Methacrylic acid copolymer, composition, molded product, method for producing film or sheet, and laminate
By adjusting the proportion of structural units in the methacrylic copolymer to increase its glass transition temperature and compatibility, the problem of insufficient heat resistance and compatibility of existing materials is solved, and efficient optical performance adjustment is achieved, which is suitable for in optical components.
Patent Information
- Application Number
- CN202180022765.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-24
- Filing Date
- 2021-03-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-22
AI Technical Summary
The existing 2,2,2-trifluoroethyl methacrylate polymer has a low glass transition temperature, insufficient heat resistance, and poor compatibility with other resins. It is difficult to control the sign of the orientation birefringence and photoelastic coefficient, which limits the Its application in optical components.
A methacrylic copolymer was developed, which contains 40 to 87% of methyl methacrylate units and 6 to 30% of units selected from lactone ring units and α-methylstyrene units. By adjusting the structural units The ratio can achieve a glass transition temperature of more than 120°C, and the orientation birefringence in the stretched film at high temperature is positive and the photoelastic coefficient is negative.
A methacrylic copolymer with high heat resistance, positive orientation birefringence, and negative photoelastic coefficient has been realized. It has excellent compatibility with other resins, can effectively reduce the birefringence of molded products, and is suitable for optical components. Material.
Smart Images

Figure FDA0004887817120000011 
Figure GDA0003854391560000031 
Figure GDA0003854391560000041
Abstract
Description
Technical Field
[0001] The present invention relates to a methacrylic copolymer, a composition, a molded product, a method for producing a film or a sheet, and a laminate. Background Art
[0002] (Meth) acrylic resin is widely used as a material for optical components such as lenses, prisms, phase difference films, light guide plates, light diffusion films, polarizer protective films, etc. due to its excellent transparency and little optical deformation. In these applications, the birefringence of the molded product affects the performance of the device. For example, in devices such as liquid crystal display devices, optical disk devices, and projection screens, if there are films and lenses with birefringence in the optical path, it will have an adverse effect on image quality and signal reading performance. Therefore, in recent years, materials that suppress birefringence as little as possible have been sought.
[0003] The birefringence exhibited by the resin includes orientation birefringence caused by the orientation of polymer molecules and photoelastic birefringence caused by stress. The signs of each are inherent properties of the polymer derived from the primary structure of the polymer. As one of the means to reduce the birefringence of the material, a method of mixing polymers with positive and negative birefringence can be cited. In order to highly control the birefringence using this method, it is necessary to make the signs of the orientation birefringence or photoelastic coefficient different from those of the main resin and use a material with high compatibility as the added resin.
[0004] As a polymer having a positive value for oriented birefringence and a negative value for photoelastic coefficient, a polymer of 2,2,2-trifluoroethyl methacrylate is known (Patent Document 1). However, the glass transition temperature of this polymer is low and there are problems with heat resistance. In addition, the compatibility with other resins is also low, and it is difficult to use it as an additive resin for controlling the birefringence of other resins with opposite signs of oriented birefringence or photoelastic coefficient. In addition, the monomer itself is expensive, so there are restrictions on industrial use.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2015 / 079694 Summary of the invention
[0008] Problems to be solved by the invention
[0009] An object of the present invention is to provide a methacrylic copolymer having high heat resistance, a positive orientation birefringence and a negative photoelastic coefficient, and excellent compatibility with other resins, and a composition, a film, a sheet, a laminate and a molded product comprising the copolymer.
[0010] Methods used to solve problems
[0011] The present inventors have conducted intensive studies to achieve the above-mentioned object, and as a result, have completed the present invention including the following aspects. [1]
[0013] A methacrylic copolymer comprising 40 to 87% by mass of methyl methacrylate units, 6 to 30% by mass of structural units (R) having at least one ring structure selected from the group consisting of lactone ring units, glutaric anhydride units and N-substituted or unsubstituted glutarimide units in the main chain, and 7 to 30% by mass of α-methylstyrene units, the copolymer having a glass transition temperature of 120° C. or higher, wherein the photoelastic coefficient has a negative value, and the orientation birefringence of a stretched film obtained by stretching a sheet of 20 mm×40 mm×1.0 mm thick by 100% in one direction at a rate of 3 mm / min at a temperature 10° C. higher than the glass transition temperature is positive. [2]
[0015] The methacrylic acid-based copolymer according to [1], wherein the structural unit (R) is an N-substituted or unsubstituted glutarimide unit represented by formula (1).
[0016]
[0017] (In formula (1), R 1 are each independently a hydrogen atom or a methyl group, R 2 It is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms and containing an aromatic ring. [3]
[0019] A composition obtained by melt-kneading the methacrylic acid copolymer according to [1] or [2] and other resin. [4]
[0021] A molded article comprising the methacrylic copolymer described in [1] or [2] or the composition described in [3]. [5]
[0023] The formed article according to [4], wherein the formed article is a film or a sheet. [6]
[0025] A method for producing a film or sheet, comprising the step of molding the methacrylic copolymer described in [1] or [2] or the composition described in [3] into a film or sheet by a melt molding method. [7]
[0027] A method for producing a film or sheet, comprising the step of forming the methacrylic copolymer described in [1] or [2] or the composition described in [3] into a film or sheet by a solution casting method. [8]
[0029] A laminate having at least one layer consisting of a film or sheet comprising the methacrylic copolymer described in [1] or [2] or the composition described in [3].
[0030] Effects of the Invention
[0031] According to the present invention, a methacrylic copolymer having high heat resistance, a positive orientation birefringence and a negative photoelastic coefficient and excellent compatibility with other resins, and a composition, film, sheet, laminate and molded product containing the copolymer can be obtained. DETAILED DESCRIPTION
[0032] (Methacrylic acid copolymer)
[0033] The methacrylic acid copolymer of the present invention contains methyl methacrylate units, α-methylstyrene units and structural units (R). The methacrylic acid copolymer of the present invention may further contain copolymerizable monomer units, methacrylic acid amide units represented by the following formula (A), and 2-(hydroxyalkyl)acrylate units represented by the following formula (B).
[0034]
[0035] (Where R 3 R is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms and containing an aromatic ring, preferably a hydrogen atom, a methyl group, an n-butyl group, a cyclohexyl group, or a benzyl group, and more preferably a methyl group, an n-butyl group, or a cyclohexyl group. 4 and R 5 Each independently represents a hydrogen atom or an organic group having 1 to 20 carbon atoms, preferably a hydrogen atom or an organic group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or an organic group having 1 to 5 carbon atoms. Here, the organic group is not particularly limited as long as it has 1 to 20 carbon atoms, and examples thereof include a linear or branched alkyl group, a linear or branched aryl group, an -OCOCH3 group, a -CN group, etc. The organic group may contain heteroatoms such as an oxygen atom. R 4 Preferably, methyl, R 5 Preferably it is a hydrogen atom.)
[0036] In the methacrylic acid copolymer of the present invention, the ratio of the methyl methacrylate unit is preferably 40 to 87% by mass, more preferably 50 to 85% by mass, and further preferably 65 to 80% by mass relative to the total structural units. When the ratio of the methyl methacrylate unit is less than this range, the total light transmittance of the obtained methacrylic acid copolymer becomes poor; when the ratio of the methyl methacrylate unit is more than this range, the heat resistance of the obtained methacrylic acid copolymer becomes low.
[0037] In the methacrylic acid copolymer of the present invention, the ratio of the α-methylstyrene unit is preferably 7 to 30% by mass, more preferably 8 to 27% by mass, and further preferably 11 to 25% by mass relative to the total structural units. When the ratio of the α-methylstyrene unit is less than this range, the saturated water absorption of the obtained methacrylic acid copolymer becomes high. In addition, the methacrylic acid copolymer in which the ratio of the α-methylstyrene unit exceeds 30% by mass has low polymerizability and reduced productivity.
[0038] The structural unit (R) is a structural unit having at least one ring structure selected from the group consisting of a lactone ring unit, a glutaric anhydride unit, and an N-substituted or unsubstituted glutarimide unit in the main chain. The structural unit may contain a methacrylic acid amide unit represented by the above formula (A) and / or a 2-(hydroxyalkyl)acrylate unit represented by the above formula (B) in the main chain.
[0039] The polymer of Comparative Example 3 of the present application, which is composed of 100% of methyl methacrylate units, has both negative orientation birefringence and photoelastic coefficient. Therefore, it is known that the methyl methacrylate units contribute to negative orientation birefringence and photoelastic coefficient.
[0040] The polymer of Comparative Example 2 of the present application, which is composed of 90% methyl methacrylate units and 10% α-methylstyrene units, has negative orientation birefringence and photoelastic coefficient, and the absolute values are larger than those of the polymer of Comparative Example 3 of the present application, which is composed of 100% methyl methacrylate units. Therefore, it can be seen that the α-methylstyrene unit contributes to the negative orientation birefringence and photoelastic coefficient.
[0041] On the other hand, the polymers of Examples 1 and 2 containing the structural unit (R) together with the methyl methacrylate unit and the α-methylstyrene unit have positive orientation birefringence and negative photoelastic coefficient. In addition, the polymer of Example 2 having a higher imidization ratio in proportion to the ratio of the structural unit (R) has a larger orientation birefringence value than the polymer of Example 1.
[0042] In the methacrylic copolymer of the present invention, the structural unit (R) contributes greatly to maintaining the photoelastic coefficient negative and converting the orientation birefringence to positive. The orientation birefringence is proportional to the structural unit (R), so by appropriately selecting the ratio of the structural unit (R), the orientation birefringence can be made positive.
[0043] One feature of the present invention is that by further introducing a structural unit (R) into a methacrylic copolymer containing a methyl methacrylate unit and an α-methylstyrene unit, a methacrylic copolymer having high heat resistance and transparency, a positive orientation birefringence and a negative photoelastic coefficient, the birefringence of a molded article can be suppressed to a low level, and excellent compatibility with other resins can be obtained. The magnitude of each of the orientation birefringence and the photoelastic coefficient can be adjusted by changing the ratio of the methyl methacrylate unit, the α-methylstyrene unit, and the structural unit (R).
[0044] The lactone ring unit is a structural unit containing a >CH-OC(=O)- group in the ring structure. In the structural unit containing a >CH-OC(=O)- group in the ring structure, the number of ring-constituting atoms is preferably 4 to 8, more preferably 5 to 6, and most preferably 6 (six-membered ring). As structural units containing a >CH-OC(=O)- group in the ring structure, lactone diyl structural units such as β-propiolactone diyl structural unit, γ-butyrolactone diyl structural unit, and δ-valerolactone diyl structural unit can be listed. The structural unit containing a >CH-OC(=O)- group in the ring structure can be obtained, for example, by intramolecular cyclization of a polymer having a hydroxyl group and an ester group using the hydroxyl group and the ester group. It should be noted that ">C" in the formula means that there are two bonds on the carbon atom C.
[0045] For example, as the δ-valerolactone diyl structural unit, there can be mentioned the structural unit represented by the formula (I).
[0046]
[0047] In formula (I), R 6 , R 7 and R 8 Each independently represents a hydrogen atom or an organic group having 1 to 20 carbon atoms, preferably a hydrogen atom or an organic group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or an organic group having 1 to 5 carbon atoms. Here, the organic group is not particularly limited as long as it has 1 to 20 carbon atoms, and examples thereof include a linear or branched alkyl group, a linear or branched aryl group, an -OCOCH3 group, a -CN group, etc. The organic group may contain heteroatoms such as an oxygen atom. R 6 and R 7 Preferably, methyl, R 8 Preferred is a hydrogen atom.
[0048] The lactone ring unit can be contained in the methacrylic acid copolymer by the method described in Japanese Patent Laid-Open No. 2000-230016, Japanese Patent Laid-Open No. 2001-151814, Japanese Patent Laid-Open No. 2002-120326, Japanese Patent Laid-Open No. 2002-254544, Japanese Patent Laid-Open No. 2005-146084, etc., for example, by intramolecular cyclization of the structural unit derived from 2-(hydroxyalkyl) acrylate and the structural unit derived from methyl (meth)acrylate. Japanese Patent Laid-Open No. 2000-230016, Japanese Patent Laid-Open No. 2001-151814, Japanese Patent Laid-Open No. 2002-120326, Japanese Patent Laid-Open No. 2002-254544, Japanese Patent Laid-Open No. 2005-146084 are incorporated herein by reference in their entirety.
[0049] The glutaric anhydride unit is a unit having a 2,6-dioxodihydropyrandiyl structure. Examples of the unit having a 2,6-dioxodihydropyrandiyl structure include a structural unit represented by formula (II).
[0050]
[0051] In formula (II), R 9 Each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and is preferably a methyl group.
[0052] The unit having a 2,6-dioxodihydropyrandiyl structure can be contained in the methacrylic acid copolymer by the method described in Japanese Patent Application Laid-Open No. 2007-197703, Japanese Patent Application Laid-Open No. 2010-96919, etc., for example, by intramolecular cyclization of two adjacent structural units derived from (meth)acrylic acid, intramolecular cyclization of a structural unit derived from (meth)acrylic acid and a structural unit derived from methyl (meth)acrylate, etc. Japanese Patent Application Laid-Open No. 2007-197703 and Japanese Patent Application Laid-Open No. 2010-96919 are incorporated herein by reference in their entirety.
[0053] The N-substituted or unsubstituted glutarimide unit is a unit having an N-substituted or unsubstituted 2,6-dioxopiperidinediyl structure.
[0054] Examples of the unit having an N-substituted or unsubstituted 2,6-dioxopiperidinediyl structure include a structural unit represented by formula (1).
[0055]
[0056] In formula (1), R 1 Each is independently a hydrogen atom or a methyl group, preferably a methyl group. 2It is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms containing an aromatic ring, preferably a hydrogen atom, a methyl group, an n-butyl group, a cyclohexyl group, or a benzyl group, and more preferably a methyl group, an n-butyl group, or a cyclohexyl group.
[0057] The structural unit represented by formula (1) can be obtained, for example, by reacting the corresponding acid anhydride (IIa) with NH2R 2 It can be produced by reaction with an imidizing agent represented by formula (A) or by intramolecular cyclization of a copolymer having a partial structure of formula (C). In order to convert the structural unit represented by formula (A) into the structural unit represented by formula (1) by intramolecular cyclization, heating is preferably performed.
[0058] Solution (i)
[0059]
[0060] (Where R 1 , R 2 As defined above.)
[0061] The N-substituted or unsubstituted glutarimide unit can be obtained by the method described in WO2005 / 10838A1, Japanese Patent Application Laid-Open No. 2010-254742, Japanese Patent Application Laid-Open No. 2008-273140, Japanese Patent Application Laid-Open No. 2008-274187, etc., specifically, by reacting two adjacent structural units derived from methyl methacrylate or glutaric anhydride units with an imidizing agent such as ammonia, methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, tert-butylamine, n-hexylamine, etc., amines containing an aliphatic hydrocarbon group, aniline, toluidine, trichloroaniline, etc., amines containing an alicyclic hydrocarbon group, such as cyclohexylamine, urea, 1,3-dimethylurea, 1,3-diethylurea, 1,3-dipropylurea, etc. Among them, methylamine is preferred. Two adjacent structural units or glutaric anhydride units derived from methyl methacrylate can be reacted with an imidizing agent, and then reacted with a dialkyl carbonate such as dimethyl carbonate to convert a carboxylic acid such as methacrylic acid into an alkyl methacrylate such as methyl methacrylate. Carboxylic acid can be generated by hydrolysis of methacrylate or glutaric anhydride units represented by formula (II), or by reaction of glutaric anhydride units represented by formula (II) with an imidizing agent to generate carboxylic acid and amide. The reaction of dimethyl carbonate can be carried out in the presence of a tertiary amine such as triethylamine. WO2005 / 10838A1, Japanese Patent Publication No. 2010-254742, Japanese Patent Publication No. 2008-273140, and Japanese Patent Publication No. 2008-274187 are incorporated herein by reference in their entirety.
[0062] In the methacrylic copolymer of the present invention, the ratio of the structural unit (R) is preferably 6 to 30% by mass, more preferably 7.5 to 25% by mass, and further preferably 8 to 25% by mass relative to the total structural units. By changing the ratio of the structural unit (R) to methyl methacrylate, the oriented birefringence of the methacrylic copolymer can be changed. In addition, the more the content of the structural unit (R), the higher the heat resistance of the methacrylic copolymer, but there is a tendency for the flexibility to decrease, the compatibility with other copolymers, and the molding processability to decrease. When the ratio of the structural unit (R) is within the above range relative to the total structural units, a methacrylic copolymer having high heat resistance and transparency, a positive value for oriented birefringence and a negative value for the photoelastic coefficient, the ability to reduce the birefringence of the molded body, and excellent compatibility with other resins can be obtained, so it is preferred.
[0063] In a preferred embodiment of the present invention, the methacrylic acid copolymer of the present invention may contain 0 to 2 mass %, more preferably 0 to 1.5 mass %, further preferably 0 to 1.0 mass %, and most preferably 0 to 0.5 mass % of the methacrylic acid amide unit represented by the above formula (A) and the 2-(hydroxyalkyl)acrylate unit represented by the above formula (B), respectively, relative to all the structural units. When the structural units of formula (A) and / or (B) exceed the above range, the saturated water absorption of the obtained methacrylic acid copolymer becomes high, or a cross-linked body is formed during molding, which becomes a foreign matter defect and the appearance quality is reduced.
[0064] The methacrylic copolymer of the present invention may also contain structural units (O) other than methyl methacrylate units, α-methylstyrene units and (R). As structural units (O), there may be listed units derived from vinyl monomers having only one polymerizable carbon-carbon double bond in one molecule, such as (meth)acrylamide, (meth)acrylonitrile, (meth)acrylic acid, styrene, structural units represented by formula (A), and structural units represented by formula (B). In the methacrylic copolymer of the present invention, the proportion of structural units (O) is preferably 10% by mass or less relative to all structural units. It should be noted that the proportions of methyl methacrylate units, α-methylstyrene units, structural units (R) and structural units (O) can be calculated by 1 H-NMR etc.
[0065] The weight average molecular weight (Mw) of the methacrylic acid copolymer of the present invention is preferably 40,000 to 200,000, more preferably 50,000 to 180,000, and even more preferably 55,000 to 160,000. When Mw is 40,000 or more, the strength and toughness of the molded article of the present invention are improved. When Mw is 200,000 or less, the fluidity of the methacrylic acid copolymer of the present invention is improved, and the molding processability is improved.
[0066] The weight average molecular weight (Mw) is a value calculated by converting a chromatogram measured by gel permeation chromatography into a molecular weight of standard polystyrene.
[0067] The acid value of the methacrylic acid copolymer of the present invention is preferably 0.01 to 0.30 mmol / g, more preferably 0.05 to 0.28 mmol / g. The acid value is a value proportional to the content of the carboxylic acid unit and the carboxylic anhydride unit in the methacrylic acid copolymer. The acid value can be calculated, for example, by the method described in Japanese Unexamined Patent Publication No. 2005-23272. When the acid value is within the above range, the balance of heat resistance, mechanical properties, and molding processability is excellent.
[0068] The glass transition temperature of the methacrylic acid copolymer of the present invention is preferably 120° C., more preferably 121° C., and further preferably 122° C. as a lower limit, and is not particularly limited as an upper limit, but is preferably 160° C. The higher the glass transition temperature of the methacrylic acid copolymer, the less likely the molded article containing the methacrylic acid copolymer is to deform or shrink due to heat, that is, the higher the heat resistance.
[0069] In this specification, "glass transition temperature (Tg)" is measured in accordance with JIS K7121. Specifically, the temperature is raised to 230°C once, then cooled to room temperature, and then the temperature is raised from room temperature to 230°C at a rate of 10°C / min, and a DSC curve is measured under such conditions. The midpoint obtained from the DSC curve measured during the second temperature increase is determined as the "glass transition temperature (Tg)".
[0070] The methacrylic copolymer of the present invention preferably has a negative sign of the photoelastic coefficient measured by the method described below and a positive sign of the orientation birefringence measured by the method described below. When such a methacrylic copolymer is included in a molded article, a molded article with low birefringence can be easily provided.
[0071] The lower limit of the above-mentioned orientation birefringence is preferably 0.1×10 -4 , more preferably 0.5×10 -4 , more preferably 1.0×10 -4 The upper limit is not particularly limited, but is preferably 2.0×10 -3 .
[0072] The upper limit of the photoelastic coefficient is preferably -0.1×10 -12 / Pa, more preferably -0.2×10 -12 / Pa, more preferably -0.5×10 -12 / Pa, the lower limit is not particularly limited, but is preferably -2.0×10 -11 / Pa.
[0073] The inventors of the present invention regard the reduction of orientation birefringence and the reduction of stress birefringence as different issues. When the methacrylic copolymer of the present invention is alloyed with other resins having birefringence of different signs, it helps to suppress the orientation birefringence and photoelastic coefficient (or stress birefringence) of the resin composition to zero or to a low level.
[0074] Regarding the photoelastic coefficient, under the conditions of a distance between chucks of 45 mm and a temperature of 23°C, for a press-formed sheet of 15 mm in width × 60 mm in length × 1.0 mm in thickness composed of a methacrylic copolymer, a tension is applied by increasing 10 N each time from 0 N until 100 N. Each time the tension increases, the birefringence of the central part of the sheet is measured at a temperature of 23°C and the D-line wavelength of Na. The relationship between the measured stress and birefringence is approximated as a linear function by the least squares method, and the slope calculated at this time is used as the photoelastic coefficient. It should be noted that the stress is the value obtained by dividing the tension by the cross-sectional area of the sheet. The cross-sectional area of the sheet is calculated as the product of the sheet width 15 mm and the thickness of the measuring point in the central part of the sheet. Birefringence is defined as the refractive index n of light having a polarization plane parallel to the stretching direction. p The refractive index n of light with a polarization plane perpendicular to the stretching direction o The difference (Δn = n p -n o ).
[0075] The orientation birefringence is the birefringence measured as follows: the central part of a stretched film obtained by stretching a methacrylic copolymer in a size of 20 mm in width, 40 mm in length, and 1.0 mm in thickness in one direction by 10% at a temperature 10°C higher than the glass transition temperature at a speed of 3 mm / min is measured without applying tension under the conditions of a temperature of 23°C and a wavelength of the Na D line. Since the methacrylic copolymer of the present invention has a positive orientation birefringence and a negative photoelastic coefficient, the magnitude of the orientation birefringence and the photoelastic coefficient can be adjusted. Therefore, by mixing other resins having different signs from the orientation birefringence or the photoelastic coefficient, such as styrene-acrylonitrile copolymer (orientation birefringence: negative, photoelastic coefficient: positive), polymethyl methacrylate (orientation birefringence: negative, photoelastic coefficient: negative), polybenzyl methacrylate (orientation birefringence: positive, photoelastic coefficient: positive), etc., at an arbitrary ratio, the orientation birefringence and photoelastic birefringence of the obtained molded product can be reduced.
[0076] The methacrylic copolymer of the present invention can be obtained by a method including a step of subjecting a copolymer of methyl methacrylate and α-methylstyrene (hereinafter sometimes referred to as a precursor polymer) to a ring structure-forming reaction.
[0077] That is, the methacrylic copolymer of the present invention can be obtained by a production method comprising the following steps: a step of continuously supplying a reaction raw material including a monomer mixture containing 70 to 93% by mass of methyl methacrylate, 30 to 7% by mass of α-methylstyrene and 0 to 10% by mass of a copolymerizable monomer, a free radical polymerization initiator and, if necessary, a chain transfer agent to a tank reactor; a step of bulk polymerizing the monomer mixture in the tank reactor until the polymerization conversion rate reaches 30 to 60% by mass to obtain a reaction product; a step of removing the monomer mixture from the reaction product; and a step of subjecting the obtained precursor polymer to a ring structure forming reaction.
[0078] The precursor polymer is a substance obtained by polymerizing a reaction raw material including a monomer mixture, a free radical polymerization initiator, and a chain transfer agent as required, wherein the monomer mixture contains 70 to 93% by mass, preferably 75 to 90% by mass of methyl methacrylate, and 30 to 7% by mass, preferably 25 to 10% by mass of α-methylstyrene.
[0079] The copolymerizable monomer is contained in an amount of 0 to 10% by mass, preferably 0 to 5% by mass.
[0080] The monomer mixture may contain monomers other than methyl methacrylate and α-methylstyrene. Examples of such monomers include alkyl methacrylates other than methyl methacrylate such as ethyl methacrylate and butyl methacrylate; aryl methacrylates such as phenyl methacrylate; cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornyl methacrylate; aryl acrylates such as phenyl acrylate; cycloalkyl acrylates such as cyclohexyl acrylate and norbornyl acrylate; aromatic vinyl monomers such as styrene; acrylamide; methacrylamide; acrylonitrile; methacrylonitrile; and other vinyl monomers having only one polymerizable olefin group in one molecule. The content of the monomers other than methyl methacrylate and alkyl acrylate in the monomer mixture is preferably 10% by mass or less, and more preferably 5% by mass or less.
[0081] The monomer mixture may contain monomers other than methyl methacrylate and α-methylstyrene. Examples of such monomers include alkyl methacrylates other than methyl methacrylate such as ethyl methacrylate and butyl methacrylate; aryl methacrylates such as phenyl methacrylate; cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornyl methacrylate; aryl acrylates such as phenyl acrylate; cycloalkyl acrylates such as cyclohexyl acrylate and norbornyl acrylate; aromatic vinyl monomers such as styrene; acrylamide; methacrylamide; acrylonitrile; methacrylonitrile; and other vinyl monomers having only one polymerizable olefin group in one molecule. The content of the monomers other than methyl methacrylate and alkyl acrylate in the monomer mixture is preferably 10% by mass or less, and more preferably 5% by mass or less.
[0082] The b* of the monomer mixture is preferably -1 to 2, more preferably -0.5 to 1.5. When b* is within this range, when the obtained methacrylic copolymer is molded, it is advantageous in that a molded product with almost no coloring is obtained with high production efficiency. It should be noted that b* is a value measured according to the International Commission on Illumination (CIE) standard (1976) or JIS Z-8722.
[0083] The monomer mixture removed from the reaction product by the step of removing the monomer mixture in the reaction product can be recovered and reused in the present invention. When the b* of the recovered monomer mixture increases due to heat applied during recovery, it is preferably purified by an appropriate method to make b* within the above range.
[0084] The polymerization initiator used in the present invention is not particularly limited as long as it generates reactive radicals. Examples thereof include tert-hexyl peroxyisopropyl monocarbonate, tert-hexyl peroxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, tert-hexyl peroxypivalate, tert-butyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1,1-bis(tert-hexylperoxy)cyclohexane, benzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, lauroyl peroxide, 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), and dimethyl 2,2'-azobis(2-methylpropionate). Of these, tert-hexyl peroxy-2-ethylhexanoate, 1,1-bis(tert-hexylperoxy)cyclohexane, and dimethyl 2,2'-azobis(2-methylpropionate) are preferred.
[0085] The average initiator concentration (I) of the polymerization initiator used in the present invention that is not cracked at the polymerization temperature in the tank reactor described below is preferably 5.1×10 -5 ~2.4×10 -4(mol / L) range.
[0086] The polymerization initiator is added to the monomer mixture in an amount to achieve the above-mentioned initiator concentration (I) depending on the polymerization temperature.
[0087] Examples of the chain transfer agent used in the present invention include alkyl mercaptans such as n-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, 1,4-butanedithiol, 1,6-hexanedithiol, ethylene glycol dithiopropionate, butanediol dithioglycolate, butanediol dithiopropionate, hexanediol dithioglycolate, hexanediol dithiopropionate, trimethylolpropane tris-(β-thiopropionate), and pentaerythritol tetrathiopropionate; and terpinolene.
[0088] Among them, monofunctional alkyl mercaptans such as n-octyl mercaptan and n-dodecyl mercaptan are preferred. These chain transfer agents can be used alone or in combination of two or more. The amount of the chain transfer agent used is preferably 0 to 1 part by mass, more preferably 0.01 to 0.8 parts by mass, and further preferably 0.02 to 0.6 parts by mass relative to 100 parts by mass of the monomer mixture.
[0089] In principle, no solvent is used in bulk polymerization, but in the case where the viscosity of the reaction solution needs to be adjusted, a solvent may be contained in the monomer mixture. As the solvent, aromatic hydrocarbons such as benzene, toluene, and ethylbenzene are preferred. These solvents may be used alone or in combination of two or more. The amount of the solvent used is preferably 30 parts by mass or less, more preferably 10 parts by mass or less relative to 100 parts by mass of the monomer mixture.
[0090] The dissolved oxygen content of the reaction raw materials used in the present invention is preferably 10 ppm or less, more preferably 5 ppm or less, further preferably 4 ppm or less, and most preferably 3 ppm or less. If the dissolved oxygen content is set to such a range, the polymerization reaction proceeds smoothly and it is easy to obtain a molded product without silver streaks or coloring.
[0091] The temperature in the tank reactor, that is, the temperature of the liquid in the reaction tank, is preferably 110 to 140° C., more preferably 114 to 135° C. When the temperature is higher than this range, it is difficult to generate a high molecular weight product containing α-methylstyrene, resulting in a decrease in heat resistance.
[0092] In the method for producing a methacrylic acid copolymer of the present invention, the water content in the reaction liquid in the tank reactor is preferably 1000 ppm or less, more preferably 700 ppm or less, and even more preferably 280 ppm or less. By making the water content 1000 ppm or less, the generation of resin foreign matter of several μm to several tens of μm during the polymerization reaction can be suppressed, and when the obtained methacrylic acid copolymer is melt-molded into a film or sheet, the generation of defects of several tens of μm in outer diameter with the resin foreign matter as the core can be greatly reduced.
[0093] In the tank reactor, bulk polymerization is preferably carried out until the polymerization conversion rate reaches 30 to 65% by mass, preferably 35 to 60% by mass.
[0094] In addition, the average residence time (θ) of the reaction raw materials in the tank reactor is preferably 1.5 to 5 hours, more preferably 2 to 4.5 hours, and further preferably 2.5 to 4 hours. When the average residence time is too short, the required amount of the polymerization initiator increases. In addition, there is a tendency that the polymerization reaction is difficult to control and the molecular weight is difficult to control due to the increase in the polymerization initiator. On the other hand, when the average residence time is too long, it takes time for the reaction to reach a stable state, and there is a tendency for productivity to decrease. The average residence time can be adjusted according to the capacity of the tank reactor and the supply amount of the reaction raw materials.
[0095] Bulk polymerization is preferably performed in an inert gas atmosphere such as nitrogen.
[0096] The manufacturing method of the present invention has a step of removing the monomer mixture in the reaction product. Here, the reaction product is not limited to the reaction product obtained by bulk polymerization in a tank reactor, but may also be a reaction product obtained by other reactors connected after the tank reactor as needed, that is, a reaction product in which the unreacted monomer mixture in the reaction product obtained by bulk polymerization in the tank reactor is further polymerized by other reactors to improve the polymerization conversion rate. In addition, in this step, the solvent is also removed at the same time as needed. There is no particular limitation on the removal method, and a heating devolatilization method is preferred. As the heating devolatilization method, equilibrium flash method and adiabatic flash method can be listed, and adiabatic flash method is preferred. The temperature for implementing the adiabatic flash method is preferably 200-280°C, more preferably 220-280°C, and further preferably 220-270°C. When the temperature for implementing the adiabatic flash method is lower than 200°C, devolatilization takes time, devolatilization becomes insufficient, and sometimes silver streaks and other poor appearance are caused in the molded product. On the other hand, when the temperature for implementing the adiabatic flash method exceeds 280°C, the methacrylic copolymer tends to be colored and depolymerized due to oxidation, scorching, decomposition, etc. The adiabatic flash method can also be performed in multiple stages. In this case, the reaction product flowing through the heat transfer tube can be heated by the vapor of the flashed monomer mixture, and the heated reaction product can be supplied to a low-pressure flash tank for flash evaporation. The reaction product can be pressurized by a pump or the like. After removing the monomer mixture, the methacrylic copolymer can be made into pellets or powder according to a known method to facilitate the handling as a molding material. The content of the monomer mixture in the methacrylic copolymer obtained in the present invention is preferably 1% by mass or less, more preferably 0.5% by mass or less.
[0097] The glass transition temperature of the precursor polymer is preferably 114°C, more preferably 115°C, and further preferably 117°C as the lower limit, and preferably 150°C as the upper limit. The glass transition temperature can be changed by adjusting the molecular weight, the amount of α-methylstyrene copolymerization, etc. The higher the glass transition temperature of the precursor polymer, the higher the heat resistance. For the methacrylic copolymer obtained using a precursor polymer with a high glass transition temperature, even if the amount of the structural unit (R) is small, it has high heat resistance, so it is difficult to cause deterioration of the saturated water absorption rate, etc.
[0098] The precursor polymer is not particularly limited as long as the total content of structural units derived from methyl methacrylate is 70 to 93% by mass and the total content of structural units derived from α-methylstyrene is 30 to 7% by mass. From the viewpoints of polymerizability, transparency, etc., the total content of structural units derived from methyl methacrylate in the precursor polymer is preferably 73% to 93% by mass, more preferably 75% to 92% by mass, and most preferably 80% to 92% by mass.
[0099] From the viewpoints of heat resistance, polymerizability, water absorption, etc., the total content of the structural units derived from α-methylstyrene in the precursor polymer is preferably 7% by mass or more and 27% by mass or less, and more preferably 8% by mass or more and 25% by mass or less. When the structural units derived from α-methylstyrene are less than this range, sufficient heat resistance cannot be obtained, and when they are more than this range, polymerizability is significantly reduced.
[0100] For the precursor polymer, in the chromatogram obtained by gel permeation chromatography, the weight average molecular weight Mw converted to polystyrene is preferably 30000 or more and 200000 or less, more preferably 40000 or more and 180000 or less, and further preferably 50000 or more and 160000 or less. When the weight average molecular weight Mw is less than this range, the obtained molded body becomes brittle, and when it is higher than this range, the productivity deteriorates. Mw can be controlled by adjusting the type, amount, addition period, etc. of the polymerization initiator or chain transfer agent (optional component) used when manufacturing the precursor polymer.
[0101] The ring structure forming reaction can be carried out using an extruder, for example. As an extruder, for example: a single screw extruder, a twin screw extruder, a multi-screw extruder, etc. can be cited. From the viewpoint of mixing performance, a twin screw extruder is preferred. The twin screw extruder includes a non-meshing co-rotating type, a meshing co-rotating type, a non-meshing counter-rotating type, and a meshing counter-rotating type. The meshing co-rotating type can rotate at a high speed and can efficiently promote mixing, so it is preferred. These extruders can be used alone or connected in series.
[0102] In the ring structure formation reaction using an extruder, for example, a precursor polymer as a raw material can be added from the raw material input part of the extruder to melt the precursor polymer. After the barrel is filled, an imidizing agent (optional component) and the like are injected into the extruder using an addition pump, thereby performing a ring structure formation reaction in the extruder. When an imidizing agent is used, the structural unit (R) generates an N-substituted or unsubstituted glutarimide unit, and may also generate a lactone ring unit and / or a glutaric anhydride unit as required. In the case of not using an imidizing agent, the structural unit (R) generates a lactone ring unit and / or a glutaric anhydride unit. Preferred imidizing agents are R 2 -NH2(R 2 As defined above). The imidizing agent is used in an amount of 1.6 to 12 parts by mass based on 100 parts by mass of the methacrylic copolymer. When the imidizing agent is used in an amount within the above range, the accompanying generation of methacrylic acid amide units can be suppressed.
[0103] The resin temperature of the reaction zone in the extruder is preferably set in the range of 180 to 280°C, more preferably in the range of 200 to 280°C. When the resin temperature of the reaction zone is lower than 180°C, there is a tendency for the heat resistance of the methacrylic copolymer to decrease due to a decrease in the reaction efficiency of the ring structure formation reaction, the concomitant generation of methacrylic acid amide units, etc. When the resin temperature of the reaction zone exceeds 280°C, there is a tendency for the decomposition of the resin to become significant, and the mechanical strength such as the tensile strength of the molded body and film composed of the obtained methacrylic acid copolymer to decrease. It should be noted that the reaction zone in the extruder refers to the area between the injection position of the imidizing agent, etc. and the resin discharge port (die head) in the barrel of the extruder.
[0104] By extending the reaction time in the reaction zone of the extruder, the ring structure formation reaction can be further carried out. The reaction time in the reaction zone of the extruder is preferably longer than 10 seconds, and more preferably longer than 30 seconds. In the case of a reaction time of less than 10 seconds, the ring structure formation reaction may hardly proceed.
[0105] The resin pressure in the extruder is preferably set within the range of atmospheric pressure to 50 MPa, and more preferably within the range of 1 to 30 MPa. When it exceeds 50 MPa, the mechanical pressure resistance limit of a normal extruder is exceeded, and a special device is required, which is not preferred in terms of cost.
[0106] It is preferred to use an extruder having vent holes capable of reducing pressure to below atmospheric pressure. With such a configuration, unreacted products, byproducts such as methanol, and monomers can be removed, and the breaking strength of the molded article containing the methacrylic acid copolymer of the present invention tends to be improved.
[0107] In the ring structure forming reaction, a reaction apparatus that can cope with high viscosity, such as a horizontal twin-screw reactor such as Bioluck manufactured by Sumitomo Heavy Industries, Ltd. or a vertical twin-screw stirring tank such as Superbronze, can be preferably used instead of an extruder.
[0108] During the ring structure formation reaction, a carboxyl group is sometimes generated in the methacrylic copolymer. The carboxyl group can be converted into an ester group by an esterifying agent or a catalyst as needed. Thus, the foaming of the resin during the manufacture of the optical film can be reduced. The ester group varies depending on the esterifying agent or catalyst used, but from the perspective of reducing the melt viscosity of the resin during melt molding, the reactivity of esterification, and the heat resistance of the resin after esterification, it is preferred to contain a methyl methacrylate unit, and more preferably contain a methyl methacrylate unit and an ethyl methacrylate unit at the same time.
[0109] As the esterification agent, dimethyl carbonate is preferred from the viewpoints of cost, reactivity, and the like.
[0110] The amount of the esterifying agent added can be set, for example, so that the acid value of the methacrylic acid-based copolymer becomes a desired value.
[0111] In addition to the above-mentioned esterification agent, a catalyst may be used in combination. The type of catalyst is not particularly limited, and examples thereof include amine compounds such as trimethylamine, triethylamine, monomethyldiethylamine, and dimethylmonoethylamine. Among them, triethylamine is preferred from the viewpoints of cost, reactivity, etc.
[0112] Additives commonly used in resin compositions may be contained within the scope of not impairing the purpose of the present invention. Examples of additives include fillers, antioxidants, heat-resistant agents, ultraviolet light absorbers, light stabilizers, lubricants, mold release agents, polymer processing aids, antistatic agents, flame retardants, colorants, dyes, pigments, light diffusers, organic pigments, matting agents, impact-resistant modifiers, phosphors, etc. The total amount of the additives other than the fillers is preferably 7% by mass or less, more preferably 5% by mass or less, and further preferably 4% by mass or less.
[0113] The antioxidant is effective in preventing the oxidative degradation of the resin in the presence of oxygen. Examples thereof include phosphorus antioxidants, hindered phenol antioxidants, thioether antioxidants, etc. These antioxidants may be used alone or in combination of two or more.
[0114] The thermal degradation inhibitor can prevent thermal degradation of the resin by capturing polymer radicals generated when the resin is exposed to high heat in a substantially oxygen-free state.
[0115] Examples of the thermal degradation inhibitor include 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-hydroxybenzyl)-4-methylphenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd.; trade name: SUMILIAZER GM), and 2,4-di-tert-amyl-6-(3',5'-di-tert-amyl-2'-hydroxy-α-methylbenzyl)phenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd.; trade name: SUMILIAZER GS).
[0116] The ultraviolet absorber is a compound that has the ability to absorb ultraviolet rays. The ultraviolet absorber is a compound that mainly has the function of converting light energy into heat energy.
[0117] Examples of ultraviolet absorbers include benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, oxalylanilides, malonic esters, and formamidines. These may be used alone or in combination of two or more. Among them, benzotriazoles, triazines, or a maximum value ε of the molar absorption coefficient at a wavelength of 380 to 450 nm are preferred. max 1200dm 3 ·mol -1 cm -1 The following ultraviolet absorbers.
[0118] Benzotriazoles have a high effect of suppressing the decrease in optical properties such as coloration caused by ultraviolet rays, and are therefore preferably used as ultraviolet absorbers when the molded article of the present invention is applied to optical applications. As benzotriazoles, 2-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (manufactured by BASF; trade name TINUVIN329), 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (manufactured by BASF; trade name TINUVIN234), 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-tert-octylphenol] (manufactured by ADEKA; trade name LA-31), 2-(5-octylthio-2H-benzotriazole-2-yl)-6-tert-butyl-4-methylphenol, etc. are preferred.
[0119] In addition, the maximum value of the molar absorption coefficient at a wavelength of 380 to 450 nm is max 1200dm 3 ·mol -1 cm -1 The following ultraviolet absorbers can suppress the yellow tint of the obtained molded body. As such ultraviolet absorbers, 2-ethyl-2'-ethoxy-oxalylanilide (manufactured by Clariant Japan Co., Ltd.; trade name SUNDUBOA VSU) and the like can be cited. Among these ultraviolet absorbers, benzotriazoles are preferably used from the viewpoint of suppressing the degradation of the resin caused by ultraviolet rays.
[0120] In addition, when it is desired to efficiently absorb short wavelengths of 380 nm or less, it is preferred to use a triazine type ultraviolet absorber. Examples of such ultraviolet absorbers include 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine (manufactured by ADEKA; trade name LA-F70), its analogues hydroxyphenyltriazine type ultraviolet absorbers (manufactured by BASF; trade names TINUVIN477, TINUVIN460, TINUVIN479), and 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine.
[0121] In addition, when it is desired to particularly effectively absorb light with a wavelength of 380 to 400 nm, it is preferred to use a metal complex having a ligand with a heterocyclic structure disclosed in WO2011 / 089794A1, WO2012 / 124395A1, Japanese Patent Publication No. 2012-012476, Japanese Patent Publication No. 2013-023461, Japanese Patent Publication No. 2013-112790, Japanese Patent Publication No. 2013-194037, Japanese Patent Publication No. 2014-62228, Japanese Patent Publication No. 2014-88542, Japanese Patent Publication No. 2014-88543, etc. as an ultraviolet absorber. WO2011 / 089794A1, WO2012 / 124395A1, Japanese Patent Application Publication No. 2012-012476, Japanese Patent Application Publication No. 2013-023461, Japanese Patent Application Publication No. 2013-112790, Japanese Patent Application Publication No. 2013-194037, Japanese Patent Application Publication No. 2014-62228, Japanese Patent Application Publication No. 2014-88542, and Japanese Patent Application Publication No. 2014-88543 are incorporated herein by reference in their entirety.
[0122] Examples of the heterocyclic ligand include 2,2'-iminobisbenzothiazole, 2-(2-benzothiazolylamino)benzo oxadiazole, 2-(2-benzothiazolylamino)benzimidazole, (2-benzothiazolyl)(2-benzimidazolyl)methane, bis(2-benzo The metal complex preferably comprises bis(2-benzothiazolyl)methane, bis(2-benzothiazolyl)methane, bis[2-(N-substituted)benzimidazolyl]methane and their derivatives. As the central metal of such a metal complex, copper, nickel, cobalt and zinc are preferably used. In addition, in order to use these metal complexes as ultraviolet absorbers, it is preferred to disperse the metal complex in a medium such as a low molecular weight compound or a polymer. The amount of the metal complex added is preferably 0.01 to 5 parts by mass, and more preferably 0.1 to 2 parts by mass relative to 100 parts by mass of the molded body of the present invention. The molar absorption coefficient of the above-mentioned metal complex at a wavelength of 380 to 400 nm is large, so there is no problem with a small amount added to obtain a sufficient ultraviolet absorption effect. When the amount added is small, the deterioration of the appearance of the molded body caused by bleeding, etc. can be suppressed. In addition, the above-mentioned metal complex has high heat resistance, so the deterioration and decomposition during molding are less. In addition, the above-mentioned metal complex has high light resistance, so the ultraviolet absorption performance can be maintained for a long time.
[0123] It should be noted that the maximum value of the molar absorption coefficient of the ultraviolet absorber is max The measurement is as follows. 10.00 mg of ultraviolet absorber is added to 1 L of cyclohexane and dissolved so that there is no undissolved matter by visual observation. The solution is injected into a quartz glass cell of 1 cm × 1 cm × 3 cm, and the absorbance at a wavelength of 380 to 450 nm is measured using a spectrophotometer (manufactured by Hitachi, Ltd.; trade name U-3410). The molecular weight (M) of the ultraviolet absorber is used to determine the absorbance. UV ) and the maximum absorbance (A max ) The maximum value of the molar absorption coefficient ε is calculated by the following formula: max .
[0124] ε max =[Amax / (10×10 -3 )]×MUV
[0125] The light stabilizer is a compound that mainly has the function of capturing free radicals generated by oxidation due to light. Preferred light stabilizers include hindered amines such as compounds having a 2,2,6,6-tetraalkylpiperidine skeleton.
[0126] Examples of the lubricant include stearic acid, behenic acid, stearamide acid, methylenebisstearamide, hydroxystearic acid triglyceride, paraffin, ketone wax, caprylic alcohol, and hydrogenated oil.
[0127] Examples of the release agent include higher alcohols such as cetyl alcohol and stearyl alcohol; higher fatty acid esters of glycerol such as stearic acid monoglyceride and stearic acid diglyceride. In the present invention, it is preferred to use higher alcohols and glycerol fatty acid monoesters in combination as the release agent. When higher alcohols and glycerol fatty acid monoesters are used in combination, the ratio is not particularly limited, and the amount of higher alcohol used: the amount of glycerol fatty acid monoester used is preferably 2.5:1 to 3.5:1, more preferably 2.8:1 to 3.2:1 in terms of mass ratio.
[0128] As a polymer processing aid, polymer particles (non-crosslinked rubber particles) having a particle size of 0.05 to 0.5 μm that can be produced by emulsion polymerization are generally used. The polymer particles may be single-layer particles composed of a polymer having a single composition ratio and a single intrinsic viscosity, or may be multi-layer particles composed of two or more polymers having different composition ratios or intrinsic viscosities.
[0129] Examples of the antistatic agent include alkyl sulfonates such as sodium heptyl sulfonate, sodium octyl sulfonate, sodium nonyl sulfonate, sodium decyl sulfonate, sodium dodecyl sulfonate, sodium hexadecyl sulfonate, sodium octadecyl sulfonate, sodium diheptyl sulfonate, potassium heptyl sulfonate, potassium octyl sulfonate, potassium nonyl sulfonate, potassium decyl sulfonate, potassium dodecyl sulfonate, potassium hexadecyl sulfonate, potassium octadecyl sulfonate, potassium diheptyl sulfonate, lithium heptyl sulfonate, lithium octyl sulfonate, lithium nonyl sulfonate, lithium decyl sulfonate, lithium dodecyl sulfonate, lithium hexadecyl sulfonate, lithium octadecyl sulfonate, and lithium diheptyl sulfonate.
[0130] As flame retardants, there can be listed: metal hydrates having hydroxyl groups or water of crystallization such as magnesium hydroxide, aluminum hydroxide, hydrated aluminum silicate, hydrated magnesium silicate, hydrotalcite, polyphosphate amines, phosphoric acid compounds such as phosphate esters, silicon compounds, etc., preferably phosphate ester flame retardants such as trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, tripentyl phosphate, trihexyl phosphate, tricyclohexyl phosphate, triphenyl phosphate, tricresyl phosphate, tri(xylene) phosphate, dimethyl ethyl phosphate, methyl dibutyl phosphate, ethyl dipropyl phosphate, and hydroxyphenyl diphenyl phosphate.
[0131] Examples of dyes / pigments include red organic pigments such as para red, fire red, pyrazolone red, thioindigo red, and perylene red; blue organic pigments such as phthalocyanine blue and indanthrene blue; and green organic pigments such as phthalocyanine green and naphthol green. One or more of these can be used.
[0132] As the organic dye, a compound having a function of converting ultraviolet light into visible light is preferably used.
[0133] Examples of the light diffusing agent and the matting agent include glass fine particles, polysiloxane crosslinked fine particles, crosslinked polymer fine particles, talc, calcium carbonate, and barium sulfate.
[0134] Examples of the fluorescent substance include fluorescent pigments, fluorescent dyes, fluorescent white dyes, fluorescent brighteners, and fluorescent bleaching agents.
[0135] The methacrylic acid copolymer composition of the present invention is not particularly limited by its production method, and can be produced, for example, by melt-kneading the methacrylic acid copolymer of the present invention, additives such as ultraviolet absorbers, and other polymers with different signs of oriented birefringence or photoelastic coefficients selected as needed. Melt-kneading can be carried out using, for example, a melt-kneading device such as a kneader, an extruder, a mixing roll, a Banbury mixer, etc. The temperature during kneading can be appropriately set according to the softening temperatures of the methacrylic acid copolymer and other polymers, for example, it can be set to 150 to 300°C. In addition, the shear rate during kneading can be set, for example, to 10 to 5000 seconds. -1 .
[0136] The methacrylic acid copolymer composition of the present invention may be in the form of pellets or the like in order to improve convenience during storage, transportation or molding.
[0137] The molded body of the present invention comprises the methacrylic copolymer or methacrylic copolymer composition of the present invention. The method for manufacturing the molded body of the present invention is not particularly limited. Examples thereof include: T-die method (lamination method, coextrusion method, etc.), inflation method (coextrusion method, etc.), compression molding method, blow molding method, calendering method, vacuum forming method, injection molding method (insertion method, two-color method, pressing method, core withdrawal method, sandwich method, etc.) and other melt molding methods and solution casting method, etc. Among them, from the perspective of productivity, cost, etc., T-die method, inflation method, injection molding method or solution casting method are preferred. The type of molded body is not limited, and films (planar molded bodies with a thickness of 5 μm or more and 250 μm or less) and sheets (planar molded bodies thicker than 250 μm) can be cited as preferred molded bodies.
[0138] The molded article of the present invention has an average absolute value of in-plane phase difference (retardation; Re) of preferably 10.0 nm or less, more preferably 6.0 nm or less, further preferably 5.0 nm or less, and further preferably 3.0 nm or less per 1 mm thickness.
[0139] The film as one mode of the molded body of the present invention can be produced by solution casting, melt casting, extrusion molding, inflation molding, blow molding, etc. Among them, extrusion molding or solution casting is preferred from the viewpoint of obtaining a film with excellent transparency, improved toughness, excellent workability, and excellent balance between toughness and surface hardness and rigidity. The temperature of the molten resin discharged from the extruder is preferably set to 160 to 270°C, more preferably 220 to 260°C.
[0140] In the extrusion molding method, from the viewpoint of obtaining a good surface smoothness, good mirror gloss, and a low haze film, the T-die method is preferred. In the T-die method, the molten resin discharged from the T-die head through an extruder, a gear pump, a polymer filter, and a mixer is sandwiched between two or more mirror rollers or mirror belts to form a film. A slope may or may not be formed when sandwiched between the mirror rollers or mirror belts. The die head has an automatic adjustment function for the die lip opening, and the air gap is preferably less than 100 mm.
[0141] The mirror roller or mirror belt is preferably made of metal. As the mirror roller, a metal rigid roller, a metal elastic roller, etc. can be used, and a metal elastic roller and a metal rigid roller are preferably used in combination. In addition, the surface temperature of the mirror roller or the mirror belt is preferably below 130°C. In addition, the surface temperature of at least one of a pair of mirror rollers or mirror belts is preferably above 60°C. If such a surface temperature is set, the molten resin ejected from the extruder can be cooled at a faster rate than natural cooling, and it is easy to manufacture a film with excellent surface smoothness and low haze. The linear pressure between a pair of rollers or belts is preferably 10N / mm or more, more preferably 30N / mm or more. The thickness of the unstretched film obtained by extrusion molding is preferably 10 to 300μm. The haze of the film is preferably 0.7% or less, more preferably 0.5% or less, and further preferably 0.3% or less when the thickness is 100μm.
[0142] The unstretched film obtained as described above can be subjected to a stretching treatment. By stretching treatment, the mechanical strength is improved, and a film that is difficult to crack can be obtained. The stretching method is not particularly limited, and examples thereof include a simultaneous biaxial stretching method, a sequential biaxial stretching method, and a tube stretching method. From the viewpoint that a film can be stretched uniformly and a high-strength film can be obtained, the lower limit of the temperature during stretching is a temperature 10°C higher than the glass transition temperature of the methacrylic copolymer or the methacrylic copolymer composition, and the upper limit of the temperature during stretching is a temperature 40°C higher than the glass transition temperature of the methacrylic copolymer or the methacrylic copolymer composition. Stretching is usually performed at 100 to 5000% / min. After stretching, a film with less heat shrinkage can be obtained by thermal fixing. The thickness of the film after stretching is preferably 10 to 200 μm.
[0143] A functional layer may be provided on the surface of the film as one embodiment of the molded article of the present invention. Examples of the functional layer include a hard coat layer, an anti-glare layer, an anti-reflection layer, an anti-adhesion layer, a diffusion layer, an anti-glare layer, an antistatic layer, an antifouling layer, and a slippery layer of microparticles.
[0144] In order to improve the adhesion strength with the functional layer or to improve the adhesion strength when laminated with other films via an adhesive or pressure-sensitive adhesive, it is preferred that a primer layer be provided on at least one surface of the film of the present invention.
[0145] By laminating a layer containing the methacrylic copolymer or methacrylic copolymer composition of the present invention with other materials (e.g., a layer containing other thermoplastic copolymers), a laminate can be obtained. Other materials used in the laminate include plastics (e.g., thermoplastic resins), glass, etc. The laminate obtained by the present invention can be suitably used for the surface of automobile interior components, mobile phone surfaces, personal computer surfaces, vending machine surfaces, etc.
[0146] The film as one embodiment of the molded article of the present invention has high transparency and heat resistance, and is therefore suitable for optical applications, and is particularly suitable for polarizer protective films, liquid crystal protective plates, surface materials of portable information terminals, display window protective films of portable information terminals, light guide films, transparent conductive films coated with silver nanowires or carbon nanotubes on the surface, and front panels of various displays. The film of the present invention has high transparency and heat resistance, and therefore, as applications other than optical applications, it can be used for infrared cut-off films, anti-fouling films, anti-scattering films, decorative films, metal decorative films, shrink films, and films for in-mold labels.
[0147] When the film as one mode of the molded body of the present invention is used as a polarizer protective film or a phase difference film, it can be laminated only on one side of the polarizer film or on both sides. When laminated with the polarizer film, it can be laminated via an adhesive layer or an adhesive layer. As the polarizer film, a stretched film composed of a polyvinyl alcohol resin and iodine can be used, and the film thickness is preferably 1 to 100 μm.
[0148] Example
[0149] Next, the present invention will be described in more detail with reference to examples. It should be noted that the present invention is not limited to the examples.
[0150] The measurement of physical properties and the like was carried out by the following methods.
[0151] (Polymerization conversion rate)
[0152] A gas chromatograph GC-14A manufactured by Shimadzu Corporation was connected to INERTCAP1 (df = 0.4 μm, 0.25 mm I.D. × 60 m) manufactured by GL Sciences Inc. as a chromatographic column, and analysis was performed under the following conditions, and calculations were performed based on the conditions.
[0153] Injection temperature = 250°C
[0154] Detector temperature = 250°C
[0155] Temperature conditions: maintain at 60°C for 5 minutes → increase the temperature to 250°C at 10°C / min → maintain at 250°C for 10 minutes
[0156] (Molecular weight distribution Mw / Mn)
[0157] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the resin are determined by GPC (gel permeation chromatography). 4 mg of the resin to be measured is dissolved in 5 ml of tetrahydrofuran to prepare a sample solution. The temperature of the column oven is set to 40°C, and 20 μl of the sample solution is injected into the device at an eluent flow rate of 0.35 ml / min to measure the chromatogram. GPC measurement is performed on 10 points of standard polystyrene with a molecular weight range of 400 to 5,000,000, and a calibration curve showing the relationship between retention time and molecular weight is prepared. Based on the calibration curve, the Mw and Mw / Mn of the resin to be measured are determined.
[0158] Equipment: GPC equipment HLC-8320 manufactured by Tosoh Corporation
[0159] Separation column: TSKguardcolumSuperHZ-H, TSKgelHZM-M and TSKgelSuperHZ4000 manufactured by Tosoh Corporation are connected in series
[0160] Eluent: Tetrahydrofuran
[0161] Eluent flow rate: 0.35ml / min
[0162] Column temperature: 40°C
[0163] Detection method: Differential refractive index (RI)
[0164] (Composition of each unit in the copolymer)
[0165] pass 1 The proton ratio of the phenyl group of the α-methylstyrene unit or the styrene unit to the methoxy group of the methyl methacrylate unit was determined by H-NMR, and the content of the α-methylstyrene unit or the styrene unit was calculated therefrom.
[0166] (Glass transition temperature Tg)
[0167] The methacrylic acid copolymer obtained in the example was measured for a DSC curve using a differential scanning calorimeter (DSC-50 (product number) manufactured by Shimadzu Corporation) in accordance with JIS K7121, with the temperature being raised to 250° C. once, then cooled to room temperature, and then raised from room temperature to 200° C. at a rate of 10° C. / min. The midpoint glass transition temperature obtained from the DSC curve measured at the second temperature rise was defined as the glass transition temperature of the present invention.
[0168] (Imidization rate)
[0169] use 1H-NMR (manufactured by Bruker; trade name ULTRA SHIELD 400PLUS) was used to analyze the copolymers. 1 In H-NMR measurement, the value obtained from the peak area A of the O-CH3 group derived from methyl methacrylate near 3.5 to 3.8 ppm and the peak area B of the N-CH3 group derived from glutarimide near 3.0 to 3.3 ppm was taken as the imidization ratio (mol %).
[0170] (imidization rate (mol%)) = [B / (A+B)] × 100
[0171] The imidization ratio (weight %) was calculated from the imidization ratio (mol %).
[0172] (Photoelastic coefficient)
[0173] The methacrylic acid copolymer is press-formed to obtain a 1.0 mm sheet. A 15 mm × 60 mm test piece is cut from the center of the obtained press-formed sheet. The two ends of the cut sheet in the long side direction are fixed in a manner with a distance between the chucks of 45 mm, and the X-axis dovetail slide B05-11BM manufactured by Suruga Seiki is used to apply tension to the sheet in stages from 0 N to 100 N, 10 N at a time. The tension T is monitored by a sensor-separated digital dynamometer ZPS-DPU-50N manufactured by IMONDA Co., Ltd. The phase difference PD under the conditions of the D-line wavelength of Na is measured using KOBRA-WR manufactured by Oji Measuring Instruments under the conditions of the Na D-line wavelength. After the phase difference is measured, the sheet is removed from the fixture and the thickness d of the phase difference measurement part is measured. The cross-sectional area S = 15 mm × d, stress σ (= T / S) and birefringence Δn (= PD / d) of the sheet were calculated from the measured values, and a plot was made with stress σ on the horizontal axis and birefringence Δn on the vertical axis. The slope of the straight line obtained by the least squares method was used as the photoelastic coefficient.
[0174] (Orientation Birefringence)
[0175] The methacrylic copolymer is press-formed to obtain a 1.0 mm sheet. A test piece of 20 mm × 40 mm is cut out from the central portion of the obtained press-formed sheet, and the test piece is set in an AUTOGRAPH (manufactured by SHIMADZU) with a heating chamber. The distance between the clamps in the AUTOGRAPH is set to 20 mm, and maintained at the glass transition temperature + 10°C for 3 minutes. Then, it is stretched 100% in one direction at a speed of 3 mm / min (the distance between the clamps is 40 mm). The obtained stretched film is cooled to 23°C, removed from the AUTOGRAPH, and the phase difference PD of the central portion of the stretched film is measured using KOBRA-WR manufactured by Oji Measuring Instruments under the condition of the D-line wavelength of Na. The thickness d of the phase difference measurement portion is measured. The birefringence Δn (=PD / d) is calculated from the measured value and is used as the oriented birefringence.
[0176] Production Example 1
[0177] In an autoclave A equipped with a stirrer, purified methyl methacrylate (MMA), α-methylstyrene (αMS), 2,2'-azobis(2-methylpropionitrile) (AIBN) and n-octyl mercaptan (n-OM) were added in the ratios shown in Table 1 and uniformly dissolved to obtain a polymerization raw material.
[0178] The polymerization raw material was continuously supplied from the autoclave A to a tank reactor controlled to the polymerization temperature described in Table 1 at 1.5 kg / hour, and a polymerization reaction was carried out by a bulk polymerization method at the average residence time described in Table 1, and a liquid containing a methacrylic acid copolymer was continuously discharged from the tank reactor. The polymerization conversion rate was the value described in Table 1. Next, the liquid discharged from the reactor was heated to 230°C and supplied to a twin-screw extruder controlled to 240°C. The volatile components mainly composed of unreacted monomers were separated and removed in the twin-screw extruder, and the methacrylic acid copolymer was extruded in the form of strands. The strands were cut with a pelletizer to obtain pellets of the methacrylic acid copolymer Aa.
[0179] Production Example 2
[0180] Except that the composition of the raw material liquid and the polymerization conditions were changed as shown in Table 1, the same procedure as in Production Example 1 was carried out to obtain pellets of a methacrylic acid-based polymer Ab.
[0181] Production Example 3
[0182] According to the method for producing the copolymer (A) described in the item [Example] of Japanese Patent Gazette No. 2003-231785, an MS resin (a copolymer of methyl methacrylate (MMA) and styrene (St)) is produced. The mass ratio of MMA, St and tert-dodecyl mercaptan (t-DM) put into the autoclave is changed to obtain a liquid containing a methacrylic copolymer Ac. Next, the liquid containing the methacrylic copolymer is heated to 230°C and supplied to a twin-screw extruder controlled at 240°C. In the twin-screw extruder, volatile components mainly composed of unreacted monomers are separated and removed, and the methacrylic copolymer is extruded in the form of strands. The strands are cut with a pelletizer to obtain pellets of the methacrylic copolymer Ac.
[0183] The copolymer pellets were used to measure the weight average molecular weight Mw, molecular weight distribution Mw / Mn, the ratio of α-methylstyrene units or styrene units, and the glass transition temperature Tg. The results are shown in Table 1. It should be noted that in this production example, the amount of units derived from MMA is the amount of units other than α-methylstyrene units or styrene units, so the description in the table is omitted.
[0184] [Table 1]
[0185] Table 1
[0186]
[0187] <Example 1>
[0188] The copolymer [Aa] shown in Preparation Example 1 was supplied at 2 kg / hour to the conveying section of a twin-screw extruder (manufactured by Teknobel; trade name KZW20TW-45MG-NH-600) which was composed of a conveying section, a melt-kneading section, a devolatilization section and a discharge section and whose screw speed was set to 120 rpm and whose temperature was set to 250°C. In the melt-kneading section provided with a kneading block, monomethylamine was injected at 0.10 kg / hour from the additive supply port of the twin-screw extruder to react the precursor polymer [Aa] with the monomethylamine. It should be noted that a reverse thread was provided on the screw at the end of the reaction zone.
[0189] In the devolatilization section set at 20 Torr (about 2.7 kPa), by-products and excess monomethylamine are volatilized from the molten resin passing through the melt-kneading section and discharged through the vent.
[0190] The molten resin extruded in the form of strands from a die provided at the end of the discharge section of the twin-screw extruder was cooled in a water tank and then cut with a pelletizer to obtain a pelletized methacrylic copolymer (Aa-1).
[0191] The copolymer (Aa-1) was supplied at 1 kg / hour to the conveying section of a twin-screw extruder (manufactured by Teknobel; trade name KZW20TW-45MG-NH-600) consisting of a conveying section, a melt-kneading section, a devolatilization section and a discharge section, the screw speed being set at 100 rpm and the temperature being set at 230°C. In the melt-kneading section provided with a kneading block, a liquid consisting of 0.8 parts by mass of dimethyl carbonate and 0.2 parts by mass of triethylamine was injected at 0.024 kg / hour to react the carboxyl groups in the methacrylic copolymer (Aa-1) with dimethyl carbonate. It should be noted that a reverse thread was provided on the screw at the end of the reaction zone.
[0192] In the devolatilization section set at 20 Torr (about 2.7 kPa), by-products and excess dimethyl carbonate are volatilized from the molten resin passing through the melt kneading section and discharged through the vent.
[0193] The molten resin extruded in the form of strands from a die provided at the end of the discharge section of the twin-screw extruder was cooled in a water tank and then cut with a pelletizer to obtain a pelletized methacrylic copolymer (Aa-2).
[0194] The methacrylic acid copolymer (Aa-2) was supplied at 1 kg / hour to the conveying section of a twin-screw extruder (manufactured by Technobel Co., Ltd.; trade name KZW20TW-45MG-NH-600) which was composed of a conveying section, a melt-kneading section, a devolatilization section and a discharge section and had a screw speed of 100 rpm and a temperature of 230°C.
[0195] In the devolatilization section set at 20 Torr (about 2.7 kPa), volatile components such as unreacted products are volatilized from the molten resin passing through the melt-kneading section and discharged through the vent.
[0196] The molten resin extruded in the form of strands from a die head provided at the end of the discharge section of the twin-screw extruder was cooled in a water tank and then cut with a pelletizer to obtain pelletized methacrylic copolymer [1]. The methacrylic copolymer [1] had an imidization rate of 8.6 mol%, a glass transition temperature of 130°C, and an orientation birefringence of 8.4×10 -4 , the photoelastic coefficient is -5.5×10 -12 Pa -1 Table 2 shows the physical properties of the methacrylic copolymer [1].
[0197] <Example 2>
[0198] In Example 1, a methacrylic acid copolymer [2] was obtained by the same method as in Example 1 except that the amount of monomethylamine added was 0.15 kg / hour and a liquid composed of 0.8 parts by mass of dimethyl carbonate and 0.2 parts by mass of triethylamine was injected at 0.036 kg / hour. The physical properties of the methacrylic acid copolymer [2] are shown in Table 2.
[0199] <Comparative Example 1>
[0200] A methacrylic acid copolymer [3] was obtained by the same method as in Example 1 except that the methacrylic acid copolymer Ac was used as the precursor resin. Table 2 shows the physical properties of the methacrylic acid copolymer [3].
[0201] <Example 3>
[0202] 50 parts by mass of the methacrylic copolymer [2] synthesized in Example 1 and 50 parts by mass of the methacrylic resin synthesized in Production Example 2 were kneaded at 230° C. using a small melt kneader to obtain a methacrylic copolymer composition. The physical properties of the methacrylic copolymer composition [4] are shown in Table 3.
[0203] <Comparative Examples 2, 3, and 4>
[0204] The physical properties were evaluated in the same manner as in Example 1 except that the copolymers [Aa], [Ab], and [Ac] shown in Production Example 1 were used instead of the methacrylic copolymer [1].
[0205] <Comparative Example 5 (3FMA)>
[0206] 100 parts by mass of 2,2,2-trifluoroethyl methacrylate (3FMA), 0.06 parts by mass of azobisisobutyronitrile, 0.2 parts by mass of octyl mercaptan, 231 parts by mass of water, 1.4 parts by mass of a dispersant, and 17.5 parts by mass of a pH adjuster were added to the autoclave. While stirring the autoclave, the liquid temperature was raised from room temperature to 70°C, maintained at 70°C for 120 minutes, and then maintained at 120°C for 60 minutes to carry out suspension polymerization. The liquid temperature was lowered to room temperature, and the polymerization reaction liquid was extracted from the autoclave. The solid component was taken out from the polymerization reaction liquid by filtration, washed with water, and dried with hot air at 80°C for 24 hours. The obtained solid component was supplied to the hopper of the twin-screw extruder and melt-kneaded at a barrel temperature of 230°C. Then, the molten resin was extruded to obtain a pelletized fluoromethylacrylate polymer. In the subsequent operation, the same operation as in Example 1 was performed to evaluate the physical properties. The evaluation results are shown in Table 3.
[0207] <Comparative Example 6>
[0208] 50 parts by mass of the fluoromethylacrylate polymer synthesized in Comparative Example 3 and 50 parts by mass of the methacrylic resin synthesized in Preparation Example 2 were kneaded at 230°C using a small melt kneader to obtain a methacrylic copolymer composition. The methacrylic copolymer composition had two glass transition temperatures of 72°C and 120°C, and was incompatible. The appearance was turbid, and the orientation birefringence and photoelastic coefficient could not be measured.
[0209] [Table 2]
[0210] Table 2
[0211] Example 1 Example 2 Comparative Example 1 Methacrylic acid copolymer [1] [2] [3] Polymers used in imidization modification Aa Aa Ac Imidization rate mol% 8.6 13.0 9.0 Content of methyl methacrylate structural unit weight% 79.5 73.6 77.3 Content of α-methylstyrene structural unit weight% 8.0 8.0 - Content of styrene structural units weight% - - 10.0 Content of N-methylglutarimide structural unit weight% 12.5 18.4 12.7 Weight average molecular weight after imidization reaction (Mw) 90k 90k 95k Glass transition temperature ℃ 130 140 120 Orientation Birefringence <![CDATA[×10 -4 ]]> 8.4 13.8 -10.3 Photoelastic coefficient <![CDATA[×10 -12 / Well]]> -5.5 -6.3 -2.4
[0212] [Table 3]
[0213] Table 3
[0214] Example 3 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Methacrylic acid copolymer[2] weight% 50 Methacrylic acid copolymer [Aa] weight% 100 Methacrylic acid polymer [Ab] weight% 50 100 50 Methacrylic acid copolymer [Ac] weight% 100 3FMA polymer weight% 100 50 Weight average molecular weight (Mw) g / mol 90k 92k 75k 95k 90k 90k Imidization rate mol% 6.5 - - - - - Glass transition temperature ℃ 130 127 120 116 72 Incompatible Orientation Birefringence <![CDATA[x10 -4 ]]> 5.6 -2.23 -2.6 -27.2 -2.6 - Photoelastic coefficient <![CDATA[×10 -12 / Well]]> -5.4 -4.0 -4.6 -3.2 -1.7 -
[0215] The methacrylic acid copolymers obtained in Examples 1 to 2 and the methacrylic acid copolymer compositions obtained in Example 3 have high heat resistance, positive orientation birefringence and negative photoelastic coefficient, and excellent compatibility with other resins, so they can be suitably used as materials constituting optical components. In particular, by mixing with other resins having different signs of orientation birefringence or photoelastic coefficient (for example, styrene-acrylonitrile copolymer (orientation birefringence: negative, photoelastic coefficient: positive), polymethyl methacrylate (orientation birefringence: negative, photoelastic coefficient: negative), polybenzyl methacrylate (orientation birefringence: positive, photoelastic coefficient: positive)), the birefringence of the phase difference of the obtained molded body can be reduced, which is useful in this respect. On the other hand, the methacrylic acid copolymers obtained in Comparative Examples 1 to 5 are not within the scope of the present invention, so they have low heat resistance and negative orientation birefringence, and the methacrylic acid copolymer composition obtained in Comparative Example 6 is an incompatible system, which are all inferior to the present invention.
Claims
1. A methacrylic acid copolymer having a glass transition temperature of 120° C. or higher, comprising 40 to 87% by mass of methyl methacrylate units, 6 to 30% by mass of structural units (R) having at least one ring structure selected from the group consisting of lactone ring units, glutaric anhydride units and N-substituted or unsubstituted glutarimide units in the main chain, and 7 to 30% by mass of α-methylstyrene units, wherein: The photoelastic coefficient of the methacrylic copolymer has a negative value, and a stretched film obtained by stretching a press-molded sheet of the methacrylic copolymer having a size of 20 mm in width, 40 mm in length, and 1.0 mm in thickness in one direction by 100% at a speed of 3 mm / min at a temperature 10° C. higher than the glass transition temperature has a positive orientation birefringence.
2. The methacrylic acid copolymer according to claim 1, wherein The structural unit (R) is an N-substituted or unsubstituted glutarimide unit represented by formula (1), In formula (1), R 1 are each independently a hydrogen atom or a methyl group, R 2 It is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms and containing an aromatic ring.
3. A composition obtained by melt-kneading the methacrylic acid copolymer according to claim 1 or 2 and other resin. 4 . A formed article comprising the methacrylic copolymer according to claim 1 or 2 or the composition according to claim 3 .
5. The formed body according to claim 4, wherein The shaped body is a film or a sheet. 6 . A method for producing a film or a sheet, comprising the step of molding the methacrylic acid copolymer according to claim 1 or 2 or the composition according to claim 3 into a film or a sheet by a melt molding method.
7. A method for producing a film or a sheet, comprising the step of forming the methacrylic acid copolymer according to claim 1 or 2 or the composition according to claim 3 into a film or a sheet by a solution casting method. 8 . A laminate having at least one layer consisting of a film or sheet comprising the methacrylic copolymer according to claim 1 or 2 or the composition according to claim 3 .