Recycled pulp compositions
A purified pulp composition with low chemical contaminants addresses the limitations of recycled pulp, enhancing its use in demanding applications by achieving a 1000X contamination reduction, ensuring mechanical integrity and safety.
Patent Information
- Application Number
- PCT/US2026/025941
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
The utilization of recycled pulp is limited due to high levels of chemical contaminants, which affect mechanical properties and safety in demanding applications, requiring a significant reduction in contamination to meet stringent quality standards.
A pulp composition comprising 85-100% post-consumer recycled pulp with low levels of specific chemical contaminants (e.g., glyphosphate, bisphenol-A, PCBs) to ensure high mechanical integrity and safety, achieved through purification processes.
The composition achieves a 1000X reduction in chemical contamination, enabling broader utilization in end markets like medical and hygiene products, maintaining mechanical properties and safety standards.
Smart Images

Figure IMGF000013_0001_TABLE 
Figure IMGF000029_0001_TABLE 
Figure IMGF000032_0001_TABLE
Abstract
Description
[0001] RECYCLED PULP COMPOSITIONS
[0002] FIELD OF THE INVENTION
[0003] The present invention generally relates to pulp compositions comprising high purity postconsumer recycled pulp.
[0004] BACKGROUND OF THE INVENTION
[0005] In the world today, hundreds of millions of tons of pulp are utilized on an annual basis. The pulps are generally produced from renewable resources. However, the utilization of virgin pulp may deplete natural resources and be a negative on energy, water, land use, etc., and increase production of greenhouse gases (GHG), primarily CO2, in the atmosphere.
[0006] Polysaccharides in fiber form are the basis of most pulps and include wood, cotton, rayon, etc. The use of recycled pulp has emerged as one solution to mitigate the issues associated with the end-of-hfe of virgin polysaccharides. Recovering and re-using polysaccharides diverts waste from landfills and reduces the demand for virgin materials.
[0007] The pulps may be used to produce various forms of paper, cardboards, etc. The pulp may be reclaimed as one of many forms and recycled into one of many forms including paper, cardboards, etc.
[0008] Today, in the US, the majority of reclaimed materials destined for recycling, including paper, cardboard, etc., are mixed into a single stream which is collected and processed by a material recovery facility (MRF). At the MRF, materials are sorted, washed, and packaged (e.g., in bales) for resale. Pulp-based materials can be sorted into individual materials.
[0009] However, the utilization of reclaimed pulp in recycling is currently limited due to contamination, which renders these less valuable compared to virgin pulp. A key enabler to increase the recycle rates and lowering the CO2 emissions is to reduce the contamination of recycled pulp to a level allowing broader utilization across more end markets, especially those involving demanding applications. Contamination potentially impacts macroscopic end-use performance, such as reduction in mechanical properties such as strength (i.e., tensile, burst, tear, etc.), elongation, absorbency, and impact and increased malodor and non-optimal color.
[0010] While contamination is problematic for all end market applications, demanding applications such as foods, hygiene, medical, etc., have even stricter requirements, especially on certain chemical contaminants or trace chemicals. The relevant chemical contaminants or trace chemicals may be grouped into various chemical classes depending on the chemical structure of the contaminants or trace chemicals. Non-limiting examples of these chemical classes ofcontaminants are PF As, heavy metals, pesticides, dioxins, furans, polychlorinated biphenyls (PCBs), phthalates, polycyclic aromatic hydrocarbons (PAHs), organotins, bisphenols, isothiazolins, glyphosphate, alkyl phenols, alkylphenol ethoxylates, aromatic amines, and flame retardants. In addition, the target levels of these contaminants or trace chemicals can be extremely low. For instance, the target levels may be on the order of parts per million (ppm), parts per billion (ppb), and parts per trillion (pptr), wherein the initial contaminated material may contain levels 1,000 times the targeted levels. Net, a l,000X reduction in chemical contamination is often required.
[0011] While the recycling of pulp through various cleaning processes is known, there remains a need for recycled pulp compositions, and compositions comprising recycled pulp compositions, that have minimum numbers and levels of contaminants, and that also have the necessary mechanical integrity or performance level of the pulp fibers that allow them to be used in various ways.
[0012] SUMMARY OF THE INVENTION
[0013] A pulp composition, comprising from about 85 wt% to about 100 wt% post-consumer recycled pulp fiber; and further comprising at least one of the following:
[0014] a. less than about 100 pg / kg of glyphosphate;
[0015] b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate;
[0016] c. less than 150 pg / kg of Bisphenol-A;
[0017] d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0018] e. less than 250 ng / kg of OCDD;
[0019] f. less than 5 ng / kg of OCDF;
[0020] g. less than 4 ng / kg of PCB 81 ;
[0021] h. less than 350 ng / kg of PCB 105;
[0022] i. less than 50 ng / kg of PCB 118;
[0023] j. less than 5,000 pg / kg of di-2ethylhexylphthalate;
[0024] k. less than 5,000 pg / kg of di-isononylphthalate;
[0025] l. less than 10 pg / kg of fluoranthene; and
[0026] m. less than 10 pg / kg of phenanthene;
[0027] as measured according to the Trace Chemicals Test Method.
[0028] Pulp Compositions
[0029] The pulp compositions of the present invention comprise recycled pulp produced from reclaimed pulp. The difference between recycled and reclaimed pulp is subtle. A reclaimed pulp isa non-virgin pulp that has been collected for potential recycling into a valuable end market. Recycled pulp is produced from the reclaimed pulp after it has been rendered acceptable for use in the end market. In cases wherein the reclaimed pulp can be used as-is in an acceptable end market, then the terms are interchangeable. While use of recycled pulp is known, the present inventive compositions may comprise high amounts of recycled pulp fiber, along with both a low number of contaminants and also low amounts of said contaminants when present Detailed herein are the ty pes of materials that may have numerous and high levels of contaminants and methods of purifying such materials. The purer materials may then make up a percentage, up to 100% in some embodiments, of the inventive compositions. In some embodiments, the purer inventive materials comprise post-consumer recycled pulp fiber; in other embodiments they comprise post-industrial recycled pulp fiber and in still other embodiments, the purer materials may be a combination of post-consumer and post-industrial recycled pulp fiber.
[0030] The inventive compositions may be characterized by the low number of contaminants present, or they may be characterized by the low amount of a particular contaminant if it is present. The inventive compositions may also be characterized by their performance in various fiber-based tests, such as water retention or strength, by their intensive properties, such as basis weight or density, their composition, such as lignin level, or other finished product characterizations.
[0031] Furthermore, the pulp compositions may be incorporated into various consumer products and package materials. Such inventions, for example, inventive sanitary tissue products and inventive packages, may contain low numbers and low7levels of contaminants while still exhibiting consumer-expected tactile feel and overall high performance.
[0032] DETAILED DESCRIPTION OF THE INVENTION
[0033] I. Definitions
[0034] As used herein, the term “pulp” refers to a fibrous composition comprising polysaccharides and may include materials originating from wood, cotton, rayon, etc. Wood pulp refers to pulp originating from a wood source.
[0035] As used herein, the term “pulp fiber” refers to the individual fibers that make-up the actual pulp. These fibers may be characterized by a range of geometric parameters including various diameters, lengths, and degree of entanglements and various polysaccharide chemistries.
[0036] As used herein, the term “paper” refers to a consolidation of pulp into a flat and relatively consistent material. The paper may contain additional additives such as binders and pigments. Paper may be further processed into other forms. Paper is typically sourced from wood pulp but cotton pulp papers are also known.■‘Fiber” and / or “Filament” as used herein means an elongate particulate having an apparent length greatly exceeding its apparent width, i.e., a length to diameter ratio of at least about 10. For purposes of the present invention, a “fiber” is an elongate particulate as described above that exhibits a length of less than 5.08 cm (2 in.) and a “filament” is an elongate particulate as described above that exhibits a length of greater than or equal to 5.08 cm (2 in.).
[0037] Fibers are typically considered discontinuous in nature. Non-limiting examples of fibers include wood pulp fibers and synthetic staple fibers such as polyester fibers.
[0038] In the present invention, “fiber” refers to papermaking fibers. Papermaking fibers useful in the present invention include cellulosic fibers commonly known as wood pulp fibers. Applicable wood pulps include chemical pulps, such as Kraft, sulfite, and sulfate pulps, as well as mechanical pulps including, for example, groundwood, thermomechanical pulp and chemically modified thermomechanical pulp. Chemical pulps, however, may be preferred since they impart a superior tactile sense of softness to tissue sheets made therefrom. Pulps derived from both deciduous trees (hereinafter, also referred to as "hardwood") and coniferous trees (hereinafter, also referred to as "softwood") may be utilized. The hardwood and softwood fibers can be blended, or alternatively, can be deposited in layers to provide a stratified web. U.S. Pat. No. 4,300,981 and U.S. Pat. No.
[0039] 3,994,771 are incorporated herein by reference for the purpose of disclosing layering of hardwood and softwood fibers. Also applicable to the present invention are fibers derived from recycled paper, which may contain any or all of the above categories as well as other non-fibrous materials such as fillers and adhesives used to facilitate the original papermaking.
[0040] In addition to the various wood pulp fibers, other fibers such as cotton linters, rayon, lyocell. trichomes, seed hairs, and bagasse can be used in this invention.
[0041] Other sources of cellulose in the form of fibers or that are capable of being spun into fibers include grasses and grain sources.
[0042] “Furnish” is an aqueous suspension of cellulose fibers that is used to make paper.
[0043] “Cellulosic pulp fiber furnish” is the mixture of fibers and other materials that are blended together in a water suspension to make paper or board.
[0044] “Dry fibrous structure” as used herein means that the fibrous structure exhibits a moisturecontent of less than 20% and / or less than 15% and / or less than 10% and / or less than 7% and / or less than 5% and / or less than 3% and / or less than 1% to 0% and or to greater than 0% by weight of the dry fibrous structure as measured according to the Water Content Test Method described herein. In one example, the dry fibrous structure of the present invention exhibits a moisture (water) content of from about 0.0001% to about 20% and / or from about 0.001% to about 15% and / or from about 0.001 % to about 12% and / or from about 0.001 % to about 10% and / or fromabout 0.001% to about 7% and / or from about 0.001% to about 5%. by weight of the dry fibrous structure.
[0045] As used herein, the term “Fibrous structure” refers to a structure that comprises one or more fibrous filaments and / or fibers. In one example, a fibrous structure according to the present invention means an orderly arrangement of filaments and / or fibers within a structure in order to perform a function. Non-limiting examples of fibrous structures of the present invention include paper, and absorbent pads (for example for diapers or feminine hygiene products).
[0046] As used herein, the term “virgin pulp” refers to pulp that has not been used to produce a material for a targeted end application. For example, virgin wood pulp is pulp that is produced from wood-based sources and has not been used for the intended purpose previously.
[0047] As used herein, the term “reclaimed pulp” refers to non-virgin pulp that has been collected for potential use in an end market. For example, reclaimed wood pulp is pulp that was originally virgin wood pulp but has already been used for an intended purpose such as paper in a 1st, 2nd, 3rd, etc., life.
[0048] As used herein, the term “recycled pulp” refers to reclaimed pulp that has been converted into a usable material with established end markets such as packaging. The recycled pulp may be purer than the reclaimed pulp fiber or may be identical except possibly in form. For example, recycled wood pulp is pulp that was reclaimed pulp and then rendered usable in the intended end market. Expanding further, recycled paper is sourced from reclaimed paper that is rendered acceptable for use as paper.
[0049] As used herein, the term “recycled pulp composition” refers to recycled pulp that may or may not contain virgin pulp or different types of recycled pulps at different concentrations.
[0050] As used herein, “pre-consumer” reclaimed pulp follows the ISO 5270 definition, that is, a descriptive term covering material diverted during a manufacturing process. This term excludes re-utilized material, such as rework, regrind or scrap that has been generated in a given process and is capable of being reclaimed within that same process. The term “post-industrial material” is sometimes used synonymously.
[0051] As used herein, “post-consumer” reclaimed pulp follows the ISO 5270 definition, that is, a descriptive term covering material, generated by the end-users of packages / products, that has fulfilled its intended purpose or can no longer be used (including material returned from within the distribution chain). The term “post-use” is sometimes used synonymously.
[0052] As used herein, the term “1stLife” refers to the first market use of a virgin material.
[0053] As used herein, the term “contaminant” refers to any undesirable material contained on or within the pulp. The term “chemical contaminant” refers to any undesirable chemical species onthe surface of the pulp or within the bulk of the pulp and comprises the molecular or elemental composition of the contaminant. The terms may be used interchangeably depending upon the intent. As used herein, the term “contamination"’ refers to the sum of all contaminants and the term “chemical contamination"’ refers to the sum of all chemical contaminants. The chemical contaminants are grouped in classes, which include chemical contaminants that have similar chemical structure. For example, As, Hg, and Cr are non-limiting chemical contaminants in the “heavy metals” classification. Each contaminant may have different chemical attributes, such as solubility and diffusivity in the pulp, and target levels depending upon concentration and end use market. The term “contaminant” may be used interchangeably herein with the term “trace chemical”, meaning a small amount of an undesirable material on or within a pulp fiber material.
[0054] As used herein, the term “surface contaminant” refers to a contaminant that is on the surface of the pulp fiber. Similarly, the term “surface chemical contaminant” refers to the molecular or elemental composition of the surface contaminant. The surface contaminant may be attached to the surface of the pulp fiber either loosely through physical attraction forces, or more strongly through polar or other forces. In general, a surface contaminant will have less than about 80% of its surface area embedded in the pulp fiber.
[0055] As used herein, the term “bulk contaminant” refers to a contaminant that is in the bulk of the pulp fiber. Similarly, the term “bulk chemical contaminant” refers to the molecular or elemental composition of the bulk contaminant. As used herein, a bulk contaminant will have more than about 95% of its surface area embedded in the pulp fiber.
[0056] As used herein, the term “surface contamination"’ and “surface chemical contamination” refers to the sum of all surface contaminants and all surface chemical contaminants, respectively.
[0057] As used herein, the term “bulk contamination” and "‘bulk chemical contamination” refers to the sum of all bulk contaminants and all bulk chemical contaminants, respectively.
[0058] As used herein, the term “total contamination” refers to the sum of the surface contamination and bulk contamination and the sum of all the surface chemical contamination and bulk chemical contamination, respectively.
[0059] As used herein, the term “permeable contaminant” refers to a chemical contaminant that is both soluble and diffusible in the pulp fiber.
[0060] As used herein, the term “impermeable contaminant” refers to a chemical contaminant that is either insoluble or non-diffusible or both in the pulp fiber.
[0061] As used herein, the term “permeable contamination” is the sum of all permeable contaminants and the term “impermeable contamination” is the sum of all impermeable contaminants. The sum of all permeable and impermeable contamination is the “chemicalcontamination’’ if described in molecular or elemental terms or just simply '‘the contamination” if described in general terms.
[0062] As used herein, the term “intentional contaminant” refers to a contaminant that is intentionally added by the supply chain for a specific purpose to benefit the producer, retailer, or consumer, but may not be desired in the recycled pulp fiber. Examples include print, adhesives for labels, pigments (such as TiCh), process additives (such as antioxidant (AO)), etc., that are necessary' for marketing, branding, processability7, and / or end use performance. As used herein, the term “intentional chemical contaminant” refers to an intentional contaminant described by its chemical composition. As used herein, the term “intentional contamination” refers to the sum of all intentional contaminants and the term “intentional chemical contamination” refers to the intentional contamination described by its chemical composition.
[0063] As used herein, the term “unintentional contaminant” refers to any contaminant not intentionally added. Examples include dirt and cross-contamination that is not intentionally added by the producer, retailer, or consumer. As used herein, the term "unintentional chemical contaminant” refers to an unintentional contaminant described by its chemical composition. As used herein, the term “unintentional contamination” refers to the sum of all unintentional contaminants and the term “unintentional chemical contamination” refers to the unintentional contamination described by its chemical composition.
[0064] As used herein, the term “degradation melting point” refers to the temperature at which the pulp begins to substantially degrade. The degradation may be determined through endothermic or exothermic processes.
[0065] As used herein, the term “limit of quantification” or “LOQ” refers to the lower detection limit for a given chemical contaminant as determined by the analytical methods disclosed in section IX. The LOQ is a function of the methods used and may vary from test method to test method. The LOQ used herein is specific to the method listed in section IX.
[0066] As used herein, the term “ppm” refers to mass parts per million, “ppb” refers to mass parts per billion, and “pptr” refers to mass parts per trillion.
[0067] “Sanitary' tissue product” as used herein means a soft, low density (i.e. < about 0.60 g / cm3) web useful as a wiping implement for post-urinary' and post-bowel movement cleaning (toilet tissue), for otorhinolaryngological discharges (facial tissue), and multi-functional absorbent and cleaning uses (absorbent towels). Non-limiting examples of suitable sanitary tissue products of the present invention include paper towels, bath tissue, facial tissue, napkins, baby wipes, adult wipes, wet wipes, cleaning wipes, polishing wipes, cosmetic wipes, car care wdpes, w'ipes that comprise an active agent for performing a particular function, cleaning substrates for use withimplements, such as a Swiffer* cleaning wipe / pad. The sanitary tissue product may be convolutedly wound upon itself about a core or without a core to form a sanitary tissue product roll.
[0068] “Basis Weight” as used herein is the weight per unit area of a sample reported in lbs / 3000 ft2or g / m2and is measured according to the Basis Weight Test Method described herein.
[0069] “Machine Direction” or “MD” as used herein means the direction parallel to the flow of The fibrous structure through the fibrous structure making machine and / or sanitary’ tissue product manufacturing equipment.
[0070] “Cross Machine Direction” or “CD” as used herein means the direction parallel to the width of the fibrous structure making machine and / or sanitary tissue product manufacturing equipment and perpendicular to the machine direction.
[0071] “Ply” as used herein means an individual, integral fibrous structure.
[0072] “Plies” as used herein means two or more individual, integral fibrous structures disposed in a substantially contiguous, face-to-face relationship with one another, forming a multi-ply fibrous structure and / or multi-ply sanitary tissue product. It is also contemplated that an individual, integral fibrous structure can effectively form a multi-ply fibrous structure, for example, by being folded on itself.
[0073] The term “natural fibers” or “pulp fiber” as used herein, refers to fibers which comprise cellulose-based fibers, bamboo based fibers, and the like. Natural fibers also refers to nonwoody fibers, such as cotton, abaca, kenaf, sabai grass, flax, esparto grass, straw, jute hemp, bagasse, milkweed floss fibers, and pineapple leaf fibers; and woody, wood, or pulp fibers such as those obtained from deciduous and coniferous trees, including softwood fibers, such as northern and southern softwood kraft fibers; hardwood fibers, such as eucalyptus, maple, birch, and aspen. Pulp fibers can be prepared in high-yield or low-yield forms and can be pulped in any known method, including kraft, sulfite, high-yield pulping methods and other know n pulping methods. The natural fibers of the present disclosure may be recycled natural fibers, virgin natural fibers or mixes thereof. Additionally, for good mechanical properties in natural fibers, it can be desirable that the natural fibers be relatively undamaged and largely unrefined or only lightly refined. The fibers can have a Canadian Standard Freeness of at least 200, more specifically at least 300, more specifically still at least 400, and most specifically at least 500.
[0074] The term “cellulose-based fibers,” as used herein, may include cellulose fibers such as wood fiber, cotton, regenerated cellulose fiber such as viscose, lyocell, rayon or Cuprammonium rayon, and high pulping yield fibers, unless specified differently. The term “cellulose-based fibers” also includes chemically treated natural fibers, such as mercerized pulps, chemically stiffened orcrosslinked fibers, or sulfonated fibers. Also included are mercerized natural fibers, regenerated natural cellulosic fibers, cellulose produced by microbes, the rayon process, cellulose dissolution and coagulation spinning processes, and other cellulosic material or cellulosic derivatives. Other cellulose-based fibers included are paper broke or recycled fibers and high yield fibers. High yield pulp fibers are those fibers produced by pulping processes providing a yield of about 65% or greater, more specifically about 75% or greater, and still more specifically about 75% to about 95%. Yield is the resulting amount of processed fibers expressed as a percentage of the initial wood mass. Such pulping processes include bleached chemithermomechanical pulp (BCTMP), chemithermomechanical pulp (CTMP), pressure / pressure thermomechanical pulp (PTMP), thermomechanical pulp (TMP), thermomechanical chemical pulp (TMCP), high yield sulfite pulps, and high yield Kraft pulps, all of which leave the resulting fibers with high levels of lignin but are still considered to be natural fibers. High yield fibers are well know n for their stiffness in both dry and wet states relative to typical chemically pulped fibers.
[0075] The term “non-recyclable material” as used herein, refers to contaminants or materials which are believed to be unsuitable for processing in the natural fiber recycling process. However, in alternative recycling streams, the materials provided with this designation may be recyclable.
[0076] The recycle pulp of the present invention may be used to make fibrous structures.
[0077] Non-limiting examples of processes for making fibrous structures include known wet-laid processes, such as wet-laid papermaking processes, and air-laid processes, such as air-laid papermaking processes. Wet-laid and / or air-laid papermaking processes typically include a step of preparing a composition comprising a plurality of fibers that are suspended in a medium, either wet, more specifically aqueous medium, or dry, more specifically gaseous medium, such as air. The aqueous medium used for wet-laid processes is oftentimes referred to as a fiber slurry. The fiber composition is then used to deposit a plurality of fibers onto a forming wire or belt such that an embry onic fibrous structure is formed, after which drying and / or bonding the fibers together results in a fibrous structure. Further processing the fibrous structure may be carried out such that a finished fibrous structure is formed. For example, in typical papermaking processes, the finished fibrous structure is the fibrous structure that is wound on the reel at the end of papermaking, and may subsequently be converted into a finished product, e.g., a sanitary tissue product.
[0078] Non-limiting examples of other known processes and / or unit operations for making fibrous structures include fabric crepe and / or belt crepe processes, ATMOS processes. NTT processes, through-air-dried processes, uncreped through-air-dried processes, and conventional wet press processes.The fibrous structures of the present invention may be homogeneous or may be layered in the direction normal to the machine direction. If layered, the fibrous structures may comprise at least two and / or at least three and / or at least four and / or at least five layers.
[0079] The fibrous structures of the present invention may be co-formed fibrous structures. “Coformed7’ as used herein means that the fibrous structure comprises a mixture of at least two different components wherein at least one of the components comprises a filament, such as a polypropylene filament, and at least one other component, different from the first component, comprises a solid additive, such as a fiber and / or a particulate. In one example, a co-formed fibrous structure comprises solid additives, such as fibers, such as wood pulp fibers and / or absorbent gel articles of manufacture and / or filler particles and / or particulate spot bonding powders and / or clays, and filaments, such as polypropylene filaments. In yet another example, a co-formed structure comprises those described in U.S. Patent No. 8,017,534 and U.S. Patent No. 7,674,467.
[0080] In one example, the fibrous structures of the present invention may comprise man-made fibers, natural fibers, and combinations thereof, and may or may not be biodegradable. Nonlimiting examples of man-made fibers include: rayon, which in turn includes but is not limited to viscose, lyocell and mixtures thereof; polyhydroxyalkanoates; polylactic acid; polyester; and mixtures thereof. Non-limiting examples of natural fibers include: pulp, cotton, wool, silk, jute, linen, ramie, hemp, flax, camel hair, kenaf, bamboo, and mixtures thereof. Non-thermoplastic fibers that are of use in the present invention are selected from the group consisting of: rayon, which in turn includes but is not limited to viscose, lyocell and mixtures thereof; pulp; cotton; wool; silk; jute; linen; ramie; hemp; flax; camel hair; kenaf; and mixtures thereof.
[0081] In one example, the fibrous structures of the present invention may be manufactured via fiber laying, fiber bonding, or combinations thereof. Fiber laying steps known in the art include, but are not limited to, spunlaying, meltblowing, carding, airlaying, wetlaying and combinations thereof, of the filaments and / or fibers comprising the fibrous structure. Fiber bonding steps known in the art include, but are not limited to, spunlacing (or hydroentangling), cold calendering, hot calendering, air thru bonding, chemical bonding, needle punching and combinations thereof. In one example, the dry fibrous structure comprises a fibrous structure selected from the group consisting of: air-laid fibrous structures, wet-laid fibrous structures, high loft nonwoven fibrous structures, needlepunched fibrous structures, hydroentangled fibrous structures, fiber tow fibrous structures, flocked fibrous structures, spunbond fibrous structures, carded fibrous structures, spunbond / meltblown fibrous structures, spunbond / meltblown / spunbond fibrous structures, meltblown fibrous structures, carded fibrous structures, coform fibrous structures, and combinations thereof.Other non-limiting examples of pulp composition characteristics suitable for use herein are described in U.S. Patent No. 11,252,966, the descriptions of which are incorporated herein by reference.
[0082] 11. Reclaimed Pulp
[0083] During pulp fiber’s lifecycle (from production through distribution, consumer utilization, and eventual reclaiming) contamination is introduced either intentionally or unintentionally.
[0084] Non-limiting examples of intentional contamination include surface print, labels, adhesives, optical brighteners, barrier plastics like polyethylene or polypropylene or waxes, binders, pigments (such as TiCh), fillers (such as CaCO3), process additives (such as antioxidant (AO), PF As such as FEP), etc. that are necessary for marketing, branding, processability, and / or end use performance. Non-limiting examples of unintentional contamination are dirt, crosscontamination, certain heavy metals, pesticides, dioxins, furans, PCBs. PF As such as PFOA, etc. Also, unintentional contamination can be produced from reactions involving intentional contaminants, such as the oxidation of pulp to dioxins, degradation of adhesives or print binders, etc. Further, oxidation of the pulp fiber during reclaiming will produce unintentional contamination. In addition, unintentional contamination may result from interaction with products. For example, packaging materials that contain cleaning mixtures (e.g., limonene, surfactants, etc.), food (e.g., various organics), etc., will potentially become contaminated with such products. Finally, unintentional contamination can enter the pulp fiber during production, e.g., contamination of a pulp fiber with reaction by-products, unreacted monomers, etc.
[0085] Pre-consumer reclaimed pulps generally have the lowest level of contamination due to their known composition and controlled history. It may include intentional contamination but because these are known and controlled, it is quite easy to find applications tolerating such known contaminants. In addition, pre-consumer reclaimed pulp tends to have low amounts of unintentional contamination due to the controlled history preventing external contamination.
[0086] Post-consumer reclaimed pulps are generally more contaminated than pre-consumer reclaimed pulps due to extensive cross-contamination from unknown sources resulting in high levels of unintentional contamination.
[0087] Surprisingly, recycled pulp in the present invention may allow the use of reclaimed pulp from pre-consumer and post-consumer sources in applications requiring low chemical contamination such as medical and hygiene. In addition, most recycled pulp customers desire purer materials beyond what is available today and the recycled pulp (along with the associated packages and products containing these) of the present invention meets this requirement.The reclaimed pulp may be in many macroscopic forms including but not limited to sheets, boards, rolls, etc.
[0088] The reclaimed pulp can be a second-life pulp (has been used only once before it entered the reclaimed pulp stream), third-life pulp (has been used twice before it entered the reclaimed pulp stream), or higher-life pulp fiber (has been used many times before it entered the reclaimed pulp stream).
[0089] The reclaimed pulp may comprise a regrind / edge- trim / in-plant waste pulp fiber or a postindustrial reclaimed pulp. The reclaimed pulp may comprise a post-industrial sheet or board.
[0090] The reclaimed pulp may comprise starch including but not limited to starches from various plants and chemically modified starches. The reclaimed pulp fiber may comprise polysaccharides, polylactic acid, polyhydroxyalkanoate, or chitin.
[0091] III. Contaminants and Contamination
[0092] The chemical contaminants in the contaminated pulp / contaminated pulp composition may be numerous and fall into various chemical classes. These chemical classes may be benign while others may be more problematic. The chemical contaminants of importance herein include but are not limited to pesticides, aldehydes, allergic fragrances, izioalines. alkylphenol ethoxylates, alkylphenols, bisphenols, dioxins, dioxin-like, furans, PCBs, organotins. metals, phthalates, polyaromatic hydrocarbons (PAHs), and PFAs (including but not limited to polymeric PF As). The concentration of these chemical contaminants are typically in the ppm, ppb, and pptr type of levels. The analytical methods used to measure these contaminants have lower sensitivity' limits. These limits are referred to as Limit of Quantification (LOQ).
[0093] Using the analytical methods disclosed in section IX Methods, the LOQs of the various contaminants may differ by orders of magnitude. For example, the LOQ of a typical pesticide is about 10 ppb; the LOQ of typical alkylphenol ethoxylate is about 50 ppb; the LOQ of a typical alkylphenol is about 5 ppb; the LOQ of bisphenol-A is about 5 ppb; the LOQ of typical dioxin is about 0.2 pptr; the LOQ of a typical furan is about 0.2 pptr; the LOQ of a typical PCB is about 5 pptr; the LOQ of atypical heavy metal is about 100 ppb; the LOQ of a typical organotin is about 300 pptr; the LOQ of typical phthalate is 50 ppb; the LOQ of a typical PAH is 1 ppb.
[0094] Several wood pulp based papers (a pulp composition) including two containing only virgin pulp and one containing post-consumer reclaimed pulp, were broadly classified for chemical contamination using the analytical methods disclosed in section IX Methods, as shown in TABLE 1. Note: To simplify the presentation of chemical contamination results, the concentration data is displayed in terms of multiples of LOQ instead of absolute weight fraction involving ppm, ppb, orpptr description. For example, if the contaminant concentration is 10 ppm and the LOQ is 1 ppm, then the concentration would be 10 X LOQ or just 10 displayed in the data tables.
[0095] TABLE 1
[0096] Chemical Contamination of Wood Pulp Based Papers
[0097] Reclaimed Post- Virgin
[0098] Consumer #1 #2 #1
[0099] LOQ xLOQ xLOQ xLOQ Pesticides
[0100] Diethyltoiuamide (DEETi 10 ppb <1 <1 2B.G Glyphosate 10 ppb <1 <1 12. C Alkylphenol ethoxylates
[0101] iso-Nanylphenolmonoethoxylate 50 ppb <1 <1 4.0 iso-Nonylphenoidiethoxylate 50 ppb <1 <1 6.2 iso-Nonylphenoltrlethoxylate 50 ppb <1 <1 7.0 iso-Nonylphenoltetsaethoxylate 50 ppb <1 <1 3.4 Bisphenols
[0102] Bisphenol A 5ppb <1 <1 32.0 Dioxins and dioxintike and PCB
[0103] 1,2,3,4,6,7,8-HpCDD 0.2 pptr <1 <1 145.5 OCDD 0.2 pptr <1 <1 1355.0 OCDF 0.2 pptr <1 <1 43.8
[0104] PCB 81 0.05 pptr <1 <1 87.8
[0105] PCB 105 5 pptr <1 <1 73.2
[0106] PCB 118 10 pptr <1 <1 58. S Phthalates
[0107] Di-2-ethylhexyl phthalate 50 ppb <1 <1 134.0 Diisoncnyl phthalate 50 ppb <1 <1 100.0
[0108] PAHs
[0109] Fluoranthene . Lspi: . <1 17.0
[0110]
[0111] Phenanthrene _ < 1.7 <1 13.0
[0112] As shown in the previous table, chemical contaminants of the types previously mentioned were generally not found in the papers sourced from virgin pulp compositions, which is likely representative of the broader virgin papers available today. However, high levels of the relevant chemical contaminants were found in the paper from reclaimed post-consumer pulp, again likely indicative of the broader reclaimed paper sources available today. For example, up to -1000 X LOQ was determined for OCDD and -100 X LOQ for the phthalates.
[0113] In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least one chemical contaminant and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least two chemical contaminants and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0114] In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least three chemical contaminants and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0115] In embodiments of the present invention, the pesticides comprise one or more of piperonyl butoxide, BAC, DEET, glyphosphate, and DDAC. In another embodiment of the present invention, the alkylphenol ethoxylates comprise one or more of iso-Nonylphenolmonoethoxylate, iso-Nonylphenoldiethoxylate, iso-Nonylphenoltriethoxylate, and iso-Nonylphenoltetraethoxylate. In yet another embodiment of the present invention, the alkyl phenols comprise one or more of iso-Nonylphenol, 4-tert-butylphenol, and 4-tert-Pentylphenol. In even yet another embodiment of the present invention, the bisphenols comprise bisphenol-A. In even yet another embodiment of the present invention, the dioxins comprise one or more of 1,2,3,6,7,8-HxCDD, 1.2.3.4.6.7.8-HpCDD, and OCDD. In even yet another embodiment of the present invention, the furans comprise OCDF. In even yet another embodiment of the present invention, the PCBs comprise one or more of PCB 77, PCB 81, PCB 126, PCB 105, PCB 1 14, PCB 118, PCB 123, PCB 156, and PCB 167. In event yet another embodiment of the present invention, the phthalates comprise one or more of di-2-propy I heptyl phthalate, disobutyl phthalate, dibutyl phthalate, di- 1 -ethylhexyl phthalate, and diisononyl phthalate. In even yet another embodiment of the present invention, the PAHs comprise one or more of acenaphthene, acenaphthylene, anthracene, benzo [a] anthracene, benzo [b]fluoroanthene, benzo[e]pyrene, benzo[g.h.i]perylene, chrysene, cyclopenta[c.d]pyrene, flyoroanthene, fluorene, naphthalene, phenanthrene, and pyrene. In even yet another embodiment of the present invention, the organotins comprise one or more of monobutylin, dibuty l tin. and dioctylin. In even yet another embodiment of the present invention, the PFAs comprise one or more of Perfluorooctanoic acid and Perfluorooctane sulfonic acid.
[0116] In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise glyphosphate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenolmonoethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoldiethoxylate. In embodiments of the present invention, the contaminants in thecontaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoltriethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoltetraethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise Bisphenol A. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise OCDD. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise OCDF. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 81. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 105. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 118. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise di-2-ethylhexyl phthalate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise di-isononyl phthalate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise fluoranthene. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise phenanthrene.
[0117] In general, the efficacy of the cleaning method of the present invention to remove a specific chemical contaminant is determined by the removal efficiency, defined as the difference in concentration of the chemical contaminant in the contaminated pulp / contaminated pulp composition and the concentration of the chemical contaminant in the purer pulp / purer pulp composition divided by the concentration of the chemical contaminant in contaminated pulp / contaminated pulp composition. However, the removal efficiency is somewhat insufficient due to the inability to determine any actual concentrations below the LOQ. For example, if a cleaning process reduces the contamination from 2 X LOQ to less than the LOQ, then the true removal efficiency could range anywhere between 50% and 100%, which is a significant difference. Thus, the removal efficiency is only completely accurate when the contaminated pulp / contaminated pulp composition and the purer pulp / purer pulp composition concentration are both above LOQ. For simplicity, if the purer pulp / purer pulp composition has a chemical contaminant concentration below LOQ, then removal efficiency is calculated by assuming the chemical contaminant concentration of the purer pulp / purer pulp composition is at the LOQ and the removal efficiency is considered a minimum value and designated with >. For the above example, the removalefficiency would be calculated as 100(2 X LOQ - 1 X LOQ) / (2 X LOQ) = 100(2-l) / 2 = 50%. Thus, the removal efficiency would be listed as > 50%. In certain cases, the purer pulp / purer pulp composition will have a higher level of a certain chemical contaminant than the initial contaminated pulp / contaminated pulp composition which contradicts the meaning of purer. This anomaly may be due to 1) measurement error / measurement variability. 2) contaminant hot spots and cold spots in the reclaimed pulp fiber, 3) external contamination during sampling, and 4) the purification process adds that specific contaminant. If this anomaly occurs consistently for a given chemical species for a given cleaning process, then such is more likely attributable to the purification process and should be more closely examined, but such was not generally the case for the cleaning processes of the present invention. Net, such isolated measurement anomalies were considered measurement error and not considered meaningful to the invention. In such cases, the removal efficiency is set to 0%.
[0118] In one embodiment, the removal efficiency of the DEET contaminant is > 70% wherein said DEET concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion. In another embodiment of the present invention, the removal efficiency of the DEET contaminant is > 85% wherein said DEET concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion.
[0119] In one embodiment of the present invention, the removal efficiency of the glyphosphate contaminant is > 50% wherein said glyphosphate concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion. In another embodiment of the present invention, the removal efficiency of the glyphosphate contaminant is > 90% wherein said glyphosphate concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per billion.
[0120] In one embodiment of the present invention, the removal efficiency of the isononylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and isononylphenoltetraethoxylate contaminant are all > 50% wherein said isononylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and isononylphenoltetraethoxylate concentration in the contaminated pulp / contaminated pulp composition is at least 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the iso-nonylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and iso-nonylphenoltetraethoxylate contaminant are all > 70% wherein said iso-nonylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and iso-nonylphenoltetraethoxylate concentration in the contaminated pulp / contaminated pulp composition is at least 50 parts per billion.In one embodiment of the present invention, the removal efficiency of the Bisphenol-A contaminant is > 50% wherein said Bisphenol-A concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per billion. In another embodiment of the present invention, the removal efficiency of the Bisphenol-A contaminant is > 95% wherein said Bisphenol-A concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per billion.
[0121] In one embodiment of the present invention, the removal efficiency of the 1,2, 3, 4, 6, 7, 8-HpCDD contaminant is > 50% wherein said 1,2,3,4,6,7.8-HpCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion. In another embodiment of the present invention, the removal efficiency of the 1,2,3,4,6,7,8-HpCDD contaminant is > 85% wherein said 1,2,3,4,6,7,8-HpCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion.
[0122] In one embodiment of the present invention, the removal efficiency of the OCDD contaminant is > 50% wherein said OCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion. In another embodiment of the present invention, the removal efficiency of the OCDD contaminant is > 85% wherein said OCDD concentration in the contaminated pulp / contaminated pulp composition is at least 0.2 parts per trillion.
[0123] In one embodiment of the present invention, the removal efficiency of the PCB 81 contaminant is > 50% wherein said PCB 81 concentration in the contaminated pulp / contaminated pulp composition is at least 0.05 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 81 contaminant is > 85% wherein said PCB 81 concentration in the contaminated pulp / contaminated pulp composition is at least 0.05 parts per trillion.
[0124] In one embodiment of the present invention, the removal efficiency of the PCB 105 contaminant is > 50% wherein said PCB 105 concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 105 contaminant is > 85% wherein said PCB 105 concentration in the contaminated pulp / contaminated pulp composition is at least 5 parts per trillion.
[0125] In one embodiment of the present invention, the removal efficiency of the PCB 118 contaminant is > 50% wherein said PCB 118 concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 118 contaminant is > 85% wherein said PCB 118 concentration in the contaminated pulp / contaminated pulp composition is at least 10 parts per trillion.In embodiments of the present invention, the removal efficiency of the Di-2-ethylhexyl phthalate contaminant is > 50% wherein said Di-2-ethylhexyl phthalate concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the Di-2-ethylhexyl phthalate contaminant is > 85% wherein said Di-2-ethylhexyl phthalate concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion.
[0126] In embodiments of the present invention, the removal efficiency of the Di-isononyl phthalate contaminant is > 50% wherein said Di-isononyl phthalate contaminant concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the Di-isononyl phthalate contaminant is > 85% wherein said Di-isononyl phthalate contaminant concentration in the contaminated pulp / contaminated pulp composition is at least about 50 parts per billion.
[0127] In embodiments of the present invention, the removal efficiency of the fluoranthene contaminant is > 50% wherein said fluoranthene concentration in the contaminated pulp / contaminated pulp composition is at least about 1 parts per billion. In another embodiment of the present invention, the removal efficiency of the fluoranthene contaminant is > 85% wherein said fluoranthene concentration in the contaminated pulp / contaminated pulp composition is at least about 1 parts per billion.
[0128] In embodiments of the present invention, the removal efficiency of the phenanthrene contaminant is > 50% wherein said phenanthrene concentration in th contaminated pulp / contaminated pulp composition is at least about 1 parts per billion. In another embodiment of the present invention, the removal efficiency of the phenanthrene contaminant is > 85% wherein said phenanthrene concentration in the contaminated pulp / contaminated pulp composition is at least about 1 parts per billion.
[0129] In embodiments of the present invention, the removal efficiency of the Perfluorooctanoic acid contaminant is > 50% wherein said Perfluorooctanoic acid concentration in the contaminated pulp / contaminated pulp composition is at least LOQ. In embodiments of the present invention, the removal efficiency of the Perfluorooctane sulfonic acid contaminant is > 50% wherein said Perfluorooctane sulfonic acid concentration in the contaminated pulp / contaminated pulp composition is at least LOQ.
[0130] In general, bulk contamination will not be appreciably removed by simple aqueous surface washing approaches of the prior art. Permeable bulk contamination can be removed by diffusion mechanisms through gradients in chemical potential, whereas bulk impermeable contamination isessentially trapped by the bulk pulp fiber, and methods to free the trapped contaminant dissolution / disintegration of the pulp fiber.
[0131] IV. Surface Purification Methods
[0132] Surface purification methods reduce surface contamination. One example of a purification process may include, but is not limited to, surface washing with a surface washing fluid that is typically water based. The reclaimed pulp fiber will generally be in the form of board, loose or compacted fibers, loose or compacted flexible packages, loose or compacted rigids, loose or compacted non-wovens, loose or compacted fibers, etc. which will be difficult to surface wash due to excessive overall size. Hence, prior to surface washing, a granulation or shredding step is preferred. The surface washing will typically include mechanical agitation to loosen surface dirt and other contaminants to allow physical removal and transfer to the washing fluid wherein the dirt or other contaminants may or may not solubilize.
[0133] Surface washing technologies are available extensively on the market for cellulosic-based reclaimed pulp fibers.
[0134] V. Bulk Purification
[0135] In general, bulk contamination will not be appreciably reduced by simple aqueous surface washing.
[0136] One example of a purification process may include, but is not limited to, extraction, which may be a preferred bulk purification method for removing permeable contaminants. Extraction involves the use of a purification solvent to remove bulk permeable contaminants through creation of a chemical potential gradient between the reclaimed pulp fiber and the solvent. The rate of permeable chemical contaminant removal will depend upon the diffusivity and solubility’ of the contaminant in the pulp fiber under the conditions created in the process. For high molecular weight pulp fibers, the diffusivity of large molecules indicative of chemical contaminants is quite low, especially in the solid state of the pulp fiber. In addition, the solubility’ may be limited due to the high MW of the reclaimed pulp fiber and lack of enthalpic mixing. Thus, the time required to remove permeable contaminants through diffusion mechanisms can be quite long and not conducive to economically viable processes at commercial scale. Methods to resolve these time scale limitations include 1). increased diffusivity through elevated temperature and / or pulp fiber relaxation through solvent swelling, 2). decrease of diffusion path length through increased surface area to volume ratio of the reclaimed pulp fiber exposed to the solvent, 3) increased convective transport of the contaminant through the pulp fiber / solvent interface by: increased solubility of thecontaminant in the solvent, increased partitioning of the contaminant within the solvent relative to the pulp fiber; increased convection around the pulp fiber / solvent interface, and increased solvent sink relative to pulp fiber sink. The solubility of the bulk purification solvent in the pulp fiber can be increased by operating the extraction at high pressures especially at. near, or above the critical pressure.
[0137] It is important for the extraction method to be scalable to large volumes at low cost. Hence, the time required for extraction should be low to allow for such scalability. In embodiments of the present invention, the total time for extraction is less than about 6 hours, preferably less than about 4 hours, more preferably less than about 2 hours, and even more preferably less than about 1 hour. If the extraction is completed in stages, then the time per stage may be less than this range but the overall time will still fall within these times.
[0138] Extractions may take place above, near, at, or below the degradation or primary melting point (whichever is lower) of the reclaimed pulp fiber. Extractions generally occur in a two-phase system involving a solvent-rich phase and a pulp fiber-rich phase. Leaching extractions are a subset of extractions typically involving a liquid state for the solvent-rich phase and a solid state for the pulp fiber-rich phase. Liquid-liquid extractions are a subset of extractions typically involving two liquid states. In an embodiment of the present invention, the extraction is leaching.
[0139] In leaching processes, the reclaimed pulp fiber may be contacted with excessive solvent during every stage and every time of the process. Such leaching processes are called flooded leaching processes. In flooded leaching processes, the mass of leaching solvent to mass of reclaimed pulp fiber exposed to the solvent at every point in time and in every stage of the process is preferably equal to or greater than about 5: 1. In certain flooded leaching processes, the solvent is rapidly stirred such that the reclaimed pulp fiber is suspended in the solvent even when the density of the reclaimed pulp fiber is greater than the solvent. Such flooded leaching processes 1) ensure complete contact between the surface of the reclaimed pulp fiber and the leaching solvent and 2) lower the mass transfer resistance within the solvent boundary layer around the reclaimed pulp fiber surface due to the convective motion. Beyond stirring, similar reduced boundary layer may be achieved in flooded leaching processes by allowing the reclaimed pulp fiber to settle through the solvent by density gradient. Examples of flooded leaching processes include stirred tanks of the continuous, semi-continuous, and batch types. Additional examples of flooded leaching processes include settling tanks wherein the reclaimed pulp fiber is allowed to settle out or through the solvent that is filled inside a tank or other vessel.
[0140] In leaching processes, the solvent may be contacted with excessive pulp fiber during every stage and every time of the process. Such leaching processes are called packed leaching processes.In packed leaching processes of the current invention, the mass of leaching solvent to mass of reclaimed pulp fiber exposed to the solvent at every point in time and in every stage of the process is preferably equal to or less than about 5:1. In certain packed leaching processes, the solvent is flowed through a packed column or bed of pulp fiber. Such packed leaching processes provide efficient means for removing contaminated solvent and ensuring optimal concentration gradient. Examples of packed leaching include but are not limited due flow through packed beds, percolation extractors, screw-based extractors, Hildebrandt extractors, etc.
[0141] In some embodiments, a purification process may include an extraction that comprises flooded leaching. In embodiments of the present invention, the extraction may comprise packed leaching. In embodiments of the present invention, the extraction comprises a combination of flooded and packed leaching.
[0142] For leaching processes of the current invention, it may be beneficial to select a leaching solvent and operating temperature and pressure such that the leaching solvent is at its boiling point during the extraction. Such designs allow the solvent to be continuously refluxed, which may enable locally high concentration gradients as the refluxed solvent contacts the reclaimed pulp fiber. In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the bulk purification is about atmospheric. In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the leaching is about atmospheric, and the leaching solvent is at or near the normal boiling point. For cellulosics, preferred leaching solvents for flooded leaching have boiling points in the 2°C to 90°C range. Examples of such solvents are THF, di-ethyl ether, hexanes, acetone, ethanol, methanol, propanol, iso-propanol, MEK. and ethyl acetate or blends thereof. The leaching solvents may contain minor amounts of water (< ~25 wt% water) that are residual within the cellulosic reclaimed pulp fiber or intentionally added to any of the aforementioned solvents. In embodiments of the present invention, said leaching solvent may have a normal boiling point between 20°C and 90°C. In embodiments of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the leaching temperature is at or near the boiling point. In another embodiment of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the purification temperature is at or near the boiling point and the pressure is at or near atmospheric. The pressure may also be between about 0.5 atm and higher. In yet another embodiment of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the pressure is above atmospheric but below 1,000 atm. The leaching solvent may also have a boiling point above the leaching temperature. In even yet another embodiment of the present invention, the leaching solvent has a normal boilingpoint above the leaching temperature. In another embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is ethyl acetate; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 0.5 atm and about 1,000 atm. In another embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is hexanes; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 0.5 atm and about 1,000 atm.
[0143] Leaching solvents with a normal boiling point below the leaching temperature are also preferred due to the elevated leaching pressures. In embodiments of the present invention, the leaching solvent has a normal boiling point below the leaching temperature. In another embodiment of the present invention, the leaching solvent is di-methyl ether (DME). In an embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is DME; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 2 atm and about 1,000 atm.
[0144] Preferred leaching solvents include solvents that have higher affinity for the chemical contaminants than for the reclaimed pulp fiber. Solvents with high affinity for the chemical contaminants include but are not limited to diethyl ether, MEK, ethyl acetate, THF, acetone, methylene chloride, iso-propanol, propanol, ethanol, and methanol. Other oxygenated and polar hydrocarbon solvents likely have similar desired affinity. Solvents lacking such characteristics can still be used, but higher solvent to pulp fiber ratios may be required. It is preferred that the solvent should not significantly dissolve the reclaimed pulp fiber at the temperature and pressure of the process (< ~5wt% may be dissolved). The solvent may slightly swell the reclaimed pulp fiber but not enough to cause agglomeration or coalescence. The solvents may contain water for various functional or non-functional reasons (below ~25wt%).
[0145] In embodiments of the present invention, said leaching solvent is selected from the group comprising hydrocarbons. In another embodiment of the present invention, said leaching solvent is selected from the group comprising aliphatic hydrocarbons. In even another embodiment of the present invention, said leaching solvent is selected from the group comprising aromatic hydrocarbons. In even yet another embodiment of the present invention, said leaching solvent is selected from the group comprising alkanes.
[0146] In embodiments of the present invention, said leaching solvent is selected from the group comprising methane, ethane, propane, normal butane, isobutane, normal pentane, isopentane, neopentane, hexanes (normal hexane, isohexane, neohexane, heptanes), octanes, or mixtures thereof.The temperature may be changed during the course of the extraction process but is generally consistent within a given stage of a unit operation. The pressure may be changed to vary solubility of the solvent in the reclaimed pulp fiber or to increase solubility of the chemical contaminant within the solvent.
[0147] A leaching extraction process may take place in stages and be combined with additional leaching extraction processes of other types not discussed in this application. The same is true for liquid-liquid extraction processes. In addition, liquid-liquid process may be combined with leaching process in various stages to form a given purification process. In embodiments of the present invention, the number of stages is one or more than one. In another embodiment of the present invention, the number of liquid-liquid stages is more than one. In yet another embodiment of the present invention, the number of leaching stages is more than one. In still yet another embodiment of the present invention, the number of liquid-liquid stages is one or more and the number of leaching stages is one or more. A single stirred tank reactor will achieve a certain removal efficiency. The efficiency can be improved by having multiple stirred tank reactors in series wherein the reclaimed pulp fiber from the 1ststage is predominately separated from the 1ststage purification solvent and this 1ststage pulp fiber is used in the 2ndstage with fresh purification solvent. This is repeated for each additional stage. This method improves the removal efficiency at the expense of additional reactors and complexity but maintains the overall time, throughput, and solvent utilization. Practically speaking, the number of reactor stages can be anywhere from 1 to ~ 10 for stirred tank systems. If a larger number of stages are needed, then a continuous counter-current method may be used.
[0148] While not wishing to be bound by theory, the theoretical maximum contaminant removal capacity for a leaching process is based upon the thermodynamic equilibrium / partitioning of the chemical contaminants between the reclaimed pulp fiber and leaching solvent at the temperature and pressure of the process. Thermodynamic equilibrium may not be achieved due to kinetic limitations in the leaching process. This is true for the complete leaching process and is also true for each leaching stage. A higher leaching solvent to reclaimed pulp fiber mass ratio will drive both thermodynamics and kinetics in favor of purification at the expense of greater solvent consumption and greater extraction process size, which equals greater cost. Thus, a balance must be found between these important design and operational variables for the targeted chemical contaminant removal efficiency. In addition, the contaminated solvent from any stage may be used “as-is” as the solvent for another stage. Contaminated solvent at any point in the process may be renewed through known methods of distillation, filtration, ion-exchange, etc., or combinations.Another important kinetic driver is surface area to volume ratio of the reclaimed pulp fiber within and exposed to the leaching solvent. In general, the time required to extract a chemical contaminant from a reclaimed pulp fiber is a strong function of the diffusion pathlength within the reclaimed pulp fiber. The diffusion pathlength is indirectly proportional to the surface area to volume ratio of the geometrical form of the reclaimed pulp fiber and the ability to access the surface area with leaching solvent. Hence, a higher surface area to volume ratio will produce a reduced diffusion pathlength and faster diffusion kinetics. For leaching processes, a high surface area to volume ratio is a critical parameter for quick and efficient contaminant removal both surface and bulk.
[0149] A known means for increasing the effective mass transfer through a given surface area to volume ratio and given set of conditions at the reclaimed pulp fiber solvent interface is through applying energy to the reclaimed pulp fiber such as but not limited to vibrational in the form of ultrasonic energy and / or micro wave.
[0150] Following the bulk purification involving extraction, the pulp fiber may be devolatilized to produce a purer recycled pulp fiber. The contaminated solvent will contain a small amount of dissolved purer recycled pulp fiber, the extracted contaminants, and the pure leaching solvent. There are many ways to recover the purer recycled pulp fiber and bulk purification solvent independent of the extracted contaminants.
[0151] In general, a small amount of reclaimed pulp fiber may dissolve into the leaching solvent regardless of process type or solvent. In particular, low molecular weight waxes are particularly prone to solubilization into the extracting solvent. These may become problematic in distillationbased recovery’ of the purified solvent due to deposition of the waxes on process equipment. Methods are known to reduce this tendency. One such method is to lower the temperature of the contaminated solvent to below the cloud point to precipitate the pulp fiber or wax phase followed by filtration. Unlike the reclaimed pulp fiber, the residual pulp fiber or waxes resulting pulp fiber from the precipitation from the contaminated solvent may contain significant chemical contamination.
[0152] Distillation and / or flash evaporation of the contaminated bulk purification solvent may be used to regenerate the solvent for re-use in the various extraction operations. However, distillation may not be economically feasible on-going considering the high solvent volume utilized in the present invention. In addition, because the chemical contaminants of interest in this invention are extremely low- in concentration, the concentration of these chemical contaminants in the contaminated solvent may be correspondingly low or even lower. Thus, a preferred method to purify the contaminated solvent is through direct removal of the contaminants without volatilizingthe bulk solvent phase. Such methods include precipitation, ion exchange, adsorption / absorption methods, etc. Non-limiting examples include passing the contaminated solvent through a bed of activated carbon or alumina. This method can be used alone or in combination with distillation to achieve the right level of purification at the right energy consumption. In addition, the contaminated solvent from any stage may be used ”as-is“ as the solvent for another stage. Contaminated solvent at any point in the process may be renewed through known methods of distillation, filtration, ion-exchange, etc., or combinations.
[0153] The purer recycled pulp fiber may contain small amounts of the solvent in either physically adsorbed or bulk absorbed form. The concentration of the solvent in the purer recycled pulp fiber may be reduced by devolatilization techniques. In an embodiment of the present invention, said purer recycled pulp fiber is devolatilized to a content of <1 wt% solvent. In an embodiment of the present invention, said purer recycled pulp fiber is devolatilized to a content of < about 50 ppm solvent.
[0154] Multi-staged stirred tank flooded extractors operating at the boiling point of a polar organic leaching solvent provide improvements in chemical contaminant removal over existing methods. For example (as shown in Examples 1 and 2), a flooded leaching process of the present invention provided targeted contaminant removal efficiencies greater than about 50%.
[0155] In embodiments of the present invention, the leaching solvent is ethyl acetate. In yet another embodiment of the present invention, the leaching solvent is ethyl acetate and the process pressure is about atmospheric pressure. In another embodiment of the present invention, said bulk purification comprises flooded leaching in a stirred tank conducted at about 77.1°C and about atmospheric pressure with a leaching solvent comprising ethyl acetate.
[0156] In embodiments of the present invention, the leaching solvent is acetone. In yet another embodiment of the present invention, the leaching solvent is acetone and the process pressure is about atmospheric pressure. In another embodiment of the present invention, said bulk purification comprises flooded leaching in a stirred tank conducted at about 56.1°C and about atmospheric pressure with a leaching solvent comprising acetone.
[0157] In another embodiment of the present invention (Example 1 and Tables), a bulk purification of a reclaimed pulp fiber involving recycled cellulosic paperboard comprises flooded leaching in a stirred tank involving 4 stages conducted at about 77.1°C and about atmospheric pressure with a leaching solvent comprising ethyl acetate; wherein the ethyl acetate to first pulp fiber mass ratio is ~ 10: 1 per stage for a leaching time of ~ 30 minutes per stage for a total ethyl acetate to recycled pulp fiber ratio of about 40: 1 and a total leaching time of about 120 minutes; wherein the % removal of the pesticides, DEET and glyphosphate, is 52.7 and > 86.7%, the alkylphenolethoxylates,isononylphenoldi ethoxy late and isononylphenoltriethoxylate, is > 94.6% and > 96.2%, the alkylphenols, isononylphenol and 4-tert-pentylphenol, is > 78.3% and 80.8%, the bisphenol A is > 98.7%, the dioxins, 1,2, 3, 4, 6, 7, 8 -HpCDD and OCDD, is 74.3% and 84.3%, the OCDF is 87.1%, the PCBs, PCB 105 and PCB 118, is 89.4% and 89.5%, the organotins, dimethyltin and trimethyltin, is 98.4% and 99.5%, the phthalates, Di-2-ethylhexylphthalate and diisononylphthalate, is 98.1% and 94.0%, and the PAHs, fluoranthene and phenanthrene, is >94.1% and 86.9% wherein the initial concentration of these contaminants in the reclaimed pulp fiber are above LOQ.
[0158] In another embodiment of the present invention (Example 2 and Tables), a bulk purification of a reclaimed pulp fiber involving a different recycled paperboard comprises flooded leaching in a stirred tank involving 4 stages conducted at about 77.1 °C and about atmospheric pressure with a leaching solvent comprising ethyl acetate; wherein the ethyl acetate to first pulp fiber mass ratio is - 10:1 per stage for a leaching time of- 30 minutes per stage for a total ethyl acetate to reclaimed pulp fiber ratio of about 40: 1 and a total leaching time of about 120 minutes; wherein the % removal of the pesticides, DEET, is > 47.4%, the alkylphenol, 4-tert-pentylphenol, is > 70.6%, the dioxins, 1,2, 3, 4, 6, 7, 8 -HpCDD and OCDD, is 59.4% and 67.5%, the OCDF is 67.3%, the PCBs, PCB 105 and PCB 118, is 78.9% and 79.6% wherein the initial concentration of these contaminants in the reclaimed pulp fiber are significantly above LOQ. The mechanical properties of paperboard produced from the purer cellulosic recycled pulp fiber are not significantly reduced compared to similar paperboard produced from the reclaimed pulp fiber (% decrease in properties < 10%).
[0159] Following the flooded leaching, the purer recycled pulp fiber may be physically wetted with the residual solvent and potentially contain a small amount of absorbed solvent. As discussed earlier, there are many ways to recover the purer recycled pulp fiber and bulk purification solvent independent of the extracted contaminants. The purer recycled pulp fiber can be dried and devolatilized by many known commercial means. One method is through cyclonic dry ing. Another method is through melt extrusion with a devolatilization section. In embodiments of the present invention, the purer recycled pulp fiber is processed to reduce the leaching solvent to below about lwt% in the reclaimed pulp fiber and more preferably less than about 50 ppm. The contaminated solvent can be cleaned with known methods of distillation, ion exchange, filtration, etc. The resulting devolatilized reclaimed pulp fiber may be used as it or may be further processed into other forms including pellets via various processes.VI. Recycled Pulp fiber
[0160] The purer recycled pulp fiber produced from the reclaimed pulp fiber will have a lower level of contamination relative to the reclaimed pulp fiber. The purer recycled pulp fiber from the bulk purification step may be further processed to produce other forms.
[0161] Without wishing to be bound by theory, the inventors have unexpectedly found the purer recycled pulp fiber of the present invention may not only exhibit a lower level of trace chemicals, but also may exhibit improved levels of pulp performance as measured by the purer recycle pulp fiber properties of Water Retention Value, Fines Level (Lw), Handsheet Tensile Strength, Handsheet Zero Span Tensile, and combinations of these performance factors as well. The purer recycled pulp fiber of the present invention may be unexpectedly rejuvenated in these pulp performance factors as well as exhibiting low levels of trace chemicals.
[0162] VI. EXAMPLES
[0163] In general, the established methods for purifying / cleaning reclaimed pulp fiber including water washing are currently not able to sufficiently remove chemical contaminants. Net, there is an unmet need for a cleaning technology that is capable of more completely removing chemical contamination sufficient for highly contaminated sources and for any market desiring purer recycled materials. In addition, there is an unmet need for recycled compositions that do not have, or have very low levels of, chemical contaminations.
[0164] COMPARATIVE EXAMPLE - Purification Method Using Traditional Water Washing of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Water-Washed Post-Consumer Recycled Pulp Composition
[0165] 2,500 grams of de-ionized water was added to a 5L stirred round bottom flask. In addition, ImL of Triton X=100 surfactant was added to the water. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanical stirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the water to ~80°C) in about 5 minutes. After reaching ~80°C, the heat input was lowered to maintain a constant temperature of ~80°C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Paper was cut into 1 cm X 1 cm squares. The -250 grams of the cut Reclaimed Post-Consumer Paper was added to the round bottom flask which contained the hot water / surfactant solution. The washing was continued for -30 minutes. The stirring was terminated, and the heat was removed. The water solution was decanted from the mixture of solids and liquids. This completed washing step #1. An additional 2,500 grams of preheated water / Triton X-100 solution was added to the paperboard in the 5L round bottom to complete a second washingstep. Stirring was started at 400 to 500 rpm while heating was applied sufficient to achieve ~80°C. The time to reach 80°C after the addition of the fresh-water solution to the paperboard was ~5 minutes. The 2nd washing continued for a total of ~30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. This completed washing step #2. An additional 2,500 grams of preheated water / Triton X-100 solution was added to the paperboard in the 5L round bottom. Stirring was started at 400 to 500 rpm while heating w as applied sufficient to achieve 80°C. The time to reach ~80°C after the addition of fresh-water solution w as -5 minutes. This washing step continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. This completed washing step #3. An additional 1,000 grams of preheated fresh w ater / Triton X-100 solution was added to the paperboard in the 5L round bottom to complete a fourth washing step. Stirring was started at 400 to 500 rpm w hile heating w as applied sufficient to achieve ~80°C in the w ater solution. The time to reach ~80°C after the addition of fresh-water solution was ~5 minutes. The 4th washing continued for a total of ~30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. The paperboard contained a small amount of contaminated w ater solution within the porosity of the paperboard. This wet paperboard was placed in a filter funnel with 60 mesh grating to further remove residual water solution via gravity. The paperboard was then completely dried of contaminated water solution at room temperature over-night to produce the purer pulp composition. The washing solution to pulp composition ratio per stage was -10:1 for four stages giving a total washing solution to pulp composition ratio of -40:1. The washing time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The contaminated pulp composition represented by Reclaimed Post-Consumer Pulp and the resulting purer pulp composition represented by the Recycled Post-Consumer Pulp discussed above was analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table 2. For the contaminants DEET, glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, and diisononylphthalate, the % removal was > 96.4%, 44.2%, 35.0%, 35.5%, 40.0%, 17.6%. 72.5%. 0.0%, 0.0%, 0.0%, 0.0%, 0.0%, 0.0%, 14.9%, and 10.0% respectively, which was indicative of generally poor contaminant removal especially for the dioxins, pcbs, and phthalates.The pulp before and after the purification was characterized for water retention value. The water wash resulted in a 10.4% reduction of water-retention value which may be indicative of increased homification.
[0166] The pulp before and after the purification were processed into handsheets following Tappi T205 and then evaluated for tensile properties and chemical composition. The tensile strength for the handsheets after purification was reduced by about 11 % possibly due to increased homification. The washing process removed about 6.5% ash but didn’t significantly remove lignin from the pulp fibers.
[0167] TABLE 2
[0168] Purification Method Using Traditional Water Washing of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Water-Washed Post-Consumer Recycled Pulp Composition
[0169] Reclaimed Post-Consumer Pulp Composition Before After 1 , ~
[0170] „ : % Removed Purification Purification 1
[0171] LOQ xLOQ xLOQ
[0172] Pesticides : 1 Diethyitoluamide (DEET) 10 pph 28.0 i <1 ( > 96.4% Glyphosate _ 10 ppb 12.0 i 6.7 | 44.2% Alkylphenol ethoxylates
[0173] iso-Nonylphenolrrionoethoxylate 50 ppb 40 : 2,6 j 35.0% iso-Nonylphenoldiethoxylate SO ppb 6.2 : 4.0 j 35.5% iso-Nonylphenoltriethoxylate 50 ppb 7 0 4.2 40.0% iso-hiDnylphenoltetrsethoxylate SO spb 3.4 i 2.8 | 17.6% Bisphenols . i . 1.
[0174] SisphenolA S ppb 32.0 : 8.8 [ 72.5%
[0175] Dioxins and dloxinlike and PCB
[0176] 1,2,3,4,6,7,8-HpCDD _ 0 2 pptr _ 145 5 _ 163.0 _ 1 0 0%
[0177] bcDD . 0.2ppt' . 1SS5.0. i .1445.0 [ .0.0% .
[0178] OCDF . 0.2 pptr 43.8 i 47.7 0.5%
[0179] PCB 81 0 05 pptr 87. S i 92.8 | C 0%
[0180] PCB 105 5 pptr 78.2 i 87.2 | 0.0%
[0181] PCB 118 10 pptr •38.9 i 83.2 | 0.9% Phthalates ! |
[0182] Di-2-ethylhexy! phthalate 50 ppb 134.0 114.0 | 14.9% Diisononyf phthalate 50 ppb 100.0 i 90.0 I 10.0% Polycyclic aromatic hydrocarbons (PAH)
[0183] Fluoranthene 1 ppb 17.0 dnt n.a.
[0184] Phenanthrene 1 ppb 13.0 i dnt i n.a.
[0185] | % increase Water Retention Value (g / g) 1.25 <7-0,1 ; 1.12 <7- 0.01 ; -10.4%
[0186] FQA Fines Level (%) 9.4 + / - 0.0 ; 10 1+ / - 0.2 ; 7 4% Handsheet Tensile Strength (kN / m) 1.8 + / - 0.1 i 1.6+ / -0.1 i -11.1% Handsheet Zero Span Tensile Strength (icg-f > 8.41 + / - 0.32 i 8.20 + / - 0.34 i -2.5%
[0187] Compositional Information wt% ; % Removed _ Ash<%j _ at T / ' %<%
[0188] Klason Lignin (%) 14.2 + / - 0.1 i 14.3 + / - 0.3 i -0.7%
[0189] Acid soluble Lignin (%) 0.9 + / - 0.0 i 0.9+ / - 0.1 i 0.0%
[0190] % Lignin Level 15.2+ / -0.1 i 15.2+ / - 0.3 i 0.0%
[0191]
[0192] INVENTIVE EXAMPLE 1 -Ethyl Acetate Leaching of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purified Post-Consumer Recycled Pulp Composition
[0193] 2,500 grams of ethyl acetate was added to a 5L stirred round bottom flask. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat j acket. The mechanical stirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the ethyl acetate to boiling (~77.1°C) in about 5 minutes. After reaching the boiling point of ethyl acetate, the heat input was lowered to achieve a consistent reflux rate of ~10 ml / min at the boiling point of ~77.1°C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Pulp Composition in paperboard form was cut into 1 cm X 1 cm squares. The -250 grams of the cut Reclaimed Post-Consumer Pulp Composition in paperboard form was added to the round bottom flask which contained the boiling ethyl acetate. The extraction was continued for -30 minutes. The stirring was terminated, and the heat was removed. The ethyl acetate was decanted from the mixture of solids and liquids. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a second extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 2nd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a third extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 3rd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a fourth extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 4th extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. The paperboard contained a small amount of contaminated solvent residual w ithin the porosity of the paperboard. This wet paperboard was placed in a filter funnel with 60 mesh grating to further remove residual ethyl acetate via gravity. The paperboard was thencompletely dried of contaminated solvent at room temperature over-night to produce the Purified Pulp Composition or specifically Recycled Post-Consumer Pulp. The leaching solvent to pulp composition ratio per stage was -10:1 for four stages giving a total solvent to pulp composition ratio of -40:1. The leaching time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The pulp composition before and after purification were analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table #3. For the contaminants DEET, glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, diisononylphthalate, fluoranthene, and phenanthrene, the % removal was 74.6%, >91.7%, >93.5%, >83.9%, >85.7%, >70.6%, >96.9%, 68.0%, 75.4%, 82.5%, 87.5%, 85.8%, 87.0%, 93.4%. 84.4%, >94.1%, and 86.9%. respectively, which was indicative of outstanding removal across a broad spectrum of chemical species and classifications.
[0194] The Pulp Composition before and after the purification was characterized for water retention value. The solvent leaching resulted in a 4.8% increase in the water-retention value which may be indicative of decreased homification, which is opposite the trend observed with traditional water washing.
[0195] The Pulp Composition before and after the purification were processed into handsheets following Tappi T205 to produce a recycled paperboard and then evaluated for tensile properties and chemical composition. The solvent leaching resulted in an 11% reduction in tensile strength despite the decreased homification. The solvent leaching process didn't remove significant ash but did significantly remove lignin at 10% removal from the pulp fibers, which is indicative of some lignin extraction possibly due to favorable partitioning between the solvent and the cellulose-based paper fibers.TABLE 3
[0196] Purification of Reclaimed Post-Consumer Fiber #1 to Produce Post-Consumer Recycled Fiber using Stirred Tank Reactor Flooded Leaching with Ethyl Acetate at Boiling Point Reclaimed Post-Consumer Pulp Composition Before After
[0197] % Removed Purification Purification
[0198] LOQ xLOQ xLOQ
[0199] Pesticides
[0200] Dsethyltoluamlde (DEET) 10 ppb 28.0 7.1 74.6% Glyphosate 10 ppb 12.0 <1 > 91.7% Alkylphenol ethoxylates
[0201] iso-Nonylphenotmonoethoxylate 50 ppb 4.0 <1 > 93.5% isc-Nonylphenoldiethoxylate 50 ppb 6,2 <1 >83.9% isc-Nonylphenoltriethoxylate 50 ppb 7.0 <1 >85.7% iso-Nonylphenoltetraethoxylate 50 ppb 3.4 <1 >70.6% Bisphenols
[0202] BisphenolA .5Ppb . 32.0 <1 >96.9% Dioxins and dioxlnltke and PCB
[0203] 1,2,3,4.6,7,8-HpCOD 0.2 ppTr 145.5 46.5 68.0%
[0204] OCDD 0.2 ppTr 1355.0 333.0 75.4%
[0205] OCDF 0.2pptr 43.8 7.7 82 5%
[0206] PCB 81 0.05 ppTr 131.0 16.4 87.5%
[0207] PCB 105 5 ppTr 73.2 10,4 85.8%
[0208] PCB 118 10 ppTr 68.9 9.0 87.0% Phthalates
[0209] Di-2-ethylhexyl phthalate 50 ppb 134.0 8.8 93.4% Diisononyl phthalate 50 ppb 100.0 15.6 84.4% Polycyclic aromatic hydrocarbons (PAH)
[0210] Fluoranthene . J.yiE . 17.0 <1 >94.1% Phenanthrene I ppb 13.0 1.7 86.9%
[0211] % Increase Water Retention Value {g / g; 1.25+ / - 0.1 1.31+ / - 0.19 4.8%
[0212] FQA Fines Level (%) 9.4+ / - 0,0 9.6+ / - 0.2 2.1% Handsheet Tensile Strength (kN / m) 1.8+ / - 0.1 1.6+ / - 0.1 -11.1% Handsheet Zero Span Tensile Strength (kg-f j 8.41 + / - 0.32 8.16+ / - 0.40 -3.1% Compositional information wt% % Removed Ash(%) _ _ 6.8 -9.7%
[0213] Klason lignin (%) 14.2+ / - 0.1 12.8+ / -C.1 9.9%
[0214] Acid soluble Lignin (%j 0.9+ / - 0.0 0.0+ / - 0.0 0.0%
[0215] % Lignin Level 15.2+7-0.1 13,7+ / - 0.1 9.9%
[0216]
[0217] INVENTIVE EXAMPLE 2 -Acetone Leaching of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purified Post-Consumer Recycled Pulp Composition 2.500 grams of acetone was added to a 5L stirred round bottom flask. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanical stirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer.The heat was applied to rapidly bring the acetone to boiling (~52°C) in about 5 minutes. After reaching the boiling point of acetone, the heat input was lowered to achieve a consistent reflux rate of -10 ml / min at the boiling point of ~52°C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Pulp Composition in paperboard form was cut into 1 cm X 1 cm squares. The -250 grams of the cut recycled Reclaimed Post-Consumer Fiber #1 was added to the round bottom flask which contained the boiling acetone. The extraction was continued for -30 minutes. The stirring was terminated, and the heat was removed. The acetone was decanted from the mixture of solids and liquids. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a second extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 2nd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a third extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 3rd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a fourth extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 4th extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. The paperboard contained a small amount of contaminated solvent residual within the porosity of the paperboard. This wet paperboard was placed in a filter flask w / o vacuum to further remove residual acetone. The paperboard was then completely dried of contaminated solvent at room temperature over-night to produce the Purified Pulp Composition or specifically Recycled Post-Consumer Pulp. The leaching solvent to pulp composition ratio per stage was -10:1 for four stages giving a total solvent to pulp composition ratio of -40:1. The leaching time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The Pulp Composition before and after purification were analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as show n in Table #4. For the contaminants For the contaminants DEET, glyphosphate,isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, and diisononylphthalate, the % removal was 85.7%, > 91.7%, > 75.0%. > 83.9%, > 85.7%, > 70.6%, > 96.9%, 89.1%, 89.8%, 85.6%, > 96.7%, 94.8%, 95.1%, 94.9%, and 12.0%, which was indicative of outstanding removal across a broad spectrum of chemical species and classifications.
[0218] The Pulp Composition before and after the purification was characterized for water retention value. The solvent leaching resulted in a 3.2% increase in the water-retention value which may be indicative of decreased homification, which is opposite the trend observed with traditional water washing.
[0219] The Pulp Composition before and after the purification were processed into handsheets following Tappi T205 to produce a recycled paperboard and then evaluated for tensile properties and chemical composition. The solvent leaching resulted in a 17% increase in tensile strength possibly due to the decreased homification. The solvent leaching process didn’t remove significant ash but did significantly remove lignin at -15% reduction from the pulp fibers, which is indicative of some lignin extraction possibly due to favorable partitioning between the solvent and the cellulose-based paper fibers.TABLE 4
[0220] Purification of Method Using Current Invention involving Acetone Leaching of Reclaimed Post- Consumer of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purified Post-Consumer Recycled Pulp Composition
[0221] Reclaimed Post-Consumer Pulp Composition Before After
[0222] % Removed Purification Purification
[0223] LOQ xLOQ xLOQ
[0224] Pesticides
[0225] Diethyltoluamide 'BEET) lOppb 28.0 4.0 85.7% Glyphosate io ppb 12.0 <1 > 91.7% Alkylphenol ethoxylates
[0226] iso-Nonylphenoimoricethoxylate 50 ppt> 4.0 <1 > 75.0% iso-Nonylphenoicllethoxyiate 50 pp!3 6.2 <1 > 83.9% iso-ltonylphenoltriethoxylate 50 ppp 7.0 <1 >85.7% iso-Nonylphenoitetraethoxylate 50 ppb 3.4 <1 > 70.6% Bisphenols
[0227] Bisphenol A 50 ppo 32.6 --1 >96.9% Dioxins and dioxinlike and PCB
[0228] 1,2.3,4,6,7,8-HpCDD _ 0.2ppTr 145.5 15.8 89.1% OCDD 0.2ppTr 1355.0 138.0 89.8% OCDF 0.2ppTr 43.8 8.3 85.6%
[0229] PCB 81 0.05 ppfr 30.0 <1 > 96.7% PCB 105 5ppTr 73.2 3.8 94.8%
[0230] PCB 118 10 ppTr 68.9 3.4 95.1% Phthalates
[0231] Dl-2-ethyihexyl phthalate SOpph 134.0 6.8 94.9% Diisononyl phthalate 50 ppb 100.0 88.0 12.0% Polycyclic aromatic hydrocarbons |PAH)
[0232] Fluoranthene ippb 17.0 dnt n.a.
[0233] Pheriariihrer’e ippb 13.0 dnt n.a.
[0234] % increase Water Retention Value (g / g) 1.25+ / 0.1 1.29 + / 0.15 3.2%
[0235] FQA Fines Level (%) 9.4+ / - C O 9.5+ / - 0.1 1 1% HandsheetTensile Strength • khi / in) 1.8+ / -C.1 2.1+ / - 0.1 16.7% Handsheet Zero Span TensileStrength (kg-fi 8.41 + / -C.32 9.31+ / - 0.44 10.7% Compositional information wt% % Removed Ash(%) i 6.2 6.1 1.6% Klason Lignin 14.2+ / - 0.1 12.0+ / - 0.1 15.5% _ Acid soluble Lignin ;%) _ _ 0.9+ / -C.0 1.0 + / - 0.0 -11.1%
[0236] % Lignin Level 15.2+ / - 0.1 12.9+ / - 0.1 15.1%
[0237]
[0238] VIII. Pulp Compositions
[0239] In embodiments of the present invention, a pulp composition may comprise from about 85 wt% to about 100 wt% post-consumer recycled pulp fiber, while also comprising a minimum number of contaminants and a maximum amount for any contaminant that is present.
[0240] In one embodiment, the pulp composition comprises from about 85 wt% to about 100 wt% post-consumer recycled pulp fiber; and further comprises at least one of the following:a. less than about 100 pg / kg of glyphosphate;
[0241] b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate; c. less than 150 pg / kg of Bisphenol-A;
[0242] d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0243] e. less than 250 ng / kg of OCDD:
[0244] f less than 5 ng / kg of OCDF:
[0245] g. less than 4 ng / kg of PCB 81 ;
[0246] h. less than 350 ng / kg of PCB 105;
[0247] i. less than 50 ng / kg of PCB 118:
[0248] j. less than 5,000 pg / kg of di-2ethylhexylphthalate;
[0249] k. less than 5,000 pg / kg of di-isononylphthalate;
[0250] l. less than 10 pg / kg of fluoranthene; and
[0251] m. less than 10 pg / kg of phenanthene;
[0252] as measured according to the Trace Chemicals Test Method.
[0253] In some embodiments, the pulp composition comprises recycled pulp fiber and comprises at least four of (a) to (m) listed above, in some embodiments at least nine of (a) to (m) listed above, and in still other embodiments, all of (a) to (m) listed above.
[0254] In some embodiments, the inventive pulp may have any one of the following properties, may have at least two of the following properties, may have at least three of the following properties, may have at least four of the following properties, or may have all five of the following properties, properties that are similar to virgin natural fiber performance:
[0255] a. a Water Retention Value of greater than about 1.25 g / g as measured according to the Water Retention Value Test Method described herein:
[0256] b. a % Fines Level (Lw) of less than about 10% as measured according to the Fiber Quality Analysis Test Method described herein;
[0257] c. a Handsheet Tensile Strength of greater than about 1.8 kN / m as measured according to the Handsheet Tensile Properties Test Method described herein:
[0258] d. a Handsheet Zero Span Tensile of greater than about 8.4 kgf as measured according to the Handsheet Zero Span Tensile Test Method described herein; and
[0259] e. a % Lignin Level of less than about 15% as measured according to the Lignin Test Method described herein.
[0260] In some embodiments, the pulp comprises a residual solvent content of less than less than 1,000 ppm, less than 500 ppm, less than 250 ppm, less than 150 ppm, less than 100 ppm, less than50 ppm, less than 10 ppm, or less than 1 ppm, as measured according to the Trace Chemicals Test Method.
[0261] In some embodiments, the pulp composition comprises from about 80 wt% to about 100 wt%, from about 85 wt% to about 100 wt%, from about 90 wt% to 100 wt%, from about 95 wt% to about 100 wt%, from about 85 wt% to about 95 wt%, or from about 90 wt% to about 95 wt% post-consumer recycled pulp fiber. The remaining amount may be virgin natural fibers.
[0262] In some embodiments, the pulp composition is primarily made up of post-industrial, rather than post-consumer, recycled pulp fiber. In some embodiments, the pulp composition may comprise from about 85 wt% to about 100 wt% post-industrial recycled pulp fiber. In general, the post-industrial recycled pulp fiber has fewer contaminants and contaminants at lower levels compared to the post-consumer recycled pulp fiber, so the resulting inventive pulp compositions comprising only post-industrial recycled materials or comprising only post-industrial recycled materials and virgin natural materials may have even lower levels of contaminants, such as the following:
[0263] a. less than about 100 pg / kg of glyphosphate;
[0264] b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate; c. less than 150 pg / kg of Bisphenol-A;
[0265] d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0266] e. less than 250 ng / kg of OCDD;
[0267] f. less than 5 ng / kg of OCDF;
[0268] g. less than 4 ng / kg of PCB 81 ;
[0269] h. less than 350 ng / kg of PCB 105;
[0270] i. less than 50 ng / kg of PCB 118;
[0271] j. less than 5,000 pg / kg of di-2ethylhexylphthalate;
[0272] k. less than 5,000 pg / kg of di-isononylphthalate;
[0273] l. less than 10 pg / kg of fluoranthene; and
[0274] m. less than 10 pg / kg of phenanthene;
[0275] as measured according to the Trace Chemicals Test Method.
[0276] In some embodiments, the inventive pulp composition may comprise a weight percent of post-consumer recycled pulp fiber and a weight percent of post-industrial recycled pulp fiber, wherein the weight percent of post-consumer recycled pulp fiber is from about 15% to about 85%, and wherein the weight percent of post-industrial recycled pulp fiber is from about 15% to about 85%. Such compositions may have from 0 wt% to 60% wt% of natural fibers. Such compositions may further comprise at least one of the following:a. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 100 pg / kg of glyphosphate;
[0277] b. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 150 Lig / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate;
[0278] c. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 150 ng / kg of Bisphenol A;
[0279] d. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0280] e. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 250 ng / kg of OCDD;
[0281] f. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5 ng / kg of OCDF
[0282] g. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 4 ng / kg ofPCB 81;
[0283] h. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 350 ng / kg ofPCB 105;
[0284] i. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 50 ng / kg ofPCB 118;
[0285] j . less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5,000 ng / kg of di-2ethylhexylphthalate;
[0286] k. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5,000 Lig / kg of di-isononylphthalate;
[0287] l. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 10 pg / kg of fluoranthene;
[0288] m. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 10 Lig / kg of phenanthene;
[0289] as measured according to the Trace Chemicals Test Method.
[0290] In other embodiments, the cellulosic pulp compositions of the present invention may be incorporated into consumer products, such as sanitary' tissue products, towel products, disposable plates, or other personal care articles. In still other embodiments, the pulp may be used in packaging materials and packages.
[0291] In some embodiments, the pulp composition may comprise from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber; wherein the pulp composition has been subjected to a purification process; and wherein the cellulosic pulp composition has a Water Retention Level atleast about 5% greater than the cellulosic pulp composition’s Water Retention Level before being subjected to the purification process. The purification process may be a bulk purification or a surface and bulk purification process, such as described herein, and / or the purification process may comprise solvent extraction in multiple stages, such as described herein.
[0292] The pulp composition may comprise from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber; wherein the pulp composition has been subjected to a purification process; and wherein the pulp composition has a % Fines Level (Lw) equal to or less than the pulp composition’s % Fines Level before being subjected to the purification process. The purification process may be a bulk purification or a surface and bulk purification process, such as described herein, and / or the purification process may comprise solvent extraction in multiple stages, such as described herein.
[0293] The pulp composition may comprise from about 90 vA% to about 100 wt% post-consumer recycled pulp fiber; wherein the pulp composition has been subjected to a purification process; and wherein the pulp composition has a Handsheet Tensile Strength at least about 16% greater than the pulp composition’s Handsheet Tensile Strength before being subjected to the purification process. The purification process may be a bulk purification or a surface and bulk purification process, such as described herein, and / or the purification process may comprise solvent extraction in multiple stages, such as described herein.
[0294] The pulp composition may comprise from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber; wherein the pulp composition has been subjected to a purification process; and wherein the pulp composition has a Handsheet Zero Span Tensile at least about 15% greater than the pulp composition’s Handsheet Zero Span Tensile before being subjected to the purification process. The purification process may be a bulk purification or a surface and bulk purification process, such as described herein, and / or the purification process may comprise solvent extraction in multiple stages, such as described herein.
[0295] The pulp composition may comprise from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber; wherein the pulp composition has been subjected to a purification process; and wherein the pulp composition has a % Lignin Level at least about 1.5 percentage points less than the cellulosic pulp composition’s % Lignin Level before being subjected to the purification process. The purification process may be a bulk purification or a surface and bulk purification process, such as described herein, and / or the purification process may comprise solvent extraction in multiple stages, such as described herein.IX. TEST METHODS
[0296] 1. TRACE CHEMICALS TEST METHOD
[0297] The content on a mass per mass basis of trace chemicals present in recycled pulp, tissue comprising recycle pulp, or packaging material comprising recycle pulp is determined using methods containing sample extraction and instrumental analysis approaches known of those of skill in the art and understood to be capable of extracting and detecting essentially all of a particular trace chemical in these materials. Suitable overall method specifics vary based on the particular trace chemical being quantified, though a common overall method structure is generally followed. A suitable method generally begins with increasing the surface area of a representative recycled pulp, tissue comprising recycle pulp, or packaging material comprising recycle pulp sample by cutting, shredding, and / or milling into small particles. An extraction step is then performed using a solvent capable of dissolving or diffusing into the sample and in which the trace chemical is readily soluble. The extraction process conditions (e.g., time and temperature) are optimized to maximize trace chemical recovery and common approaches include but are not limited to Soxhlet extraction, accelerated solvent extraction, and / or ultrasonic extraction. Internal standards (usually stable-isotope-labeled versions of the trace chemicals if mass spectrometry-based detection approaches are used) are added during the extraction step to account for potential losses during extraction and subsequent processing steps. After extraction is complete, the extraction solvent is isolated and worked up for instrumental analysis. Depending on the solvent used for extraction, the required quantitation limit, and the specific instrumental approach used, generation of a specimen suitable for instrumental analysis may require multiple cleanup and / or concentration steps including but not limited to centrifugation / filtration, liquid / liquid extraction, and / or column chromatography. The trace chemical in the worked-up specimen is then quantified using instrumental methods (e.g., GC-MS, GC-MS / MS, GC-HRMS, LC-MS / MS, etc.) known to those of skill in the art and specifically adapted to the trace chemical of interest. Suitable instrumental approaches may be developed de novo or may be based on standard, known methods for particular trace chemicals (e.g., US EPA Method 1613 in the case of dioxins and furans or US EPA 1668 for PCBs). Based on a combination of raw instrumental quantitative results, extraction solvent workup steps, original extraction volume, and starting specimen mass, the mass content of a trace chemical per mass of starting specimen material is calculated and is reported as the level of the trace chemical in the material tested. Given the generally low levels of trace chemicals present, common units used in reported levels of trace chemicals are pg / kg and ng / kg (equivalent to the ppb and ppt levels, respectively).One of skill in the art will recognize that trace chemicals are often present at very low “trace” levels, meaning that under some circumstances, environmental and / or laboratory background levels of these same trace chemicals may give rise to false positive detects or falsely elevated results if appropriate precautions are not taken. While one of skill in the art recognizes that a suite of measures may be needed to minimize such false results, one obligatory measure is to include a true “blank” beginning with solvent carried in parallel through the extraction step, extraction solvent workup, and instrumental analysis.
[0298] Using the suitable overall methodology outlined above, one of skill in the art may quantify a range of trace chemicals potentially present in a recycled pulp, tissue comprising recycle pulp, or packaging material comprising recycle pulp sample of interest. For example, just to describe a few of the trace chemicals listed herein, the level of isononylphenol (CAS RN 11066-49-2) may be determined and reported as mass of trace chemical per mass of material in units of pg / kg. Similarly, the level of PCB 118 (CAS RN 31508-00-6) may be determined and reported in units of ng / kg, the level of OCDD (CAS RN 3268-87-9), a dioxin, may be determined and reported in units of ng / kg, the level of bisphenol A (CAS RN 80-05-7), also known as BPA, may be determined and reported in units of pg / kg, and the level of diisononyl phthalate (CAN RN 28553-12-0), also known as DINP, may be determined and reported in units of pg / kg.
[0299] 2. WATER RETENTION VALUE TEST METHOD
[0300] The w ater retention value of pulp was measured according to Tappi UM 256.
[0301] 3. % FINES LEVEL (FIBER QUALITY ANALYSIS TEST METHOD)
[0302] The pulp morphology including fiber length, width, coarseness, fines was characterized optically according Tappi T271 om-23 using a Fiber Quality Analyzer (FQA-360).
[0303] 4. HANDSHEET TENSILE PROPERTIES TEST METHOD
[0304] Handsheet was made according to Tappi T205 for paper mechanical properties test. The tensile properties of hand sheet were measured according to Tappi T494.
[0305] 5 HANDSHEET ZERO SPAN TENSILE TEST METHOD
[0306] The Zero-span breaking strength of pulp was measured according to Tappi T231.
[0307] 6 % LIGNIN LEVEL TEST METHOD
[0308] The % lignin level in pulp was determined according to the standard protocol provided by the National Renewable Energy Laboratory. (J. Agric. Food Chem. 2010, 58, 16, 9043-9053).7. WATER CONTENT TEST METHOD
[0309] The water (moisture) content present in a fibrous structure is measured using the following Water Content Test Method.
[0310] A fibrous structure or portion thereof (“sample’') is placed in a conditioned room at a temperature of 73°F ± 4°F (about 23°C ± 2.2°C) and a relative humidity of 50% ± 10% for at least 24 hours prior to testing. The weight of the sample is recorded when no further weight change is detected for at least a 5 minute period. Record this weight as the “equilibrium weight” of the sample. Next, place the sample in a drying oven for 24 hours at 70°C with a relative humidity of about 4% to dry the sample. After the 24 hours of drying, immediately weigh the sample. Record this weight as the “dry weight” of the sample. The water (moisture) content of the sample is calculated as follows:
[0311] % Water (moisture) in sample = 100% x (Equilibrium weight of sample - Dry weight of sample)
[0312] Dry weight of sample
[0313] The % Water (moisture) in sample for 3 replicates is averaged to give the reported % Water (moisture) in sample.
[0314] X. COMBINATIONS
[0315] A. A pulp composition, comprising from about 85 wt% to about 100 wt% post-consumer recycled pulp fiber; and further comprising at least one of the following:
[0316] a. less than about 100 pg / kg of gly phosphate;
[0317] b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate; c. less than 150 pg / kg of Bisphenol-A;
[0318] d. less than 25 ng / kg of 1, 2,3,4, 6,7, 8-HpCDD;
[0319] e. less than 250 ng / kg of OCDD;
[0320] f. less than 5 ng / kg of OCDF;
[0321] g. less than 4 ng / kg of PCB 81;
[0322] h. less than 350 ng / kg of PCB 105;
[0323] i. less than 50 ng / kg of PCB 118;
[0324] j. less than 5,000 pg / kg of di-2ethylhexylphthalate;
[0325] k. less than 5.000 pg / kg of di-isononylphthalate;
[0326] l. less than 10 pg / kg of fluoranthene; and
[0327] m. less than 10 pg / kg of phenanthene;
[0328] as measured according to the Trace Chemicals Test Method.B. The pulp composition of paragraph A, wherein the composition comprises at least 4 of (a) -(m).
[0329] C. The pulp composition of paragraph A or B, wherein the composition comprises at least 9 of (a) - (m).
[0330] D. The pulp composition of any one of paragraphs A-C, wherein the composition comprises all of (a) - (m).
[0331] E. The pulp composition of any one of paragraphs A-D, wherein the composition exhibits a Water Retention Value of greater than about 1.25 g / g as measured according to the W ater Retention V alue Test Method described herein.
[0332] F. The pulp composition of any one of paragraphs A-E, wherein the composition exhibits a % Fines Level (Lw) of less than about 10% as measured according to the Fiber Quality Analysis Test Method described herein.
[0333] G. The pulp composition of any one of paragraphs A-F, wherein the composition exhibits a Handsheet Tensile Strength of greater than about 1.8 kN / m as measured according to the Handsheet Tensile Properties Test Method described herein.
[0334] H. The pulp composition of any one of paragraphs A-G, wherein the composition exhibits a Handsheet Zero Span Tensile of greater than about 8.4 kgf as measured according to the Handsheet Zero Span Tensile Test Method described herein.
[0335] I. The pulp composition of any one of paragraphs A-H, wherein the composition exhibits a % Lignin Level of less than about 15% as measured according to the % Lignin Level Test Method described herein.
[0336] J. The pulp composition of any one of paragraphs A-I, wherein the composition exhibits two or more of the following properties:
[0337] a. a Water Retention Value of greater than about 1.25 g / g as measured according to the Water Retention Value Test Method described herein;
[0338] b. a % Fines Level (Lw) of less than about 10% as measured according to the Fiber Quality Analysis Test Method described herein;
[0339] c. a Handsheet Tensile Strength of greater than about 1.8 kN / m as measured according to the Handsheet Tensile Properties Test Method described herein;
[0340] d. a Handsheet Zero Span Tensile of greater than about 8.4 kgf as measured according to the Handsheet Zero Span Tensile Test Method described herein; and
[0341] e. a % Lignin Level of less than about 15% as measured according to the Lignin Test Method described herein.K. The pulp composition of any one of paragraphs A-J, wherein the composition exhibits all five of the following properties:
[0342] a. a Water Retention Value of greater than about 1.25 g / g as measured according to the Water Retention Value Test Method described herein;
[0343] b. a % Fines Level (Lw) of less than about 10% as measured according to the Fiber Quality Analysis Test Method described herein;
[0344] c. a Handsheet Tensile Strength of greater than about 1.8 kN / m as measured according to the Handsheet Tensile Properties Test Method described herein;
[0345] d. a Handsheet Zero Span Tensile of greater than about 8.4 kgf as measured according to the Handsheet Zero Span Tensile Test Method described herein; and
[0346] e. a % Lignin Level of less than about 1 % as measured according to the Lignin Test Method described herein.
[0347] L. The pulp composition of any one of paragraphs A-K, wherein the composition comprises a residual solvent content of less than 1,000 ppm, as measured according to the Trace Chemicals Test Method.
[0348] M. The pulp composition of any one of paragraphs A-L, wherein the composition comprises from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber.
[0349] N. A tissue product comprising the pulp composition of any one of paragraphs A-M.
[0350] O. A towel product comprising the pulp composition of any one of paragraphs A-N.
[0351] P. A package material comprising the pulp composition of any one of paragraphs A-O.
[0352] Q. A personal care article comprising the pulp composition of any one of paragraphs A-P.
[0353] R. A disposable plate comprising the pulp composition of any one of paragraphs A-Q.
[0354] S. A pulp composition according to any one of paragraphs A-R, comprising a weight percent of post-consumer recycled pulp fiber and a weight percent of post-industrial recycled pulp fiber; wherein the weight percent of post-consumer recycled pulp fiber is from about 15% to about 85%;
[0355] wherein the weight percent of post-industrial recycled pulp fiber is from about 15% to about 85%;
[0356] and wherein the pulp composition comprises at least one of the following:
[0357] a. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 100 pg / kg of glyphosphate;
[0358] b. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 150 pg / kg of isononylphenol(mono, di, tri, and tetra)exthoxylate;c. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 150 ng / kg of Bisphenol A;
[0359] d. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;
[0360] e. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 250 ng / kg of OCDD;
[0361] f. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5 ng / kg of OCDF
[0362] g. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 4 ng / kg ofPCB 81;
[0363] h. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 350 ng / kg ofPCB 105;
[0364] i. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 50 ng / kg ofPCB 118;
[0365] j. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5,000 pg / kg of di-2ethylhexylphthalate;
[0366] k. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5,000 pg / kg of di-isononylphthalate;
[0367] l. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 10 pg / kg of fluoranthene;
[0368] m. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 10 pg / kg of phenanthene;
[0369] as measured according to the Trace Chemicals Test Method.
[0370] T. A pulp composition according to any one of paragraphs A-S, comprising from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber;
[0371] wherein the pulp composition has been subjected to a purification process;
[0372] and wherein the cellulosic pulp composition has a Water Retention Level at least about 5% greater than the cellulosic pulp composition’s Water Retention Level before being subjected to the purification process.
[0373] U. The composition of any one of paragraphs A-T. wherein the purification process is a bulk purification or a surface and bulk purification process.
[0374] V. The composition of any one of paragraphs A-U, wherein the purification process comprises solvent extraction in multiple stages.W. A pulp composition according to any one of paragraphs A-V, comprising from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber;
[0375] wherein the pulp composition has been subjected to a purification process;
[0376] and wherein the pulp composition has a % Fines Level (Lw) equal to or less than the pulp composition’s % Fines Level before being subjected to the purification process.
[0377] X. The composition according to any one of paragraphs A-W, wherein the purification process is a bulk purification or a surface and bulk purification process.
[0378] Y. The composition according to any one of paragraphs A-X, wherein the purification process comprises solvent extraction in multiple stages.
[0379] Z. A pulp composition according to any one of paragraphs A-Y comprising from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber;
[0380] wherein the pulp composition has been subjected to a purification process;
[0381] and wherein the pulp composition has a Handsheet Tensile Strength at least about 16% greater than the pulp composition’s Handsheet Tensile Strength before being subjected to the purification process.
[0382] AA. The composition according to any one of paragraphs A-Z, wherein the purification process is a bulk purification or a surface and bulk purification process.
[0383] BB. The composition according to any one of paragraphs A-AA, wherein the purification process comprises solvent extraction in multiple stages.
[0384] CC. A pulp composition according to any one of paragraphs A-BB comprising from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber;
[0385] wherein the pulp composition has been subjected to a purification process;
[0386] and wherein the pulp composition has a Handsheet Zero Span Tensile at least about 15% greater than the pulp composition’s Handsheet Zero Span Tensile before being subjected to the purification process.
[0387] DD. The composition according to any one of paragraphs A-CC, wherein the purification process is a bulk purification or a surface and bulk purification process.
[0388] EE. The composition according to any one of paragraphs A-DD, wherein the purification process comprises solvent extraction in multiple stages.
[0389] FF. A pulp composition according to any one of paragraphs A-EE comprising from about 90 wt% to about 100 wt% post-consumer recycled pulp fiber;
[0390] wherein the pulp composition has been subjected to a purification process;and wherein the pulp composition has a % Lignin Level at least about 1.5 percentage points less than the cellulosic pulp composition’s % Lignin Level before being subjected to the purification process.
[0391] GG. The composition according to any one of paragraphs A-FF, wherein the purification process is a bulk purification or a surface and bulk purification process.
[0392] HH. The composition according to any one of paragraphs A-GG, w herein the purification process comprises solvent extraction in multiple stages.
[0393] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as “40 mm” is intended to mean “about 40 mm.”
[0394] Every document cited herein, including any cross referenced or related patent or application and any patent application or patent to which this application claims priority or benefit thereof, is hereby incorporated herein by reference in its entirety unless expressly excluded or otherwise limited. The citation of any document is not an admission that it is prior art with respect to any invention disclosed or claimed herein or that it alone, or in any combination with any other reference or references, teaches, suggests or discloses any such invention. Further, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall govern.
[0395] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended to cover in the appended claims all such changes and modifications that are within the scope of this invention.
Claims
CLAIMSWhat is claimed is:
1. A pulp composition, comprising from 85 wt% to 100 wt% post-consumer recycled pulp fiber; and further comprising at least one of the following:a. less than 100 pg / kg of glyphosphate;b. less than 150 pg / kg of isononylphenol(mono, di, tri, and tctra)cxthoxy late: c. less than 150 pg / kg of Bisphenol-A;d. less than 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;c. less than 250 ng / kg of OCDD;f. less than 5 ng / kg of OCDF;g. less than 4 ng / kg of PCB 81;h. less than 350 ng / kg of PCB 105;i. less than 50 ng / kg of PCB 118;j. less than 5.000 pg / kg of di-2ethylhexylphthalate;k. less than 5,000 pg / kg of di-isononylphthalate;l. less than 10 pg / kg of fluoranthene; andm. less than 10 pg / kg of phenanthene;as measured according to the Trace Chemicals Test Method.
2. The pulp composition of claim 1, wherein the composition comprises at least 4 of (a) - (in).
3. The pulp composition of claim 1, wherein the composition comprises all of (a) - (m).
4. The pulp composition of claim 1. wherein the composition exhibits a Water Retention Value of greater than 1.25 g / g as measured according to the Water Retention Value Test Method described herein.
5. The pulp composition of claim 1, wherein the composition exhibits a % Fines Level (Lw) of less than 10% as measured according to die Fiber Quality Analysis Test Method described herein.
6. The pulp composition of claim 1. wherein the composition exhibits a Handsheet Tensile Strength of greater than 1.8 kN / m as measured according to the Handsheet Tensile Properties Test Method described herein.
7. The pulp composition of claim 1, wherein the composition exhibits a Handshcct Zero Span Tensile of greater than 8.4 kgf as measured according to the Handsheet Zero Span Tensile Test Method described herein.
8. The pulp composition of claim 1. wherein the composition exhibits a % Lignin Level of less than 15% as measured according to the Lignin Test Method described herein.
9. The pulp composition of claim 1, wherein the composition exhibits two or more of the following properties:a. a Water Retention Value of greater than 1.25 g / g as measured according to the Water Retention Value Test Method described herein;b. a % Fines Level (Lw) of less than 10% as measured according to the Fiber Quality Analysis Test Method described herein;c. a Handsheet Tensile Strength of greater than 1.8 kN / m as measured according to the Handsheet Tensile Properties Test Method described herein;d. a Handsheet Zero Span Tensile of greater than 8.4 kgf as measured according to the Handsheet Zero Span Tensile Test Method described herein; ande. a % Lignin Level of less than 15% as measured according to the % Lignin Level Test Method described herein.
10. The pulp composition of claim 1, wherein the composition exhibits all five of the following properties:a. a Water Retention Value of greater than 1.25 g / g as measured according to the Water Retention Value Test Method described herein;b. a % Fines Level (Lw) of less than 10% as measured according to the Fiber Quality’ Analy sis Test Method described herein;c. a Handsheet Tensile Strength of greater than 1.8 kN / m as measured according to the Handsheet Tensile Properties Test Method described herein;d. a Handsheet Zero Span Tensile of greater than 8.4 kgf as measured according to the Handsheet Zero Span Tensile Test Method described herein; ande. a % Lignin Level of less than 15% as measured according to the % Lignin Level Test Method described herein.
11. The pulp composition of claim 1, wherein the composition comprises a residual solvent content of less than 1.000 ppm, as measured according to the Trace Chemicals Test Method.
12. The pulp composition of claim 1, wherein the composition comprises from 90 wt% to 100 wt% post-consumer recycled pulp fiber.
13. An article comprising the pulp composition of claim 1, wherein the article is selected from the group consisting of a tissue product, a towel product, a package, a personal care article, and a disposable plate.
14. A pulp composition, comprising a weight percent of post-consumer recycled pulp fiber and a weight percent of post-industrial recycled pulp fiber;wherein the weight percent of post-consumer recycled pulp fiber is from 15% to 85%; wherein the weight percent of post-industrial recycled pulp fiber is from 15% to 85%; and wherein the pulp composition comprises at least one of the following: a. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 100 pg / kg of glyphosphate;b. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 150 pg / kg of isononylphenol(mono, di. tri, and tetra)exthoxylate;c. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 150 ng / kg of Bisphenol A;d. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 25 ng / kg of 1,2,3,4,6,7,8-HpCDD;e. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 250 ng / kg of OCDD;f. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5 ng / kg of OCDF g. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 4 ng / kg of PCB 81;h. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 350 ng / kg of PCB 105;i. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 50 ng / kg of PCB 118;j. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5,000 pg / kg of di-2ethylhexylphthalate;k. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 5,000 pg / kg of di-isonony Iphthalate ;l. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 10 pg / kg of fluoranthene;m. less than (the weight percent of post-consumer recycled pulp fiber / 100) x 10 pg / kg of phenanthene;as measured according to die Trace Chemicals Test Method.
15. A pulp composition comprising from 90 wt% to 100 wt% post-consumer recycled pulp fiber;wherein the pulp composition has been subjected to a purification process; and wherein the composition exhibits at least one of the following properties;a. the pulp composition has a Water Retention Level at least 5% greater than the cellulosic pulp composition’s Water Retention Level before being subjected to the purification process;b. the pulp composition has a % Fines Level (Lw) equal to or less than the pulp composition’s % Fines Level before being subjected to the purification process;c. the pulp composition has a Handsheet Tensile Strength at least 16% greater than the pulp composition’s Handsheet Tensile Strength before being subjected to the purification process; d. the pulp composition has a Handsheet Zero Span Tensile at least 15% greater than the pulp composition’s Handsheet Zero Span Tensile before being subjected to the purification process; ande. the pulp composition has a % Lignin Level at least 1.5 percentage points less than the cellulosic pulp composition’s % Lignin Level before being subjected to the purification process.