also lead to problems such as oil spillage and rutting, affecting its road performance. When the amount of modified emulsified asphalt added is less than 90 parts, the modified emulsified asphalt will not be able to adequately wrap the aggregates, resulting in insufficient internal bonding strength within the asphalt mixture, affecting the early strength of the asphalt mixture and resulting in insufficient road performance.

[0049] Coarse aggregate forms a skeleton structure and plays a role in supporting the asphalt mixture. Therefore, its addition amount is limited to 400-600 parts. If the addition amount of coarse aggregate is greater than 600 parts, the internal voids of the asphalt mixture will become larger. When the amount of fine aggregate and modified emulsified asphalt remains unchanged, the modified emulsified asphalt covering the aggregate will decrease, which will seriously affect the bonding strength between the aggregates in the asphalt mixture and its road performance. If the addition amount of coarse aggregate is less than 400 parts, the modified emulsified asphalt and fine aggregate in the asphalt mixture will be excessive, resulting in the asphalt mixture being too dense and difficult to form a skeleton structure. When it is used to pave the road, it will cause problems such as oil spillage and displacement, affecting its road performance.

[0050] Fine aggregate mainly plays the role of filling the skeleton structure and ensuring the bonding strength of asphalt mixture. Therefore, its addition amount is limited to 400-600 parts. If the addition amount of fine aggregate is greater than 600 parts, it will lead to the inability to form a sufficiently strong skeleton interlocking effect between the coarse aggregates, which will weaken the strength and stability of the asphalt mixture. At the same time, it will also cause the asphalt mortar composed of modified emulsified asphalt and mineral filler to overflow, affecting the bonding strength and shear resistance of the asphalt mixture, and affecting its road performance; if the addition amount of fine aggregate is less than 400 parts, it will lead to too many voids inside the mixture and fail to fully fill the skeleton structure, affecting the strength and stability of the skeleton structure, and ultimately affecting the early strength and shear resistance of the asphalt mixture, and affecting its road performance.

[0051] Mineral filler is one of the raw materials for forming asphalt mortar to fill the voids in the skeleton structure of the mixture. When the amount of mineral filler added is less than 10 parts, it cannot form asphalt mortar of sufficient strength with the modified emulsified asphalt, the adhesion is reduced, and it is difficult to bond the aggregates together, affecting the early strength of the asphalt mixture; when the amount of mineral filler added is greater than 30 parts, it also makes it difficult to extrude the aggregates, affecting the early strength of the asphalt mixture, and the oil film thickness between the aggregates is too large, resulting in insufficient shear resistance of the asphalt mixture. At the same time, it will also cause problems such as oil spillage and rutting, affecting its road performance.

[0052] It is further described that the crosslinking degree of the water-reactive resin demulsifier is 0.05 to 1.0%;

[0053] The molecular weight of the water-reactive resin demulsifier is 2 to 7 million.

[0054] The degree of cross-linking refers to the degree to which polymer molecular chains are connected to each other through chemical bonds or physical bonds. It determines the structural strength and swelling properties of water-reactive resin demulsifiers. The appropriate degree of cross-linking helps ensure the demulsification function of water-reactive resin demulsifiers. If the cross-linking degree of the water-reactive resin demulsifier is greater than 1.0%, the number of cross-linking points increases, and due to the shortened cross-linking distance, the internal rotation effect of the single bond of the cross-linking point is gradually lost, which will greatly limit the realization of the demulsification function of the water-reactive resin demulsifier; if the cross-linking degree of the water-reactive resin demulsifier is less than 0.05%, on the one hand, the molecular chain of the water-reactive resin demulsifier will swell or even break due to the penetration of water molecules, affecting the realization of its demulsification function. On the other hand, it will also cause the water-reactive resin demulsifier to demulsify too quickly, resulting in significantly uneven demulsification, affecting the early strength of the asphalt mixture and the speed of early strength formation, and also affecting the road performance and durability of the asphalt such as crack resistance and impact resistance. Therefore, in one embodiment of the present technical solution, the cross-linking degree of the water-reactive resin demulsifier is 0.05-1.0%, ensuring that the asphalt mixture has a higher early strength, further guaranteeing its road performance, and at the same time improving the speed of early strength formation.

[0055] In a preferred embodiment of the present technical solution, the molecular weight of the water-reactive resin demulsifier is 2 to 7 million, thereby further ensuring the early strength of the asphalt mixture and ensuring its road performance; at the same time, increasing the speed of early strength formation.

[0056] It is further explained that the water absorption rate of the water-reactive resin demulsifier is 30-100.

[0057] The water absorption ratio refers to the amount of water that can be consumed per unit dose of a water-reactive resin demulsifier. It reflects the hydrophilicity of the water-reactive resin demulsifier and determines its demulsification rate. If the water absorption ratio of the water-reactive resin demulsifier is greater than 100, the modified emulsified asphalt demulsifies quickly, affecting its adhesion to aggregates. This leads to insufficient bonding strength within the asphalt mixture, affecting the early strength of the asphalt mixture and its road performance. If the water absorption ratio of the water-reactive resin demulsifier is less than 30, its reaction rate with water in the modified emulsified asphalt slows down, affecting the speed of early strength development. Therefore, in another embodiment of the present technical solution, the water absorption ratio of the water-reactive resin demulsifier is between 30 and 100 to further ensure the road performance of the asphalt mixture and its rapid early strength development.

[0058] It is further explained that the water-reactive resin demulsifier includes a hydrophilic acrylic organic compound, sodium hydroxide, water, an initiator and a cross-linking agent.

[0059] In one embodiment of the present invention, the raw materials of the water-reactive resin demulsifier include a hydrophilic propylene organic compound, sodium hydroxide, water, an initiator, and a cross-linking agent. Water is used as a solvent to dissolve the sodium hydroxide to obtain a sodium hydroxide solution, which helps remove impurities in the sodium hydroxide. The sodium hydroxide chemically reacts with the hydrophilic propylene organic compound to form an propylene salt, which increases the hydrophilicity and reactivity of the hydrophilic propylene organic compound. This facilitates the polymerization of the hydrophilic propylene organic compound under the action of the initiator and cross-linking agent to form a water-reactive resin demulsifier with a three-dimensional network structure, ensuring that the water-reactive resin demulsifier has a molecular weight, cross-linking degree, and water absorption rate within the expected range, as well as good mechanical strength and stability. If the hydrophilic propylene organic compound is directly polymerized under the action of the initiator and cross-linking agent without the addition of sodium hydroxide, the polymerization reaction will be incomplete and the polymerization reaction rate will be slow, which will also affect the molecular weight, cross-linking degree, and water absorption rate of the water-reactive resin demulsifier, and ultimately also affect the road performance and early strength development rate of the asphalt mixture.

[0060] It is further described that the mass mixing ratio of the hydrophilic propylene organic compound to the sodium hydroxide is (1.5-2):1;

[0061] The mass mixing ratio of the initiator to the hydrophilic propylene organic compound is (2-3):2000;

[0062] The mass mixing ratio of the cross-linking agent to the hydrophilic acrylic organic compound is (3-5):4000.

[0063] In one embodiment of the present technical solution, the mass mixing ratio of the hydrophilic propylene organic compound and sodium hydroxide is preferably (1.5-2):1, so that the hydrophilic propylene organic compound and sodium hydroxide react completely, thereby improving the hydrophilicity and reactivity of the hydrophilic propylene organic compound. If the mass mixing ratio of the hydrophilic propylene organic compound and sodium hydroxide is less than 1.5:1, it is easy to cause the presence of incompletely reacted hydroxide ions in the solution, which increases the pH value of the solution, resulting in unstable reaction conditions and difficult to control, which is not conducive to the subsequent polymerization reaction of the hydrophilic propylene organic compound, affecting the molecular weight and water absorption rate of the water-reactive resin demulsifier and other properties, and ultimately affecting the road performance of the asphalt mixture and the speed of early strength formation; if the mass mixing ratio of the hydrophilic propylene organic compound and sodium hydroxide is greater than 2:1, the hydrophilic propylene organic compound is not completely reacted, and there are unneutralized hydrophilic groups, which is not conducive to improving the hydrophilicity and reactivity of the hydrophilic propylene organic compound, which will affect the molecular weight and water absorption rate of the water-reactive resin demulsifier and other properties, and ultimately affect the road performance of the asphalt mixture and the speed of early strength formation.

[0064] In another embodiment of the present technical solution, the mass mixing ratio of the initiator to the hydrophilic propylene organic compound is preferably (2-3):2000, and at the same time, the mass mixing ratio of the cross-linking agent to the hydrophilic propylene organic compound is preferably (3-5):4000, to ensure that the water-reactive resin demulsifier has a suitable degree of cross-linking, thereby ensuring that the asphalt mixture has a higher early strength, further ensuring its road performance, and at the same time improving the early strength formation rate. If the amount of initiator and cross-linker added is too small, it will easily lead to insufficient cross-linking degree of the obtained water-reactive resin demulsifier, and the cross-linking degree determines the structural strength and swelling performance of the water-reactive resin demulsifier. Therefore, if the amount of initiator and cross-linker added is too small, it will easily lead to the molecular chain of the obtained water-reactive resin demulsifier swelling or even breaking due to the penetration of water molecules, causing the water-reactive resin demulsifier to dissolve in water, and the demulsification function will be weakened. The demulsification function has a greater influence on the early strength and early strength of asphalt mixture. Therefore, if the amount of initiator and cross-linker added is too small, it will also affect the road performance of asphalt mixture and the speed of formation of early strength; if the amount of initiator and cross-linker added is too large, it will easily lead to excessive cross-linking of the obtained water-reactive resin demulsifier, limiting the realization of the demulsification function of the water-reactive resin demulsifier, and also affecting the road performance of asphalt mixture and the speed of formation of early strength.

[0065] It is further described that the hydrophilic acrylic organic compound includes any one or a combination of two of acrylic acid and acrylamide;

[0066] The initiator includes any one of sodium persulfate and ammonium persulfate or a combination of the two;

[0067] The cross-linking agent is divinylbenzene.

[0068] In a preferred embodiment of the present technical solution, the hydrophilic acrylic organic compound includes any one or a combination of two of acrylic acid and acrylamide. Acrylic acid contains a hydrophilic group carboxyl, and acrylamide contains a hydrophilic group amide. This gives the water-reactive resin demulsifier obtained by polymerization reaction of the acrylic organic compound good hydrophilicity, increases the reaction rate of the water-reactive resin demulsifier with water in the modified emulsified asphalt, and thus increases the speed of forming early strength.

[0069] Since sodium persulfate and ammonium persulfate have good stability at room temperature, are easy to store, convenient to use and safe, in another preferred embodiment of the present technical solution, any one or a combination of sodium persulfate and ammonium persulfate is used as an initiator to make the crosslinking degree of the water-reactive resin demulsifier meet actual requirements, and at the same time, it is easy to store and use.

[0070] Since different cross-linking agents have different reactivity and cross-linking efficiency, in another preferred embodiment of the present technical solution, the cross-linking agent is preferably divinylbenzene to meet the cross-linking degree requirement of the water-reactive resin demulsifier.

[0071] It is further stated that, in terms of mass percentage, the solid content of the modified emulsified asphalt is 62-65%;

[0072] The modified emulsified asphalt includes an SBS modifier, and the amount of the SBS modifier added is ≥8% by mass;

[0073] The modified emulsified asphalt includes any one of star-shaped SBS modified asphalt and linear SBS modified asphalt.

[0074] In a preferred embodiment of this technical solution, the solids content of the modified emulsified asphalt is 62-65% by weight, further enhancing the viscoelastic properties of the modified emulsified asphalt, thereby further improving the early strength of the asphalt mixture and its road performance. If the solids content of the modified asphalt is outside this range, the emulsification properties, stability, viscosity, and high-temperature performance of the modified emulsified asphalt will be affected, thereby affecting the road performance of the asphalt pavement formed by the asphalt mixture, such as rutting resistance and cracking resistance.

[0075] In another preferred embodiment of the present technical solution, the modified emulsified asphalt includes an SBS modifier, and the added amount of the SBS modifier is ≥8% calculated by mass, which further improves the early strength of the asphalt mixture and further improves its road performance.

[0076] Preferably, the modified emulsified asphalt includes an SBS modifier, and the added amount of the SBS modifier is ≥ 10% calculated as a percentage by mass.

[0077] More preferably, in one embodiment of the present technical solution, the modified emulsified asphalt includes any one of star-shaped SBS modified asphalt or linear SBS modified asphalt. The star-shaped SBS modified asphalt or linear SBS modified asphalt can not only adhere to the surface of the aggregate at room temperature to form an asphalt film to wrap and bond the aggregate, so that the asphalt mixture is bonded to form a whole, ensuring that the asphalt mixture has good early strength, but also has excellent viscoelastic properties, further improving the early strength of the asphalt mixture, thereby improving its road performance.

[0078] Further description: the modified emulsified asphalt has an elastic recovery of ≥95% at 25°C and a composite shear modulus G at 60°C. * ≥10KPa, 60℃ dynamic viscosity ≥40,000Pa·s, G of evaporation residue * / sinδ≥2.2kPa, critical temperature≥88℃.

[0079] In a preferred embodiment of the present technical solution, the modified emulsified asphalt has an elastic recovery of ≥95% at 25°C, a composite shear modulus G* ≥10 kPa at 60°C, a dynamic viscosity ≥40,000 Pa·s at 60°C, a G* / sinδ of the evaporation residue ≥2.2 kPa, and a critical temperature ≥88°C, which further improves the early strength of the asphalt mixture and further improves its road performance.

[0080] A method for preparing an emulsifier-type cold-mix cold-paved asphalt mixture, for preparing the emulsifier-type cold-mix cold-paved asphalt mixture, comprises the following steps:

[0081] A. mixing the coarse aggregate and the fine aggregate to obtain a first mixed aggregate;

[0082] B. adding modified emulsified asphalt and mineral filler to the first mixed aggregate and stirring to obtain a second mixed aggregate;

[0083] C. adding a water-reactive resin demulsifier to the second mixed aggregate and stirring the mixture to obtain an emulsifier-type cold-mix cold-paved asphalt mixture;

[0084] D. Compact the prepared emulsified cold-mixed cold-laid asphalt mixture at room temperature and cure it at 110°C for 11 to 13 hours.

[0085] This technical solution also proposes a method for preparing an emulsifier-type cold-mixed and cold-laid asphalt mixture, which has simple steps and strong operability, is conducive to avoiding weakening the relevant properties of the asphalt mixture during the preparation process, and is conducive to later recycling and utilization. In addition, the prepared emulsifier-type cold-mixed cold-laid asphalt mixture is compacted at room temperature and cured at a temperature of 110°C for 11 to 13 hours, with a water loss rate of more than 98%, which can meet the road performance and realize the opening of the asphalt pavement as soon as possible; and the asphalt pavement paved with the asphalt mixture in the present technical solution has a water loss rate of more than 99% after curing at a temperature of 110°C for 24 hours, while the asphalt pavement paved with the traditional emulsifier-type cold-mixed cold-laid asphalt mixture has a water loss rate of 87% to 93% after curing at 110°C for 24 hours. Therefore, the early water loss rate and water loss rate of the asphalt pavement paved with the asphalt mixture in the present technical solution are higher than those of the asphalt pavement paved with the traditional emulsifier-type cold-mixed cold-laid asphalt mixture. The water loss rate in the asphalt mixture is closely related to its strength. The higher the water loss rate, the higher its strength. Therefore, the early strength and early strength rate of the asphalt mixture obtained by the present technical solution are higher than those of the traditional asphalt mixture. Under the premise of ensuring its road performance, the speed of early strength formation of the asphalt mixture is accelerated.

[0086] Preferably, in steps A, B and C, the stirring should be carried out uniformly to further ensure the relevant properties of the asphalt mixture.

[0087] Preferably, in step C, the water-reactive resin demulsifier is added to the second mixed aggregate at a constant rate and stirred, so that the water-reactive resin demulsifier and the second mixed aggregate are stirred more evenly, thereby making the water-reactive resin demulsifier react more evenly with the modified emulsified asphalt, strengthening the wrapping and adhesion of the modified emulsified asphalt to the second mixed aggregate, which is beneficial to improving the early strength of the asphalt mixture and improving its road performance.

[0088] Preferably, in step D, the prepared emulsifier type cold mix cold paving asphalt mixture is compacted at room temperature and cured at a temperature of 110°C for 12 hours, thereby ensuring the performance of the emulsifier type cold mix cold paving asphalt mixture while shortening the open time of the asphalt.

[0089] Further description: the stirring time of step A is 20 to 40 s; the stirring time of step B is 50 to 70 s, the stirring time of step C is 20 to 60 s, and the total stirring time of steps A, B and C is ≥108 s.

[0090] In a preferred embodiment of the present technical solution, the stirring time of step B is 20 to 40 seconds, so that the coarse aggregate and fine aggregate are distributed more evenly. At the same time, it avoids stirring for too long, which may cause the coarse aggregate to be excessively worn during the stirring process, and the angularity and integrity are damaged, thereby weakening the adhesion with asphalt, affecting the early strength and affecting its road performance.

[0091] In another preferred embodiment of the present technical solution, the stirring time of step C is 50 to 70 seconds, the stirring time of step D is 20 to 60 seconds, and the total stirring time of steps B, C and D is ≥108 seconds, which is conducive to ensuring the relevant performance of the asphalt mixture.

[0092] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0093] Example 1

[0094] Prepare a water-reactive resin demulsifier: the water-reactive resin demulsifier has a molecular weight of 1 million, a cross-linking degree of 0.05%, and a water absorption rate of 30;

[0095] Prepare asphalt mixture raw materials according to mass parts: 400 parts of diabase crushed stone, 600 parts of limestone machine-made sand, 160 parts of star-shaped SBS modified asphalt, 10 parts of mineral powder and 2 parts of water-reactive resin demulsifier. Among them, the solid content of star-shaped SBS modified asphalt is 62%, the addition amount of modifier is 8%, the elastic recovery of star-shaped SBS modified asphalt at 25℃ is 95%, and the composite shear modulus G at 60℃ is 100%. * The dynamic viscosity is 10KPa, the 60℃ dynamic viscosity is 40,000Pa·s, and the G of the evaporation residue is * / sinδ is 2.2kPa and the critical temperature is 88℃.

[0096] The coarse aggregate and the fine aggregate are stirred for 20 seconds to obtain a first mixed aggregate;

[0097] adding modified emulsified asphalt and mineral filler into the first mixed aggregate and stirring for 50 seconds to obtain a second mixed aggregate;

[0098] A water-reactive resin demulsifier is added to the second mixed aggregate and stirred for 60 seconds to obtain an emulsifier-type cold-mix cold-paved asphalt mixture;

[0099] The prepared emulsifier type cold mix cold paving asphalt mixture was compacted at room temperature and cured at a temperature of 110°C for 11 hours.

[0100] Example 2

[0101] Prepare water-reactive resin demulsifier raw materials: acrylic acid and sodium hydroxide in a mass ratio of 1.5:1, sodium persulfate and acrylic acid in a mass ratio of 1:1000, and divinylbenzene and acrylic acid in a mass ratio of 3:4000; the water-reactive resin demulsifier has a molecular weight of 5 million, a cross-linking degree of 0.5%, and a water absorption ratio of 50;

[0102] Prepare asphalt mixture raw materials according to mass parts: 500 parts of diabase crushed stone, 500 parts of limestone machine-made sand, 125 parts of linear SBS modified asphalt, 20 parts of mineral powder and 5 parts of water-reactive resin demulsifier. Among them, the solid content of linear SBS modified asphalt is 63.5%, the addition amount of modifier is 10%, the elastic recovery of linear SBS modified asphalt at 25℃ is 95%, and the composite shear modulus G at 60℃ is 10%. * The dynamic viscosity is 10KPa, the 60℃ dynamic viscosity is 40,000Pa·s, and the G of the evaporation residue is * / sinδ is 2.2kPa and the critical temperature is 88℃.

[0103] The hydrophilic acrylic organic compound, sodium hydroxide, water, an initiator and a cross-linking agent are reacted for 1 hour to obtain a water-reactive resin demulsifier;

[0104] The coarse aggregate and the fine aggregate are stirred for 30 seconds to obtain a first mixed aggregate;

[0105] adding modified emulsified asphalt and mineral filler into the first mixed aggregate and stirring for 60 seconds to obtain a second mixed aggregate;

[0106] A water-reactive resin demulsifier is added to the second mixed aggregate and stirred for 20 seconds to obtain an emulsifier-type cold-mix cold-paved asphalt mixture;

[0107] The prepared emulsified cold-mixed cold-paved asphalt mixture was compacted at room temperature and cured at 110°C for 12 hours.

[0108] Example 3

[0109] Prepare water-reactive resin demulsifier raw materials: acrylamide and sodium hydroxide in a mass mixing ratio of 2:1, sodium persulfate and acrylamide in a mass mixing ratio of 3:2000, and divinylbenzene and acrylamide in a mass mixing ratio of 5:4000; the water-reactive resin demulsifier has a molecular weight of 10 million, a cross-linking degree of 1.00%, and a water absorption rate of 100;

[0110] Prepare asphalt mixture raw materials according to mass parts: 600 parts of diabase crushed stone, 400 parts of limestone machine-made sand, 90 parts of star-shaped SBS modified asphalt, 30 parts of mineral powder and 8 parts of water-reactive resin demulsifier. Among them, the solid content of star-shaped SBS modified asphalt is 65.5%, the addition amount of modifier is 10%, the elastic recovery of star-shaped SBS modified asphalt at 25℃ is 95%, and the composite shear modulus G at 60℃ is 10%. * The dynamic viscosity is 10KPa, the 60℃ dynamic viscosity is 40,000Pa·s, and the G of the evaporation residue is * / sinδ is 2.2kPa and the critical temperature is 88℃.

[0111] The hydrophilic acrylic organic compound, sodium hydroxide, water, an initiator and a cross-linking agent are reacted for 2 hours to obtain a water-reactive resin demulsifier;

[0112] The coarse aggregate and the fine aggregate are stirred for 40 seconds to obtain a first mixed aggregate;

[0113] adding modified emulsified asphalt and mineral filler into the first mixed aggregate and stirring for 70 seconds to obtain a second mixed aggregate;

[0114] A water-reactive resin demulsifier is added to the second mixed aggregate and stirred for 40 seconds to obtain an emulsifier-type cold-mix cold-paved asphalt mixture;

[0115] The prepared emulsified cold-mix cold-paved asphalt mixture was compacted at room temperature and cured at 110°C for 13 hours.

[0116] Comparative Example 1

[0117] Emulsified asphalt mixture I was prepared according to a conventional method for asphalt mixture; wherein, in parts by mass, the emulsified asphalt mixture I included 545 parts of diabase crushed stone, 455 parts of limestone machine-made sand, 106 parts of star-shaped SBS modified asphalt and 16 parts of mineral powder; the prepared emulsified asphalt mixture I was compacted at room temperature and cured at a temperature of 110°C for 12 hours.

[0118] Comparative Example 2

[0119] Emulsified asphalt mixture II was prepared according to the conventional method of asphalt mixture; wherein, in terms of mass, it included 540 parts of diabase crushed stone, 460 parts of limestone machine-made sand, 109 parts of star-shaped SBS modified asphalt, 16 parts of mineral powder and 15 parts of ordinary Portland cement No. 42.5; the prepared emulsified asphalt mixture I was compacted at room temperature and cured at a temperature of 110°C for 12 hours.

[0120] The asphalt mixtures of Examples 1-3, Comparative Example 1, and Comparative Example 2 were used to pave asphalt pavements. The paving thicknesses were shown in Table 1 below. The paved asphalt pavements were tested for relevant properties according to the standards specified in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011). The results are shown in Table 1 below.

[0121] Table 1 Test results of relevant performance of asphalt pavement

[0122] From the performance test results in Table 1, it can be seen that the asphalt pavement paved by an emulsifier-type cold-mixed cold-laid asphalt mixture according to the present technical solution has a higher water loss rate after curing at 110°C for 12 hours and 24 hours than the asphalt pavement paved by the traditional cement-free emulsified asphalt mixture I and the asphalt pavement paved by the cement-containing emulsified asphalt mixture II. In addition, the asphalt pavement paved by the asphalt mixture according to the present technical solution has a higher water loss rate after curing at 110°C for 12 hours than the asphalt pavement paved by the traditional cement-free emulsified asphalt mixture I after curing at 110°C for 24 hours. The water loss rate is closely related to the strength of the asphalt pavement. The higher the water loss rate, the higher its strength. Therefore, the early strength and early strength speed of the asphalt mixture obtained by the present technical solution are higher than those of the traditional cement-free emulsified asphalt mixture I and the cement-containing emulsified asphalt mixture II.

[0123] In addition, it can be seen from Table 1 that the freeze-thaw splitting strength ratio of the asphalt pavement obtained by the present technical solution is higher than that of the asphalt pavement paved with the traditional cement-free emulsified asphalt mixture I and the asphalt pavement paved with the cement-containing emulsified asphalt mixture II. The freeze-thaw splitting strength ratio reflects the cracking property of the asphalt pavement. The higher the freeze-thaw splitting strength ratio, the stronger the anti-cracking performance. Therefore, the asphalt mixture obtained by the present technical solution has stronger anti-cracking performance than the traditional cement-free emulsified asphalt mixture I and the cement-containing emulsified asphalt mixture II.

[0124] At the same time, it can be seen from Table 1 that, except for the water loss rate and freeze-thaw splitting strength ratio, all other performance test indicators of the asphalt pavement obtained by this technical solution are superior to those of the asphalt pavement paved with the traditional cement-free emulsified asphalt mixture I. This breaks through the limitations of the use of the traditional cement-free emulsified asphalt mixture I, accelerates the speed of early strength formation of the asphalt mixture without using cement and ensuring its road performance, and solves the technical problem of the difficulty in recycling the pavement paved with the asphalt mixture, thereby overcoming the shortcomings of the existing technology.

[0125] The technical principles of the present invention have been described above with reference to specific embodiments. These descriptions are intended solely to illustrate the principles of the present invention and are not to be construed in any way as limiting the scope of protection of the present invention. Based on the explanations herein, those skilled in the art will readily conceive of other specific embodiments of the present invention without inventive effort, and such embodiments will fall within the scope of protection of the present invention.

Claims

1. An emulsifier type cold mix cold paving asphalt mixture, characterized by: According to the mass proportion, the composition comprises 400-600 parts of coarse aggregate, 400-600 parts of fine aggregate, 90-160 parts of modified emulsified asphalt, 10-30 parts of mineral filler and 2-8 parts of water-reactive resin demulsifier; wherein the molecular weight of the water-reactive resin demulsifier is 1 to 10 million.

2. The emulsified cold mix cold paving asphalt mixture according to claim 1, characterized in that: The crosslinking degree of the water-reactive resin demulsifier is 0.05 to 1.0%; The molecular weight of the water-reactive resin demulsifier is 2 to 7 million.

3. The emulsifier type cold mix cold paving asphalt mixture according to claim 1, characterized in that: The water-reactive resin demulsifier has a water absorption ratio of 30 to 100.

4. The emulsified cold mix cold paving asphalt mixture according to claim 1, characterized in that: The water-reactive resin demulsifier comprises a hydrophilic propylene organic compound, sodium hydroxide, water, an initiator and a cross-linking agent.

5. The emulsified cold mix cold paving asphalt mixture according to claim 4, characterized in that: The mass mixing ratio of the hydrophilic propylene organic compound to the sodium hydroxide is (1.5-2):1; The mass mixing ratio of the initiator to the hydrophilic propylene organic compound is (2-3):2000; The mass mixing ratio of the cross-linking agent to the hydrophilic acrylic organic compound is (3-5):4000.

6. The emulsifier type cold mix cold paving asphalt mixture according to claim 4, characterized in that: The hydrophilic acrylic organic compound includes any one or a combination of two of acrylic acid and acrylamide; The initiator includes any one of sodium persulfate and ammonium persulfate or a combination of the two; The crosslinking agent is divinylbenzene.

7. The emulsifier type cold mix cold paving asphalt mixture according to claim 1, characterized in that: In terms of mass percentage, the solid content of the modified emulsified asphalt is 62-65%; The modified emulsified asphalt includes an SBS modifier, and the added amount of the SBS modifier is ≥ 8% by mass percentage; The modified emulsified asphalt includes any one of star-shaped SBS modified asphalt and linear SBS modified asphalt.

8. The emulsifier type cold mix cold paving asphalt mixture according to claim 1, characterized in that: The modified emulsified asphalt has an elastic recovery of ≥95% at 25°C and a composite shear modulus G at 60°C. * ≥10KPa, 60℃ dynamic viscosity ≥40,000Pa·s, G of evaporation residue * / sinδ≥2.2kPa, critical temperature≥88℃.

9. A method for preparing an emulsified cold mix cold paving asphalt mixture, characterized in that: The method for preparing the emulsified cold mix cold paving asphalt mixture according to any one of claims 1 to 8 comprises the following steps: A. mixing the coarse aggregate and the fine aggregate to obtain a first mixed aggregate; B. adding modified emulsified asphalt and mineral filler into the first mixed aggregate and stirring to obtain a second mixed aggregate; C. adding a water-reactive resin demulsifier to the second mixed aggregate and stirring the mixture to obtain an emulsifier-type cold-mix cold-paved asphalt mixture; D. Compact the prepared emulsified cold-mixed cold-paved asphalt mixture at room temperature and cure it at 110°C for 11 to 13 hours.

10. The method for preparing an emulsified cold mix cold paving asphalt mixture according to claim 9, characterized in that: The stirring time of step A is 20 to 40 seconds; the stirring time of step B is 50 to 70 seconds, the stirring time of step C is 20 to 60 seconds, and the total stirring time of steps A, B and C is ≥108 seconds.

Citation Information

Patent Citations

  • Environment-friendly cold mixing high viscosity modified emulsified asphalt

    CN109337387A

  • Cement-waterborne acrylic resin emulsified asphalt concrete and preparation method thereof

    CN110156378A

  • Early-strength emulsified asphalt cold-mixed mixture and preparation method thereof

    CN116425457A

  • Emulsifier type cold-mixed and cold-laid asphalt mixture and preparation method thereof

    CN116789393A

  • Waterborn polymer-modified emulsified asphalt mixture and process for producing the same

    US20160185966A1

Cited By

  • Emulsified asphalt and steel slag ultrathin overlay mixture as well as preparation method and application thereof

    CN120698748A

  • Emulsified asphalt steel slag ultra-thin overlay mixture, preparation method and application thereof

    CN120698748B

  • Fiber reinforced asphalt mixture and preparation method thereof

    CN120829269A

  • Cold-mix asphalt mixture and preparation method thereof

    CN121270150A