Anode active material, anode for lithium secondary battery, lithium secondary battery, battery module and battery pack
By manufacturing a silicon carbon composite lithium secondary battery electrode under controlled conditions to achieve a specific efficiency slope, the battery achieves high energy density and capacity with enhanced lifespan and stability.
Patent Information
- Application Number
- PCT/KR2026/096724
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-05-07
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-12
AI Technical Summary
Existing lithium secondary batteries face challenges in achieving high energy density and capacity while maintaining lifespan characteristics due to issues with silicon-based and carbon-based active materials, particularly under high electrode density and rolling pressure, leading to volume expansion and capacity efficiency loss.
A negative electrode active material comprising a silicon carbon composite is manufactured under multiple conditions with varying electrode densities, and the initial efficiency is measured to ensure a slope between electrode density and initial efficiency falls within a specific range (-50 to -10), optimizing the electrode structure for high energy density and stability.
The optimized silicon carbon composite maintains high energy density and capacity characteristics while ensuring physical and electrical stability, improving lifespan characteristics and reducing capacity development issues.
Smart Images

Figure KR2026096724_12112026_PF_FP_ABST
Abstract
Description
Cathode active material, cathode for lithium secondary battery, lithium secondary battery, battery module and battery pack
[0001] This application is based on Korean Patent Application No. 10-2025-0060379, which was filed with the Korean Intellectual Property Office on May 9, 2025, and whose contents are incorporated herein in their entirety by reference, and claims priority thereof.
[0002] The present application relates to a negative electrode active material, a negative electrode for a lithium secondary battery, a lithium secondary battery, a battery module, and a battery pack.
[0003] Due to the rapid increase in the use of fossil fuels, there is a growing demand for alternative or clean energy. As part of this effort, the fields of power generation and energy storage utilizing electrochemical reactions are the most actively researched.
[0004] Recently, accompanied by the rapid proliferation of battery-powered electronic devices such as mobile phones, laptop computers, and electric vehicles, as well as power tools and vacuum cleaners, the demand for rechargeable batteries that are small and lightweight yet possess relatively high capacity and / or high output is rapidly increasing. In particular, lithium-ion batteries are gaining prominence as power sources for electronic devices due to their lightweight nature and high energy density. Accordingly, active research and development efforts are underway to improve the performance of lithium-ion batteries.
[0005] In a lithium secondary battery, electrical energy is produced by oxidation and reduction reactions when lithium ions are inserted into or removed from the anode and cathode while the anode and cathode are filled with an organic or polymer electrolyte between an anode and a cathode made of active materials capable of lithium ion intercalation and deintercalation.
[0006] Metal oxides such as LiCoO2, LiMnO2, LiMn2O4, or LiNiO2 are used as the positive electrode active material constituting the positive electrode of a lithium secondary battery, while carbon-based materials such as metallic lithium, graphite, or activated carbon, or materials such as Si / C are used as the negative electrode active material constituting the negative electrode. Among the above negative electrode active materials, metallic lithium was primarily used in the early stages; however, as charge and discharge cycles progressed, lithium atoms grew on the surface of the metallic lithium, damaging the separator and causing battery failure; consequently, carbon-based materials have been predominantly used recently.
[0007] Although graphite is mainly used as the negative electrode active material for lithium secondary batteries, it is difficult to increase the capacity of lithium secondary batteries because graphite has a low capacity per unit mass of 372 mAh / g. Accordingly, to increase the capacity of lithium secondary batteries, negative electrode materials such as silicon, tin, and their oxides are being developed as non-carbon negative electrode materials that have a higher energy density than graphite. However, in the case of these non-carbon negative electrode materials, although the capacity is high, there is a problem in that the initial efficiency is low, resulting in high lithium consumption during the initial charge and discharge cycles and large irreversible capacity loss.
[0008] Accordingly, methods to increase capacity and improve energy density by applying carbon-based active materials are being studied, or research is underway to secure energy density and capacity along with lifespan performance by appropriately combining silicon-based and carbon-based active materials; however, a lithium secondary battery anode capable of solving the aforementioned problems has not yet been developed.
[0009] In particular, research on silicon-carbon composites is underway as next-generation silicon-based active materials. These materials are known to be suitable for high-energy-density lithium-ion batteries due to their high capacity and efficiency. However, achieving high energy density requires high electrode density, which necessitates high electrode density and strong rolling pressure. Consequently, applying such density and pressure leads to issues with capacity efficiency realization and a degradation of lifespan characteristics.
[0010] Accordingly, there is a need to develop a cathode that can effectively improve battery life characteristics while using silicon-based and / or carbon-based active materials, and achieve rapid charging performance and high energy density.
[0011] <Prior Art Literature>
[0012] Japanese Patent Publication No. 2009-080971
[0013] This application relates to a negative electrode active material, and more specifically, to a negative electrode active material used in manufacturing a negative electrode that does not exhibit capacity efficiency even under high electrode density and strong rolling pressure. Specifically, it was discovered that the problem can be solved by manufacturing a negative electrode containing the above-mentioned negative electrode active material under multiple conditions with different electrode densities, measuring the initial efficiency for each of the negative electrodes, and using a negative electrode active material in which the slope of the graph showing the relationship between electrode density (x-axis) and initial efficiency (y-axis) is below a certain range. Accordingly, this application relates to a negative electrode for a lithium secondary battery, a lithium secondary battery, a battery module, and a battery pack capable of securing high energy density and high capacity along with lifespan characteristics.
[0014] One embodiment of the present specification provides a negative electrode active material comprising a silicon carbon composite, wherein a negative electrode comprising the negative electrode active material is manufactured under multiple conditions with different electrode densities, and after measuring the initial efficiency for each of the negative electrodes, the slope of a graph showing the relationship between electrode density (x-axis) and initial efficiency (y-axis) is -50 or greater and -10 or less.
[0015] In one embodiment of the present application, a negative electrode for a lithium secondary battery is provided, comprising: a negative electrode current collector layer; and a negative electrode active material layer provided on one or both sides of the negative electrode current collector layer, wherein the negative electrode active material layer comprises a negative electrode active material layer composition comprising the aforementioned negative electrode active material.
[0016] In one embodiment of the present application, a lithium secondary battery is provided comprising: a positive electrode; a negative electrode for a lithium secondary battery according to the present application; a separator provided between the positive electrode and the negative electrode; and an electrolyte.
[0017] In one embodiment of the present application, a battery module including the lithium secondary battery is provided.
[0018] Finally, a battery pack comprising the above-mentioned lithium secondary battery or the above-mentioned battery module is provided.
[0019] In the development of automotive batteries, high energy density and high capacity performance are essential to improve driving performance. To satisfy these performance requirements, silicon-carbon composites must be used as negative electrode active materials; however, this leads to issues with lifespan performance due to volume expansion, as well as problems with negative electrode slurry stability and capacity development due to high rolling density.
[0020] The cathode active material according to the present application comprises a silicon carbon composite, and cathodes containing the cathode active material are manufactured under multiple conditions with different electrode densities, and after measuring the initial efficiency for each of the cathodes, the slope of the graph showing the relationship between electrode density (x-axis) and initial efficiency (y-axis) is characterized by being -50 or greater and -10 or less.
[0021] That is, when manufacturing a silicon carbon composite, if the amount of carbon coating layer of porous carbon and the specific surface area of the silicon carbon composite are controlled accordingly, the slope of the graph shape, in which the x-axis represents electrode density and the y-axis represents initial efficiency, can be satisfied as being between -50 and -10 depending on charging and discharging, and the carbon coating layer in the silicon carbon composite wraps well around the silicon, thereby having the above-mentioned characteristics.
[0022] When using a silicon carbon composite having the above-mentioned characteristics, high energy density and high capacity characteristics can be achieved, and at the same time, it is physically and electrically stable even at high electrode densities, so that the slope of the initial efficiency according to electrode density satisfies the aforementioned range, thereby improving lifespan characteristics and simultaneously resolving the problem of capacity development.
[0023] FIG. 1 is a diagram showing a stacked structure of a negative electrode for a lithium secondary battery according to one embodiment of the present application.
[0024] FIG. 2 is a diagram showing a stacked structure of a lithium secondary battery according to one embodiment of the present application.
[0025] Figure 3 is a figure showing the graph of electrode density vs. initial efficiency of the examples and comparative examples according to the present application.
[0026] <Explanation of Symbols>
[0027] 10: Cathode current collector layer
[0028] 20: Cathode active material layer
[0029] 100: Negative electrode for lithium secondary battery
[0030] 50: Positive current collector layer
[0031] 40: Positive active material layer
[0032] 200: Cathode for lithium secondary batteries
[0033] 30: Separator
[0034] Before describing the present invention, some terms are defined first.
[0035] In this specification, when a part is described as "comprising" a certain component, it means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0036] In this specification, 'p to q' means a range of 'p or more and q or less'.
[0037] In this specification, "specific surface area" is measured by the BET method, specifically calculated from the amount of nitrogen gas adsorbed at a liquid nitrogen temperature (77K) using BELSORP-mino II of BEL Japan. That is, in this application, the BET specific surface area may refer to the specific surface area measured by the above measurement method.
[0038] In this specification, "Dn" refers to the particle size distribution and represents the particle size at the n% point of the cumulative distribution of the number of particles according to particle size. That is, D50 is the particle size (average particle size) at the 50% point of the cumulative distribution of the number of particles according to particle size, D90 is the particle size at the 90% point of the cumulative distribution of the number of particles according to particle size, and D10 is the particle size at the 10% point of the cumulative distribution of the number of particles according to particle size. Meanwhile, the particle size distribution can be measured using the laser diffraction method. Specifically, after dispersing the powder to be measured in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the difference in diffraction patterns according to particle size is measured as the particles pass through the laser beam to calculate the particle size distribution.
[0039] In this specification, the meaning that a polymer contains a monomer in monomer units means that the monomer participates in a polymerization reaction and is included as a repeating unit within the polymer. In this specification, when it is stated that a polymer contains a monomer, this is interpreted as the same as the polymer containing the monomer in monomer units.
[0040] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers unless specified as "homopolymer."
[0041] In this specification, the weight-average molecular weight (Mw) and the number-average molecular weight (Mn) are polystyrene equivalent molecular weights measured by gel permeation chromatography (GPC), using commercially available monodisperse polystyrene polymers of various degrees of polymerization (standard samples) for molecular weight measurement as standard materials. In this specification, the term "molecular weight" means weight-average molecular weight unless otherwise specified.
[0042] Hereinafter, the present invention will be described in detail with reference to the drawings so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in various different forms and is not limited to the description below.
[0043] One embodiment of the present application provides a negative electrode active material comprising a silicon carbon composite, wherein a negative electrode comprising the negative electrode active material is manufactured under multiple conditions with different electrode densities, and after measuring the initial efficiency for each of the negative electrodes, the slope of a graph showing the relationship between electrode density (x-axis) and initial efficiency (y-axis) is -50 or greater and -10 or less.
[0044] In the present application, the negative electrode active material may be composed of a silicon carbon composite.
[0045] When using a cathode active material (silicon carbon composite) having the above-mentioned characteristics, high energy density and high capacity characteristics can be achieved, and at the same time, it is physically and electrically stable even at high electrode densities, so that the slope of the initial efficiency according to electrode density satisfies the aforementioned range, thereby improving lifespan characteristics and simultaneously resolving the problem of capacity development.
[0046] In the present application, a graph shape in which the x-axis represents electrode density and the y-axis represents initial efficiency can be obtained through the following process.
[0047] 1. Electrode manufacturing
[0048] A slurry containing a silicon carbon composite (Si / C), a binder, and a conductive material is prepared as a negative electrode active material (by mixing the materials in a mortar and pestle) and applied to a Cu foil.
[0049] At this time, the binder and conductive material described below may be used without restriction.
[0050] 2. Electrode rolling
[0051] The electrode manufactured above is rolled using a roll press. At this time, the electrode density is determined during the process and may vary depending on the operation (e.g., expansion of Si / C material and generation of by-products); however, the electrode density changing due to operation is not measured separately, and the change in the initial efficiency value is observed according to the density of the initially manufactured electrode.
[0052] 3. Electrode drying
[0053] The above rolled electrode is vacuum dried at 120°C for 8 hours.
[0054] 4. Electrode density measurement
[0055] After measuring the weight and thickness of the above electrode and Cu foil, respectively, the electrode density is calculated according to the following formula.
[0056] Electrode density = ((Electrode weight - Cu foil weight) / Electrode area) / (Electrode thickness - Cu foil thickness)
[0057] 5. CHC Assembly and Evaluation
[0058] A coin cell is assembled using the above electrodes, and the initial efficiency is calculated based on the first charge / discharge capacity (at 1.0V). Then, a graph of electrode density versus initial efficiency is plotted. In this case, lithium metal is used as the counter electrode.
[0059] At this time, the slope can be obtained by plotting the graph using the above method and then deriving the slope when a linear trend line is found based on the initial efficiency values for five or more different rolling densities. That is, the slope when a linear trend line is found based on the initial efficiency values for five or more cathodes with different electrode densities is derived.
[0060] In the present application, the silicon carbon composite can be represented as Si / C.
[0061] In this specification, the silicon carbon composite is a composite of Si and C and is distinguished from silicon carbide denoted as SiC. Since the silicon carbide does not electrochemically react with lithium, all performance characteristics, such as lifespan, can be measured as zero.
[0062] The above silicon carbon composite may be a composite of silicon and graphite, etc., and may form a structure in which graphene or amorphous carbon, etc. surrounds a core composed of silicon and graphite, etc. In the above silicon carbon composite, the silicon may be nano silicon. For example, the nano silicon may be silicon in the range of 1 nm to 999 nm.
[0063] Meanwhile, the average particle size (D50 particle size) of the silicon carbon composite of the present invention is 1 μm or more and 10 μm or less, specifically 2 μm to 8 μm, and more specifically 3 μm to 8 μm. When the average particle size falls within the above range, the specific surface area of the particles is within a suitable range, and the viscosity of the cathode slurry is formed within an appropriate range. Accordingly, the dispersion of the particles constituting the cathode slurry becomes smooth. In addition, since the size of the silicon carbon composite has a value greater than or equal to the lower limit range, the contact area between the silicon particles and the conductive materials is excellent due to the composite composed of the conductive material and the binder within the cathode slurry, which increases the likelihood of the conductive network continuing and thereby increases the capacity retention rate. Meanwhile, when the average particle size satisfies the above range, excessively large silicon particles are excluded, and the surface of the cathode is formed smoothly, thereby preventing current density non-uniformity during charging and discharging.
[0064] In addition, in one embodiment of the present application, the silicon carbon composite may not include particles having a particle size of less than 1 μm. Specifically, the silicon carbon composite may include particles having a particle size of 1 μm or more and 10 μm or less, and the particles having a particle size of less than 1 μm may be included in an amount of 1 part by weight or less, specifically 0.1 part by weight or less, based on 100 parts by weight of the silicon carbon composite particles. That is, the silicon carbon composite according to the present application is characterized by not including fine particles.
[0065] The present application provides a negative electrode for a lithium secondary battery, wherein the silicon carbon composite comprises porous carbon; and silicon deposited on the porous carbon, and the silicon carbon composite further comprises a carbon coating layer.
[0066] In the present application, the amount of carbon coating in the carbon coating layer may be 5 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of the silicon carbon composite, specifically 5 parts by weight or more and 20 parts by weight or less, and more specifically 5 parts by weight or more and 15 parts by weight or less.
[0067] In the case of the above carbon coating amount, the carbon coating amount can be calculated based on the total weight of the silicon carbon composite of 100, and specifically, the C coating amount (%) can be calculated as (Weight of Si / C after C coating - Weight of Si / C before C coating) x 100 / Weight of SiC after C coating.
[0068] In this case, the composition and manufacturing method of the carbon coating layer may use methods used in the industry.
[0069] In one embodiment of the present application, if the carbon coating amount is excessively low, the silicon surface is not sufficiently covered, leading to increased direct contact with the electrolyte. Consequently, SEI formation proceeds excessively, which may result in a decrease in initial efficiency. Furthermore, the inability to cope with volume changes in silicon during charging and discharging may cause the collapse of the electrode structure and electrical interruption. On the other hand, if the carbon coating amount is excessively high, the silicon content is relatively reduced, which may lower the overall capacity. Additionally, due to the thick carbon layer, the lithium ion diffusion path becomes longer, increasing reaction resistance and potentially degrading high-rate performance.
[0070] In the present application, the specific surface area (BET) of the silicon carbon composite is 0.1 m 2 / g or more than 5 m 2 It may be less than / g.
[0071] In one embodiment of the present application, the silicon-carbon composite generally has a characteristic BET surface area. The BET surface area of the silicon-based active material is preferably 0.1 to 5 m² 2 / g, more preferably 0.1 to 4.5 m 2 / g, particularly preferably 0.2 to 4 m 2 / g, most preferably 0.2 to 3.5 m 2 / g. The BET surface area is measured according to DIN 66131 (using nitrogen).
[0072] In this case, the specific surface area of the silicon carbon composite refers to the specific surface area of the silicon carbon composite including the carbon coating layer when the carbon coating layer is included, and may refer to the specific surface area of the silicon carbon composite itself when the carbon coating layer is not included.
[0073] In one embodiment of the present application, if the specific surface area of the silicon carbon composite is less than the above range, the inter-particle bonding becomes excessively dense, restricting the penetration of the electrolyte, and the reaction surface area of lithium ions is insufficient, so activation may not be sufficiently achieved. As a result, the initial efficiency and capacity development characteristics may be reduced.
[0074] Conversely, if the aforementioned specific surface area exceeds a certain range, the excessive surface area increases the contact area with the electrolyte, leading to excessive SEI formation and an increase in initial irreversible capacity, which may result in reduced initial efficiency. Additionally, excessive porosity may increase, making it difficult to secure electrode density.
[0075] In one embodiment of the present application, when the carbon coating amount and the specific surface area simultaneously satisfy the optimal range, the carbon coating layer can uniformly surround the silicon particles while suppressing an excessive increase in surface area.
[0076] In particular, when the carbon coating amount is secured at an appropriate level and the specific surface area is controlled within the above range, the diffusion path of lithium ions is sufficiently secured while reducing unnecessary contact with the electrolyte, thereby allowing for simultaneous improvement of initial efficiency and reactivity.
[0077] Conversely, if either of the two parameters falls outside the above range, SEI overformation or reduced reactivity may occur, and electrode characteristics may rapidly deteriorate.
[0078] In one embodiment of the present application, when the carbon coating amount and specific surface area satisfy the aforementioned range, the slope of the graph of the relationship between the aforementioned electrode density (x-axis) and initial efficiency (y-axis) may satisfy a range of -50 or more and -10 or less.
[0079] Specifically, if the slope is excessively steep (less than -50), it implies that the initial efficiency decreases rapidly as electrode density increases, which may be attributed to reduced ion mobility within the electrode or electrical contact instability; conversely, if the slope exceeds -10, the change in initial efficiency with respect to changes in electrode density is excessively small, which may indicate that the electrode structure is not sufficiently optimized or that substantial improvement in reaction characteristics is limited.
[0080] Therefore, when the slope satisfies a range of -50 to -10 as in the present application, the decrease in initial efficiency is controlled smoothly even if the electrode density increases, which means that electrical and physical stability within the electrode is secured.
[0081] In one embodiment of the present application, the silicon carbon composite may exist, for example, in a crystalline or amorphous form and is preferably not porous. The silicon particles are preferably spherical or fragmentary particles. Alternatively, but less preferably, the silicon particles may also have a fibrous structure or exist in the form of a silicon-containing film or coating.
[0082] In the present application, the silicon may be 40 parts by weight or more and 60 parts by weight or less based on 100 parts by weight of the silicon carbon composite.
[0083] In another embodiment, based on 100 parts by weight of the silicon carbon composite, the silicon may be 40 parts by weight or more and 60 parts by weight or less, specifically 45 parts by weight or more and 60 parts by weight or less, and may be 45 parts by weight or more and 55 parts by weight or less.
[0084] The silicon-carbon composite is formed by depositing silicon onto porous carbon, and by satisfying the silicon content as described above, it is possible to secure high energy density along with lifespan characteristics. In other words, by satisfying an appropriate silicon flow rate, it can be densely deposited onto porous carbon, thereby enabling the aforementioned effects to be exhibited.
[0085] In the present application, a cathode comprising the above-described cathode active material is manufactured under multiple conditions with different electrode densities, and after measuring the initial efficiency for each of the cathodes, a cathode active material is provided having a slope of -50 or greater and -10 or less in a graph showing the relationship between electrode density (x-axis) and initial efficiency (y-axis).
[0086] In another embodiment, the slope may be -10 or less, specifically -11 or less, more specifically -12 or less, and -50 or more, specifically -45 or more.
[0087] Cathodes using silicon-carbon composites are employed to achieve high energy density and high capacity; therefore, achieving high energy density requires high electrode density, and high rolling pressure is applied during the manufacturing process. Since silicon-carbon composites consist of silicon deposited on porous carbon, they crumble when subjected to high rolling pressure, leading to problems such as gas generation due to reaction with water.
[0088] However, the negative electrode active material according to the present application satisfies the slope as described above, which corresponds to a result in which, when using a silicon carbon composite, the amount of carbon coating layer deposition and the specific surface area of the silicon carbon composite are controlled, resulting in excellent electrical conductivity and simultaneously maintaining initial efficiency well even at high electrode densities.
[0089] That is, the cathode according to the present application is characterized by controlling the silicon-carbon composite to maintain a form that effectively encases the physically deposited silicon, thereby being stable, having excellent electrical conductivity, and having excellent lifespan characteristics.
[0090] In one embodiment of the present application, the silicon carbon composite may have a non-spherical shape, and the sphericity is, for example, 0.9 or less, for example, 0.7 to 0.9, for example, 0.8 to 0.9, for example, 0.85 to 0.9.
[0091] In the present application, the circularity is determined by the following formula 1-A, where A is the area and P is the boundary line.
[0092] [Equation 1-A]
[0093] 4πA / P 2
[0094] The present application provides a negative electrode for a lithium secondary battery comprising: a negative current collector layer; and a negative active material layer provided on one or both sides of the negative current collector layer, wherein the negative active material layer comprises a negative active material layer composition including the aforementioned negative active material.
[0095] That is, the above-described negative electrode active material layer is characterized by comprising a negative electrode active material layer composition that includes a negative electrode active material such that the carbon coating amount and specific surface area satisfy a specific range as described above, so that the slope of the relationship between electrode density and initial efficiency is between -50 and -10. Accordingly, it is possible to secure excellent electrical conductivity and structural stability while effectively suppressing the decrease in initial efficiency due to increased electrode density, thereby providing a negative electrode for a lithium secondary battery that can simultaneously achieve high energy density and high capacity characteristics along with improved lifespan characteristics.
[0096] FIG. 1 is a diagram showing a stacked structure of a negative electrode for a lithium secondary battery according to one embodiment of the present application. Specifically, a negative electrode (100) for a lithium secondary battery including a negative active material layer (20) on one surface of a negative current collector layer (10) can be seen, and FIG. 1 shows that the negative active material layer is formed on one surface, but it can be included on both surfaces of the negative current collector layer.
[0097] This is explained in more detail below.
[0098] In one embodiment of the present application, the negative current collector layer generally has a thickness of 1 μm to 100 μm, specifically a thickness of 8 μm to 15 μm. Such a negative current collector layer is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy may be used. In addition, fine irregularities may be formed on the surface to strengthen the bonding strength of the negative active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven body, etc.
[0099] In one embodiment of the present application, the thickness of the negative current collector layer may be 1 μm or more and 100 μm or less.
[0100] However, the thickness may vary depending on the type and application of the cathode used, and is not limited thereto.
[0101] The present application provides a negative electrode for a lithium secondary battery, wherein the negative electrode active material layer composition further comprises a carbon-based active material.
[0102] In one embodiment of the present invention, the carbon-based active material may include artificial graphite and natural graphite.
[0103] In the present application, a negative electrode active material is provided in which the weight ratio of natural graphite to artificial graphite based on the carbon-based active material is 5:95 or higher and 50:50 or lower.
[0104] In another embodiment, the weight ratio of natural graphite to artificial graphite based on the carbon-based standard may satisfy 5:95 or more and 50:50 or less, preferably 7:93 to 45:55, and more preferably 10:90 to 40:60.
[0105] In the present application, the carbon-based active material includes graphite, and the graphite may include artificial graphite and natural graphite. Since it has been confirmed that artificial graphite has superior cell characteristics compared to natural graphite, the use of natural graphite is being reduced and the amount of artificial graphite used is being increased. However, from a cost perspective, artificial graphite requires the calcination and graphitization of coke, which poses a problem due to high processing costs. Accordingly, if the above range is satisfied, it has the characteristic of being able to improve cell characteristics along with addressing cost issues.
[0106] In the present application, the natural graphite is characterized by satisfying the range of Formula 1.
[0107] In the present application, the average particle size (D50) of the natural graphite is 10 μm or more and 30 μm or less, the tap density of the natural graphite is 0.5 g / cc or more and 2.0 g / cc or less, and the specific surface area of the natural graphite is 1 m² 2 / g or more than 5m 2 It may be less than / g.
[0108] In another embodiment, the average particle size (D50) of the natural graphite may be 10 μm or more and 30 μm or less, specifically 12 μm or more and 27 μm or less, and more specifically 15 μm or more and 20 μm or less.
[0109] In another embodiment, the tap density of the natural graphite may be 0.5 / cc or more and 2.0g / cc or less, specifically 0.7 / cc or more and 1.5g / cc or less, and more specifically 0.9 / cc or more and 1.2g / cc or less.
[0110] In another embodiment, the specific surface area of the natural graphite is 1 m² 2 / g or more than 5m 2 / g or less, specifically 1m 2 / g or more than 4m 2 / g or less, more specifically 1m 2 / g or more than 3m 2 It may be less than / g.
[0111] In the present application, the average particle size (D50) of the artificial graphite is 10 μm or more and 25 μm or less, the tap density of the artificial graphite is 0.5 g / cc or more and 1.5 g / cc or less, and the specific surface area of the artificial graphite is 0.1 m² 2 / g or more 3.0m 2 It can be less than / g.
[0112] In another embodiment, the average particle size (D50) of the artificial graphite may be 10 μm or more and 25 μm or less, specifically 12 μm or more and 24 μm or less, and more specifically 14 μm or more and 23 μm or less.
[0113] In another embodiment, the tap density of the artificial graphite may be 0.5 / cc or more and 1.5g / cc or less, specifically 0.7 / cc or more and 1.3g / cc or less, and more specifically 0.9 / cc or more and 1.1g / cc or less.
[0114] In another embodiment, the specific surface area of the artificial graphite is 0.1 m² 2 / g or more 3.0m 2 / g or less, specifically 0.2m 2 / g or more than 2.5m 2 / g or less, more specifically 0.2m 2 / g or more than 2.5m2 It may be less than / g.
[0115] The present application provides a negative electrode for a lithium secondary battery, wherein the negative electrode active material and the carbon-based active material comprise a combined total of 95 parts by weight or less based on 100 parts by weight of the negative electrode active material layer composition.
[0116] In another embodiment, based on 100 parts by weight of the cathode active material layer composition, the cathode active material and the carbon-based active material may be in a combined total of 95 parts by weight or less, specifically 90 parts by weight or less, and 50 parts by weight or more, preferably 70 parts by weight or more.
[0117] The present application provides a negative electrode for a lithium secondary battery, wherein the negative electrode active material comprises 50 parts by weight or less based on a total of 100 parts by weight of the negative electrode active material and the carbon-based active material.
[0118] In another embodiment, based on a total of 100 parts by weight of the cathode active material and the carbon-based active material, the cathode active material may comprise 1 part by weight or more and 50 parts by weight or less, specifically 5 parts by weight or more and 45 parts by weight or less, and more specifically 10 parts by weight or more and 35 parts by weight or less.
[0119] By including a negative electrode active material within the range described above, the negative electrode possesses the characteristic of being able to secure capacity characteristics and energy density. That is, while increasing the content of the silicon-carbon composite can improve energy density, it leads to severe volume expansion and a decrease in lifespan characteristics; conversely, if the content of the silicon-carbon composite is low, high energy density and rapid charging performance cannot be secured. Therefore, using the above-mentioned content allows for the simultaneous improvement of high energy density and rapid charging performance.
[0120] Conventionally, it was common practice to use only graphite-based compounds as negative electrode active materials; however, with the recent rise in demand for high-capacity batteries, there have been increasing attempts to mix in silicon-based compounds to increase capacity. Nevertheless, silicon-based compounds have a limitation in that their volume expands rapidly during the charging and discharging process, damaging the conductive pathways formed within the negative electrode active material layer and actually degrading battery performance.
[0121] Accordingly, in one embodiment of the present application, a negative electrode for a lithium secondary battery is provided, wherein the negative electrode active material layer composition further comprises a negative electrode conductive material; and a negative electrode binder.
[0122] In one embodiment of the present application, the cathode conductive material may be any material that is generally used in the art without limitation, and specifically may include one or more selected from the group consisting of point conductive materials; planar conductive materials; and linear conductive materials.
[0123] In one embodiment of the present application, the dot-shaped conductive material can be used to improve conductivity of the cathode and refers to a conductive material having a dot shape or a sphere that is conductive without causing chemical changes. Specifically, the dot-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, Farnes black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably may include carbon black in terms of achieving high conductivity and excellent dispersibility.
[0124] In one embodiment of the present application, the point-shaped conductive material has a BET specific surface area of 40 m² 2 / g or more 70m 2 It may be less than / g, preferably 45m 2 / g or more 65m2 / g or less, more preferably 50m 2 / g or more 60m 2 It may be less than / g.
[0125] In one embodiment of the present application, the particle size of the dot-shaped conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 20 nm to 60 nm.
[0126] In one embodiment of the present application, the cathode conductive material may include a planar conductive material.
[0127] The above-mentioned planar conductive material can be described as a plate-shaped conductive material or a bulk-shaped conductive material, as it can improve conductivity by increasing surface contact between silicon particles within the cathode and simultaneously suppress the interruption of conductive pathways due to volume expansion.
[0128] In one embodiment of the present application, the planar conductive material may comprise at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and preferably may be plate-shaped graphite.
[0129] In one embodiment of the present application, the average particle size (D50) of the planar conductive material may be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 4 μm to 5 μm. When the above range is satisfied, dispersion is easy without causing an excessive increase in the viscosity of the cathode slurry due to the sufficient particle size. Therefore, when dispersion is performed using the same equipment and time, the dispersion effect is excellent.
[0130] In one embodiment of the present application, the planar conductive material provides a cathode composition in which D10 is 0.5 μm or more and 1.5 μm or less, D50 is 2.5 μm or more and 3.5 μm or less, and D90 is 7.0 μm or more and 15.0 μm or less.
[0131] In one embodiment of the present application, the planar conductive material may be a high specific surface area planar conductive material having a high BET specific surface area; or a low specific surface area planar conductive material.
[0132] In one embodiment of the present application, a planar conductive material with a high specific surface area or a planar conductive material with a low specific surface area may be used without limitation as the planar conductive material; however, since the planar conductive material according to the present application may be affected to some extent by dispersion in electrode performance, it may be particularly preferable to use a planar conductive material with a low specific surface area that does not cause problems with dispersion.
[0133] In one embodiment of the present application, the planar conductive material has a BET specific surface area of 5 m² 2 It can be more than / g.
[0134] In another embodiment, the planar conductive material has a BET specific surface area of 5m² 2 / g or more than 500m 2 It may be less than / g, preferably 5m 2 / g or more than 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2 It may be less than / g.
[0135] In another embodiment, the planar conductive material is a high specific surface area planar conductive material, and has a BET specific surface area of 50 m² 2 / g or more than 500m 2 / g or less, preferably 80m 2 / g or more than 300m 2 / g or less, more preferably 100m 2 / g or more than 300m 2 It can satisfy a range of / g or less.
[0136] In another embodiment, the planar conductive material is a low specific surface area planar conductive material, and the BET specific surface area is 5m² 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 It can satisfy a range of / g or less.
[0137] Other conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. The bundled carbon nanotubes may comprise a plurality of carbon nanotube units. Specifically, "bundle type" here refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged in parallel or intertwined with the axes along the length direction of the carbon nanotube units in substantially the same orientation, unless otherwise noted. The carbon nanotube units have a graphite sheet having a cylindrical shape with a nano-sized diameter and an sp2 bonding structure. Depending on the angle and structure in which the graphite sheet is rolled, it may exhibit conductive or semiconductor properties. Compared to entangled type carbon nanotubes, the bundled carbon nanotubes described above can be uniformly dispersed during cathode manufacturing and smoothly form a conductive network within the cathode, thereby improving the conductivity of the cathode.
[0138] In particular, the linear conductive material according to one embodiment of the present application may be a single-walled carbon nanotube (SWCNT).
[0139] The above single-walled carbon nanotube is a material in which carbon atoms arranged in a hexagonal shape form a tube. Depending on its unique chirality, it exhibits insulating, conductive, or semiconductor properties. Since the carbon atoms are connected by strong covalent bonds, it has a tensile strength approximately 100 times greater than that of steel, excellent flexibility and elasticity, and is chemically stable.
[0140] The average diameter of the single-walled carbon nanotubes is 0.5 nm to 15 nm. According to one embodiment of the present invention, the average diameter of the single-walled carbon nanotubes may be 1 to 10 nm, or 1 nm to 5 nm, or 1 nm to 2 nm. When the average diameter of the single-walled carbon nanotubes satisfies these ranges, the electrical conductivity of the cathode can be maintained even when the single-walled carbon nanotubes are included in a very small amount, and desirable viscosity and solid content can be obtained when preparing a conductive material dispersion. In the conductive material dispersion, the single-walled carbon nanotubes may clump together and exist in an entangled state (aggregate). Accordingly, the above average diameter can be derived by confirming the diameter of any entangled single-walled carbon nanotube aggregate extracted from the above conductive material dispersion using SEM or TEM, and then dividing the diameter of the aggregate by the number of single-walled carbon nanotubes constituting the aggregate.
[0141] The BET specific surface area of the above single-walled carbon nanotube is 500 m² 2 / g to 1,500 m 2 / g, or 900 m 2 / g to 1,200 m 2 It can be / g, specifically 250 m 2 / g to 330 m 2 It may be / g. If the above range is satisfied, a conductive material dispersion with a desirable solid content is obtained, and the viscosity of the cathode slurry is prevented from rising excessively. The above BET specific surface area can be measured through the nitrogen adsorption BET method.
[0142] The aspect ratio of the single-walled carbon nanotube may be 50 to 20,000, or the length of the single-walled carbon nanotube may be 5 to 100 μm or 5 to 50 μm. When the aspect ratio or length satisfies these ranges, the specific surface area is high, so the single-walled carbon nanotube can be adsorbed to the active material particles within the cathode with a strong attractive force. Accordingly, the conductive network can be smoothly maintained even with the volume expansion of the cathode active material. The aspect ratio can be confirmed by calculating the average of the aspect ratios of 15 single-walled carbon nanotubes with a large aspect ratio and 15 single-walled carbon nanotubes with a small aspect ratio when observing the single-walled carbon nanotube powder through SEM.
[0143] Compared to multi-walled or double-walled carbon nanotubes, single-walled carbon nanotubes have a large aspect ratio, making them long and bulky; therefore, they are advantageous in that they can construct electrical networks using only a small amount.
[0144] In one embodiment of the present application, the cathode conductive material may satisfy an amount of 1 part by weight or more and 30 parts by weight or less based on 100 parts by weight of the cathode active material layer composition.
[0145] In another embodiment, the cathode conductive material may be 1 part by weight or more and 30 parts by weight or less, preferably 5 parts by weight or more and 25 parts by weight or less, based on 100 parts by weight of the cathode active material layer composition, more preferably 10 parts by weight or more and 15 parts by weight or less.
[0146] In one embodiment of the present application, the cathode conductive material comprises a point conductive material; a planar conductive material; and a linear conductive material, wherein the ratio of the point conductive material:planar conductive material:linear conductive material may satisfy a ratio of 1:1:0.01 to 1:1:1.
[0147] In one embodiment of the present application, the point-shaped conductive material may satisfy a range of 1 part by weight or more and 60 parts by weight or less, preferably 5 parts by weight or more and 50 parts by weight or less, based on 100 parts by weight of the cathode conductive material.
[0148] In one embodiment of the present application, the planar conductive material may satisfy a range of 1 part by weight or more and 60 parts by weight or less, preferably 5 parts by weight or more and 50 parts by weight or less, based on 100 parts by weight of the cathode conductive material.
[0149] In one embodiment of the present application, the linear conductive material may satisfy a range of 0.01 parts by weight or more and 10 parts by weight or less, preferably 0.05 parts by weight or more and 8 parts by weight or less, and more preferably 0.1 parts by weight or more and 5 parts by weight or less, based on 100 parts by weight of the cathode conductive material.
[0150] In one embodiment of the present application, the cathode conductive material may include a linear conductive material and a planar conductive material.
[0151] In one embodiment of the present application, the cathode conductive material comprises a linear conductive material and a planar conductive material, and the ratio of the linear conductive material to the planar conductive material may satisfy 0.01:1 to 0.1:1.
[0152] In one embodiment of the present application, the negative electrode conductive material specifically comprises a linear conductive material and a planar conductive material, each satisfying the composition and ratio, so that the lifespan characteristics of the existing lithium secondary battery are not significantly affected, and the number of charge and discharge points increases, resulting in excellent output characteristics at a high C-rate.
[0153] In one embodiment of the present application, the cathode conductive material may be made of a linear conductive material.
[0154] At this time, the linear conductive material may be 0.01 to 2 parts by weight, or 0.02 to 0.7 parts by weight, or 0.02 to 0.3 parts by weight, based on 100 parts by weight of the cathode active material layer composition. When the content of the linear conductive material satisfies these ranges, an electrical network can be sufficiently established within the cathode active material layer, and it is advantageous in terms of mixing and coating processability during electrode manufacturing.
[0155] The cathode conductive material according to the present application has a completely separate composition from the anode conductive material applied to the anode. That is, the second cathode conductive material according to the present application serves to hold the contact points between silicon-based active materials, which undergo significant volume expansion of the electrodes due to charging and discharging. The anode conductive material, on the other hand, acts as a buffer during rolling and provides partial conductivity; thus, its composition and role are completely different from those of the cathode conductive material of the present invention.
[0156] In one embodiment of the present application, the cathode binder may comprise at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and materials in which hydrogens thereof are substituted with Li, Na, or Ca, etc., and may also comprise various copolymers thereof.
[0157] The cathode binder according to one embodiment of the present application serves to hold the active material and the conductive material to prevent distortion and structural deformation of the cathode structure during volume expansion and relaxation of the cathode active material. Any general binder that satisfies the above role can be applied, specifically a water-based binder can be used, and more specifically, a PAM-based binder can be used.
[0158] In one embodiment of the present application, the cathode binder is 30 parts by weight or less, preferably 25 parts by weight or less, more preferably 20 parts by weight or less, based on 100 parts by weight of the cathode active material layer composition, and may be 5 parts by weight or more, or 10 parts by weight or more.
[0159] In one embodiment of the present application, a cathode slurry comprising the cathode active material layer composition and a cathode slurry solvent is provided.
[0160] In the present application, the solid content of the cathode slurry may satisfy a range of 10% to 40%.
[0161] The above slurry solvent can be used without limitation as used in the industry, and specifically, water can be used.
[0162] In the present application, the cathode slurry can be coated on one or both sides of the cathode current collector layer to form a cathode active material layer. At this time, the coating method may use any method known in the art without limitation.
[0163] The present application provides a lithium secondary battery in which the rolled density of the negative electrode active material layer is 0.9 g / cc or more and 1.3 g / cc or less.
[0164] High capacity can be achieved by obtaining the rolling density described above, and the resulting issues regarding lifespan characteristics and capacity development were resolved by controlling the properties of the aforementioned silicon carbon composite.
[0165] In one embodiment of the present application, a lithium secondary battery is provided comprising: a positive electrode; a negative electrode for a lithium secondary battery according to the present application; a separator provided between the positive electrode and the negative electrode; and an electrolyte.
[0166] FIG. 2 is a diagram showing a stacked structure of a lithium secondary battery according to one embodiment of the present application. Specifically, a negative electrode (100) for a lithium secondary battery including a negative active material layer (20) on one surface of a negative current collector layer (10) can be seen, and a positive electrode (200) for a lithium secondary battery including a positive active material layer (40) on one surface of a positive current collector layer (50) can be seen, and the structure is formed such that the negative electrode (100) for a lithium secondary battery and the positive electrode (200) for a lithium secondary battery are stacked with a separator (30) in between.
[0167] A secondary battery according to one embodiment of the present specification may particularly include a negative electrode for a lithium secondary battery as described above. Specifically, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the negative electrode is identical to the negative electrode described above. Since the negative electrode has been described above, a detailed description thereof is omitted.
[0168] The above positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and comprising the positive electrode active material.
[0169] In the above-mentioned positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above-mentioned positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesion of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0170] The above-mentioned positive electrode active material may be a commonly used positive electrode active material. Specifically, the above-mentioned positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7, etc.; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3Examples include lithium manganese composite oxides represented by O2 (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, satisfying 0.01≤c3≤0.1) or Li2Mn3MO8 (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); and LiMn2O4 in which a portion of the Li in the chemical formula is substituted with alkaline earth metal ions, but are not limited thereto. The anode may also be Li-metal.
[0171] The above-described positive active material layer may include a positive conductive material and a positive binder together with the positive active material described above.
[0172] At this time, the positive electrode conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that has electronic conductivity without causing chemical changes can be used without special limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used.
[0173] In addition, the anode binder serves to improve adhesion between anode active material particles and adhesion between the anode active material and the anode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.
[0174] As a separator, it separates the negative and positive electrodes and provides a pathway for the movement of lithium ions. Any separator typically used in secondary batteries can be used without special restrictions, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. Specifically, a porous polymer film, such as a porous polymer film made from a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.
[0175] Examples of the above electrolytes that can be used in the manufacture of lithium secondary batteries include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., but are not limited to these.
[0176] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0177] As the above-mentioned non-aqueous organic solvent, for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyl lactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolone, formamide, dimethylformamide, dioxolone, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolone derivative, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivative, tetrahydrofuran derivative, ether, methyl propionate, ethyl propionate, etc. may be used.
[0178] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts, so they can be used preferably. Furthermore, if low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed with these cyclic carbonates in appropriate proportions, an electrolyte with high electrical conductivity can be produced, making it even more preferable to use.
[0179] The metal salt mentioned above may be a lithium salt, and the lithium salt is a substance that dissolves well in the non-aqueous electrolyte; for example, as the anion of the lithium salt, F - , Cl - , I - , NO3 -, N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more types selected from the group consisting of can be used.
[0180] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride.
[0181] One embodiment of the present invention provides a battery module including the secondary battery as a unit cell and a battery pack including the same. Since the battery module and the battery pack include the secondary battery having high capacity, high rate capability and cycle capability, they can be used as a power source for a medium-to-large device selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles and power storage systems.
[0182] Hereinafter, preferred embodiments are presented to aid in understanding the present invention; however, the above embodiments are merely illustrative of the description, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and spirit of the description, and that such variations and modifications fall within the scope of the appended claims.
[0183] <Preparation Example>
[0184] <Example 1>
[0185] Manufacture of Silicon Carbon Composites
[0186] Biomass-based raw materials, such as cellulose powder or coconut shells, or resin-based raw materials were placed in a turbular furnace, and the atmosphere inside the furnace was replaced with an inert gas for 2 hours under an Ar atmosphere at a flow rate of 50–200 ml / min, without increasing the temperature. Subsequently, the temperature was raised to 400°C at a rate of 5°C / min and heated under an argon atmosphere for 2 hours. The carbonization process was then carried out by raising the temperature to 900°C at a rate of 5°C / min and heating under an argon atmosphere for 2 hours; the powder obtained after the reaction was washed 2–3 times with ethanol. Carbon-based particles dried at 100°C for more than 12 hours were heated at 700°C for 3 hours under an argon atmosphere using CO2 as a 10–20% balance gas to expand pores. Afterward, they were washed with distilled water and dried at 100°C for more than 12 hours. As an activation process, 1,800 m2 After obtaining porous carbon with a specific surface area of the level of / g, fine particles smaller than 1μm are removed through classification.
[0187] The above-mentioned porous carbon, after classification is completed, is placed in the hot zone of a CVD device as carbon-based particles, and under a low-pressure environment of 1 to 10 Torr, SiH4 / H A silicon-carbon composite was prepared by flowing 2= 5 / 95 gas at a flow rate of 50 to 210 ml / min at 600℃ for 3 hours.
[0188] As described above, after depositing silicon, a C coating (protective coating) of about 1~2 wt% was performed in the silicon deposition facility, and then transferred to another carbon coating facility to perform the carbon coating.
[0189] <Example 2>
[0190] Manufacture of Silicon Carbon Composites
[0191] In the above Example 1, after applying a C coating (protective coating) of about 3~4 wt% in a silicon deposition facility, the process was transferred to another carbon coating facility to apply the carbon coating.
[0192] <Comparative Example 1>
[0193] In the above Example 1, the silicon carbon composite was manufactured in the same manner as Example 1, except that a carbon layer was not formed on the surface of the silicon carbon composite.
[0194] Coin half cell manufacturing
[0195] To verify the slope as shown in Table 1 below, electrodes were manufactured and evaluated using the following manufacturing method.
[0196] A negative electrode active material layer composition was prepared using the silicon-carbon composite prepared above as a silicon-based active material (average particle size (D50): 5 μm), carbon black (Super C), and polyacrylamide as a binder in a weight ratio of 80:10:10. A negative electrode slurry was prepared by adding distilled water as a solvent for forming the negative electrode slurry. (Solid content 28 wt%)
[0197] The above carbon black and binder were dispersed using a mixer at 2000 rpm for 10 minutes, and then a silicon carbon composite was added and dispersed using a mixer at 2000 rpm for 5 to 10 minutes to prepare a slurry.
[0198] As a cathode current collector, the above cathode slurry is applied at a rate of 3.00 mg / cm² on both sides of a copper current collector (thickness: 15 μm). 2 A negative active material layer (thickness: 23 μm) was formed by coating with a loading amount, rolling, and drying in a vacuum oven at 130°C for 10 hours.
[0199] After assembling the coin half cell manufactured above and calculating the initial efficiency based on the first charge / discharge capacity (based on 1.0V), a graph of electrode density vs. initial efficiency was plotted, the results are shown in Figure 3 below, and the slope values in Table 1 were verified.
[0200] Slope Example 1-13.3~-15 Example 2-23 Comparative Example 1-60
[0201] Experimental Example 1: Evaluation of Dose Retention Rate
[0202] A negative electrode active material layer composition was prepared using the above-prepared silicon-carbon composite (average particle size (D50): 5 μm) as a silicon-based active material, graphite, carbon black (Super C), and polyacrylamide as a binder in a weight ratio of 10:80:5:5. A negative electrode slurry was prepared by adding distilled water as a solvent for forming the negative electrode slurry. (Solid content 28 wt%)
[0203] As a mixing method, the carbon black, binder, and water were dispersed using a homo mixer at 2500 rpm for 30 minutes, then the active material was added and dispersed at 2500 rpm for 30 minutes to prepare a cathode slurry.
[0204] As a cathode current collector, the above cathode slurry is applied at a rate of 3.00 mg / cm² on both sides of a copper current collector (thickness: 15 μm). 2 A negative active material layer (thickness: 23 μm) was formed by coating with a loading amount, rolling, and drying in a vacuum oven at 130°C for 10 hours.
[0205] Charge and discharge were performed on the coin half cell manufactured above, and the discharge capacity, initial efficiency, and capacity retention rate were evaluated and listed in Table 2 below.
[0206] The 1st and 2nd cycles were charged and discharged at 0.1C, and from the 3rd cycle to the 300th cycle, the charging and discharging were performed at 1.0C. The process was terminated at the 300th discharge cycle.
[0207] Charging conditions: CC (constant current) / CV (constant voltage) (5mV / 0.005C current cut-off)
[0208] Discharge condition: CC (constant current) condition 1.5V
[0209] The discharge capacity (mAh) and initial efficiency (%) were derived from the results of a single charge and discharge cycle. Specifically, the initial efficiency (%) was derived by the following calculation.
[0210] Initial efficiency (%) = (Discharge capacity per cycle / Charge capacity per cycle) × 100
[0211] The capacity retention rates were each derived by the following calculations.
[0212] Capacity Retention Rate (%) = (299 Discharge Cycles Capacity / 1 Discharge Cycle Capacity) × 100
[0213] Discharge Capacity (mAh) Initial Efficiency (%) Lifespan Characteristics (%) Example 1 7891.398 Example 2 7791.296 Comparative Example 1 7891.292
[0214] Experimental Example 2: Verification and Evaluation of Gas Generation Amount
[0215] 20g of the cathode slurry prepared in Experimental Example 1 above was sealed in an aluminum pouch and stored, and the pouch containing the cathode slurry was stored in a 45℃ chamber for 7 days and the volume change was measured.
[0216] Specifically, the pouch was stored in a 45°C chamber, and the change in pouch volume was measured up to day 7. The volume change was measured by comparing the readings when the pouch was placed in a graduated cylinder filled with water versus when it was not. The increase in volume relative to the initial pouch volume was measured in ml, and the results are listed in Table 3 below.
[0217] Gas generation amount (ml) Examples 10~5 Examples 28~15 Comparative Example 120 or more
[0218] As can be seen from the experiment above, when controlling the amount of carbon coating layer deposited on porous carbon during the manufacture of a silicon carbon composite, the slope of the graph shape, in which the x-axis represents electrode density and the y-axis represents initial efficiency, can be satisfied between -50 and -10 depending on charging and discharging. It was found that the carbon coating layer in the silicon carbon composite effectively encases the silicon, thereby achieving high energy density and high capacity characteristics, while simultaneously being physically and electrically stable even at high electrode densities, which can improve lifespan characteristics and solve the problem of capacity development.
[0219] In addition, as can be seen from the evaluation of gas generation amount, it can be confirmed that Examples 1 and 2 according to the present application have a lower gas generation amount compared to Comparative Example 1, and from this, it can be seen that the problem of gas generation can also be solved when using the silicon carbon composite according to the present application.
Claims
1. A negative electrode active material comprising a silicon carbon composite, A cathode active material having a slope of -50 or greater and -10 or less on a graph showing the relationship between electrode density (x-axis) and initial efficiency (y-axis), after manufacturing a cathode containing the above cathode active material under multiple conditions with different electrode densities and measuring the initial efficiency for each of the above cathodes.
2. In Claim 1, The above silicon carbon composite comprises porous carbon; and silicon deposited on the porous carbon, and The above silicon carbon composite is a negative electrode active material that further includes a carbon coating layer.
3. In Claim 2, A negative electrode active material in which the carbon coating amount of the carbon coating layer is 5 parts by weight or more and 30 parts by weight or less based on 100 parts by weight of the silicon carbon composite.
4. In Claim 1, The specific surface area (BET) of the above silicon-carbon composite is 0.1 m 2 / g or more than 5 m 2 A negative electrode active material with a g or less.
5. In Claim 1, A negative electrode active material in which the silicon is 40 parts by weight or more and 60 parts by weight or less, based on 100 parts by weight of the silicon carbon composite.
6. In Claim 1, A negative electrode active material having an average particle size (D50) of 1 μm or more and 10 μm or less of the silicon carbon composite.
7. A negative electrode for a lithium secondary battery comprising: a negative current collector layer; and a negative active material layer provided on one or both sides of the negative current collector layer, A negative electrode for a lithium secondary battery, wherein the negative electrode active material layer comprises a negative electrode active material layer composition comprising a negative electrode active material according to any one of claims 1 to 6.
8. In Claim 7, The above negative electrode active material layer composition further comprises a carbon-based active material, for a negative electrode for a lithium secondary battery.
9. In Claim 8, A negative electrode for a lithium secondary battery, wherein the negative electrode active material comprises 50 parts by weight or less based on a total of 100 parts by weight of the negative electrode active material and the carbon-based active material.
10. In Claim 7, The above-mentioned negative electrode active material layer composition further comprises a negative electrode conductive material; and a negative electrode binder, for a negative electrode for a lithium secondary battery.
11. In Claim 7, A negative electrode for a lithium secondary battery having a rolled density of the above negative electrode active material layer of 0.9 g / cc or more and 1.3 g / cc or less.
12. Anode; Negative electrode for a lithium secondary battery according to claim 7; A separator provided between the anode and the cathode; and A lithium secondary battery containing an electrolyte.
13. A battery module comprising a lithium secondary battery according to claim 12.
14. A battery pack comprising a lithium secondary battery according to claim 12.
15. A battery pack comprising a battery module according to claim 13.