Magnetic ion exchange resin, preparation method therefor, and use thereof

By using low-power ultraviolet light to initiate polymerization and alkylating agents to extend the carbon chain of quaternary ammonium groups, the problems of slow reaction rate and low adsorption efficiency in the preparation of magnetic ion exchange resins were solved, and efficient adsorption and removal of target anions were achieved.

WO2026232760A1PCT designated stage Publication Date: 2026-11-12MUNICIPAL ENVIRONMENTAL PROTECTION ENG CO LTD OF CREC SHANGHAI GRP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/130348
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2025-10-28
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for preparing magnetic ion exchange resins have slow reaction rates, are cumbersome to operate, and the quaternary ammonium groups in the resin are close together, making it impossible to efficiently adsorb target anions.

Method used

Low-power ultraviolet light is used to initiate the polymerization of glycidyl methacrylate, divinylbenzene, and magnetic materials to form a three-dimensional network structure. The carbon chain of the quaternary ammonium group is extended by an alkylating agent to improve the adsorption capacity.

Benefits of technology

The reaction time was shortened, a uniform three-dimensional network structure was formed, the spacing and contact area of ​​the quaternary ammonium groups were increased, and the adsorption capacity and removal efficiency of the target anions were improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025130348_12112026_PF_FP_ABST
    Figure CN2025130348_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a magnetic ion exchange resin, a preparation method therefor, and a use thereof. The method comprises: step 1, subjecting glycidyl methacrylate, divinylbenzene, a magnetic material, and a photoinitiator to a polymerization reaction under initiation by a light source, to obtain magnetic microspheres; step 2, adding an amination reagent to the magnetic microspheres to carry out an amination reaction, to obtain aminated magnetic microspheres; and step 3, adding an alkylating agent to the aminated magnetic microspheres to carry out a nucleophilic substitution reaction, to obtain a magnetic ion exchange resin, wherein the alkylating agent is any one of 1-iodohexane, 1-chlorohexane, and 1-bromohexane. The preparation method can shorten the process cycle and simplify a preparation apparatus; and the prepared magnetic ion exchange resin can efficiently adsorb more target anions, increase the adsorption capacity, achieve efficient removal of the target anions, and be well applied to wastewater treatment.
Need to check novelty before this filing date? Find Prior Art

Description

A magnetic ion exchange resin, its preparation method and its uses Technical Field

[0001] This invention relates to the field of wastewater treatment technology, and in particular to a magnetic ion exchange resin, its preparation method, and its uses. Background Technology

[0002] In the current field of environmental governance, ensuring water quality safety and the sustainable use of water resources remain the core priorities, and the importance of water treatment technology is self-evident.

[0003] Magnetic ion exchange resin, as an innovative water treatment material, forms a composite system by embedding magnetic materials into a polymer network, possessing both chemical adsorption and magnetic separation characteristics. Utilizing the resin's magnetic response properties, it achieves rapid separation from the treated water, significantly simplifying the operation process and reducing the use of chemical reagents compared to traditional resin acid-base regeneration processes. In the treatment of complex water qualities, magnetic ion exchange resin exhibits significant advantages: for example, in high-salinity industrial wastewater, its strong resistance to ion interference allows it to selectively bind to target pollutants such as heavy metal ions, achieving effective removal of heavy metals and ensuring treatment results; in the treatment of electroplating wastewater, saturated resin can rapidly enrich and recover precious metals through magnetic separation, achieving efficient resource utilization while simultaneously purifying the wastewater.

[0004] Existing methods for preparing magnetic ion exchange resins often employ thermal initiation techniques, resulting in slow reaction rates (typically 5-10 hours) and involving multiple instruments and equipment, making the operation cumbersome. Furthermore, to impart ion exchange properties to the resin, quaternary ammonium groups are introduced to chemically adsorb and bind target anions. However, the relatively short distances between quaternary ammonium groups containing short-chain alkyl groups hinder the entry of target anions into the resin for adsorption. Additionally, the shorter alkyl chains reduce the contact area between the quaternary ammonium groups and the target anions, resulting in inefficient adsorption and thus affecting the resin's removal efficiency.

[0005] The statements herein provide only background information in relation to the present invention and do not necessarily constitute prior art. Summary of the Invention

[0006] The purpose of this invention is to provide a simple and efficient method for preparing magnetic ion exchange resin, which shortens the process cycle, simplifies the preparation equipment, and increases the adsorption capacity of the resin for target anions, thereby achieving efficient removal of target anions.

[0007] To achieve the above objectives, the present invention provides a method for preparing a magnetic ion exchange resin, the method comprising:

[0008] Step 1: Glycidyl methacrylate, divinylbenzene, magnetic materials and photoinitiator undergo a polymerization reaction under the initiation of a light source to obtain magnetic microspheres;

[0009] Step 2: Add an ammoniation reagent to the magnetic microspheres to induce an ammoniation reaction, thereby obtaining ammoniation-treated magnetic microspheres;

[0010] Step 3: An alkylating agent is added to the ammoniated magnetic microspheres to undergo a nucleophilic substitution reaction, thereby obtaining a magnetic ion exchange resin; the alkylating agent comprises any one of 1-iodohexane, 1-chlorohexane, and 1-bromohexane.

[0011] Optionally, before step 1, the method further includes: modifying the magnetic material.

[0012] Optionally, in step 1, the light source includes any one of ultraviolet light, visible light, and near-infrared light.

[0013] Optionally, in step 1, the mass ratio of glycidyl methacrylate to divinylbenzene is (4.5-10):1, and the mass ratio of glycidyl methacrylate to magnetic material is (8-10):1.

[0014] Optionally, in step 1, the magnetic material includes either ferric oxide or magnetite.

[0015] Optionally, in step 1, the photoinitiator comprises any one of 2-hydroxy-2-methylphenylacetone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, camphorquinone, and indocyanine green-triethylamine complex.

[0016] Optionally, in step 2, the amination reagent includes either trimethylamine hydrochloride or trimethylamine hydroxide.

[0017] Optionally, step 3 may further include adding a catalyst, wherein the catalyst comprises any one of ferric chloride, aluminum chloride, and titanium tetrachloride.

[0018] The present invention also provides a magnetic ion exchange resin obtained by the above preparation method, wherein the magnetic ion exchange resin has a core-shell structure of the ammoniated magnetic microspheres coated with magnetic material; the degree of quaternization of the magnetic ion exchange resin is 65%-75%, and the mass ratio of the ammoniated magnetic microspheres to the magnetic material is (15-25):1.

[0019] The present invention also provides an application of the magnetic ion exchange resin obtained by the above preparation method, wherein the magnetic ion exchange resin is used for wastewater treatment, and the temperature of the wastewater in the wastewater treatment process is 5℃-35℃.

[0020] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects:

[0021] 1) Under low-power ultraviolet light irradiation, the photoinitiator absorbs light energy and decomposes to generate free radicals. The free radicals rapidly initiate the opening of the carbon-carbon double bonds of the glycidyl methacrylate monomer, and carry out a chain polymerization reaction to form a polymer chain. During the polymerization process, the ends of polymer chains typically carry free radicals, giving them the ability to continue reacting. At this point, one double bond of divinylbenzene reacts with the free radical-carrying polymer chain, while the other double bond can further react with other polymer chains or divinylbenzene molecules, thus linking different polymer chains together to achieve a cross-linking reaction and form a three-dimensional network structure. Because the magnetic material is modified with oleic acid or a silane coupling agent (KH570), the unsaturated double bonds in oleic acid and the acrylic groups in glyceryl methacrylate undergo chemical bonding via free radical polymerization. The silane groups of the silane coupling agent (KH570) react chemically with the surface of the magnetic material to form silicon-oxygen metal bonds, thereby fixing the silane coupling agent to the surface of the magnetic material. Furthermore, the acrylic groups of the silane coupling agent (KH570) can participate in the polymerization reaction of glyceryl methacrylate monomers or divinylbenzene, forming a three-dimensional network structure. Through the above chemical reactions, the magnetic material is encapsulated within this three-dimensional network structure.

[0022] Compared with traditional thermal initiation, the low-power UV initiation of this invention achieves a significantly higher polymerization rate (reaction time 1h-3h) than thermal initiation (reaction time 5h-10h), greatly improving the speed and efficiency of monomer to polymer conversion. Furthermore, it can rapidly initiate the reaction at room temperature, allowing more molecules and active sites to fully participate in the crosslinking reaction within a short time. Active sites have more opportunities to react with molecules in different directions and positions, avoiding prolonged stagnation in a localized area. This prevents variations in crosslinking density in localized areas, reduces over- or under-crosslinking, and makes the spatial distribution of crosslinking points more random and uniform, facilitating the formation of a uniform three-dimensional network structure. This, in turn, promotes the diffusion of target anions within the resin, increasing adsorption capacity.

[0023] 2) Alkylating agents can extend the carbon chain length of the quaternary ammonium group in the resin to the hexyl group. On the one hand, the extended carbon chain increases the spacing between the quaternary ammonium groups, overcoming the steric hindrance problem of the quaternary ammonium groups, which is conducive to more target anions entering the resin and being adsorbed. On the other hand, the extended carbon chain increases the contact area between the quaternary ammonium groups and the target anions, which can efficiently adsorb more target anions and increase the adsorption capacity, thereby achieving efficient removal of target anions and making it well applied to wastewater treatment. Attached Figure Description

[0024] Figure 1 is a flowchart of the preparation method of the magnetic ion exchange resin of the present invention.

[0025] Figure 2 shows SEM images of the magnetic ion exchange resins prepared in Examples 1 and 2 of the present invention; wherein, a is the magnetic ion exchange resin prepared in Example 1, and b is the magnetic ion exchange resin prepared in Example 2.

[0026] Figure 3 shows the adsorption kinetics of phosphate ions by the magnetic ion exchange resins prepared in Examples 1 and 2 of the present invention; wherein, a is the magnetic ion exchange resin prepared in Example 1, and b is the magnetic ion exchange resin prepared in Example 2.

[0027] Figure 4 is an isotherm equilibrium diagram of the adsorption of phosphate ions by the magnetic ion exchange resins prepared in Examples 1 and 2 of the present invention; wherein, a is the magnetic ion exchange resin prepared in Example 1, and b is the magnetic ion exchange resin prepared in Example 2.

[0028] Figure 5 is a schematic diagram showing the effect of exogenous ions and natural organic matter on the adsorption of phosphate ions by the magnetic ion exchange resins prepared in Examples 1 and 2; where a is a schematic diagram showing the effect of exogenous ions on the adsorption of phosphate ions by the resin, and b is a schematic diagram showing the effect of natural organic matter on the adsorption of phosphate ions by the resin.

[0029] Figure 6 shows the Fourier transform infrared spectra of the magnetic ion exchange resins prepared in Examples 1 and 2 of the present invention; wherein, a is the magnetic ion exchange resin prepared in Example 1, and b is the magnetic ion exchange resin prepared in Example 2.

[0030] Figure 7 shows the X-ray diffraction comparison of the magnetic ion exchange resins prepared in Examples 1 and 2 of this invention before and after adsorption of phosphate ions. Detailed Implementation

[0031] The preparation method of the magnetic ion exchange resin proposed in this invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. The advantages and features of this invention will become clearer from the following description. It should be noted that the drawings are in a very simplified form and use non-precise proportions, only for the purpose of conveniently and clearly illustrating the embodiments of this invention. Please refer to the drawings to make the objectives, features, and advantages of this invention more apparent and understandable. It should be understood that the structures, proportions, sizes, etc., depicted in the accompanying drawings are only for the purpose of assisting those skilled in the art in understanding and reading the content disclosed in the specification, and are not intended to limit the implementation conditions of this invention. Therefore, they have no substantial technical significance. Any modifications to the structure, changes in the proportional relationships, or adjustments to the size, without affecting the effects and objectives achieved by this invention, should still fall within the scope of the technical content disclosed in this invention.

[0032] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0033] The resin described in this article is a chloride-type ion exchange resin, which contains chloride ions. Chloride ions have a large ionic radius and low charge density, resulting in a weak electrostatic attraction between them and the positively charged quaternary ammonium groups on the resin surface. When the resin is placed in a solution containing target anions (such as phosphate ions), the phosphate ions have a high charge density and a strong electrostatic attraction with the positively charged quaternary ammonium groups on the resin surface. Therefore, the chloride ions on the resin are replaced by phosphate ions, thereby achieving ion exchange.

[0034] As described in the background section, the preparation of magnetic ion exchange resins using traditional thermal initiation techniques results in slow reaction rates, long reaction times, complex equipment, and cumbersome operation. Furthermore, the quaternary ammonium groups in the resin, which have ion exchange capabilities, contain short-chain alkyl groups with relatively close proximity, hindering the entry and adsorption of target anions into the resin. Simultaneously, the short alkyl chains of the quaternary ammonium groups reduce the contact area with target anions, resulting in inefficient adsorption and thus diminishing the resin's removal efficiency.

[0035] To address the aforementioned problems, this invention provides a method for preparing a magnetic ion exchange resin. First, glycidyl methacrylate, divinylbenzene, magnetic materials, and a photoinitiator undergo a polymerization reaction under a light source to obtain magnetic microspheres. Then, an ammoniation reagent is added to the magnetic microspheres to induce an ammoniation reaction, resulting in ammoniated magnetic microspheres. Finally, an alkylating agent is added to the ammoniated magnetic microspheres to induce a nucleophilic substitution reaction, yielding the magnetic ion exchange resin. At room temperature, ultraviolet light initiation promotes the decomposition of the photoinitiator to generate free radicals. These free radicals rapidly initiate the polymerization reaction of the glycidyl methacrylate monomer and the crosslinking reaction between the polymer chain and divinylbenzene, promoting the formation of a uniform three-dimensional network structure, which is beneficial for the diffusion of target anions within the resin. Simultaneously, the alkylating agent extends the carbon chain length of the quaternary ammonium group in the resin to the hexyl group, increasing the spacing between the quaternary ammonium groups and the contact area between the quaternary ammonium groups and the target anion, thereby increasing the resin's adsorption capacity for the target anion and achieving efficient removal of the target anion. Specifically, as shown in Figure 1, this invention provides a method for preparing a magnetic ion exchange resin, which includes:

[0036] Step 1: Glycidyl methacrylate, divinylbenzene, magnetic materials, and photoinitiators undergo a polymerization reaction under the initiation of a light source to obtain magnetic microspheres.

[0037] Polyvinyl alcohol, sodium chloride, and gelatin were used as the aqueous phase, while glycidyl methacrylate, divinylbenzene, magnetic materials, dodecanol, cyclohexanol, and a photoinitiator were used as the oil phase. The aqueous and oil phases were mixed and stirred, then irradiated with ultraviolet light. At room temperature, the photoinitiator absorbed light energy and decomposed to generate free radicals. These free radicals rapidly initiated the opening of the carbon-carbon double bonds in the glycidyl methacrylate monomer, leading to a chain polymerization reaction and the formation of polymer chains. During the polymerization process, the ends of the polymer chains typically carried free radicals, giving them the ability to continue reacting. At this point, one double bond of the divinylbenzene reacted with the polymer chain carrying the free radicals, while the other double bond could further react with other polymer chains or divinylbenzene molecules, thereby linking different polymer chains together to achieve a cross-linking reaction and forming a three-dimensional network structure. This three-dimensional network structure encapsulated the magnetic material, ultimately yielding magnetic microspheres. After the reaction, the magnetic microspheres were separated, washed three times alternately with ultrapure water and anhydrous ethanol, and then dried in a drying oven.

[0038] It is worth noting that since the free radicals generated by the photoinitiator react with oxygen, the above polymerization and crosslinking reactions must be carried out in an inert environment.

[0039] Dodecanol acts as a dispersant, helping to improve the dispersibility of materials in resins and ensuring that various materials are evenly distributed within the resin.

[0040] Cyclohexanol, acting as a pore-forming agent, is partially or completely removed after washing, forming a porous structure inside the magnetic microspheres, increasing their porosity, and thus improving the adsorption performance of the resin.

[0041] In some embodiments, the light source includes any one of ultraviolet light, visible light, and near-infrared light. In this embodiment, ultraviolet light is used as the light source, and the conditions for ultraviolet light initiation are: power 10W-50W, wavelength 200nm-300nm. Compared with traditional thermal initiation, low-power ultraviolet light initiation not only greatly improves the speed and efficiency of monomer to polymer conversion, but also enables rapid initiation of the reaction at room temperature. More molecules and active sites fully participate in the crosslinking reaction in a short time. Active sites have more opportunities to react with molecules in different directions and positions, and will not remain in a certain local area for a long time. This avoids differences in crosslinking density in local areas, reduces the situation of excessive or insufficient crosslinking in local areas, and makes the spatial distribution of crosslinking points more random and uniform, which is conducive to the formation of a uniform three-dimensional network structure. This is beneficial to the diffusion of target anions inside the resin and increases the adsorption capacity.

[0042] In some embodiments, the mass ratio of glycidyl methacrylate to divinylbenzene is (4.5-10):1, and the mass ratio of glycidyl methacrylate to magnetic material is (8-10):1.

[0043] In some embodiments, the photoinitiator comprises any one of 2-hydroxy-2-methylphenylacetone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, camphorquinone, and indocyanine green-triethylamine complex.

[0044] In some embodiments, the magnetic material comprises either ferric oxide or magnetite.

[0045] When ferric oxide (Fe₂O₃) is selected as the magnetic material, it needs to be modified with oleic acid. Oleic acid is a fatty acid with long-chain alkyl groups. The long-chain alkyl portion of the oleic acid molecule can bind to the surface of ferric oxide through hydrophobic interactions, reducing its surface energy and making it more hydrophobic, thereby improving the dispersibility of ferric oxide in organic solvents. Through coordination and adsorption with the ferrite surface, a stable surface structure is formed, thereby increasing the stability of ferric oxide under different environmental conditions (especially humid environments). At the same time, the unsaturated double bonds of oleic acid and the acrylic groups in glyceryl methacrylate undergo chemical bonding through free radical polymerization, thus effectively coating ferric oxide. The specific modification steps are as follows: a certain amount of ferric oxide, ammonia, oleic acid, and acetone are added to ultrapure water and stirred in a water bath. A brown dispersion is obtained by magnetic separation and washed with ultrapure water until the pH value is neutral. After washing, it is placed in a drying oven for drying. The modified ferric oxide is labeled as OA, and the magnetic microspheres prepared with OA are labeled as MOA.

[0046] When magnetite (Fe3O4) is selected as the magnetic material, it needs to be modified with a silane coupling agent. On one hand, the silicon-containing end of the silane coupling agent can react with the surface of inorganic materials, while the organic-containing end can react with other organic materials, thereby improving the dispersibility of magnetite, enhancing its compatibility with organic materials, and strengthening interfacial adhesion. On the other hand, the silane groups of the silane coupling agent react chemically with the surface of magnetite to form silicon-oxygen metal bonds, thus fixing the silane coupling agent to the surface of magnetite. Furthermore, the acrylic groups of the silane coupling agent can participate in the polymerization reaction of glyceryl methacrylate monomers or divinylbenzene, forming a three-dimensional network structure, thus effectively coating magnetite. The specific modification steps are the same as those for OA preparation, except that the silane coupling agent must be hydrolyzed before modification. The hydrolysis step is as follows: a certain amount of deionized water and anhydrous ethanol are mixed, the pH of the solution is adjusted to between 8.0 and 10.0 with ammonia water, and then the silane coupling agent is added to the solution for hydrolysis. Through hydrolysis, the silicon-ethoxy bonds in the silane coupling agent break, forming chemically reactive silanol groups. These silanol groups can covalently bond with hydroxyl groups or other surface functional groups on the inorganic material surface, enhancing the bonding force between the silane coupling agent and the inorganic material, thereby improving interfacial bonding strength and the mechanical properties and stability of the resin. Modified iron oxide (Fe3O4) is labeled MPS, and magnetic microspheres prepared using MPS are labeled MMPS.

[0047] Step 2: Add an ammoniation reagent to the magnetic microspheres to induce an ammoniation reaction, thereby obtaining ammoniation-treated magnetic microspheres.

[0048] After the magnetic microspheres were prepared, an ammoniation reagent was added to them, and an ammoniation reaction was carried out in a water bath. The ammoniation reagent is nucleophilic, and its nitrogen atom uses its lone pair electrons to attack the epoxy group in glycidyl methacrylate, causing a ring-opening reaction, thereby obtaining ammoniation magnetic microspheres with a tertiary amine structure. After the reaction, the ammoniation magnetic microspheres were separated, washed with ultrapure water until the pH was neutral, and then dried in a drying oven.

[0049] In some embodiments, the amination agent comprises either trimethylamine hydrochloride or trimethylamine hydroxide.

[0050] Step 3: An alkylating agent is added to the ammoniated magnetic microspheres to undergo a nucleophilic substitution reaction, thereby obtaining a magnetic ion exchange resin; the alkylating agent is any one of 1-iodohexane, 1-chlorohexane, and 1-bromohexane.

[0051] Aminated magnetic microspheres are dissolved in anhydrous ethanol. An alkylating agent is added to the solution and stirred in a water bath to induce a nucleophilic substitution reaction. The tertiary amine structure in the aminated magnetic microspheres is nucleophilic. Its nitrogen atom uses its lone pair electrons to attack the carbon atom of the alkylating agent (such as 1-iodohexane) that is bonded to iodine. The iodide ion leaves, and the nitrogen atom becomes positively charged and forms a quaternary ammonium group, thus obtaining a magnetic ion exchange resin. The magnetic ion exchange resin is a core-shell structure in which aminated magnetic microspheres are coated with magnetic material. The degree of quaternization of the magnetic ion exchange resin is 65%-75%, and the mass ratio of aminated magnetic microspheres to magnetic material is (15-25):1. Alkylating agents extend the carbon chain length of the quaternary ammonium group in the resin to the hexyl group. On the one hand, the extended carbon chain increases the spacing between the quaternary ammonium groups, overcoming the steric hindrance problem of the quaternary ammonium groups, which is conducive to more target anions entering the resin and being adsorbed. On the other hand, the extended carbon chain increases the contact area between the quaternary ammonium groups and the target anions, which can efficiently adsorb more target anions and increase the adsorption capacity, thereby achieving efficient removal of target anions.

[0052] In some embodiments, the addition of a catalyst to the solution is also included to promote the nucleophilic substitution reaction. The catalyst comprises any one of ferric chloride, aluminum chloride, and titanium tetrachloride.

[0053] Following step 3, the process further includes rinsing the obtained magnetic ion exchange resin with a sodium chloride solution to remove soluble impurities, and then drying it in a vacuum drying oven. Magnetic ion exchange resin coated with OA is labeled MGD-OA, and magnetic ion exchange resin coated with MPS is labeled MGD-MPS. Example 1

[0054] (1) Preparation of modified ferric oxide (OA): 5 g of ferric oxide, 50 mL of ammonia, 5 mL of oleic acid and 25 mL of acetone were added to an Erlenmeyer flask containing 400 mL of ultrapure water. The solution was mechanically stirred in a water bath at 353 K for 30 min. A brown dispersion was obtained by magnetic separation and washed with ultrapure water until the pH value was neutral. After washing, the solution was placed in a drying oven at 333 K for 12 h.

[0055] (2) Preparation of Magnetic Microspheres (MOA) from OA: 0.1 g polyvinyl alcohol, 10 g sodium chloride, and 1 g gelatin were added to a flask containing 200 mL of ultrapure water as the aqueous phase. 45 g glycidyl methacrylate, 5 g divinylbenzene, 5 g OA, 5 g dodecanol, 45 g cyclohexanol, and 0.5 g 2-hydroxy-2-methylphenylacetone were added to a beaker as the oil phase. The oil and aqueous phases were mixed and stirred at 500 rpm. Polymerization was carried out under nitrogen atmosphere and irradiated with 48 W, 254 nm ultraviolet light for 2 h. After the reaction, the magnetic microspheres were separated, washed three times alternately with ultrapure water and anhydrous ethanol, and then dried in a 323 K drying oven for 12 h.

[0056] (3) Preparation of OA-coated magnetic ion exchange resin (MGD-OA): 20g MOA and 20g trimethylamine hydrochloride were added to a flask containing 100mL ultrapure water and subjected to ammoniation in a 353K water bath for 12h. After the reaction, the ammonified magnetic microspheres were separated, washed with ultrapure water until the pH was neutral, and dried in a 323K drying oven for 12h. Subsequently, 80mL of anhydrous ethanol and 20mL of ammonified magnetic microspheres were added to a three-necked round-bottom flask, followed by 50mL of 1-iodohexane and 0.5g of ferric chloride. The mixture was stirred at 300rpm for 8h in a 353K water bath to obtain the magnetic ion exchange resin. Finally, the resin was rinsed with 10% sodium chloride solution and dried to constant weight in a vacuum drying oven at 80℃.

[0057] The structure of MGD-OA is shown in Figure 2a; the adsorption kinetics of MGD-OA is shown in Figure 3a; the isothermal equilibrium diagram of MGD-OA is shown in Figure 4a; the effect of exogenous ions on the adsorption of phosphate ions by MGD-OA is shown in Figure 5a; the effect of natural organic matter on the adsorption of phosphate ions by MGD-OA is shown in Figure 5b; the Fourier transform infrared spectrum of MGD-OA is shown in Figure 6a; and the X-ray diffraction of MGD-OA before and after the adsorption of phosphate ions is shown in Figure 7. Example 2

[0058] (1) Preparation of modified magnetite (MPS): 50 mL of deionized water and 100 mL of anhydrous ethanol were added to a beaker. The pH of the solution was adjusted to between 8.0 and 10.0 with ammonia. 1 mL of silane coupling agent (KH570) was added to the solution for hydrolysis for 30 min. Then, 300 mL of deionized water, 5 g of magnetite, 50 mL of ammonia and 25 mL of acetone were added. The solution was mechanically stirred in a water bath at 353 K for 30 min. The black dispersion was obtained by magnetic separation and washed with ultrapure water until the pH was neutral. After washing, the solution was dried in a drying oven at 333 K for 12 h.

[0059] (2) Preparation of magnetic microspheres (MMPS) with MPS: 0.1 g polyvinyl alcohol, 10 g sodium chloride, and 1 g gelatin were added to a flask containing 200 mL of ultrapure water as the aqueous phase. 45 g glycidyl methacrylate, 5 g divinylbenzene, 5 g MPS, 5 g dodecanol, 45 g cyclohexanol, and 0.5 g 2-hydroxy-2-methylphenylacetone were added to a beaker as the oil phase. The oil and aqueous phases were mixed and stirred at 500 rpm. Polymerization was carried out under nitrogen atmosphere and irradiated with 48 W, 254 nm ultraviolet light for 2 h. After the reaction, the magnetic microspheres were separated, washed three times alternately with ultrapure water and anhydrous ethanol, and then dried in a 323 K drying oven for 12 h.

[0060] (3) Preparation of MPS-coated magnetic ion exchange resin (MGD-MPS): 20 g MMPS and 20 g trimethylamine hydrochloride were added to a flask containing 100 mL of ultrapure water and subjected to ammoniation in a 353 K water bath for 12 h. After the reaction, the ammonified magnetic microspheres were separated, washed with ultrapure water until the pH was neutral, and dried in a 323 K drying oven for 12 h. Subsequently, 80 mL of anhydrous ethanol and 20 mL of ammonified magnetic microspheres were added to a three-necked round-bottom flask, followed by 50 mL of 1-iodohexane and 0.5 g of ferric chloride. The mixture was stirred at 300 rpm for 8 h in a 353 K water bath to obtain the magnetic ion exchange resin. Finally, the resin was rinsed with 10% sodium chloride solution and dried to constant weight in a vacuum drying oven at 80 °C.

[0061] The structure of MGD-MPS is shown in Figure 2b; the adsorption kinetics of MGD-MPS is shown in Figure 3b; the isothermal equilibrium diagram of MGD-MPS is shown in Figure 4b; the effect of exogenous ions on the adsorption of phosphate ions by MGD-MPS is shown in Figure 5a; the effect of natural organic matter on the adsorption of phosphate ions by MGD-MPS is shown in Figure 5b; the Fourier transform infrared spectrum of MGD-MPS is shown in Figure 6b; and the X-ray diffraction of MGD-MPS before and after the adsorption of phosphate ions is shown in Figure 7.

[0062] As shown in Figure 2, both MGD-OA and MGD-MPS have spherical structures, with ammonium-modified magnetic microspheres as the outer shell and magnetic material as the core (not shown in the figure).

[0063] To further investigate the adsorption of phosphate ions by the resin, the adsorption kinetics of MGD-OA prepared in Example 1 and MGD-MPS prepared in Example 2 were fitted, as shown in Figures 3a and 3b. MGD-OA or MGD-MPS at concentrations of 5 mg / L, 10 mg / L, and 20 mg / L were added to the wastewater. With increasing adsorption time, the higher the concentration of MGD-OA or MGD-MPS, the greater the adsorption capacity. This is because more quaternary ammonium groups facilitate the chemical adsorption and binding of more phosphate ions through electrostatic attraction. During the entire adsorption process, the adsorption rate was high in the first 40 minutes and low after 40 minutes, indicating that the adsorption was not merely monolayer adsorption. Monolayer adsorption is achieved through van der Waals forces or hydrogen bonds, where each adsorption site adsorbs only one molecule, and there is no interaction between the adsorbed molecules; the longer the adsorption time, the greater the adsorption rate. However, in this example, the longer the adsorption time, the lower the adsorption rate, indicating that multilayer adsorption or other more complex adsorption processes may exist.

[0064] As shown in Figures 4a and 4b, the adsorption capacity increases with increasing concentration of MGD-OA or MGD-MPS and lower wastewater temperature. When the concentration of MGD-OA or MGD-MPS is 40 mg / mL, a wastewater temperature between 15℃ and 35℃ is conducive to maintaining a high adsorption capacity. Furthermore, further research shows that the resin of this invention can still be used at a wastewater temperature of 5℃, with an adsorption capacity not significantly different from that at 15℃. During use, excessively low temperatures may lead to a decrease in the exchange reaction rate and resin damage; excessively high temperatures may lead to resin degradation and failure.

[0065] As shown in Figure 5a, exogenous ions HCO3- are added to MGD-OA or MGD-MPS solutions. - Afterwards, HCO3 - Hydrolysis produces OH - Raising the pH of the solution creates an alkaline environment where the target anion (phosphate ion) may more readily form precipitates with some metal ions, thus promoting phosphate ion removal. Adding exogenous ions (CO3) to the solution... 2- Later, due to CO3 2- Competition for adsorption sites on the resin surface significantly inhibits phosphate ion removal. The removal of phosphate by the resin primarily depends on Cl... - The ion exchange process, when phosphate ions and Cl- ions in the solution... - When present, Cl - It will undergo ion exchange with phosphate ions, causing the phosphate ions to be adsorbed or fixed by the resin, thus achieving the purpose of removing phosphate ions; however, when the Cl in the solution... -When the amount of [agent] is excessive, it can reverse the ion exchange process that is normally conducive to the removal of phosphate ions. That is, phosphate ions that were originally adsorbed by the resin may be replaced by Cl [agent]. - The exchanged ions are released back into the solution, hindering the removal of phosphate ions and leading to a reduced removal rate. Compared with other exogenous ions, SO42-... 2- The SO42- can compete for more adsorption sites on the resin surface, resulting in a significant reduction in the amount of phosphate ions adsorbed by the resin. 2- With a smaller ionic radius, it can more easily access adsorption sites on the resin surface; at the same time, its high charge density results in stronger interaction with the resin surface, enabling it to occupy adsorption sites more effectively; when SO4 2- After occupying the adsorption sites, phosphate ions are difficult to adsorb onto the resin surface, thus significantly inhibiting the adsorption process of phosphate ions. As shown in Figure 5b, as the concentration of hyaluronic acid gradually increases, the adsorption capacity of MGD-OA or MGD-MPS for phosphate ions remains basically unchanged, proving that natural organic matter has almost no effect on the adsorption of anionic pollutants by the resin.

[0066] As shown in Figure 6, the Fourier transform infrared spectra of the magnetic microspheres (MOA, MMPS) underwent significant changes after ammoniation and nucleophilic substitution reactions, proving the successful acquisition of magnetic ion exchange resins (MGD-OA, MGD-MPS). Taking MGD-MPS as an example, the ammoniation process resulted in a 1107.74 cm⁻¹... -1 A distinct secondary alcohol peak was observed at -COC (909.15 cm⁻¹). -1 The C=O bond almost disappeared, with the C=O bond appearing at 1728.87 cm⁻¹. -1 Shifted to 1724.64cm -1 This indicates that the amination reaction was successful. The nucleophilic substitution process produced an NH bond (1640.14 cm⁻¹). -1 CN key (1485.91cm) -1 The bending vibration of alkyl-CH2 (1388.73 cm⁻¹) -1 ) and -CH3 (2954.22cm -1 The fact that it bends at an asymmetric angle indicates that the nucleophilic substitution reaction was successful.

[0067] In addition, the absorption peak of the -OH stretching vibration in MGD-OA that adsorbs phosphate ions shifts to 3393.66 cm⁻¹. -1 The absorption peak of the -OH stretching vibration in MGD-MPS adsorbed with phosphate ions shifts to 3421.12 cm⁻¹. -1 This indicates a hydrogen bonding interaction between the phosphate ion and the -OH group; the CO stretching vibration peak in MGD-OA with adsorbed phosphate ions shifts to 1156.33 cm⁻¹. -1The CO stretching vibration peak in MGD-MPS adsorbed with phosphate ions shifts to 1150 cm⁻¹. -1 This indicates that there is a hydrophobic interaction between the resin and phosphate ions.

[0068] As shown in Figure 7, ferric oxide and magnetite did not undergo crystal changes before and after the adsorption of phosphate ions by MGD-OA or MGD-MPS, maintaining strong magnetic and chemical stability.

[0069] In summary, the method of this invention uses low-power UV initiation technology to prepare magnetic ion exchange resins. Compared with traditional thermal initiation, the polymerization rate of low-power UV initiation (reaction time 1h-3h) is significantly higher than that of thermal initiation (reaction time 5h-10h), greatly improving the speed and efficiency of monomer-to-polymer conversion. Furthermore, it can rapidly initiate the reaction at room temperature, allowing more molecules and active sites to participate in the crosslinking reaction. Active sites have more opportunities to react with molecules in different directions and positions, not being limited to local areas, thus reducing the possibility of excessive or insufficient local crosslinking and resulting in a more random and uniform spatial distribution of crosslinking points. This process facilitates the formation of a uniform three-dimensional network structure, which in turn promotes the diffusion of target anions within the resin and increases the adsorption capacity. Simultaneously, the alkylating agent extends the carbon chain length of the quaternary ammonium group in the resin to the hexyl group. On one hand, the extended carbon chain increases the spacing between the quaternary ammonium groups, overcoming the steric hindrance problem and allowing more target anions to enter the resin and be adsorbed. On the other hand, the extended carbon chain increases the contact area between the quaternary ammonium group and the target anion, enabling efficient adsorption of more target anions and increasing the adsorption capacity. This results in highly efficient removal of target anions and makes it well-suited for wastewater treatment.

[0070] Although the present invention has been described in detail through the preferred embodiments above, it should be understood that the above description should not be considered as a limitation of the present invention. Various modifications and substitutions to the present invention will be apparent to those skilled in the art after reading the above description. Therefore, the scope of protection of the present invention should be defined by the appended claims.

Claims

1. A method for preparing a magnetic ion exchange resin, characterized in that, The method includes: Step 1: Glycidyl methacrylate, divinylbenzene, magnetic materials and photoinitiator undergo a polymerization reaction under the initiation of a light source to obtain magnetic microspheres; Step 2: Add an ammoniation reagent to the magnetic microspheres to induce an ammoniation reaction, thereby obtaining ammoniation-treated magnetic microspheres; Step 3: An alkylating agent is added to the ammoniated magnetic microspheres to undergo a nucleophilic substitution reaction, thereby obtaining a magnetic ion exchange resin; the alkylating agent comprises any one of 1-iodohexane, 1-chlorohexane, and 1-bromohexane.

2. The method for preparing the magnetic ion exchange resin as described in claim 1, characterized in that, Before step 1, the method further includes: modifying the magnetic material.

3. The method for preparing the magnetic ion exchange resin as described in claim 1, characterized in that, In step 1, the light source includes any one of ultraviolet light, visible light, and near-infrared light.

4. The method for preparing the magnetic ion exchange resin as described in claim 1, characterized in that, In step 1, the mass ratio of glycidyl methacrylate to divinylbenzene is (4.5-10):1, and the mass ratio of glycidyl methacrylate to magnetic material is (8-10):

1.

5. The method for preparing the magnetic ion exchange resin according to claim 1, characterized in that, In step 1, the magnetic material includes either ferric oxide or magnetite.

6. The method for preparing the magnetic ion exchange resin according to claim 1, characterized in that, In step 1, the photoinitiator comprises any one of 2-hydroxy-2-methylphenylacetone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, camphorquinone, and indocyanine green-triethylamine complex.

7. The method for preparing the magnetic ion exchange resin according to claim 1, characterized in that, In step 2, the amination reagent includes either trimethylamine hydrochloride or trimethylamine hydroxide.

8. The method for preparing the magnetic ion exchange resin according to claim 1, characterized in that, Step 3 also includes adding a catalyst, which includes any one of ferric chloride, aluminum chloride, and titanium tetrachloride.

9. A magnetic ion exchange resin obtained by the preparation method according to any one of claims 1-8, characterized in that, The magnetic ion exchange resin has a core-shell structure in which the ammoniated magnetic microspheres are coated with magnetic material; the degree of quaternization of the magnetic ion exchange resin is 65%-75%, and the mass ratio of the ammoniated magnetic microspheres to the magnetic material is (15-25):

1.

10. The use of a magnetic ion exchange resin obtained by the preparation method according to any one of claims 1-8, characterized in that, The magnetic ion exchange resin is used for wastewater treatment, and the temperature of the wastewater in the wastewater treatment process is 5℃-35℃.