Pole production system, slurry re-coating equipment and method

By using slurry re-coating equipment for machine vision inspection and mechanical re-coating in the production of electrode pads, the problem of active material layer defects is solved, the quality and production efficiency of the electrode pads are improved, and battery performance is ensured.

CN118357126BActive Publication Date: 2024-10-18CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410799783.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-18
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

The active material layer of the electrode plate is prone to defects such as leakage, scratches, and bubbles during the production process, which affects the performance of the electrode plate, leading to reduced battery performance and material waste.

Method used

Using slurry recoating equipment including a detection device and a recoating device, the defect information of the active material layer is obtained through machine vision inspection, and mechanical recoating is performed based on the defect information to ensure the integrity of the active material layer of the electrode pole piece.

Benefits of technology

It effectively alleviates the waste of materials and manpower, improves the yield rate and production efficiency of electrode pole pieces, and ensures the stability of battery performance and output power.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118357126B_ABST
    Figure CN118357126B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of battery technology, and specifically relates to a pole piece production system, and a slurry re-coating device and method. The slurry re-coating device includes a first detection device and a slurry re-coating device. The first detection device detects the active material layer of the electrode pole piece to obtain the slurry defect information of the active material layer, and the slurry re-coating device performs slurry re-coating on the slurry defective part of the active material layer according to the slurry defect information. The first detection device and the slurry re-coating device work together to achieve mechanical re-coating of the slurry defective part of the active material layer, so that the defective part of the active material layer can be filled with slurry, so that the electrode pole piece with slurry defect in the active material layer can be used normally, effectively alleviating the waste of materials and manpower; the slurry re-coating device can also be integrated into each process of the production process of the electrode pole piece, so as to improve the yield rate of the electrode pole piece and improve production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of battery technology, and in particular relates to a pole piece production system, and slurry re-coating equipment and method. Background Art

[0002] A battery is generally composed of multiple battery cells, and the electrode assembly of a battery cell is formed by winding or folding multiple electrode plates and separators. Therefore, the electrode plates are important components of the battery cell.

[0003] The electrode plate generally includes a current collector and an active material layer covering the surface of the current collector. Defects in the active material layer during the manufacturing process, such as missing coating, scratches, bubbles, etc., will directly affect the performance of the electrode plate, thereby affecting the normal use of the battery cell.

[0004] The above statements are only used to provide background information related to the present application and do not necessarily constitute prior art. Summary of the invention

[0005] The purpose of the embodiments of the present application is to provide an electrode production system, and slurry re-coating equipment and method, including but not limited to solving technical problems that affect the performance of electrode plates due to defects in the active material layer of the electrode plates, such as missing coating, scratches, bubbles, etc.

[0006] The technical solution adopted in the embodiment of the present application is:

[0007] In a first aspect, a slurry re-coating device is provided, comprising:

[0008] A first detection device is configured to perform image detection on the active material layer of the electrode plate through machine vision to obtain slurry defect information of the active material layer;

[0009] A slurry re-coating device, which is communicatively connected to the first detection device and is configured to re-coat the slurry defective part of the active material layer with slurry according to the slurry defective information;

[0010] Among them, the first detection device at least detects the thickness value of the slurry at the slurry defect site of the active material layer and the area value corresponding to the contour of the slurry defect site, and compares the thickness value and the area value with the preset thickness value and the area value one by one, and calculates the thickness difference and the area difference. The slurry defect information at least includes the thickness difference and the area difference. The slurry filling device at least locates the slurry defect site according to the thickness difference and the area difference, and fills the slurry defect site with slurry.

[0011] The slurry re-coating equipment of the embodiment of the present application includes a first detection device and a slurry re-coating device, wherein the first detection device is used to detect the active material layer of the electrode plate, so as to obtain slurry defect information of the active material layer, and the slurry re-coating device is communicatively connected to the first detection device, and is used to perform slurry re-coating on the slurry defective part of the active material layer according to the slurry defect information obtained by the first detection device. In this way, the first detection device and the slurry re-coating device work together to achieve mechanical re-coating of the slurry-deficient parts of the active material layer of the electrode plate, so that the defective parts of the active material layer can be filled with slurry, so that the electrode plate with slurry defects in the active material layer can be used normally, effectively alleviating the waste of materials and manpower; in addition, the slurry re-coating equipment for the active material layer can also be integrated into various processes of the production process of the electrode plate, and perform real-time dynamic detection and slurry re-coating on the electrode plates in various states processed in each process (such as large rolled electrode plates, single film area rolls obtained after pre-slitting, small rolled electrode plates obtained after die-cutting and slitting, etc.), thereby improving the yield rate of the electrode plates, and then improving the production efficiency of the electrode plates.

[0012] In some embodiments, the first detection device includes at least one of a camera detection device, a laser detection device, an infrared detection device, an X-ray detection device, and an ultrasonic detection device.

[0013] By adopting the technical solution of this embodiment, the active material layer of the electrode plate can be detected by using any one of a camera detection device, a laser detection device, an infrared detection device, an X-ray detection device and an ultrasonic detection device, thereby obtaining the slurry defect information of the active material layer.

[0014] In some embodiments, the first detection device is a CCD visual detector or a 3D profilometer.

[0015] By adopting the technical solution of this embodiment, the slurry defect information of the active material layer is obtained by visually inspecting the active material layer of the electrode plate using a CCD visual inspection instrument or a 3D profilometer.

[0016] In some embodiments, the slurry re-coating device includes a displacement drive mechanism and a slurry re-coating mechanism, both of which are communicatively connected to the first detection device. The displacement drive mechanism is drivably connected to the slurry re-coating mechanism to drive the slurry re-coating mechanism to move and perform slurry re-coating on the slurry-deficient area.

[0017] By adopting the technical solution of this embodiment, the displacement driving component drives the slurry re-coating mechanism to move according to the slurry defect information of the first detection device, and the slurry re-coating mechanism then re-coats the slurry defective part of the active material layer according to the slurry defect information.

[0018] In some embodiments, the slurry re-coating equipment also includes a slurry feeding device, the slurry re-coating mechanism includes a slurry delivery pump and a re-coating head installed at the outlet of the slurry delivery pump, the slurry delivery pump is configured to deliver the slurry from the slurry feeding device to the re-coating head, and the displacement drive mechanism is driven and connected to the re-coating head.

[0019] By adopting the technical solution of this embodiment, the slurry delivery pump delivers the slurry from the slurry feeding device to the re-coating head, and the displacement driving mechanism drives the re-coating head to move according to the slurry re-coating information to complete the slurry re-coating of the slurry defective part.

[0020] In some embodiments, the touch-up head includes at least one of an extrusion head and a spray head.

[0021] By adopting the technical solution of this embodiment, the slurry can be extruded and applied to the slurry defective part using an extrusion discharge head, or the slurry can be sprayed to the slurry defective part using a spray head, so that the slurry can be evenly applied.

[0022] In some embodiments, the slurry re-coating mechanism includes a 3D printer.

[0023] By adopting the technical solution of this embodiment, 3D printing technology is used for slurry re-coating, the slurry is transported to the material chamber of the 3D printer for containing printing materials, the first detection device is communicated with the 3D printer, and the 3D printer prints the slurry in the material chamber layer by layer to the slurry defective part according to the slurry defect information, thereby realizing automatic slurry re-coating of the slurry defective part.

[0024] In some embodiments, the slurry re-coating device further includes a feeding mechanism, which is configured to sequentially transport the electrode plates to be re-coated with slurry to the first detection device and the slurry re-coating device.

[0025] By adopting the technical solution of this embodiment, the feeding mechanism transports the electrode plate through the first detection device and the slurry re-coating device in sequence, and the collection of slurry defect information and slurry re-coating are carried out in an orderly manner, forming a streamlined operation, which helps to improve the slurry re-coating efficiency of the electrode plate.

[0026] In some embodiments, the slurry re-coating equipment further includes a drying mechanism, and the drying mechanism is configured to dry the electrode plate after the slurry is re-coated by the slurry re-coating device.

[0027] By adopting the technical solution of this embodiment, the electrode plate that has been re-coated with slurry is dried to obtain a dry electrode plate.

[0028] In some embodiments, the slurry re-coating equipment further includes a second detection device, which is configured to detect the active material layer of the electrode plate after being dried by the drying mechanism.

[0029] By adopting the technical solution of this embodiment, after the electrode plate is re-coated with slurry and dried, it is detected by the second detection device to determine whether there are still slurry defects in the active material layer of the electrode plate. If there are still slurry defects, the slurry re-coating device can continue to be used for slurry re-coating. If the second detection device detects that no slurry defects are found in the electrode plate, the material can be collected for processing.

[0030] In some embodiments, the first detection device and the second detection device have the same structure.

[0031] By adopting the technical solution of this embodiment, the electrode plates are inspected before and after slurry recoating using a detection device with the same structure. The detection deviation between devices is small, and the consistency of data detection for the same parameter is higher, which helps to improve the slurry recoating effect of the electrode plates.

[0032] In some embodiments, the first detection device, the slurry re-coating device, the drying mechanism and the second detection device are arranged sequentially along the feeding direction of the feeding mechanism.

[0033] By adopting the technical solution of this embodiment, the electrode plate passes through the first detection device, the slurry re-coating device, the drying mechanism and the second detection device in sequence along its conveying direction. In this way, slurry defect information detection, slurry re-coating, drying and judging whether the electrode plate still has slurry defects are carried out in sequence to improve the efficiency and quality of slurry re-coating of the electrode plate.

[0034] In some embodiments, the slurry re-coating device comprises:

[0035] Two first detection devices, which are respectively arranged at the sides of two opposite surfaces of the electrode plate and are respectively configured to detect the active material layers on the two opposite surfaces of the electrode plate;

[0036] Two slurry re-coating devices are respectively arranged on the sides of the two opposite surfaces of the electrode plate, and are respectively configured to perform slurry re-coating on the active material layers on the two opposite surfaces of the electrode plate.

[0037] By adopting the technical solution of this embodiment, two first detection devices are set to detect the active material layers on the opposite two sides of the electrode plate, and the two first detection devices can be arranged at intervals along the conveying direction of the electrode plate. At the same time, two slurry re-coating devices are set to re-coat the active material layers on the opposite two sides of the electrode plate, and the two slurry re-coating devices can be arranged at intervals along the conveying direction of the electrode plate. In this way, since the two opposite surfaces of the electrode plate are provided with active material layers, a first detection device and a slurry re-coating device are arranged in sequence to detect and re-coat the active material layer on one side of the electrode plate, and another first detection device and another slurry re-coating device are arranged in sequence to detect and re-coat the active material layer on the other side of the electrode plate, so that the slurry re-coating operations of the active material layers on the opposite sides of the electrode plate do not affect or interfere with each other, thereby further improving the effect of slurry re-coating.

[0038] In a second aspect, a method for re-coating a slurry of an electrode plate is provided, comprising:

[0039] Use machine vision to perform image detection on the active material layer of the electrode plate to obtain slurry defect information of the active material layer;

[0040] Applying slurry to the slurry defective part of the active material layer according to the slurry defect information;

[0041] Wherein, obtaining the slurry defect information of the active material layer at least includes obtaining the thickness value of the slurry at the slurry defect part of the active material layer and the area value corresponding to the outline of the slurry defect part, and comparing the thickness value and the area value with the preset thickness value and area value one by one, and calculating the thickness difference and the area difference, and the slurry defect information at least includes the thickness difference and the area difference;

[0042] Filling the slurry defective part of the active material layer with slurry according to the slurry defect information at least includes: locating the slurry defective part according to the thickness difference and the area difference, and filling the slurry defective part with slurry.

[0043] The slurry re-coating method for an electrode plate in an embodiment of the present application detects the active material layer of the electrode plate to obtain slurry defect information of the active material layer, and then re-coats the slurry defective portion of the active material layer, so that the slurry defective portion of the active material layer of the electrode plate is filled with slurry, so that the electrode plate with slurry defect in the active material layer can be used normally, which effectively alleviates the problem of waste of materials and manpower and helps to improve the yield rate of the electrode plate.

[0044] In a third aspect, a pole piece production system is provided, comprising the above-mentioned slurry re-coating equipment, and / or, adopting the above-mentioned slurry re-coating method.

[0045] The electrode sheet production system of the embodiment of the present application integrates the slurry re-coating equipment and / or slurry re-coating method of the active material layer into each process of the electrode sheet production process, and performs real-time dynamic detection and slurry re-coating on the electrode sheets in various states processed in each process (such as large rolled electrode sheets, single film area rolls obtained after pre-slitting, small rolled electrode sheets obtained after die-cutting and stripping, etc.), thereby improving the yield rate of the electrode sheets and further improving the production efficiency of the electrode sheets.

[0046] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0048] Figure 1 A schematic diagram of the structure of a vehicle provided in one embodiment of the present application;

[0049] Figure 2 This is a schematic cross-sectional view of an electrode sheet according to an embodiment of the present application;

[0050] Figure 3 This is a schematic structural diagram of a slurry re-coating device according to an embodiment of the present application;

[0051] Figure 4 for Figure 3 The schematic diagram of the main structure of the slurry re-coating equipment shown;

[0052] Figure 5 for Figure 3 A schematic structural diagram of a slurry re-coating device of the slurry re-coating equipment shown;

[0053] Figure 6 for Figure 4 The enlarged view of point A in the middle;

[0054] Figure 7 for Figure 3 A schematic structural diagram of a slurry feeding device of a slurry re-coating device shown;

[0055] Figure 8 This is a flow chart of a method for re-coating a slurry on an electrode plate according to an embodiment of the present application;

[0056] Fig. 9 A flow chart of a method for re-coating a slurry on an electrode plate according to another embodiment of the present application;

[0057] Fig.10 This is a flow chart of a method for re-coating a slurry on an electrode sheet according to another embodiment of the present application;

[0058] Fig.11 This is a flow chart of a method for re-coating a slurry on an electrode sheet according to another embodiment of the present application;

[0059] Fig.12 This is a flow chart of a method for re-coating slurry on an electrode plate according to yet another embodiment of the present application.

[0060] Among them, the reference numerals in the figure are:

[0061] 1. Battery; 2. Controller; 3. Motor;

[0062] 10. Electrode plate; 11. Current collector; 12. Active material layer; 121. Front slurry layer; 122. Back slurry layer;

[0063] 20. A first detection device;

[0064] 30. Slurry re-coating device; 31. Displacement drive mechanism; 311. First drive member; 312. Second drive member; 313. Third drive member; 314. Guide rail; 315. Sliding block; 316. Motor; 32. Slurry re-coating mechanism; 321. Slurry delivery pump; 322. Re-coating head;

[0065] 40. feeding mechanism; 41. first roller; 42. second roller;

[0066] 50. Drying mechanism; 51. Oven; 511. Box; 512. Feed hole; 513. Discharge hole; 514. Heat dissipation hole; 515. Exhaust fan;

[0067] 60. A second detection device;

[0068] 70. Slurry feeding device; 71. Stirring tank; 72. Stirring motor; 73. Feed inlet; 74. Discharge outlet; 75. Discharge valve. DETAILED DESCRIPTION

[0069] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application clearer, the following Figures 1 to 12 It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0070] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0071] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include one or more of the features.

[0072] Reference to "embodiments" herein means that the specific features, structures, or characteristics described in conjunction with the embodiments may be included in at least some embodiments of the present application. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments in any suitable manner.

[0073] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0074] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two), similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple sheets" refers to more than two sheets (including two sheets). "Several" means one or more than one, unless otherwise clearly and specifically defined.

[0075] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0076] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0077] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or indirectly connected to the other element.

[0078] In the related art, a battery cell generally includes an electrode assembly, which is composed of a positive electrode sheet, a negative electrode sheet and a separator. Among them, the positive electrode sheet includes a positive electrode collector and a positive electrode active material layer, the positive electrode active material layer is coated on the surface of the positive electrode collector, the positive electrode collector not coated with the positive electrode active material layer protrudes from the positive electrode collector coated with the positive electrode active material layer, and the positive electrode collector not coated with the positive electrode active material layer serves as a positive electrode ear; the negative electrode sheet includes a negative electrode collector and a negative electrode active material layer, the negative electrode active material layer is coated on the surface of the negative electrode collector, the negative electrode collector not coated with the negative electrode active material layer protrudes from the negative electrode collector coated with the negative electrode active material layer, and the negative electrode collector not coated with the negative electrode active material layer serves as a negative electrode ear. Among them, the positive electrode sheet and the negative electrode sheet can be collectively referred to as electrode sheets, the positive electrode collector and the negative electrode collector are collectively referred to as current collectors, and the positive electrode active material layer and the negative electrode active material layer are collectively referred to as active material layers.

[0079] Generally, the production process of electrode sheets is as follows: first prepare the current collector, then coat the electrode slurry on the upper and lower surfaces of the current collector respectively, and finally dry the coated electrode slurry to form a large rolled electrode sheet with active material layers on both the upper and lower surfaces. In the subsequent battery production process, the large rolled electrode sheet needs to be pre-cut into single-film area rolls, and finally the single-film area rolls are die-cut and stripped to obtain small rolled electrode sheets. The small rolled electrode sheets obtained after die-cutting and stripping are then wound or stacked to form electrode assemblies.

[0080] In the manufacturing process of electrode plates, such as slurry coating, slurry drying, large roll slitting, die-cutting and striping, it is easy for various reasons to cause missing coating, scratches or bubbles in the active material layer. Missing slurry coating and scratches on the active material layer will cause obvious defects in the active material layer of the electrode plate. When bubbles exist, the bubbles will burst and explode during the drying process of the electrode plate, which will also cause defects in the active material layer. On the one hand, defects in the active material layer will reduce the battery output power (the output power of a battery refers to the output current and voltage of the battery under a certain working condition, and is an important indicator for measuring battery performance) and shorten the battery life. For example, the uneven surface of the electrode plate caused by missing coating, scratches, bubbles and bubble explosions will increase the internal resistance and current density of the battery, thereby affecting the conductivity and stability of the battery, resulting in a decrease in the battery output power. In addition, defects in the active material layer will also affect the compactness and conductivity of the active material layer (positive electrode active material layer and negative electrode active material layer), resulting in uneven distribution of active substances in the active material layer, thereby affecting the capacity of the battery, causing the battery to deform or crack easily during the charge and discharge process, seriously shortening the battery life; on the other hand, defects in the active material layer will also cause an imbalance in the consistency of the battery, resulting in unstable battery performance and increasing the risk of thermal runaway of the battery.

[0081] However, the current production process of electrode plates cannot effectively avoid the above-mentioned problems. Electrode plates with defects in the active material layer can only be removed through quality inspection and cannot be used normally, resulting in a waste of labor and materials.

[0082] Based on this, an embodiment of the present application provides a slurry re-coating device, which includes a first detection device and a slurry re-coating device. The first detection device detects the active material layer of the electrode plate, thereby obtaining slurry defect information of the active material layer. The slurry re-coating device is connected to the first detection device in communication, and performs slurry re-coating on the slurry defective part of the active material layer according to the slurry defect information obtained by the first detection device. The first detection device and the slurry re-coating device work together to achieve mechanical re-coating of the slurry defective part of the active material layer of the electrode plate, so that the defective part of the active material layer can be filled with slurry, so that the electrode plate with slurry defect in the active material layer can be used normally, thereby effectively alleviating the problem of material and manpower waste.

[0083] The technical solution described in the embodiment of the present application is suitable for performing slurry repair on defects such as missing coating, scratches and bubbles in the active material layer of the electrode plate, so as to obtain an electrode plate with a complete and uniform active material layer. The obtained electrode plate can be used for battery cells, and the battery cells can be used for batteries and electrical devices using batteries.

[0084] Among them, batteries can be widely used in various electronic devices, including mobile phones, laptops, electric vehicles, electric cars, electric ships, electric toy cars, electric toy ships, electric toy planes and electric tools. Batteries are devices that can store and release electrical energy to provide the required power for these electronic devices. Batteries can also be energy storage devices. Energy storage devices include energy storage containers, energy storage cabinets, etc.

[0085] Electrical devices may be vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys and electric tools, etc. Spacecraft include airplanes, rockets, space shuttles and spacecrafts, etc. Electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys and electric airplane toys, etc. Electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers, etc.

[0086] For the convenience of description, the following embodiments are described by taking a vehicle as an example of an electrical device in some embodiments of the present application.

[0087] See also Figure 1 , Figure 1 A schematic diagram of the structure of a vehicle provided for some embodiments of the present application. The vehicle may be a fuel vehicle, a gas vehicle or a new energy vehicle, and the new energy vehicle may be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 1 is provided inside the vehicle, and the battery 1 may be provided at the bottom, head or tail of the vehicle. The battery 1 is used to power the vehicle, for example, the battery 1 can be used as an operating power source for the vehicle. The vehicle may also include a controller 2 and a motor 3, and the controller 2 is used to control the battery 1 to power the motor 3, for example, for starting, navigating and driving the vehicle. Working power requirements.

[0088] In the embodiment of the present application, the battery 1 can be used not only as an operating power source for the vehicle, but also as a driving power source for the vehicle, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle.

[0089] In the battery 1 , there may be multiple battery cells, and the multiple battery cells may be connected in series, in parallel, or in mixed connection. Mixed connection means that the multiple battery cells are connected in series and in parallel.

[0090] In one embodiment, multiple battery cells can be directly connected in series, in parallel, or in hybrid connection, and then the whole formed by the multiple battery cells is accommodated inside; of course, the battery 1 can also be a battery module formed by connecting multiple battery cells in series, in parallel, or in hybrid connection, and then the multiple battery modules are connected in series, in parallel, or in hybrid connection to form a whole and accommodated inside. The battery 1 can also include other structures, for example, the battery 1 can also include a busbar component for realizing electrical connection between multiple battery cells.

[0091] Each battery cell may be a secondary battery or a primary battery, or a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited thereto. The battery cell may be cylindrical, flat, rectangular, or in other shapes.

[0092] The battery cell in the embodiment of the present application includes an electrode assembly and a housing, and the electrode assembly is installed in the housing to protect the electrode assembly through the housing.

[0093] The electrode assembly consists of a positive electrode sheet, a negative electrode sheet and a separator. The electrode assembly mainly relies on the movement of metal ions between the positive electrode sheet and the negative electrode sheet to work. The positive electrode sheet includes a positive current collector and a positive active material layer. The positive active material layer is coated on the surface of the positive current collector. The part of the positive current collector that is not coated with the positive active material layer protrudes from the part that is coated with the positive active material layer. The part that is not coated with the positive active material layer serves as a positive electrode tab, or a metal conductor is welded on the positive current collector and led out to serve as a positive electrode tab. Taking lithium-ion batteries as an example, the material of the positive current collector can be aluminum, and the positive active material can be lithium cobalt oxide, lithium iron phosphate, ternary lithium or lithium manganese oxide, etc. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is coated on the surface of the negative electrode current collector. The portion of the negative electrode current collector that is not coated with the negative electrode active material layer protrudes from the portion that is coated with the negative electrode active material layer. The portion that is not coated with the negative electrode active material layer serves as a negative electrode tab, or a metal conductor is welded on the negative electrode current collector and led out to serve as a negative electrode tab. The material of the negative electrode current collector can be copper, and the negative electrode active material can be carbon or silicon, etc. When the battery cell is charged, the current converts electrical energy into chemical energy through the chemical reaction between the electrolyte and the electrode assembly and stores it in the battery cell. During the discharge process, the chemical energy is converted into electrical energy and released.

[0094] Below, combined with the attached Figures 2 to 7 The slurry re-coating equipment of the present application is described in detail with reference to specific embodiments.

[0095] In the embodiments of the present application, Figures 2 to 4As shown, the slurry re-coating device includes a first detection device 20 and a slurry re-coating device 30. The first detection device 20 is configured to detect the active material layer 12 of the electrode plate 10 to obtain slurry defect information of the active material layer 12; the slurry re-coating device 30 is connected to the first detection device 20 for communication, and is configured to re-coat the slurry defect position of the active material layer 12 according to the slurry defect information.

[0096] It should be noted that, in the present embodiment, the first detection device 20 is configured to detect the active material layer 12 of the electrode plate 10 to obtain the slurry defect information of the active material layer 12, which means that the first detection device 20 is an image detection mechanism, which performs image detection on the active material layer 12 of the electrode plate 10 through machine vision, thereby obtaining information of the active material layer 12, and the first detection device 20 stores preset information of the active material layer 12, such as the contour information, thickness information, surface density (mass per unit area of ​​a material of a specified thickness) information and roughness information of the active material layer 12, etc., and the preset information is the information of the standard active material layer 12 that meets the use requirements, and the first detection device 20 compares the detected information with the preset information pre-stored in the device, thereby obtaining the slurry defect information of the active material layer 12. Among them, the slurry defect information refers to: the first detection device 20 compares the information of the active material layer 12 obtained by the detection with the preset information, and obtains the difference information. Exemplarily, the first detection device 20 detects the thickness value of the slurry at the slurry defect site and the area value corresponding to the contour of the slurry defect site, compares the thickness value and area value with the preset thickness value and area value one by one, and calculates the thickness difference and area difference, which correspond to the slurry defect information.

[0097] Exemplarily, the standard contour information and thickness information of the active material layer 12 are pre-input and stored in the first detection device 20. The first detection device 20 detects the active material layer 12 and obtains the contour information and thickness information of the active material layer 12 in the current state, and compares the detected contour information and thickness information with the pre-stored preset information. When the detected information is consistent with the preset information, it indicates that there is no slurry defect in the active material layer 12 currently detected, and when the detected information is inconsistent with the preset information, it indicates that there is a slurry defect in the active material layer 12 currently detected. For example, when there are missing coatings, scratches or bubbles in the active material layer 12 (bubbles explode during the drying operation, so the direct manifestation of the bubbles on the active material layer 12 is the missing coating of slurry at the bubble position), the contour and thickness of the active material layer 12 will change, so that the detected information is inconsistent with the preset information.

[0098] It should be noted that, in the present embodiment, the communication connection between the slurry re-coating device 30 and the first detection device 20 means that the slurry re-coating device 30 and the first detection device 20 interact through signal transmission, thereby establishing communication between the two, so that signals can be transmitted between the slurry re-coating device 30 and the first detection device 20. Exemplarily, the slurry re-coating device 30 and the first detection device 20 can be connected by wired communication or wireless communication, or a central control device such as a computer or a PLC controller can be provided to connect the slurry re-coating device 30 and the first detection device 20 respectively.

[0099] It should be noted that, in the present embodiment, the slurry re-coating device 30 is configured to perform slurry re-coating on the slurry defective portion of the active material layer 12 according to the slurry defect information, which means that: the first detection device 20 compares the detected slurry defect information with the preset information, and when the two are inconsistent, transmits the slurry defect information to the slurry re-coating device 30, and the slurry re-coating device 30 performs slurry re-coating on the slurry defective portion of the active material layer 12 according to the obtained slurry defect information. Exemplarily, the first detection device 20 detects the thickness value of the slurry at the slurry defect site and the area value corresponding to the contour of the slurry defect site, compares the thickness value and area value with the preset thickness value and area value one by one, and calculates the thickness difference and area difference. The first detection device 20 transmits the thickness difference and area difference as slurry defect information to the slurry filling device 30. The slurry filling device 30 then locates the slurry defect site according to the thickness difference and area difference, and then fills the slurry defect site with slurry until the slurry fills the contour of the slurry defect site and the slurry thickness at the slurry defect site is equal to the preset thickness. Alternatively, the first detection device 20 and the slurry repairing device 30 are communicatively connected via the central control device, and the first detection device 20 transmits the thickness value of the slurry at the slurry defective part and the area value corresponding to the contour of the slurry defective part detected to the central control device, and the central control device compares the thickness value and area value with the preset thickness value and area value one by one, and calculates the thickness difference and area difference, and the central control device then transmits the thickness difference and area difference as slurry defect information to the slurry repairing device 30, and the slurry repairing device 30 then performs slurry repair on the slurry defective part according to the thickness difference and area difference.

[0100] The slurry re-coating equipment of the embodiment of the present application includes a first detection device 20 and a slurry re-coating device 30, wherein the first detection device 20 is used to detect the active material layer 12 of the electrode plate 10, so as to obtain slurry defect information of the active material layer 12, and the slurry re-coating device 30 is communicatively connected with the first detection device 20, and is used to perform slurry re-coating on the slurry defective part of the active material layer 12 according to the slurry defect information detected by the first detection device 20. In this way, the first detection device 20 and the slurry re-coating device 30 work together to achieve mechanical re-coating of the slurry-deficient parts of the active material layer 12 of the electrode plate 10, so that the defective parts of the active material layer 12 can be filled with slurry, so that the electrode plate 10 with slurry defects in the active material layer 12 can be used normally, effectively alleviating the waste of materials and manpower; in addition, the slurry re-coating equipment can also be integrated into various processes of the production process of the electrode plate 10, and perform real-time dynamic detection and slurry re-coating on the electrode plates 10 in various states processed in each process (such as large rolled electrode plates, single film area rolls obtained after pre-slitting, small rolled electrode plates obtained after die-cutting and slitting, etc.), thereby improving the yield rate of the electrode plates 10, and then improving the production efficiency of the electrode plates 10.

[0101] In some embodiments, the first detection device 20 includes at least one of a camera detection device, a laser detection device, an infrared detection device, and an ultrasonic detection device.

[0102] In this embodiment, the first detection device 20 may be any one of a camera detection device, a laser detection device, an infrared detection device, an X-ray detection device, and an ultrasonic detection device. By using any one of the camera detection device, the laser detection device, the infrared detection device, and the ultrasonic detection device, the active material layer 12 of the electrode plate 10 can be detected, thereby obtaining the slurry defect information of the active material layer 12.

[0103] In some embodiments, the first detection device 20 can adopt a camera detection device, which is one of the detection devices with more mature technology and relatively commonly used. It collects images of objects through optical sensors and extracts feature information such as contour, thickness, texture, roughness group, color, etc. through image processing algorithms to achieve object detection, identification and analysis.

[0104] In this embodiment, the camera detection device collects the image of the active material layer 12 of the electrode plate 10 through an optical sensor, and extracts the characteristic information of the active material layer 12 through an image processing algorithm, and the characteristic information includes but is not limited to contour information, thickness information, surface density information and roughness information. For example, the camera detection device extracts the thickness information of the active material layer 12, and compares the detected thickness information with the preset thickness information to calculate the difference in thickness information, or extracts the contour information of the active material layer 12, and compares the detected contour information with the preset contour information to calculate the difference in contour area, etc.

[0105] In another embodiment, the first detection device 20 may be a laser detection device, which uses a laser beam to scan an object and obtains the shape and surface features of the object by measuring the reflection or scattering of the laser beam. The laser detection device has the characteristics of high precision, non-contact and high speed, and is widely used in the fields of three-dimensional detection, contour detection and surface defect detection.

[0106] In this embodiment, the laser detection device collects an image of the active material layer 12 of the electrode plate 10 by reflection or scattering of a laser beam, and extracts characteristic information of the active material layer 12 by an image processing algorithm. The characteristic information includes but is not limited to contour information, thickness information, surface density information, and roughness information.

[0107] In other embodiments, the first detection device 20 may be an infrared detection device, which uses infrared light to scan an object and obtains thermal characteristics and infrared images of the object by measuring infrared radiation or reflection. In this embodiment, the infrared detection device collects an image of the active material layer 12 of the electrode plate 10 by infrared radiation or reflection, and extracts characteristic information of the active material layer 12 by an image processing algorithm, and the characteristic information includes but is not limited to contour information, thickness information, surface density information, and roughness information.

[0108] In some embodiments, the first detection device 20 may be an X-ray detection device that uses X-rays to penetrate an object and obtains the internal structure and composition information of the object by measuring the absorption and scattering of the X-rays. In this embodiment, the X-ray detection device collects an image of the active material layer 12 of the electrode plate 10 by measuring the absorption and scattering of the X-rays, and extracts characteristic information of the active material layer 12 through an image processing algorithm, and the characteristic information includes but is not limited to contour information, thickness information, surface density information, and roughness information.

[0109] In other embodiments, the first detection device 20 may also be an ultrasonic detection device, which uses an ultrasonic beam to scan an object, and obtains the internal structure and defect information of the object by measuring the propagation speed and reflection intensity of the ultrasonic wave. In this embodiment, the ultrasonic detection device collects the image of the active material layer 12 of the electrode plate 10 by the propagation speed and reflection intensity of the ultrasonic wave, and extracts the characteristic information of the active material layer 12 by an image processing algorithm, and the characteristic information includes but is not limited to contour information, thickness information, surface density information, and roughness information.

[0110] In some embodiments, the first detection device 20 is a CCD visual detector or a 3D profilometer.

[0111] The slurry defect information of the active material layer 12 is obtained by visually inspecting the active material layer 12 of the electrode sheet 10 using a CCD visual inspection instrument or a 3D profilometer.

[0112] In a specific implementation, the first detection device may be a CCD visual detector. The CCD detection device is an instrument that detects the appearance of an object through a display through a CCD component. The machine vision detection system of the detection device in the CCD has a measurement function, and can automatically measure the appearance dimensions of the active material layer 12, such as the measurement of the contour, area, thickness, pore size and other dimensions. In this way, the CCD detection device is used to perform visual inspection on the active material layer 12 of the electrode plate 10, and the slurry defect information of the active material layer 12 can be obtained.

[0113] In other implementations, the first detection device 20 may use a 3D profiler, which is a high-precision measuring instrument. The 3D profiler uses the principle of laser triangulation. The laser emitter projects a laser plane onto the surface of the object to be measured. The laser reflected by the object to be measured passes through the lens and is captured by the image sensor. Subsequently, the image data collected by the image sensor is processed to reconstruct the 3D shape of the object to be measured, thereby achieving high-precision measurement and detection. In this way, the 3D profiler is used to visually detect the active material layer 12 of the electrode plate 10, and the slurry defect information of the active material layer 12 can be obtained.

[0114] In some embodiments, Figures 3 to 5 As shown, the slurry re-coating device 30 includes a displacement driving mechanism 31 and a slurry re-coating mechanism 32, both of which are communicatively connected to the first detection device 20. The displacement driving mechanism 31 is drivingly connected to the slurry re-coating mechanism 32 to drive the slurry re-coating mechanism 32 to move and perform slurry re-coating on the slurry-deficient part.

[0115] In this way, the displacement driving component drives the slurry re-coating mechanism 32 to move according to the slurry defect information of the first detection device 20, and the slurry re-coating mechanism 32 then re-coats the slurry defective part of the active material layer 12 according to the slurry defect information, thereby achieving slurry re-coating of the slurry defective part.

[0116] Among them, it should be noted that:

[0117] The communication connection between the displacement drive mechanism 31 and the first detection device 20 means that the displacement drive mechanism 31 and the first detection device 20 interact through signal transmission, thereby establishing communication between the two, so that signals can be transmitted between the displacement drive mechanism 31 and the first detection device 20. Exemplarily, the displacement drive mechanism 31 and the first detection device 20 can be connected by wired communication or wireless communication, or a central control device such as a computer or a PLC controller can be provided to connect the displacement drive mechanism 31 and the first detection device 20 respectively.

[0118] The displacement driving mechanism 31 drives the slurry re-coating mechanism 32 to move, which means that the displacement driving mechanism 31 drives the slurry re-coating mechanism 32 to move according to the slurry defect information transmitted by the first detection device 20. Exemplarily, the first detection device 20 converts the slurry defect information into coordinates or distance information, and the displacement driving mechanism 31 drives the slurry re-coating mechanism 32 to move according to the coordinate information or distance information.

[0119] The communication connection between the slurry re-coating mechanism 32 and the first detection device 20 means that the slurry re-coating mechanism 32 and the first detection device 20 interact through signal transmission, thereby establishing communication between the two, so that signals can be transmitted between the slurry re-coating mechanism 32 and the first detection device 20. Exemplarily, the slurry re-coating mechanism 32 and the first detection device 20 can be connected by wired communication or wireless communication, or a central control device such as a computer or a PLC controller can be provided to connect the slurry re-coating mechanism 32 and the first detection device 20 respectively.

[0120] The slurry re-coating mechanism 32 moves and re-coats the slurry defective part with slurry, which means that the slurry re-coating mechanism 32 re-coats the slurry defective part with slurry according to the slurry defect information transmitted by the first detection device 20. Exemplarily, the first detection device 20 converts the slurry defect information into an area difference and a thickness difference, and the slurry re-coating mechanism 32 moves and re-coats the slurry according to the area difference and the thickness difference under the drive of the displacement drive mechanism 31.

[0121] In some embodiments, Figure 4 and Figure 5As shown, the displacement driving mechanism 31 includes a first driving member 311, a second driving member 312 and a third driving member 313, wherein the slurry coating mechanism 32 is installed on the driving end of the third driving member 313, the third driving member 313 is installed on the driving end of the second driving member 312, and the second driving member 312 is installed on the driving end of the first driving member 311. The first driving member 311 drives the second driving member 312, the third driving member 313 and the slurry coating mechanism 32 to reciprocate along the X direction, the second driving member 312 drives the first driving member 311 and the slurry coating mechanism 32 to reciprocate along the Y direction, and the third driving member 313 drives the slurry coating mechanism 32 to reciprocate along the Z direction. In this way, with the cooperation of the first driving member 311, the second driving member 312 and the third driving member 313, the slurry coating mechanism 32 can be driven to move in three-dimensional space, thereby realizing slurry coating of sauce defective parts at any position. Among them, the X direction, the Y direction and the Z direction are perpendicular to each other, and the X direction, the Y direction and the Z direction are as follows Figure 4 The directions indicated by arrows F1, F2, and F3 in the coordinate system.

[0122] In a specific embodiment, Figure 4 and Figure 5 As shown, the first driving member 311, the second driving member 312 and the third driving member 313 can adopt a linear module, which includes a rotatable screw arranged along the driving direction, a displacement nut threadedly connected to the screw, a slider 315 fixedly connected to the displacement nut and connected to the component to be driven and serving as a driving end, and a motor 316 connected to one end of the screw. In this way, the motor 316 runs, drives the screw to rotate, drives the displacement nut to move linearly along the driving direction, and the component to be driven fixed to the slide can achieve linear motion, as shown in FIG. Figure 5 Generally, the first driving member 311, the second driving member 312 and the third driving member 313 all include a slide rail for guiding and supporting, and the slide plate is adapted to be slidably connected with the slider 315, so as to guide the movement of the driving member.

[0123] For example, Figure 5As shown, the first driving member 311 includes a guide rail 314 extending along the X direction, a slider 315 slidably mounted on the guide rail 314, a motor 316 mounted on the guide rail 314, and a rotatable screw rod respectively mounted on the guide rail 314, and a displacement nut threadedly connected to the screw rod. The second driving member 312 is slidably mounted on the guide rail 314 through the slider 315, the slider 315 is threadedly connected to the screw rod through the displacement nut, and the motor 316 is connected to one end of the screw rod. The motor 316 runs to drive the screw rod to rotate, and the rotation of the screw rod drives the displacement nut to move linearly along the X direction. The displacement nut drives the slider 315 to move linearly along the X direction. The slider 315 then drives the second driving member 312 connected thereto to move along the X direction. The movement of the second driving member 312 drives the third driving member 313 and the slurry re-coating mechanism 32 to move synchronously along the X direction. In a specific embodiment, one slide rail can be provided, or two can be provided at intervals along the Y direction. The second driving member 312 is slidably connected to the two slide rails through two sliders 315.

[0124] It can be understood that when the second driving member 312 and the third driving member 313 adopt linear modules, they can have a structure similar to that of the first driving member 311, which will not be described in detail here.

[0125] In other embodiments, the first driving member 311, the second driving member 312 and the third driving member 313 can also be the X-direction driving member, the Y-direction driving member and the Z-direction driving member of the three-dimensional mechanical arm, that is, the first driving member 311, the second driving member 312 and the third driving member 313 are integrated into a mechanical arm structure, and the mechanical arm can at least realize free movement in the X direction, the Y direction and the Z direction, and the slurry re-coating mechanism 32 is installed at the output end of the mechanical arm. Alternatively, in other more embodiments, the first driving member 311, the second driving member 312 and the third driving member 313 can also adopt driving members of other structural forms, and the specific structures of the first driving member 311, the second driving member 312 and the third driving member 313 are not limited here.

[0126] In some embodiments, Figure 4 , Figure 5 and Figure 7 As shown, the slurry re-coating equipment also includes a slurry feeding device 70, and the slurry re-coating mechanism 32 includes a slurry delivery pump 321 and a re-coating head 322 installed at the outlet of the slurry delivery pump 321, the slurry delivery pump 321 is configured to deliver the slurry from the slurry feeding device 70 to the re-coating head 322, and the displacement driving mechanism 31 is drivingly connected to the re-coating head 322.

[0127] Among them, it can be understood that the driving connection between the displacement drive mechanism 31 and the re-coating head 322 means that the re-coating head 322 is installed at the power output end of the displacement drive mechanism 31. Exemplarily, when the displacement drive mechanism 31 includes the first drive member 311, the second drive member 312 and the third drive member 313 in the above embodiment, the re-coating head 322 is installed at the output end of the first three drive members, such as when the third drive member 313 is a linear module, the re-coating head 322 is installed on the slider 315. Alternatively, when the displacement drive mechanism 31 is a three-dimensional mechanical arm, the re-coating head 322 is installed at the gripper position of the mechanical arm.

[0128] It should be noted that the slurry delivery pump 321 is configured to deliver the slurry from the slurry feeding device 70 to the re-coating head 322, which means that the slurry delivery pump 321 quantitatively pumps the slurry from the slurry feeding device 70 according to the slurry defect information provided by the first detection device 20, and pressure-feeds the pumped slurry to the re-coating head 322 to output it to the slurry defect site, thereby achieving slurry re-coating. The slurry delivery pump 321 can be a high-precision screw pump or a small-flow centrifugal pump, etc.

[0129] In this embodiment, the slurry delivery pump 321 delivers the slurry from the slurry feeding device 70 to the re-coating head 322, and the displacement driving mechanism 31 drives the re-coating head 322 to move according to the slurry re-coating information to complete the slurry re-coating of the slurry defective part.

[0130] In some embodiments, the touch-up head 322 includes at least one of an extrusion head and a spray head.

[0131] In a specific embodiment, the re-coating head 322 includes an extrusion head. The extrusion head provides extrusion force through the slurry delivery pump 321, and slurry is squeezed to be output from the outlet of the extrusion head. The slurry is extruded and output. By controlling the extrusion force and the amount of slurry output in a single extrusion, the slurry defective part can be evenly re-coated layer by layer under the directional movement drive of the displacement drive mechanism 31.

[0132] In some other embodiments, the re-coating head 322 includes a spray head.

[0133] In this embodiment, the spray head provides pressure through the slurry delivery pump 321, squeezes the slurry to spray out from the spray head, and the slurry is sprayed to the slurry defective part. By controlling the spraying pressure and the amount of slurry sprayed in a single time, under the directional movement drive of the displacement drive mechanism 31, the slurry defective part can be evenly re-coated layer by layer.

[0134] In other embodiments, the slurry re-coating device 30 is a 3D printer.

[0135] In this embodiment, a 3D printer is used to print the slurry to the slurry defective part, so as to achieve slurry re-coating. In this way, the slurry re-coating is performed using 3D printing technology, and the slurry is transported to the material chamber of the 3D printer for accommodating the printing material. The first detection device 20 is connected to the 3D printer in communication, and the 3D printer prints the slurry in the material chamber layer by layer to the slurry defective part according to the slurry defect information, so as to achieve automatic slurry re-coating of the slurry defective part. 3D printing technology is a rapid prototyping technology, also known as additive manufacturing technology. The first detection device 20 is connected to the 3D printer in communication, and transmits the slurry defect information to the 3D printer. The 3D printer reads the obtained slurry defect information, such as the contour information and thickness information of the slurry defective part, obtains the cross-sectional information of the slurry defective part, and then uses the slurry in the material chamber to print these sections layer by layer to the slurry defective part, so as to complete the slurry re-coating.

[0136] It can be understood that in this embodiment, the displacement drive mechanism 31 and the slurry re-coating mechanism 32 can be integrated into one, that is, the 3D printer structure itself is provided with the displacement drive mechanism 31 and the slurry re-coating mechanism 32, and there is no need to set up a displacement drive mechanism 31 independent of the 3D printer to perform the printing drive action. The equipment has high integration and is easy to repair and manage.

[0137] It can be understood that in the above embodiment, the slurry feeding device 70 can be a slurry feeding device used in the electrode production system, or can be a separate feeding device that only feeds the slurry re-coating device.

[0138] Exemplarily, the slurry feeding device 70 includes a stirring tank 71 for containing slurry, a stirring paddle arranged in the stirring tank 71 and used to rotate and stir the slurry, and a stirring motor 72 connected to the stirring paddle and used to drive the stirring paddle to rotate, wherein the stirring tank 71 is provided with a feed port 73 and a discharge port 74, the inlet of the material chamber of the 3D printer or the slurry delivery pump 321 is connected to the discharge port 74, the discharge port 74 is installed with a discharge valve 75 and a liquid level sensor, the liquid level sensor and the discharge valve 75 cooperate to quantitatively deliver slurry to the material chamber of the 3D printer or the slurry delivery pump 321, and the stirring paddle stirs the slurry to increase the activity of the slurry used for recoating.

[0139] In some embodiments, Figure 3 and Figure 4 As shown, the slurry re-coating device further includes a feeding mechanism 40 , which is configured to sequentially transport the electrode plates 10 to be re-coated with slurry to the first detection device 20 and the slurry re-coating device 30 .

[0140] By adopting the technical solution of this embodiment, the electrode plate 10 is transported by the feeding mechanism 40 to move. When the electrode plate 10 passes through the first detection device 20, the first detection device 20 obtains the slurry defect information of the active material layer 12 of the electrode plate 10. After passing through the first detection device 20, the electrode plate 10 continues to move to the slurry re-coating device 30. The slurry re-coating device 30 re-coats the slurry on the slurry defective part according to the slurry defect information provided by the first detection device 20. The feeding mechanism 40 transports the electrode plate 10 through the first detection device 20 and the slurry re-coating device 30 in sequence. The collection of slurry defect information and slurry re-coating are carried out in an orderly manner, forming a streamlined operation, which helps to improve the slurry re-coating efficiency of the electrode plate 10.

[0141] In a specific embodiment, Figure 4 and Figure 5 As shown, the feeding mechanism 40 includes a plurality of conveying rollers driven by a motor or a cylinder, etc. The plurality of conveying rollers are arranged at intervals along the conveying direction of the electrode sheet 10 to roll and convey the electrode sheet 10 . Exemplarily, the feeding mechanism 40 includes a plurality of first rollers 41 and a plurality of second rollers 42, wherein the plurality of first rollers 41 are arranged at intervals on one side of the electrode sheet 10 along the conveying direction of the electrode sheet 10, and are in rolling contact with the surface of one side of the electrode sheet 10, for example, the first roller 41 is located on the side of the positive electrode slurry layer of the electrode sheet 10 and is in rolling contact with the positive electrode slurry layer, and the plurality of second rollers 42 are arranged at intervals on the other opposite side of the electrode sheet 10 along the conveying direction of the electrode sheet 10, and are in rolling contact with the other opposite side surface of the electrode sheet 10, for example, the second roller 42 is located on the side of the negative electrode slurry layer of the electrode sheet 10 and is in rolling contact with the negative electrode slurry layer, and adjacent first rollers 41 and second rollers 42 are arranged at intervals along a direction perpendicular to the active material layer 12 of the electrode sheet 10, so that the roller shafts of the first rollers 41 and the second rollers 42 rotate in the same direction and at the same speed, thereby realizing the transmission of the electrode sheet 10. The conveying direction of the electrode sheet 10 is along Figure 3 The direction indicated by the dashed arrow.

[0142] In a specific embodiment, along the conveying direction of the electrode sheet 10, the first detection device 20 is arranged in front of the slurry re-coating device 30, so that the first detection device 20 first detects and obtains the slurry defect information of the active material layer 12 in a section of the electrode sheet 10 along the length direction, and then the feeding mechanism 40 conveys the section to the slurry re-coating device 30, and the slurry re-coating device 30 re-coats the slurry defective part in the section. Among them, the length direction of the electrode sheet 10 is in the same direction as the conveying direction of the electrode sheet 10.

[0143] It can be understood that in a specific embodiment, the electrode plate 10 can be moved at a slow and uniform speed. The first detection device 20 detects the slurry defect information during the movement of the electrode plate 10. The slurry re-coating device 30 also re-coats the slurry defective part during the movement of the electrode plate 10. The moving speed of the electrode plate 10, the detection speed of the first detection device 20, and the slurry re-coating speed of the slurry re-coating device 30 can be set and adjusted and controlled in real time as needed, so as to achieve dynamic slurry re-coating. Of course, in other embodiments, the feeding mechanism 40 can also intermittently convey the electrode plate 10, the first detection device 20 detects the slurry defect information of the static electrode plate 10, and the slurry re-coating device 30 re-coats the static electrode plate 10 with slurry.

[0144] In some embodiments, Figure 3 , Figure 4 and Figure 6 As shown, the slurry re-coating equipment further includes a drying mechanism 50, and the drying mechanism 50 is configured to dry the electrode plate 10 after the slurry re-coating device 30 has been re-coated with slurry. The drying mechanism 50 is used to dry the active material layer 12 after the slurry is re-coated.

[0145] It should be noted that, in the present embodiment, the drying mechanism 50 is configured to perform a drying operation on the electrode plate 10 after the slurry re-coating device 30 has been re-coated with slurry, which means that after the active material layer 12 of the electrode plate 10 has been re-coated with slurry by the slurry re-coating device 30, the drying mechanism 50 performs a drying operation on the electrode plate 10 re-coated with slurry. When performing the drying operation, the electrode plate 10 can enter the drying mechanism 50 in whole or in part, and the parameters for executing drying of the drying mechanism 50 can be set according to the amount of re-coated slurry, so that the drying effect of the part of the active material layer 12 after the slurry is re-coated is completely consistent with the drying effect of the other part of the active material layer 12 that does not need to be re-coated with slurry. Among them, the drying mechanism 50 can be a device such as an oven 51, a furnace, etc. that dries the active material layer 12 by raising the ambient temperature.

[0146] For example, Figure 5 and Figure 6As shown, the drying mechanism 50 includes a box body 511 and a heater installed in the box body 511. One end of the box body 511 is provided with a feed hole 512 for the electrode plate 10 to pass through, and the other opposite end of the box body 511 is provided with a discharge hole 513 for the electrode plate 10 to pass out. The feed hole 512 and the discharge hole 513 are arranged opposite to each other along the conveying direction of the electrode plate 10, so that the electrode plate 10 can pass through the feed hole 512 and then pass out from the discharge hole 513 under the drive of the feeding mechanism 40. A plurality of heat dissipation holes 514 are also provided on the box body 511. The heat dissipation holes 514 are connected to the internal space of the box body 511 and are used to dissipate the heat in the box body 511 so that the temperature in the box body 511 remains relatively constant. The box body 511 is also provided with a plurality of exhaust fans 515, which are installed at intervals on the side walls of the box body 511. The exhaust fans 515 are used to circulate the gas inside the box body 511, so that the heat inside the box body 511 is evenly distributed, so that the temperature inside the box body 511 is kept uniform, and the drying effect of the electrode plate 10 is guaranteed. In addition, the exhaust fans 515 can also be used to dissipate heat from the internal space of the box body 511. In particular, when the temperature inside the box body 511 is too high and exceeds the drying temperature of the electrode plate 10, the exhaust fans 515 can be turned on to dissipate heat and reduce the temperature inside the box body 511 in time.

[0147] In some embodiments, the slurry re-coating equipment further includes a second detection device 60 , and the second detection device 60 is configured to detect the active material layer 12 of the electrode plate 10 after being dried by the drying mechanism 50 .

[0148] In this embodiment, if Figure 3 and Figure 4 As shown, after the electrode plate 10 is re-coated with slurry and dried, it is inspected using the second detection device 60 to determine whether the active material layer 12 of the electrode plate 10 still has slurry defects. If there are still slurry defects, the slurry re-coating device 30 can continue to be used for slurry re-coating. If the second detection device 60 detects that no slurry defects are found in the electrode plate 10, the material can be collected for processing.

[0149] Among them, it can be understood that the second detection device 60 is an image detection mechanism, which obtains information about the active material layer 12 by performing image detection on the active material layer 12 of the electrode plate 10. The second detection device 60 stores preset information of the active material layer 12, such as contour information, thickness information, surface density information and roughness information of the active material layer 12. The preset information is standard information of the active material layer 12 that meets the use requirements. The second detection device 60 compares the detected information with the preset information pre-stored in the device. When the comparison result is consistent, it indicates that there is no slurry defect in the active material layer 12 of the electrode plate 10 currently being detected, and when the comparison result is inconsistent, it indicates that there is still a slurry defect in the active material layer 12 of the electrode plate 10 currently being detected.

[0150] In some embodiments, the first detection device 20 and the second detection device 60 have the same structure.

[0151] In this way, the electrode plate 10 is inspected before and after slurry recoating using a detection device of the same structure. The detection deviation between devices is small, and the consistency of data detection for the same parameter is higher, which helps to improve the slurry recoating effect of the electrode plate 10.

[0152] Exemplarily, in a specific embodiment, the first detection device 20 and the second detection device 60 may both adopt CCD visual detection devices, or the first detection device 20 and the second detection device 60 may both adopt 3D profilometers.

[0153] It can be understood that when the first detection device 20 and the second detection device 60 of the same structure are selected, that is, the second detection device 60 can also obtain the slurry deficiency information of the electrode plate 10, the second detection device 60 can also be communicated with the slurry re-coating device 30. After the electrode plate 10 is detected by the second detection device 60, it can be directly transported to the slurry re-coating device 30 without passing through the first detection device 20. The slurry re-coating device 30 can perform slurry re-coating according to the slurry deficiency information transmitted by the second detection device 60.

[0154] It should be noted that, in other embodiments, the first detection device 20 and the second detection device 60 may also use different equipment, so as to accurately detect the active material layer 12 of the electrode plate 10. For example, in a specific embodiment, the second detection device 60 can be used only for image detection of the electrode plate 10 to determine whether there is a slurry defect in the electrode plate 10, without having the ability to obtain slurry defect information, that is, the second detection device 60 only obtains the information of the active material layer 12, and compares it with the preset information of the active material layer 12 stored in the second detection device 60, without calculating the difference between the two information. When the second detection device 60 detects that there is a slurry defect in the active material layer 12 of the electrode plate 10, the electrode plate 10 is transported to the first detection device 20, and the first detection device 20 detects again and calculates the slurry defect information.

[0155] In some embodiments, Figure 3 and Figure 4 As shown, the first detection device 20 , the slurry re-coating device 30 , the drying mechanism 50 and the second detection device 60 are arranged sequentially along the feeding direction of the feeding mechanism 40 .

[0156] In this way, the electrode plate 10 passes through the first detection device 20, the slurry re-coating device 30, the drying mechanism 50 and the second detection device 60 in sequence along its conveying direction. In this way, slurry defect information detection, slurry re-coating, drying and judging whether the electrode plate 10 still has slurry defects are carried out in sequence to improve the efficiency and quality of the slurry re-coating of the electrode plate 10.

[0157] In some embodiments, Figure 3 and Figure 4 As shown, the slurry re-coating equipment includes two first detection devices 20 and two slurry re-coating devices 30, wherein the two first detection devices 20 are respectively arranged on the sides of the two opposite surfaces of the electrode plate 10, and are respectively configured to detect the active material layers 12 on the two opposite surfaces of the electrode plate 10, and the two slurry re-coating devices 30 are respectively arranged on the sides of the two opposite surfaces of the electrode plate 10, and are respectively configured to perform slurry re-coating on the active material layers 12 on the two opposite surfaces of the electrode plate 10.

[0158] In this embodiment, two first detection devices 20 are provided to detect the active material layer 12 on the opposite two sides of the electrode sheet 10, and the two first detection devices 20 can be arranged at intervals along the conveying direction of the electrode sheet 10. At the same time, two slurry re-coating devices 30 are provided to re-coat the active material layer 12 on the opposite two sides of the electrode sheet 10, and the two slurry re-coating devices 30 can be arranged at intervals along the conveying direction of the electrode sheet 10. In this way, since the active material layer 12 is provided on the opposite two sides of the electrode sheet 10, that is, Figure 2The active material layer 12 of the electrode plate 10 shown includes a front slurry layer 121 and a back slurry layer 122 arranged on the opposite side surfaces of the current collector 11, a first detection device 20 and a slurry re-coating device 30, which are arranged in sequence for detecting and re-coating the front slurry layer 121 of the electrode plate 10, and another first detection device 20 and another slurry re-coating device 30, which are arranged in sequence for detecting and re-coating the back slurry layer 122 of the electrode plate 10, so that the slurry re-coating operations on the two opposite surfaces of the electrode plate 10 do not affect or interfere with each other, thereby further improving the slurry re-coating effect.

[0159] It is understandable that a drying mechanism 50 may be provided after the two slurry re-coating devices 30, wherein the first drying mechanism 50 is used to dry the front slurry layer 121 after slurry re-coating, and the second detection device 60 is used to dry the back slurry layer 122 after slurry re-coating.

[0160] It is understandable that a second detection device 60 can also be set after the two drying mechanisms 50, wherein the first second detection device 60 is used to detect and determine whether there are still slurry defects in the front slurry layer 121, and the second second detection device 60 is used to detect and determine whether there are still slurry defects in the back slurry layer 122.

[0161] For example, in a specific embodiment, Figure 3 and Figure 4 As shown, along the conveying direction of the electrode plate 10, a first detection device 20, a slurry re-coating device 30, a drying mechanism 50, a second detection device 60, a first detection device 20, a slurry re-coating device 30, a drying mechanism 50 and a second detection device 60 are provided in sequence from front to back, wherein the first four are used for re-coating the slurry on the front slurry layer 121 of the electrode plate 10, and the last four are used for re-coating the slurry on the back slurry layer 122 of the electrode plate 10.

[0162] Please also read Figure 4 ,and Figures 8 to 12 Another embodiment of the present application further provides a slurry re-coating method for an electrode plate 10, comprising the following steps:

[0163] S10, detecting the active material layer 12 of the electrode plate 10 to obtain slurry defect information of the active material layer 12;

[0164] S10 , applying slurry to the slurry defective portion of the active material layer 12 according to the slurry defective information.

[0165] Among them, it should be noted that:

[0166] In step S10, the active material layer 12 of the electrode plate 10 is detected to obtain the slurry defect information of the active material layer 12, which means that the active material layer 12 of the electrode plate 10 can be image-detected by an image detection device, etc., so as to obtain the information of the active material layer 12. The image detection device, etc. stores preset information of the active material layer 12, such as the contour information, thickness information, surface density information and roughness information of the active material layer 12. The preset information is the information of the standard active material layer 12 that meets the use requirements. The image detection device, etc. compares the detected information with the preset information pre-stored in the device, so as to obtain the slurry defect information of the active material layer 12. Among them, the slurry defect information is basically the same as the slurry defect information in the above embodiments.

[0167] For example, in a specific embodiment, the first detection device 20 in the above embodiments may be used to perform image detection on the active material layer 12 of the electrode plate 10 to obtain slurry defect information of the active material layer 12 .

[0168] In step S20, applying slurry to the slurry defective part of the active material layer 12 according to the slurry defect information means that: the detection device transmits the slurry defect information to the slurry applying device 30, and the slurry applying device 30 applies slurry to the slurry defective part of the active material layer 12 according to the obtained slurry defect information. Exemplarily, the slurry applying device 30 in each of the above embodiments can be used to apply slurry to the slurry defective part. For example, when the first detection device 20 in any of the above embodiments is used to detect and obtain slurry defect information, the first detection device 20 transmits the detected slurry defect information to the slurry applying device 30, and the slurry applying device 30 then applies slurry to the slurry defective part according to the slurry defect information transmitted by the first detection device 20, until the slurry fills the contour of the slurry defective part and the slurry thickness of the slurry defective part is equal to the preset thickness.

[0169] For example, in a specific embodiment, a camera detection device, a laser detection device, an infrared detection device, an X-ray detection device, an ultrasonic detection device, etc. may be used to detect the profile, thickness, surface density, and surface roughness of the active material layer 12 .

[0170] The slurry re-coating method for the electrode plate of the embodiment of the present application detects the active material layer 12 of the electrode plate 10 to obtain the slurry defect information of the active material layer 12, and then re-coats the slurry defective portion of the active material layer 12 with slurry, so that the slurry defective portion of the active material layer 12 of the electrode plate 10 can be filled with slurry, so that the electrode plate 10 with slurry defect in the active material layer 12 can be used normally, which effectively alleviates the waste of materials and manpower and helps to improve the yield rate of the electrode plate 10.

[0171] In some embodiments, in step S10 , detecting the active material layer 12 of the electrode plate 10 at least includes: detecting one or more of the profile, thickness, surface density and surface roughness of the active material layer 12 .

[0172] The slurry defect information of the active material layer 12 is obtained by detecting one or more of the profile, thickness, surface density and surface roughness of the active material layer 12 .

[0173] In some embodiments, in step S10 , obtaining the slurry defect information of the active material layer 12 includes: obtaining at least the contour information and thickness information of the slurry defect location of the active material layer 12 .

[0174] By detecting the contour information and thickness information of the active material layer 12 and comparing the obtained contour information and thickness information with the preset information, the slurry defect information of the active material layer 12 can be obtained. In particular, for the slurry defect, by determining the area corresponding to the contour of the slurry defect part and the slurry thickness value at each position within the contour range, the amount of slurry defect in the slurry defect part can be obtained, and the slurry re-coating device 30 can re-coat the slurry defect part with slurry according to the contour information and thickness information.

[0175] In some embodiments, in step S20, applying slurry to the slurry defective portion of the active material layer 12 according to the slurry defect information at least includes: applying slurry along the contour of the slurry defective portion according to the thickness information and the contour information, so that the slurry defective portion is filled with slurry and the slurry thickness is equal to the preset slurry thickness of the active material layer 12.

[0176] According to the contour information, the slurry is applied along the contour of the slurry-deficient part, and according to the thickness information, the slurry is applied until the slurry fills the contour of the slurry-deficient part, and the slurry thickness at the slurry-deficient part is equal to the preset thickness. In this way, the slurry application at the slurry-deficient part can be completed.

[0177] In some embodiments, in the step of obtaining the slurry defect information of the active material layer 12, the information value obtained by detecting the active material layer 12 is compared with the preset information value, and the difference between the information value obtained by the detection and the preset information value is calculated, and the slurry defect information includes the difference.

[0178] By calculating the difference between the information value obtained and the preset information, the slurry defect information of the slurry defective part can be obtained, and then the slurry can be reapplied according to the slurry defect information.

[0179] Exemplarily, the first detection device 20 of any of the above-mentioned embodiments is used to detect the active material layer 12. The first detection device 20 detects and obtains the thickness value of the slurry at the slurry defect site and the area value corresponding to the contour of the slurry defect site, compares the thickness value and area value with the preset thickness value and area value one by one, and calculates the thickness difference and area difference. The first detection device 20 transmits the thickness difference and area difference as slurry defect information to the slurry filling device 30. The slurry filling device 30 then fills the slurry defect site with slurry according to the thickness difference and area difference, until the slurry fills the contour of the slurry defect site and the slurry thickness at the slurry defect site is equal to the preset thickness.

[0180] In some embodiments, obtaining the slurry defect information of the active material layer 12 includes: respectively obtaining the slurry defect information of the active material layer 12 on two opposite sides of the electrode plate 10 .

[0181] The active material layers 12 (front slurry layer 121 and back slurry layer 122) on the opposite side surfaces of the electrode plate 10 are respectively detected to obtain the slurry defect information of the front slurry layer 121 and the back slurry layer 122 of the electrode plate 10 respectively, so that the acquisition of the slurry defect information on the opposite side surfaces of the electrode plate 10 does not affect or interfere with each other, thereby further improving the effect of slurry recoating.

[0182] In some embodiments, performing slurry re-coating on the slurry defective parts of the active material layer 12 according to the slurry defect information includes: performing slurry re-coating on the slurry defective parts of the active material layer 12 on opposite sides of the electrode plate 10 .

[0183] The active material layers 12 (the front slurry layer 121 and the back slurry layer 122 ) on the opposite side surfaces of the electrode plate 10 are respectively re-coated with slurry, so that the slurry re-coating operations of the active material layers 12 on the opposite side surfaces of the electrode plate 10 do not affect or interfere with each other.

[0184] Among them, it can be understood that in a specific embodiment, different detection devices can be respectively set to detect the front slurry layer 121 and the back slurry layer 122 of the electrode plate 10, and different slurry re-coating devices 30 can be respectively set to re-coat the slurry defective parts of the active material layer 12 on the opposite two sides of the electrode plate 10. Exemplarily, the first detection devices 20 in the two above-mentioned embodiments can be used to detect the front slurry layer 121 and the back slurry layer 122 of the electrode plate 10, and the slurry re-coating devices 30 in the above-mentioned embodiments can be used to re-coat the slurry defective parts of the front slurry layer 121 and the back slurry layer 122.

[0185] In some embodiments, Fig. 9 As shown, after the slurry defective part of the active material layer 12 is re-coated with slurry according to the slurry defect information, that is, after step S20, the following further includes: S30, drying the electrode plate 10 after the slurry defective part is re-coated with slurry.

[0186] The electrode plate 10 that has been re-coated with slurry is dried to obtain a dry electrode plate 10. In this way, after the active material layer 12 of the electrode plate 10 is re-coated with slurry by the slurry re-coating device 30, the drying mechanism 50 performs a drying operation on the electrode plate 10 re-coated with slurry. When performing the drying operation, the electrode plate 10 can enter the drying mechanism 50 as a whole or in part, and the parameters for executing drying of the drying mechanism 50 can be set according to the amount of re-coated slurry, so that the drying effect of the part of the active material layer 12 after the slurry is re-coated is completely consistent with the drying effect of the other part of the active material layer 12 that does not need to be re-coated with slurry. Among them, the drying mechanism 50 can adopt the drying mechanism 50 in the above-mentioned embodiments.

[0187] It can be understood that, in a specific embodiment, the front slurry layer 121 and the back slurry layer 122 of the electrode plate 10 are dried separately, so that the drying operations on the two opposite sides of the electrode plate 10 do not affect or interfere with each other.

[0188] In some embodiments, Fig. 9 As shown, after the electrode plate 10 after the slurry recoating is dried, that is, after step S30, the following further includes: S40, detecting the dried active material layer 12, and determining whether there are still slurry defective parts in the dried active material layer 12.

[0189] After the electrode plate 10 is re-coated with slurry and dried, it is tested again to determine whether there are still slurry defects in the active material layer 12 of the electrode plate 10. If there are still slurry defects, the slurry can be re-coated. If no slurry defects are found in the second test, the electrode plate 10 can be collected and processed.

[0190] It is understandable that an image detection device can also be used to perform image detection on the active material layer 12 of the electrode plate 10 after slurry recoating and drying, for example, the first detection device 20 or the second detection device 60 in the above embodiments can be used.

[0191] In some embodiments, in step S40 , detecting the dried active material layer 12 at least includes: detecting one or more of the profile, thickness, surface density and surface roughness of the active material layer 12 .

[0192] By detecting one or more of the profile, thickness, surface density and surface roughness of the active material layer 12 , the slurry defect information of the active material layer 12 is obtained, thereby determining whether the active material layer 12 has slurry defects.

[0193] In some embodiments, Fig.11 As shown, after the dried active material layer 12 is tested, that is, after step S40, the following steps are further included:

[0194] S50, when it is detected that there is a slurry defective part in the active material layer 12, the slurry defect information of the slurry defective part is obtained, the slurry defective part of the active material layer 12 is re-coated with slurry according to the slurry defective information, and the electrode plate 10 after the slurry defective part is dried.

[0195] In this way, the electrode plate 10 that still has slurry defects after the first slurry re-coating is re-coated with slurry a second time or multiple times until there are no slurry defects in the electrode plate 10, thereby improving the reliability of the slurry re-coating.

[0196] In some embodiments, Fig.12 As shown, after the dried active material layer 12 is tested, that is, after step S40, the following steps are further included:

[0197] S50 ′: When it is detected that there are no slurry defective portions in the active material layers 12 on the two opposite surfaces of the electrode sheet 10 , the electrode sheet 10 is collected.

[0198] It should be noted that, in the above-mentioned embodiments, the detection device for obtaining the slurry defect information of the active material layer 12 of the electrode plate 10 can adopt the first detection device 20 in the above-mentioned embodiments, and it can also adopt other detection devices, so as to obtain the required information and data, and it is not limited to it here. The slurry re-coating device 30 for re-coating the slurry defective part can adopt the slurry re-coating device 30 in the above-mentioned embodiments, and of course it can also adopt other re-coating equipment, so as to be able to accurately re-coat the slurry defective part, and it is not limited to it here.

[0199] Another embodiment of the present application further provides a pole piece production system, which includes the slurry re-coating equipment in any of the above embodiments.

[0200] The electrode sheet production system of the present embodiment integrates the slurry re-coating equipment of the active material layer 12 into each process of the production process of the electrode sheet 10, and performs real-time dynamic detection and slurry re-coating on the electrode sheets 10 in various states obtained in each process (such as large rolled electrode sheets, single film area rolls obtained after pre-slitting, small rolled electrode sheets obtained after die-cutting and slitting, etc.), thereby improving the yield rate of the electrode sheets 10 and further improving the production efficiency of the electrode sheets 10.

[0201] Since the electrode production system adopts the slurry re-coating equipment of the above-mentioned embodiments, the electrode production system at least has all the beneficial effects of the above-mentioned slurry re-coating equipment, which will not be repeated here.

[0202] Another embodiment of the present application further provides a pole piece production system, which includes the slurry re-coating method in any of the above embodiments.

[0203] The electrode sheet production system of the present embodiment integrates the slurry re-coating operation of the active material layer 12 into each process of the production process of the electrode sheet 10 by adopting the above-mentioned slurry re-coating method, and performs real-time dynamic detection and slurry re-coating on the electrode sheets 10 in various states obtained in each process (such as large rolled electrode sheets, single film area rolls obtained after pre-slitting, small rolled electrode sheets obtained after die-cutting and slitting, etc.), thereby improving the yield rate of the electrode sheets 10 and further improving the production efficiency of the electrode sheets 10.

[0204] Since the pole piece production system adopts the slurry re-coating method of the above-mentioned embodiments, the pole piece production system at least has all the beneficial effects of the above-mentioned slurry re-coating equipment, which will not be described in detail here.

[0205] The above description of various embodiments tends to emphasize the differences between the various embodiments. The same or similar aspects can be referenced to each other, and for the sake of brevity, they will not be repeated herein.

[0206] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A slurry re-coating device, characterized in that: include: A first detection device is configured to perform image detection on the active material layer of the electrode plate through machine vision to obtain slurry defect information of the active material layer; a slurry re-coating device, which is communicatively connected to the first detection device and is configured to perform slurry re-coating on the slurry defective part of the active material layer according to the slurry defect information; Among them, the first detection device at least detects the thickness value of the slurry at the slurry defect site of the active material layer and the area value corresponding to the contour of the slurry defect site, and compares the thickness value and the area value with the preset thickness value and area value one by one, and calculates the thickness difference and the area difference, the slurry defect information at least includes the thickness difference and the area difference, the slurry re-coating device at least locates the slurry defect site according to the thickness difference and the area difference, and performs slurry re-coating on the slurry defect site.

2. The slurry re-coating equipment according to claim 1, characterized in that: The first detection device includes at least one of a camera detection device, a laser detection device, an infrared detection device, an X-ray detection device and an ultrasonic detection device.

3. The slurry re-coating equipment according to claim 1, characterized in that: The first detection device is a CCD visual detector or a 3D profiler.

4. The slurry re-coating equipment according to claim 1, characterized in that: The slurry re-coating device includes a displacement driving mechanism and a slurry re-coating mechanism, both of which are communicatively connected to the first detection device. The displacement driving mechanism is drivably connected to the slurry re-coating mechanism to drive the slurry re-coating mechanism to move and perform slurry re-coating on the slurry-deficient area.

5. The slurry re-coating equipment according to claim 4, characterized in that: The slurry re-coating equipment also includes a slurry feeding device, and the slurry re-coating mechanism includes a slurry delivery pump and a re-coating head installed at the outlet of the slurry delivery pump, the slurry delivery pump is configured to deliver the slurry from the slurry feeding device to the re-coating head, the displacement drive mechanism is drivingly connected to the re-coating head, and the slurry delivery pump is communicatively connected to the first detection device.

6. The slurry re-coating equipment according to claim 5, characterized in that: The re-coating head includes at least one of an extrusion head and a spray head.

7. The slurry re-coating equipment according to claim 4, characterized in that: The slurry re-coating device is a 3D printer.

8. The slurry re-coating equipment according to any one of claims 1 to 7, characterized in that: The slurry re-coating equipment further includes a feeding mechanism, which is configured to sequentially transport the electrode plates to be re-coated with slurry to the first detection device and the slurry re-coating device.

9. The slurry re-coating equipment according to claim 8, characterized in that: The slurry re-coating equipment further includes a drying mechanism, and the drying mechanism is configured to dry the electrode plate after the slurry is re-coated by the slurry re-coating device.

10. The slurry re-coating equipment according to claim 9, characterized in that: The slurry re-coating equipment further includes a second detection device, which is configured to detect the active material layer of the electrode plate after being dried by the drying mechanism.

11. The slurry re-coating equipment according to claim 10, characterized in that: The first detection device and the second detection device have the same structure.

12. The slurry re-coating equipment according to claim 10, characterized in that: The first detection device, the slurry re-coating device, the drying mechanism and the second detection device are arranged in sequence along the feeding direction of the feeding mechanism.

13. The slurry re-coating equipment according to any one of claims 1 to 7, characterized in that: The slurry re-coating equipment comprises: two first detection devices, the two first detection devices are respectively arranged at the sides of two opposite surfaces of the electrode plate, and are respectively configured to detect the active material layers on two opposite surfaces of the electrode plate; The two slurry re-coating devices are respectively arranged on the sides of the two opposite surfaces of the electrode plate, and are respectively configured to perform slurry re-coating on the active material layers on the two opposite surfaces of the electrode plate.

14. A slurry re-coating method, characterized in that: include: Using machine vision to perform image detection on the active material layer of the electrode plate to obtain slurry defect information of the active material layer; Performing slurry repair on the slurry defective part of the active material layer according to the slurry defective information; Wherein, obtaining the slurry defect information of the active material layer at least includes obtaining the thickness value of the slurry at the slurry defect part of the active material layer and the area value corresponding to the contour of the slurry defect part, and comparing the thickness value and the area value with the preset thickness value and area value one by one, and calculating the thickness difference and the area difference, and the slurry defect information at least includes the thickness difference and the area difference; The performing slurry re-coating on the slurry defective part of the active material layer according to the slurry defect information at least includes: locating the slurry defective part according to the thickness difference and the area difference, and performing slurry re-coating on the slurry defective part.

15. The slurry re-coating method according to claim 14, characterized in that: The image detection of the active material layer of the electrode plate by using machine vision at least includes: detecting one or more of the contour, thickness, surface density and surface roughness of the active material layer.

16. The slurry re-coating method according to claim 14, characterized in that: The positioning of the slurry defective portion according to the thickness difference and the area difference, and the slurry patching of the slurry defective portion at least includes: patching the slurry along the contour of the slurry defective portion according to the thickness difference and the area difference, so that the slurry defective portion is fully filled with slurry and the slurry thickness is equal to the preset slurry thickness of the active material layer.

17. The slurry re-coating method according to claim 14, characterized in that: The obtaining of the slurry defect information of the active material layer includes: respectively obtaining the slurry defect information of the active material layer on two opposite sides of the electrode plate.

18. The slurry re-coating method according to claim 14, characterized in that: The performing slurry re-coating on the slurry defective parts of the active material layer according to the slurry defect information includes: performing slurry re-coating on the slurry defective parts of the active material layer on opposite sides of the electrode plate respectively.

19. The slurry re-coating method according to claim 14, characterized in that: After the slurry defective part of the active material layer is re-coated with slurry according to the slurry defect information, the method further includes: drying the electrode plate after the slurry defective part is re-coated with slurry.

20. The slurry re-coating method according to claim 19, characterized in that: After the electrode plate after the slurry re-coating is dried, the method further includes: detecting the dried active material layer and determining whether there are any slurry-deficient areas in the dried active material layer.

21. The slurry re-coating method according to claim 20, characterized in that: The detecting of the active material layer after drying at least includes: detecting one or more of the profile, thickness, surface density and surface roughness of the active material layer.

22. The slurry re-coating method according to claim 21, characterized in that: After the active material layer after drying is tested, the method further includes: When it is detected that the active material layer has the slurry defective part, the slurry defective part is obtained, the slurry defective part is re-coated with slurry according to the slurry defective information, and the electrode plate after the slurry defective part is dried; When it is detected that no slurry defective parts exist in the active material layers of the electrode plates, the electrode plates are collected.

23. A pole piece production system, characterized in that: It comprises the slurry re-coating equipment as described in any one of claims 1 to 13, and / or, adopts the slurry re-coating method as described in any one of claims 14 to 22.

Citation Information

Patent Citations

  • Plate damage automatic repair device

    CN108582315A

  • Automatic electrophoresis powder spraying and coating system

    CN115261953A

  • Gluing area detection method, electronic equipment and computer readable storage medium

    CN116917935A

  • Supplementary coating control method, pole piece supplementary coating equipment and pole piece production system

    CN117139079A

  • Application device and image formation apparatus

    JP2021010858A

Cited By

  • Electrode sheet production system, and slurry repair coating apparatus and method

    WO2025260476A1