Cement composition for periodontal fixation
By using a specific ratio of polymerizable monomer compositions and photopolymerization technology, the problems of complicated operation and uneven toughness in fixing loose teeth have been solved. A soft cement that can be quickly cured and adapt to changes in tooth spacing has been achieved, avoiding the influence of saliva contamination.
Patent Information
- Application Number
- PCT/CN2026/092710
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-24
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for fixing loose teeth are complicated to operate, have an uneven balance of softness and toughness, cannot easily adapt to changes in tooth spacing, and are easily affected by saliva contamination, leading to bonding failure.
A polymerizable monomer composition in a specific ratio, including methacryloyl or acryloyl dipolymer functional group monomers, acid-containing group monomers, photopolymerization initiators and polymerization inhibitors, is used to achieve rapid curing through photopolymerization, forming a soft and tough adhesive.
It enables easy fixation of loose teeth, can cure in a short time to obtain the necessary bond strength, adapts to changes in tooth spacing during biting, and avoids bond failure caused by saliva contamination.
Smart Images

Figure PCTCN2026092710-FTAPPB-I100001 
Figure PCTCN2026092710-FTAPPB-I100002 
Figure PCTCN2026092710-FTAPPB-I100003
Abstract
Description
A cement composition for periodontal fixation Technical Field
[0001] This invention relates to periodontal fixation techniques, and in particular to a cement composition for periodontal fixation that can easily and directly fix loose teeth. Background Technology
[0002] With the increasing elderly population, the demand for stabilizing loose teeth is also constantly growing. Current methods for stabilizing loose teeth include wire ligation, lingual periodontal banding, and direct fixation with adhesive resin. Wire ligation is less commonly used due to its potential damage to the tooth structure and aesthetic concerns. While lingual periodontal banding avoids these issues, the placement of the periodontal band and the resin used to fix it on the lingual side can cause a foreign body sensation and discomfort in the patient's mouth. Direct fixation with adhesive resin uses a flexible polymethyl methacrylate (PMMA) cement to directly bond and fix the adjacent surfaces of the tooth, achieving a bond that can adapt to changes in the interdental spaces during chewing, thus stabilizing the loose tooth. However, because this cement consists of liquid monomers, polymer powder, and a liquid catalyst, its application is complex, and the curing process requires 5-6 minutes or more, during which saliva contamination or contact with the tooth can easily lead to bonding failure.
[0003] Existing technologies incorporate block elastomeric polymers into polymeric monomers to achieve compositions with a certain degree of flexibility suitable for fixing loose teeth. However, these compositions involve the dissolution of the block elastomeric polymer within the monomer phase, leading to difficulties in formulation, insufficient balance between flexibility and toughness, and a tendency for breakage and detachment during use. Other technologies involve incorporating cross-linked polymeric flexible fillers insoluble in polymeric monomers into high-elasticity, high-strength monomers to achieve cement compositions with a certain degree of flexibility suitable for fixing loose teeth. Since these compositions are essentially heterogeneous, dispersing flexible fillers within high-elasticity, high-strength monomers, the cured cement still exhibits a high flexural modulus (>1 GPa), requiring significant force to induce deformation. This hinders the cement's ability to properly adapt to changes in inter-tooth spacing during chewing, failing to meet clinical requirements. Therefore, existing technologies for fixing loose teeth do not yet meet the requirements in terms of ease of use and performance. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide a cement composition for periodontal fixation, which addresses the above-mentioned deficiencies of the prior art.
[0005] To achieve the above objectives, the present invention provides a cement composition for periodontal fixation, comprising a polymerizable monomer composition and a photopolymerization initiator. The polymerizable monomer composition comprises 35 to 95 parts by weight of a first component, wherein the first component is a methacryloyl or acryloyl dipolymerizable monomer with a unit volume polymerizable functional group density between 1 and 4. The polymerizable functional group density of the monomer is calculated as follows: Monomer polymerizable functional group concentration = k × D × 1000 / M;
[0006] Wherein, the concentration of polymeric functional groups of monomer is in millimoles per milliliter, k is the number of polymeric functional groups in one monomer molecule, D is the density of polymeric monomer in grams per milliliter, and M is the molar mass of polymeric monomer in grams per mole.
[0007] The above-mentioned cementitious composition for periodontal fixation further includes 1 to 10 parts by weight of a second component, wherein the second component is a polymeric monomer containing an acidic group.
[0008] In the above-mentioned cement composition for periodontal fixation, the acidic group of the second component is selected from at least one of a carboxyl group, a carboxylic anhydride group, a phosphate group, or a sulfonic acid group.
[0009] The above-mentioned cementitious composition for periodontal fixation, wherein the second component is selected from (meth)acrylic acid and its anhydride, 1,4-di(meth)acryloyloxyethylpyromellitic acid, 6-(meth)acryloyloxyethylnaphthalene 1,2,6-tricarboxylic acid, N-(meth)acryloyl-p-aminobenzoic acid, N-(meth)acryloyl-o-aminobenzoic acid, N-(meth)acryloyl-m-aminobenzoic acid, N-(meth)acryloyl-5-aminosalicylic acid, N-(meth)acryloyl-4-aminosalicylic acid, 4-(meth)acryloyloxyethyl trimellitic acid and its anhydride, 4-(meth)acryloyloxybutyl trimellitic acid and its anhydride, 4-(meth)acryloyloxyhexyl trimellitic acid and its anhydride, 4-(meth)acryloyloxydecyl trimellitic acid and its anhydride, 2-(meth)acrylic acid, ethyl ... At least one of the following: 3-(meth)acryloyloxybenzoic acid, 4-(meth)acryloyloxybenzoic acid, β-(meth)acryloyloxyethyl succinate, β-(meth)acryloyloxyethyl maleate, β-(meth)acryloyloxyethyl phthalate, 11-(meth)acryloyloxy-1,1-undecanedicarboxylic acid, p-vinylbenzoic acid, (2-(meth)acryloyloxyethyl)phosphate, (2-(meth)acryloyloxyethylphenyl)phosphate, 10-(meth)acryloyloxydecyl phosphate, 10-methacryloyloxydecyl phosphate, 11-(meth)acryloyloxyundecyl phosphate, 11-methacryloyloxyundecyl phosphate, p-styrenesulfonic acid, and 2-acrylamido-2-methylpropanesulfonic acid.
[0010] The above-mentioned cement composition for periodontal fixation, wherein the first component is selected from at least one of ethoxylated bisphenol A di(meth)acrylate with 8-20 ethoxy groups and polyurethane di(meth)acrylate with 4-8 intramolecular carbamoyl groups.
[0011] In the above-mentioned cement composition for periodontal fixation, the number of polymeric functional groups k in one monomer molecule is 2.
[0012] The above-mentioned cement composition for periodontal fixation, wherein the polymeric monomer composition further includes a third component, the third component being a monofunctional polymeric monomer and / or a polyfunctional polymeric monomer, the content of the third component being 0-60 parts by weight, and the total amount of the first component, the second component and the third component being 100 parts by weight.
[0013] The aforementioned cement composition for periodontal fixation further includes a photopolymerization initiator accelerator, wherein the photopolymerization initiator accelerator is 0.5-3 times the weight of the photopolymerization initiator; and the content of the photopolymerization initiator and the photopolymerization initiator accelerator is 0.1 to 5 parts by weight of the total weight.
[0014] The aforementioned cement composition for periodontal fixation further includes a polymerization inhibitor, wherein the amount of the polymerization inhibitor added is 50 to 20,000 ppm relative to the polymerizable monomer composition.
[0015] The aforementioned cement composition for periodontal fixation further includes water, wherein the amount of water added is 0 to 5 parts by weight relative to the polymeric monomer composition.
[0016] The aforementioned cement composition for periodontal fixation further includes a thickener, wherein the thickener is at least one of silica, titanium dioxide, or alumina inorganic micropowder with a particle size of 0.002-0.05 micrometers obtained by gas-phase method.
[0017] The technical advantages of this invention are as follows:
[0018] The adhesive composition of this invention exhibits good flexibility and toughness after curing, and can achieve the necessary bond strength in a short time. It can easily bond and fix loose teeth, appropriately follow the changes in the gap between teeth during occlusion, and avoids the bonding failure caused by saliva contamination or contact with teeth during the curing process of room temperature curing adhesive compositions.
[0019] The present invention will be described in detail below with reference to specific embodiments and comparative examples, but this is not intended to limit the present invention. Detailed Implementation
[0020] The structural and working principles of this invention are described in detail below:
[0021] The present invention relates to a cement composition for periodontal fixation, comprising a polymerizable monomer composition (A) and a photopolymerization initiator (B). The polymerizable monomer composition (A) comprises 35 to 95 parts by weight of a first component (a1), wherein the first component is a methacryloyl or acryloyl dipolymerizable monomer with a unit volume polymerizable functional group density between 1 and 4. The polymerizable functional group density of the monomer is calculated as follows: Monomer polymerizable functional group concentration = k × D × 1000 / M;
[0022] Wherein, the concentration of polymeric functional groups of monomer is in millimoles per milliliter, k is the number of polymeric functional groups in one monomer molecule, D is the density of polymeric monomer in grams per milliliter, and M is the molar mass of polymeric monomer in grams per mole.
[0023] Preferably, the number of polymerizable functional groups k in a monomer molecule is 2. The first component (a1) of the polymerizable monomer (A) is selected from at least one of polyethoxylated (n+m=8-20) bisphenol A di(meth)acrylate and polyurethane di(meth)acrylate with 4-8 intramolecular carbamoyl groups.
[0024] The density of polymeric functional groups in the first component (a1) of this invention is particularly important for the performance of the adhesive composition. When the polymeric functional group density of the monomer is higher than 4 mmol / mL, the cross-linking density of the adhesive composition is too high during photopolymerization, resulting in a brittle and hard adhesive after curing (flexural modulus > 1 GPa), which cannot achieve the required flexibility. A large external force is required for the adhesive to undergo a certain deformation, which is not conducive to the adhesive properly following the changes in interdental space during chewing in clinical use. When the polymeric functional group density of the monomer is lower than 1 mmol / mL, the cross-linking density of the adhesive composition is too low during photopolymerization, and the adhesive after curing cannot achieve the required strength.
[0025] The first component (a1) is a methacryloyl or acryloyl dipolymerizable monomer with a unit volume polymerizable functional group density between 1 and 4, and may be an alicyclic or aromatic di(meth)acrylate as shown in the following formula:
[0026] Where R is a hydrogen atom or a methyl group, m and n may be the same or different, and are numbers from 4 to 10. 1 for
[0027] And di(meth)acrylates of polyurethanes having 4-10 carbamoyl groups in the molecules shown below:
[0028] Where R is a hydrogen atom or a methyl group, and n is a number from 1 to 4, R 2 R is a straight-chain alkylene group having 2 to 4 carbon atoms. 1 for:
[0029] The following compounds are particularly preferred:
[0030] The following compound is shown in the formula:
[0031] Where R is a hydrogen atom or a methyl group, and n is a number from 1 to 3, R 2 R is a straight-chain alkylene group with 3 carbon atoms. 1 for:
[0032] These methacryloyl or acryloyl dimerizable monomers with a unit volume polymerizable functional group density between 1 and 4 can be used alone or in combination of two or more.
[0033] The amount of the first component (a1) containing a dimeric functional group of methacryloyl or acryloyl with a unit volume polymeric functional group density between 1 and 4 is preferably 35 to 95 parts by weight, more preferably 40 to 90 parts by weight, and particularly preferably 50 to 80 parts by weight, relative to 100 parts by weight of the polymeric monomer composition (including the first component a1, the second component a2, and the third component a3, which contains other monofunctional and difunctional polymeric monomers). When the amount is less than 35 parts by weight, the cured composition does not achieve the required flexibility.
[0034] In some embodiments of the present invention, the polymerizable monomer composition further includes 1 to 10 parts by weight of a second component (a2), the second component being a polymerizable monomer containing an acidic group. The acidic group of the second component (a2) is selected from at least one of a carboxyl group, a carboxylic anhydride group, a phosphate group, or a sulfonic acid group. The second component is selected from (meth)acrylic acid and its anhydride, 1,4-di(meth)acryloyloxyethylpyromellitic acid, 6-(meth)acryloyloxyethylnaphthalene 1,2,6-tricarboxylic acid, N-(meth)acryloyl-p-aminobenzoic acid, N-(meth)acryloyl-o-aminobenzoic acid, N-(meth)acryloyl-m-aminobenzoic acid, N-(meth)acryloyl-5-aminosalicylic acid, N-(meth)acryloyl-4-aminosalicylic acid, 4-(meth)acryloyloxyethyl trimellitic acid and its anhydride, 4-(meth)acryloyloxybutyl trimellitic acid and its anhydride, 4-(meth)acryloyloxyhexyl trimellitic acid and its anhydride, 4-(meth)acryloyloxydecyl trimellitic acid and its anhydride, 2-(meth)acryloyloxybenzoic acid, 3-(meth)acryloyloxybenzoic acid Formic acid, 4-(meth)acryloyloxybenzoic acid, β-(meth)acryloyloxyethyl succinate, β-(meth)acryloyloxyethyl maleate, β-(meth)acryloyloxyethyl phthalate, 11-(meth)acryloyloxy-1,1-undecanedicarboxylic acid, p-vinylbenzoic acid, etc., monomers having a carboxylic acid group or its anhydride group; (2-(meth)acryloyloxyethyl)phosphoric acid, (2-(meth)acryloyloxyethylphenyl)phosphoric acid, 10-(meth)acryloyloxydecyl phosphoric acid, 10-methacryloyloxydecyl phosphate, 11-(meth)acryloyloxyundecyl phosphoric acid, 11-methacryloyloxyundecyl phosphate, etc., monomers having a phosphate group; p-styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, etc., monomers having a sulfonic acid group, etc., at least one of them. The second component (a2) is preferably 4-methacryloyloxyethyl trimellitic acid / 4-methacryloyloxyethyl trimellitic anhydride, or 10-methacryloyloxydecyl phosphate and / or di-10-methacryloyloxydecyl phosphate, 11-(meth)acryloyloxyundecyl phosphate and / or di-11-methacryloyloxyundecyl phosphate. These acidic monomers can be used alone or in combination.
[0035] The amount of the second component (a2) is preferably 1-10 parts by weight, more preferably 2-8 parts by weight, relative to a total of 100 parts by weight of the polymerizable monomer compositions a1, a2, and the other monofunctional and difunctional polymerizable monomers a3 described later.
[0036] In some embodiments of the present invention, without affecting the performance of the composition of the present invention, the polymerizable monomer composition may further include a third component (a3), wherein the third component is a monofunctional polymerizable monomer and / or a polyfunctional polymerizable monomer, the content of the third component is 0-60 parts by weight, and the total amount of the first component, the second component and the third component is 100 parts by weight.
[0037] Among them, the monofunctional (meth)acrylate monomer can be selected from methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, lauryl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, isobornyl methacrylate, and other alkyl methacrylates; 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 5-hydroxypentyl methacrylate, 6-hydroxyhexyl methacrylate, glyceryl methacrylate, erythritol mono(meth)acrylate, and other hydroxyalkyl methacrylates; diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, etc. Polyethylene glycol mono(meth)acrylates, such as acrylates, polyethylene glycol mono(meth)acrylates, and polydipropylene glycol mono(meth)acrylates; (poly)diol monoalkyl ether (meth)acrylates, such as ethylene glycol monomethyl ether (meth)acrylates, ethylene glycol monoethyl ether (meth)acrylates, diethylene glycol monomethyl ether (meth)acrylates, triethylene glycol monomethyl ether (meth)acrylates, polyethylene glycol monomethyl ether (meth)acrylates, and polypropylene glycol monoalkyl ether (meth)acrylates; fluoroalkyl esters of (meth)acrylates, such as perfluorooctyl (meth)acrylates and hexafluorobutyl (meth)acrylates; silane compounds containing (meth)acryloyloxyalkyl groups, such as γ-(meth)acryloyloxypropyltrimethoxysilane and γ-(meth)acryloyloxypropyltris(trimethylsiloxy)silane; and (meth)acrylates containing heterocyclic groups, such as tetrafurfuryl (meth)acrylates.
[0038] The multifunctional (meth)acrylate monomers may be selected from ethylene glycol dimethacrylate, propylene glycol dimethacrylate, butanediol dimethacrylate, neopentyl alcohol dimethacrylate, hexanediol dimethacrylate, heptaethylene glycol dimethacrylate, octyl glycol dimethacrylate, nonanediol dimethacrylate, 2-hydroxypropyl dimethacrylate; diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, dipropylene glycol dimethacrylate, polypropylene glycol dimethacrylate, and dibutylene glycol dimethacrylate;
[0039] Alicyclic or aromatic di(meth)acrylates of the following formula:
[0040] Where R is a hydrogen atom or a methyl group, m and n may be the same or different, and are numbers from 0 to 3, where R 1 for:
[0041] And difunctional (meth)acrylates with carbamoyl bonds in the molecules shown below;
[0042] Where R is a hydrogen atom or a methyl group, R 1 for:
[0043] Among them, alkyl methacrylates such as methyl methacrylate and ethyl methacrylate are particularly preferred as monofunctional methacrylates; hydroxyl-containing methacrylates such as 2-hydroxyethyl methacrylate, 1,3-dihydroxypropyl monomethacrylate, and erythritol monomethacrylate; and methacrylates with an intramolecular ethylene glycol chain such as triethylene glycol monomethyl ether methacrylate and triethylene glycol monomethacrylate.
[0044] As a multifunctional (meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and other di(meth)acrylates with an ethylene glycol chain in the molecule, as well as 2-hydroxypropyl di(meth)acrylate, are particularly preferred.
[0045] The following compound is shown in the formula:
[0046] The following compound is shown in the formula:
[0047] These polymeric monomers, the third component (a3), can be used alone or in combination of two or more.
[0048] The photopolymerization initiator of the present invention is not particularly limited to any photopolymerization initiator that generates free radicals by irradiation with light. The wavelength used during photopolymerization is generally 365 nm to 520 nm, practically preferably 370 nm to 520 nm, and more preferably 380 nm to 500 nm. The photopolymerization initiator that generates free radicals at the wavelength of light used during photopolymerization can be an α-diketone compound, an alkylbenzene compound, an acylphosphine oxide compound, adicenocene compound, an oxime ester compound, abenzenein compound, acetophenone compound, benzophenone compound, thioxanone compound, an α-acyloxime ester compound, abenzene ester compound, benzoyl carboxylate compound, azo compound, diphenyl sulfide compound, organic pigment compound, iron-phthalocyanine compound, abenzenein ether compound, anthraquinone compound, etc. Among these, alkylbenzene compounds and acylphosphine oxide compounds are preferred. As an α-diketone compound, it can be α-cyclohexanedione, d,l camphorquinone, camphorquinone-10-carboxylic acid, camphorquinone-10-carboxysulfonic acid, etc. As an alkylphenyl ketone compound, it can be 1-hydroxy-cyclohexyl-phenyl-ketone. As an acylphosphine oxide compound, it can be bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide. This embodiment may contain only one photopolymerization initiator, or it may contain two or more.
[0049] In some embodiments of the present invention, the adhesive composition may further include a photopolymerization initiator / accelerator as needed, wherein the photopolymerization initiator / accelerator is 0.5-3 times the weight of the photopolymerization initiator; the content of the photopolymerization initiator and the photopolymerization initiator / accelerator is 0.1 to 5 parts by weight of the total weight (100 parts by weight of polymerizable monomer (A) and photopolymerization initiator (B), more preferably 0.2 to 4.5 parts by weight, and particularly preferably 0.3 to 4 parts by weight). The polymerization accelerator may be an amine compound, a sulfinic acid compound, a barbiturate compound, an aldehyde compound, or a thiol compound. The amine compound may be p-tolyldimethylamine, p-tolyldiethylamine, p-tolyldiethanolamine, alkyl esters such as ethyl p-dimethylaminobenzoate, alkyl esters such as p-diethylaminobenzoic acid and methyl p-diethylaminobenzoate, N,N-dimethylaminoethyl methyl methacrylate, etc.
[0050] In other embodiments of the invention, the adhesive composition may also include a polymerization inhibitor as needed to increase storage stability. The amount of the polymerization inhibitor added is 50 to 20,000 ppm relative to the polymerizable monomer composition (A), more preferably 100 to 15,000 ppm, and particularly preferably 200 to 10,000 ppm. The polymerization inhibitor used may be hydroquinone, butylhydroquinone, or other hydroquinone compounds; hydroquinone monomethyl ether; phenols such as 2,6-di-tert-butylphenol and 2,6-di-tert-butyl-p-cresol; catechol; pyrogallol; benzoquinone; 2-hydroxybenzoquinone; p-methoxyphenol; tert-butylcatechol; butylated hydroxyanisole; butylated hydroxytoluene; or tert-butylhydroquinone. The polymerization inhibitor may be used alone or in combination of two or more. A mixture of hydroquinone monomethyl ether and 2,6-di-tert-butyl-p-cresol is preferred.
[0051] In some other embodiments of the invention, the adhesive composition may also include a small amount of water as needed, wherein the amount of water added is 0 to 5 parts by weight relative to the polymeric monomer composition (A), more preferably 0.2 to 4 parts by weight, and particularly preferably 0.3 to 3 parts by weight. There are no particular limitations on the water added to the composition of the invention; purified water or distilled water is preferred.
[0052] The adhesive composition of the present invention may also include a thickener as needed. The thickener may be selected from inorganic micropowders of silica, titanium dioxide, or alumina with a particle size of 0.002 to 0.05 micrometers obtained by gas-phase method. Silica micropowder with a particle size of 0.002 to 0.05 micrometers is preferred. These inorganic micropowders can be subjected to surface hydrophobic treatments such as silane treatment. These thickeners can be used alone or in combination. The amount of thickener used is preferably 0 to 30 parts by weight, more preferably 3 to 25 parts by weight, and particularly preferably 5 to 20 parts by weight, relative to 100 parts by weight of the total polymerizable monomer (A) and photopolymerization initiator (B).
[0053] The present invention will be further described in detail below based on embodiments, but the present invention is not limited to these embodiments.
[0054] The abbreviations used below refer to the following compounds:
[0055] P8UDA: Poly(8)urethane diacrylate (as shown in the following formula, where n=3, R is a hydrogen atom, R 2 R is a straight-chain alkylene group with 3 carbon atoms. 1 for: );
[0056] B8EODMA: 8-ethoxylated bisphenol A dimethacrylate (as shown in the formula below, where m+n=8, R is methyl);
[0057] B10EODMA: 10-ethoxylated bisphenol A dimethacrylate (as shown in the formula above, where m+n=10, R is methyl);
[0058] B17EODMA: 17-ethoxylated bisphenol A dimethacrylate (as shown in the formula above, where m+n=17, R is methyl);
[0059] 4-MET: 4-Methylacryloyloxyethyltriphenyltriacrylic acid;
[0060] 4-META: 4-Methylacryloyloxyethyltriphenyltrihydride;
[0061] MDP: 10-Methacryloxydecyl phosphate;
[0062] MUP: 11-Methacryloxyundecylphosphonic acid;
[0063] HEMA: 2-Hydroxyethyl methacrylate;
[0064] GCMA: Glyceryl methacrylate;
[0065] UDMA: Diurea dimethacrylate;
[0066] B2EODMA: 2-ethoxylated bisphenol A dimethacrylate (as shown in the formula below, where m+n=2, R is methyl);
[0067] TEGDMA: Triethylene glycol dimethyl methacrylate;
[0068] CQ: Camphorquinone;
[0069] DMABEE: Ethyl p-dimethylaminobenzoate;
[0070] TPO: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide;
[0071] MEHQ: Hydroquinone monomethyl ether;
[0072] BHT: 2,6-di-tert-butylphenol;
[0073] Silicon micropowder: Vapor phase nano-silicon powder.
[0074] Example 1
[0075] The adhesive composition was prepared according to the formulation of Example 1 in Table 1. The mechanical properties of the cured composition and the bond strength between the composition and tooth enamel were measured. The bipolymer functional group monomer (a1) P8UDA used had a molecular weight of 1300 and a density of 1.05 g / ml. The polymer functional group density was calculated as 1.62 mmol / ml using the formula: Monomer polymer functional group density = 2 × D × 1000 / M.
[0076] Mechanical properties of the cured composition:
[0077] Cured specimens (sample number: 3) for the 3-point bending test were prepared according to YY1042-2023 Dental Polymer-Based Restorative Materials 7.11. After immersing the specimens in water at 37°C for 24 hours, the 3-point bending test was performed at a crosshead speed of 1.0 mm / min. The bending modulus, the maximum bending deformation at specimen fracture, and the external force required for a 3 mm bending deformation were measured.
[0078] The results are shown in Table 1.
[0079] Bond strength between the component and tooth enamel:
[0080] Referring to YY / T 0519-2022 Dentistry and Testing of Bonding to Tooth Structures, the following tests were conducted on the bond strength immediately after bonding and the bond strength.
[0081] 1) While submerged in water, use coarse diamond sandpaper to grind the labial side of the bovine anterior teeth to expose a flat enamel surface. Then, use 600-grit diamond sandpaper to polish and form an adhesive surface. After drying the adhesive surface, treat it with a 35% (by weight) phosphoric acid etching solution for 10 seconds, rinse with water for 10 seconds, and air dry for 15 seconds. Then, apply 4mm diameter perforated cellophane tape to the adhesive surface to define the bonding area.
[0082] 2) Apply the composition to the bonding surface prepared in step 1), place an acrylic rod with a diameter of 6 mm and a length of 8 mm on it and press it down gently. Use a light irradiator to irradiate the composition between the bonding surface and the acrylic rod to cure it and make a sample for adhesion strength test; make 5 test samples.
[0083] 3) Place the sample for adhesion strength test at room temperature for 30 minutes, then immerse it in distilled water at 37°C for 24 hours. Measure the shear bond strength between the acrylic rod and the enamel, and take the average of the 5 test values.
[0084] As can be seen from the results of Example 1, the adhesive composition, consisting of a polymeric monomer (a1) with a suitable amount of polymeric functional groups at a density of 1.62 mmol / mL, a suitable amount of polymeric monomer (a2) containing acidic groups, and a photopolymerization initiator (B), exhibits a flexural modulus of 0.19 GPa after curing, does not break even after bending deformation greater than 8 mm, and requires an external force of 2.1 N for 3 mm bending deformation. It also demonstrates good flexibility and toughness (flexural modulus < 1 GPa; external force required for 3 mm bending deformation < 10 N) and good bond strength with tooth enamel (10.2 MPa).
[0085] Examples 2 and 3
[0086] The difference between Examples 2 and 3 and Example 1 is that the content of the first component a1 is different. See Table 1 for the specific proportions and results.
[0087] As can be seen from the results of Examples 2 and 3 in Table 1, the adhesive composition consisting of 50 parts by weight and 40 parts by weight of the first component (a1), an appropriate amount of polymerizable monomer with acidic groups (a2), and a photopolymerization initiator (B) gradually increases the flexural modulus after curing as the content of (a1) decreases, while still maintaining good softness and toughness. It also exhibits good bonding strength with tooth enamel.
[0088] Example 4
[0089] The difference between Example 4 and Example 1 is that the first component a1 is different. See Table 1 for the specific proportions and results.
[0090] The bipolymer functional group monomer (a1) B8EODMA used in Example 4 has a molecular weight of 716 and a density of 1.12 g / ml. The polymer functional group density is calculated to be 3.12 mmol / ml according to the formula.
[0091] As can be seen from the results of Example 4 in Table 1, the adhesive composition consisting of 70 parts by weight of polymeric functional group (a1) with a density of 3.12 mmol / mL, an appropriate amount of polymeric monomer containing acidic groups (a2), and a photopolymerization initiator (B) can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0092] Examples 5 and 6
[0093] The difference between Examples 5 and 6 and Example 1 is that the first component a1 is different. See Table 1 for the specific proportions and results.
[0094] The bipolymer functional group monomer (a1) B10EODMA used in Examples 5 and 6 has a molecular weight of 804 and a density of 1.12 g / ml. The polymer functional group density was calculated to be 2.79 mmol / ml according to the formula.
[0095] As can be seen from the results of Examples 5 and 6 in Table 1, the adhesive composition consisting of 70 parts by weight and 90 parts by weight of polymeric functional group density of 2.79 mmol / mL (a1), an appropriate amount of polymeric monomer containing acidic groups (a2), and polymerization initiator B can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0096] Example 7
[0097] The difference between Example 7 and Example 1 is that the first component a1 is different. See Table 1 for the specific proportions and results.
[0098] The bipolymer functional group monomer (a1) B17EODMA used in Example 7 has a molecular weight of 1113 and a density of 1.13 g / ml. The polymer functional group density is calculated to be 2.03 mmol / ml according to the formula.
[0099] As can be seen from the results of Example 7 in Table 1, the adhesive composition consisting of 70 parts by weight of polymeric functional group (a1) with a density of 2.03 mmol / mL, an appropriate amount of polymeric monomer containing acidic groups (a2), and a photopolymerization initiator (B) can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0100] Table 1. Examples 1-7
[0101] Example 8
[0102] The difference between Example 8 and Example 1 is that the first component a1 is different. The first component a1 consists of P8UDA with a polymeric functional group density of 1.62 mmol / mL and B10EODMA with a polymeric functional group density of 2.79 mmol / mL. The specific ratios and results are shown in Table 2.
[0103] As can be seen from the results of Example 8 in Table 2, the adhesive composition consisting of P8UDA with a polymeric functional group density of 1.62 mmol / mL and B10EODMA with a polymeric functional group density of 2.79 mmol / mL (a1), an appropriate amount of polymeric monomers containing acidic groups (a2), and a photopolymerization initiator (B) can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0104] Example 9
[0105] The difference between Example 9 and Example 1 is that the second component a2 is different, and a small amount of distilled water is added to the adhesive. See Table 2 for the specific proportions and results.
[0106] The a2 used in Example 9 is 4-methacryloyloxyethyl trimellitic anhydride.
[0107] As can be seen from the results of Example 9 in Table 2, the adhesive composition consisting of a polymeric monomer (a1) containing an appropriate amount of polymeric functional groups with a density of 1.62 mmol / mL of dipolymeric functional groups, an appropriate amount of polymeric monomer (a2) containing acidic groups, a photopolymerization initiator (B), and a small amount of distilled water can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0108] Examples 10, 11
[0109] The difference between Examples 10 and 11 and Example 1 is that the second component a2 is different. See Table 2 for the specific proportions and results.
[0110] In Examples 10 and 11, a2 was 11-methacryloyloxyundecyl phosphoric acid.
[0111] As can be seen from the results of Examples 10 and 11 in Table 2, the adhesive composition consisting of a polymeric monomer (a1) with a suitable amount of polymeric functional group density, a suitable amount of polymeric monomer (a2) containing acidic groups, and a photopolymerization initiator (B) can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0112] Example 12
[0113] The difference between Example 12 and Example 1 is that the photopolymerization initiator (B) is different. See Table 2 for the specific ratios and results.
[0114] The photopolymerization initiator (B) used in Example 12 was 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide.
[0115] As can be seen from the results of Example 12 in Table 2, the adhesive composition consisting of a polymerizable monomer (a1) with an appropriate amount of suitable polymerizable functional group density, an appropriate amount of polymerizable monomer (a2) containing acidic groups, and a photopolymerization initiator (B) (2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide) can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0116] Example 13
[0117] The difference between Example 13 and Example 1 is that the first component a1 is different. See Table 2 for the specific proportions and results.
[0118] In Example 13, a1 was B10EODMA with a polymer functional group density of 2.79 mmol / mL, and a2 was 10-methacryloyloxydecyl phosphate.
[0119] As can be seen from the results of Example 13 in Table 2, the adhesive composition consisting of a polymeric monomer (a1) containing an appropriate amount of polymeric functional group density with dipolymeric functional groups, an appropriate amount of polymeric monomer (a2) containing acidic groups, and a photopolymerization initiator (B) can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0120] Example 14
[0121] The difference between Example 14 and Example 1 is that the first component a1 is different, and the content of the second component a2 is different. See Table 2 for the specific proportions and results.
[0122] In Example 14, a1 was B10EODMA with a polymeric functional group density of 2.79 mmol / mL, and the content of the polymeric monomer a2 containing acidic groups was 5 parts by weight.
[0123] As can be seen from the results of Example 14 in Table 2, the adhesive composition consisting of a polymeric monomer (a1) with a suitable density of polymeric functional groups, a suitable amount of polymeric monomer (a2) containing acidic groups, and a photopolymerization initiator (B) can produce a cured product with good softness and toughness and good bonding strength with tooth enamel.
[0124] Table 2. Examples 8-14
[0125] Comparative Example 1
[0126] The difference between Comparative Example 1 and Example 1 is that the content of the first component a1 is different. See Table 3 for the specific proportions and results.
[0127] As can be seen from the results of Comparative Example 1 in Table 3, the adhesive composition consisting of a polymeric monomer (a1) with a dipolymeric functional group density of 1.62 mmol / mL (by weight), an appropriate amount of a polymeric monomer containing acidic groups (a2), and a photopolymerization initiator (B), exhibits a flexural modulus of 0.98 GPa after curing, a flexural deformation at fracture of 3.9 mm, and a required external force of 13.9 N for a 3 mm flexural deformation. It does not possess the softness and toughness required for periodontal fixation adhesives.
[0128] Compare Examples 2 and 3
[0129] The difference between Comparative Examples 2 and 3 and Example 1 lies in the different first component a1 and its content. See Table 3 for specific proportions and results.
[0130] Comparative Examples 2 and 3 used B10EODMA with a polymer functional group density of 2.79 mmol / mL and a content of 30 parts by weight.
[0131] As can be seen from the results of Comparative Examples 2 and 3 in Table 3, the adhesive composition consisting of 30 parts by weight of a polymerizable monomer (a1) of B10EODMA with a polymeric functional group density of 2.79 mmol / mL, an appropriate amount of a polymerizable monomer containing acidic groups (a2), and a photopolymerization initiator (B) does not have the softness and toughness required for periodontal fixation adhesives after curing (Comparative Example 2: flexural modulus of 1.11 GPa, flexural deformation at fracture of 3.9 mm, and the external force required for 3 mm flexural deformation is 14.8 N; Comparative Example 3: flexural modulus of 2.0 GPa, flexural deformation at fracture of 3.3 mm, and the external force required for 3 mm flexural deformation is 24.6 N).
[0132] Comparative Example 4
[0133] The difference between Comparative Example 4 and Example 1 is that UDMA with a polymeric functional group density greater than 4 mmol / mL was used to replace the first component a1. See Table 3 for the specific proportions and results.
[0134] Comparative Example 4 used UDMA with a molecular weight of 470 and a density of 1.11 g / ml. The polymer functional group density was calculated to be 4.72 mmol / ml according to the formula: Monomer polymer functional group density = 2 × D × 1000 / M.
[0135] As can be seen from the results of Comparative Example 4 in Table 3, the adhesive composition consisting of a polymerizable monomer with a polymeric functional group density greater than 4 mmol / mL by weight, an appropriate amount of a polymerizable monomer containing an acidic group (a2), and a photopolymerization initiator (B) exhibits greater rigidity after curing and does not possess the softness and toughness required for periodontal fixation adhesives (flexural modulus of 2.5 GPa and flexural deformation at fracture of 2.3 mm).
[0136] Comparative Example 5
[0137] The difference between Comparative Example 5 and Example 1 is that the composition does not contain component a2 of the first component. See Table 3 for specific proportions and results.
[0138] As can be seen from the results of Comparative Example 5 in Table 3, the adhesive composition consisting of a polymerizable monomer (a1) with an appropriate amount of suitable polymerizable functional group density and a photopolymerization initiator (B) can produce a cured product with good softness and toughness, but because it does not contain the acidic monomer a2, the bond strength with the enamel is relatively low.
[0139] Table 3. Comparative Examples 1-5
[0140] In summary, the cured periodontal fixation component of the present invention exhibits good flexibility and toughness, and can achieve the necessary bond strength in a short time. In clinical use, it can appropriately follow changes in the interdental gaps during occlusion and avoids bonding failure caused by saliva contamination or contact with teeth during the curing process, which is common with room temperature curing bonding components.
[0141] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the appended claims.
Claims
1. A cementitious composition for periodontal fixation, characterized in that, The mixture includes a polymerizable monomer composition and a photopolymerization initiator. The polymerizable monomer composition includes a first component, which is a dipolymerizable monomer with a unit volume polymerizable functional group density of methacryloyl or acryloyl groups between 1 and 4. The polymerizable functional group density of the monomer is calculated as follows: Monomer functional group concentration = k × D × 1000 / M; Wherein, the concentration of polymeric functional groups of monomer is in millimoles per milliliter, k is the number of polymeric functional groups in one monomer molecule, D is the density of polymeric monomer in grams per milliliter, and M is the molar mass of polymeric monomer in grams per mole.
2. The cement composition for periodontal fixation according to claim 1, characterized in that, The polymerizable monomer composition further includes a second component, which is a polymerizable monomer containing an acidic group; wherein the polymerizable monomer composition includes 35 to 95 parts by weight of the first component and 1 to 10 parts by weight of the second component.
3. The cement composition for periodontal fixation according to claim 2, characterized in that, The acidic group of the second component is selected from at least one of a carboxyl group, a carboxylic anhydride group, a phosphate group, or a sulfonic acid group.
4. The cement composition for periodontal fixation according to claim 3, characterized in that, The second component is selected from (meth)acrylic acid and its anhydride, 1,4-di(meth)acryloyloxyethylpyromellitic acid, 6-(meth)acryloyloxyethylnaphthalene 1,2,6-tricarboxylic acid, N-(meth)acryloyl-p-aminobenzoic acid, N-(meth)acryloyl-o-aminobenzoic acid, N-(meth)acryloyl-m-aminobenzoic acid, N-(meth)acryloyl-5-aminosalicylic acid, N-(meth)acryloyl-4-aminosalicylic acid, 4-(meth)acryloyloxyethyl trimellitic acid and its anhydride, 4-(meth)acryloyloxybutyl trimellitic acid and its anhydride, 4-(meth)acryloyloxyhexyl trimellitic acid and its anhydride, 4-(meth)acryloyloxydecyl trimellitic acid and its anhydride, 2-(meth)acryloyloxybenzoic acid The acid, 3-(meth)acryloyloxybenzoic acid, 4-(meth)acryloyloxybenzoic acid, β-(meth)acryloyloxyethyl succinate, β-(meth)acryloyloxyethyl maleate, β-(meth)acryloyloxyethyl phthalate, 11-(meth)acryloyloxy-1,1-undecanedicarboxylic acid, p-vinylbenzoic acid, (2-(meth)acryloyloxyethyl)phosphate, (2-(meth)acryloyloxyethylphenyl)phosphate, 10-(meth)acryloyloxydecyl phosphate, 10-methacryloyloxydecyl phosphate, 11-(meth)acryloyloxyundecyl phosphate, 11-methacryloyloxyundecyl phosphate, p-styrenesulfonic acid, and at least one of 2-acrylamido-2-methylpropanesulfonic acid.
5. The cement composition for periodontal fixation according to claim 1, characterized in that, The first component is selected from at least one of ethoxylated bisphenol A di(meth)acrylate with 8-20 ethoxy groups and polyurethane di(meth)acrylate with 4-8 intramolecular carbamoyl groups.
6. The cement composition for periodontal fixation according to claim 2, characterized in that, The polymerizable monomer composition further includes a third component, which is a monofunctional polymerizable monomer and / or a polyfunctional polymerizable monomer, and the content of the third component is 0-60 parts by weight, and the total amount of the first component, the second component and the third component is 100 parts by weight.
7. The cement composition for periodontal fixation according to claim 1, characterized in that, It also includes a photopolymerization initiator accelerator, wherein the photopolymerization initiator accelerator is 0.5-3 times the weight of the photopolymerization initiator; the total weight of the polymerizable monomer and the photopolymerization initiator is 100 parts by weight, and the content of the photopolymerization initiator and the photopolymerization initiator accelerator is 0.1 to 5 parts by weight of the total weight.
8. The cement composition for periodontal fixation according to claim 7, characterized in that, It also includes a polymerization inhibitor, wherein the amount of the polymerization inhibitor added is 50 to 20,000 ppm relative to the polymerizable monomer composition.
9. The cement composition for periodontal fixation according to claim 2, characterized in that, It also includes water, in an amount of 0 to 5 parts by weight relative to the polymeric monomer composition.
10. The cement composition for periodontal fixation according to claim 1, characterized in that, It also includes a thickener, which is at least one of silica, titanium dioxide or alumina inorganic micro powder with a particle size of 0.002-0.05 micrometers obtained by gas-phase method.
11. The cement composition for periodontal fixation according to claim 1, characterized in that, The density of polymeric functional groups per unit volume of the first component is 1.62–3.12 mmol / mL.
12. The cement composition for periodontal fixation according to claim 5, characterized in that, The first component is selected from at least one of the following substances: poly(8)urethane diacrylate, 8 ethoxylated bisphenol A dimethyl acrylate, 10 ethoxylated bisphenol A dimethyl acrylate, and 17 ethoxylated bisphenol A dimethyl acrylate.