Rice husk ash cement-based material and preparation method, system and storage medium thereof
By using rice husk ash as the internal curing material in UHPC and optimizing the proportion of rice husk ash, cement, water and chemical admixtures, the problems of UHPC self-shrinkage and cracking are solved, the compressive strength and mechanical properties are improved, and a more efficient Anti-crack effect.
Patent Information
- Application Number
- CN202410419717.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Although existing internal curing materials such as SAP can effectively alleviate the cracking problem of ultra-high performance concrete (UHPC) due to autogenous shrinkage during the hydration reaction, it will affect the mechanical properties, and its incorporation will cause pores and affect the compressive strength.
Rice husk ash is used as the internal curing material, and the proportions of rice husk ash, cement, water and chemical additives are adjusted through surface fitting operations to optimize the compressive strength, reduce autogenous shrinkage and reduce the risk of cracking.
It effectively reduces the autogenous shrinkage of UHPC, improves the compressive strength and stiffness, and reduces the risk of cracking. At the same time, the liquid absorption capacity of rice husk ash and volcanic ash reaction are used to improve the mechanical properties of cement-based materials.
Smart Images

Figure CN118184247B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cement-based materials, and in particular to a rice husk ash cement-based material and a preparation method, system and storage medium thereof. Background Art
[0002] Ultra-high performance concrete (UHPC) has the advantages of good ductility, high compressive strength and good durability. It has been widely used in civil engineering in recent decades. But at the same time, there are still some problems with ultra-high performance concrete, and cracking caused by shrinkage is one of them. Autogenous shrinkage is the phenomenon that the macroscopic volume of cement-based materials decreases due to self-drying caused by the hydration reaction of cementitious materials and the decrease in internal relative humidity under the condition of no material exchange with the outside world. Due to the low water-binder ratio of UHPC, the self-drying caused by cement hydration is much higher than that of ordinary Portland cement concrete, which in turn causes a large autogenous shrinkage. The autogenous shrinkage problem seriously hinders the application of UHPC in actual engineering.
[0003] In order to alleviate the shrinkage of UHPC and reduce the risk of cracking, researchers have carried out a lot of research. Internal curing technology is recognized as a technical means to effectively reduce shrinkage and resist cracking. At present, the concrete internal curing materials that are widely studied and applied are mainly lightweight aggregate (LWA) and super absorbent resin (SAP). Since LWA affects the mechanical properties, it is not applicable in UHPC. SAP is the most commonly used internal curing material in UHPC. SAP is a polymer material that can absorb liquid and keep the liquid in its pore structure. Studies have shown that the shrinkage reduction rate can reach more than 50% by adding SAP to concrete. Although SAP can effectively alleviate the shrinkage of UHPC, there are still some problems. For example, the addition of SAP will cause pores in the cement matrix of UHPC, which will have a negative impact on the mechanical properties of UHPC. Summary of the invention
[0004] The present invention provides a rice husk ash cement-based material and a preparation method, system and storage medium thereof. Rice husk ash is used as an internal curing material, thereby reducing the self-shrinkage of UHPC and lowering the risk of cracking.
[0005] The present specification discloses a method for preparing a rice husk ash cement-based material, comprising:
[0006] Obtain compressive strength, rice husk ash ratio, cement ratio, water ratio and chemical admixture ratio;
[0007] The cement ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a first matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and a cement ratio surface fitting equation are obtained, and the three-dimensional surface is recorded as a first compressive reference domain;
[0008] The water ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a second matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and a water ratio surface fitting equation are obtained, and the three-dimensional surface is recorded as a second compressive reference domain;
[0009] The chemical admixture ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a third matrix is formed, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and a chemical admixture ratio surface fitting equation, and the three-dimensional surface is recorded as a third compressive reference domain;
[0010] Based on the first compressive resistance reference domain, the second compressive resistance reference domain and the third compressive resistance reference domain, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
[0011] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0012] Get temperature and humidity;
[0013] The temperature and humidity are used as row vectors, and the rice husk ash ratio is used as a column vector to form a fourth matrix, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and a temperature and humidity surface fitting equation, and the three-dimensional surface is recorded as a fourth compressive reference domain;
[0014] Based on the first compressive reference domain, the second compressive reference domain, the third compressive reference domain and the fourth compressive reference domain, the real-time temperature and humidity, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength. The rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred at the adjusted real-time temperature and humidity to obtain the rice husk ash cement-based material.
[0015] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0016] Get the aggregate ratio;
[0017] The aggregate ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a fifth matrix is formed, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and an aggregate ratio surface fitting equation, and the three-dimensional surface is recorded as a fifth compressive reference domain;
[0018] Based on the first compressive reference domain, the second compressive reference domain, the third compressive reference domain and the fifth compressive reference domain, the real-time aggregate ratio, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the aggregate, rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
[0019] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0020] Obtain fly ash ratio;
[0021] The fly ash ratio is used as a row vector, and the rice husk ash ratio is used as a column vector to form a sixth matrix, and then the compressive strength is imported, and a surface fitting operation is performed to obtain a three-dimensional surface and a fly ash ratio surface fitting equation, and the three-dimensional surface is recorded as a sixth compressive reference domain;
[0022] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the sixth compressive resistance reference domain, the real-time fly ash ratio, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the fly ash, rice husk ash, cement, water and chemical admixtures with adjusted ratios are stirred to obtain rice husk ash cement-based material.
[0023] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0024] Get aggregate gradation;
[0025] The aggregate gradation is used as a row vector, the rice husk ash ratio is used as a column vector, a seventh matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and an aggregate gradation surface fitting equation are obtained, and the three-dimensional surface is recorded as the seventh compressive reference domain;
[0026] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the seventh compressive resistance reference domain, the real-time aggregate gradation, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the aggregate gradation, rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
[0027] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0028] Obtain the mud content of aggregate;
[0029] The aggregate mud content is used as a row vector, and the rice husk ash ratio is used as a column vector to form an eighth matrix, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and an aggregate mud content surface fitting equation, and the three-dimensional surface is recorded as the eighth compressive reference domain;
[0030] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the eighth compressive resistance reference domain, the real-time aggregate mud content, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the adjusted aggregate mud content and the adjusted ratios of rice husk ash, cement, water and chemical admixture are stirred to obtain a rice husk ash cement-based material.
[0031] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0032] Obtain flexural strength;
[0033] The flexural strength is used as a row vector, and the rice husk ash ratio is used as a column vector to form a ninth matrix, and then the compressive strength is imported, and a surface fitting operation is performed to obtain a three-dimensional surface and a flexural strength surface fitting equation, and the three-dimensional surface is recorded as a ninth compressive reference domain;
[0034] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the ninth compressive resistance reference domain, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to maximize the real-time compression ratio, and the rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
[0035] The embodiments of the present specification also disclose a rice husk ash cement-based material, which is prepared by any of the above-mentioned methods for preparing a rice husk ash cement-based material.
[0036] The present specification also discloses a system for preparing a rice husk ash cement-based material, which is used to implement the method for preparing a rice husk ash cement-based material as described above;
[0037] The preparation system of the rice husk ash cement-based material comprises:
[0038] an acquisition module for acquiring compressive strength, rice husk ash ratio, cement ratio, water ratio and chemical admixture ratio;
[0039] A first fitting module is used to use the cement ratio as a row vector and the rice husk ash ratio as a column vector to form a first matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a cement ratio surface fitting equation, and record the three-dimensional surface as a first compressive reference domain;
[0040] A second fitting module is used to use the water ratio as a row vector and the rice husk ash ratio as a column vector to form a second matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a water ratio surface fitting equation, and record the three-dimensional surface as a second compressive reference domain;
[0041] A third fitting module is used to use the chemical admixture ratio as a row vector and the rice husk ash ratio as a column vector to form a third matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a chemical admixture ratio surface fitting equation, and record the three-dimensional surface as a third compressive reference domain;
[0042] A preparation module is used to adjust the real-time rice husk ash ratio, real-time cement ratio, real-time water ratio and real-time chemical admixture ratio based on the first compressive resistance reference domain, the second compressive resistance reference domain and the third compressive resistance reference domain to optimize the real-time compressive strength, and stir the rice husk ash, cement, water and chemical admixture with adjusted ratios to obtain a rice husk ash cement-based material.
[0043] The embodiments of the present specification also disclose a computer-readable storage medium, wherein the storage medium stores computer instructions. When a computer reads the computer instructions, the computer executes any one of the above-described methods for preparing the rice husk ash cement-based material.
[0044] The embodiments of this specification can at least achieve the following beneficial effects:
[0045] By obtaining the compressive strength, rice husk ash ratio, cement ratio, water ratio and chemical admixture ratio, and then performing surface fitting operations respectively, the first compressive reference domain, the second compressive reference domain and the third compressive reference domain are obtained respectively. Finally, based on the first compressive reference domain, the second compressive reference domain and the third compressive reference domain, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength. The rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain the rice husk ash cement-based material. The compressive strength is optimized from multiple perspectives, and the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted with the goal of optimizing the compressive strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0047] Figure 1 It is a schematic diagram of the preparation method of the rice husk ash cement-based material involved in the present invention.
[0048] Figure 2 It is a schematic diagram of the final setting time test results involved in the present invention.
[0049] Figure 3 It is a schematic diagram of the chemical shrinkage test results involved in the present invention.
[0050] Figure 4 It is a schematic diagram of the relative humidity test results involved in the present invention.
[0051] Figure 5 It is a schematic diagram of the compressive strength test results involved in the present invention.
[0052] Figure 6 It is a schematic diagram of the autogenous shrinkage test results involved in the present invention. DETAILED DESCRIPTION
[0053] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the embodiments of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0054] The disclosure below provides many different embodiments or examples to implement different structures of the embodiments of the present invention. In order to simplify the disclosure of the embodiments of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the embodiments of the present invention. In addition, the embodiments of the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.
[0055] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0056] like Figure 1 As shown, the present specification discloses a method for preparing a rice husk ash cement-based material, comprising:
[0057] Obtain compressive strength, rice husk ash ratio, cement ratio, water ratio and chemical admixture ratio;
[0058] The cement ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a first matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and a cement ratio surface fitting equation are obtained, and the three-dimensional surface is recorded as a first compressive reference domain;
[0059] The water ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a second matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and a water ratio surface fitting equation are obtained, and the three-dimensional surface is recorded as a second compressive reference domain;
[0060] The chemical admixture ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a third matrix is formed, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and a chemical admixture ratio surface fitting equation, and the three-dimensional surface is recorded as a third compressive reference domain;
[0061] Based on the first compressive resistance reference domain, the second compressive resistance reference domain and the third compressive resistance reference domain, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
[0062] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0063] Get temperature and humidity;
[0064] The temperature and humidity are used as row vectors, and the rice husk ash ratio is used as a column vector to form a fourth matrix, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and a temperature and humidity surface fitting equation, and the three-dimensional surface is recorded as a fourth compressive reference domain;
[0065] Based on the first compressive reference domain, the second compressive reference domain, the third compressive reference domain and the fourth compressive reference domain, the real-time temperature and humidity, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength. The rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred at the adjusted real-time temperature and humidity to obtain the rice husk ash cement-based material.
[0066] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0067] Get the aggregate ratio;
[0068] The aggregate ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a fifth matrix is formed, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and an aggregate ratio surface fitting equation, and the three-dimensional surface is recorded as a fifth compressive reference domain;
[0069] Based on the first compressive reference domain, the second compressive reference domain, the third compressive reference domain and the fifth compressive reference domain, the real-time aggregate ratio, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the aggregate, rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a cement-based material.
[0070] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0071] Obtain fly ash ratio;
[0072] The fly ash ratio is used as a row vector, and the rice husk ash ratio is used as a column vector to form a sixth matrix, and then the compressive strength is imported, and a surface fitting operation is performed to obtain a three-dimensional surface and a fly ash ratio surface fitting equation, and the three-dimensional surface is recorded as a sixth compressive reference domain;
[0073] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the sixth compressive resistance reference domain, the real-time fly ash ratio, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the fly ash, rice husk ash, cement, water and chemical admixtures with adjusted ratios are stirred to obtain rice husk ash cement-based material.
[0074] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0075] Get aggregate gradation;
[0076] The aggregate gradation is used as a row vector, the rice husk ash ratio is used as a column vector, a seventh matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and an aggregate gradation surface fitting equation are obtained, and the three-dimensional surface is recorded as the seventh compressive reference domain;
[0077] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the seventh compressive resistance reference domain, the real-time aggregate gradation, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the aggregate gradation, rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
[0078] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0079] Obtain the mud content of aggregate;
[0080] The aggregate mud content is used as a row vector, and the rice husk ash ratio is used as a column vector to form an eighth matrix, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and an aggregate mud content surface fitting equation, and the three-dimensional surface is recorded as the eighth compressive reference domain;
[0081] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the eighth compressive resistance reference domain, the real-time aggregate mud content, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the adjusted aggregate mud content and the adjusted ratios of rice husk ash, cement, water and chemical admixture are stirred to obtain a rice husk ash cement-based material.
[0082] In some embodiments of this specification, the method for preparing the rice husk ash cement-based material further comprises:
[0083] Obtain flexural strength;
[0084] The flexural strength is used as a row vector, and the rice husk ash ratio is used as a column vector to form a ninth matrix, and then the compressive strength is imported, and a surface fitting operation is performed to obtain a three-dimensional surface and a flexural strength surface fitting equation, and the three-dimensional surface is recorded as a ninth compressive reference domain;
[0085] Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the ninth compressive resistance reference domain, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to maximize the real-time compression ratio, and the rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
[0086] In practice, before surface fitting, the matrix can be preprocessed to remove NaN values or 0 values, and then the rice husk ash ratio can be imported to perform the surface fitting operation.
[0087] It can be understood that the above embodiments can be used in combination accordingly, that is, the present invention comprehensively considers the influence of rice husk ash ratio, cement ratio, water ratio, chemical admixture ratio, temperature and humidity, aggregate ratio, fly ash ratio, aggregate gradation, aggregate mud content and flexural strength on compressive strength, that is, based on the first compressive reference domain, the second compressive reference domain, the third compressive reference domain, the fourth compressive reference domain, the fifth compressive reference domain, the sixth compressive reference domain, the seventh compressive reference domain, the eighth compressive reference domain and the ninth compressive reference domain, adjust the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio, the real-time chemical admixture ratio, the real-time temperature and humidity, the real-time aggregate ratio, the real-time fly ash ratio, the real-time aggregate gradation, the real-time aggregate mud content and the real-time flexural strength to make the real-time compressive strength (in other embodiments, after obtaining the matrix, the folding-compression ratio (that is, the compressive strength is replaced by the folding-compression ratio) is introduced for surface fitting, with the folding-compression ratio as the goal) optimal, and the combination of all embodiments is as follows (can be selectively combined and applied in practice):
[0088] In this embodiment, the real-time cement ratio is substituted into the cement ratio surface fitting equation to obtain a target value. If the target value is greater than 0, the first rice husk ash ratio corresponding to the real-time cement ratio is obtained based on the first compressive resistance reference domain.
[0089] Substituting the real-time water ratio into the water ratio surface fitting equation to obtain a target value, and if the target value is greater than 0, obtaining a second rice husk ash ratio corresponding to the real-time water ratio based on a second compressive resistance reference domain;
[0090] Substituting the real-time chemical admixture ratio into the chemical admixture ratio surface fitting equation to obtain a target value, and if the target value is greater than 0, obtaining a third rice husk ash ratio corresponding to the real-time chemical admixture ratio based on the third compressive resistance reference domain;
[0091] Substituting the real-time temperature and humidity ratio into the temperature and humidity surface fitting equation to obtain a target value, and if the target value is greater than 0, obtaining a fourth rice husk ash ratio corresponding to the real-time temperature and humidity based on the fourth compressive resistance reference domain;
[0092] Substituting the real-time aggregate ratio into the aggregate ratio surface fitting equation to obtain a target value, and if the target value is greater than 0, obtaining the fifth rice husk ash ratio corresponding to the real-time aggregate ratio based on the fifth compressive resistance reference domain;
[0093] Substituting the real-time fly ash ratio into the fly ash ratio surface fitting equation to obtain a target value, and if the target value is greater than 0, obtaining a sixth rice husk ash ratio corresponding to the real-time fly ash ratio based on the sixth compressive resistance reference domain;
[0094] Substitute the real-time aggregate gradation into the aggregate gradation surface fitting equation to obtain the target value. If the target value is greater than 0, then based on the seventh compressive resistance reference domain, obtain the seventh rice husk ash ratio corresponding to the real-time aggregate gradation;
[0095] Substitute the real-time aggregate mud content into the aggregate mud content surface fitting equation to obtain the target value. If the target value is greater than 0, then based on the eighth compressive resistance reference domain, obtain the eighth rice husk ash ratio corresponding to the real-time aggregate mud content;
[0096] Substitute the real-time flexural strength into the flexural strength surface fitting equation to obtain a target value. If the target value is greater than 0, then based on the ninth compressive resistance reference domain, obtain a ninth rice husk ash ratio corresponding to the real-time flexural strength.
[0097] The real-time rice husk ash ratio is compared with the average of the first rice husk ash ratio, the second rice husk ash ratio, the third rice husk ash ratio, the fourth rice husk ash ratio, the fifth rice husk ash ratio, the sixth rice husk ash ratio, the seventh rice husk ash ratio, the eighth rice husk ash ratio and the ninth rice husk ash ratio;
[0098] If they are equal (an error is allowed during comparison, and the error can be set according to actual conditions, such as the error can be the minimum difference greater than 0 among the first rice husk ash ratio, the second rice husk ash ratio, the third rice husk ash ratio, the fourth rice husk ash ratio, the fifth rice husk ash ratio, the sixth rice husk ash ratio, the seventh rice husk ash ratio, the eighth rice husk ash ratio and the ninth rice husk ash ratio), the real-time rice husk ash ratio is used as the benchmark (that is, the rice husk ash ratio is not adjusted), based on the first pressure resistance reference domain, the second pressure resistance reference domain, the third pressure resistance reference domain, the fourth pressure resistance reference domain, the fifth rice husk ash ratio, the sixth rice husk ash ratio, the seventh rice husk ash ratio, the eighth rice husk ash ratio and the ninth rice husk ash ratio the first compression reference domain, the second compression reference domain, the third compression reference domain, the fourth compression reference domain, the fifth compression reference domain, the sixth compression reference domain, the seventh compression reference domain, the eighth compression reference domain and the ninth compression reference domain, respectively adjusting the real-time cement ratio, the real-time water ratio, the real-time chemical admixture ratio, the real-time temperature and humidity, the real-time aggregate ratio, the real-time fly ash ratio, the real-time aggregate gradation and the real-time aggregate mud content to the cement ratio, water ratio, chemical admixture ratio, temperature and humidity, aggregate ratio, fly ash ratio, aggregate gradation and aggregate mud content corresponding to the real-time rice husk ash ratio;
[0099] If they are not equal, the real-time rice husk ash ratio is adjusted to the average of the nine ratios, namely, the first rice husk ash ratio, the second rice husk ash ratio, the third rice husk ash ratio, the fourth rice husk ash ratio, the fifth rice husk ash ratio, the sixth rice husk ash ratio, the seventh rice husk ash ratio, the eighth rice husk ash ratio and the ninth rice husk ash ratio, based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain, the fourth compressive resistance reference domain, the fifth compressive resistance reference domain, the sixth compressive resistance reference domain, the seventh compressive resistance reference domain, the eighth compressive resistance reference domain and the ninth compressive resistance reference domain, and the real-time cement ratio, real-time water ratio, real-time chemical admixture ratio, real-time temperature and humidity, real-time aggregate ratio, real-time fly ash ratio, real-time aggregate gradation and real-time aggregate mud content are respectively adjusted to the cement ratio, water ratio, chemical admixture ratio, temperature and humidity, aggregate ratio, fly ash ratio, aggregate gradation and aggregate mud content corresponding to the average of the nine ratios (rice husk ash ratio).
[0100] It is clear that the relevant adjustments of rice husk ash ratio, cement ratio, water ratio, chemical admixture ratio, temperature and humidity, aggregate ratio, fly ash ratio, aggregate grading and aggregate mud content are prior art, and the present invention does not improve them, and specific reference may be made to the prior art.
[0101] The starting point for the present invention to use rice husk ash as internal curing material is as follows:
[0102] Rice husk ash (RHA) has received increasing attention due to its potential for internal curing. When rice husks are completely incinerated, the residue is called rice husk ash. 90%-96% of the components in rice husk ash are amorphous silica. Rice husk ash powder is a porous structure, and the pore volume of rice husk ash is larger than that of most volcanic ash materials with similar particle sizes. Due to its high porosity and large liquid absorption and release capacity, rice husk ash can be an effective internal curing material, thereby reducing the shrinkage of UHPC and reducing the risk of cracking.
[0103] As the amount of rice husk ash increases, the final setting time decreases sharply, and the final setting time reflects the stiffness of the cementitious material. Rice husk ash has a strong ability to absorb liquid, and there is less free water in the rice husk ash cement-based material, resulting in a shorter distance between unhydrated cement particles, so the cement-based material mixed with rice husk ash has stronger stiffness.
[0104] The content of cementitious materials in rice husk ash cement-based materials is low, so the addition of rice husk ash will produce a dilution effect. There is less silicate cement available for hydration in rice husk ash cement-based materials, so the chemical shrinkage of cement-based materials mixed with rice husk ash is smaller.
[0105] Rice husk ash particles will quickly absorb the liquid within a few minutes, and the mass ratio of absorbed liquid to rice husk ash is about 0.6. Rice husk ash has a strong ability to absorb and release liquid. Saturated rice husk ash will release water during the hydration process to replenish the moisture inside the cement-based material. The water released by rice husk ash will alleviate the self-drying caused by the hydration reaction and keep the relative humidity at a high level.
[0106] The compressive strength of cement-based materials increases with the increase of rice husk ash content. On the one hand, the volcanic ash reaction of rice husk ash produces more calcium silicate hydrate, which plays an important role in the compressive strength of cementitious materials. On the other hand, the presence of rice husk ash accelerates the growth of calcium aluminate, which is also conducive to the increase of compressive strength. In addition to the above reasons, the liquid absorption capacity of rice husk ash also helps to improve the compressive strength. The rice husk ash particles added to the cement-based materials will absorb water. Because there is less free water in the rice husk ash cement-based materials, the porosity of the rice husk ash cement-based materials is lower. The skeleton structure of the rice husk ash cement-based materials with low porosity is denser and the compressive strength is higher.
[0107] There may be two main reasons for the mitigation of the autogenous shrinkage of cement-based materials by rice husk ash. First, due to the internal curing effect of rice husk ash, the autogenous drying of hydrated cement-based materials is alleviated. Free water is consumed during the hydration process, resulting in a decrease in the internal relative humidity (RH) of the cement-based material. Rice husk ash cement-based materials can release the water adsorbed on rice husk ash particles into the cement-based material, keeping the relative humidity at a high level and mitigating the autogenous shrinkage caused by autogenous drying. Secondly, the addition of rice husk ash improves the mechanical properties of cement-based materials. At the same age, the addition of rice husk ash will increase the compressive strength of cement-based materials, and at the same time, it will also increase the stiffness of cement-based materials. Stiffness reflects the resistance of the material to deformation. Under the same internal driving force, the greater the stiffness of the cement-based material, the smaller the autogenous shrinkage. Rice husk ash has a significant mitigation effect on the autogenous shrinkage of cement-based materials.
[0108] If rice husks are left alone, a series of environmental problems will arise. The present invention incorporates solid waste rice husk ash into the production of ultra-high performance concrete, which effectively reduces cracking caused by self-shrinkage while reducing the burden of rice husk ash solid waste on the environment and the cost of treatment, providing a new idea for the treatment of rice husk ash, and has good economic and social benefits.
[0109] The comparative effect experiment is as follows:
[0110] Experimental Example 1: The cement-based material without rice husk ash was prepared according to the weight ratio of 100% of 52.5 grade ordinary Portland cement and 0.016% of Glenium 51 polycarboxylate water reducer. Water was added according to 25% of the total weight of the cementitious material. The cement-based material was mixed using a 5L ring Hobart mixer and stirred for 3 minutes. The desired product was obtained. The performance test results are shown in Figures 2 to 6 .
[0111] Experimental Example 2: Cement-based materials mixed with rice husk ash were prepared according to the weight ratio of 90% of 52.5 grade ordinary Portland cement, 10% of rice husk ash, and 0.016% of Glenium 51 polycarboxylate water reducer. Water was added according to 25% of the total weight of the cementitious material. The cement-based materials were mixed using a 5L ring Hobart mixer and stirred for 3 minutes. The desired product was obtained. The performance test results are shown in Figures 2 to 6 .
[0112] Experimental Example 3: Cement-based materials mixed with rice husk ash were prepared according to the weight ratio of 80% of 52.5 grade ordinary Portland cement, 20% of rice husk ash, and 0.016% of Glenium 51 polycarboxylate water reducer. Water was added according to 25% of the total weight of the cementitious material. The cement-based materials were mixed using a 5L ring Hobart mixer and stirred for 3 minutes. The desired product was obtained. The performance test results are shown in Figures 2 to 6 .
[0113] The embodiments of the present specification also disclose a rice husk ash cement-based material, which is prepared by any of the above-mentioned methods for preparing a rice husk ash cement-based material.
[0114] It can be understood that chemical admixtures include retarders, water reducers, early strength agents, air entraining agents, thickeners and waterproofing agents, etc. The optimal proportional relationship between different chemical admixtures can be determined by referring to the above-mentioned surface fitting operation, that is, different chemical admixtures are used as row vectors, and rice husk ash ratios are used as column vectors to form a matrix, and then the compressive strength or compression ratio is introduced, and the surface fitting operation is performed to obtain the corresponding three-dimensional surface and surface fitting equation, and the three-dimensional surface is recorded as the compressive reference domain; the real-time different chemical admixture ratios are substituted into the corresponding surface fitting equations to obtain different rice husk ash ratios, and the real-time rice husk ash ratio is compared with the mean between different rice husk ash ratios. If they are equal, the real-time rice husk ash ratio is used as a benchmark, and the ratio between different chemical admixtures is adjusted based on the corresponding compressive reference domain. If they are not equal, the mean between different rice husk ash ratios is used as a benchmark, and the real-time rice husk ash ratio is adjusted to the mean between different rice husk ash ratios, and the ratio between different chemical admixtures is adjusted based on the corresponding compressive reference domain.
[0115] The prepared rice husk ash cement-based material can be cement paste, cement mortar and concrete. For example, cement paste is made without using aggregate, cement mortar is made with aggregate (sand), and concrete is made with aggregate (sand+stone).
[0116] The present specification also discloses a system for preparing a rice husk ash cement-based material, which is used to implement the method for preparing a rice husk ash cement-based material as described above;
[0117] The preparation system of the rice husk ash cement-based material comprises:
[0118] an acquisition module for acquiring compressive strength, rice husk ash ratio, cement ratio, water ratio and chemical admixture ratio;
[0119] A first fitting module is used to use the cement ratio as a row vector and the rice husk ash ratio as a column vector to form a first matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a cement ratio surface fitting equation, and record the three-dimensional surface as a first compressive reference domain;
[0120] A second fitting module is used to use the water ratio as a row vector and the rice husk ash ratio as a column vector to form a second matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a water ratio surface fitting equation, and record the three-dimensional surface as a second compressive reference domain;
[0121] A third fitting module is used to use the chemical admixture ratio as a row vector and the rice husk ash ratio as a column vector to form a third matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a chemical admixture ratio surface fitting equation, and record the three-dimensional surface as a third compressive reference domain;
[0122] A preparation module is used to adjust the real-time rice husk ash ratio, real-time cement ratio, real-time water ratio and real-time chemical admixture ratio based on the first compressive resistance reference domain, the second compressive resistance reference domain and the third compressive resistance reference domain to optimize the real-time compressive strength, and stir the rice husk ash, cement, water and chemical admixture with adjusted ratios to obtain a rice husk ash cement-based material.
[0123] It can be understood that, when combined with the corresponding embodiments, the fitting module can be increased accordingly, and the functional uses of the acquisition module and the preparation module can also be increased accordingly, which will not be repeated here.
[0124] It should be understood that the above-mentioned surface fitting operation can adopt existing software tools, such as Curve Fitting tool in Matlab. Each module can be a data reading module of an existing data detection (collection) / measurement device / sensor or simulation system.
[0125] It is clear that by obtaining corresponding data in advance through existing equipment, a large amount of test data can be obtained. These test data can be used to prepare experimental data for simulation in the laboratory, or can be used to prepare data for actual measurement in practice.
[0126] The embodiments of the present specification also disclose a computer-readable storage medium, wherein the storage medium stores computer instructions. When a computer reads the computer instructions, the computer executes any one of the above-described methods for preparing the rice husk ash cement-based material.
[0127] The above-described embodiments are used to illustrate the present invention, not to limit the present invention, so changes in the exemplified values or replacement of equivalent elements should still fall within the scope of the present invention.
[0128] From the above detailed description, it can be understood by those skilled in the art that the present invention can indeed achieve the aforementioned objectives and is in compliance with the provisions of the Patent Law.
[0129] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concepts. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
[0130] It should be noted that the above description of the relevant process is only for example and explanation, and does not limit the scope of application of this specification. For those skilled in the art, various modifications and changes can be made to the process under the guidance of this specification. However, these modifications and changes are still within the scope of this specification.
[0131] The basic concepts have been described above. Obviously, for those of ordinary skill in the art who have read this application, the above invention disclosure is only for example and does not constitute a limitation of this application. Although not explicitly stated here, those of ordinary skill in the art may make various modifications, improvements and amendments to this application. Such modifications, improvements and amendments are suggested in this application, so such modifications, improvements and amendments still belong to the spirit and scope of the exemplary embodiments of this application.
[0132] At the same time, the present application uses specific words to describe the embodiments of the present application. For example, "one embodiment", "an embodiment", and / or "some embodiments" refer to a certain feature, structure or characteristic related to at least one embodiment of the present application. Therefore, it should be emphasized and noted that "one embodiment" or "an embodiment" or "an alternative embodiment" mentioned twice or more in different positions in this specification does not necessarily refer to the same embodiment. In addition, some features, structures or characteristics in one or more embodiments of the present application can be appropriately combined.
[0133] In addition, it will be appreciated by those skilled in the art that various aspects of the present application may be illustrated and described by a number of patentable categories or situations, including any new and useful combination of processes, machines, products or substances, or any new and useful improvements thereto. Therefore, various aspects of the present application may be implemented entirely by hardware, entirely by software (including firmware, resident software, microcode, etc.), or by a combination of hardware and software. The above hardware or software may all be referred to as "units", "modules" or "systems". In addition, various aspects of the present application may take the form of a computer program product embodied in one or more computer-readable media, wherein computer-readable program code is contained therein.
[0134] The computer program code required for the operation of each part of the application can be written in any one or more programming languages, including object-oriented programming languages such as Java, Scale, Smalltalk, Elffell, JADE, Emerald, C++, C#, VB.NET, Python, etc., such as C programming language, Visual Basic, Fortran2103, Perl, COBOL2102, PHP, ABAP, such as Python, Ruby and Groovy dynamic programming language or other programming languages. The program code can be run completely on the user's computer, or run on the user's computer as an independent software package, or partly run on the user's computer and partly run on the remote computer, or run completely on the remote computer or server. In the latter case, the remote computer can be connected to the user's computer by any network form, such as local area network (LAN) or wide area network (WAN), or be connected to an external computer (such as by the Internet), or in a cloud computing environment, or as a service, such as software as a service (SaaS).
[0135] In addition, unless explicitly stated in the claims, the order of the processing elements and sequences described in this application, the use of alphanumeric characters, or the use of other names are not intended to limit the order of the processes and methods of this application. Although the above disclosure discusses some invention embodiments that are currently considered useful through various examples, it should be understood that such details are only for illustrative purposes, and the attached claims are not limited to the disclosed embodiments. On the contrary, the claims are intended to cover all modifications and equivalent combinations that are consistent with the essence and scope of the embodiments of this application. For example, although the implementation of the various components described above can be embodied in a hardware device, it can also be implemented as a pure software solution, for example, installation on an existing server or mobile device.
[0136] Similarly, it should be noted that in order to simplify the description disclosed in this application and thus help understand one or more embodiments of the invention, in the above description of the embodiments of the application, multiple features are sometimes combined into one embodiment, figure or description thereof. However, this method of the application should not be interpreted as reflecting the intention that the claimed object requires more features than those explicitly stated in each claim. On the contrary, the subject of the invention should have fewer features than the above single embodiment.
Claims
1. A method for preparing a rice husk ash cement-based material, characterized in that: include: Obtain compressive strength, rice husk ash ratio, cement ratio, water ratio and chemical admixture ratio; The cement ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a first matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and a cement ratio surface fitting equation are obtained, and the three-dimensional surface is recorded as a first compressive reference domain; The water ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a second matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and a water ratio surface fitting equation are obtained, and the three-dimensional surface is recorded as a second compressive reference domain; The chemical admixture ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a third matrix is formed, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and a chemical admixture ratio surface fitting equation, and the three-dimensional surface is recorded as a third compressive reference domain; Based on the first compressive resistance reference domain, the second compressive resistance reference domain and the third compressive resistance reference domain, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
2. The method for preparing the rice husk ash cement-based material according to claim 1, characterized in that: Also includes: Get temperature and humidity; The temperature and humidity are used as row vectors, and the rice husk ash ratio is used as a column vector to form a fourth matrix, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and a temperature and humidity surface fitting equation, and the three-dimensional surface is recorded as a fourth compressive reference domain; Based on the first compressive reference domain, the second compressive reference domain, the third compressive reference domain and the fourth compressive reference domain, the real-time temperature and humidity, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength. The rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred at the adjusted real-time temperature and humidity to obtain the rice husk ash cement-based material.
3. The method for preparing the rice husk ash cement-based material according to claim 1, characterized in that: Also includes: Get the aggregate ratio; The aggregate ratio is used as a row vector, the rice husk ash ratio is used as a column vector, a fifth matrix is formed, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and an aggregate ratio surface fitting equation, and the three-dimensional surface is recorded as a fifth compressive reference domain; Based on the first compressive reference domain, the second compressive reference domain, the third compressive reference domain and the fifth compressive reference domain, the real-time aggregate ratio, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the aggregate, rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a cement-based material.
4. The method for preparing the rice husk ash cement-based material according to claim 1, characterized in that: Also includes: Obtain fly ash ratio; The fly ash ratio is used as a row vector, and the rice husk ash ratio is used as a column vector to form a sixth matrix, and then the compressive strength is imported, and a surface fitting operation is performed to obtain a three-dimensional surface and a fly ash ratio surface fitting equation, and the three-dimensional surface is recorded as a sixth compressive reference domain; Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the sixth compressive resistance reference domain, the real-time fly ash ratio, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the fly ash, rice husk ash, cement, water and chemical admixtures with adjusted ratios are stirred to obtain rice husk ash cement-based material.
5. The method for preparing rice husk ash cement-based material according to claim 1, characterized in that: Also includes: Get aggregate gradation; The aggregate gradation is used as a row vector, the rice husk ash ratio is used as a column vector, a seventh matrix is formed, and then the compressive strength is introduced, a surface fitting operation is performed, a three-dimensional surface and an aggregate gradation surface fitting equation are obtained, and the three-dimensional surface is recorded as the seventh compressive reference domain; Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the seventh compressive resistance reference domain, the real-time aggregate gradation, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the aggregate gradation, rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
6. The method for preparing rice husk ash cement-based material according to claim 1, characterized in that: Also includes: Obtain the mud content of aggregate; The aggregate mud content is used as a row vector, and the rice husk ash ratio is used as a column vector to form an eighth matrix, and then the compressive strength is introduced, and a surface fitting operation is performed to obtain a three-dimensional surface and an aggregate mud content surface fitting equation, and the three-dimensional surface is recorded as the eighth compressive reference domain; Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the eighth compressive resistance reference domain, the real-time aggregate mud content, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to optimize the real-time compressive strength, and the adjusted aggregate mud content and the adjusted ratios of rice husk ash, cement, water and chemical admixture are stirred to obtain a rice husk ash cement-based material.
7. The method for preparing the rice husk ash cement-based material according to any one of claims 1 to 6, characterized in that: Also includes: Obtain flexural strength; The flexural strength is used as a row vector, and the rice husk ash ratio is used as a column vector to form a ninth matrix, and then the compressive strength is imported, and a surface fitting operation is performed to obtain a three-dimensional surface and a flexural strength surface fitting equation, and the three-dimensional surface is recorded as a ninth compressive reference domain; Based on the first compressive resistance reference domain, the second compressive resistance reference domain, the third compressive resistance reference domain and the ninth compressive resistance reference domain, the real-time rice husk ash ratio, the real-time cement ratio, the real-time water ratio and the real-time chemical admixture ratio are adjusted to maximize the real-time compression ratio, and the rice husk ash, cement, water and chemical admixture with adjusted ratios are stirred to obtain a rice husk ash cement-based material.
8. A rice husk ash cement-based material, characterized in that: The rice husk ash cement-based material is prepared by the method for preparing the rice husk ash cement-based material according to any one of claims 1 to 7.
9. A system for preparing rice husk ash cement-based materials, characterized in that: A method for preparing the rice husk ash cement-based material according to any one of claims 1 to 7; The preparation system of the rice husk ash cement-based material comprises: an acquisition module for acquiring compressive strength, rice husk ash ratio, cement ratio, water ratio and chemical admixture ratio; A first fitting module is used to use the cement ratio as a row vector and the rice husk ash ratio as a column vector to form a first matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a cement ratio surface fitting equation, and record the three-dimensional surface as a first compressive reference domain; A second fitting module is used to use the water ratio as a row vector and the rice husk ash ratio as a column vector to form a second matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a water ratio surface fitting equation, and record the three-dimensional surface as a second compressive reference domain; A third fitting module is used to use the chemical admixture ratio as a row vector and the rice husk ash ratio as a column vector to form a third matrix, then import the compressive strength, perform a surface fitting operation, obtain a three-dimensional surface and a chemical admixture ratio surface fitting equation, and record the three-dimensional surface as a third compressive reference domain; A preparation module is used to adjust the real-time rice husk ash ratio, real-time cement ratio, real-time water ratio and real-time chemical admixture ratio based on the first compressive resistance reference domain, the second compressive resistance reference domain and the third compressive resistance reference domain to optimize the real-time compressive strength, and stir the rice husk ash, cement, water and chemical admixture with adjusted ratios to obtain a rice husk ash cement-based material.
10. A computer-readable storage medium, characterized in that: The storage medium stores computer instructions, and when a computer reads the computer instructions, the computer executes the method for preparing the rice husk ash cement-based material according to any one of claims 1 to 7.