Preparation method of micro-membrane adsorption material for quickly and efficiently adsorbing radionuclide thorium ion
Patent Information
- Application Number
- CN202310499379.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2026-09-29
- Estimated Expiration
- 2043-05-06
AI Technical Summary
[0008]本发明主要是解决传统的吸附工艺中,吸附剂吸附效率低,活性位点少和难以回收等问题,因此,提供了一种快速且高效地去除放射性废水中核素离子的微膜吸附材料及其制备方法
[0018]本发明提供的是一种快速高效吸附核素离子的微膜吸附材料的制备方法和其他方法相比,具体有以下有益效果:
Smart Images

Figure CN116550307B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of adsorbing thorium ions from radioactive wastewater, specifically relating to a novel micromembrane adsorption material for rapidly and efficiently adsorbing radioactive ion ions and its preparation method. Background Technology
[0002] Thorium (Th(IV)) is a widely used, naturally occurring radioactive element, mostly distributed in the Earth's crust. As a key element in the nuclear fuel cycle, thorium's high efficiency and economy have made it a crucial element in nuclear energy projects. However, due to its radioactivity, toxicity, and high mobility, it poses potential ecological and health risks to the biosphere. Therefore, research on thorium removal and remediation in aquatic environments is of great significance for reducing the threat of thorium pollution to organisms and the ecosystem. Because the specific activity and salinity of various radioactive waste liquids differ greatly, the treatment methods also vary. Radioactive waste liquids from the nuclear industry generally require multi-stage purification treatment, and commonly used methods for treating low- and intermediate-level radioactive waste liquids include chemical precipitation, evaporation concentration, ion exchange, adsorption separation, biological treatment, and membrane technology. Among these methods, adsorption is the most efficient and thorough, and is therefore widely used.
[0003] In recent years, various literatures have reported on the adsorption and removal of radioactive metal ions in water by various adsorbents. Currently, a large number of materials are used to remove Th(IV), such as activated carbon, clay minerals, polymer fibers, modified bentonite, polymers, metal oxides, and metal-organic frameworks (MOFs). MOFs are a new type of porous material composed of metal ions / ion clusters and organic bridging ligands. They have attracted widespread attention due to their high specific surface area, large porosity, tunable pore size, controllable functional groups, and excellent performance in fields such as gas storage, gas and dye separation, sensing, catalysis, and drug delivery. In recent years, various MOFs have been used to adsorb radioactive waste liquids from water, showing broad application prospects in thorium adsorption. The zeolite-type imidazole framework-67 (ZIF-67), composed of Co(II) and 2-methylimidazolium, is a subclass of MOFs with a zeolite topology. ZIF-67 exhibits significant chemical and thermal stability and a wide range of accessible surfaces (approximately 420–1800 μm). 2 With its unique structure and active surface sites, it is one of the MOF materials with excellent adsorption properties.
[0004] However, ZIF-67, as a hydrophobic powder material, is generally not conducive to separation and recovery from water, easily causing secondary pollution and clogging. However, if nanoparticles are immobilized on the inner wall of the membrane pores using a deep-penetration method, more active sites, better stability, and repeatability can be obtained. Unlike other adsorbent materials immobilized on the membrane surface, loading on the inner wall of the membrane pores yields more active sites, a larger specific surface area, and better loading capacity. Furthermore, the uniform pore size distribution not only improves the dispersibility of nanoparticles but also enhances the efficiency of fluid flow. With the aid of external force and using a deep-penetration method, reactants can be completely infiltrated into the membrane pores, generating nanoparticles in situ on the inner wall.
[0005] In the invention patent application with application number CN202110674739.0, a high-efficiency adsorbent for treating uranium-containing wastewater based functionalized nanocomposite microspheres is introduced. Although functionalized microspheres are a new type of functional material, they can be made functional through surface grafting and modification. However, their repeatability is low and they are not easy to recycle, which can easily cause secondary pollution.
[0006] In Chinese patent application CN202210564303.0, a ZIF-67-loaded nanofiber membrane material for adsorbing phenolic substances from wastewater and its preparation method are disclosed. Using ZIF-67 nanocrystals as the material improves the adsorption performance of polyvinyl butyral fiber membranes for phenols, and using polyvinyl butyral as the material improves the spinning performance of polyurethane fiber membranes. Although this method avoids high raw material costs and cumbersome experimental operations, the retention rate of MOFs is low, and the hydrophobicity of electrospinning greatly limits their practical application.
[0007] To our knowledge, there are currently no experimental studies on the preparation of ZIF-67@PA composite materials for thorium removal using deep permeation methods. Therefore, this invention proposes a method for preparing a rapid and efficient micromembrane adsorbent material for Th(IV) removal. To ensure that the reactants completely permeate into the membrane pores and adhere to the inner wall, forming specialized adsorption channels, we use a deep permeation synthesis (DPSF) method with synergistic permeation reaction to load ZIF-67 nanoparticles into the pore walls of a PA membrane. Then, we apply the ZIF-67@PA composite adsorbent membrane material to remove radioactive thorium ions from the solution. This method achieves higher active sites within the membrane pores, significantly improving adsorption capacity and efficiency, and allows for reusability without causing secondary pollution. Summary of the Invention
[0008] This invention primarily addresses the problems of low adsorption efficiency, limited active sites, and difficulty in recovery of adsorbents in traditional adsorption processes. Therefore, it provides a micromembrane adsorption material and its preparation method for rapidly and efficiently removing radionuclide ions from radioactive wastewater. The product uses cobalt nitrate hexahydrate and 2-methylimidazole as raw materials, and a polyamide microporous membrane as the substrate membrane. ZIF-67 nanoparticles are synthesized in situ on the surface of the polyamide microporous membrane and the inner walls of the pores using a deep permeation method.
[0009] The technical problems to be solved by this invention are as follows: existing nanopowder materials not only have low adsorption capacity and low reusability, but aerogels are also limited by their lack of sufficient flexibility and stability, and the hydrophobic properties of electrospun materials also cause problems. Therefore, a novel microfilm adsorption preparation method for rapidly and efficiently removing thorium ions from radioactive wastewater is proposed.
[0010] To solve the above technical problems, the present invention adopts the following technical solution:
[0011] S1: First, commercial polyamide microporous membranes (PA) are placed in a 50w% formic acid solution for 30min to activate them, causing the long chains on the polyamide to break down and thus exposing more functional groups.
[0012] S2: Next, the activated PA membrane is placed in the membrane module filter, and under a certain pressure, 0.048 mol / L cobalt nitrate hexahydrate (Co(NO3)2·6H2O) is slowly permeated through the membrane at a certain flow rate.
[0013] S3: After the permeation is complete, place the membrane in a vacuum drying oven and dry for 30 minutes. The dried Co(NO3)2·6H2O will recrystallize and precipitate on the membrane pore walls of the PA membrane.
[0014] S4: Using the same method, a PA membrane with Co(NO3)2·6H2O attached to the membrane pore wall is installed in a membrane module, and an aqueous solution containing 2-methylimidazole (2-MI) is slowly permeated under a certain pressure.
[0015] S5: After permeation, place the membrane in a vacuum drying oven and dry for 30 minutes. Repeat the above steps 4-6 times to obtain PA membrane material with ZIF-67 nanoparticles attached to the membrane pore walls;
[0016] S6: Finally, ultrasonic cleaning is used to remove unreacted ligands and residual nanoparticles from the PA film surface.
[0017] Beneficial effects:
[0018] The present invention provides a method for preparing a micromembrane adsorption material for rapid and efficient adsorption of radionuclide ions. Compared with other methods, it has the following advantages:
[0019] (1) The technical solution of the present invention uses a polyamide microporous membrane as the base membrane. The membrane has good hydrophilicity and chemical stability, and can withstand high concentrations of acidic solutions and appropriate concentrations of alkaline solutions. The porous membrane has a uniform pore size distribution, which can improve the dispersibility of nano-adsorbent materials.
[0020] (2) The zeolite-type imidazole framework-67 used in the technical solution of this invention is a subclass of metal-organic framework materials with a zeolite topology. Zeolite-type imidazole framework-67 exhibits significant chemical and thermal stability and a wide range of accessible surfaces (approximately 420–1800 μm). 2 / g), providing more active surface sites;
[0021] (3) The technical solution of the present invention uses a deep penetration method to synthesize ZIF-67 nanoparticles in situ and introduce them into a polyamide microporous membrane rich in various functional groups. By applying external pressure, the reactants are forced to flow and can eventually penetrate into the inner wall of the membrane pores. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the preparation of ZIF-67@PA, including Co(II) loading on the membrane substrate, the synthesis of ZIF-67, the cross-sectional structure of the membrane, and the schematic diagram of the bonding between ZIF-67 and the PA membrane.
[0023] Figure 2 A schematic diagram of the adsorption process using micromembrane adsorption materials and ZIF-67 powder materials;
[0024] Figure 3 The BET spectra of the ZIF-67@PA microfilm adsorption material are shown, which are nitrogen adsorption-desorption isotherms and pore size distribution curves, respectively.
[0025] Figure 4 XRD pattern of ZIF-67@PA microfilm adsorption material;
[0026] Figure 5 The FTIR spectrum of the ZIF-67@PA microfilm adsorption material;
[0027] Figure 6 SEM image (ac) of PA membrane, SEM image (df) of ZIF-67@PA micromembrane adsorption material;
[0028] Figure 7 Energy dispersive spectroscopy-surface scan of ZIF-67@PA microfilm adsorption material;
[0029] Figure 8 XPS spectra of ZIF-67@PA micromembrane adsorption material;
[0030] Figure 9 Contact angle diagrams of PA membrane, ZIF-67 nanoparticles, and ZIF-67@PA micromembrane adsorption material;
[0031] Figure 10 A graph showing the adsorption capacity of ZIF-67@PA micromembrane adsorbent material for Th(IV) as the solution pH changes.
[0032] Figure 11 A graph showing the kinetic model of Th(IV) adsorption by ZIF-67@PA micromembrane adsorbent material as a function of adsorbing radioactive thorium ions over time.
[0033] Figure 12 A graph showing the adsorption isotherm of Th(IV) on ZIF-67@PA microfilm adsorbent material for adsorbing radioactive thorium ions.
[0034] Figure 13 Thermodynamic curves of Th(IV) adsorption by ZIF-67@PA micromembrane adsorbent material for adsorbing radioactive thorium ions as a function of temperature.
[0035] Figure 14 A graph showing the adsorption capacity of ZIF-67@PA micromembrane adsorbent material for Th(IV) during recycling. Detailed Implementation
[0036] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0037] Example 1:
[0038] (1) Material preparation steps:
[0039] 1) Preparation of ZIF-67 nanoparticles: 1.4 g Co(NO3)2·6H2O and 8.0 g 2-methylimidazole were dissolved in 80.0 mL and 30.0 mL of deionized water, respectively. Then, 2-methylimidazole was added to the Co(NO3)2·6H2O solution and stirred rapidly for 5 minutes. After keeping the purple suspension at room temperature for 24 hours, it was centrifuged three times with deionized water to ensure purity. Finally, the precipitate was dried overnight at 60 °C in a vacuum drying oven.
[0040] 2) Preparation of ZIF-67@PA micromembrane adsorbent material: First, a commercially available PA membrane was activated in a 50% formic acid solution for 30 min to break the long chains on the polyamide, thereby exposing more amino groups. Next, it was placed in a membrane module filter, and under a certain pressure, a Co(NO3)2·6H2O solution (0.048 mol / L, 25 mL) was slowly added to the membrane at a flow rate of 0.25 mL / L. After permeation, the membrane was dried in a vacuum drying oven at 60℃ for 30 min. The dried Co(NO3)2·6H2O recrystallized and precipitated in the pores of the PA membrane. Then, using the same method, a PA membrane already loaded with Co(NO3)2·6H2O in the pores was installed in a membrane module, and under a certain pressure, a mixed solution of 2-Hmim (2.0 g) and methanol (20 mL) was slowly permeated. After permeation, it was dried at 60℃ for 1 h. Repeat the above steps 3-4 times to obtain a PA membrane material with ZIF-67 nanoparticles loaded in the membrane pores. Finally, ultrasonic cleaning is used to remove unreacted ligands and residual nanoparticles from the PA membrane surface.
[0041] (2) Adsorption experiment:
[0042] The adsorption experiment was conducted at room temperature (298 K). ZIF-67 nanoparticles were placed in a thorium ion solution (30 mL). After a predetermined adsorption time, the supernatant was collected by centrifugation. A colorimetric reagent was added to the solution, and the thorium ion content in the sample was determined using a visible spectrophotometer. Similarly, PA micromembrane material loaded with ZIF-67 was placed in a membrane module, and peristaltic pumps were used to circulate and permeate different concentrations of thorium(IV) solutions (30 mL) at a certain flow rate, as shown in the attached figure. Figure 2 As shown. After the predetermined adsorption time, a colorimetric reagent was added to the solution, and the thorium ion content in the sample was determined by a visible spectrophotometer. The thorium ion solution was prepared by dissolving an appropriate amount of thorium nitrate tetrahydrate (Th(NO3)4·4H2O) in deionized water.
[0043] Experimental Example 1:
[0044] This invention employs a deep-penetration method to synthesize ZIF-67 nanoparticles in situ on the inner wall and surface of a polyamide microporous membrane. The large specific surface area and uniform pore size distribution of the membrane pores provide more possibilities for nanoparticle loading, not only without affecting the pore size but also improving dispersion and adsorption performance. Characterization tests performed on the samples in Example 1 show that the ZIF-67@PA micromembrane adsorbent material has been successfully prepared. Adsorption capacity tests for thorium ions were conducted on the samples, exploring performance under different pH values, adsorption times, initial adsorption concentrations, temperatures, and reusability. The results indicate that the ZIF-67@PA micromembrane adsorbent material possesses an extremely high adsorption capacity for Th(IV) and good reproducibility.
[0045] (1) Chemical composition analysis of ZIF-67@PA micromembrane adsorption material: XRD, BET, FTIR, SEM, EDS and XPS analyses were performed. The results are shown in the appendix. Figure 3-8 .from Figure 3 As can be seen, the ZIF-67 nanoparticles synthesized in situ on the pore walls of the PA membrane still have a high specific surface area and porosity. Figure 4 The XRD pattern shown indicates that characteristic peaks of ZIF-67 appear at 2θ = 7.2°, 17.7°, 22.4°, and 26.0°, suggesting that ZIF-67 is loaded within the membrane pore walls. Figure 5 As can be seen, at 3186cm -1 2865cm -1 1415cm -1 and 428cm -1 Characteristic peaks were observed in all samples, which proves that ZIF-67 nanoparticles were successfully loaded onto the PA film and that the characteristic structure and characteristic peaks remained unchanged. Figure 6 and Figure 7 SEM-EDS characterization analysis was used to further investigate and prove the uniform distribution and morphological characteristics of ZIF-67 nanoparticles in the PA membrane pores. Figure 8 The XPS analysis of (ae) also demonstrated the successful loading of ZIF-67 nanoparticles.
[0046] (2) Quantitative analysis of the hydrophilicity and hydrophobicity of the materials: The contact angle (CA) was used to evaluate the PA film, ZIF-67 nanoparticles, and ZIF-67@PA microfilm adsorption materials. Generally, a CA greater than 90° is considered hydrophobic, and a CA less than 90° is considered hydrophilic. Figure 9As shown, ZIF-67 crystals exhibit strong hydrophobicity (83.9°) due to the presence of imidazole groups, while the PA film, containing phenolic hydroxyl and imino groups, is inherently hydrophilic (24.9°). The loading of ZIF-67 nanoparticles enhances its hydrophobicity to a certain extent. This is because the addition of 2-methylimidazole increases the hydrophobic properties, but the contact angle of 47.4° still falls within the hydrophilic range.
[0047] (3) Performance testing of ZIF-67@PA micromembrane adsorption material:
[0048] Thorium ion solutions of different concentrations were prepared, and different pH values, initial concentrations, adsorption times, and test temperatures were set to test the adsorption capacity. Specific experimental results are attached. Figure 10-13 .
[0049] like Figure 10 As shown in the figure, when pH < 5, the adsorption capacity increases linearly, which is attributed to the adsorption effect of the adsorbent material. After pH > 5, Th... 4+ The reduction in ion concentration and the tendency for mononuclear complexes to precipitate from the solution significantly diminish the adsorption efficiency of the micromembrane adsorbent material. Finally, we conclude that selecting pH=5.0 and using the ZIF-67@PA micromembrane adsorbent material for quantitative adsorption of tetravalent thorium ions yields the best results. Figure 11 As shown, to investigate the effect of adsorption time on the adsorption performance of ZIF-67@PA micromembrane adsorbent material for thorium ions, the obtained experimental data were nonlinearly fitted using pseudo-first-order and pseudo-second-order kinetic models. It can be seen that before 40 min, the adsorption capacity increases rapidly with increasing adsorption time, and then gradually plateaus after 50 min, ceasing its increase. The R² of the second-order kinetic model (0.987) is higher than that of the pseudo-first-order kinetic model (0.963), indicating that the adsorption capacity of the pseudo-second-order kinetic model is more consistent with the experimental values. Furthermore, the qe value calculated by the pseudo-second-order kinetic model (692.72 mg / g) is closer to the experimentally measured value (703.59 mg / g), further indicating that the adsorption process is mainly controlled by chemical bonds, rather than a simple physical reaction. Figure 12The degree of overlap between the experimental curves and the two isotherm models is shown. It is clear that the Langmuir adsorption isotherm model better matches the original experimental data. This means that the adsorption of Th(IV) by the ZIF-67@PA microfilm adsorbent material tends to be a monolayer combination, with chemisorption being the main interaction mechanism. Furthermore, the maximum adsorption capacity of Th(IV) by the ZIF-67@PA microfilm adsorbent material is 703.59 mg / L, obtained using the Langmuir isotherm adsorption model. To evaluate the effect of temperature on the adsorption process, a series of adsorption experiments were conducted under the conditions of pH=5, initial Th(IV) concentration of 300 mg / g, adsorption time of 50 min, and a range of 298 K–318 K, determining its adsorption thermodynamic parameters for thorium. Within the range of 298 K–318 K, the adsorption capacity of the ZIF-67@PA microfilm adsorbent material for Th(IV) is determined by… Figure 13 It can be seen that the adsorption capacity of the ZIF-67@PA microfilm adsorbent material increases with increasing temperature, indicating that the adsorption process is a spontaneous endothermic process. The Gibbs free energy (ΔG0) decreases with increasing temperature, indicating that the adsorption process of the ZIF-67@PA microfilm material is more likely to occur under high temperature conditions.
[0050] (4) Repeatability test of ZIF-67@PA micromembrane adsorbent material for thorium ion solution:
[0051] from Figure 14 The experimental results show that, in order to evaluate the regenerability of the prepared ZIF-67@PA adsorbent for repeated use of Th(IV) ions, 0.1 mol / L HNO3 solution was used as the eluent, and 7 adsorption-desorption cycles were completed. The adsorption capacity was measured after each cycle. With the increase of the number of cycles, the Th(IV) adsorption-desorption efficiency of the adsorbent gradually decreased to 78%, but it still had good adsorption capacity.
[0052] In summary, based on the above embodiments and experimental results, the beneficial effects of the present invention are manifested in the following aspects:
[0053] (1) Fast and efficient: By studying the adsorption kinetics of adsorption time, this invention shows that the microfilm adsorption material can reach adsorption equilibrium within 50 minutes, with a fast adsorption rate and high adsorption efficiency.
[0054] (2) Large adsorption capacity: In this implementation example 1, we investigated the effect of adsorption concentration and also conducted an analysis of the isothermal adsorption model fitting data, and found that the maximum adsorption capacity of ZIF-67@PA microfilm adsorption material for Th(IV) was 703.59 mg / L.
[0055] (3) Good repeatability: Most of the powder adsorbent materials studied by scholars not only have low adsorption capacity but also low reusability. Aerogels are limited by their lack of sufficient flexibility and stability, and the hydrophobic properties of electrospun materials also pose a problem. In comparison, this invention not only has the ability to rapidly and efficiently adsorb nuclide ions but also has good repeatability.
[0056] The above description is not intended to limit the present invention in any way. Although the present invention has been disclosed through the above embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some changes or modifications to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. The application of a micromembrane adsorption material in the adsorption of radioactive thorium (IV) ions, characterized in that, The preparation method of the micromembrane adsorption material is as follows: S1: The commercial polyamide microporous membrane was placed in a 50wt% formic acid solution for 30 minutes to activate it, causing the long chain portion of the polyamide to break, thereby exposing more amino groups; S2: The activated polyamide microporous membrane is placed in the membrane module filter, and under a certain pressure, a cobalt nitrate hexahydrate solution with a concentration of 0.048 mol / L slowly permeates through the polyamide microporous membrane at a certain flow rate. S3: After the permeation is complete, place the polyamide microporous membrane in a vacuum drying oven at 40℃-60℃ for 30 minutes to allow cobalt nitrate hexahydrate to recrystallize and precipitate on the membrane pore walls of the polyamide microporous membrane. S4: Using the same method, a polyamide microporous membrane with cobalt nitrate hexahydrate attached to the membrane pore wall is installed in the membrane module filter. Under certain pressure conditions, a solution containing 2-methylimidazole is slowly permeated. After permeation, the membrane is placed in a vacuum drying oven and dried at 60°C for 1 hour. S5: Repeat steps S2 to S4 3-4 times to obtain a polyamide microporous membrane material with ZIF-67 nanoparticles attached to the pore walls of the polyamide microporous membrane. S6: Use ultrasonic cleaning to remove unreacted ligands and residual nanoparticles from the surface of the polyamide microporous membrane.
Citation Information
Patent Citations
Preparation method of nanofiber membrane with adsorption performance
CN114855368A
Solidified tannin polyamide microporous membrane and preparation method and application thereof
CN108031450A
Titanium-based functionalized nano-composite microsphere efficient adsorbent for treating uranium-containing wastewater and preparation method thereof
CN113398876A
Preparation method of micro-membrane adsorber for quickly and efficiently adsorbing heavy metal ions
CN114452957A