Acrylic composition and molded article
By synthesizing a copolymer containing methyl methacrylate, ring structure and α-methylstyrene in an acrylic resin and adding an elastomer, the problem of deterioration of the heat-resistant resin in the prior art is solved, and high Heat resistance, low water absorption and excellent dimensional stability and surface hardness.
Patent Information
- Application Number
- CN202180022720.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-26
- Filing Date
- 2021-03-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-03-26
AI Technical Summary
When the existing heat-resistant acrylic resin improves mechanical strength and surface hardness, the dimensional stability and water absorption problems have not been fully solved, resulting in deterioration of its performance.
51 to 99 mass % acrylic copolymer is used, and contains 30 to 87 mass % methyl methacrylate units, 6 to 40 mass % structural units having a ring structure and 7 to 30 mass % α-methylbenzene. An ethylene unit was added to 1 to 49% by mass of the elastomer, and acrylic resin composition with high heat resistance and low water absorption was formed by specific polymerization and imidation reactions.
High heat resistance, low water absorption, excellent dimensional stability and surface hardness are achieved, which prevents the brittleness and dimensional changes of the resin and improves the overall performance of the molded body.
Smart Images

Figure BDA0003854294600000031 
Figure BDA0003854294600000051 
Figure BDA0003854294600000071
Abstract
Description
Technical Field
[0001] The present invention relates to an acrylic resin composition and a molded body. Background Art
[0002] Methacrylic resins are excellent in transparency, weather resistance, surface hardness, etc. By molding an acrylic resin composition containing a methacrylic resin, various components for display components, electronic and electrical components, transport components, etc. can be obtained. In recent years, there has been a demand for improvement in the performance of various components, and in particular, there has been a strong demand for improvement in heat resistance.
[0003] In order to improve heat resistance, an acrylic resin composition having a ring structure in the main chain skeleton has been proposed. For example, Patent Document 1 discloses a modified methacrylic resin containing a structural unit derived from methyl methacrylate or the like, and a structural unit having at least one ring structure in the main chain and selected from the group consisting of a lactone ring unit, a glutaric anhydride unit, and an N-substituted or unsubstituted glutarimide unit. In addition, Patent Document 2 discloses a copolymer containing a (meth)acrylate monomer unit, an unsaturated dicarboxylic anhydride monomer unit, and an unsaturated aromatic vinyl monomer unit.
[0004] In addition, since acrylic resins with high heat resistance have relatively low strength and low toughness, there is a concern that the impact resistance of the molded body is insufficient, and the productivity is deteriorated in terms of the molding processability and operability of the film. As a technology for improving the strength of heat-resistant acrylic resins, a technology containing an elastomer is disclosed. Patent document 3 discloses a technology in which a cross-linked elastomer having a multilayer structure is included as an elastomer in an acrylic resin containing a glutaric anhydride unit. In addition, patent document 4 discloses a technology in which acrylic rubber is added as an elastomer to an acrylic resin containing a maleic anhydride unit. In addition, patent document 5 discloses a technology in which a block copolymer containing a methacrylate polymer block and an acrylate polymer block is added as an elastomer to an acrylic resin containing a structural unit having at least one ring structure in the main chain, the structural unit being selected from the group consisting of a lactone ring unit, a maleic anhydride unit, a glutaric anhydride unit, a glutarimide unit, an N-substituted maleimide unit, and a tetrahydropyran ring structural unit. Patent Document 6 discloses a technique of adding a graft copolymer as an elastomer to an acrylic resin having a glass transition temperature of 120° C. or higher and a refractive index of 1.50 or higher, and an imidized resin of a methyl methacrylate-styrene copolymer as the acrylic resin is described in the examples.
[0005] Citation List
[0006] Patent Literature
[0007] Patent Document 1: JP2017-179103A
[0008] Patent Document 2: WO2014 / 021264A1
[0009] Patent Document 3: JP2000-178399A
[0010] Patent Document 4: JPH05-119217A
[0011] Patent Document 5: JP2016-008225A
[0012] Patent Document 6: JP2009-203348A Summary of the invention
[0013] Technical issues
[0014] In any of the techniques disclosed in the prior art, the strength of the heat-resistant acrylic resin is improved, but deterioration of surface hardness, deterioration of dimensional stability due to increased water absorption, etc. are observed, and the excellent characteristics inherent in the acrylic resin cannot be fully exhibited.
[0015] In view of the above circumstances, an object of the present invention is to provide an acrylic resin composition and a molded article which maintain heat resistance and mechanical strength (toughness) and have excellent surface hardness and dimensional stability.
[0016] Solution to the problem
[0017] As a result of studies for achieving the above-mentioned object, the present invention including the following embodiments has been completed. [1]
[0019] An acrylic resin composition, comprising:
[0020] 51 to 99% by mass of an acrylic copolymer (A) containing 30 to 87% by mass of methyl methacrylate units, 6 to 40% by mass of a structural unit (R) having at least one ring structure in the main chain, 7 to 30% by mass of an α-methylstyrene unit, and 0 to 20% by mass of other vinyl monomer units (C) copolymerizable with methyl methacrylate, wherein the structural unit (R) is selected from the group consisting of a glutaric anhydride unit and an N-substituted or unsubstituted glutarimide unit; and
[0021] 1 to 49% by mass of the elastomer (B). [2]
[0023] The acrylic resin composition according to [1], wherein the structural unit (R) is an N-substituted glutarimide unit represented by formula (I):
[0024]
[0025] In formula (I), R 1 are each independently a hydrogen atom or a methyl group, and R 2 It is an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aromatic ring-containing organic group having 6 to 15 carbon atoms. [3]
[0027] The acrylic resin composition according to [1] or [2], wherein the other vinyl monomer unit (C) copolymerizable with the methyl methacrylate unit comprises at least one selected from the group consisting of an acrylic acid ester monomer, an aromatic vinyl monomer and a vinyl cyanide monomer. [4]
[0029] The acrylic resin composition according to any one of [1] to [3], wherein the other vinyl monomer unit (C) copolymerizable with the methyl methacrylate unit comprises at least one selected from the group consisting of methyl acrylate, ethyl acrylate, styrene and acrylonitrile. [5]
[0031] The acrylic resin composition according to any one of [1] to [3], wherein the other vinyl monomer unit (C) copolymerizable with the methyl methacrylate unit contains styrene. [6]
[0033] The acrylic resin composition according to any one of [1] to [5], wherein the elastomer (B) comprises a multilayer copolymer elastomer containing a methacrylate unit and an acrylate unit. [7]
[0035] The acrylic resin composition according to any one of [1] to [6], wherein the elastomer (B) contains a block copolymer elastomer comprising a polymer block (b1) containing a methacrylate unit and a polymer block (b2) containing an acrylate unit. [8]
[0037] The acrylic resin composition according to any one of [1] to [7], wherein the softening temperature of the molded article is 110° C. or higher when measured by the method specified in the B50 method of JIS K7206. [9]
[0039] The acrylic resin composition according to any one of [1] to [8], wherein the saturated water absorption is 2.5% or less.
[10]
[0041] A molded body comprising the acrylic resin composition according to any one of [1] to [9].
[11]
[0043] A film comprising the acrylic resin composition according to any one of [1] to [9].
[0044] Advantageous Effects of the Invention
[0045] According to the present invention, a molded body having high heat resistance and low water absorption, and a film having excellent dimensional stability and high surface hardness can be obtained. DETAILED DESCRIPTION
[0046] The acrylic resin composition of the present invention contains an acrylic copolymer (A) and an elastomer (B). The content of the acrylic copolymer (A) in the acrylic resin composition is 51 to 99% by mass, preferably 55 to 95% by mass, and more preferably 60 to 90% by mass. When the content of the acrylic copolymer (A) in the acrylic resin composition is 51% by mass or more, heat resistance and surface hardness are excellent, and when the content of the acrylic copolymer (A) in the acrylic resin composition is 99% by mass or less, brittleness is prevented.
[0047] (Acrylic copolymer (A))
[0048] The acrylic copolymer (A) according to the present invention contains methyl methacrylate units, α-methylstyrene units and structural units (R). The acrylic copolymer according to the present invention may further contain other vinyl monomer units (C) copolymerizable with methyl methacrylate. The other vinyl monomer units (C) copolymerizable with methyl methacrylate may contain methacrylamide units represented by the following formula (A) and methyl 2-(hydroxyalkyl)acrylate units represented by the following formula (B).
[0049]
[0050] (In the formula, R 3 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aromatic ring-containing organic group having 6 to 15 carbon atoms, preferably a hydrogen atom, a methyl group, an n-butyl group, a cyclohexyl group or a benzyl group, more preferably a methyl group, an n-butyl group or a cyclohexyl group, and R 4 and R 5Each independently is a hydrogen atom or an organic group having 1 to 20 carbon atoms, preferably a hydrogen atom or an organic group having 1 to 10 carbon atoms, more preferably a hydrogen atom or an organic group having 1 to 5 carbon atoms, wherein the organic group is not particularly limited as long as it has 1 to 20 carbon atoms, and examples thereof include a linear or branched alkyl group, a linear or branched aryl group, -OCOCH 3 The organic group may contain heteroatoms such as oxygen atoms, and R 4 Preferably, it is a methyl group, and R 5 Preferably it is a hydrogen atom.)
[0051] In the acrylic copolymer (A) according to the present invention, the ratio of the methyl methacrylate unit relative to all structural units is 30 to 87 mass %, preferably 40 to 85 mass %, and more preferably 55 to 80 mass %. When the ratio of the methyl methacrylate unit is less than this range, the total light transmittance of the obtained acrylic copolymer is deteriorated, and when the ratio of the methyl methacrylate unit is greater than this range, the heat resistance of the obtained acrylic copolymer is deteriorated.
[0052] In the acrylic copolymer (A) according to the present invention, the ratio of the α-methylstyrene unit relative to all structural units is 7 to 30% by mass, preferably 8 to 27% by mass, and more preferably 11 to 25% by mass. When the ratio of the α-methylstyrene unit is less than this range, the saturated water absorption of the obtained acrylic copolymer increases. In addition, the acrylic copolymer having a ratio of the α-methylstyrene unit exceeding 30% by mass has low polymerizability and low productivity.
[0053] The structural unit (R) is a structural unit having at least one ring structure in the main chain, and the structural unit (R) is selected from the group consisting of glutaric anhydride units and N-substituted or unsubstituted glutarimide units. The acrylic copolymer according to the present invention may contain a methacrylamide unit represented by formula (A) and / or a 2-(hydroxyalkyl)acrylate unit represented by formula (B) in the main chain.
[0054] The glutaric anhydride unit is a unit having a 2,6-dioxodihydropyrandiyl structure. Examples of the unit having a 2,6-dioxodihydropyrandiyl structure may include a structural unit represented by formula (II).
[0055]
[0056] In formula (II), R 6 are each independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and the two R 6 Preferred is a methyl group.
[0057] The unit having a 2,6-dioxodihydropyrandiyl structure can be included in the acrylic copolymer by the methods described in JP2007-197703A, JP2010-096919A, etc., for example, by intramolecular cyclization of two adjacent structural units derived from (meth)acrylic acid, intramolecular cyclization of a structural unit derived from (meth)acrylic acid and a structural unit derived from methyl (meth)acrylate, etc. JP2007-197703A and JP2010-096919A are incorporated herein by reference in their entirety.
[0058] The N-substituted or unsubstituted glutarimide unit is a unit having an N-substituted or unsubstituted 2,6-dioxopiperidinediyl structure.
[0059] Examples of the unit having an N-substituted or unsubstituted 2,6-dioxopiperidinediyl structure may include a structural unit represented by Formula (I).
[0060]
[0061] In formula (I), R 1 are each independently a hydrogen atom or a methyl group, and the two R 1 Preferably it is a methyl group. 2 It is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aromatic ring-containing organic group having 6 to 15 carbon atoms. Since it can reduce the water absorption rate, a methyl group, an n-butyl group, a cyclohexyl group or a benzyl group is preferred, a methyl group, an n-butyl group or a cyclohexyl group is more preferred, and a methyl group is most preferred.
[0062] The structural unit represented by formula (I) can be obtained, for example, by reacting the corresponding acid anhydride (IIa) with a compound represented by R 2 NH 2 It can be prepared by reacting an imidizing agent represented by, or by intramolecular cyclization of a copolymer having a partial structure of formula (III). It is preferred to heat to convert the structural unit represented by formula (III) into the structural unit represented by formula (I) by intramolecular cyclization.
[0063] Solution (i)
[0064]
[0065] (In the formula, R 1 and R 2 As defined above.)
[0066] The N-substituted or unsubstituted glutarimide unit can be obtained by the methods described in WO2005 / 10838A1, JP2010-254742A, JP2008-273140A, JP2008-274187A, etc., specifically, by reacting two adjacent structural units derived from methyl methacrylate or glutaric anhydride units with an imidizing agent, such as an amine containing an aliphatic hydrocarbon group such as ammonia, methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, tert-butylamine or n-hexylamine, an amine containing an aromatic hydrocarbon group such as aniline, toluidine or trichloroaniline, an amine containing an alicyclic hydrocarbon group such as cyclohexylamine, urea, 1,3-dimethylurea, 1,3-diethylurea or 1,3-dipropylurea. Among them, methylamine is preferred. WO2005 / 10838A1, JP2010-254742A, JP2008-273140A and JP2008-274187A are incorporated herein by reference in their entirety. During the imidization reaction, a portion of the methyl methacrylate unit may be hydrolyzed to become a carboxyl group, and the carboxyl group is preferably restored to the original methyl methacrylate unit by an esterification reaction treated with an esterifying agent. The esterifying agent is not particularly limited as long as it can show the effect of the present application, and dimethyl carbonate and trimethylacetate can be appropriately used. In addition, in addition to the esterifying agent, tertiary amines such as trimethylamine, triethylamine or tributylamine can also be used in combination as a catalyst.
[0067] In the acrylic copolymer (A) according to the present invention, the ratio of the structural unit (R) relative to all structural units is 6 to 40% by mass, preferably 7.5 to 35% by mass, and more preferably 8 to 30% by mass. The orientation birefringence of the acrylic copolymer can be changed by changing the ratio of the structural unit (R) to methyl methacrylate. In addition, as the content of the structural unit (R) increases, the heat resistance of the acrylic copolymer improves, but the flexibility, compatibility with other copolymers and molding processability of the acrylic copolymer tend to deteriorate.
[0068] Examples of other vinyl monomer units (C) copolymerizable with the methyl methacrylate unit (hereinafter, may be described as monomer units (C)) include acrylic acid ester monomer units (C-1), aromatic vinyl monomer units (C-2), vinyl cyanide monomer units (C-3) and monomer units other than these units (C-4). Other vinyl monomer units (C) copolymerizable with the methyl methacrylate unit may be used alone or in combination of two or more thereof.
[0069] As the monomer unit (C), a suitable material may be selected according to the properties required of the acrylic copolymer of the present invention, and in the case where properties such as thermal stability, fluidity, chemical resistance, optical properties and compatibility with other resins are particularly required, at least one selected from the group consisting of an acrylic acid ester monomer unit, an aromatic vinyl monomer unit and a vinyl cyanide monomer unit is preferred.
[0070] The acrylic acid ester monomer unit (C-1) constituting the acrylic copolymer according to the present invention is not particularly limited, and from the viewpoints of heat resistance, fluidity, heat resistance stability, productivity, etc., preferably is methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, sec-butyl acrylate, 2-ethylhexyl acrylate, benzyl acrylate, cyclohexyl acrylate, phenyl acrylate, etc., more preferably is methyl acrylate, ethyl acrylate, n-butyl acrylate, etc., and from the viewpoint of productivity, methyl acrylate, ethyl acrylate, etc. are even more preferred.
[0071] The acrylic acid ester monomer units (C-1) may be used alone or in combination of two or more thereof.
[0072] When the acrylic acid ester monomer unit (C-1) is used, the content thereof is preferably 20% by mass or less, more preferably 10% by mass or less, based on all structural units, from the viewpoint of heat resistance and thermal stability.
[0073] The aromatic vinyl monomer unit (C-2) constituting the acrylic copolymer according to the present invention is not particularly limited, and from the viewpoints of heat resistance, fluidity, heat resistance stability, productivity, etc., styrene (St), o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, p-tert-butylstyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 1,1-diphenylethylene, isopropenyltoluene, isopropenylethylbenzene, isopropenylpropylbenzene, isopropenylbutylbenzene, isopropenylbenzylbenzene, isopropenylhexylbenzene, isopropenyloctylbenzene, etc. are preferred, and from the viewpoint of copolymerization reactivity with α-methylstyrene during the production of a precursor polymer described below, styrene is more preferred.
[0074] The aromatic vinyl monomer units (C-2) may be used alone or in combination of two or more thereof.
[0075] When the aromatic vinyl monomer unit (C-2) is used, the content thereof is preferably 3 mass % to 20 mass % and more preferably 4 mass % to 15 mass % based on all structural units from the viewpoint of heat resistance and thermal stability.
[0076] The vinyl cyanide monomer unit (C-3) constituting the acrylic copolymer according to the present invention is not particularly limited, but is preferably acrylonitrile (AN), methacrylonitrile, vinylene cyanide, etc. from the viewpoints of heat resistance, fluidity, heat resistance stability, chemical resistance, productivity, etc., and among them, acrylonitrile is preferred from the viewpoints of availability and chemical resistance impartment.
[0077] The vinyl cyanide monomer unit (C-3) may be used alone or in combination of two or more thereof.
[0078] When the vinyl cyanide monomer unit (C-3) is used, the content thereof is preferably 20% by mass or less, more preferably 10% by mass or less, based on all structural units, from the viewpoint of heat resistance and thermal stability.
[0079] The monomer forming the monomer unit (C-4) other than (C-1) to (C-3) constituting the acrylic copolymer according to the present invention is not particularly limited and may be a monomer corresponding to the methacrylamide unit represented by formula (A) or a monomer corresponding to the 2-(hydroxyalkyl)acrylate unit represented by formula (B), and examples thereof include amides such as acrylamide and methacrylamide; monomers obtained by esterifying the hydroxyl groups at both ends of ethylene glycol or its oligomer with acrylic acid or methacrylic acid, such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate; monomers obtained by esterifying the hydroxyl groups of two alcohols with acrylic acid or methacrylic acid, such as neopentyl glycol di(meth)acrylate; and monomers obtained by esterifying a polyol derivative with acrylic acid or methacrylic acid, such as trimethylolpropane and pentaerythritol.
[0080] Among the monomers constituting the above-mentioned monomer unit (C), at least one selected from the group consisting of methyl acrylate (MA), ethyl acrylate, styrene and acrylonitrile is preferred from the viewpoint of availability, and styrene is more preferred from the viewpoint of moisture resistance.
[0081] In the acrylic copolymer according to the present invention, the ratio of the other vinyl monomer units (C) copolymerizable with the methyl methacrylate units is preferably 0 to 20% by mass, more preferably 0 to 15% by mass, and even more preferably 0 to 10% by mass, relative to all the structural units. When the ratio of the other vinyl monomer units (C) copolymerizable with the methyl methacrylate units exceeds 20% by mass, the heat resistance and rigidity of the acrylic copolymer are reduced. It should be noted that the ratio of the methyl methacrylate units, α-methylstyrene units, structural units (R) and monomer units (C) can be adjusted by 1H-NMR, 13 C-NMR etc.
[0082] The weight average molecular weight (Mw) of the acrylic copolymer (A) according to the present invention is preferably 40,000 to 200,000, more preferably 50,000 to 180,000, and even more preferably 55,000 to 160,000. When Mw is 40,000 or more, the strength, toughness, etc. of the molded body of the present invention are improved. When Mw is 200,000 or less, the flowability of the acrylic copolymer is improved, and the molding processability is improved.
[0083] The weight average molecular weight (Mw) is a value calculated by converting a chromatogram measured by gel permeation chromatography into a molecular weight of standard polystyrene.
[0084] The acid value of the acrylic copolymer (A) according to the present invention is preferably 0.01 to 0.30 mmol / g, more preferably 0.05 to 0.28 mmol / g. The acid value is a value proportional to the content of the carboxylic acid unit and the carboxylic anhydride unit in the acrylic copolymer. The acid value can be calculated, for example, by the method described in JP2005-23272A. When the acid value is within the above range, the balance between heat resistance, mechanical properties and molding processability is excellent.
[0085] The lower limit of the glass transition temperature of the acrylic copolymer (A) according to the present invention is preferably 130°C, more preferably 131°C, still more preferably 132°C, and the upper limit of the glass transition temperature of the acrylic copolymer according to the present invention is not particularly limited, and is preferably 160°C.
[0086] Herein, the "glass transition temperature (Tg)" is measured according to JIS K7121. Specifically, once the temperature is raised to 230°C, cooling is performed to room temperature, and then a DSC curve is measured under the condition of heating from room temperature to 230°C at 10°C / min. The midpoint obtained from the DSC curve measured at the second heating is determined as the "glass transition temperature (Tg)".
[0087] The saturated water absorption of the acrylic copolymer (A) according to the present invention is measured under the following conditions. The acrylic copolymer is pressed into a sheet having a thickness of 1.0 mm. A test piece having a size of 50 mm×50 mm is cut out from the central portion of the obtained pressed sheet, and the test piece is dried at 80°C for more than 16 hours using a dryer. After the dried test piece is cooled to room temperature in a dryer, the weight is measured to the nearest 0.1 mg, and the weight is defined as the initial weight Wo. The test piece is immersed in distilled water at 23°C, and after immersion for 24 hours, the test piece is taken out of the water, and the moisture on the surface is completely wiped off with a clean and dry cloth or filter paper. Within 1 minute of being taken out of the water, the test piece is weighed again to the nearest 0.1 mg. The test piece is immersed again, and after 24 hours, the weight is measured again in the same manner as described above. The weight at which the weight change rate of the test piece becomes within 0.02% of Wo is defined as the saturated weight Ws. The saturated water absorption is calculated by formula (2).
[0088] Saturated water absorption rate = ((Ws–Wo) / Wo) × 100 (2)
[0089] The saturated water absorption is preferably 2.5% or less, more preferably 2.1% or less, and still more preferably 2.0% or less.
[0090] The 1% weight loss temperature of the acrylic copolymer (A) according to the present invention in a nitrogen atmosphere is preferably 265° C. or higher, more preferably 270° C. or higher.
[0091] The acrylic copolymer (A) according to the present invention can be obtained by a method comprising subjecting a copolymer of methyl methacrylate, α-methylstyrene and, as required, other vinyl monomer units (C) copolymerizable with methyl methacrylate (hereinafter may be referred to as a precursor polymer) to a ring structure forming reaction.
[0092] That is, the manufacturing method may include:
[0093] A step of continuously supplying a reaction raw material to a tank reactor, wherein the reaction raw material contains a monomer mixture of 60 to 93% by mass of methyl methacrylate, 30 to 7% by mass of α-methylstyrene and 0 to 20% by mass of a copolymerizable monomer (C), a radical polymerization initiator and, if necessary, a chain transfer agent;
[0094] The step of bulk polymerizing the monomer mixture in the tank reactor until the polymerization conversion rate reaches 30 to 60% by mass to obtain a reaction product;
[0095] a step of removing the monomer mixture in the reaction product to obtain a precursor polymer; and
[0096] The obtained precursor polymer is subjected to a step of performing a ring structure forming reaction, wherein each step can be performed by a known technique.
[0097] The precursor polymer is produced by polymerization of a reaction raw material containing a monomer mixture, a free radical polymerization initiator and, if necessary, a chain transfer agent, and the monomer mixture contains 51 to 90% by mass, preferably 65 to 85% by mass of methyl methacrylate. In addition, the content of α-methylstyrene in the monomer mixture is 49 to 10% by mass, preferably 35 to 15% by mass. In addition, the content of the copolymerizable monomer (C) in the monomer mixture is 0 to 20% by mass, preferably 0 to 15% by mass.
[0098] In the monomer mixture, b* is preferably -1 to 2, more preferably -0.5 to 1.5. When b* is within this range, it is advantageous to obtain a molded product with almost no coloring at high manufacturing efficiency when the obtained acrylic copolymer composition is molded. It should be noted that b* is a value measured according to the International Commission on Illumination (CIE) standard (1976) or JIS Z8722.
[0099] The polymerization initiator used is not particularly limited as long as it generates reactive radicals. Examples thereof include peroxide-based initiators such as diisopropylbenzene hydroperoxide or tert-butyl hydroperoxide, and azo-based initiators such as 2,2'-azobis(2-methylpropionitrile).
[0100] It is desirable that the average uncleaved initiator concentration of the polymerization initiator used at the polymerization temperature in the tank reactor described below be 5.1×10 -5 ~2.4×10 -4 The amount of the polymerization initiator used is adjusted to the polymerization temperature, and the polymerization initiator is added to the monomer mixture to achieve an initiator concentration.
[0101] As the chain transfer agent used, monofunctional alkyl mercaptan such as n-octyl mercaptan and n-dodecyl mercaptan are preferred. These chain transfer agents can be used alone or in combination of two or more thereof. The amount of the chain transfer agent used is preferably 0 to 1 part by mass, more preferably 0.01 to 0.8 part by mass, and even more preferably 0.02 to 0.6 part by mass relative to 100 parts by mass of the monomer mixture.
[0102] The temperature in the tank reactor, that is, the temperature of the solution in the reactor, is preferably 110 to 140° C., more preferably 114 to 135° C. When the temperature is higher than this range, it is difficult to prepare a high molecular weight compound containing α-methylstyrene, which results in deterioration of heat resistance.
[0103] In the tank reactor, bulk polymerization is preferably carried out until the polymerization conversion rate reaches 30 to 65% by mass, preferably 35 to 60% by mass.
[0104] In addition, the average residence time (θ) of the reaction raw materials in the tank reactor is preferably 1.5 to 5 hours, more preferably 2 to 4.5 hours, and even more preferably 2.5 to 4 hours. When the average residence time is too short, the amount of the required polymerization initiator increases. In addition, the amount of the polymerization initiator increases so that it is difficult to control the polymerization reaction and tends to be difficult to control the molecular weight. On the other hand, when the average residence time is too long, it takes time for the reaction to become a steady state, and the productivity tends to decrease. The average residence time can be adjusted by the capacity of the tank reactor and the supply amount of the reaction raw materials.
[0105] The bulk polymerization is preferably carried out in an inert gas atmosphere such as nitrogen.
[0106] The manufacturing method according to the present invention includes a step of removing the monomer mixture in the reaction product. The removal method is not particularly limited and is preferably a heating devolatilization method. After removing the monomer mixture, in order to facilitate handling as a forming material, the acrylic resin composition can be formed into pellets or powder particles according to a known method. The content of the monomer mixture in the obtained acrylic resin composition is preferably 1% by mass or less, more preferably 0.5% by mass or less.
[0107] The lower limit of the glass transition temperature of the precursor polymer is preferably 115°C, more preferably 120°C, and even more preferably 125°C, and the upper limit of the glass transition temperature of the precursor polymer is preferably 150°C. The glass transition temperature can be changed by adjusting the molecular weight, the amount of α-methylstyrene copolymerization, etc. The higher the glass transition temperature of the precursor polymer, the more improved the heat resistance. The acrylic copolymer obtained using the precursor polymer having a high glass transition temperature has high heat resistance even when the amount of the structural unit (R) is small. Therefore, the acrylic copolymer hardly causes deterioration of saturated water absorption, etc.
[0108] The precursor polymer is not particularly limited as long as the total content of structural units derived from methyl methacrylate is 60 to 93% by mass, the total content of structural units derived from α-methylstyrene is 30 to 7% by mass, and the amount of structural units derived from the copolymerizable monomer (C) is 0 to 20% by mass. From the viewpoint of polymerizability, transparency, etc., the total content of structural units derived from methyl methacrylate in the precursor polymer is preferably 65% by mass or more and 93% by mass or less, more preferably 70% by mass or more and 92% by mass or less, and most preferably 75% by mass or more and 92% by mass or less.
[0109] From the viewpoints of heat resistance, polymerizability, water absorption, etc., the total content of the structural units derived from α-methylstyrene in the precursor polymer is preferably 7% by mass or more and 30% by mass or less, more preferably 8% by mass or more and 27% by mass or less, and even more preferably 11 to 25% by mass. When the content of the structural units derived from α-methylstyrene is less than this range, sufficient heat resistance cannot be obtained, and when the content of the structural units derived from α-methylstyrene is greater than this range, the polymerizability is significantly deteriorated. The total content of the structural units derived from the copolymerizable monomer (C) in the precursor polymer is 0 to 20% by mass, preferably 0 to 15% by mass.
[0110] In the chromatogram obtained by gel permeation chromatography, the weight average molecular weight Mw of the precursor polymer converted in terms of polystyrene is preferably 30,000 or more and 200,000 or less, more preferably 40,000 or more and 180,000 or less, and even more preferably 50,000 or more and 160,000 or less. When the weight average molecular weight Mw is less than the range, the resulting molded body is brittle, and when the weight average molecular weight Mw is greater than the range, productivity deteriorates. Mw can be controlled by adjusting the type, amount, addition time, etc. of the polymerization initiator or chain transfer agent (optional component) used in the manufacture of the precursor polymer.
[0111] The ring structure formation reaction can be carried out, for example, using an extruder. The example of an extruder includes a single screw extruder, a twin screw extruder and a multi-screw extruder. From the viewpoint of mixing performance, a twin screw extruder is preferred. The twin screw extruder includes a non-meshing co-rotating twin screw extruder, a meshing co-rotating twin screw extruder, a non-meshing counter-rotating twin screw extruder and a meshing counter-rotating twin screw extruder. The meshing counter-rotating twin screw extruder is preferred because it can rotate at high speed and can effectively promote mixing. These extruders can be used alone or can be connected in series with each other.
[0112] In the ring structure forming reaction using an extruder, for example, a precursor polymer as a raw material is supplied through a raw material supply part of the extruder, the precursor polymer is melted to fill the inside of the barrel, and then, an imidizing agent (optional component) and the like are injected into the extruder using a feeding pump, so that the ring structure forming reaction can be carried out in the extruder. When an imidizing agent is used, as a structural unit (R), an N-substituted or unsubstituted glutarimide unit may be contained, and as required, a lactone ring unit and / or a glutaric anhydride unit may be contained. A preferred imidizing agent is composed of R 2 -NH 2 (R 2As defined above). The amount of the imidizing agent used is preferably 1.6 to 12 parts by mass relative to 100 parts by mass of the acrylic copolymer. When the amount of the imidizing agent used is within the above range, by-production of methacrylamide units can be suppressed.
[0113] The resin temperature in the reaction zone of the extruder is preferably in the range of 180 to 280°C, more preferably in the range of 200 to 280°C. When the resin temperature in the reaction zone is lower than 180°C, the heat resistance of the acrylic copolymer tends to deteriorate due to reduced reaction efficiency of the ring structure formation reaction, by-production of methacrylamide units, etc. When the resin temperature in the reaction zone is higher than 280°C, the decomposition of the resin becomes significant, and the mechanical strength of the molded body and film formed by the obtained acrylic copolymer, such as tensile strength at break, tends to deteriorate. It should be noted that the reaction zone in the extruder refers to the area in the extruder barrel from the injection position of the imidizing agent, etc. to the resin discharge port (die head).
[0114] By increasing the residence time in the extruder reaction zone, the ring structure formation reaction can be carried out. The residence time in the reaction zone of the extruder is preferably longer than 10 seconds, more preferably longer than 30 seconds. When the residence time is less than 10 seconds, the ring structure formation reaction may be difficult to carry out.
[0115] The resin pressure in the extruder is preferably in the range of atmospheric pressure to 50 MPa, more preferably in the range of 1 to 30 MPa. When the resin pressure is 50 MPa or more, the resin pressure exceeds the limit of the mechanical pressure of a general extruder and requires a special device, which is not preferred in terms of cost.
[0116] It is preferred to use an extruder having a vent hole capable of reducing the pressure to below atmospheric pressure. With such a structure, unreacted substances, such as byproducts of methanol, or monomers can be removed, and the breaking strength of the molded body containing the acrylic resin composition of the present invention tends to be improved.
[0117] In the ring structure forming reaction, a reactor suitable for high viscosity materials manufactured by Sumitomo Heavy Industries, Ltd., for example, a horizontal twin-screw reactor such as BIVOLAK or a vertical twin-screw stirring tank such as SUPERBLEND may be preferably used instead of an extruder.
[0118] During the ring structure forming reaction, a carboxyl group may be generated as a by-product in the acrylic copolymer. If necessary, the carboxyl group can be converted into an ester group by an esterifying agent, a catalyst, etc. This makes it possible to reduce the foaming of the resin when manufacturing the optical film. Such an ester group varies depending on the esterifying agent or catalyst used, and from the viewpoint of the reduction of the melt viscosity of the resin during melt forming, the esterification reactivity, and the heat resistance of the resin after esterification, it is preferred to contain a methyl methacrylate unit, and more preferably contain a methyl methacrylate unit and an ethyl methacrylate unit at the same time.
[0119] From the viewpoints of cost, reactivity, etc., dimethyl carbonate is preferred as the esterification agent.
[0120] (Elastomer (B))
[0121] The content of the elastomer (B) in the acrylic resin composition of the present invention is 1 to 49% by mass, preferably 5 to 45% by mass, and more preferably 10 to 40% by mass. When the content of the elastomer (B) in the acrylic resin composition of the present invention is within the range of 1 to 49% by mass, brittleness is prevented.
[0122] The elastomer (B) used in the present invention is not particularly limited as long as a resin composition is obtained by kneading with the acrylic copolymer (A). The elastomer (B) preferably forms a dispersed phase in the resin composition. The form of the dispersed phase is not particularly limited, and examples thereof include spherical, ellipsoidal, rod-shaped, flat and linear.
[0123] The elastomer (B) preferably contains an acrylate unit. Examples of the acrylate include alkyl acrylates such as methyl acrylate, ethyl acrylate and butyl acrylate, aryl acrylates such as phenyl acrylate and benzyl acrylate, and cycloalkyl acrylates such as cyclohexyl acrylate and norbornene acrylate, preferably alkyl acrylate, and most preferably butyl acrylate.
[0124] The amount of the acrylic acid ester unit in the elastomer (B) is preferably 30% by mass or more, more preferably 35% by mass or more and 90% by mass or less, still more preferably 40% by mass or more and 80% by mass or less.
[0125] The elastomer (B) may contain a vinyl monomer unit having only one polymerizable carbon-carbon double bond in one molecule in addition to the acrylate unit. Examples of the vinyl monomer include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate; aryl methacrylates such as phenyl methacrylate; cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornene methacrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; acrylamide; methacrylamide; acrylonitrile; and methacrylonitrile.
[0126] The elastomer (B) may contain a vinyl monomer unit having only one polymerizable carbon-carbon double bond in one molecule in addition to the acrylate unit. Examples of the vinyl monomer include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate; aryl methacrylates such as phenyl methacrylate; cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornene methacrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; acrylamide; methacrylamide; acrylonitrile; and methacrylonitrile.
[0127] The elastomer (B) may further contain a conjugated diene monomer unit. Examples of the conjugated diene monomer unit include 1,3-butadiene, isoprene, and a monomer unit containing these two units.
[0128] The elastomer (B) is not particularly limited in its molecular form, and examples thereof include linear polymer elastomers, branched polymer elastomers, multilayer copolymer elastomers, and block copolymer elastomers. Among them, the elastomer (B) preferably comprises a multilayer copolymer elastomer containing methacrylate units and acrylate units, or a block copolymer elastomer containing a polymer block (b1) mainly containing methacrylate units and a polymer block (b2) containing acrylate units. The elastomer (B) may contain a combination of a block copolymer elastomer and a multilayer copolymer elastomer.
[0129] Examples of the multilayer copolymer elastomer include a multilayer copolymer elastomer comprising an outermost layer formed of a thermoplastic polymer (P) and an inner layer formed of a crosslinked polymer in contact with the outermost layer to cover the outermost layer, and preferably the inner layer and the outermost layer form a core and a shell. Examples of the multilayer copolymer elastomer include a two-layer polymer elastomer in which the core (inner layer) is a crosslinked rubber polymer (Q) and the outer shell (outermost layer) is a thermoplastic polymer (P), a three-layer polymer elastomer in which the core (inner layer) is a crosslinked polymer (R), the inner shell (inner layer) is a crosslinked rubber polymer (Q), and the outer shell (outermost layer) is a thermoplastic polymer (P), and a four-layer polymer elastomer in which the core (inner layer) is a crosslinked rubber polymer (Q), the first inner shell (inner layer) is a crosslinked polymer (R), the second inner shell (inner layer) is a crosslinked rubber polymer (Q), and the outer shell (outermost layer) is a thermoplastic polymer (P).
[0130] From the viewpoint of transparency, the polymer contained in each layer is preferably selected so that the difference in refractive index between adjacent layers is preferably less than 0.005, more preferably less than 0.004, still more preferably less than 0.003.
[0131] The mass ratio of the inner layer to the outermost layer in the multilayer copolymer elastomer is preferably 60 / 40 to 95 / 5, more preferably 70 / 30 to 90 / 10. In the inner layer, the proportion of the layer containing the crosslinked rubber polymer (Q) is preferably 20 to 70 mass %, more preferably 30 to 50 mass %.
[0132] The average particle size of the multilayer copolymer elastomer is preferably 0.05 to 3 μm, more preferably 0.1 to 2 μm, and even more preferably 0.2 to 1 μm. When the multilayer copolymer elastomer has an average particle size within the above range, especially when a multilayer copolymer elastomer having an average particle size of 0.2 to 1 μm is used, toughness can be exhibited by blending a small amount of the multilayer copolymer elastomer, and therefore, rigidity or surface hardness is not impaired. It should be noted that the average particle size herein is an average value of a volume-based particle size distribution measured by a light scattering method.
[0133] The thermoplastic polymer (P) is a polymer composed of an alkyl methacrylate unit having an alkyl group having 1 to 8 carbon atoms and, if necessary, a monofunctional monomer unit other than the alkyl methacrylate. The thermoplastic polymer (P) preferably does not contain a polyfunctional monomer unit.
[0134] The amount of the alkyl methacrylate unit having an alkyl group having 1 to 8 carbon atoms constituting the thermoplastic polymer (P) is preferably 80 to 100% by mass, more preferably 85 to 95% by mass, based on the mass of the thermoplastic polymer (P).
[0135] As the alkyl methacrylate having an alkyl group having 1 to 8 carbon atoms (hereinafter referred to as C1-8 alkyl methacrylate), for example, methyl methacrylate is preferred.
[0136] The amount of the monofunctional monomer units other than C1-8 alkyl methacrylate constituting the thermoplastic polymer (P) is preferably 0 to 20% by mass, more preferably 5 to 15% by mass, based on the mass of the thermoplastic polymer (P).
[0137] Examples of the monofunctional monomer other than the C1-8 alkyl methacrylate include acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate; and aromatic vinyl compounds such as styrene.
[0138] The outermost layer may be a single layer formed of one thermoplastic polymer (P) or a multilayer formed of two or more thermoplastic polymers (P).
[0139] The amount of the thermoplastic polymer (P) is preferably 40 to 75% by mass, more preferably 45 to 70% by mass, and still more preferably 50 to 65% by mass, relative to the amount of the multilayer copolymer elastomer.
[0140] The cross-linked elastic body layer as the inner layer includes an intermediate layer formed of a cross-linked rubber polymer (Q) and an inner layer formed of a cross-linked polymer (R) and in contact with the intermediate layer so as to cover the intermediate layer.
[0141] The cross-linked polymer (R) contains methyl methacrylate units, monofunctional monomer units other than methyl methacrylate, and polyfunctional monomer units.
[0142] The amount of the methyl methacrylate unit constituting the cross-linked polymer (R) is preferably 40 to 98.5% by mass, more preferably 45 to 95% by mass, based on the mass of the cross-linked polymer (R).
[0143] The amount of the monofunctional monomer units other than methyl methacrylate constituting the cross-linked polymer (R) is preferably 1 to 59.5% by mass, more preferably 5 to 55% by mass, based on the mass of the cross-linked polymer (R).
[0144] Examples of the monofunctional monomer other than methyl methacrylate include acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate; and aromatic vinyl compounds such as styrene.
[0145] The amount of the multifunctional monomer unit constituting the cross-linked polymer (R) is preferably 0.05 to 0.4% by mass, more preferably 0.1 to 0.3% by mass, based on the mass of the cross-linked polymer (R).
[0146] Examples of the multifunctional monomer include ethylene glycol dimethacrylate, propylene glycol dimethacrylate, triethylene glycol dimethacrylate, hexylene glycol dimethacrylate, ethylene glycol diacrylate, propylene glycol diacrylate, triethylene glycol diacrylate, allyl methacrylate, and triallyl isocyanurate.
[0147] The amount of the cross-linked polymer (R) is preferably 5 to 40% by mass, more preferably 7 to 35% by mass, and still more preferably 10 to 30% by mass, relative to the amount of the multilayer copolymer elastomer.
[0148] The crosslinked rubber polymer (Q) contains an alkyl acrylate unit having an alkyl group having 1 to 8 carbon atoms and / or a conjugated diene unit, and a polyfunctional monomer unit.
[0149] The amount of the alkyl acrylate unit having an alkyl group having 1 to 8 carbon atoms and / or the conjugated diene unit constituting the crosslinked rubber polymer (Q) is preferably 85 to 99% by mass, more preferably 95 to 98% by mass, based on the amount of the crosslinked rubber polymer (Q).
[0150] Examples of the alkyl acrylate having an alkyl group having 1 to 8 carbon atoms include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate.
[0151] Examples of the conjugated diene unit include 1,3-butadiene and isoprene.
[0152] Examples of the crosslinked rubber polymer (Q) containing 1,3-butadiene as a monomer include 1,3-polybutadiene homopolymers or copolymers containing 50% by weight or more of 1,3-polybutadiene units. As examples of copolymers, for example, butadiene-aromatic vinyl compound copolymers such as butadiene-styrene copolymers or butadiene-vinyltoluene copolymers are included, and further include terpolymers containing 50% by weight or more of 1,3-butadiene units. These copolymers can generally be easily prepared by known emulsion polymerization.
[0153] The amount of the multifunctional monomer units constituting the crosslinked rubber polymer (Q) is preferably 1 to 1.7 mass %, more preferably 1.2 to 1.6 mass %, still more preferably 1.3 to 1.5 mass %, relative to the mass of the crosslinked rubber polymer (Q).
[0154] Examples of the polyfunctional monomer include those exemplified for the cross-linked polymer (R).
[0155] From the viewpoint of improving bending resistance, the ratio of the mass of the multifunctional monomer units in the crosslinked polymer (R) to the mass of the multifunctional monomer units in the crosslinked rubber polymer (Q) is preferably 0.05 to 0.25, more preferably 0.1 to 0.2. The glass transition temperature of the crosslinked rubber polymer (Q) is preferably lower than the glass transition temperature of the crosslinked polymer (R).
[0156] The amount of the crosslinked rubber polymer (Q) is preferably 20 to 55% by mass, more preferably 25 to 45% by mass, still more preferably 30 to 40% by mass, relative to the amount of the multilayer copolymer elastomer.
[0157] In the multilayer copolymer elastomer, the average diameter (d) of the crosslinked elastomer layer is preferably 60 to 110 nm, more preferably 65 to 105 nm, and even more preferably 70 to 100 nm. The average diameter d (nm) of the crosslinked elastomer layer can be measured as follows. A hydraulic forming machine is used with a die size of 50 mm × 120 mm, a pressing temperature of 250° C., a preheating time of 3 minutes, and a pressing pressure of 50 kg / cm 2 , pressing time is 30 seconds, cooling temperature is 20°C, pressure during cooling is 50kg / cm 2 And under the condition of a cooling time of 10 minutes, the resin composition containing the multilayer copolymer elastomer is formed into a 3m thick flat plate. The obtained flat plate is cut using a microtome at -100°C in a direction parallel to the long side to obtain a thin slice with a thickness of 40nm, and the thin slice is dyed with ruthenium. The dyed thin slice is observed with a scanning transmission electron microscope (manufactured by JEOL Ltd., JSM7600F) at an accelerating voltage of 25kV, and an image is taken. The short axis and long axis of the part stained with ruthenium (the exposed part of the thin slice of the cross-linked elastomer layer) are measured, and (short axis + long axis) / 2 is defined as the diameter of the cross-linked elastomer layer. More than 20 slices are measured, and then the number average (average diameter) thereof is calculated.
[0158] The multilayer copolymer elastomer is not particularly limited by its production method, and examples thereof may include emulsion polymerization.
[0159] In the case of emulsion polymerization, for example, the monomer (r) constituting the cross-linked polymer (R) can be emulsion polymerized to obtain a latex containing the cross-linked polymer (R), the monomer (q) for constituting the cross-linked rubber polymer (Q) can be added to the latex, and the monomer (q) can be subjected to seed emulsion polymerization to obtain a latex containing the cross-linked polymer (R) and the cross-linked rubber polymer (q), and the monomer (p) for constituting the thermoplastic polymer (P) can be added to the latex, and the monomer (p) can be subjected to seed emulsion polymerization to obtain a latex containing a multilayer copolymer elastomer. It should be noted that emulsion polymerization is a known method for obtaining a latex containing a polymer. Seed emulsion polymerization is a method of performing a polymerization reaction of monomers on the surface of seed particles. Seed emulsion polymerization is preferably used to obtain polymer particles having a core-shell structure.
[0160] The block copolymer elastomer preferably comprises a polymer block (b1) mainly comprising methacrylate units and a polymer block (b2) comprising acrylate units.
[0161] The block copolymer elastomer may contain only one polymer block (b1) or a plurality of polymer blocks (b1) in one molecule. In addition, the block copolymer elastomer may contain only one polymer block (b2) or a plurality of polymer blocks (b2) in one molecule.
[0162] The amount of the methacrylate unit contained in the polymer block (b1) is preferably 80% by mass or more, more preferably 90% by mass or more, still more preferably 95% by mass or more, and further still more preferably 98% by mass or more. As the methacrylate, for example, methyl methacrylate is preferred. For the polymer block (b1), the methacrylate may be used alone or in combination of two or more thereof.
[0163] From the viewpoints of transparency, flexibility, bending resistance, impact resistance, softness, moldability, surface smoothness, etc., the amount of the polymer block (b1) contained in the block copolymer elastomer is preferably 40 mass % or more and 90 mass % or less, and more preferably 45 mass % or more and 80 mass % or less.
[0164] The glass transition temperature of the polymer block (b2) is preferably 20°C or lower, more preferably -20°C or lower.
[0165] The amount of the acrylate unit contained in the polymer block (b2) is preferably 90% by mass or more. Examples of acrylates include n-butyl acrylate and benzyl acrylate. These acrylates can be used for the polymer block (b2) alone or in combination of two or more thereof.
[0166] The polymer block (b2) may contain monomer units other than acrylic acid esters as long as the objects and effects of the present invention are not impaired.
[0167] The polymer block (b2) preferably contains an alkyl acrylate unit and an aromatic (meth)acrylate unit from the viewpoint of transparency, etc. The mass ratio of the alkyl acrylate unit / aromatic (meth)acrylate unit is preferably 50 / 50 to 90 / 10, more preferably 60 / 40 to 80 / 20.
[0168] The combination form of the polymer block (b1) and the polymer block (b2) contained in the block copolymer elastomer is not particularly limited. For example, a block copolymer in which one end of the polymer block (b2) is connected to one end of the polymer block (b1) (b1-b2 diblock copolymer) or a block copolymer in which one end of the polymer block (b1) is connected to each of the two ends of the polymer block (b2) (b1-b2-b1 triblock copolymer) is preferred.
[0169] The weight average molecular weight of the block copolymer elastomer is preferably more than 52,000 and less than 400,000, more preferably more than 60,000 and less than 300,000. In addition, the ratio of the weight average molecular weight to the number average molecular weight of the block copolymer elastomer is preferably more than 1.01 and less than 2.00, more preferably more than 1.05 and less than 1.60. The weight average molecular weight and number average molecular weight of the block copolymer elastomer can be appropriately set from the viewpoints of formability, tensile strength, appearance, etc. Weight average molecular weight and number average molecular weight are values converted by standard polystyrene measured by gel permeation chromatography (GPC).
[0170] The method for producing the block copolymer elastomer is not particularly limited and can be obtained by known methods. For example, a method comprising living polymerization of the monomers constituting each polymer is generally used. As a living polymerization method, a method comprising anionic polymerization in the presence of an organic alkali metal compound and an organic aluminum compound is preferred because a high-purity block copolymer elastomer can be obtained, the molecular weight or composition ratio is easily controlled, and the cost is low.
[0171] (Acrylic resin composition)
[0172] From the viewpoint of impact resistance and surface hardness, in the acrylic resin composition of the present invention, the mass ratio of acrylic copolymer (A) / elastomer (B) is 99 / 1 to 51 / 49, preferably 95 / 5 to 55 / 45, and more preferably 90 / 10 to 60 / 40.
[0173] The melt flow rate of the acrylic resin composition of the present invention at 230° C. and a load of 3.8 kg is preferably 1 g / 10 min or more, more preferably 1.5 to 35 g / 10 min, and even more preferably 2 to 20 g / 10 min. It should be noted that the melt flow rate is a value of the melt mass flow rate measured according to JIS K7210.
[0174] The glass transition temperature of the acrylic resin composition of the present invention is preferably 100 to 160° C., more preferably 105 to 155° C., and still more preferably 110 to 150° C. When the glass transition temperature is 100° C. or lower, heat resistance and the like tend to deteriorate, and when the glass transition temperature is 160° C. or higher, moldability and the like tend to deteriorate.
[0175] In the acrylic resin composition of the present invention, the softening temperature of the molded article is preferably 110° C. or higher, more preferably 115° C. or higher, and still more preferably 120° C. or higher when measured by the method specified in the B50 method of JIS K7206. When the softening temperature is 110° C. or higher, the molded article is excellent in heat resistance and high temperature dimensional stability.
[0176] The acrylic resin composition according to the present invention has a saturated water absorption of 2.5% or less, more preferably 2.1% or less, and even more preferably 2.0% or less when measured under the same conditions as the saturated water absorption of the acrylic copolymer (A). When the saturated water absorption is 2.5% or less, the dimensional stability under high humidity is excellent.
[0177] The acrylic resin composition of the present invention may contain a filler as required, as long as the effect of the present invention is not impaired. Examples of the filler may include calcium carbonate, talc, carbon black, titanium oxide, silica, clay, barium sulfate and magnesium carbonate. The amount of filler that may be contained in the resin composition of the present invention is preferably 3% by mass or less, more preferably 1.5% by mass or less.
[0178] The acrylic resin composition of the present invention may contain other polymers as long as the effects of the present invention are not impaired. Examples of the other polymers may include polyolefin resins such as polyethylene, polypropylene, polybutene-1, poly-4-methylpentene-1, polynorbornene; vinyl ionomers; styrene resins such as polystyrene, styrene-maleic anhydride copolymer, high impact polystyrene, AS resin, ABS resin, AES resin, AAS resin, ACS resin and MBS resin; methyl methacrylate polymers other than the acrylic copolymer (A) and methyl methacrylate-styrene copolymers; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polyamides such as nylon 6, nylon 66 and polyamide elastomers; polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl alcohol copolymers, polyacetal, polyvinylidene fluoride, polyurethane, phenoxy resins, modified polyphenylene ethers, polyphenylene sulfides and silicone modified resins; silicone rubbers; styrene thermoplastic elastomers such as SEPS, SEBS and SIS; and olefin rubbers such as IR, EPR and EPDM. The amount of other polymers that may be contained in the resin composition of the present invention is preferably 10% by mass or less, more preferably 5% by mass or less, and most preferably 0% by mass.
[0179] The acrylic resin composition of the present invention may contain additives such as antioxidants, thermal degradation inhibitors, ultraviolet absorbers, light stabilizers, lubricants, release agents, polymer processing aids, antistatic agents, flame retardants, dyes and pigments, light diffusers, organic dyes, matting agents and fluorescent substances within a range that does not impair the effects of the present invention.
[0180] The antioxidant alone effectively prevents oxidative degradation of the resin in the presence of oxygen. Examples of the antioxidant include phosphorus antioxidants, hindered phenol antioxidants and thioether antioxidants. These antioxidants can be used alone or in combination of two or more thereof. Among them, from the viewpoint of the effect of preventing degradation of optical properties due to coloring, phosphorus antioxidants or hindered phenol antioxidants are preferred, and a combination of phosphorus antioxidants and hindered phenol antioxidants is preferred.
[0181] When a combination of a phosphorus antioxidant and a hindered phenol antioxidant is used, the ratio thereof is not particularly limited, and the mass ratio of phosphorus antioxidant / hindered phenol antioxidant is preferably 1 / 5 to 2 / 1, more preferably 1 / 2 to 1 / 1.
[0182] Examples of the phosphorus antioxidant include 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite (manufactured by ADEKA Corporation; trade name: ADK STAB HP-10), tris(2,4-di-tert-butylphenyl)phosphite (manufactured by Ciba Specialty Chemicals KK; trade name: IRUGAFOS168), and 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (manufactured by ADEKA Corporation; trade name: ADK STAB PEP-36).
[0183] Examples of the hindered phenol antioxidant include pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (manufactured by Ciba Specialty Chemicals; trade name: IRGANOX 1010) and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (manufactured by Ciba Specialty Chemicals; trade name: IRGANOX 1076).
[0184] Examples of the thermal degradation inhibitor are compounds that can prevent thermal degradation of the resin by scavenging polymer radicals when exposed to high heat in a substantially oxygen-free state, and examples thereof include 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-hydroxybenzyl)-4-methylphenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd., trade name: Sumilizer GM) and 2,4-di-tert-amyl-6-(3',5'-di-tert-amyl-2'-hydroxy-α-methylbenzyl)phenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd., trade name: Sumilizer GS).
[0185] The ultraviolet absorber is a compound having the ability to absorb ultraviolet rays. The ultraviolet absorber is a compound having the function of mainly converting light energy into heat energy.
[0186] Examples of the ultraviolet absorber may include benzophenone, benzotriazole, triazine, benzoate or ester, salicylate or ester, cyanoacrylate or ester, oxalic acid aniline, malonate and formamidine. These ultraviolet absorbers can be used alone or in combination of two or more thereof. Among them, benzotriazole, triazine, or a maximum value εmax of the molar absorption coefficient at a wavelength of 380 to 450 nm of 1,200 dm is preferred. 3 mol -1 cm -1 The following ultraviolet absorbers.
[0187] As the benzotriazoles, preferred are 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (manufactured by BASF SE; trade name: TINUVIN329), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (manufactured by BASF SE; trade name: TINUVIN234), 2,2′-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol] (manufactured by ADEKA; trade name: LA-31), and 2-(5-octylthio-2H-benzotriazol-2-yl)-6-tert-butyl-4-methylphenol.
[0188] In addition, in the case of effectively absorbing short wavelengths below 380 nm, it is preferred to use a triazine ultraviolet absorber. Examples of such ultraviolet absorbers may include 2,4,6-tris (2-hydroxy-4-hexyloxy-3-methylphenyl) -1,3,5-triazine (manufactured by ADEKA; trade name: LA-F70), hydroxyphenyl triazine ultraviolet absorbers as analogs thereof (manufactured by BASF; trade name: TINUVIN477, TINUVIN460 or TINUVIN479) and 2,4-diphenyl-6- (2-hydroxy-4-hexyloxyphenyl) -1,3,5-triazine.
[0189] It should be noted that the maximum value of the molar absorption coefficient of the ultraviolet absorber is max The measurement is as follows. 10.00 mg of ultraviolet absorber is added to 1 L of cyclohexane and dissolved so that there is no undissolved matter when visually observed. The solution is injected into a quartz glass cell with a size of 1 cm × 1 cm × 3 cm, and the absorbance at a wavelength of 380 to 450 nm is measured using a spectrophotometer (manufactured by Hitachi, Ltd.; trade name: U-3410). The maximum value of the molar absorption coefficient ε max is the molecular weight of the UV absorber used (M UV ) and the maximum absorbance (A max ) is calculated by the following formula.
[0190] ε max =[A max / (10×10 -3 )]×M UV
[0191] The light stabilizer is a compound having a function of scavenging free radicals generated mainly by photooxidation. Examples thereof include hindered amines such as compounds having a 2,2,6,6-tetraalkylpiperidine skeleton.
[0192] Examples of the lubricant include stearic acid, behenic acid, stearamide acid, methylenebisstearamide, hydroxystearic acid triglyceride, paraffin wax, ketone wax, octanol, and hardened oil.
[0193] The release agent is a compound having a function of promoting the release of a molded product from a mold, and examples thereof include higher alcohols such as cetyl alcohol and stearyl alcohol, and glycerol higher fatty acid esters such as stearic acid monoglyceride and stearic acid diglyceride. Since the use of glycerol higher fatty acid esters may generate gel-like foreign matter, it is preferred to use higher alcohols.
[0194] The polymer processing aid is a compound that has an effect on thickness accuracy and thin film formation when the acrylic resin composition is formed. The polymer processing aid can usually be prepared by emulsion polymerization. The polymer processing aid is preferably a polymer particle with a particle size of 0.05 to 0.5 μm.
[0195] The polymer particles may be single-layer particles formed of a polymer having a single composition ratio and a single intrinsic viscosity, or may be multi-layer particles formed of two or more polymers having different composition ratios or intrinsic viscosities. Among them, particles having a double-layer structure are preferred, wherein a polymer layer having a low intrinsic viscosity is included as an inner layer and a polymer layer having a high intrinsic viscosity of 5 dl / g or more is included as an outer layer. The polymer processing aid preferably has an intrinsic viscosity of 3 to 6 dl / g. When the intrinsic viscosity is too small, the effect of improving the formability is low. When the intrinsic viscosity is too large, the melt fluidity of the acrylic resin composition tends to decrease.
[0196] Examples of the antistatic agent include alkyl sulfonates such as sodium heptyl sulfonate, sodium octyl sulfonate, sodium nonyl sulfonate, sodium decyl sulfonate, sodium dodecyl sulfonate, sodium cetyl sulfonate, sodium octadecyl sulfonate, sodium diheptyl sulfonate, potassium heptyl sulfonate, potassium octyl sulfonate, potassium nonyl sulfonate, potassium decyl sulfonate, potassium dodecyl sulfonate, potassium hexadecyl sulfonate, potassium octadecyl sulfonate, potassium diheptyl sulfonate, lithium heptyl sulfonate, lithium octyl sulfonate, lithium nonyl sulfonate, lithium decyl sulfonate, lithium dodecyl sulfonate, lithium cetyl sulfonate, lithium octadecyl sulfonate, and lithium diheptyl sulfonate.
[0197] Examples of the flame retardant include metal hydrates having a hydroxyl group or crystal water, such as magnesium hydroxide, aluminum hydroxide, hydrated aluminum silicate, hydrated magnesium silicate or hydrotalcite; phosphoric acid compounds such as polyphosphoric acid amine or phosphoric acid ester; and silicon compounds, and preferably a phosphoric acid flame retardant such as trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, tripentyl phosphate, trihexyl phosphate, tricyclohexyl phosphate, triphenyl phosphate, tricresyl phosphate, tri(xylyl) phosphate, dimethyl ethyl phosphate, methyl dibutyl phthalate, ethyl dipropyl phosphate or hydroxyphenyl diphenyl phosphate.
[0198] Examples of the dye and the pigment include red organic pigments such as para red, fire red, pyrazolone red, thioindigo red or perylene red, blue organic pigments such as cyanine blue or indanthrene blue, and green organic pigments such as cyanine green or naphthol green, and one or more of these dyes and pigments may be used.
[0199] As the organic dye, a compound having a function of converting ultraviolet light into visible light is preferably used.
[0200] Examples of the light diffusing agent or the matting agent may include glass fine particles, polysiloxane-based cross-linked fine particles, cross-linked polymer fine particles, talc, calcium carbonate, and barium sulfate.
[0201] Examples of the fluorescent substance may include fluorescent pigments, fluorescent dyes, fluorescent white dyes, fluorescent brighteners, and fluorescent bleaching agents.
[0202] These additives can be used alone or in combination of two or more thereof. In addition, these additives can be added to the polymerization reaction solution when manufacturing the acrylic copolymer (A) and the elastomer (B), can be added to the prepared acrylic copolymer (A) or the cross-linked rubber (B), or can be added when preparing the acrylic resin composition of the present invention. From the viewpoint of suppressing the appearance defects of the molded body, the total amount of additives contained in the acrylic resin composition of the present invention is preferably 7% by mass or less, more preferably 5% by mass or less, and even more preferably 4% by mass or less, relative to the acrylic resin composition.
[0203] The preparation method of the acrylic resin composition of the present invention is not particularly limited. Examples thereof include a method in which a monomer mixture containing methyl methacrylate, etc. is polymerized in the presence of an elastomer (B) to prepare an acrylic copolymer (A) and a method in which an acrylic copolymer (A) and an elastomer (B) are melt-mixed. During melt-mixing, other polymers and additives may be mixed as required, the acrylic copolymer (A) may be mixed with the elastomer (B) after being mixed with other polymers and additives, the elastomer (B) may be mixed with the acrylic copolymer (A) after being mixed with other polymers and additives, or other methods may be used. Mixing may be carried out using a known mixer or mixer such as a kneader-ruder, an extruder, a mixing roll or a Banbury mixer. Among them, a twin-screw extruder is preferred.
[0204] In order to improve convenience during storage, transportation or molding, the acrylic resin composition of the present invention may be in the form of pellets or the like.
[0205] The molded body of the present invention contains the acrylic resin composition of the present invention. The manufacturing method of the molded body of the present invention is not particularly limited. Its examples may include melt forming methods, such as T-die method (lamination method, coextrusion method, etc.), inflation method (coextrusion method, etc.), compression molding method, blow molding method, calendaring method, vacuum forming method, injection molding method (insertion method, two-color method, pressing method, core back method, sandwich method, etc.), and solution casting method. Among them, from the viewpoints of high productivity, cost, etc., T-die method, inflation method or injection molding method are preferred. The type of molded body is not limited, preferably a film (a planar molded body with a thickness of more than 5 μm and less than 250 μm) or a sheet (a planar molded body with a thickness exceeding 250 μm), and among them, a film is particularly preferred.
[0206] The film as one form of the molded body of the present invention can be produced by solution casting, melt casting, extrusion molding, inflation molding, blow molding, etc. Among them, extrusion molding is preferred from the viewpoint of obtaining a film having excellent transparency, improved toughness, excellent operability, and excellent balance of toughness, surface hardness and rigidity. The temperature of the molten resin discharged from the extruder is preferably set to 160 to 270°C, more preferably 220 to 260°C.
[0207] In the extrusion molding method, from the viewpoint of obtaining a film having excellent surface smoothness, excellent mirror gloss and low haze, the T-die method is preferred. In the T-die method, the molten resin discharged from the T-die head through the extruder, gear pump, polymer filter and mixer is preferably sandwiched between two or more mirror rollers or mirror belts to be formed into a film. When the molten resin is inserted between the mirror rollers or mirror belts, a bank may or may not be formed. The die head has a lip opening automatic adjustment function, and the air gap is preferably 100 mm or less.
[0208] The mirror roller or the mirror belt is preferably formed of metal. As the mirror roller, a metal rigid roller, a metal elastic roller, etc. can be used, and a combination of a metal elastic roller and a metal rigid roller is preferably used. In addition, the temperature of both surfaces of the mirror roller or the mirror belt is preferably 130°C or less. In addition, the temperature of at least one surface of a pair of mirror rollers or mirror belts is preferably 60°C or more. When the surface temperature is set as described above, the molten resin discharged from the extruder can be cooled at a faster rate than natural cooling, and a film with excellent surface smoothness and low haze can be easily manufactured. The linear pressure between a pair of rollers or belts is preferably 10N / mm or more, more preferably 30N / mm or more. The thickness of the unstretched film obtained by extrusion molding is preferably 10 to 300μm. The haze of the film is preferably 0.57% or less at a thickness of 100μm, more preferably 0.35% or less, and even more preferably 0.3% or less.
[0209] The unstretched film obtained as described above may be subjected to a stretching treatment. The mechanical strength is improved by the stretching treatment, and a film that is hardly cracked can be obtained. The stretching method is not particularly limited, and examples thereof may include a simultaneous biaxial stretching method, a sequential biaxial stretching method, and a tubular stretching method. From the viewpoint of obtaining a film that can be uniformly stretched and has high strength, the lower limit of the temperature during stretching is a temperature 10°C higher than the glass transition temperature of the acrylic copolymer or the acrylic resin composition, and the upper limit of the temperature during stretching is a temperature 40°C higher than the glass transition temperature of the acrylic copolymer or the acrylic resin composition. Stretching is generally performed at 100 to 5,000% / min. A film with less heat shrinkage can be obtained by thermally fixing after stretching. The thickness of the film after stretching is preferably 10 to 200 μm.
[0210] A functional layer may be provided on the surface of a film as one form of the formed body of the present invention. Examples of the functional layer may include a hard coat layer, an antiglare layer, an antireflection layer, an antisticking layer, a diffusion layer, an antiglare layer, an antistatic layer, an antifouling layer, and an easy-slip layer such as fine particles.
[0211] In addition, it is preferred to provide a primer layer on at least one surface of the film of the present invention in order to improve the adhesion strength with the functional layer, or to improve the adhesion strength when laminated with other films via an adhesive or a pressure-sensitive adhesive.
[0212] The acrylic resin composition of the present invention is suitable as a molding material. The molded body of the present invention can be a component for various applications. Examples of specific applications may include sign components or logo films such as advertising towers, vertical signs, cantilever signs, lintel signs or roof signs; display components such as display windows, partitions or store displays; lighting components such as fluorescent lampshades, atmosphere lampshades, lampshades, skylights, light walls or chandeliers; indoor components such as furniture, pendants or mirrors; building components such as doors, domes, safety window glass, partitions, stair sidings, balcony sidings or leisure building roofs; transportation equipment related components such as aircraft windshields, pilot visors, motorcycle windshields, Motorboat windshields, bus visors, car side visors, rear visors, head wings, headlight covers, car interior parts, or car exterior parts such as bumpers; electronic equipment parts such as audio and video nameplates, audio covers, TV protective covers, vending machines, mobile phones or personal computers; medical equipment parts such as incubators or X-ray parts; instrument-related parts such as machine covers, instrument covers, experimental devices, rulers, dials or observation windows; optical parts such as liquid crystal protection plates, light guide plates, light guide films, Fresnel lenses, double convex lenses, front panels of various displays, or diffusers; traffic-related parts such as road signs, direction signs, curved mirrors or soundproof walls; and greenhouses, large sinks, box sinks, bathroom components, clock panels, bathtubs, toilets, table mats, game components, toys, musical instruments, masks for face protection during welding, solar cell back panels, flexible solar cell front panels and decorative films; and surface materials for personal computers, mobile phones, furniture, vending machines or bathroom components.
[0213] The laminate can be obtained by laminating a layer containing the acrylic resin composition of the present invention with other materials (e.g., a layer containing other thermoplastic copolymers). Examples of the other materials used in the laminate may include steel, plastics (e.g., thermoplastic resins), wood, and glass. The laminate obtained by the present invention can be preferably used for wallpaper; surfaces of automotive interior components; surfaces of automotive exterior components such as bumpers; surfaces of mobile phones; surfaces of furniture; surfaces of computers; surfaces of vending machines; and surfaces of bathroom components such as bathtubs.
[0214] The film as one form of the molded body of the present invention is suitable for optical applications due to its high transparency and heat resistance, and is particularly suitable for polarizer protective films, liquid crystal protective plates, surface materials of portable information terminals, display window protective films of portable information terminals, light guide films, transparent conductive films coated with silver nanowires or carbon nanotubes, and front panels of various displays. Since the film of the present invention has high transparency and heat resistance, as applications other than optical applications, the film can be used as an infrared blocking film, an anti-crime film, an anti-scattering film, a decorative film, a metal decorative film, a shrink film, and a film for in-mold labeling.
[0215] When the film as a form of the formed body of the present invention is used as a polarizer protective film or a phase difference film, the film may be laminated only on one surface or both surfaces of the polarizing film. When laminated with a polarizing film, the film may be laminated with an adhesive layer or a pressure-sensitive adhesive layer. As the polarizing film, a stretched film formed of a polyvinyl alcohol resin and iodine may be used, and the film thickness thereof is preferably 1 to 100 μm.
[0216] [Example]
[0217] Next, the present invention will be described in more detail with reference to examples. It should be noted that the present invention is not limited to the examples.
[0218] Physical properties and the like were measured by the following methods.
[0219] (Weight average molecular weight)
[0220] The weight average molecular weight (Mw) of the resin obtained in each manufacturing example is determined by gel permeation chromatography (GPC method). The sample solution is prepared by dissolving 4 mg of the resin to be tested in 5 ml of tetrahydrofuran. The temperature of the column oven is set to 40°C, 20 μl of the sample solution is injected into the device at an eluent flow rate of 0.35 ml / min, and the chromatogram is measured. GPC measurement was performed on 10 standard polystyrenes with molecular weights ranging from 400 to 5,000,000, and a calibration curve showing the relationship between retention time and molecular weight was prepared. Based on the calibration curve, the Mw of the resin to be tested is determined. The value corresponding to the molecular weight of the standard styrene obtained from the chromatogram measured by gel permeation chromatography (GPC) is defined as the molecular weight of the copolymer.
[0221] Apparatus: GPC apparatus HLC-8320 manufactured by Tosoh Corporation
[0222] Separation column: TSK guard column Super HZ-H, TSKgel HZM-M and TSKgel Super HZ4000 connected in series, manufactured by Tosoh Corporation
[0223] Eluent: Tetrahydrofuran
[0224] Eluent flow rate: 0.35 ml / min
[0225] Column temperature: 40°C
[0226] Detection method: Differential refractive index (RI)
[0227] (Composition of each unit in the copolymer)
[0228] pass 13C-NMR measures the carbon ratio among the phenyl group of the α-methylstyrene unit, the carbonyl group of the methyl methacrylate unit, and the phenyl group of the styrene unit, and each unit composition is calculated using the carbon ratio.
[0229] (Glass transition temperature Tg)
[0230] The resin obtained in each manufacturing example was heated to 250° C. using a differential scanning calorimeter (manufactured by SHIMADZU CORPORATION, DSC-50 (product number)) in accordance with JIS K7121, then cooled to room temperature, and then a DSC curve was measured under the condition that the temperature was increased from room temperature to 200° C. at 10° C. / min. The glass transition temperature at the midpoint obtained from the DSC curve measured at the second temperature increase is defined as the glass transition temperature in the present invention.
[0231] (Composition of each unit of acrylic copolymer)
[0232] The α-methylstyrene unit and the styrene unit have the same composition as the respective unit compositions of the precursor polymer. 1 The acrylic copolymers were analyzed by H-NMR (manufactured by Bruker Corporation, trade name: ULTRA SHIELD 400PLUS). 1 The content (mol %) of each monomer unit such as glutarimide unit, methyl methacrylate unit and aromatic vinyl (α-methylstyrene and styrene) unit in the acrylic copolymer was determined by H-NMR measurement, and the content (mol %) was converted into content (weight %) using the molecular weight of each monomer unit.
[0233] (1% thermal weight loss temperature)
[0234] The acrylic copolymer obtained in each manufacturing example and the acrylic resin composition obtained in each example and comparative example were heated at 10° C. / min in a nitrogen atmosphere using a thermogravimetric measuring apparatus (manufactured by Shimadzu Corporation, TGA-50), and the temperature at which 1% weight loss occurred was defined as the 1% thermal weight loss temperature.
[0235] (Vicat softening temperature)
[0236] The acrylic resin composition obtained in each of the Examples and Comparative Examples was injection molded using an injection molding machine (manufactured by Meiki Co., Ltd., M-100C) under the conditions of a cylinder temperature of 260° C., a mold temperature of 50° C., and an injection speed of 50 mm / sec to obtain a rectangular test piece having a thickness of 4 mm, a long piece of 80 mm, and a short side of 10 mm. The Vicat softening temperature (VST) of each test piece was measured according to the method described in the B50 method of JIS K7206 using an HDT tester 3M-2 manufactured by Toyo Seiki Seisaku-sho, Ltd.
[0237] (Flexural modulus)
[0238] The acrylic copolymer obtained in each manufacturing example and the acrylic resin composition obtained in each example and comparative example were injection molded using an injection molding machine (manufactured by Meiki Co., Ltd., M-100C) under the conditions of a barrel temperature of 260° C., a mold temperature of 50° C., and an injection speed of 50 mm / sec to obtain a rectangular test piece having a thickness of 4 mm, a long piece of 80 mm, and a short side of 10 mm. The flexural modulus of each test piece was measured according to the method described in JIS K7171 using a precision universal testing machine Autograph AG-IS 5kN manufactured by Shimadzu Corporation.
[0239] (Saturated water absorption)
[0240] The acrylic copolymer obtained in each manufacturing example and the acrylic resin composition obtained in each embodiment and comparative example were injection molded using an injection molding machine (manufactured by Mingji Co., Ltd., M-100C) at a barrel temperature of 260°C, a mold temperature of 50°C and an injection speed of 50mm / second to obtain a square test piece with a thickness of 3mm and a side length of 50mm. The test piece was vacuum dried for 24 hours at a temperature of 80°C and 5mmHg. Subsequently, the test piece was cooled in a dryer. After taking out the test piece from the dryer, the mass (initial mass) was immediately measured. Subsequently, the test piece was immersed in distilled water at 23°C. The test piece was taken out of the water, the water attached to the surface was wiped off, and the mass was measured. Repeat immersion in distilled water and measuring the mass until the mass did not change. Using the mass (water absorption mass) when there was no mass change and the initial mass, the saturated water absorption rate was calculated by the following formula.
[0241] Saturated water absorption (%) = [(water absorption mass - initial mass) / initial mass] × 100
[0242] (Formability)
[0243] The acrylic resin composition obtained in each example and comparative example was injection molded using an injection molding machine (manufactured by Meiki Co., Ltd., M-100C) under the conditions of a barrel temperature of 280° C., a mold temperature of 75° C., and a molding cycle of 1 minute to produce a flat plate having a length of 205 mm, a width of 160 mm, and a thickness of 0.5 mm. The ratio of the resin flow length (190 mm) to the thickness was 380.
[0244] In addition, the acrylic resin composition obtained in each Example and Comparative Example was extruded from a T-die having a width of 150 mm at a resin temperature of 260° C. using a single screw extruder having a screw diameter of 20 mm to obtain a single layer film having a width of 100 mm and a thickness of 80 μm.
[0245] The appearance of the flat plate was visually observed. The quality of the formability was determined based on the presence or absence of forming defects such as sink marks and silver streaks. In addition, the appearance of the film was visually observed. The quality of the formability was determined based on the presence or absence of bubbles or gel particles.
[0246] A: No sink marks and no silver streaks occur in the molded product, and no bubbles and no gelation defects occur in the film.
[0247] C: Sink marks or silver streaks appear in the molded product, or bubbles or gelation defects appear in the film.
[0248] (Dimensional stability)
[0249] The acrylic resin composition obtained in each of the Examples and Comparative Examples was injection molded using an injection molding machine (manufactured by Meiki Co., Ltd., M-100C) under the conditions of a barrel temperature of 280° C., a mold temperature of 75° C., and a molding cycle of 1 minute to produce a flat plate having a length of 205 mm, a width of 160 mm, and a thickness of 0.5 mm. The ratio of the resin flow length (190 mm) to the thickness was 380.
[0250] The plate was placed in a thermostat at (1) 60°C and 90% relative humidity and (2) 90°C and 60% relative humidity, and the plate was left in the atmosphere for 500 hours. The plate was taken out of the thermostat and the lengthwise dimension was measured. The dimensional change rate compared to the lengthwise dimension before the plate was placed in the thermostat was calculated.
[0251] The dimensional change rate of 0.3% or less under both conditions (1) and (2) is marked as "H".
[0252] A dimensional change rate of 0.3% or less under either of conditions (1) and (2) is marked as "A", and
[0253] The dimensional change rate greater than 0.3% under both conditions (1) and (2) was marked as "C".
[0254] (Pencil hardness)
[0255] The acrylic resin composition obtained in each of the Examples and Comparative Examples was injection molded using an injection molding machine (manufactured by Meiki Co., Ltd., M-100C) under the conditions of a cylinder temperature of 260° C., a mold temperature of 50° C., and an injection speed of 50 mm / sec to obtain a square test piece having a thickness of 3 mm and a side length of 50 mm.
[0256] In addition, the acrylic resin composition obtained in each Example and Comparative Example was extruded from a T-die having a width of 150 mm at a resin temperature of 260° C. using a single screw extruder having a screw diameter of 20 mm to obtain a single layer film having a width of 100 mm and a thickness of 80 μm.
[0257] The pencil hardness of each test piece and the single-layer film was measured under a load of 0.75 kg in accordance with JIS K5600-5-4.
[0258] A: The pencil hardness of each test piece and the single-layer film is H or higher
[0259] C: The pencil hardness of the test piece or single-layer film is F or less
[0260] (Precursor polymer)
[0261] Precursor polymers Aa to Af and Ah according to this Production Example were prepared by the following method.
[0262] Precursor polymers Aa~Af and Ah
[0263] Purified methyl methacrylate (MMA), α-methylstyrene (αMSt), styrene (St), 2,2'-azobis(2-methylpropionitrile) (AIBN) and n-octyl mercaptan (n-OM) were charged into an autoclave with a stirrer in the proportions shown in Table 1, and the mixture was uniformly dissolved to obtain a polymerization raw material. Nitrogen was blown into the reaction raw material to remove dissolved oxygen to 3 ppm. Subsequently, the interior of a continuous flow tank reactor equipped with a brine cooling condenser was replaced with nitrogen. The polymerization raw material was continuously supplied to the tank reactor at a constant flow rate to have an average residence time shown in Table 1, the polymerization raw material was bulk polymerized at the polymerization temperature shown in Table 1, and a solution containing a precursor polymer was continuously discharged from the tank reactor. It should be noted that the pressure in the tank reactor was adjusted by a pressure regulating valve connected to the brine cooling condenser. The polymerization conversion rate is the value shown in Table 1. Subsequently, the solution discharged from the reactor was heated to 230°C and supplied to a twin-screw extruder controlled at 240°C. In the twin-screw extruder, volatiles consisting of unreacted monomers as the main component are separated and removed, and the precursor polymer is extruded as a strip material. The strip material is cut with a granulator to obtain the precursor polymer. The weight average molecular weight Mw, the ratio of each monomer unit and the glass transition temperature of the obtained precursor polymer are measured. The results are shown in Table 1.
[0264] Precursor polymer Ag
[0265] MS resin (copolymer of methyl methacrylate (MMA) and styrene (St)) was produced according to the method for producing copolymer (A) described in the [Example] section of JP2003-231785A. By changing the mass ratio of MMA, St and tert-dodecyl mercaptan (t-DM) charged into the autoclave, a precursor polymer Ag having Mw = 95,000, Tg = 116°C and a styrene monomer unit content of 10% by mass was obtained.
[0266] (Acrylic copolymer (A))
[0267] Production Example 1
[0268] The conveying section of a twin-screw extruder (manufactured by The Japan Steel Works, LTD., trade name: TEX30α-77AW-3V) which includes a conveying section, a melt-kneading section, a devolatilization section and a discharge section and in which the screw speed and temperature are set to 100 rpm and 230° C., respectively, is supplied with an acrylic copolymer [Aa] at 10 kg / hour, and in the melt-kneading section installed in the kneading block, the amount of monomethylamine is adjusted so that the content of the structural unit derived from glutarimide is as shown in Table 1, and monomethylamine is injected through the additive supply port of the twin-screw extruder to react the acrylic copolymer [Aa] with the monomethylamine. It should be noted that most of the melt-kneading section includes a kneading disk, and sealing elements are connected to both ends thereof. In the devolatilization section, by-products and excess monomethylamine are volatilized from the molten resin passing through the melt-kneading section and discharged through multiple exhaust ports.
[0269] The molten resin discharged as a strand from the die head provided at the end of the discharge section of the twin-screw extruder was cooled in a water tank, and then the strand was cut by a pelletizer to obtain pelletized imidized resin [A-1]. The content of the structural unit derived from glutarimide in the imidized resin [A-1] was 9% by weight. The composition and physical properties of the imidized resin [A-1] are shown in Table 1.
[0270] Production Example 2
[0271] An imidized resin [A-2] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ab] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 7 wt %. The composition and physical properties of the imidized resin [A-2] are shown in Table 1.
[0272] Production Example 3
[0273] An imidized resin [A-3] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ab] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 15% by weight. The composition and physical properties of the imidized resin [A-3] are shown in Table 1.
[0274] Production Example 4
[0275] An imidized resin [A-4] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ac] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 8% by weight. The composition and physical properties of the imidized resin [A-4] are shown in Table 1.
[0276] Production Example 5
[0277] An imidized resin [A-5] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ad] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 9% by weight. The composition and physical properties of the imidized resin [A-5] are shown in Table 1.
[0278] Production Example 6
[0279] An imidized resin [A-6] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ad] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 23% by weight. The composition and physical properties of the imidized resin [A-6] are shown in Table 1.
[0280] Production Example 7
[0281] An imidized resin [A-7] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ad] was used instead of the acrylic copolymer [Aa] and the amount of ammonia added was changed instead of monomethylamine so that the content of the structural unit derived from glutarimide was 15% by weight. The composition and physical properties of the imidized resin [A-7] are shown in Table 1.
[0282] Production Example 8
[0283] An imidized resin [A-8] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ae] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 19% by weight. The composition and physical properties of the imidized resin [A-8] are shown in Table 1.
[0284] Production Example 9
[0285] An imidized resin [A-9] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Af] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 12% by weight. The composition and physical properties of the imidized resin [A-9] are shown in Table 1.
[0286] Production Example 10
[0287] An imidized resin [A-10] was obtained in the same manner as in Example 1, except that the acrylic copolymer [Ab] was used instead of the acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 45% by weight. The composition and physical properties of the imidized resin [A-10] are shown in Table 1.
[0288] Production Example 11
[0289] An imidized resin [A-11] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ag] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 10% by weight. The composition and physical properties of the imidized resin [A-11] are shown in Table 1.
[0290] Production Example 12
[0291] An imidized resin [A-12] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ag] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 44% by weight. The composition and physical properties of the imidized resin [A-12] are shown in Table 1.
[0292] Production Example 13
[0293] An imidized resin [A-13] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ah] was used instead of an acrylic copolymer [Aa] and the amount of monomethylamine added was changed so that the content of the structural unit derived from glutarimide was 24% by weight. The composition and physical properties of the imidized resin [A-13] are shown in Table 1.
[0294] Production Example 14
[0295] An imidized resin [A-14] was obtained in the same manner as in Example 1, except that an acrylic copolymer [Ab] was used instead of the acrylic copolymer [Aa] and the acrylic copolymer was passed through an extruder without adding an imidizing agent. The composition and physical properties of the imidized resin [A-14] are shown in Table 1.
[0296] [Table 1]
[0297]
[0298] (Elastomer)
[0299] Production Example 15
[0300] 1,050 parts by mass of ion exchange water, 0.44 parts by mass of polyoxyethylene tridecyl ether sodium acetate and 0.7 parts by mass of sodium carbonate were loaded into a reactor equipped with an agitator, a thermometer, a nitrogen inlet pipe, a monomer inlet pipe and a reflux condenser, and the interior of the reactor was fully replaced with nitrogen. Subsequently, the internal temperature was set to 80 ° C. 0.25 parts by mass of potassium persulfate was added thereto and stirred for 5 minutes. 245 parts by mass of a monomer mixture containing 95.4% by mass of methyl methacrylate, 4.4% by mass of methyl acrylate and 0.2% by mass of allyl methacrylate were continuously added thereto for 60 minutes. After the addition was completed, a polymerization reaction was further carried out for 30 minutes so that the polymerization conversion rate was 98% or more.
[0301] Subsequently, 0.32 parts by mass of potassium persulfate was added to the same reactor and stirred for 5 minutes. Thereafter, 315 parts by mass of a monomer mixture containing 80.5% by mass of butyl acrylate, 17.5% by mass of styrene and 2% by mass of allyl methacrylate was continuously dripped therein over 60 minutes. After the dripping was completed, a polymerization reaction was further carried out for 30 minutes, so that the polymerization conversion rate was 98% or more.
[0302] Next, 0.14 parts by mass of potassium persulfate was added to the same reactor and stirred for 5 minutes. Thereafter, 140 parts by mass of a monomer mixture containing 95.2% by mass of methyl methacrylate, 4.4% by mass of methyl acrylate and 0.4% by mass of n-octyl mercaptan was continuously dripped over 30 minutes. After the dripping was completed, a polymerization reaction was further carried out for 60 minutes so that the polymerization conversion rate was more than 98%. Through the above operation, a latex containing a multilayer copolymer elastomer was obtained. The latex was frozen and solidified. Subsequently, the latex was washed with water and dried to obtain a multilayer copolymer elastomer (B-1). The average particle size of the multilayer copolymer elastomer (B-1) is 0.2 μm.
[0303] Production Example 16
[0304] Into a pressure-resistant autoclave were charged 150 parts by mass of ion-exchanged water, 85 parts by mass of 1,3-butadiene, 15 parts by mass of styrene, 0.5 parts by mass of tert-dodecyl mercaptan, 0.4 parts by mass of diisopropylbenzene hydroperoxide, 1.5 parts by mass of sodium pyrophosphate, 0.02 parts by mass of ferrous sulfate, 1.0 parts by mass of dextrose and 1.0 parts by mass of potassium oleate, and the mixture was reacted at 50° C. for 15 hours with stirring, thereby producing a butadiene-based rubber polymer latex.
[0305] 65 parts of the butadiene rubber polymer latex (in terms of solid content) were placed in a flask and purged with nitrogen. 1.2 parts by mass of NaHCO in the form of a 10% aqueous solution was added. 3 , and stirred for 30 minutes. 1 part of potassium oleate in the form of a 7% aqueous solution was added to the solution to stabilize the solution. Thereafter, 0.6 parts by mass of Rongalite was added, the solution temperature was maintained at 70°C, and 35 parts by mass of a monomer mixture having the following composition was graft polymerized with the butadiene rubber polymer latex.
[0306] A mixture of 40 parts by mass of methyl methacrylate, 5 parts by mass of ethyl acrylate and 0.1 parts by mass of tert-butyl hydroperoxide (t-BH) was added dropwise over 1 hour based on 100 parts by mass of the total graft monomer mixture as a monomer mixture for the first grafting stage, and the mixture was continuously stirred for 2 hours for polymerization. Thereafter, a mixture of 40 parts by mass of styrene and 0.1 parts by mass of t-BH was added dropwise over 1 hour as a monomer mixture for the second grafting stage, and the mixture was continuously stirred for 2 hours for polymerization. Finally, a mixture of 15 parts by mass of methyl methacrylate and 0.05 parts by mass of t-BH was added dropwise over 1 hour as a monomer mixture for the third grafting stage, and the mixture was continuously stirred for 2 hours for polymerization, thereby obtaining a latex of a multilayer copolymer elastomer (B-2).
[0307] 0.5 parts by mass of BHT was added to the obtained latex of the multilayer copolymer elastomer (B-2), and a 0.2% sulfuric acid aqueous solution was added to coagulate the multilayer copolymer elastomer (B-2), and heat-treated and cured at 90° C. Thereafter, the coagulant was washed with warm water and further dried to obtain a multilayer copolymer elastomer (B-2) powder. The average particle size of the multilayer copolymer elastomer (B-2) was 0.2 μm.
[0308] Production Example 17
[0309] At room temperature, 3 m 3735 kg of anhydrous toluene, 0.4 kg of hexamethyltriethylenetetramine and 39.4 kg of a toluene solution containing 20 mol of isobutylbis(2,6-di-tert-butyl-4-methylphenoxy)aluminum were added to a glass-lined reaction vessel (the reaction vessel was capable of brine cooling and equipped with a jacket and a stirrer), and further 1.17 mol of sec-butyllithium was added. 35.0 kg of methyl methacrylate was added thereto, and the mixture was reacted at room temperature for 1 hour to obtain a methyl methacrylate polymer (polymer block (b1-1)) having a weight average molecular weight (referred to as Mw(b1-1)) of 40,000.
[0310] Subsequently, while the reaction container was maintained at -25°C, a mixed solution of 24.5 kg of n-butyl acrylate and 10.5 kg of benzyl acrylate was added dropwise over 0.5 hours, and a polymer block (b2) of a copolymer containing n-butyl acrylate and benzyl acrylate was grown from one end of the polymer block (b1-1), thereby obtaining a diblock copolymer elastomer (B-3) having a weight average molecular weight of 80,000. Since the weight average molecular weight of the polymer block (b1-1) was 40,000, the weight average molecular weight (Mw(b2)) of the polymer block (b2) was determined to be 40,000. The content of acrylate in the diblock copolymer elastomer (B-3) was 50% by mass.
[0311] Example 1
[0312] 80 parts by mass of the acrylic copolymer (A-1) and 20 parts by mass of the multilayer copolymer elastomer (B-1) were mixed with each other, and the mixture was melt-kneaded and extruded at 250° C. using a twin-screw extruder having a screw diameter of 20 mm to obtain a pelletized acrylic resin composition (C-1) having a glass transition temperature of 120° C. The evaluation results are shown in Table 2.
[0313] Examples 2 to 12
[0314] An acrylic resin composition was obtained in the same manner as in Example 1 except for the formulation described in Table 2. The evaluation results are shown in Table 2.
[0315] [Table 2]
[0316]
[0317] Comparative Examples 1 to 7
[0318] An acrylic resin composition was obtained in the same manner as in Example 1 except for the formulation described in Table 2. The evaluation results are shown in Table 3.
[0319] [Table 3]
[0320]
[0321] As shown in Tables 1 to 3, since the acrylic resin composition of the present invention contains an acrylic copolymer having an excellent balance of heat resistance, low water absorption and thermal decomposition resistance, the acrylic resin composition maintains high heat resistance, low water absorption and high rigidity even when an elastomer is added, and has excellent thermal stability. The acrylic resin composition of the present invention can provide a molded body and a film having excellent dimensional stability, moldability and surface hardness.
Claims
1. An acrylic resin composition, comprising: 51 to 99% by mass of an acrylic copolymer (A) containing 30 to 87% by mass of methyl methacrylate units, 6 to 40% by mass of a structural unit (R), 7 to 30% by mass of an α-methylstyrene unit, and 0 to 20% by mass of other vinyl monomer units (C) copolymerizable with methyl methacrylate, wherein the structural unit (R) is an N-substituted glutarimide unit represented by formula (I) In formula (I), R 1 are each independently a hydrogen atom or a methyl group, and R 2 is an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aromatic ring-containing organic group having 6 to 15 carbon atoms; and 1 to 49% by mass of an elastomer (B), The other vinyl monomer units (C) copolymerizable with the methyl methacrylate units include at least one selected from the group consisting of acrylic acid ester monomers, aromatic vinyl monomers and vinyl cyanide monomers. 2 . The acrylic resin composition according to claim 1 , wherein the other vinyl monomer unit (C) copolymerizable with the methyl methacrylate unit is formed of at least one selected from the group consisting of methyl acrylate, ethyl acrylate, styrene and acrylonitrile. 3 . The acrylic resin composition according to claim 1 , wherein the other vinyl monomer unit (C) copolymerizable with the methyl methacrylate unit is formed of styrene. 4 . The acrylic resin composition according to claim 1 , wherein the elastomer (B) comprises a multi-layer copolymer elastomer containing a methacrylate unit and an acrylate unit. 5 . The acrylic resin composition according to claim 1 , wherein the elastomer (B) comprises a block copolymer elastomer composed of a polymer block (b1) containing a methacrylate unit and a polymer block (b2) containing an acrylate unit. 6 . The acrylic resin composition according to claim 1 , wherein the softening temperature of the molded article is 110° C. or higher when measured by the method specified in the B50 method of JIS K7206.
7. The acrylic resin composition according to claim 1 or 2, wherein the saturated water absorption is 2.5% or less. 8 . A molded body comprising the acrylic resin composition according to claim 1 . 9 . A film comprising the acrylic resin composition according to claim 1 .