A method for comprehensively recovering copper, gold and silver from low-grade copper-sulfur ore
Patent Information
- Application Number
- CN202410274101.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2026-11-03
- Estimated Expiration
- 2044-03-11
AI Technical Summary
现有技术在回收低品位铜硫矿石中的铜、金、银时,抑制黄铁矿的难度大,导致伴生金、银回收率低,且常用石灰抑制方法影响铜、金、银的回收效果。
A combination of inhibitors (sodium polycarboxylated xanthate, sodium humate, sodium bicarbonate) and collectors (sodium decaalkyl ether sulfate, ethyl thiocyanate, polyaluminum chloride) were used for flotation under low pH conditions. A specific flotation process was used to improve the recovery rate of copper, gold and silver and reduce the difficulty of inhibiting pyrite.
The system achieved efficient recovery of copper, gold, and silver under low pH conditions, improved the recovery rate of copper concentrate and associated gold and silver, reduced the floatability of pyrite, reduced the impact of slime, and simplified the flotation process.
Smart Images

Figure CN118253408B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of copper mineral recovery technology, and in particular to a method for the comprehensive recovery of copper, gold and silver from low-grade copper-sulfur ore. Technical Background
[0002] Copper sulfide minerals are classified into primary copper deposits and secondary copper deposits, which often coexist in open-pit mines. Primary copper sulfide deposits primarily contain chalcopyrite and a small amount of bornite, mainly in the form of disseminated veinlets. Non-primary deposits mainly contain chalcocite, a small amount of cuprite, and native copper. The ore primarily exhibits a porphyritic or porphyritic texture, with a predominantly massive structure and a very small amount of brecciated structure. The main sulfides in the ore are chalcopyrite and pyrite, and the main recoverable elements are copper and some associated gold and silver. In copper-sulfur deposits containing associated gold and silver, the gold and silver are embedded in smaller grains, mainly in the form of fine grains encased within chalcopyrite, pyrite, and gangue minerals.
[0003] For copper-sulfur ores, suppressing pyrite is an unavoidable problem during the recovery process. When the ore contains secondary copper, copper ions in the slurry will activate pyrite and further increase the difficulty of suppressing it. Currently, the most common suppression method is to add a large amount of lime during the beneficiation process. However, since gold and silver minerals are quite sensitive to lime, this method will inevitably affect the recovery of associated gold and silver.
[0004] Therefore, developing suitable beneficiation methods for this type of ore to achieve efficient recovery of associated gold and silver during copper ore recovery is a technical problem that needs to be solved. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a method for the comprehensive recovery of copper, gold, and silver from low-grade copper-sulfur ore.
[0006] The present invention adopts the following technical solution:
[0007] A method for the comprehensive recovery of copper, gold, and silver from low-grade copper-sulfur ore includes the following steps:
[0008] S1. Grinding: The raw ore is ground to produce a slurry with a mass concentration of 30%, and the grinding process is carried out at a rate of 200g / t. 原矿 Add a combination inhibitor, wherein the combination inhibitor is obtained by mixing sodium polycarboxyxanthate, sodium humate and sodium bicarbonate in a mass ratio of 2:1:1;
[0009] S2. Mixed Flotation: The pulp prepared in S1 is mixed with the combined collector and subjected to two roughing flotations. The flotation froth from the two roughing flotations is collected and combined to obtain the rough concentrate. The combined collector is composed of sodium decaalkyl ether sulfate, ethyl thiocyanate, and polyaluminum chloride in a mass ratio of 1:1:1. The addition amount in the first roughing flotation is 20 g / t.原矿 The amount added in the second roughing process was 10g / t. 原矿 ;
[0010] S3. Fine Concentration: The rough concentrate is first regrinded, and then the rough concentrate slurry undergoes two stages of fine concentration flotation. The fine concentration flotation is carried out at a rate of 100g / t. 原矿 A combination of inhibitors is added, in which the flotation foam from the first stage of fine flotation is used as the input mineral for the second stage of fine flotation, and the flotation tailings from the second stage of fine flotation are returned to the first stage of fine flotation. The flotation foam collected from the second stage of fine flotation is the copper, gold and silver mixed concentrate.
[0011] In this invention, the obtained copper, gold, and silver mixed concentrate can be separated in the later stages using existing separation methods such as smelting.
[0012] Preferably, in step S1, the ore is ground until the particle size of the ore particles smaller than 200 mesh accounts for more than 60% of the total ore mass content.
[0013] Preferably, in step S3, the pH value of the second-stage fine flotation is 11-12.
[0014] Preferably, in step S2, the pH value of the pulp is controlled at 9-10 in the first roughing flotation, and the flotation tailings enter the second roughing flotation, where the pH value of the pulp is controlled at 10-11, and the flotation tailings, i.e., tailings 1, are discarded.
[0015] Preferably, in step S3, the regrinding process results in mineral particles with a diameter of less than 0.044 mm accounting for more than 80% of the total ore mass content.
[0016] Preferably, it also includes a fine scavenging step, which involves collecting the flotation tailings from the first-stage fine flotation in step S3, and mixing the flotation tailings with 3g / t 原矿 After the combined collectors are mixed and the slurry is prepared, it is sent to the flotation machine for fine scavenging. The flotation froth from the fine scavenging is returned to the regrinding operation in step S3, and the tailings from the fine scavenging, namely tailings 2, are discarded.
[0017] The beneficial effects of this invention are as follows:
[0018] This invention provides a comprehensive recovery method for associated gold and silver in primary and secondary open-pit copper-sulfur mines. Through a special combination of inhibitors and collectors, the recovery of copper, gold, and silver is achieved under low pH conditions.
[0019] 1) Collectors sodium decaalkyl ether sulfate, ethyl thiocyanate (Z-200), and polyaluminum chloride (PAC) are used in a 1:1:1 mass ratio. The main characteristic of sodium decaalkyl ether sulfate as a collector is that it does not collect pyrite. When used for flotation of copper- and iron-containing sulfide ores, it can significantly improve the separation effect between chalcopyrite and pyrite and their gangue. Z-200 has good selective collecting ability for copper under low-alkali conditions. PAC has good collecting effect on gold and silver and can significantly improve the recovery rate of associated gold and silver.
[0020] The collector combination provided by this invention produces a synergistic copper effect, enabling enhanced collection of copper, gold, and silver under low-alkali conditions, thereby improving the recovery rate of copper, gold, and silver. Furthermore, the combined collector has a weak collecting ability for pyrite, which can reduce the pressure on copper-sulfur separation in beneficiation operations. And because both Z-200 and PAC have weak foaming properties, no further foaming agent is needed after adding the combined collector.
[0021] 2) The combined inhibitor consists of sodium polycarboxylated xanthate, sodium humate, and sodium bicarbonate used in a mass ratio of 2:1:1. Sodium polycarboxylated xanthate reacts with the surface of pyrite to produce a hydrophilic film, thus inhibiting pyrite formation. Sodium humate reacts with metal ions on the surface of pyrite, eliminating the activation effect of metal ions on pyrite and reducing its floatability, thereby inhibiting pyrite formation. Sodium bicarbonate disperses the slime, reducing its impact on flotation. Simultaneously, as a strong base-weak acid salt, sodium bicarbonate helps adjust the pH of the pulp.
[0022] The main function of the combined inhibitor is to disperse the slime and eliminate the activation of pyrite by metal ions. It achieves the inhibition of pyrite under low pH conditions and has a slightly better effect on the collection of associated gold and silver.
[0023] 3) The middlings have a relatively high yield of coarse particles, a high copper content in the coarse particles, and a relatively high copper loss rate. In this invention, the middlings are returned to the regrinding and classification process and then subjected to two-stage cleaning flotation, which greatly improves the liberation effect of middlings monomers, significantly reduces the copper content in the coarse particles of middlings, and effectively improves the copper concentrate recovery rate. Attached Figure Description
[0024] Figure 1 The distribution characteristics of chalcopyrite in the ore in Example 1 of the present invention are shown in Figure A, where coarse-grained chalcopyrite is irregularly distributed in gangue minerals; Figure B shows fine-grained chalcopyrite is irregularly distributed in gangue minerals; Figure C shows chalcopyrite replacing pyrite; and Figure D shows chalcopyrite distributed in fine veins in pyrite fissures.
[0025] Figure 2 This is a schematic diagram of the mineral processing flow of the present invention;
[0026] Figure 3This is a schematic diagram of the mineral processing flow in the existing technology. Detailed Implementation
[0027] The technical solution of the present invention will be described in more detail below with reference to the embodiments.
[0028] Example 1
[0029] The primary copper minerals in a South American open-pit mine are mainly chalcopyrite and a small amount of bornite, mainly in the form of disseminated veinlets; the non-primary minerals are mainly chalcocite, a small amount of cuprite, native copper, etc.; the main sulfides in the ore are chalcopyrite and pyrite, and the main recoverable elements are copper and some associated gold and silver.
[0030] See Figure 1 Chalcopyrite is mainly distributed in gangue minerals as anhedral granular and granular aggregates. Some occur as fine grains, while others are distributed as veins. Chalcopyrite is sometimes found to coexist with pyrite, and a small amount is distributed as fine veins in pyrite fissures. Occasionally, chalcopyrite is found to coexist with minerals such as tetrahedrite, sphalerite, magnetite, and pyrrhotite.
[0031] The gold minerals in the ore are mainly native gold, followed by silver-gold minerals, with trace amounts of copper-gold minerals. Native gold is mainly distributed as inclusions in gangue minerals such as potassium feldspar, with a small amount encapsulated in pyrite. Its shape is mainly granular and rectangular. Some native gold is distributed between potassium feldspar and sodium feldspar grains, and between chalcopyrite and quartz grains; a small amount is also distributed in the fissures of quartz and potassium feldspar. The embedding characteristics of native gold are shown in Table 1.
[0032] Table 1. Dispersion characteristics of native gold in ore
[0033]
[0034] The silver minerals are mainly argentite, followed by argentite and native silver. Argentite is mainly distributed in granular, rectangular form between quartz and potassium feldspar grains, and sometimes between quartz and potassium feldspar, or chalcopyrite and calcium barium feldspar grains; secondly, some argentite is encased in gangue minerals such as potassium feldspar, quartz, and chlorite; occasionally, argentite is found in the fissures of potassium feldspar, sodium feldspar, and chalcopyrite. The intercalation characteristics of argentite are shown in Table 2.
[0035] Table 2. Dissemination characteristics of argentite in the ore
[0036]
[0037]
[0038] For recycling using the method of this invention, see [link to relevant documentation]. Figure 2 The process is as follows:
[0039] S1. Grinding: The raw ore is fed into a ball mill for grinding until the ore particles with a diameter less than 200 mesh account for more than 60% of the total ore mass, thus producing a slurry with a mass concentration of 30%. During the grinding process, the grinding concentration is 200g / t. 原矿 A combination inhibitor is added, wherein the combination inhibitor is obtained by mixing sodium polycarboxylated xanthate, sodium humate and sodium bicarbonate in a mass ratio of 2:1:1.
[0040] S2. Mixed flotation: The pulp prepared in S1 is mixed with the combined collector and subjected to two roughing flotations. The combined collector is composed of sodium decaalkyl ether sulfate, ethyl thiocyanate, and polyaluminum chloride in a mass ratio of 1:1:1.
[0041] 1) Coarse selection I, add 20g / t 原矿 The combined collector, under pH 9.5 conditions, is stirred for 5 minutes and then fed into the flotation machine for flotation. The flotation froth 1, i.e. the rough concentrate, enters the regrinding operation, and the flotation tailings enter the roughing II operation.
[0042] 2) For coarse selection II, add 10g / t 原矿 The combined collector is stirred for 10 minutes at a pH of 10.5 and then fed into the flotation machine for flotation. The flotation froth 2, i.e. the rough concentrate, enters the regrinding operation, and the flotation tailings 1 are discarded.
[0043] S3. Fine Concentration: Collect the flotation foam from step S2 and combine them to obtain rough concentrate. The rough concentrate is first regrinded and then classified by hydrocyclone. The hydrocyclone overflow (mineral particles with a diameter less than 0.044 mm account for more than 80% of the total ore mass content) enters the fine concentration operation, and the hydrocyclone underflow is returned to the regrinding operation.
[0044] The refining process includes two-stage refining flotation:
[0045] 1) Fine Selection 1: Add 100g / t to the flotation machine 原矿 The combined inhibitors inhibit the flotation of pyrite and chalcopyrite, with the flotation froth entering the second cleaning stage and the flotation tailings entering the scavenging stage.
[0046] 2) Selected 2: The flotation foam in Selected 2 is copper concentrate, which also contains recovered associated gold and silver. The flotation tailings are returned to Selected 1.
[0047] S4. Fine Scavenging Operation: Add 3g / t of tailings from the finest flotation stage 1. 原矿 The combined collector is stirred for 3 minutes and then fed into the flotation machine for fine scavenging. The flotation froth, i.e. middlings, is returned to the hydrocyclone for classification. The flotation tailings are tailings 2.
[0048] In the above process, different collectors and inhibitors were used individually, and the following mineral processing indicators were measured:
[0049] Table 3 Mineral processing indicators for different collectors used alone / %
[0050]
[0051] Table 4. Mineral processing indexes when different inhibitors are used alone / %
[0052]
[0053] The ore is recovered using conventional processes in existing technologies. (See process details below.) Figure 3 The measured mineral processing indicators and middlings particle size information are as follows:
[0054] Table 5. Existing technology mineral processing indicators / %
[0055]
[0056] Table 6 Mineral Processing Indicators of the Invention / %
[0057]
[0058] This beneficiation method improves the grade and recovery rate of copper concentrate, and significantly increases the recovery rates of Au and Ag compared to existing technologies.
[0059] Table 7. Grain size analysis results of middlings before modification / %
[0060]
[0061] Table 8. Particle size analysis results of minerals in this invention / %
[0062]
[0063] As can be seen from the table, this beneficiation method increases the content of fine-grained minerals, fully liberates minerals and avoids mud formation, while also improving the grade of Cu and S in the ore.
[0064] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for the comprehensive recovery of copper, gold, and silver from low-grade copper-sulfur ore, characterized in that, Includes the following steps: S1. Grinding: The raw ore is ground to produce a slurry with a mass concentration of 30%, and the grinding process is carried out at a rate of 200g / t. 原矿 Add a combination inhibitor, wherein the combination inhibitor is obtained by mixing sodium polycarboxyxanthate, sodium humate and sodium bicarbonate in a mass ratio of 2:1:1; S2. Mixed Flotation: The pulp prepared in S1 is mixed with the combined collector and subjected to two roughing flotations. The flotation froth from the two roughing flotations is collected and combined to obtain the rough concentrate. The combined collector is composed of sodium decaalkyl ether sulfate, ethyl thiocyanate, and polyaluminum chloride in a mass ratio of 1:1:
1. The addition amount in the first roughing flotation is 20 g / t. 原矿 The amount added in the second roughing process was 10g / t. 原矿 ; S3. Fine Concentration: The rough concentrate is first regrinded, and the regrinded concentrate slurry is then subjected to two stages of fine flotation. The first stage of fine flotation is carried out at a concentration of 100g / t. 原矿 By adding a combined inhibitor, the flotation foam from the first stage of fine flotation is used as the input mineral for the second stage of fine flotation, and the flotation tailings from the second stage of fine flotation are returned to the first stage of fine flotation. The flotation foam collected from the second stage of fine flotation is the copper, gold and silver mixed concentrate.
2. The method for comprehensively recovering copper, gold, and silver from low-grade copper-sulfur ore as described in claim 1, characterized in that, In step S1, the ore is ground until the particle size of the ore particles smaller than 200 mesh accounts for more than 60% of the total ore mass content.
3. The method for comprehensively recovering copper, gold, and silver from low-grade copper-sulfur ore as described in claim 1, characterized in that, In step S2, the pH value of the pulp is controlled at 9-10 in the first roughing flotation, and the flotation tailings enter the second roughing flotation. The pH value of the pulp is controlled at 10-11 in the second roughing flotation, and the flotation tailings, namely tailings 1, are discarded.
4. The method for comprehensively recovering copper, gold, and silver from low-grade copper-sulfur ore as described in claim 1, characterized in that, In step S3, the regrinding process is carried out until the mineral particles with a diameter of less than 0.044 mm account for more than 80% of the total ore mass content.
5. The method for comprehensively recovering copper, gold, and silver from low-grade copper-sulfur ore as described in claim 1, characterized in that, In step S3, the pH value of the second-stage fine flotation is 11-12.
6. The method for comprehensive recovery of copper, gold, and silver from low-grade copper-sulfur ore as described in claim 1, characterized in that, It also includes a fine scavenging step, which involves collecting the flotation tailings from the first-stage fine flotation in step S3, and mixing these tailings with 3g / t 原矿 After the combined collectors are mixed and the slurry is prepared, it is sent to the flotation machine for fine scavenging. The flotation froth from the fine scavenging is returned to the regrinding operation in step S3, and the tailings from the fine scavenging, namely tailings 2, are discarded.
Citation Information
Patent Citations
Mineral processing technology for recovering copper from copper-sulfur ore containing secondary copper sulfide ore
CN114749270A
Beneficiation method for recovering valuable metal from high-grade copper and sulfur symbiotic polymetallic ore
CN116510884A